Anode layer, method for producing anode layer, and all-solid-state battery
The use of a negative electrode layer with lithium titanate, sulfide solid electrolyte, and a controlled rubber binder adsorption ratio addresses the resistance issue in all-solid-state batteries, enhancing their efficiency.
Patent Information
- Application Number
- JP2021212462
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-12-27
AI Technical Summary
All-solid-state batteries require a negative electrode layer with low resistance to enhance input and output efficiency.
A negative electrode layer comprising lithium titanate, a sulfide solid electrolyte, and a rubber-based binder, with a specific adsorption ratio of the rubber binder on lithium titanate of 1.35% or less, is used to minimize binder adsorption and reduce resistance.
The solution results in a negative electrode layer with reduced resistance, improving the performance of all-solid-state batteries.
Smart Images

Figure 0007590317000002 
Figure 0007590317000003 
Figure 0007590317000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a negative electrode layer, a method for producing the negative electrode layer, and an all-solid-state battery. [Background technology]
[0002] An all-solid-state battery is a battery that has a solid electrolyte layer between a positive electrode layer and a negative electrode layer, and has the advantage that it is easier to simplify safety devices compared to liquid batteries that have an electrolyte solution containing a flammable organic solvent.
[0003] Titanium oxide is known as an anode active material used in all-solid-state batteries. Titanium oxide has a small volume change associated with charging and discharging. For example, Patent Document 1 discloses an anode for all-solid-state batteries including an anode active material layer, the anode active material layer including a first particle group made of titanium oxide and a second particle group made of a sulfide solid electrolyte, and the contact interface length between the first particle group and the second particle group in the cross section of the anode active material layer is 3.77 mm or more. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-128885 Summary of the Invention [Problem to be solved by the invention]
[0005] In order to increase the input / output of all-solid-state batteries, a negative electrode layer with low resistance is required. The present disclosure has been made in view of the above problems, and has as its main object to provide a negative electrode layer with low resistance. [Means for solving the problem]
[0006] In order to solve the above problems, the present disclosure provides a negative electrode layer for use in an all-solid-state battery, the negative electrode layer including lithium titanate, a sulfide solid electrolyte, and a rubber-based binder, and a ratio (A / B) of an adsorption amount A of the rubber-based binder adsorbed to the lithium titanate to a total content B of the rubber-based binder included in the negative electrode layer is 1.35% or less.
[0007] According to the present disclosure, the ratio of the rubber-based binder adsorbed to lithium titanate to the total content of the rubber-based binder contained in the negative electrode layer is equal to or less than a predetermined value, resulting in a negative electrode layer with low resistance.
[0008] In the above disclosure, the rubber-based binder may include styrene-butadiene rubber.
[0009] The present disclosure also provides a method for producing an anode layer used in an all-solid-state battery, the method including: a dispersion preparation step of preparing a dispersion in which a sulfide solid electrolyte and a first component are dispersed in a dispersion medium; an addition step of adding and dispersing a second component in the dispersion to obtain an anode paste; and an anode layer formation step of applying and drying the anode paste to form an anode layer, wherein one of the first component and the second component is lithium titanate, and the other is a rubber-based binder.
[0010] According to the present disclosure, there is provided a dispersion preparation step of preparing a dispersion in which at least a sulfide solid electrolyte is dispersed, and by separately adding a rubber-based binder and lithium titanate in the dispersion preparation step and the subsequent addition step, the rubber-based binder is preferentially adsorbed to the sulfide solid electrolyte, thereby making it possible to produce a negative electrode layer with low resistance.
[0011] The present disclosure also provides an all-solid-state battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the negative electrode layer is the above-mentioned negative electrode layer.
[0012] According to the present disclosure, by using the above-mentioned negative electrode layer, an all-solid-state battery with low resistance is obtained. Effect of the Invention
[0013] The present disclosure has an effect of providing a negative electrode layer having low resistance. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a flow diagram showing an example of a method for producing a negative electrode layer in the present disclosure. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of an all-solid-state battery according to the present disclosure. [Diagram 3] FIG. 4 is a flow diagram showing an example of a method for manufacturing a negative electrode layer according to a comparative example. [Figure 4] 3 shows an SEM image and an element mapping image of a cross section of a negative electrode layer in an evaluation battery obtained in an example. [Diagram 5] FIG. 2 is an image processing process diagram for extracting a binder adsorbed to lithium titanate in the negative electrode layer of the evaluation battery obtained in the example. [Figure 6] 1 shows an SEM image, an element mapping image, and an extracted image of a binder adsorbed to lithium titanate of a cross section of a negative electrode layer in evaluation batteries obtained in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The negative electrode layer, the method for producing the negative electrode layer, and the all-solid-state battery according to the present disclosure will be described in detail below.
[0016] A. Negative electrode layer The negative electrode layer in the present disclosure includes lithium titanate, a sulfide solid electrolyte, and a rubber-based binder, and the ratio (A / B) of the amount A of the rubber-based binder adsorbed to the lithium titanate to the total content B of the rubber-based binder contained in the negative electrode layer is 1.35% or less. The negative electrode layer in the present disclosure is used in an all-solid-state battery.
[0017] According to the present disclosure, the ratio of the rubber-based binder adsorbed to the lithium titanate to the total content of the rubber-based binder contained in the negative electrode layer is equal to or less than a predetermined value, resulting in a negative electrode layer with low resistance. As described above, in the case of a negative electrode layer containing lithium titanate and a rubber-based binder, the affinity between the lithium titanate and the rubber-based binder is high. Therefore, the rubber-based binder is easily adsorbed to the lithium titanate, and the surface of the lithium titanate is covered, thereby reducing the reactive area as an active material, which may result in high resistance.
[0018] For example, silicon-based particles are known as a negative electrode active material used in batteries. The affinity between the silicon-based particles and the rubber-based binder is lower than that between the lithium titanate and the rubber-based binder. Therefore, in the case of a negative electrode layer using silicon-based particles as the negative electrode active material, the binder is less likely to be adsorbed to the negative electrode active material, resulting in a high resistance problem.
[0019] In addition, fluoride-based binders such as polyvinylidene fluoride (PVDF) have low dispersibility in the dispersion medium used with the sulfide solid electrolyte, and therefore tend to aggregate in the negative electrode layer. Therefore, in the case of a negative electrode layer using a fluoride-based binder as the binder, there is a low possibility of the problem of high resistance occurring due to the binder being easily adsorbed to the negative electrode active material.
[0020] Thus, the problem of high resistance is particularly evident in a negative electrode layer that uses lithium titanate as the negative electrode active material and a rubber-based binder as the binder. In contrast, in the negative electrode layer of the present disclosure, the ratio of the rubber-based binder adsorbed to lithium titanate to the total content of the rubber-based binder contained in the negative electrode layer is equal to or less than a predetermined value, so that the decrease in the reaction area can be suppressed and the resistance of the negative electrode layer can be reduced.
[0021] 1. Rubber-based binder The negative electrode layer in the present disclosure has a rubber-based binder. In the present disclosure, the ratio (A / B) of the amount A of the rubber-based binder adsorbed to lithium titanate to the total content B of the rubber-based binder contained in the negative electrode layer is usually 1.35% or less, and may be 1.0% or less. If the ratio is large, the reaction area of lithium titanate decreases, resulting in high resistance. On the other hand, the ratio is, for example, 0% or more, and may be 0.5% or more. The ratio (A / B) is measured by the following procedure.
[0022] (Electrode staining) In an inert atmosphere such as a glove box, at least a part of the exterior body of the all-solid-state battery is peeled off to expose the power generating element. In the exposed state, the power generating element is set in a chamber not exposed to the atmosphere and transferred to a vacuum electron staining device. As the vacuum electron staining device, for example, a VSC4TWDH (manufactured by Filgen Co., Ltd.) is used. After creating a vacuum atmosphere inside the vacuum electron staining device, the chamber is opened and osmium tetroxide (OsO 4 ) gas is introduced, and the staining time and gas concentration are adjusted to perform osmium (Os) staining. 4 ) reacts with the double bonds of the rubber binder and is adsorbed to the rubber binder.
[0023] (Preparation of test specimens) The osmium-stained power generation element is cut to an appropriate size in an inert atmosphere. This produces a test piece of the power generation element. Using a milling holder that is not exposed to the atmosphere, the cut surface of the sample piece is cross-sectionally processed by an ion milling device. For example, an ion milling device "IM4000PLUS" (or an equivalent product) manufactured by Hitachi High-Technologies Corporation may be used. The cross-sectional processing is performed in a vacuum atmosphere or an inert atmosphere. The sample piece may be cooled during the cross-sectional processing.
[0024] (Image Acquisition) After cross-section processing, the sample piece is introduced into a field emission scanning electron microscope (FE-SEM). For example, a Hitachi High-Technologies Corporation FE-SEM "Regulus8230" (or an equivalent product) may be used. A vacuum atmosphere is maintained between cross-section processing and introduction into the SEM so that the sample piece is not exposed to the atmosphere.
[0025] The cross section of the negative electrode layer of the sample piece is observed by FE-SEM. It is preferable to select a position where the conductive material is not observed as the observation position. This is because the total content B of the rubber-based binder can be accurately calculated. At the observation position, a secondary electron image and a backscattered electron image are observed by SEM. The observation magnification is, for example, 5000 times. At the same observation position, a mapping image of carbon (C), a mapping image of sulfur (S), and further a mapping image of sulfur (S) and osmium (Os) are obtained by EDX (energy dispersive x-ray spectroscopy). The above observation is preferably performed at a plurality of positions. In this case, for example, six observation positions are set at approximately equal intervals in a planar direction parallel to the negative electrode current collector (i.e., a direction perpendicular to the thickness direction of the negative electrode layer).
[0026] (Image analysis) Using the images obtained above, (1) the total rubber binder content B, and (2) the adsorption amount A of the rubber binder adsorbed on the lithium titanate are measured.
[0027] (1) Measurement of total rubber binder content B First, the carbon mapping image is subjected to binarization processing, and the pixel number P1 of the extracted image of the C element is counted. The carbon mapping image is literally an image in which the presence of carbon is mapped, and corresponds to a simple image in terms of image processing, so that the pixel number P1 can be counted with high accuracy by a known binarization processing. The binarization threshold is preferably set in consideration of at least one of the volume ratio of lithium titanate, the volume ratio of the conductive material, and the volume ratio of the rubber-based binder, for example.
[0028] Next, the mapping image of sulfur is subjected to binarization processing, and the number of pixels P2 of the extracted image of the S element is counted. The mapping image of sulfur is literally an image in which the presence of sulfur is mapped, and corresponds to a simple image in terms of image processing, so that the number of pixels P2 can be counted with high accuracy by known binarization processing. The threshold value for binarization is preferably set in consideration of at least one of the volume ratio of lithium titanate and the volume ratio of the sulfide solid electrolyte, for example.
[0029] Next, the number of pixels P3 is calculated by subtracting the above P2 from the above P1. In this disclosure, the above P3 is defined as the total content B of the rubber-based binder. In addition to the shape of the sulfide solid electrolyte, the shape of lithium titanate is also observed in the carbon mapping image, but this is due to the surface functional groups of lithium titanate and solvent residues, both of which are small in amount. Therefore, the above P3 can be defined as the total content B of the rubber-based binder.
[0030] (2) Measurement of the amount A of rubber binder adsorbed on lithium titanate The mapping images of osmium (Os) and sulfur (S) are separated into areas where Os elements and S elements are present and other areas. Next, by removing the large areas (S elements in the sulfide solid electrolyte and Os elements covering the S elements in the sulfide solid electrolyte), the remaining Os elements, i.e., Os elements adsorbed on the lithium titanate, are extracted. The number of pixels P4 of the extracted Os element image is counted.
[0031] The ratio is calculated by dividing the number of pixels P4 obtained in (2) above by the number of pixels P3 obtained in (1) above and expressing the result as a percentage ((P4 / P3) x 100(%)). If observations are made at multiple positions (e.g., six positions), ((P4 / P3) x 100(%)) is calculated at each observation position, and the average of these is taken as the ratio (A / B).
[0032] (Rubber-based binder) As the rubber-based binder in the present disclosure, any known rubber-based binder that is used as a binder for an all-solid-state battery can be used. Examples of rubbers contained in the rubber-based binder include butadiene rubber, hydrogenated butadiene rubber, styrene butadiene rubber (SBR), hydrogenated styrene butadiene rubber, nitrile butadiene rubber, hydrogenated nitrile butadiene rubber, and ethylene propylene rubber. Among them, styrene butadiene rubber (SBR) is preferable.
[0033] The proportion of the rubber-based binder in the negative electrode layer is, for example, 1 vol% or more and 20 vol% or less, and may be 5 vol% or more and 20 vol% or less.
[0034] 2. Lithium titanate The negative electrode layer in the present disclosure contains lithium titanate, which functions as a negative electrode layer active material.
[0035] Lithium titanate (LTO) is a compound containing Li, Ti, and O. A part of Ti in lithium titanate may be replaced with another metal element (e.g., a transition metal element). A part of Li in lithium titanate may be replaced with another metal element (e.g., an alkali metal element). Lithium titanate may have a crystal phase with a spinel structure.
[0036] The composition of lithium titanate is, for example, Li x Ti y O z(3.5≦x≦4.5, 4.5≦y≦5.5, 11≦z≦13). x may be 3.7 or more and 4.3 or less, or 3.9 or more and 4.1 or less. y may be 4.7 or more and 5.3 or less, or 4.9 or more and 5.1 or less. z may be 11.5 or more and 12.5 or less, or 11.7 or more and 12.3 or less. Lithium titanate is Li 4 Ti 5 O 12 It is preferable that the composition is represented by the following formula:
[0037] The shape of lithium titanate may be, for example, particulate. The average particle diameter (D 50 ) is, for example, 10 nm or more and 50 μm or less, and may be 100 nm or more and 20 μm or less. 50 ) refers to the particle size (median diameter) at the cumulative 50% of the cumulative particle size distribution, and is calculated, for example, from measurements using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).
[0038] The specific surface area of lithium titanate is, for example, 2 m 2 / g or more, 10m 2 / g or less, and 2 / g or more, 8m 2 / g or less, and 2 / g or more, 6.5m 2 The specific surface area may be calculated, for example, from a measurement using a gas adsorption method such as the BET method.
[0039] Lithium titanate preferably exhibits good electronic conductivity by inserting Li. The electronic conductivity (25° C.) of lithium titanate in the Li-inserted state is, for example, 8.0×10 -1 S / cm or more.
[0040] The ratio of lithium titanate in the negative electrode layer is, for example, 20% by volume or more and 80% by volume or less, or may be 30% by volume or more and 70% by volume or less, or 40% by volume or more and 65% by volume or less. If the ratio of lithium titanate is low, the volumetric energy density may be low. On the other hand, if the ratio of lithium titanate is high, the ion conduction path may not be sufficiently formed.
[0041] 3.Sulfide solid electrolyte The negative electrode layer in the present disclosure contains a sulfide solid electrolyte. The sulfide solid electrolyte constitutes an ion conduction path in the negative electrode layer. The sulfide solid electrolyte usually contains sulfur (S) as a main component of an anion element. The sulfide solid electrolyte contains, for example, Li, A (A is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. It is preferable that A contains at least P, and the sulfide solid electrolyte may contain at least one of Cl, Br, and I as a halogen. The sulfide solid electrolyte may also contain O.
[0042] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte, a glass ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. In addition, when the sulfide solid electrolyte has a crystalline phase, examples of the crystalline phase include a Thio-LISICON type crystalline phase, a LGPS type crystalline phase, and an Argyrodite type crystalline phase.
[0043] The composition of the sulfide solid electrolyte is not particularly limited, but may be, for example, xLi 2 S·(100-x)P 2 S 5 (70≦x≦80), yLiI・zLiBr・(100-yz)(xLi 2 S (1-x)P 2 S 5 ) (0.7≦x≦0.8, 0≦y≦30, 0≦z≦30).
[0044] The sulfide solid electrolyte has the general formula: Li 4-x Ge 1-xP x S 4 It may have a composition represented by (0 < x < 1). In the above general formula, at least a part of Ge may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a part of P may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, a part of Li may be substituted with at least one of Na, K, Mg, Ca, and Zn. In the above general formula, a part of S may be substituted with a halogen (at least one of F, Cl, Br, and I).
[0045] As other compositions of the sulfide solid electrolyte, for example, Li 7-x-2y PS 6-x-y X y , Li 8-x-2y SiS 6-x-y X y , Li 8-x-2y GeS 6-x-y X y may be mentioned. In these compositions, X is at least one of F, Cl, Br, and I, and x and y satisfy 0 ≤ x, 0 ≤ y.
[0046] The sulfide solid electrolyte preferably has a high Li-ion conductivity. The Li-ion conductivity of the sulfide solid electrolyte at 25°C is, for example, 1×10 -4 S / cm or more, and preferably 1×10 -3 S / cm or more. The sulfide solid electrolyte preferably has high insulation. The electron conductivity of the sulfide solid electrolyte at 25°C is, for example, 10 -6 S / cm or less, may be 10 -8 S / cm or less, and may be 10 -10 S / cm or less. Further, as the shape of the sulfide solid electrolyte, for example, particulate form may be mentioned. The average particle diameter (D 50 ) of the sulfide solid electrolyte is, for example, 0.1 μm or more and 50 μm or less.
[0047] The proportion of the sulfide solid electrolyte in the negative electrode layer is, for example, 15% by volume or more and 75% by volume or less, and may be 15% by volume or more and 60% by volume or less. If the proportion of the sulfide solid electrolyte is low, there is a possibility that the ion conduction path is not sufficiently formed. On the other hand, if the proportion of the sulfide solid electrolyte is high, there is a possibility that the volumetric energy density is low.
[0048] 4. Negative electrode layer The negative electrode layer in the present disclosure may or may not contain a conductive material. In the present disclosure, the "conductive material" refers to a material having a higher electronic conductivity than that of lithium titanate (strictly speaking, the electronic conductivity of lithium titanate in a state in which Li is inserted). Examples of the conductive material include carbon materials, metal particles, and conductive polymers. Examples of the carbon material include particulate carbon materials such as acetylene black (AB) and ketjen black (KB), and fibrous carbon materials such as carbon fibers, carbon nanotubes (CNT), and carbon nanofibers (CNF). The proportion of the conductive material in the negative electrode layer is, for example, 0.1% by volume or more and 10% by volume or less, and may be 0.3% by volume or more and 10% by volume or less. On the other hand, when the negative electrode layer does not contain a conductive material, it is preferable that the material having the highest electronic conductivity in the negative electrode layer is lithium titanate.
[0049] The thickness of the negative electrode layer is, for example, not less than 0.1 μm and not more than 1000 μm.
[0050] B. Method of manufacturing the negative electrode layer FIG. 1 is a flow diagram showing an example of a method for producing a negative electrode layer in the present disclosure. In the production method shown in FIG. 1, first, a dispersion in which a sulfide solid electrolyte and a first component are dispersed in a dispersion medium is prepared (dispersion preparation step). Next, a second component is added to the dispersion and dispersed to obtain a negative electrode paste (addition step). Here, one of the first component and the second component is lithium titanate, and the other is a rubber-based binder. Next, the negative electrode paste is applied and dried to form a negative electrode layer (negative electrode layer formation step).
[0051] The affinity of the rubber-based binder for the sulfide solid electrolyte is slightly higher than that of the rubber-based binder for lithium titanate, but is approximately the same. Therefore, when lithium titanate comes into contact with the rubber-based binder in the absence of the sulfide solid electrolyte during the manufacturing process of the negative electrode paste, the amount of the rubber-based binder adsorbed to the lithium titanate increases.
[0052] On the other hand, the method for producing the negative electrode layer in the present disclosure includes a dispersion preparation step of preparing a dispersion in which at least a sulfide solid electrolyte is dispersed, and in the dispersion preparation step and the subsequent addition step, the rubber-based binder is added separately from the lithium titanate, so that the rubber-based binder preferentially coats the sulfide solid electrolyte, thereby reducing the amount of the rubber-based binder that covers the lithium titanate.
[0053] In the present disclosure, it is preferable that the first component is lithium titanate and the second component is a rubber-based binder. Also, the first component may be a rubber-based binder and the second component may be lithium titanate.
[0054] 1. Dispersion preparation process This step is a step of preparing a dispersion in which a sulfide solid electrolyte and a first component are dispersed in a dispersion medium. The first component is lithium titanate or a rubber-based binder. The first component is preferably lithium titanate. The sulfide solid electrolyte, lithium titanate, and rubber-based binder are the same as those described above in "A. Negative electrode layer," and therefore will not be described here.
[0055] The dispersion medium in the present disclosure imparts fluidity to the dispersion. The dispersion medium may also dissolve a part of the sulfide solid electrolyte and the first component. Examples of the dispersion medium include esters such as butyl butyrate, dibutyl ether, and ethyl acetate, ketones such as diisobutyl ketone (DIBK), methyl ketone, and methyl propyl ketone, aromatic hydrocarbons such as xylene, benzene, and toluene, alkanes such as heptane, dimethylbutane, and methylhexane, and amines such as tributylamine and allylamine. The solid content concentration of the dispersion may be, for example, 30% by weight or more and 80% by weight or less, or 50% by weight or more and 70% by weight or less.
[0056] The method for producing the dispersion in the present disclosure is not particularly limited. For example, as shown in Fig. 1, a production method having a step of obtaining a precursor dispersion by adding a first component (lithium titanate in Fig. 1) to a dispersion medium and performing a first dispersion treatment, and a step of obtaining a dispersion by adding a sulfide solid electrolyte to the precursor dispersion and performing a second dispersion treatment, can be mentioned.
[0057] On the other hand, although not shown, another method for producing a dispersion includes a process of adding a sulfide solid electrolyte to a dispersion medium and performing a first dispersion treatment to obtain a precursor dispersion, and a process of adding a first component to the precursor dispersion and performing a second dispersion treatment to obtain a dispersion. Yet another method for producing a dispersion includes a process of adding both the first component and the sulfide solid electrolyte to a dispersion medium and performing a dispersion treatment to obtain a dispersion.
[0058] The dispersion treatment method may be any known method, for example, a method using an ultrasonic homogenizer. It is preferable to appropriately adjust the dispersion treatment conditions so as to obtain a desired dispersion.
[0059] In the present disclosure, a conductive material may be added in this step. The conductive material may be added simultaneously with the first component, the sulfide solid electrolyte, or both the first component and the sulfide solid electrolyte. Alternatively, the conductive material may be added separately from the first component and the sulfide solid electrolyte.
[0060] 2. Addition process This step is a step of adding and dispersing the second component into the dispersion prepared in the above "1. Dispersion Preparation Step" to obtain a negative electrode paste. The second component is lithium titanate or a rubber-based binder. The second component is preferably a rubber-based binder.
[0061] In this disclosure, the distributed processing method is the same as that described above, so the description thereof will be omitted here.
[0062] In the present disclosure, a conductive material may be added in this step. In this case, the conductive material and the second component may be added simultaneously, the conductive material may be added first and then the second component, or the second component may be added first and then the conductive material may be added.
[0063] 3.Negative electrode layer formation process This step is a step of forming a negative electrode layer by applying the negative electrode paste obtained in the above "2. Addition step" and drying it. The above negative electrode paste is preferably applied onto a current collector. The method of applying the paste is not particularly limited, and any known application method can be adopted. In addition, the negative electrode layer produced by each of the above steps is the same as that described in the above "A. Negative electrode layer", so the description here is omitted.
[0064] C. All-solid-state battery Fig. 2 is a schematic cross-sectional view illustrating an example of an all-solid-state battery in the present disclosure. The all-solid-state battery 10 shown in Fig. 2 has a positive electrode layer 1, a negative electrode layer 2, a solid electrolyte layer 3 disposed between the positive electrode layer 1 and the negative electrode layer 2, a positive electrode current collector 4 that collects current from the positive electrode layer 1, and a negative electrode current collector 5 that collects current from the negative electrode layer 2. In the present disclosure, the negative electrode layer 2 is the negative electrode layer described above in "A. Negative electrode layer".
[0065] According to the present disclosure, by using the above-described negative electrode layer, an all-solid-state battery with low resistance is obtained.
[0066] 1. Negative electrode layer The negative electrode layer in this disclosure is similar to the content described above in "A. Negative electrode layer," and therefore will not be described here.
[0067] 2. Positive electrode layer The positive electrode layer in the present disclosure contains at least a positive electrode active material, and may further contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary. Examples of the positive electrode active material include oxide active materials. Examples of the oxide active material include LiCoO 2 , LiMnO 2 , LiNiO 2 , LiVO 2 , LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 Rock salt layered active materials such as LiMn 2 O 4 , Li 4 Ti 5 O 12 , Li(Ni 0.5 Mn 1.5 )O 4 Spinel-type active materials such as LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4Examples of the olivine-type active material include LiNbO. The surface of the positive electrode active material is preferably coated with an ion-conductive oxide. This is because it is possible to suppress the reaction between the positive electrode active material and the solid electrolyte (particularly, a sulfide solid electrolyte) and the generation of a high resistance layer. Examples of the ion-conductive oxide include LiNbO. 3 The thickness of the ion conductive oxide is, for example, 1 nm or more and 30 nm or less.
[0068] The proportion of the positive electrode active material in the positive electrode layer is, for example, 20% by volume or more, may be 30% by volume or more, or may be 40% by volume or more. If the proportion of the positive electrode active material is low, the volumetric energy density may be low. On the other hand, the proportion of the positive electrode active material is, for example, 80% by volume or less, may be 70% by volume or less, or may be 60% by volume or less. If the proportion of the positive electrode active material is high, the ion conductive path and the electron conductive path may not be sufficiently formed.
[0069] The solid electrolyte is not particularly limited, and may be, for example, a sulfide solid electrolyte. Details of the sulfide solid electrolyte are the same as those described above in "A. Negative electrode layer." The conductive material and binder are the same as those described above in "A. Negative electrode layer." The thickness of the positive electrode layer is, for example, 0.1 μm or more and 1000 μm or less.
[0070] 3.Solid electrolyte layer The solid electrolyte layer in the present disclosure is disposed between the positive electrode layer and the negative electrode layer. The solid electrolyte layer contains at least a solid electrolyte, and may further contain a binder. The solid electrolyte and the binder are the same as those described in "2. Positive electrode layer", and therefore the description here is omitted. The thickness of the solid electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less.
[0071] 4.All-solid-state battery In the present disclosure, the term "all-solid-state battery" refers to a battery having a solid electrolyte layer (at least a layer containing a solid electrolyte). The all-solid-state battery in the present disclosure also includes a power generating element having a positive electrode layer, a solid electrolyte layer, and a negative electrode layer. The power generating element usually has a positive electrode current collector and a negative electrode current collector. The positive electrode current collector is disposed, for example, on the surface of the positive electrode layer opposite to the solid electrolyte layer. Examples of the material for the positive electrode current collector include metals such as aluminum, SUS, and nickel. Examples of the shape of the positive electrode current collector include foil and mesh. On the other hand, the negative electrode current collector is disposed, for example, on the surface of the negative electrode layer opposite to the solid electrolyte layer. Examples of the material for the negative electrode current collector include metals such as copper, SUS, and nickel. Examples of the shape of the negative electrode current collector include foil and mesh.
[0072] The all-solid-state battery in the present disclosure may include an exterior body that houses the power generating element. Examples of the exterior body include a laminate-type exterior body and a case-type exterior body. The all-solid-state battery in the present disclosure may also include a restraining jig that applies a restraining pressure in the thickness direction to the power generating element. A known jig can be used as the restraining jig. The restraining pressure may be, for example, 0.1 MPa or more and 50 MPa or less, and may be 1 MPa or more and 20 MPa or less. If the restraining pressure is small, there is a possibility that a good ion conductive path and a good electron conductive path will not be formed. On the other hand, if the restraining pressure is large, the restraining jig may become large, and the volumetric energy density may decrease.
[0073] The type of all-solid-state battery in the present disclosure is not particularly limited, but is typically a lithium-ion secondary battery. The use of the all-solid-state battery is not particularly limited, but examples thereof include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), electric vehicles (BEVs), gasoline-powered vehicles, and diesel-powered vehicles. In particular, it is preferable to use the all-solid-state battery as a driving power source for hybrid electric vehicles, plug-in hybrid electric vehicles, or electric vehicles. In addition, the all-solid-state battery in the present disclosure may be used as a power source for moving bodies other than vehicles (for example, railways, ships, and aircraft), and may be used as a power source for electrical products such as information processing devices.
[0074] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0075] [Example] (Preparation of negative electrode paste) Li as negative electrode active material 4 Ti 5 O 12 Particles (LTO, density 3.5g / cc), conductive material (VGCF, density 2g / cc), binder (SBR, density 0.9g / cc), dispersion medium (butyl butyrate), sulfide solid electrolyte (LiI-LiBr-Li 2 SP 2 S 5 A glass ceramic having a density of 2 g / cc was weighed.
[0076] A negative electrode paste was prepared according to the flow diagram shown in FIG. 1. First, the LTO particles were added to the dispersion medium, and a first dispersion process was performed using an ultrasonic homogenizer (UH-50 manufactured by SMT) to obtain a precursor dispersion. Next, the sulfide solid electrolyte was added to the obtained precursor dispersion, and a second dispersion process was performed using an ultrasonic homogenizer (UH-50 manufactured by SMT) to obtain a dispersion. Next, the binder was added to the dispersion, and the dispersion was dispersed using an ultrasonic homogenizer (UH-50 manufactured by SMT) to obtain a negative electrode paste.
[0077] (Preparation of positive electrode paste) As a positive electrode active material, LiNbO 3 Surface treated with LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2The positive electrode active material, conductive material (VGCF), sulfide solid electrolyte, binder (SBR), and dispersion medium (butyl butyrate) were weighed and mixed using an ultrasonic homogenizer (UH-50 manufactured by SMT Corporation). As a result, a positive electrode paste was obtained.
[0078] (Preparation of SE layer paste) A polypropylene container was filled with a dispersion medium (heptane), a binder (heptane solution containing 5% by mass of butadiene rubber binder), and a sulfide solid electrolyte (LiI-LiBr-Li 2 SP 2 S 5 Glass ceramics, average grain size D 50 The mixture was mixed for 30 seconds using an ultrasonic homogenizer (UH-50 manufactured by SMT Corporation). The container was then shaken for 3 minutes using a shaker. This resulted in a paste for a solid electrolyte layer (a paste for an SE layer).
[0079] (Production of all-solid-state batteries) First, the positive electrode paste was applied onto the positive electrode collector (aluminum foil) by the blade method using an applicator. After application, it was dried on a hot plate at 100°C for 30 minutes. This resulted in a positive electrode having a positive electrode collector and a positive electrode layer. Next, the negative electrode paste was applied onto the negative electrode collector (copper foil). After application, it was dried on a hot plate at 100°C for 30 minutes. This resulted in a negative electrode having a negative electrode collector and a negative electrode layer. Here, the basis weight of the negative electrode layer was adjusted so that the specific charge capacity of the negative electrode was 1.15 times that of the specific charge capacity of the positive electrode, when the specific charge capacity of the positive electrode was 185mAh / g.
[0080] Next, the positive electrode was pressed. The surface of the pressed positive electrode layer was coated with a paste for the SE layer by a die coater, and dried on a hot plate at 100°C for 30 minutes. Then, roll pressing was performed at a linear pressure of 2 ton / cm. This resulted in a positive electrode side laminate having a positive electrode current collector, a positive electrode layer, and a solid electrolyte layer. Next, the negative electrode was pressed. The surface of the pressed negative electrode layer was coated with a paste for the SE layer by a die coater, and dried on a hot plate at 100°C for 30 minutes. Then, roll pressing was performed at a linear pressure of 2 ton / cm. This resulted in a negative electrode side laminate having a negative electrode current collector, a negative electrode layer, and a solid electrolyte layer.
[0081] The positive electrode side laminate and the negative electrode side laminate were each punched and arranged so that the solid electrolyte layers faced each other, and an unpressed solid electrolyte layer was placed between them. Then, they were roll pressed at 130°C with a linear pressure of 2 ton / cm to obtain a power generating element having a positive electrode, a solid electrolyte layer, and a negative electrode in this order. The obtained power generating element was laminated and sealed, and restrained at 5 MPa to obtain an all-solid-state battery for evaluation.
[0082] [Calculation of ratio (A / B) (%)] The power generating element of the all-solid-state battery prepared in the examples was exposed and set in a chamber not exposed to the atmosphere, and transferred to a vacuum electron staining device (VSC4TWDH (manufactured by Filgen Co., Ltd.)). After creating a vacuum atmosphere inside the vacuum electron staining device, osmium tetroxide (OsO 4 ) gas was introduced, the chamber was opened, and the staining time and gas concentration were adjusted, and osmium (Os) staining was performed.
[0083] (Preparation of test specimens) The osmium-stained power generating element was cut to an appropriate size in an inert atmosphere to prepare a test piece. The cut surface of the sample piece was processed in a vacuum atmosphere using an ion milling device (IM4000PLUS, Hitachi High-Technologies Corporation).
[0084] (Image Acquisition) After cross-section processing, the sample was introduced into a field emission scanning electron microscope (FE-SEM "Regulus8230" manufactured by Hitachi High-Technologies Corporation). A vacuum atmosphere was maintained between cross-section processing and introduction into the SEM so that the sample was not exposed to the atmosphere.
[0085] The cross section of the negative electrode layer of the sample piece was observed by FE-SEM. Six observation positions were set at approximately equal intervals in a planar direction parallel to the negative electrode current collector (i.e., a direction perpendicular to the thickness direction of the negative electrode layer). The observation positions were selected so that the conductive material was not visible. At each observation position, SEM observation of secondary electron images and backscattered electron images was performed. The observation magnification was 5000 times. At the same observation positions, elemental mapping images of carbon (C), sulfur (S), and further sulfur (S) and osmium (Os) were obtained by EDX (energy dispersive x-ray spectroscopy). Figure 4(a) shows an SEM image of the cross section of the negative electrode layer, Figure 4(b) shows a mapping image of carbon (C image), Figure 4(c) shows a mapping image of sulfur (S image), and Figure 4(d) shows a mapping image of sulfur and osmium (S,Os image).
[0086] (Image analysis) Using the images obtained above, (1) the total rubber binder content B, and (2) the amount A of the rubber binder adsorbed on the lithium titanate were measured.
[0087] (1) Measurement of total rubber binder content B First, the carbon mapping image (C image) was subjected to binarization processing. The number of pixels P1 in the extracted image of the C element was counted and found to be 193,890 pixels.
[0088] Next, the sulfur mapping image (S image) was subjected to binarization processing. The number of pixels P2 of the extracted image of the S element was counted and found to be 100660 pixels.
[0089] Next, the number of pixels P3 was calculated by subtracting P2 from P1, and the result was 93,230 pixels.
[0090] (2) Measurement of the amount A of rubber binder adsorbed on lithium titanate First, the mapping images of sulfur (S) and osmium (Os) obtained above (Figure 5(a)) were separated by coloring the areas where Os element exists and the areas where S element exists in red and the other areas in black (Figure 5(b)). Next, by removing the large area of mass (the area consisting of S in the sulfide solid electrolyte and Os covering the S in the sulfide solid electrolyte), the remaining Os element, i.e., the Os element adsorbed on the lithium titanate, was extracted (Figure 5(c)). The number of pixels P4 of the extracted Os element was counted and found to be 1265 pixels.
[0091] The ratio of the amount A of the rubber-based binder adsorbed to lithium titanate to the total content B of the rubber-based binder contained in the negative electrode layer was calculated as a percentage ((P4 / P3)×100(%)) by dividing the number of pixels P4 obtained in (2) above by the number of pixels P3 obtained in (1) above, and found to be 1.35%.
[0092] [Comparative Example] First, as in the examples, Li was used as the negative electrode active material. 4 Ti 5 O 12 Particles (LTO, density 3.5g / cc), conductive material (VGCF, density 2g / cc), binder (SBR, density 0.9g / cc), dispersion medium (butyl butyrate), sulfide solid electrolyte (LiI-LiBr-Li 2 SP 2 S 5 A glass ceramic having a density of 2 g / cc was weighed.
[0093] A negative electrode paste was obtained according to the flow diagram shown in FIG. 3. First, the LTO particles were added to the dispersion medium and dispersed using an ultrasonic homogenizer (UH-50 manufactured by SMT) to obtain a precursor dispersion. Next, the binder was added to the obtained precursor dispersion and dispersed using an ultrasonic homogenizer (UH-50 manufactured by SMT) to obtain a dispersion. Next, the sulfide solid electrolyte was added to the dispersion and dispersed using an ultrasonic homogenizer (UH-50 manufactured by SMT) to obtain a negative electrode paste. Except for using the obtained negative electrode paste, an all-solid-state battery for evaluation was obtained in the same manner as in the example.
[0094] For the all-solid-state battery for evaluation manufactured in the comparative example, the preparation of a test piece, the acquisition of an image, and the image analysis were performed in the same manner as in the example. The pixel number P1 of the extracted image of the C element was 690624 pixels, the pixel number P2 of the extracted image of the S element was 241380 pixels, and the pixel number P3 was calculated to be 449244. The pixel number P4 was 21008 pixels. FIG. 6(d) shows an SEM image of the cross section of the negative electrode layer of the comparative example, FIG. 6(e) shows a mapping image of sulfur and osmium (S, Os image), and FIG. 6(f) shows an extracted Os image of LTO adsorption. From the above, the ratio of the adsorption amount A of the rubber-based binder adsorbed on lithium titanate to the total content B of the rubber-based binder contained in the negative electrode layer was calculated to be 4.68%. For comparison, the SEM image, S, Os image, and Os image of LTO adsorption of the all-solid-state battery for evaluation of the example are shown in FIG. 6(a), (b), and (c).
[0095] [evaluation] (DC resistance measurement) The DC resistance of the all-solid-state battery produced in the examples and comparative examples was specified. Specifically, the all-solid-state battery was charged at a constant current equivalent to 1C, and after the cell voltage reached 2.95V, it was charged at a constant voltage, and the charging was terminated when the charging current reached 0.01C. Thereafter, it was discharged at a constant current equivalent to 1C, and the charging was terminated when it reached 1.5V. Thereafter, the all-solid-state battery was charged at a constant current equivalent to 3C, and the difference between the voltage before charging and the voltage after charging for 10 seconds was divided by the current equivalent to 3C to calculate the DC resistance (charging resistance). The results are shown in Table 1. The charging resistance ratio value in Table 1 is a relative value to the comparative example.
[0096] [Table 1]
[0097] As shown in Table 1, it was confirmed that the charging resistance ratio of the Examples was lower than that of the Comparative Examples. The reason why the charging resistance ratio of the Examples was lower than that of the Comparative Examples is presumably because the proportion of the binder amount adsorbed to the negative electrode active material (lithium titanate) was low, thereby suppressing the reduction in the reaction area of the negative electrode active material. [Explanation of symbols]
[0098] 1 ... Positive electrode layer 2 ... Negative electrode layer 3...Solid electrolyte layer 4...Positive electrode current collector 5...Negative electrode current collector 10...All-solid-state battery
Claims
1. A negative electrode layer for use in an all-solid-state battery, the negative electrode layer includes lithium titanate, a sulfide solid electrolyte, and a rubber-based binder; Regarding the negative electrode layer in which the rubber-based binder is dyed with osmium tetroxide, in an EDX mapping image at an observation magnification of 5000 times, the number of pixels P2 of the extracted image of the S element is subtracted from the number of pixels P1 of the extracted image of the C element to obtain a total content P3 of the rubber-based binder B, and the number of pixels of the image of the Os element is the adsorption amount A. a ratio (A / B) of the adsorption amount A of the rubber-based binder adsorbed to the lithium titanate to the total content B of the rubber-based binder contained in the negative electrode layer is 1.35% or less.
2. The anode layer of claim 1 , wherein the rubber binder comprises a styrene butadiene rubber.
3. A method for producing an anode layer according to claim 1 or claim 2, comprising the steps of: A dispersion preparation step of preparing a dispersion in which the sulfide solid electrolyte and a first component are dispersed in a dispersion medium; an addition step of adding and dispersing a second component into the dispersion to obtain a negative electrode paste; and a negative electrode layer forming step of applying the negative electrode paste and drying it to form the negative electrode layer, one of the first component and the second component is the lithium titanate, and the other is the rubber-based binder.
4. An all-solid-state battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, The negative electrode layer according to claim 1 or 2,
Citation Information
Patent Citations
All-solid type secondary battery, composition for electrode active material layer, electrode sheet for all-solid type secondary battery, and manufacturing methods for all-solid type secondary battery and electrode sheet for all-solid type secondary battery
JP2016212990A
Method for manufacturing slurry, method for manufacturing active material layer and method for manufacturing all-solid battery
JP2020177755A
Negative electrode for all-solid-state battery
JP2021128885A
Manufacturing method of electrode and manufacturing method of all-solid-state battery
JP2021193645A