Biomass-based sodium ion hard carbon negative electrode material with low cost and high performance

Through the pretreatment and combined heat treatment technology of biomass-based materials, high-performance sodium ion hard carbon anode material is formed, solving the problems of energy density and low Coulomb efficiency of existing sodium ion battery hard carbon anode materials, and achieving cost reduction and performance promote.

CN119050352AActive Publication Date: 2024-11-29大秦新能源科技(泰州)有限公司

Patent Information

Application Number
CN202411166428.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing sodium ion battery hard carbon anode materials have low energy density, low Coulomb efficiency, high cost, and their structural control methods are not targeted enough, resulting in difficult performance improvement.

Method used

The hard carbon negative electrode material is prepared by biomass-based materials. Through the combination of biomass pretreatment, low-temperature cracking, low-temperature preoxidation and hydrothermal preoxidation, impurities are removed, oxygen-containing functional groups are introduced, and pseudographite layers and amorphous non-forming non- Crystal domains, combined with graphite phase g-C3N4, perform high-temperature calcination, regulate the pore structure, and improve sodium storage capacity and electrochemical properties.

Benefits of technology

It significantly improves the energy density and electrochemical performance of sodium ion hard carbon anode material, improves the reversible sodium storage capacity and rate performance, and reduces the cost, optimizes the pore size distribution and specific surface area of ​​the material, which is suitable for the embedding and detachment of sodium ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050352A_ABST
    Figure CN119050352A_ABST
Patent Text Reader

Abstract

The invention relates to the field of sodium ion battery materials, in particular to a biomass-based sodium ion hard carbon negative electrode material with low cost and high performance. A preparation method of the low-cost and high-performance biomass-based sodium ion hard carbon negative electrode material comprises the following steps: biomass pretreatment: cleaning, drying, crushing and screening a biomass material to obtain precursor powder; precursor pretreatment: the obtained precursor powder is pretreated, the pretreatment comprises one or more combined treatments of low-temperature cracking, low-temperature pre-oxidation and hydrothermal pre-oxidation, and a hard carbon precursor is obtained; cleaning and purifying: cleaning the pretreated sample, and drying; high-temperature calcination: uniformly mixing the treated sample and graphite phase g-C3N4 according to a mass ratio of 1: (1-3), introducing a protective gas, heating to a final temperature at a heating rate of 0.5-10 DEG C / min, carrying out a constant-temperature reaction for 0.5-8 h, and cooling to a room temperature at a cooling rate of 0.1-10 DEG C / min; and pickling and drying: pickling and drying the sample to obtain the hard carbon negative electrode material. The low-cost and high-performance biomass-based sodium ion hard carbon negative electrode material has good sodium storage performance, higher reversible specific capacity and first coulombic efficiency, shows excellent reversible sodium storage capacity, does not cause reduction of the performance of a graphite negative electrode material while reducing the cost, and has good application prospects. And the excellent performance of the hard carbon negative electrode material can still be maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of sodium ion battery materials, and more specifically, to a low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material. Background Art

[0002] Electrochemical energy storage systems represented by lithium-ion batteries are widely used in the field of energy storage due to their advantages such as high energy density and high efficiency. With the continuous development of science and technology, lithium-ion batteries are widely used in electronic digital consumer batteries and electric vehicle power batteries. The limited reserves and uneven distribution of lithium have led to high costs in the field of energy storage, which cannot meet the needs of large-scale applications in the future. The new generation of energy storage battery systems needs to have the characteristics of abundant resources, low prices, environmental friendliness, and electrochemical properties similar to lithium. Sodium and lithium belong to the same group of elements, have similar physical and chemical properties to lithium, are abundant in resources and environmentally friendly, and are low in price. Sodium ions have more stable electrochemical properties and safety performance.

[0003] As the negative electrode material of lithium-ion batteries, graphite has a layered structure. Lithium ions can be inserted into the graphite layer. However, the ionic radius of sodium ions (r = 0.113nm) is at least 35% larger than that of lithium ions (r = 0.076nm), which makes sodium ions relatively stable in the rigid lattice. In the regular graphite structure and high-temperature graphitized carbon mesophase microspheres, there is almost no sodium embedding capacity. The emergence of hard carbon materials solves this key problem. Hard carbon materials have the advantages of abundant sources and simple preparation. However, the low first coulomb efficiency and insufficient capacity of hard carbon materials lead to low energy density of sodium ion batteries, which limits the development of hard carbon negative electrodes. At the same time, since the sodium storage mechanism of hard carbon is not clear, the structural regulation method of hard carbon is not targeted, which makes it particularly difficult to improve the performance of hard carbon. In addition, although the source of hard carbon is abundant, its cost increases significantly after multiple treatments. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the present application provides a low-cost and high-performance biomass-based sodium ion hard carbon negative electrode material and a preparation method thereof.

[0005] In the first aspect, the present application provides a low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material, which adopts the following technical solution: A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material, the preparation method of the hard carbon negative electrode material comprising: (1) Biomass pretreatment: washing, drying, crushing and screening the biomass material to obtain precursor powder; (2) Precursor pretreatment: pretreating the precursor powder obtained in (1), wherein the pretreatment includes one or more combined treatments of low-temperature pyrolysis, low-temperature pre-oxidation and hydrothermal pre-oxidation to obtain a hard carbon precursor; (3) Cleaning and purification: cleaning and drying the sample after the above pretreatment; (4) High temperature calcination: the sample treated in (3) and the graphite phase g-C3N4 are mixed uniformly at a mass ratio of 1:(1-3), a protective gas is introduced, the temperature is increased at a rate of 0.5-10°C / min to the final temperature, and the reaction is kept at a constant temperature for 0.5-8h, and the temperature is reduced to room temperature at a rate of 0.1-10°C / min; (5) Acid washing and drying: The above samples are acid washed and dried to obtain hard carbon negative electrode materials.

[0006] By adopting the above technical scheme, hard carbon materials are prepared using biomass as a precursor. By pretreating the cheap and easily available biomass materials, impurities can be effectively removed, and the particle size range of the precursor powder can be controlled to improve the consistency of the performance of the biomass-derived hard carbon materials. Then, by limiting the combined steps of the precursor pretreatment, the organic matter in the biomass material reacts to produce a large amount of coal tar and other impurities. The pre-oxidation treatment can introduce oxygen-containing functional groups and other components into the biomass material, so that the pore structure and chemical environment are changed, and the basis for forming a material with rich pseudo-graphite layer microcrystalline domains and amorphous non-crystalline domains is improved to form a hard carbon precursor. Then, by washing, the residual impurities are removed to improve the purity. Subsequently, the graphite phase g-C3N4 is added in proportion, and the stable network structure can be used as a template to guide the graphitization of hard carbon under high-temperature calcination, forming a pseudo-graphite layer and expanding the interlayer spacing, while forming rich pores. It also reduces defects and impurity functional groups, improves the degree of graphitization, and further improves the sodium storage capacity of hard carbon. The stable structure is conducive to the free movement of sodium ions between layers, and is more conducive to the embedding / ejection of sodium ions, making the energy density of hard carbon materials higher and enhancing the rate performance. By adjusting the heating rate, the ratio of open pores to closed pores can be effectively regulated, thereby significantly improving the electrochemical properties of sodium ion hard carbon negative electrode materials. The electrochemical properties of the materials within the mass ratio range of the treated samples and the graphite phase g-C3N4 of the present application are optimal. This may be because too little graphite phase g-C3N4 cannot fully guide calcination and provide a stable network structure, which is not conducive to the embedding / ejection of sodium ions. Too much graphite phase g-C3N4, on the contrary, leads to excessive hardness of the material, poor modifiable processability, and a relatively concentrated pore size distribution range, which is not conducive to the migration and diffusion of sodium ions, affecting the reversible embedding / ejection of sodium ions.

[0007] In a specific embodiment, the hard carbon negative electrode material is an active negative electrode material having a large number of pseudo-graphite microcrystalline domains and amorphous non-crystalline domains.

[0008] The active negative electrode material forms a pseudo-graphite layer, which contains amorphous domains in addition to crystalline domains, and is accompanied by rich edges, defects and pores, and contains a large number of saturated carbon-carbon bonds, aromatic rings or their combinations. Therefore, the microcrystalline domain area with high arrangement and molecular order can be surrounded by the amorphous non-crystalline domain area with less arrangement and looseness, so that the pseudo-graphite layer of the negative electrode material of the sodium ion battery presents short-range order and long-range disorder, and there are a large number of micropores, further optimizing the internal pore size and improving the modifiability of the pores, thereby regulating and improving the composition and structure of the derived hard carbon, increasing the sodium storage capacity of the hard carbon, and increasing the disorder of the hard carbon, improving the reversible sodium storage capacity, which can reduce the irreversible adsorption of sodium ions, making the sodium ions penetrate and escape faster, and significantly improving the electrochemical performance.

[0009] In a specific embodiment, the biomass material in (1) is sunflower seed husk.

[0010] By adopting the above technical scheme, the hard carbon negative electrode material of sodium ion battery is prepared with cheap and easily available sunflower seed shell biomass as raw material. Compared with other biomass materials, the impurity content is lower and no complicated impurity removal process is required. Secondly, compared with other biomass materials, the sunflower seed shell can obtain a suitable specific surface area and more pores through pretreatment and high-temperature calcination process, and the pore size distribution is larger. The mesopore pores are conducive to the migration and diffusion of sodium ions, and the micropores provide sodium storage sites for reversible insertion / removal of sodium ions.

[0011] In a specific embodiment, the hydrothermal pre-oxidation in (2) is to add 0.5-5wt% hydrogen peroxide solution, disperse (5-8)g of precursor powder per 100ml hydrogen peroxide solution, and perform constant temperature hydrothermal reaction at 100-200°C for 12-24h.

[0012] By adopting the above technical solution, hydrothermal pre-oxidation can increase the overall porosity and specific surface area of ​​the material, provide more sites for the storage of sodium ions, and reduce the ion diffusion barrier, so that sodium ions can penetrate and escape faster, and enhance the reversible specific capacity and rate performance. The hydrothermal oxidation temperature can control the pre-oxidation degree of the biomass precursor. If the temperature is too high, the material porosity and specific surface area will be too high, affecting the penetration and escape speed of sodium ions. If the temperature is too low, it is not conducive to the embedding of sodium ions.

[0013] In a specific embodiment, the low temperature cracking in (2) is to heat the temperature to 500-800°C at a rate of 0.5-10°C / min under a protective atmosphere, react at a constant temperature for 0.5-8h, and then cool the temperature to room temperature at a rate of 0.1-10°C / min.

[0014] In a specific embodiment, the protective atmosphere is at least one of argon and nitrogen, and the gas flow rate is 10-100 mL / min.

[0015] Preferably, the pretreatment is low-temperature pre-oxidation followed by low-temperature cracking treatment to obtain a hard carbon precursor; In view of the large amount of cellulose and lignin in sunflower seed shells, low-temperature pre-oxidation is first used to break the hydrogen bonds in the molecules, thereby forming short carbon rings, which is the basis for the material to have advantages such as high specific surface area and pore structure, and to enhance the sodium ion energy storage; in this process, hydrogen peroxide solution is added, and the cellulose in the sunflower seed shells is oxidized, making the hydrothermal oxidation reaction more thorough, with a higher oxygen content, forming more sodium storage sites, and enhancing the sodium storage performance; in addition, oxygen-containing functional groups can make the graphite phase g-C3N4 produce more electron holes, optimize the structure of the precursor, and increase the sodium storage capacity of hard carbon; and then low-temperature pyrolysis is used to remove impurities such as coal tar, thereby improving the thermal efficiency of carbonization and the quality of the product. The applicant found that the low-temperature pre-oxidation followed by low-temperature pyrolysis treatment has better performance than the pre-treatment by low-temperature pre-oxidation or low-temperature pyrolysis alone. This may be because, through the two-step pre-treatment, the particle size of the precursor powder is further regulated within a suitable range, and the consistency of the performance of the biomass-derived hard carbon material is improved; a material with richer pseudo-graphite layer microcrystalline domains and amorphous non-crystalline domains is formed. The cracking temperature environment can regulate the structural morphology, crystals, amorphous structure, and carbon layer spacing of the obtained hard carbon material. If the temperature is too high, the hard carbon material will be over-carbonized, the pore size distribution of the hard carbon material will be too large, and the layer spacing will expand, which is not conducive to the embedding of sodium ions, thereby affecting the sodium storage performance. If the temperature is too low, the carbonization effect is poor, which affects the high-temperature calcination process, reduces the hard carbon sodium storage capacity of the hard carbon negative electrode material, and thus affects its electrochemical performance.

[0016] In a specific embodiment, the cleaning in (3) comprises one or more of acid cleaning, 60-80° C. alkaline solution immersion cleaning and water cleaning.

[0017] Preferably, the sample is first washed with 2 wt % hydrochloric acid, then immersed and washed with 5 mol / L potassium hydroxide solution heated to 70° C., the solid-liquid ratio of the sample to the alkali solution is 1:15 g / mL, and finally washed with water 2-3 times.

[0018] Preferably, the drying in (3) comprises freeze drying at a temperature of -50 to 45°C for 9 to 11 hours.

[0019] By adopting the above technical scheme, soluble ionic impurities such as natural organic matter in sunflower seed shells are removed by acid washing, and insoluble impurities such as oil impurities are removed by alkaline soaking to prevent pore blockage. The residual water molecules after washing are then quickly freeze-dried at low temperature to remove the water molecules, and there is still a certain pore-forming effect at the original position, which further improves the electrochemical performance.

[0020] In a specific embodiment, the low-temperature pre-oxidation in (2) is to heat the temperature to 200-300°C at a rate of 0.5-10°C / min, react at a constant temperature for 0.5-8h, and then cool the temperature to room temperature at a rate of 0.1-10°C / min.

[0021] By adopting the above technical solution, oxygen-containing functional groups can be introduced through pre-oxidation treatment, thereby increasing the disorder of hard carbon and improving the reversible sodium storage capacity.

[0022] In a specific embodiment, the final temperature in (4) is 1100-1600°C.

[0023] By adopting the above technical solution, the temperature range can make the graphitization degree of the hard carbon negative electrode material so that the appropriate pseudo-graphite interlayer spacing is formed, which is conducive to the graphitization of hard carbon, reduces the pseudo-graphite interlayer spacing, and improves the low-voltage platform capacity and the first coulomb efficiency of hard carbon. However, if the temperature is too high, the interlayer spacing will be too small, which is not conducive to the intercalation and embedding of sodium ions, and the sodium storage capacity of hard carbon will decrease. If the temperature is too low, the degree of graphitization is small, which is not conducive to the stable embedding of sodium ions, affecting the capacity and the first coulomb efficiency of the hard carbon negative electrode material.

[0024] In a specific embodiment, the protective gas is at least one of argon and nitrogen, and the gas flow rate is 30-100 mL / min.

[0025] In summary, this application has the following beneficial effects: 1. Prepare hard carbon materials using biomass as a precursor. By pretreating cheap and readily available biomass materials, impurities can be effectively removed and the particle size range of the precursor powder can be controlled to improve the consistency of the performance of biomass-derived hard carbon materials. Then, by limiting the combined steps of the precursor pretreatment, the organic matter in the biomass material reacts to produce a large amount of coal tar and other impurities. The pre-oxidation treatment can introduce oxygen-containing functional groups and other components into the biomass material, so that the pore structure and chemical environment are changed, and the basis for forming a material with rich pseudo-graphite layer microcrystalline domains and amorphous non-crystalline domains is improved to form a hard carbon precursor. Then, by washing, the residual impurities are removed to improve the purity. Subsequently, the graphite phase g-C3N4 is added in proportion to stabilize the network. The g-C3N4-like structure can be used as a template to guide the graphitization of hard carbon under high-temperature calcination, forming pseudo-graphite layers and expanding the interlayer spacing, while forming rich pores and reducing defects and impurity functional groups, thereby improving the degree of graphitization and further improving the sodium storage capacity of hard carbon. The stable structure is conducive to the free movement of sodium ions between layers and is more conducive to the embedding / ejection of sodium ions, making the hard carbon material have a higher energy density and enhanced rate performance. By adjusting the heating rate, the ratio of open and closed pores can be effectively controlled, thereby significantly improving the electrochemical properties of sodium ion hard carbon negative electrode materials. Too much graphite phase g-C3N4 will lead to excessive hardness of the material, poor modifiable processability, and a relatively concentrated pore size distribution range, which is not conducive to the migration and diffusion of sodium ions and affects the reversible embedding / ejection of sodium ions.

[0026] 2. The pseudo-graphite layer is formed by high-temperature calcination. In addition to the crystal domain, it also contains amorphous domains, and is accompanied by rich edges, defects and pores, and contains a large number of saturated carbon-carbon bonds, aromatic rings or their combinations. Therefore, the microcrystalline domain area with high arrangement and molecular order can be surrounded by the less arranged and looser amorphous non-crystalline domain area, so that the pseudo-graphite layer of the negative electrode material of the sodium ion battery presents short-range order and long-range disorder, and there are a large number of micropores, further optimizing the internal pore size and improving the modifiability of the pores, thereby regulating and improving the composition and structure of the derived hard carbon, increasing the sodium storage capacity of the hard carbon, and increasing the disorder of the hard carbon, improving the reversible sodium storage capacity, reducing the irreversible adsorption of sodium ions, making the sodium ions penetrate and escape faster, and significantly improving the electrochemical performance.

[0027] 3. For the cellulose and lignin in sunflower seed shells, low-temperature pre-oxidation is first used to break the hydrogen bonds in the molecules, thereby forming short carbon rings, which are the basis for the material to have advantages such as high specific surface area and pore structure, and enhance the sodium ion energy storage. In this process, hydrogen peroxide solution is added, and the cellulose in the sunflower seed shells is oxidized, making the hydrothermal oxidation reaction more thorough, with higher oxygen content, forming more sodium storage sites, and enhancing the sodium storage performance. In addition, oxygen-containing functional groups can make the graphite phase g-C3N4 produce more electron holes, optimizing and adjusting the precursor structure, improve the sodium storage capacity of hard carbon; and then remove impurities such as coal tar through subsequent low-temperature cracking to improve the thermal efficiency of carbonization and product quality. The cracking temperature environment can regulate the structural morphology, crystal, amorphous structure, and carbon layer spacing of the obtained hard carbon material. If the temperature is too high, the hard carbon material will be over-carbonized, the pore size distribution of the hard carbon material will be too large, and the layer spacing will be expanded, which is not conducive to the embedding of sodium ions, thereby affecting the sodium storage performance. If the temperature is too low, the carbonization effect is poor, which affects the high-temperature calcination process, and the hard carbon sodium storage capacity of the hard carbon negative electrode material becomes smaller, thereby affecting its electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a scanning electron microscope (SEM) image of the hard carbon negative electrode material in Example 1 of the present invention; Figure 2 This is a transmission electron microscope (TEM) image of the hard carbon negative electrode material in Example 1 of the present invention; Figure 3 is the nitrogen adsorption-desorption curve in Example 1 of the present invention; Figure 4 is the pore size distribution curve of the hard carbon negative electrode material in Example 1 of the present invention; Figure 5 This is the first cycle charge and discharge curve of the hard carbon negative electrode material in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] The present application is further described in detail below with reference to the embodiments.

[0030] The raw materials used in the examples and comparative examples that are not otherwise specified are all conventional products that can be purchased from the market. Example

[0031] Example 1 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was first washed with 2wt% hydrochloric acid, and then immersed and washed with 5mol / L potassium hydroxide solution heated to 70°C. The solid-liquid ratio of the sample to the alkali solution was 1:15g / mL. Finally, it was washed with water 3 times and freeze-dried at -45°C for 9h. The dried sample and the graphite phase g-C3N4 were mixed evenly with a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon was introduced at a flow rate of 60mL / min, and the temperature was increased to a final temperature of 1400°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0032] Example 2 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was first washed with 2wt% hydrochloric acid, and then immersed and washed with 5mol / L potassium hydroxide solution heated to 70°C. The solid-liquid ratio of the sample to the alkali solution was 1:15g / mL. Finally, it was washed with water 3 times and freeze-dried at -45°C for 9h. The dried sample was mixed with the graphite phase g-C3N4 in a mass ratio of 1:1, and then placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon was introduced at a flow rate of 60mL / min, and the temperature was increased to a final temperature of 1600°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0033] Example 3 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was first washed with 2wt% hydrochloric acid, and then immersed and washed with 5mol / L potassium hydroxide solution heated to 70°C. The solid-liquid ratio of the sample to the alkali solution was 1:15g / mL. Finally, it was washed with water 3 times and freeze-dried at -45°C for 9h. The dried sample and the graphite phase g-C3N4 were mixed evenly with a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon was introduced at a flow rate of 60mL / min, and the temperature was increased to a final temperature of 1000°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0034] Example 4 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was first washed with 2wt% hydrochloric acid, and then immersed and washed with 5mol / L potassium hydroxide solution heated to 70°C. The solid-liquid ratio of the sample to the alkali solution was 1:15g / mL. Finally, it was washed with water 3 times and freeze-dried at -45°C for 9h. The dried sample and the graphite phase g-C3N4 were mixed evenly with a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon was introduced at a flow rate of 60mL / min, and the temperature was increased to a final temperature of 1800°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0035] Example 5 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was first washed with 2wt% hydrochloric acid, and then immersed and washed with 5mol / L potassium hydroxide solution heated to 70°C. The solid-liquid ratio of the sample to the alkali solution was 1:15g / mL. Finally, it was washed with water 3 times and freeze-dried at -45°C for 9h. The dried sample and the graphite phase g-C3N4 were mixed evenly with a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon was introduced at a flow rate of 60mL / min, and the temperature was increased to a final temperature of 1100°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0036] Example 6 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed, and sieved to obtain a precursor powder; the precursor powder is placed in a muffle furnace for low-temperature pre-oxidation treatment, and the temperature is increased to the final temperature at a heating rate of 5°C / min under a final temperature condition of 300°C, and after constant temperature reaction for 2h, the temperature is cooled to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor; the hard carbon precursor is first washed with 2wt% hydrochloric acid, and then heated to 7 with a potassium hydroxide solution with a concentration of 5mol / L The sample was soaked and cleaned at 0℃, the solid-liquid ratio of the sample to the alkali solution was 1:15g / mL, and finally washed with water for 3 times. After freeze-drying at -45℃ for 9h, the dried sample and graphite phase g-C3N4 were mixed evenly with a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination. Argon gas was introduced at a flow rate of 60mL / min as protective gas, and the temperature was increased to a final temperature of 1400℃ at a heating rate of 5℃ / min. After constant temperature reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5℃ / min, washed with 2wt% hydrochloric acid, and dried at 60℃ to obtain a hard carbon negative electrode material for sodium ion batteries.

[0037] Example 7 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed, and sieved to obtain a precursor powder; then a 2wt% hydrogen peroxide solution is added, and 5g of the precursor powder is dispersed per 100ml of the hydrogen peroxide solution, and the precursor powder is placed in a hydrothermal reactor in a constant temperature box for hydrothermal pre-oxidation treatment, and the temperature is 100°C, and the constant temperature hydrothermal reaction is performed for 24h, and the hard carbon precursor is first washed with 2wt% hydrochloric acid, and then heated to 70 with a potassium hydroxide solution with a concentration of 5mol / L ℃ soaking and cleaning, the solid-liquid ratio of the sample to the alkali solution is 1:15g / mL, and finally washed with water for 3 times. After freeze-drying at -45℃ for 9h, the dried sample and graphite phase g-C3N4 are mixed evenly with a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination. Argon gas with a flow rate of 60mL / min is introduced, and the temperature is increased to a final temperature of 1400℃ at a heating rate of 5℃ / min. After isothermal reaction for 2h, the temperature is cooled to room temperature at a cooling rate of 5℃ / min, washed with 2wt% hydrochloric acid, and dried at 60℃ to obtain a hard carbon negative electrode material for sodium ion batteries.

[0038] Example 8 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed, and sieved to obtain a precursor powder; then a 2wt% hydrogen peroxide solution is added, and 5g of the precursor powder is dispersed per 100ml of hydrogen peroxide solution and placed in a hydrothermal reactor in a constant temperature box for hydrothermal pre-oxidation treatment. After a constant temperature hydrothermal reaction of 24h at a temperature of 100°C, the precursor powder is placed in a tubular furnace for low-temperature cracking treatment, and a protective gas argon gas with a flow rate of 60mL / min is introduced, and the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking. After a constant temperature reaction of 2h, the precursor powder is cooled to room temperature at a cooling rate of 5°C / min. temperature to obtain a hard carbon precursor; the hard carbon precursor is first washed with 2wt% hydrochloric acid, and then immersed and washed with a 5mol / L potassium hydroxide solution heated to 70°C, the solid-liquid ratio of the sample to the alkali solution is 1:15g / mL, and finally washed with water 3 times, freeze-dried at a temperature of -45°C for 9h, and the dried sample and the graphite phase g-C3N4 are mixed evenly with a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination, and a protective gas argon gas is introduced with a flow rate of 60mL / min, and the temperature is increased to a final temperature of 1400°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature is cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for a sodium ion battery.

[0039] Example 9 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed, and sieved to obtain a precursor powder; the precursor powder is placed in a hydrothermal reactor in a constant temperature box for hydrothermal pre-oxidation treatment at a temperature of 100°C for a constant temperature time of 24h, and cooled to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor; the hard carbon precursor is first washed with 2wt% hydrochloric acid, and then heated to 70°C in a potassium hydroxide solution with a concentration of 5mol / L for soaking and washing. The solid-liquid ratio of the sample to the alkali solution is 1:15g / mL. Finally, it is washed with water 3 times and freeze-dried at -45°C for 9h. Then, the dried sample and graphite phase g-C3N4 are mixed evenly in a mass ratio of 1:3 and placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon is introduced at a flow rate of 60mL / min, and the temperature is increased to a final temperature of 1400°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature is cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0040] Example 10 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was washed with deionized water several times and dried in a vacuum oven for 12 hours. The dried sample and graphite phase g-C3N4 were mixed evenly in a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination. Argon gas was introduced at a flow rate of 60 mL / min as protective gas, and the temperature was increased to a final temperature of 1400°C at a heating rate of 5°C / min. After constant temperature reaction for 2 hours, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0041] Comparative Example Comparative Example 1 A low-cost and high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder and the graphite phase g-C3N4 are evenly mixed in a mass ratio of 1:3, and then placed in a high-temperature tube furnace for high-temperature calcination, and a protective gas argon gas is introduced with a flow rate of 60 mL / min, and the temperature is increased to a final temperature of 1400°C at a heating rate of 5°C / min. After isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min, and the mixture is washed with 2wt% hydrochloric acid and dried at 60°C to obtain a sodium ion battery hard carbon negative electrode material.

[0042] Comparative Example 2 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was first washed with 2wt% hydrochloric acid, and then soaked and washed with 5mol / L potassium hydroxide solution heated to 70°C. The solid-liquid ratio of the sample to the alkali solution was 1:15g / mL. Finally, it was washed with water 3 times and freeze-dried at -45°C for 9h. The dried sample and the graphite phase g-C3N4 were mixed evenly with a mass ratio of 1:4, and then placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon was introduced at a flow rate of 60mL / min, and the temperature was increased to a final temperature of 1400°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0043] Comparative Example 3 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was first washed with 2wt% hydrochloric acid, and then immersed and washed with 5mol / L potassium hydroxide solution heated to 70°C. The solid-liquid ratio of the sample to the alkali solution was 1:15g / mL. Finally, it was washed with water 3 times and freeze-dried at -45°C for 9h. The dried sample was placed in a high-temperature tubular furnace for high-temperature calcination. Argon gas was introduced at a flow rate of 60mL / min as a protective gas. The temperature was increased to a final temperature of 1400°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for a sodium ion battery.

[0044] Comparative Example 4 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor and the graphite phase g-C3N4 were mixed evenly in a mass ratio of 1:3, and then placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon was introduced at a flow rate of 60 mL / min, and the temperature was increased to a final temperature of 1400°C at a heating rate of 5°C / min. After constant temperature reaction for 2 hours, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0045] Comparative Example 5 A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material is prepared according to the following steps: the biomass material is washed, dried, crushed and sieved to obtain a precursor powder; the precursor powder is placed in a tubular furnace for low-temperature cracking pretreatment, a protective gas argon gas with a flow rate of 60 mL / min is introduced, the temperature is increased to a final temperature of 650°C at a heating rate of 5°C / min for low-temperature cracking, after isothermal reaction for 2 hours, the temperature is reduced to room temperature at a cooling rate of 5°C / min to obtain a hard carbon precursor. The hard carbon precursor was first washed with 2wt% hydrochloric acid, and then immersed and washed with 5mol / L potassium hydroxide solution heated to 70°C. The solid-liquid ratio of the sample to the alkali solution was 1:15g / mL. Finally, it was washed with water 3 times and freeze-dried at -45°C for 9h. The dried sample and the graphite phase g-C3N4 were mixed evenly with a mass ratio of 2:1, and then placed in a high-temperature tubular furnace for high-temperature calcination. The protective gas argon was introduced at a flow rate of 60mL / min, and the temperature was increased to a final temperature of 1400°C at a heating rate of 5°C / min. After isothermal reaction for 2h, the temperature was cooled to room temperature at a cooling rate of 5°C / min, washed with 2wt% hydrochloric acid, and dried at 60°C to obtain a hard carbon negative electrode material for sodium ion batteries.

[0046] Performance Testing The physical and chemical performance test technical indicators of a low-cost and high-performance biomass-based sodium ion hard carbon negative electrode material prepared in the embodiment and comparative example are measured by the following method: a. Specific surface area and pore size analysis: The N2 isothermal adsorption-desorption curve was measured using the BEL-SorpMaxII specific surface and vapor adsorption analyzer produced by MicrotracBEL of Japan. Before the adsorption test, the sample was activated as required, and the specific surface area was calculated by Brunauer-EmmettTeller (BET) in the relative pressure range of 0.05 to 0.20, and the pore volume of the material was calculated based on the adsorption amount when the relative pressure was about 0.99.

[0047] b. Electrical performance test: The test was conducted by a half-cell test method, specifically: the hard carbon negative electrode material of the above embodiment and comparative example: sodium alginate: Super-p = 90:5:5 (weight ratio), water was added to adjust the slurry, coated on aluminum foil and dried in a vacuum drying oven for 12 hours to form a negative electrode sheet, 1 mol of NaPF6 was dissolved in 1L of ethylene carbonate and diethyl carbonate solution with a volume ratio of 1:1 as the electrolyte, a polypropylene microporous membrane was used as the diaphragm, and the counter electrode was a sodium sheet, and assembled into a battery. A constant current charge and discharge experiment was conducted in the LAND battery test system, and the charge and discharge voltage was limited to 0.01-2.0V. The results are shown in Table 1: Table 1 Performance test results As can be seen from Table 1, the low-cost and high-performance biomass-based sodium ion hard carbon negative electrode material obtained in the above embodiment has a large pore size distribution range and porosity, a particle size of 1-10 μm and a typical granular morphology, and a relatively large specific surface area (110 m 2 / g or more), has good sodium storage performance, higher reversible specific capacity and first coulombic efficiency, and shows excellent reversible sodium storage capacity. While reducing the cost, it does not lead to a decrease in the performance of the graphite negative electrode material, and can still maintain the excellent performance of the hard carbon negative electrode material, which is conducive to promotion and application.

[0048] By comparing Example 1 with Examples 6-8 and Comparative Example 1, it can be seen that the specific surface area, reversible specific capacity, low potential platform specific capacity and first coulombic efficiency of the low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material prepared in Comparative Example 1 are all lower than those in Examples 6-8. Comparative analysis shows that, in view of the relatively large amount of cellulose and lignin in sunflower seed shells, a two-stage pretreatment and high-temperature calcination are adopted. First, low-temperature pre-oxidation is performed to break the intramolecular hydrogen bonds, thereby forming a short carbon ring, which is the basis for the material to have the advantages of high specific surface area and pore structure, and to enhance the sodium ion energy storage. In this process, a hydrogen peroxide solution is added, and the cellulose in the sunflower seed shells is oxidized, making the hydrothermal oxidation reaction more thorough, the oxygen content is higher, and more sodium storage sites are formed, thereby enhancing the sodium storage performance. Subsequently, impurities such as coal tar are removed by low-temperature pyrolysis, the thermal efficiency and product quality of carbonization are improved, the edges, defects and pores of pseudo-graphite microcrystalline domains and amorphous nanodomains are optimized, the hard carbon sodium storage capacity is improved, the pseudo-graphite interlayer spacing is regulated, and the electrochemical properties such as the hard carbon sodium storage capacity of the hard carbon negative electrode material are improved.

[0049] By comparing Example 1 with Comparative Examples 2-3 and Comparative Example 5, it can be seen that: by adding graphite phase g-C3N4 in proportion, the stable network structure can be used as a template to guide the graphitization of hard carbon under high-temperature calcination, forming a pseudo-graphite layer and expanding the interlayer spacing, while forming rich pores and reducing defects and impurity functional groups, thereby improving the degree of graphitization, and further improving the sodium storage capacity of hard carbon. The stable structure is conducive to the free movement of sodium ions between layers, and is more conducive to the embedding / ejection of sodium ions, making the energy density of the hard carbon material higher and enhancing the rate performance; adjusting the heating rate can effectively control the opening of the pores. and closed-pore ratio, thereby significantly improving the electrochemical properties of the sodium ion hard carbon negative electrode material. The electrochemical performance of the material within the mass ratio range of the treated sample and the graphite phase g-C3N4 of the present application is optimal. This may be because too little graphite phase g-C3N4 cannot fully guide the calcination and provide a stable network structure, which is not conducive to the embedding / ejection of sodium ions. Too much graphite phase g-C3N4 will lead to excessive hardness of the material, poor modifiable processability, and a relatively concentrated pore size distribution range, which is not conducive to the migration and diffusion of sodium ions and affects the reversible embedding / ejection of sodium ions.

[0050] Comparison of Examples 1-5 shows that the specific surface area, reversible specific capacity, low potential platform specific capacity and first coulombic efficiency of the low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material obtained in Examples 3-4 are all lower than those in Examples 1-2 and 5. Comparative analysis shows that the temperature range disclosed in this application can increase the degree of graphitization of the hard carbon negative electrode material, so that an appropriate pseudo-graphite interlayer spacing is formed, which is beneficial to the graphitization of hard carbon, reduces the pseudo-graphite interlayer spacing, and improves the low voltage platform capacity and first coulombic efficiency of hard carbon. Too high a temperature will make the interlayer spacing too small, which is not conducive to the intercalation and embedding of sodium ions, and the sodium storage capacity of hard carbon will decrease. If the temperature is too low, the degree of graphitization is small, which is not conducive to the stable embedding of sodium ions, and affects the capacity and first coulombic efficiency of the hard carbon negative electrode material.

[0051] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material, characterized by: The preparation method of the hard carbon negative electrode material comprises: (1) Biomass pretreatment: washing, drying, crushing and screening the biomass materials to obtain precursor powder; (2) Precursor pretreatment: pretreating the precursor powder obtained in (1), wherein the pretreatment includes one or more combined treatments of low-temperature pyrolysis, low-temperature pre-oxidation and hydrothermal pre-oxidation to obtain a hard carbon precursor; (3) Cleaning and purification: Cleaning and drying the samples after the above pretreatment; (4) High temperature calcination: the sample treated in (3) and the graphite phase g-C3N4 are mixed uniformly at a mass ratio of 1:(1-3), and then a protective gas is introduced. The temperature is raised to the final temperature at a rate of 0.5-10°C / min, and the reaction is kept at a constant temperature for 0.5-8h, and then the temperature is lowered to room temperature at a rate of 0.1-10°C / min; (5) Acid washing and drying: The above samples are acid washed and dried to obtain hard carbon negative electrode materials.

2. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 1, characterized in that: The hard carbon negative electrode material is an active negative electrode material having a large number of pseudo-graphite microcrystalline domains and amorphous non-crystalline domains.

3. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 1, characterized in that: The biomass material in (1) is sunflower seed husk.

4. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 1, characterized in that: The hydrothermal pre-oxidation in (2) is to add 0.5-5wt% hydrogen peroxide solution, disperse (5-8)g of precursor powder per 100ml hydrogen peroxide solution, and perform constant temperature hydrothermal reaction at 100-200°C for 12-24h.

5. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 1, characterized in that: The low temperature cracking in (2) is to heat the mixture to 500-800°C at a rate of 0.5-10°C / min under a protective atmosphere, react at a constant temperature for 0.5-8h, and then cool the mixture to room temperature at a rate of 0.1-10°C / min.

6. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 5, characterized in that: The protective atmosphere is at least one of argon and nitrogen, and the gas flow rate is 10-100 mL / min.

7. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 1, characterized in that: The cleaning in (3) includes one or more of acid cleaning, 60-80°C alkaline solution immersion cleaning and water cleaning.

8. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 1, characterized in that: The low temperature pre-oxidation in (2) is to heat up to 200-300°C at a rate of 0.5-10°C / min, react at a constant temperature for 0.5-8h, and then cool to room temperature at a rate of 0.1-10°C / min.

9. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 1, characterized in that: The final temperature in (4) is 1100-1600°C.

10. The low-cost, high-performance biomass-based sodium ion hard carbon negative electrode material according to claim 1, characterized in that: The protective gas is at least one of argon and nitrogen, and the gas flow rate is 30-100 mL / min.

Citation Information

Patent Citations

  • Biomass hard carbon prepared by adopting tobacco stems and preparation method thereof

    CN110137444A

  • High-performance lamellar hard carbon and preparation method thereof

    CN116102000A

  • Preparation method and application of hard carbon negative electrode material for sodium ion battery

    CN116873898A

  • Preparation method of high-rate modified biomass hard carbon material

    CN117383540A

  • Biomass hard carbon material as well as two-stage carbonization preparation method and application thereof

    CN117735525A

Cited By

  • Preparation method of sodium-ion battery negative electrode material with high capacity and high first effect

    CN119551660A

  • Durian shell biological hard carbon material for negative electrode of sodium ion battery and preparation method of durian shell biological hard carbon material

    CN119569035A

  • A durian shell bio-hard carbon material for sodium ion battery negative electrode and its preparation method

    CN119569035B

  • Preparation method and application of heteroatom coordination modified biomass-based hard carbon material

    CN119898748A

  • Easily-prepared, economic and environment-friendly high-performance sodium ion secondary battery negative electrode material

    CN119929794A