Graft modified product, adhesive, olefin resin composition and laminate
A graft modified product using a carbodiimide monomer enhances the adhesive strength of polyolefins on polar resins, addressing compatibility issues and enabling efficient laminating with materials like polyester and polyphenylene sulfide.
Patent Information
- Application Number
- JP2022566932
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-04
- Filing Date
- 2021-11-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-11-30
AI Technical Summary
Polyolefins lack sufficient compatibility and adhesiveness with polar resins, limiting their use in blending or laminating with materials like polyester and polyphenylene sulfide, and existing grafting methods do not provide adequate adhesive strength in a timely manner.
A graft modified product using a carbodiimide monomer with a carbodiimide group and a polymerizable double bond is applied to polyolefins, enhancing adhesion by forming a layer with high adhesive strength on polar group-containing materials such as polyester or polyphenylene sulfide.
The modified product achieves high adhesive strength quickly on polar group-containing materials, improving compatibility and adhesion, and is suitable for use in adhesives and laminates with materials like polyester and polyphenylene sulfide.
Smart Images

Figure 0007590458000001 
Figure 0007590458000002 
Figure 0007590458000003
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention relates to a graft modified product, an adhesive, an olefin resin composition, or a laminate. [Background technology]
[0002] Polyolefins such as polyethylene and polypropylene have excellent mechanical strength, rigidity, heat resistance, chemical resistance, oil resistance, transparency, and impact resistance at low temperatures. Taking advantage of these properties, they are widely used as packaging and covering materials such as films, sheets, and bottles, as well as decorative materials such as wallpaper.
[0003] However, since polyolefins do not contain polar groups in their molecules, they have poor compatibility with polar resins such as polyesters, polyphenylene sulfide, polyamides, polyacetals, polycarbonates, poly(meth)acrylates, modified fluororesins, and biomass plastics, and poor adhesion to metals, glass, paper, or the above-mentioned polar resins, and therefore there are limitations to their use in blending with or laminating with these materials.
[0004] In order to solve such problems, a method of grafting a polar group-containing monomer onto a polyolefin to improve the compatibility and adhesiveness has been widely used. For example, a method of grafting glycidyl (meth)acrylate onto a polyolefin is widely used (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-145260 Summary of the Invention [Problem to be solved by the invention]
[0006] The modified polyolefin obtained by the method described in Patent Document 1 can improve the compatibility and adhesion to a certain extent, but the compatibility and adhesion are not sufficient. In particular, the adhesive strength is insufficient, or it takes a long time to develop sufficient adhesive strength.
[0007] One embodiment of the present invention provides a graft modified polymer capable of forming a layer with high adhesive strength even in a short period of time on a substrate having a polar group, such as polyester or polyphenylene sulfide. [Means for solving the problem]
[0008] As a result of the inventor's research, it has been found that the above-mentioned problems can be solved by the following configuration example.
[0009] [1] A graft-modified product of at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond.
[0010] [2] The graft modified product according to [1], wherein the carbodiimide monomer is a carbodiimide monomer represented by the following formula (1):
[0011] [ka] [In formula (1), R1 is a hydrogen atom or a methyl group, and R2 is a hydrocarbon group which may have a substituent.]
[0012] [3] The graft modified product according to [2], wherein R2 is an aliphatic hydrocarbon group having 4 to 20 carbon atoms and containing an alicyclic ring.
[0013] [4] The graft modified product according to [1], wherein the carbodiimide monomer is a carbodiimide monomer represented by the following formula (2):
[0014] [ka] [In formula (2), R3 is a hydrogen atom or a methyl group, R4 is a hydrocarbon group which may have a substituent, and m is an integer of 2 or more.]
[0015] [5] The graft modified compound according to [4], wherein R3 is a methyl group, R4 is a branched and non-ring-containing alkyl group, and m is 2.
[0016] [6] The graft modified product according to any one of [1] to [5], wherein the base polymer is a polymer that does not have at least one active hydrogen-containing group selected from a carboxy group, an acid anhydride group, an amino group, a hydroxyl group, and a thiol group.
[0017] [7] The graft-modified product according to any one of [1] to [6], wherein the polyolefin is at least one selected from an ethylene-based polymer and a propylene-based polymer.
[0018] [8] An olefin resin composition comprising the graft modified product according to any one of [1] to [7] and one or more olefin polymers.
[0019] [9] An adhesive comprising the graft modified product according to any one of [1] to [7] or the olefin resin composition according to claim 8.
[0020]
[10] A laminate comprising: a layer (A) selected from a layer containing the graft modified product according to any one of [1] to [7] and a layer containing the olefin-based resin composition according to [8]; and a base layer (B).
[0021]
[11] The laminate according to
[10] , wherein the base material layer (B) is a layer having a polar group.
[12] The laminate according to
[11] , wherein the polar group is a carboxy group or a hydroxy group. Effect of the Invention
[0022] According to one embodiment of the present invention, it is possible to provide a graft modified material capable of forming a layer with high adhesive strength even in a short time (short sealing time) on a substrate having a polar group, such as polyester or polyphenylene sulfide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Graft modified product The graft modified product according to one embodiment of the present invention (hereinafter also referred to as "the modified product") is a graft modified product of at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond, in other words, a graft modified product in which at least one base polymer selected from polyolefins is graft modified with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond. The modified product can also be said to be a graft modified product containing at least one base polymer portion selected from polyolefins and a graft portion derived from a carbodiimide monomer having a carbodiimide group and a polymerizable double bond.
[0024] The modified product can form a layer with high adhesive strength even in a short time on a substrate having a polar group, such as polyester or polyphenylene sulfide. This modified product has higher reactivity with polar groups present in polyesters, polyphenylene sulfides, etc. than the graft modified product with glycidyl (meth)acrylate, and therefore has remarkably excellent adhesion to these substrates. Furthermore, the present modified product exhibits the above-mentioned effects since it is not a block copolymer or random copolymer of an olefin monomer such as ethylene or propylene with the above-mentioned carbodiimide monomer but a graft modified product.
[0025] The graft ratio in the present modified product is preferably 0.3 to 7 mass%, more preferably 0.5 to 5 mass%, from the viewpoints of ease of synthesis of the present modified product, ease of obtaining a graft modified product having superior compatibility and adhesion, and prevention of the obtained graft modified product from being too hard. The graft ratio is the mass of a structure derived from a carbodiimide monomer in the graft modified product, 1 It can be determined by H-NMR measurement, specifically, the method described in the examples below.
[0026] <Carbodiimide monomer> The carbodiimide monomer used in graft-modifying the base polymer is not particularly limited as long as it is a compound having a carbodiimide group and a polymerizable double bond. From the viewpoint of better exerting the effects of the present invention, however, it is preferable that the carbodiimide monomer is a compound represented by the following formula (1) or (2). The carbodiimide monomer used when graft-modifying the base polymer may be of two or more types, but is usually of one type.
[0027] [ka]
[0028] In formula (1), R1 is a hydrogen atom or a methyl group, and a hydrogen atom is preferred from the viewpoint that the present modified product having a high graft ratio can be easily obtained.
[0029] In formula (1), R2 is a hydrocarbon group which may have a substituent. Specific examples of the hydrocarbon group include an alkyl group or an aryl group which may have a substituent. The alkyl group which may have a substituent may be chain-like (may be linear or branched) or may contain an alicyclic ring. The number of carbon atoms in the hydrocarbon group which may have a substituent is preferably 1 or more, more preferably 3 or more, and is preferably 20 or less, more preferably 12 or less, and even more preferably 8 or less. Examples of the substituent that the hydrocarbon group may have include a halogen atom, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a carboxylate group having 1 to 8 carbon atoms, a sulfonate group having 1 to 8 carbon atoms, a carbonyl group having 1 to 8 carbon atoms, an amide group having 1 to 8 carbon atoms, an amino group having 1 to 8 carbon atoms, a sulfide group having 1 to 8 carbon atoms, a phosphate group having 1 to 8 carbon atoms, an alkylsilyl group having 1 to 8 carbon atoms, and an alkoxysilyl group having 1 to 8 carbon atoms.
[0030] Among these, R2 is preferably an aliphatic hydrocarbon group containing an alicycle having 4 to 20 carbon atoms, and more preferably an alicyclic hydrocarbon group having 5 to 7 carbon atoms, from the standpoints of the solubility of the carbodiimide monomer, ease of availability, ease of purification of the resulting graft modified product, and the like. Examples of the alicyclic ring include a cyclobutyl ring, a cyclopentyl ring, a cyclohexyl ring, a cycloheptyl ring, and rings having a hydrocarbon group. The alicyclic ring may be a polycyclic ring such as an adamantyl ring or a methyladamantyl ring.
[0031] [ka]
[0032] In formula (2), R3 is a hydrogen atom or a methyl group, and a methyl group is preferred from the viewpoint that the present modified product having excellent adhesive strength to a substrate having a polar group can be easily obtained.
[0033] In formula (2), R4 is a hydrocarbon group which may have a substituent. Specific examples of the hydrocarbon group include an alkyl group or an aryl group which may have a substituent. The alkyl group which may have a substituent may be chain-like (may be linear or branched) or may contain an alicyclic ring. The number of carbon atoms in the hydrocarbon group which may have a substituent is preferably 1 or more, more preferably 3 or more, and is preferably 20 or less, more preferably 12 or less, and even more preferably 8 or less. Examples of the substituent that the hydrocarbon group may have include a halogen atom, a hydrocarbon group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a carboxylate group having 1 to 8 carbon atoms, a sulfonate group having 1 to 8 carbon atoms, a carbonyl group having 1 to 8 carbon atoms, an amide group having 1 to 8 carbon atoms, an amino group having 1 to 8 carbon atoms, a sulfide group having 1 to 8 carbon atoms, a phosphate group having 1 to 8 carbon atoms, an alkylsilyl group having 1 to 8 carbon atoms, and an alkoxysilyl group having 1 to 8 carbon atoms.
[0034] Among these, R4 is preferably a branched, non-cyclic alkyl group, and more preferably a branched, non-cyclic alkyl group having 3 to 7 carbon atoms, from the viewpoint that the present modified product having excellent adhesive strength to a substrate having a polar group, particularly to polyester, can be easily obtained.
[0035] Preferable examples of the branched and ring-free alkyl group include an isopropyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, a 1-methylbutyl group, a 1,2-dimethylpropyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 1-ethylpropyl group, a 1,1-dimethylpropyl group, a 2,2-dimethylpropyl group, a 1-methylpentyl group, a 1,2-dimethylbutyl group, a 1,3-dimethylbutyl group, a 1,2,2-trimethylpropyl group, a 2-methylpentyl group, a 2 ,2-dimethylbutyl group, 2,3-dimethylbutyl group, 2-ethylbutyl group, 3-methylpentyl group, 3,3-dimethylbutyl group, 4-methylpentyl group, 1-ethyl-2-methylpropyl group, 1-ethylbutyl group, 1,1-dimethylbutyl group, 1,1,2-trimethylpropyl group, 1-ethyl-1-methylpropyl group, 1-methylhexyl group, 1,2-dimethylpentyl group, 1,3-dimethylpentyl group, 1,4-dimethylpentyl group, 1,2,3-trimethylbutyl group, 1 ,2,2-trimethylbutyl group, 1,3,3-trimethylbutyl group, 2-methylhexyl group, 2,3-dimethylpentyl group, 2,4-dimethylpentyl group, 2,3,3-trimethylbutyl group, 1,1-dimethylpentyl group, 1,1,2-trimethylbutyl group, 1,1,3-trimethylbutyl group, 1,1,2,2-tetramethylpropyl group, 2,2-dimethylpentyl group, 2,2,3-trimethylbutyl group, 3-methylhexyl group, 3,4-dimethylpentyl group, 3,3-dimethyl Examples of such groups include an ethyl pentyl group, a 1-ethylpentyl group, a 1-ethyl-2-methylbutyl group, a 1-ethyl-3-methylbutyl group, a 1-ethyl-2,2-dimethylpropyl group, a 2-ethylpentyl group, a 2-ethyl-3-methylbutyl group, a 1-ethyl-1-methylbutyl group, a 1-ethyl-1,2-dimethylpropyl group, a 3-ethylpentyl group, a 1,1-diethylpropyl group, a 2,2-diethylpropyl group, a 1-propylbutyl group, a diisopropylmethyl group, and a 1-isopropylbutyl group.
[0036] In formula (2), m is an integer of 2 or more, and from the standpoints of the solubility of the carbodiimide monomer, ease of availability, ease of purification of the resulting graft modified product, etc., m is preferably an integer of 2 to 6, more preferably an integer of 2 to 4, and particularly preferably 2.
[0037] <Base polymer> The base polymer before being graft-modified with the carbodiimide monomer is at least one polymer selected from polyolefins. Specific examples of the olefin include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, and 4-methyl-1-pentene. The polyolefin may be a homopolymer of these olefins, a copolymer of two or more of these olefins, or a copolymer of one or more of these olefins with one or more of the following copolymers. Among these, the polyolefin is preferably at least one polymer selected from an ethylene-based polymer, a propylene-based polymer, and a butene-based polymer, and more preferably at least one polymer selected from an ethylene-based polymer and a propylene-based polymer from the viewpoints of excellent solubility in the solvent when a solvent is used during the graft reaction and excellent separability from impurities after the graft reaction. The base polymer may be of two or more types, but is usually of one type.
[0038] In order to more effectively exert the effects of the present invention, the base polymer is preferably a polymer that does not have at least one active hydrogen-containing group selected from a carboxy group, an acid anhydride group, an amino group, a hydroxyl group, and a thiol group. In addition, in order to better exert the effects of the present invention, it is also preferable that the base polymer is a polymer that does not have a carboxylic acid derivative group such as an acid halide, amide, imide or ester, or a group that is easily converted by water or the like into a group having an active hydrogen, such as an epoxy group.
[0039] The weight average molecular weight (Mw) of the base polymer is not particularly limited, but from the viewpoint of ease of synthesis of the present modified product, it is preferably 100,000 or more, more preferably 150,000 or more, and preferably 1,000,000 or less, more preferably 700,000 or less. The number average molecular weight (Mn) of the base polymer is not particularly limited, but for the same reasons, it is preferably 40,000 or more, more preferably 50,000 or more, and preferably 500,000 or less, more preferably 300,000 or less. The molecular weight distribution (Mw / Mn) of the base polymer is not particularly limited, but is preferably 1.5 or more, more preferably 2.0 or more, and is preferably 6.0 or less, more preferably 5.0 or less.
[0040] The Mw and Mn values were measured under the following conditions using a gel permeation chromatograph (GPC) HLC-8321 GPC / HT type manufactured by Tosoh Corporation. Separation columns: TSKgel GMH6-HT (2 columns) and TSKgel GMH6-HTL (2 columns) (both 7.5 mm I.D. x 30 cm, Tosoh Corporation) Column temperature: 140℃ Mobile phase: o-dichlorobenzene (containing 0.025% dibutylhydroxytoluene (BHT)) Development speed: 1.0mL / min Sample concentration: 0.1% (w / v) Sample injection volume: 0.4mL Detector: Differential refractometer Calibration of the instrument: Monodisperse polystyrene (Tosoh Corporation, #3std set) was used.
[0041] The base polymer can be synthesized by a conventionally known method, or a commercially available product may be used. The conventionally known method is not particularly limited, and may be, for example, a method using a coordination polymerization catalyst system containing transition metal.Specifically, may be a method of synthesizing by (co)polymerizing ethylene or propylene and, if necessary, a comonomer described later, in the presence of a catalyst such as a magnesium chloride supported titanium catalyst, a vanadium catalyst containing a soluble vanadium compound and an alkylaluminum halide compound, or a metallocene catalyst containing a metallocene compound and an organoaluminum oxy compound.
[0042] [Ethylene polymer] The ethylene-based polymer is not particularly limited as long as the content of ethylene-derived structural units in the polymer is 50% by mass or more, and may be a homopolymer of ethylene or a copolymer of ethylene and a comonomer. In the case of a copolymer, the structure is not particularly limited.
[0043] The comonomer may be, for example, at least one monomer selected from propylene, α-olefins having 4 to 20 carbon atoms, and conjugated polyenes. Among these, propylene and α-olefins having 4 to 20 carbon atoms are preferred. The α-olefin having 4 to 20 carbon atoms may be linear or branched, and examples thereof include 1-butene, 2-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. The content of the comonomer-derived structural units in the ethylene-based polymer is preferably 50% by mass or less, more preferably 30% by mass or less, and particularly preferably 20% by mass or less, from the viewpoints of preventing blocking of pellets or powder and making them easy to handle, etc. In this specification, an ethylene-based polymer having a content of propylene-derived or butene-derived structural units of 50% by mass is referred to as an ethylene-based polymer.
[0044] [Propylene polymer] The propylene-based polymer is not particularly limited as long as the content of propylene-derived structural units in the polymer is 50% by mass or more, and may be a homopolymer of propylene or a copolymer of propylene and a comonomer. The structure of these (co)polymers is not particularly limited.
[0045] The comonomer may be, for example, at least one monomer selected from ethylene, α-olefins having 4 to 20 carbon atoms, and conjugated polyenes. Among these, ethylene and α-olefins having 4 to 20 carbon atoms are preferred. Examples of the α-olefin having 4 to 20 carbon atoms include the same α-olefins having 4 to 20 carbon atoms as those listed in the section on ethylene-based polymers. The content of the comonomer-derived structural unit in the propylene-based polymer is preferably 50% by mass or less, more preferably 30% by mass or less, and particularly preferably 20% by mass or less, from the viewpoints of no blocking of pellets or powder and easy handling, etc. In this specification, a propylene-based polymer having a butene-derived structural unit content of 50% by mass is referred to as a propylene-based polymer.
[0046] [Butene polymer] The butene polymer is not particularly limited as long as the content of butene-derived structural units in the polymer is 50% by mass or more, and may be a homopolymer of butene, particularly 1-butene, or a copolymer of butene (particularly 1-butene) and a comonomer. The structure of these (co)polymers is not particularly limited.
[0047] The comonomer may be, for example, at least one monomer selected from ethylene, propylene, α-olefins having 5 to 20 carbon atoms, and conjugated polyenes. Among these, ethylene, propylene, and α-olefins having 5 to 20 carbon atoms are preferred. Examples of the α-olefin having 5 to 20 carbon atoms include the same α-olefins having 5 to 20 carbon atoms as those listed in the section on ethylene-based polymers. The content of the structural units derived from the comonomer in the butene polymer is preferably 50% by mass or less, more preferably 30% by mass or less, and particularly preferably 20% by mass or less, from the viewpoints of preventing blocking of pellets or powder and making them easy to handle.
[0048] <Method of synthesizing the modified compound> The method for synthesizing the modified product is not particularly limited as long as the base polymer is graft-modified with the carbodiimide monomer, but from the viewpoint of easy synthesis of the modified product, a method is preferred in which a radical initiator and the carbodiimide monomer are added to a solution in which the base polymer is dissolved or dispersed in a solvent, preferably a solution in which the base polymer is dissolved in an organic solvent, and reacted (grafted) with the solution. When a reaction device having a stirring ability capable of uniformly flowing the base polymer is used, a solvent is not required. According to the above method, graft polymerization occurs, so that a graft modified product can be obtained.
[0049] The amount of the carbodiimide monomer used in the graft reaction is preferably 10 to 1,000 mol, more preferably 10 to 800 mol, per mol of the base polymer, from the viewpoints that the present modified product having a graft rate within the above range can be easily obtained and the production of a polymer of the carbodiimide monomer itself (hereinafter also referred to as a "non-grafted polymer") can be suppressed.
[0050] Examples of the radical initiator include organic peroxides and azo compounds. Specific examples of the radical initiator include benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoate)hexyne-3, 1,4-bis(tert-butylperoxyisopropyl)benzene, lauroyl peroxide, tert-butyl peracetate, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(te Examples of the organic peroxides include organic peroxides such as tert-butylperoxy)hexane, tert-butylperbenzoate, tert-butylperphenylacetate, tert-butylperisobutyrate, tert-butylper-sec-octoate, tert-butylperpivalate, cumylperpivalate, tert-butylperdiethylacetate, and tert-butylperoxyisopropylmonocarbonate; and azo compounds such as azobisisobutyronitrile and dimethylazoisobutyrate. Among these, organic peroxides such as dicumylperoxide, di-tert-butylperoxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,4-bis(tert-butylperoxyisopropyl)benzene, and tert-butylperoxyisopropylmonocarbonate are preferred. The radical initiators may be used alone or in combination of two or more.
[0051] The amount of the radical initiator used in the graft reaction is preferably 0.01 mol or more, more preferably 0.05 mol or more, and is preferably 0.7 mol or less, more preferably 0.5 mol or less, per 1 mol of carbodiimide monomer, from the viewpoints that the graft reaction occurs efficiently and the present modified product having a graft rate in the above range can be easily obtained.
[0052] The organic solvent is preferably an organic solvent that does not significantly inhibit the graft reaction of the carbodiimide monomer and has affinity with the base polymer in the temperature range in which the graft reaction is carried out.Specific examples of such organic solvents include aromatic hydrocarbon solvents such as benzene, toluene, and xylene, aliphatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, and decane, alicyclic hydrocarbon solvents such as cyclohexane, methylcyclohexane, and decahydronaphthalene, chlorinated hydrocarbon solvents such as chlorobenzene, dichlorobenzene, trichlorobenzene, methylene chloride, chloroform, carbon tetrachloride, and tetrachloroethylene, alcohol solvents such as methanol, ethanol, n-propanol, iso-propanol, n-butanol, sec-butanol, and tert-butanol, ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ester solvents such as ethyl acetate and dimethyl phthalate, and ether solvents such as dimethyl ether, diethyl ether, di-n-amyl ether, tetrahydrofuran, and dioxyanisole.In addition, suspension polymerization and emulsion polymerization can be carried out using water as a solvent. These solvents may be used alone or in combination of two or more. It is preferable that the reaction solution becomes a homogeneous phase by using these solvents, but it does not matter if the reaction solution becomes a heterogeneous multiple phase.
[0053] In order to carry out the graft reaction in a region where the liquid containing the base polymer can be stirred homogeneously, the concentration of the base polymer in the liquid is usually set to 50 to 500 g / L, but in order to achieve a high graft rate, it is preferable that the concentration be 200 to 500 g / L.
[0054] The radical initiator and the carbodiimide monomer may be added all at once to a liquid containing the base polymer (or the base polymer itself) to initiate the graft reaction. However, in order to achieve a high graft rate, it is preferable to carry out the graft reaction by gradually adding them over a period of about 0.1 to 5 hours. In addition, when the radical initiator and the carbodiimide monomer are added to the base polymer or a liquid in which the base polymer is dissolved or dispersed in a solvent, the order of addition is not particularly limited. For example, when these are added sequentially as described above, the radical initiator and the carbodiimide monomer may be added sequentially, or the carbodiimide monomer may be added first and then the radical initiator may be added sequentially.
[0055] The graft reaction is desirably carried out at a temperature of usually 60° C. or higher, preferably 100° C. or higher, usually 200° C. or lower, preferably 160° C. or lower, for usually 2 hours or more, preferably 3 hours or more, usually 10 hours or less, preferably 8 hours or less.
[0056] The present modified product obtained by the graft reaction may be purified and isolated by using a known method, such as a combination of filtration, centrifugation, reprecipitation and / or washing, as necessary, to remove the solvent used, unreacted radical initiator or carbodiimide monomer, and by-produced non-grafted polymer. In this case, it is desirable to purify and isolate the present modified product so that the content of the non-grafted polymer contained in the present modified product is preferably 5% by mass or less, more preferably 2% by mass or less, in order to easily obtain the present modified product having superior compatibility and adhesiveness.
[0057] <Uses of the modified substance> The modified product has excellent compatibility with polar resins such as polyesters, polyphenylene sulfide, polyamides, polyacetals, polycarbonates, poly(meth)acrylates, modified fluororesins, and biomass plastics, and olefin-based polymers, and can therefore be used as a compatibilizer for compositions containing these polar resins and olefin-based polymers; has excellent adhesion to metals, glass, paper, or the polar resins and olefin-based polymers, and can therefore be used as an adhesive for substrates containing these; and has excellent dispersibility in olefin-based polymers, and can therefore be mixed with olefin-based polymers and used as an olefin-based resin composition, etc. Among these, the present modified product has excellent adhesion to polyester and polyphenylene sulfide, and therefore is preferably used as an adhesive for polyester or polyphenylene sulfide (or a layer containing same) or as an olefin-based resin composition, from the viewpoint of better exerting the effects of the present invention.
[0058] The olefin-based polymer is not particularly limited as long as it is a polymer mainly composed of olefin, and various known olefin-based polymers can be used.Specific examples of the olefin-based polymer include homopolymers or copolymers of α-olefins such as ethylene, propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene, etc. (e.g., high-pressure low-density polyethylene, linear low-density polyethylene (LLDPE), medium-density polyethylene, high-density polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, low-crystalline or amorphous ethylene-propylene random copolymers, ethylene-1-butene random copolymers, and propylene-1-butene random copolymers), ethylene-vinyl acetate copolymers (EVA) or saponification products thereof, ethylene-(meth)acrylic acid copolymers or metal salts (ionomers) thereof, ethylene-cyclic olefin copolymers, and polymers obtained by graft-modifying these (co)polymers with polar compounds such as maleic acid and silane compounds.
[0059] When the present modified product is used for various applications, various additives may be added to the present modified product as necessary within the scope of the invention. Examples of the additives include softeners, stabilizers, fillers, antioxidants, crystal nucleating agents, waxes, thickeners, mechanical stability agents, leveling agents, wetting agents, film-forming assistants, crosslinking agents, preservatives, rust inhibitors, pigments, dispersants, antifreeze agents, antifoaming agents, tackifiers, other thermoplastic polymers, water, and organic solvents. Each of these may be used alone or in combination of two or more.
[0060] <Olefin-based resin composition> The olefin-based resin composition according to one embodiment of the present invention is not particularly limited as long as it contains the present modified product and one or more olefin-based polymers, and the present modified product contained in the olefin-based resin composition may be one type or two or more types. The olefin resin composition may contain one or more of the above-mentioned additives.
[0061] The olefin resin composition can be used not only as an adhesive (adhesive resin composition) but also as, for example, a printing ink, a paint, a machine cleaner for polymer processing, and a binder.
[0062] The content of the present modified product in the olefin resin composition is not particularly limited, but from the standpoints of moldability, controllability of adhesive ability, economic efficiency, etc., it is usually 0.5 mass% or more, preferably 1 mass% or more, and usually 40 mass% or less, preferably 25 mass% or less.
[0063] Examples of the olefin polymer contained in the olefin resin composition include the same polymers as the olefin polymers described in the section on uses of the present modified product. The content of the olefin polymer in the olefin resin composition is not particularly limited, but from the standpoints of moldability, controllability of adhesive ability, economic efficiency, etc., it is usually 60 mass% or more, preferably 75 mass% or more, and usually 99.5 mass% or less, preferably 99 mass% or less.
[0064] <Adhesive> The adhesive (including the pressure-sensitive adhesive) according to one embodiment of the present invention is not particularly limited as long as it contains the present modified product or the olefin-based resin composition, and the present modified product and the olefin-based resin composition contained in the adhesive may each be one type or two or more types. The adhesive may be an adhesive consisting only of the present modified product, or may contain one or more of the above-mentioned olefin polymers and additives. The content of the present modified product in the adhesive containing the present modified product is not particularly limited, but is usually 5 to 100% by mass, and preferably 10 to 100% by mass.
[0065] The adhesive can be used in various known forms, for example, as a water-dispersed adhesive, an organic solvent adhesive, or a hot melt adhesive.
[0066] Examples of objects to be adhered to by the adhesive include layers containing or made of metal; glass; wood; paper; cloth; thermoplastic resins such as polyester, polyphenylene sulfide, polyamide, polyacetal, polycarbonate, poly(meth)acrylate, olefin polymers, polystyrene, rubber, modified fluororesin, biomass plastics, and other engineering plastics; and thermosetting resins.
[0067] <Laminate> The laminate according to one embodiment of the present invention is not particularly limited as long as it includes a layer (A) containing the present modified product or the olefin resin composition and a base layer (B), and may include two or more layers of the layer (A), or may include two or more layers of the base layer (B). When two or more layers (A) are included, these layers may be the same layer or different layers. Similarly, when two or more base layers (B) are included, these layers may be the same layer or different layers. The laminate is preferably a laminate including a layer (A) and a base layer (B), or a laminate including a base layer (B), a layer (A), and a base layer (B) in this order.
[0068] The layer (A) can be obtained using the present modified product, the adhesive, or the olefin-based resin composition. The presence of the present modified product in the layer (A) can be determined by infrared spectroscopic analysis.
[0069] The thickness of the layer (A) is not particularly limited and may be appropriately selected depending on the application of the laminate, but is preferably 2 to 1000 μm. The thickness of the base layer (B) is not particularly limited and may be appropriately selected depending on the application of the laminate, but is preferably 2 to 1000 μm.
[0070] Examples of the base layer (B) include layers containing or consisting of metal; glass; wood; paper; cloth; thermoplastic resins such as polyester, polyphenylene sulfide, polyamide, polyacetal, polycarbonate, poly(meth)acrylate, olefin polymers, polystyrene, rubber, modified fluororesin, biomass plastics, and other engineering plastics; and thermosetting resins.
[0071] Examples of the thermoplastic resin include various known thermoplastic resins, such as olefin polymers (e.g., polymers similar to those listed in the section on uses of the present modified product), polyesters (e.g., polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate), polyphenylene sulfide, polyamides (e.g., nylon-6, nylon-66, polymetaxylene adipamide), polyvinyl chloride, polyvinylidene chloride, polymethyl methacrylate, polyvinyl acetate, thermoplastic polyimide, polyvinyl alcohol, polyacrylonitrile, polyacetal, polycarbonate, polystyrene, thermoplastic polyurethane, biodegradable plastics (e.g., aliphatic polyesters such as polylactic acid), modified fluororesins, and biomass plastics (e.g., starch resins).
[0072] Examples of the thermosetting resin include various known thermosetting resins, such as epoxy resin, unsaturated polyester resin, phenol resin, urea-melamine resin, polyurethane resin, silicone resin, and polyimide.
[0073] The base layer (B) is preferably a layer having a polar group. When such a substrate layer (B) is used, the carbodiimide group in the modified product reacts with the polar group in the substrate layer (B) and is bonded to the modified product, thereby improving the adhesion between the layer (A) and the substrate layer (B). In this case, the layer (A) contains not only the modified product but also the modified product in which the carbodiimide group has reacted with the polar group in the substrate layer (B).
[0074] Examples of the polar group include a carboxy group, a hydroxy group, an amino group, an ester group, and a carbonyl group. Among these, a carboxy group and a hydroxy group are preferable. The base layer (B) may have two or more kinds of polar groups. For example, polyesters usually have a carboxyl group or a hydroxyl group at the terminals, polyphenylene sulfide usually has a carboxyl group at the terminals, and glass and metals usually have a hydroxyl group.
[0075] The layer containing a thermoplastic resin or a thermosetting resin or the layer made of these may contain, as necessary, an additive that is usually added to a resin and used, such as a phenol-based antioxidant, a phosphorus-based antioxidant, a sulfur-based antioxidant, a metal compound, or a metal salt of a higher fatty acid, within a range that does not impair the object of the present invention.
[0076] The laminate is not limited to a laminate film (sheet) shape, but may be any of various known shapes such as a hollow container, a cup, a tray, and the like.
[0077] The method for producing the laminate varies depending on the shape, size, required properties, etc. of the final product, and is not particularly limited. For example, the following methods can be mentioned. (1) A method of heat fusion using a calendar roll molding machine, a compression molding machine, etc. at a temperature equal to or higher than the melting temperature of at least one of the preformed layer (A) and the base layer (B). (2) A method in which a preformed layer (A) or a substrate layer (B) is heat-sealed to another layer which is being extruded or calendared. (3) When a layer containing a thermoplastic resin is used as the base layer (B), the layer (A) and the base layer (B) are extruded simultaneously using a multilayer extrusion molding machine to perform heat fusion (co-extrusion molding). (4) When a layer containing a thermoplastic resin is used as the base layer (B), a method in which the molten material for forming layer (A) and the molten material for forming base layer (B) are injected into a mold with different injection timing (e.g., two-layer injection molding, sandwich injection molding).
[0078] The laminate has a layer (A) containing the present modified product or the olefin-based resin composition, and therefore has excellent interlayer adhesion, and even if the laminate is heat-treated at a high temperature of, for example, 200 to 250°C, a laminate in which the interlayer adhesion strength is not easily reduced can be obtained. Furthermore, since the laminate has a layer (A) containing the present modified product or the olefin-based resin composition, it has excellent interlayer adhesion and, for example, when heat-sealing at 230°C, a layer with high adhesive strength can be formed even if the heat-sealing time is short, preferably 20 seconds or less, more preferably 10 seconds or less, and even more preferably 5 seconds or less. EXAMPLES
[0079] Hereinafter, one embodiment of the present invention will be described with reference to examples, but the present invention is not limited to these examples.
[0080] <Method of measuring graft ratio> The graft ratio was measured using a Bruker Biospin AVANCEIIIcryo-500 nuclear magnetic resonance spectrometer (500MHz) under the following measurement conditions: measurement solvent: 1,1,2,2-tetrachloroethane-d2, measurement temperature: 120°C, spectrum width: 20 ppm, pulse repetition time: 7.0 seconds, pulse width: 5.00 μsec (45° pulse). 1 The H-NMR spectrum was measured. The graft ratio was calculated from the peak intensity ratio of the protons of the hydrocarbon group bonded to the carbodiimide group present at 3.0 ppm to 4.0 ppm and the protons bonded to all the hydrocarbon groups originating from the raw polymer present at 0.3 ppm to 2.5 ppm in the obtained spectrum.
[0081] [Example 1] 25.0g of LLDPE (base polymer, comonomer type: 1-hexene, comonomer amount: 1.6% by mass, Mw: 164,000, Mn: 63,000, Mw / Mn: 2.60) and 150mL of toluene were charged into a 1L autoclave, and the inside of the autoclave was replaced with nitrogen and then sealed. Then, the internal temperature of the autoclave was raised to 140°C, and while maintaining the temperature, 28.1mmol of vinylphenylcyclohexylcarbodiimide and 2.2mmol of dicumyl peroxide were fed over 2 hours while stirring at a stirring speed of 400 rpm using a double anchor blade. After stirring for another 2 hours, 250mL of toluene was fed over 15 minutes to dilute the reaction liquid.
[0082] The autoclave was then cooled to 50°C, and the pressure was released, after which the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated two more times. The solid content after the third filtration was dried in a vacuum dryer at 70° C. for 10 hours to obtain a graft polymer (P-1). The yield of the graft polymer (P-1) was 25.71 g (mass increase: 0.71 g). The graft ratio was 2.7 mass%.
[0083] [Example 2] In a 500mL glass vessel, 25.0g of PP (base polymer, propylene homopolymer, Mw: 313,000, Mn: 70,800, Mw / Mn: 4.43) and 110mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Then, the inside temperature of the vessel was raised to 120°C, and while maintaining the temperature, 28.1mmol of vinylphenylcyclohexylcarbodiimide and 2.2mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene were fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor impeller. After further stirring for 3 hours, 200mL of xylene was fed to dilute the reaction liquid.
[0084] After that, the inside temperature of the vessel was cooled to 50°C, and the pressure was released, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.13 g of a graft polymer (P-2). The graft rate was 1.5% by mass.
[0085] [Example 3] In a 500mL glass vessel, 25.0g of LLDPE (the same polymer as the base polymer used in Example 1) and 110mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120°C, and while maintaining the temperature, 14mmol of vinylphenylphenylcarbodiimide was charged, and then 1.1mmol of tert-butylperoxyisopropylmonocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 200mL of xylene was fed to dilute the reaction liquid.
[0086] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.62 g of a graft polymer (P-3). The graft rate was 3.4% by mass.
[0087] [Example 4] In a 500mL glass vessel, 12.5g of 4-methylpentene homopolymer (base polymer, Mw: 671,000, Mn: 297,000, Mw / Mn: 2.26) and 50mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120°C, and while maintaining the temperature, 14mmol of vinylphenylcyclohexylcarbodiimide was charged, and then 1.1mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor impeller. After further stirring for 3 hours, 150mL of xylene was fed to dilute the reaction liquid.
[0088] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 12.71 g of a graft polymer (P-4). The graft rate was 1.4% by mass.
[0089] [Example 5] In a 500 mL glass vessel, 25.0 g of EBR (base polymer, DF710, manufactured by Mitsui Chemicals, Inc.) and 110 mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120° C., and while maintaining the temperature, 14 mmol of vinylphenylcyclohexylcarbodiimide was charged, and then 1.1 mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, manufactured by NOF Corp.) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor impeller. Then, stirring was continued for another 3 hours.
[0090] Then, 400 mL of acetone was added to the reaction solution, and the mixture was stirred for 10 minutes. The mixture was then filtered to separate the solids and the filtrate. The process of adding acetone to the solids and filtering them was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 26.08 g of a graft polymer (P-5). The graft rate was 3.3% by mass.
[0091] [Example 6] In a 500mL glass vessel, 25.0g of LLDPE (the same polymer as the base polymer used in Example 1) and 110mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120°C, and while maintaining the temperature, 33.4mmol of ethylphenylcarbodiimide methacrylate was charged, and then 2.2mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was dropped over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 200mL of xylene was fed to dilute the reaction liquid.
[0092] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.87 g of a graft polymer (P-6). The graft rate was 2.4% by mass.
[0093] [Example 7] In a 500 mL glass container, 17.0 g of LLDPE (the same polymer as the base polymer used in Example 1) and 78 mL of xylene were charged, and the inside of the container was replaced with nitrogen. Thereafter, the inside temperature of the container was raised to 120° C., and while maintaining the temperature, 24.5 mmol of ethylcyclohexylcarbodiimide methacrylate was charged, and then 1.68 mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10 mL of xylene was dropped over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. After further stirring for 3 hours, 150 mL of xylene was charged to dilute the reaction liquid.
[0094] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 17.49 g of a graft polymer (P-7). The graft rate was 3.0% by mass.
[0095] [Example 8] In a 500mL glass vessel, 25.0g of LLDPE (the same polymer as the base polymer used in Example 1) and 110mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120°C, and while maintaining the temperature, 35.0mmol of ethyl methacrylate-tert-butylcarbodiimide was charged, and then 2.2mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 200mL of xylene was fed to dilute the reaction liquid.
[0096] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.49 g of a graft polymer (P-8). The graft rate was 1.7% by mass.
[0097] [Example 9] In a 500mL glass vessel, 17.1g of LLDPE (the same polymer as the base polymer used in Example 1) and 73mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120°C, and while maintaining the temperature, 23.8mmol of ethyl methacrylate-n-butylcarbodiimide was charged, and then 1.6mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 150mL of xylene was fed to dilute the reaction liquid.
[0098] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 17.38 g of a graft polymer (P-9). The graft rate was 1.6% by mass.
[0099] [Example 10] In a 500mL glass vessel, 14.0g of LLDPE (the same polymer as the base polymer used in Example 1) and 57mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120°C, and while maintaining the temperature, 19.0mmol of ethyl methacrylate-p-chlorophenylcarbodiimide was charged, and then 1.3mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 150mL of xylene was fed to dilute the reaction liquid.
[0100] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 14.43 g of a graft polymer (P-10). The graft rate was 2.8% by mass.
[0101] [Example 11] In a 500mL glass vessel, 17.0g of LLDPE (the same polymer as the base polymer used in Example 1) and 73mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120°C, and while maintaining the temperature, 22.5mmol of ethyl methacrylate-p-methoxyphenylcarbodiimide was charged, and then 1.5mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 150mL of xylene was fed to dilute the reaction liquid.
[0102] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 17.37 g of a graft polymer (P-11). The graft rate was 1.6% by mass.
[0103] [Example 12] In a 500 mL glass container, 20.0 g of PP (the same polymer as the base polymer used in Example 2) and 86 mL of xylene were charged, and the inside of the container was replaced with nitrogen. Thereafter, the inside temperature of the container was raised to 120° C., and while maintaining the temperature, 22.6 mmol of ethyl phenyl carbodiimide methacrylate was charged, and then 9.2 mmol of tert-butyl peroxy isopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor blade. After further stirring for 3 hours, 200 mL of xylene was fed to dilute the reaction liquid.
[0104] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 19.89 g of a graft polymer (P-12). The graft rate was 1.5% by mass.
[0105] [Example 13] In a 500mL glass container, 19.0g of PP (the same polymer as the base polymer used in Example 2) and 81mL of xylene were charged, and the inside of the container was replaced with nitrogen. Thereafter, the inside temperature of the container was raised to 120°C, and while maintaining the temperature, 20mmol of ethylcyclohexylcarbodiimide methacrylate was charged, and then 9.2mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 200mL of xylene was fed to dilute the reaction liquid.
[0106] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 18.89 g of a graft polymer (P-13). The graft rate was 1.4% by mass.
[0107] [Example 14] In a 500mL glass container, 15.0g of PP (the same polymer as the base polymer used in Example 2) and 62mL of xylene were charged, and the inside of the container was replaced with nitrogen. Thereafter, the inside temperature of the container was raised to 120°C, and while maintaining the temperature, 22.1mmol of ethyl methacrylate-tert-butylcarbodiimide was charged, and then 9.2mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 150mL of xylene was fed to dilute the reaction liquid.
[0108] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 15.37 g of a graft polymer (P-14). The graft rate was 1.3% by mass.
[0109] [Example 15] In a 500mL glass container, 15.0g of PP (the same polymer as the base polymer used in Example 2) and 62mL of xylene were charged, and the inside of the container was replaced with nitrogen. Thereafter, the inside temperature of the container was raised to 120°C, and while maintaining the temperature, 17.8mmol of ethyl methacrylate-p-chlorophenylcarbodiimide was charged, and then 6.9mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 150mL of xylene was fed to dilute the reaction liquid.
[0110] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 14.60 g of a graft polymer (P-15). The graft rate was 1.6% by mass.
[0111] [Example 16] In a 500mL glass container, 20.0g of PP (the same polymer as the base polymer used in Example 2) and 86mL of xylene were charged, and the inside of the container was replaced with nitrogen. Thereafter, the inside temperature of the container was raised to 120°C, and while maintaining the temperature, 22.5mmol of ethyl methacrylate-p-methoxyphenylcarbodiimide was charged, and then 9.2mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor blade. After further stirring for 3 hours, 200mL of xylene was fed to dilute the reaction liquid.
[0112] After that, the inside temperature of the vessel was cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 20.30 g of a graft polymer (P-16). The graft rate was 1.6% by mass.
[0113] [Example 17] In a 500 mL glass vessel, 10.0 g of EBR (the same polymer as the base polymer used in Example 5) and 38 mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120° C., and while maintaining the temperature, 13.4 mmol of ethyl methacrylate-tert-butylcarbodiimide was charged, and then 0.9 mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10 mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor impeller. Then, stirring was continued for another 3 hours.
[0114] Then, 400 mL of acetone was added to the reaction solution, and the mixture was stirred for 10 minutes. The mixture was then filtered to separate the solids and the filtrate. The process of adding acetone to the solids and filtering them was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 18.91 g of a graft polymer (P-17). The graft rate was 4.1% by mass.
[0115] [Example 18] In a 500mL separable flask, 23g of LLDPE (the same polymer as the base polymer used in Example 1) and 100mL of xylene were charged, and the atmosphere in the separable flask was replaced with nitrogen, and then the internal temperature was raised to 120°C, and while maintaining the temperature, 30mmol of ethyl isopropyl carbodiimide methacrylate was charged, and then 2.0mmol of tert-butyl peroxy isopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor impeller. After further stirring for 3 hours, 200mL of xylene was fed to dilute the reaction liquid.
[0116] The internal temperature of the separable flask was then cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 23.54 g of a graft polymer (P-18). The graft rate was 1.7% by mass.
[0117] [Example 19] In a 500mL separable flask, 13.2g of PP (the same polymer as the base polymer used in Example 2) and 54mL of xylene were charged, and the atmosphere in the separable flask was replaced with nitrogen, and then the internal temperature was raised to 120°C, and while maintaining the temperature, 19.5mmol of ethyl isopropyl carbodiimide methacrylate was charged, and then 8.0mmol of tert-butyl peroxy isopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor impeller. After further stirring for 3 hours, 150mL of xylene was fed to dilute the reaction liquid.
[0118] The internal temperature of the separable flask was then cooled to 50°C, and the slurry-like reaction liquid was taken out. 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The stirred liquid was then filtered to separate the solid matter and the filtrate. The process from adding acetone to the solid matter obtained to filtering was repeated three more times. The solid content after the fourth filtration was dried in a vacuum dryer at 90° C. for 10 hours to obtain 13.29 g of a graft polymer (P-19). The graft rate was 1.7% by mass.
[0119] [Comparative Example 1] In a 500mL glass vessel, 25.0g of LLDPE (the same polymer as the base polymer used in Example 1) and 110mL of xylene were charged, and the inside of the vessel was replaced with nitrogen. Thereafter, the inside temperature of the vessel was raised to 120°C, 33.4mmol of glycidyl methacrylate was charged into the vessel, and then 2.21mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10mL of xylene was fed over 10 minutes while stirring at a stirring speed of 400rpm using a double anchor impeller. Then, stirring was continued for another 3 hours.
[0120] Then, 250 mL of xylene was added, and the temperature was raised again to 120°C, after which the internal temperature of the vessel was gradually cooled to 50°C. The reaction liquid was taken out, and 400 mL of acetone was added to the reaction liquid obtained, and the mixture was stirred for 10 minutes. The reaction liquid was then filtered, and separated into a solid content and a filtrate. The solid content obtained was washed three times with 400 mL of acetone, and the solid content after the fourth filtration was dried in a vacuum dryer at 70°C for 10 hours to obtain a graft polymer (CP-1). The yield of the obtained graft polymer (CP-1) was 25.95 g, and the graft ratio was 2.4 mass %.
[0121] [Comparative Example 2] In a 500 mL glass container, 25.0 g of PP (the same polymer as the base polymer used in Example 2) and 120 mL of xylene were charged, and the inside of the container was replaced with nitrogen. Thereafter, the inside temperature of the container was raised to 120° C., and while maintaining the temperature, 33.4 mmol of glycidyl methacrylate was charged, and then 11 mmol of tert-butylperoxyisopropyl monocarbonate (Perbutyl I, NOF Corp.) dissolved in 10 mL of xylene was dropped over 10 minutes while stirring at a stirring speed of 400 rpm using a double anchor impeller. Then, the mixture was further stirred for 3 hours.
[0122] Then, 200 mL of xylene was added, and the internal temperature of the container was gradually cooled to 50°C. The slurry-like reaction liquid was taken out, and 400 mL of acetone was added to the resulting reaction liquid, and the mixture was stirred for 10 minutes. The reaction liquid was then filtered, and separated into a solid fraction and a filtrate. The resulting solid fraction was washed three times with 400 mL of acetone to remove unreacted glycidyl methacrylate and homopolymers of glycidyl methacrylate. The obtained solid content was dried in a vacuum dryer at 90° C. for 10 hours to obtain 25.26 g of a graft polymer (CP-2). The graft ratio was 1.0% by mass.
[0123] [Example 20] 11 parts by mass of the graft polymer (P-1) produced in Example 1 and 89 parts by mass of LLDPE (the same polymer as the base polymer used in Example 1) were mixed using a Labo Plastomill at a temperature of 190°C, a screw rotation speed of 60 rpm, and a mixing time of 10 minutes, and then press-molded under conditions of a temperature of 180°C, a pressure of 4 MPa, a preheat time of 5 minutes, and a pressurization time of 3 minutes, and then quenched using a press molding machine set at 20°C to obtain an olefin-based resin composition C-1 (a press sheet having a thickness of 500 μm, a length of 80 mm, and a width of 80 mm). The obtained olefin resin composition C-1 had an MFR (190°C, 2.16 kg load) of 2.7 g / 10 min and a density of 0.903 g / cm 3 It was.
[0124] [Example 21] An olefin resin composition C-2 was obtained in the same manner as in Example 20, except that 12 parts by mass of the graft polymer (P-2) produced in Example 2 and 88 parts by mass of PP (the same polymer as the base polymer used in Example 2) were used. The obtained olefin resin composition C-2 had an MFR (190°C, 2.16 kg load) of 0.6 g / 10 min and a density of 0.893 g / cm 3 It was.
[0125] [Example 22] An olefin resin composition C-3 was obtained in the same manner as in Example 20, except that 12 parts by mass of the graft polymer (P-6) produced in Example 6 and 88 parts by mass of LLDPE (the same polymer as the base polymer used in Example 1) were used. The obtained olefin resin composition C-3 had an MFR (190°C, 2.16 kg load) of 2.93 g / 10 min and a density of 0.903 g / cm 3 It was.
[0126] [Example 23] An olefin resin composition C-4 was obtained in the same manner as in Example 20, except that 10 parts by mass of the graft polymer (P-7) produced in Example 7 and 90 parts by mass of LLDPE (the same polymer as the base polymer used in Example 1) were used. The obtained olefin resin composition C-4 had an MFR (190°C, 2.16 kg load) of 3.1 g / 10 min and a density of 0.902 g / cm 3 It was.
[0127] [Example 24] An olefin resin composition C-5 was obtained in the same manner as in Example 20, except that 16 parts by mass of the graft polymer (P-8) produced in Example 8 and 84 parts by mass of LLDPE (the same polymer as the base polymer used in Example 1) were used. The obtained olefin resin composition C-5 had an MFR (190°C, 2.16 kg load) of 3.5 g / 10 min and a density of 0.902 g / cm 3 It was.
[0128] [Example 25] An olefin resin composition C-6 was obtained in the same manner as in Example 20, except that 17 parts by mass of the graft polymer (P-9) produced in Example 9 and 83 parts by mass of LLDPE (the same polymer as the base polymer used in Example 1) were used. The resulting olefin resin composition C-6 had an MFR (190° C., 2.16 kg load) of 2.73 g / 10 min.
[0129] [Example 26] An olefin resin composition C-7 was obtained in the same manner as in Example 20, except that 12 parts by mass of the graft polymer (P-10) produced in Example 10 and 88 parts by mass of LLDPE (the same polymer as the base polymer used in Example 1) were used.
[0130] [Example 27] An olefin resin composition C-8 was obtained in the same manner as in Example 20, except that 21 parts by mass of the graft polymer (P-11) produced in Example 11 and 79 parts by mass of LLDPE (the same polymer as the base polymer used in Example 1) were used.
[0131] [Example 28] An olefin resin composition C-9 was obtained in the same manner as in Example 20, except that 12 parts by mass of the graft polymer (P-12) produced in Example 12 and 88 parts by mass of PP (the same polymer as the base polymer used in Example 2) were used. The obtained C-9 had an MFR (190° C., 2.16 kg load) of 1.0 g / 10 min.
[0132] [Example 29] An olefin resin composition C-10 was obtained in the same manner as in Example 20, except that 14 parts by mass of the graft polymer (P-13) produced in Example 13 and 86 parts by mass of PP (the same polymer as the base polymer used in Example 2) were used. The resulting olefin resin composition C-10 had an MFR (190° C., 2.16 kg load) of 1.8 g / 10 min.
[0133] [Example 30] An olefin resin composition C-11 was obtained in the same manner as in Example 20, except that 13 parts by mass of the graft polymer (P-14) produced in Example 14 and 87 parts by mass of PP (the same polymer as the base polymer used in Example 2) were used. The obtained olefin resin composition C-11 had an MFR (190°C, 2.16 kg load) of 2.0 g / 10 min and a density of 0.892 g / cm 3 It was.
[0134] [Example 31] An olefin resin composition C-12 was obtained in the same manner as in Example 20, except that 13 parts by mass of the graft polymer (P-15) produced in Example 15 and 87 parts by mass of PP (the same polymer as the base polymer used in Example 2) were used.
[0135] [Example 32] An olefin resin composition C-13 was obtained in the same manner as in Example 20, except that 13 parts by mass of the graft polymer (P-16) produced in Example 16 and 87 parts by mass of PP (the same polymer as the base polymer used in Example 2) were used.
[0136] [Comparative Example 3] An olefin resin composition CC-1 was obtained in the same manner as in Example 20, except that 10 parts by mass of the graft polymer (CP-1) produced in Comparative Example 1 and 90 parts by mass of LLDPE (the same polymer as the base polymer used in Example 1) were used. The obtained olefin resin composition CC-1 had an MFR (190°C, 2.16 kg load) of 3.2 g / 10 min and a density of 0.902 g / cm 3 It was.
[0137] [Comparative Example 4] An olefin resin composition CC-2 was obtained in the same manner as in Example 20, except that 12 parts by mass of the graft polymer (CP-2) produced in Comparative Example 2 and 88 parts by mass of PP (the same polymer as the base polymer used in Example 2) were used. The obtained olefin resin composition CC-2 had an MFR (190°C, 2.16 kg load) of 1.9 g / 10 min and a density of 0.892 g / cm 3 It was.
[0138] <Adhesion evaluation> -Press sheet production Each of the graft polymers obtained in Examples 1 and 3 and Comparative Example 1 was press molded under conditions of a temperature of 180°C, a pressure of 4 MPa, a preheating time of 5 minutes, and a pressurizing time of 3 minutes, and then quenched in a press molding machine set at 20°C to produce a pressed sheet having a thickness of 500 μm, a length of 80 mm, and a width of 80 mm.
[0139] -Laminate fabrication As the base layer, a polyethylene terephthalate (PET) sheet (product name: Lumirror T60, manufactured by Toray Industries, Inc.) having a thickness of 50 μm, a length of 80 mm and a width of 80 mm was used. A PET sheet, a press sheet and a PET sheet were stacked in that order, and the stack was sandwiched between Teflon (registered trademark) sheets. The stack was then heat sealed for 5, 10 or 30 seconds using a heat sealer with the press plate (lower) temperature set to 230°C and the press plate (upper) temperature set to 230°C or 250°C to produce a three-layer laminate.
[0140] Peel test For the prepared laminate, the upper PET sheet (the PET sheet on the (upper) side of the press plate) and the press sheet were T-peeled at a peeling atmosphere temperature of 23°C, a peeling speed of 300 mm / min, and a peel width of 15 mm to measure the peel strength between the PET sheet and the press sheet. The results are shown in Table 1. Note that because the adhesive strength is strong, the case where the PET sheet itself breaks, rather than the interface between the PET sheet and the press sheet, is indicated as "PET resin break".
[0141] [Table 1]
[0142] <Adhesion evaluation> As the base layer, a polyethylene terephthalate (PET) sheet (product name: Lumirror T60, manufactured by Toray Industries, Inc.) having a thickness of 50 μm, a length of 80 mm and a width of 80 mm was used. A PET sheet, a press sheet (the olefin resin composition obtained in Examples 20 to 32 or Comparative Examples 3 to 4) and a PET sheet were stacked in that order, and the stack was sandwiched between Teflon (registered trademark) sheets. The stack was then heat-sealed for 3 seconds using a heat sealer with the upper and lower press plate temperatures set to 200°C or 230°C to produce a three-layer laminate. The laminate thus produced was subjected to a peel test in the same manner as described above, and the results are shown in Table 2.
[0143] [Table 2]
Claims
1. A graft-modified product of at least one base polymer selected from polyolefins with a carbodiimide monomer having a carbodiimide group and a polymerizable double bond, The graft ratio in the graft modified product is 0.3 to 7 mass%. Graft modified material.
2. The graft modified substance according to claim 1, wherein the carbodiimide monomer is a carbodiimide monomer represented by the following formula (1): 【Chemistry 1】 In formula (1), R 1 is a hydrogen atom or a methyl group, R 2 is a hydrocarbon group which may have a substituent.
3. The R 2 The graft modified product according to claim 2, wherein is an aliphatic hydrocarbon group having 4 to 20 carbon atoms and containing an alicyclic ring.
4. The graft modified substance according to claim 1, wherein the carbodiimide monomer is a carbodiimide monomer represented by the following formula (2): 【Chemistry 2】 In formula (2), R 3 is a hydrogen atom or a methyl group, R 4 represents a hydrocarbon group which may have a substituent, and m is an integer of 2 or more.
5. The R 3 is a methyl group, R 4 The graft modified product according to claim 4 , wherein R is a branched and non-ring alkyl group, and m is 2.
6. The graft modified product according to any one of claims 1 to 5, wherein the base polymer is a polymer that does not have at least one active hydrogen-containing group selected from a carboxy group, an acid anhydride group, an amino group, a hydroxyl group, and a thiol group.
7. The graft modified product according to any one of claims 1 to 6, wherein the polyolefin is at least one selected from the group consisting of ethylene-based polymers and propylene-based polymers.
8. An olefin-based resin composition comprising the graft modified product according to any one of claims 1 to 7 and one or more olefin-based polymers.
9. An adhesive comprising the graft modified product according to any one of claims 1 to 7 or the olefin-based resin composition according to claim 8.
10. A laminate comprising: a layer (A) selected from a layer containing the graft modified product according to any one of claims 1 to 7 and a layer containing the olefin-based resin composition according to claim 8; and a base layer (B).
11. The laminate according to claim 10 , wherein the base material layer (B) is a layer having a polar group.
12. The laminate according to claim 11, wherein the polar group is a carboxy group or a hydroxy group.
Citation Information
Patent Citations
Modified polyolefin
JP1994145260A
Carbodiimide compound and polymer thereof, gelatinous composition, ionic conductive composition, electrochemical element, and surface-modified substrate
JP2005048127A