Heat Shrink Connectors

A heat-shrinkable tube using ethylene-tetrafluoroethylene copolymer addresses heat damage and sealing issues for high-heat-resistant wires by controlling storage modulus and melting point, ensuring reliable and uniform shrinkage and sealing performance.

JP7590534B2Active Publication Date: 2024-11-26SUMITOMO ELECTRIC FINE POLYMER INC +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023211529
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-24
Filing Date
2023-12-14
Publication Date
2024-11-26
Estimated Expiration
2042-01-21

Smart Images

  • Figure 0007590534000014
    Figure 0007590534000014
  • Figure 0007590534000015
    Figure 0007590534000015
  • Figure 0007590534000016
    Figure 0007590534000016
Patent Text Reader

Abstract

To provide a heat-shrinkable tube with excellent heat-resistance and heat-shrinking property for use as a heat-shrinkable connecting component for a highly heat-resistant insulated wire.SOLUTION: There is provided a heat-shrinkable tube that contains an ethylene-tetrafluoroethylene copolymer as a main component, and has a melting point of 210°C or more and 250°C or less, and a storage modulus at 250°C or more and 280°C or less of 0.8 MPa or more and 2.8 MPa or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to heat shrink connectors.

[0002] This application claims priority to Japanese Application No. 2021-27985, filed on February 24, 2021, and incorporates by reference all of the contents of the above-mentioned Japanese application. [Background technology]

[0003] Wire bundles consisting of multiple insulated wires bound together with connecting bands or adhesive tape are used in wire harnesses for aircraft, electronic components, railway vehicles, automobiles, and motorcycles. Each insulated wire is generally constructed by covering a bundle of wires made of one or more conductors such as copper alloys with an insulator. The joints (joints) at the ends and middle of this wire bundle expose the wires, requiring electrical insulation, mechanical protection, and waterproofing. Heat-shrinkable tubing is used for electrical insulation, mechanical protection, and waterproofing. Heat-shrinkable connectors, equipped with heat-shrinkable tubing that is heat-shrinkable in the radial direction, are particularly used for waterproofing. When the heat-shrinkable tubing included in these connectors is wrapped around the connection between insulated wires and heated, it shrinks to the shape of the connection and adheres tightly due to its shape memory effect, protecting the connection between electric wires, pipes, etc.

[0004] A suitable material for such heat-shrinkable tubing is polytetrafluoroethylene (PTFE), which has excellent heat resistance, mechanical strength, and a low coefficient of friction. However, since PTFE has a high storage modulus and is not easy to mold, a technology has been proposed in which the PTFE tube is crosslinked by irradiating it with radiation, making the molding process easier (see Patent Document 1). Furthermore, polyvinylidene fluoride (PVDF), which has a low melting point and excellent moldability, is also widely used as a material for heat-shrinkable tubing. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2010 / 038800 Summary of the Invention

[0006] A heat-shrinkable tube according to one embodiment of the present disclosure contains an ethylene-tetrafluoroethylene copolymer as a main component, has a storage modulus of 0.8 MPa or more and 2.8 MPa or less at 250°C or more and 280°C or less, and has a melting point of 210°C or more and 250°C or less.

[0007] A method for producing a heat-shrinkable tube according to another embodiment of the present disclosure is a method for producing a heat-shrinkable tube, comprising the steps of extruding a resin composition containing an ethylene-tetrafluoroethylene copolymer as a main component into a tubular shape, crosslinking the tube formed by the extrusion molding step by irradiation, heating the tube after the crosslinking step at a temperature of 250°C or more and 280°C or less, and expanding the tube by increasing the pressure inside the tube by 50 kPa or more higher than the pressure outside the tube, wherein the heat-shrinkable tube has a storage modulus of 0.8 MPa or more and 2.8 MPa or less at 250°C or more and a melting point of 210°C or more and 250°C or less. [Brief explanation of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic perspective view showing a heat-shrinkable tube according to an embodiment of the present disclosure. [Figure 2] FIG. 2 is a schematic perspective view showing a heat-shrinkable connecting component according to one embodiment of the present disclosure. [Figure 3] FIG. 3 is a schematic perspective view showing a heat-shrinkable connecting part according to another embodiment of the present disclosure. [Figure 4] FIG. 4 is a schematic perspective view showing a heat-shrinkable connecting part according to another embodiment of the present disclosure. [Figure 5] FIG. 5 is a schematic perspective view showing a heat-shrinkable connecting part according to another embodiment of the present disclosure. [Figure 6] FIG. 6 is a schematic perspective view showing a heat-shrinkable connecting part according to another embodiment of the present disclosure. [Figure 7]FIG. 7 is a schematic diagram illustrating a state before conductors exposed from two insulated wires are inserted into a heat-shrinkable connecting component according to an embodiment of the present disclosure. [Figure 8] FIG. 8 is a schematic diagram illustrating a state in which the connection portion of two insulated wires is covered with a heat-shrinkable connecting component according to an embodiment of the present disclosure. [Figure 9] FIG. 9 is a schematic diagram illustrating a state in which a heat-shrinkable connecting component according to an embodiment of the present disclosure has started to heat-shrink. [Figure 10] FIG. 10 is a schematic diagram illustrating a state in which the sealant of the heat-shrinkable connecting part according to an embodiment of the present disclosure is melted. [Figure 11] FIG. 11 is a schematic diagram illustrating a state in which the solder material of the heat-shrinkable connecting part according to an embodiment of the present disclosure is melted. DETAILED DESCRIPTION OF THE INVENTION

[0009] [Problem to be solved by this disclosure] Because PTFE has a melting point of 327°C, it is highly susceptible to damage during shrinkage of heat-shrinkable tubing, potentially damaging the insulation layer of high-heat-resistant insulated wires containing ethylene-tetrafluoroethylene copolymers or silicone. Heat-shrinkable connectors for insulated wires must not only protect the connections but also provide high levels of waterproofing to prevent water from entering the connections. Furthermore, because heat-shrinkable tubing shrinks at temperatures above its melting point, the use of PVDF, which has a melting point of 160°C, may result in insufficient reliability in applications requiring higher heat resistance. Thus, heat-shrinkable tubing used in heat-shrinkable connectors for high-heat-resistant insulated wires must possess high heat resistance and waterproofing capabilities while also being able to shrink without causing thermal damage to the insulated wires it covers.

[0010] The present disclosure has been made in light of the above circumstances, and aims to provide a heat-shrinkable tube that has excellent heat resistance and heat-shrinkability and is suitable for use as a heat-shrinkable connecting part for highly heat-resistant insulated electric wires.

[0011] [Effects of this disclosure] According to the present disclosure, a heat-shrinkable tube having excellent heat resistance and heat-shrinkability can be provided for use as a heat-shrinkable connecting part for highly heat-resistant insulated electric wires.

[0012] [Description of the embodiments of the present disclosure] First, embodiments of the present disclosure will be listed and described.

[0013] A heat-shrinkable tube according to one embodiment of the present disclosure is primarily composed of ethylene-tetrafluoroethylene copolymer (ETFE), has a storage modulus of 0.8 MPa or more and 2.8 MPa or less at 250°C or more and 280°C or less, and has a melting point of 210°C or more and 250°C or less.

[0014] The heat-shrinkable tubing, which contains an ethylene-tetrafluoroethylene copolymer as its main component, allows for easy control of its melting point and storage modulus above the melting point. The heat-shrinkable tubing has a melting point between 210°C and 250°C, ensuring heat resistance and suppressing thermal damage to the object being covered. Furthermore, the storage modulus between 250°C and 280°C is between 0.8MPa and 2.8MPa, providing excellent deformability when heated above the melting point and facilitating expansion (diameter expansion) during manufacturing. Furthermore, the wall thickness distribution and length change rate during shrinkage can be controlled within a favorable range, providing excellent shrinkability, allowing the tubing to shrink to its original shape. Uniform shrinkage along the length prevents end face tilt during shrinkage. Therefore, the heat-shrinkable tubing offers excellent heat resistance and heat-shrinkability for use as a heat-shrinkable connector for highly heat-resistant insulated electric wires whose insulating layer contains ethylene-tetrafluoroethylene copolymer, silicone, or the like. Furthermore, since the heat-shrinkable tube of the present invention is a single-layer tube in which the wall thickness deviation rate and length change rate can be controlled within a good range, it does not encounter the manufacturing efficiency and cost issues that arise with conventional two-layer types that have a fluid adhesive layer on the inside, and it can suppress the occurrence of gaps between the tube and the object to be covered and have good shrinkage properties.

[0015] The "major component" of the heat-shrinkable tube refers to the component with the highest content, which accounts for 95% by mass or more of the total mass of the heat-shrinkable tube and 98% by mass or more of the total mass of the resin components. The "storage modulus" is a value measured in accordance with the dynamic mechanical property testing method described in JIS-K7244-4 (1999), and is a value measured using a viscoelasticity measuring device at the above temperature and frequency under the conditions of tensile mode and 0.08% strain. The viscoelasticity measuring device can be, for example, the "DVA-220" manufactured by IT Instrument & Control Co., Ltd.

[0016] In the heat-shrinkable tube, the fluorine content in the ethylene-tetrafluoroethylene copolymer is preferably 58% by mass or more and 62% by mass or less. By setting the fluorine content in the ethylene-tetrafluoroethylene copolymer within this range, the melting point and the storage modulus above the melting point of the heat-shrinkable tube can be controlled within appropriate ranges.

[0017] The ratio n / m of the number of tetrafluoroethylene units n to the number of ethylene units m in the ethylene-tetrafluoroethylene copolymer is preferably 1.02 or more and 1.20 or less. When the ratio n / m of the number of tetrafluoroethylene units n to the number of ethylene units m is in the above range, the melting point and the storage modulus at temperatures above the melting point of the heat-shrinkable tube can be controlled within appropriate ranges.

[0018] The heat-shrinkable tube preferably has a storage modulus of 500 MPa or more and 900 MPa or less at 25° C. When the storage modulus at 25° C. is within the above range, the strength and flexibility of a heat-shrinkable connecting part in which the heat-shrinkable tube is used can be maintained within a favorable range.

[0019] The arithmetic mean roughness Ra of the surface is preferably 0.1 μm or more and 2.0 μm or less. By having the arithmetic mean roughness Ra in this range, visibility of the inside of the heat-shrinkable tube can be ensured and infrared absorption during infrared (IR) heating during the manufacturing process of the heat-shrinkable tube can be improved. The arithmetic mean roughness Ra is a value measured in accordance with JIS-B0601 (2013).

[0020] The heat-shrinkable tube preferably has a transmittance of 90.0% to 99.0% for infrared rays with a wavelength of 1 μm. By setting the infrared transmittance within the above range, the heating efficiency in the manufacturing process of the heat-shrinkable tube can be improved. Furthermore, the shrink behavior of heat-shrinkable connecting parts using the heat-shrinkable tube can be improved. The infrared transmittance can be measured using a spectrophotometer UV-3600 manufactured by Shimadzu Corporation.

[0021] A heat-shrinkable connection part according to another aspect of the present disclosure is a heat-shrinkable connection part for connecting insulated electric wires whose wires are covered with an insulating layer, and includes the heat-shrinkable tube and a pair of sealing portions disposed on the inner circumferential surface of both ends of the heat-shrinkable tube. Because the heat-shrinkable connection part includes the heat-shrinkable tube, the heat-shrinkable connection part has good shrinkage performance, sealing properties, and heat resistance as a heat-shrinkable connection part.

[0022] The sealing material constituting the sealing portion preferably has a shear viscosity of 1000 Pa·s or more and 2000 Pa·s or less at 250°C and a shear rate of 100 / s. Having a shear viscosity of 1000 Pa·s or more and 2000 Pa·s or less at 250°C and a shear rate of 100 / s reduces the likelihood of gaps forming during shrinkage of the heat-shrinkable tubing, improving the sealing properties of the heat-shrinkable connecting part. The shear viscosity can be measured using a rotational rheometer ("MCR302" manufactured by Anton Paar) to evaluate the shear viscosity at a predetermined temperature and shear rate.

[0023] The sealing material constituting the sealing portion preferably has a shear viscosity of 7000 Pa·s or more and 70000 Pa·s or less at 215°C and a shear rate of 0.01 / s. When the sealing material constituting the sealing portion has a shear viscosity of 7000 Pa·s or more and 70000 Pa·s or less at 215°C and a shear rate of 0.01 / s, the sealing material has appropriate fluidity, thereby improving sealing properties.

[0024] The heat-shrinkable connecting part preferably further comprises a solder part disposed on the inner circumferential surface of the heat-shrinkable tube between the pair of sealing parts, thereby further improving the connectivity between the insulated wires.

[0025] In the heat-shrinkable connecting component, it is preferable that the melting point of the solder material constituting the solder portion is 210°C or higher and 240°C or lower, and the softening point of the sealing material is 80°C or higher and 170°C or lower. When the melting point of the solder material and the softening point of the sealing material are within the above ranges, the heat-shrinkable tube, the solder material, and the sealing material can be combined to improve the heat resistance, sealing properties, and insulated wire connectivity of the heat-shrinkable connecting component. Here, the "softening point" refers to the temperature at which the thickness is reduced by 50% when heated while being pressurized at a pressure of 5 kPa using a thermomechanical analyzer.

[0026] The melting point of the sealing material is preferably 110° C. or higher and 170° C. or lower. When the melting point of the sealing material is 110° C. or higher and 170° C. or lower, the sealing material has better fluidity and is more effective in filling gaps, thereby further improving the sealing properties.

[0027] In the heat-shrinkable connecting part, the transmittance of the sealing material for infrared rays with a wavelength of 1 μm is preferably 1.0% or more and 30.0% or less. When the transmittance of the sealing material for infrared rays with a wavelength of 1 μm is in the above range, the infrared absorption of the heat-shrinkable connecting part during infrared heating can be improved, and good heat-shrink behavior of the heat-shrinkable connecting part can be obtained.

[0028] A method for producing a heat-shrinkable tube according to another embodiment of the present disclosure includes the steps of extruding a resin composition containing an ethylene-tetrafluoroethylene copolymer as a main component into a tubular shape, crosslinking the tube formed by the extrusion molding step by irradiation, heating the tube after the crosslinking step at a temperature of 250°C or higher and 280°C or lower, and expanding the tube by increasing the pressure inside the tube by 50 kPa or more higher than the pressure outside the tube, wherein the heat-shrinkable tube has a storage modulus of 0.8 MPa or higher and 2.8 MPa or lower at 250°C or higher and a melting point of 210°C or higher and 250°C or lower. This method for producing a heat-shrinkable tube can produce a heat-shrinkable tube with excellent heat resistance and heat-shrinkability suitable for use as a heat-shrinkable connecting part for highly heat-resistant insulated electric wires.

[0029] A method for manufacturing a heat-shrinkable connecting part according to another aspect of the present disclosure includes the steps of providing sealing portions on the inner circumferential surface of both end sides of the heat-shrinkable tubing and fixing the sealing portions by shrinking the heat-shrinkable tubing, wherein the softening point of the sealing material constituting the sealing portions is 80° C. or higher and 170° C. or lower. According to this method for manufacturing a heat-shrinkable connecting part, the method includes the steps of providing a pair of sealing portions on the inner circumferential surface of both end sides of the heat-shrinkable tubing and shrinking and fixing the sealing portions, and since the softening point of the sealing material constituting the sealing portions is 80° C. or higher and 170° C. or lower, a heat-shrinkable connecting part with good shrinkability, sealing ability, and heat resistance can be easily manufactured.

[0030] [Details of the embodiments of the present disclosure] Hereinafter, a heat shrinkable tube according to an embodiment of the present disclosure will be described in detail with reference to the drawings as appropriate.

[0031] <Heat shrink tubing> A heat-shrinkable tube according to an embodiment of the present disclosure is used as a covering material for protecting an object to be covered. The heat-shrinkable tube is a tube that shrinks in diameter when heated. More specifically, the object to be covered is protected by inserting the heat-shrinkable tube into the heat-shrinkable tube, heating the tube on the object, and covering the object with the shrinkable heat-shrinkable tube.

[0032] The heat-shrinkable tube 1 in FIG. 1 is composed of a cylindrical single-layer base material layer. The heat-shrinkable tube 1 is used to cover, for example, the connection between objects to be covered, the terminals of wiring, metal pipes, etc., for protection, insulation, waterproofing, corrosion prevention, etc. The heat-shrinkable tube 1 is formed from a resin composition for forming heat-shrinkable tubes, and the heat-shrinkable tube 1 contains an ethylene-tetrafluoroethylene copolymer as its main component. By using an ethylene-tetrafluoroethylene copolymer as its main component, the heat-shrinkable tube 1 can easily control its melting point and its storage modulus above the melting point.

[0033] The lower limit of the fluorine content in the ethylene-tetrafluoroethylene copolymer is preferably 58% by mass, more preferably 59% by mass. On the other hand, the upper limit of the fluorine content is preferably 62% by mass, more preferably 61% by mass. If the fluorine content is below the lower limit, the melting point of the heat-shrinkable tube 1 may increase, resulting in a decrease in the storage modulus at or above the melting point. If the fluorine content exceeds the upper limit, the melting point of the heat-shrinkable tube 1 may decrease, resulting in an excessively high storage modulus at or above the melting point. By keeping the fluorine content within the above range, the melting point and the storage modulus at or above the melting point of the heat-shrinkable tube can be controlled within appropriate ranges. The fluorine content can be measured by gas ion chromatography.

[0034] The lower limit of the ratio n / m of the number of tetrafluoroethylene units n to the number of ethylene units m in the ethylene-tetrafluoroethylene copolymer is preferably 1.02, more preferably 1.03, and even more preferably 1.04. On the other hand, the upper limit of the ratio n / m of the number of tetrafluoroethylene units n to the number of ethylene units m is preferably 1.20, more preferably 1.15, and even more preferably 1.12. If the ratio n / m of the number of tetrafluoroethylene units n to the number of ethylene units m is less than the lower limit, the melting point of the heat-shrinkable tube 1 may be high, and the storage modulus at or above the melting point may be reduced. If the ratio n / m of the number of tetrafluoroethylene units n to the number of ethylene units m exceeds the upper limit, the melting point of the heat-shrinkable tube 1 may be low, and the storage modulus at or above the melting point may be too high. By setting the ratio n / m of the number of tetrafluoroethylene units n to the number of ethylene units m within the above range, the melting point and the storage modulus at or above the melting point of the heat-shrinkable tube can be controlled within appropriate ranges.

[0035] The lower limit of the storage modulus of the heat-shrinkable tube 1 at temperatures between 250°C and 280°C is 0.8 MPa, preferably 1.0 MPa, and more preferably 1.2 MPa. The upper limit of the storage modulus is 2.8 MPa, preferably 2.0 MPa, and more preferably 1.6 MPa. If the storage modulus at temperatures between 250°C and 280°C is less than the lower limit, the heat-shrinkable tube 1 may have insufficient strength and shrink performance (shape memory effect) at high temperatures. On the other hand, if the storage modulus exceeds the upper limit, the tube may be difficult to expand, making it difficult to suppress variation in the quality of the heat-shrinkable tube 1. Furthermore, the wall thickness deviation during expansion may be poor, resulting in large values ​​and variations in the rate of change in length of the heat-shrinkable tube during shrinkage. By setting the storage modulus within the above range, the heat-shrinkable tube 1 has excellent deformability when heated above its melting point, allowing for easy and reliable diameter expansion during the manufacturing process. This reduces variation in quality.

[0036] The lower limit of the storage modulus of the heat-shrinkable tube 1 at 25°C is preferably 500 MPa, more preferably 550 MPa, and even more preferably 600 MPa. Meanwhile, the upper limit of the storage modulus at 25°C is preferably 900 MPa, more preferably 850 MPa, and even more preferably 800 MPa. If the storage modulus at 25°C is below the lower limit, the strength of a heat-shrinkable connecting part using the heat-shrinkable tube 1 may be insufficient and the part may be prone to breakage. On the other hand, if the storage modulus at 25°C exceeds the upper limit, the flexibility of the heat-shrinkable connecting part may be reduced, making the heat-shrinkable connecting part prone to breakage during assembly. In order to maintain the shape of a heat-shrinkable connecting part during handling, such as assembly and shrinkage, the heat-shrinkable tube used is required to be semi-rigid. By having the storage modulus at 25°C of the heat-shrinkable tube 1 within the above range, the strength and flexibility of a heat-shrinkable connecting part using the heat-shrinkable tube 1 can be maintained within a favorable range.

[0037] The lower limit of the melting point of the heat shrinkable tube 1 is 210°C, and more preferably 215°C. If the melting point of the heat shrinkable tube 1 is below this lower limit, the heat shrinkable tube may soften or deform when used at high temperatures. On the other hand, the upper limit of the melting point of the heat shrinkable tube 1 is 250°C, and more preferably 240°C. If the melting point of the heat shrinkable tube 1 exceeds this upper limit, the shrinking temperature when the manufactured heat shrinkable tube 1 is heat-shrunk becomes high, which may cause heat damage to the object to be covered. By having a melting point within the above range, the heat shrinkable tube can ensure heat resistance and suppress heat damage to the object to be covered.

[0038] The lower limit of the arithmetic mean roughness Ra of the surface of the heat-shrinkable tube 1 is preferably 0.1 μm, more preferably 0.3 μm, and even more preferably 0.5 μm. If the arithmetic mean roughness Ra of the surface of the heat-shrinkable tube 1 is less than the above lower limit, there is a risk of insufficient heating due to low absorption when heated with an infrared heating device. On the other hand, the upper limit of the arithmetic mean roughness Ra is preferably 2.0 μm or less, more preferably 1.5 μm, and even more preferably 1.0 μm. If the arithmetic mean roughness Ra of the surface of the heat-shrinkable tube 1 exceeds the above upper limit, visible light scattering increases, reducing the visibility of the interior of the heat-shrinkable tube 1, which may make it difficult to check the degree of shrinkage of a heat-shrinkable connecting member including the heat-shrinkable tube 1. Heat-shrinkable connecting parts for insulated electric wires require visibility of the interior of the heat-shrinkable tube 1 in order to check the shrink state, melting of the solder material, the connection state of the electric wires, and the like. Therefore, transparency is required for heat-shrinkable tubes used in heat-shrinkable connecting parts. In the heat-shrinkable tube 1, since the arithmetic mean roughness Ra is within the above range, visibility of the inside of the heat-shrinkable tube 1 can be ensured and the infrared absorption during infrared (IR) heating during the manufacturing process of the heat-shrinkable tube 1 can be improved.

[0039] For the heat-shrinkable tube 1, the lower limit of the transmittance of infrared rays with a wavelength of 1 μm is preferably 90.0%, more preferably 92%. If the infrared transmittance of the heat-shrinkable tube 1 is less than the lower limit, the heat-shrinkable tube 1 may be heated preferentially during shrinkage of a heat-shrinkable connecting part using the heat-shrinkable tube 1, which may result in insufficient heating of the inside of the heat-shrinkable connecting part. On the other hand, the upper limit of the infrared transmittance is preferably 99.0%, more preferably 97%. If the infrared transmittance exceeds the upper limit, the heating efficiency may decrease when the heat-shrinkable tube 1 is heated by infrared heating. For the heat-shrinkable tube 1, if the transmittance of infrared rays with a wavelength of 1 μm is within the above range, the heating efficiency during the manufacturing process of the heat-shrinkable tube 1 can be improved, and the shrink behavior of a heat-shrinkable connecting part using the heat-shrinkable tube 1 can be improved.

[0040] The average inner diameter and average thickness of the heat-shrinkable tube 1 are appropriately selected depending on the application, etc. The average inner diameter of the heat-shrinkable tube 1 before heat-shrinking can be, for example, 1 mm or more and 60 mm or less. The average inner diameter of the heat-shrinkable tube 1 after heat-shrinking can be, for example, 25% or more and 65% or less of the average inner diameter before heat-shrinking. The average thickness of the heat-shrinkable tube 1 can be, for example, 0.1 mm or more and 5 mm or less.

[0041] The heat-shrinkable tube 1 preferably contains substantially no inorganic substances. Here, "substantially no inorganic substances" means that it does not contain any inorganic substances as fillers. The heat-shrinkable tube 1 may unavoidably contain a small amount of inorganic substances as impurities. The content of inorganic impurities in the heat-shrinkable tube 1 is preferably, for example, 5% by mass or less, and more preferably 1% by mass or less.

[0042] The heat-shrinkable tube 1 may contain other additives as needed. Examples of such additives include strength-retaining agents, antioxidants, flame retardants, copper inhibitors, cross-linking aids, colorants, thermal stabilizers, infrared absorbers, and ultraviolet absorbers. The content of the additives in the heat-shrinkable tube 1 is preferably less than 5% by mass, and more preferably less than 3% by mass. If the content of the additives is equal to or greater than the upper limit, the performance of the heat-shrinkable tube 1 may be more likely to vary.

[0043] This heat-shrinkable tube has excellent heat resistance and heat-shrinkability and can be used as a heat-shrinkable connecting part for highly heat-resistant insulated wires. The heat-shrinkable tube can be suitably used for protecting, insulating, waterproofing, and corrosion-preventing wires, such as insulated wires or cables. Specifically, the heat-shrinkable tube can be applied to wire splices and wire harnesses. The heat-shrinkable tube can be combined with a solder material and a sealing material to form a heat-shrinkable connecting part. It can also be combined with an adhesive layer and a crimp sleeve to form a crimp terminal.

[0044] <Heat-shrinkable connecting material> The heat-shrinkable connecting part is a heat-shrinkable connecting part for connecting insulated electric wires whose wires are covered with an insulating layer. Fig. 2 is a schematic perspective view showing a heat-shrinkable connecting part according to an embodiment of the present disclosure. As shown in Fig. 2, the heat-shrinkable connecting part 40 includes the heat-shrinkable tube 1 and a pair of sealing portions 3 disposed on the inner circumferential surface at both ends of the heat-shrinkable tube 1. The sealing portions 3 are made of a sealing material. The heat-shrinkable connecting part 40 includes the heat-shrinkable tube 1, and therefore has good shrinkage performance, sealing properties, and heat resistance as a heat-shrinkable connecting part.

[0045] It is preferable that the heat-shrinkable connecting part further comprises a solder portion disposed on the inner circumferential surface of the heat-shrinkable tube between the pair of sealing portions. By providing the heat-shrinkable connecting part with a solder portion disposed on the inner circumferential surface of the heat-shrinkable tube between the pair of sealing portions, the connectivity between insulated electric wires can be further improved. The heat-shrinkable connecting part 50 shown in Fig. 3 comprises the heat-shrinkable tube 1, a pair of sealing portions 3 disposed on the inner circumferential surface of the heat-shrinkable tube 1 at both ends, and a solder portion 2 disposed on the inner circumferential surface of the heat-shrinkable tube 1 between the pair of sealing portions 3. The solder portion 2 is made of a solder material.

[0046] The heat-shrinkable connection part can include an insulated grounding wire. A heat-shrinkable connection part 51 shown in FIG. 4 includes the heat-shrinkable tube 1, a pair of sealing portions 3 disposed on the inner circumferential surface of both ends of the heat-shrinkable tube 1, a solder portion 2 disposed on the inner circumferential surface of the heat-shrinkable tube 1 between the pair of sealing portions 3, and an insulated grounding wire 25. The insulated grounding wire 25 includes an element wire 23 and an insulating layer 24 covering the element wire 23. The heat-shrinkable connection part 51 includes the insulated grounding wire 25, which allows for easy grounding. The insulating covering of the insulated grounding wire may be made of resin or braided.

[0047] In this heat-shrinkable connecting component, the lower limit of the shear viscosity of the sealing material at 250°C and a shear rate of 100 / s is preferably 1000 Pa·s, more preferably 1100 Pa·s, and even more preferably 1200 Pa·s. If the shear viscosity of the sealing material at 250°C and a shear rate of 100 / s is lower than 1000 Pa·s, the heat-shrinkable tubing will soften and change shape during shrinkage, which may lead to gaps and reduced sealing performance. On the other hand, the upper limit of the shear viscosity of the sealing material at 250°C and a shear rate of 100 / s is preferably 2000 Pa·s, more preferably 1900 Pa·s, and even more preferably 1800 Pa·s. If the shear viscosity of the sealing material at 250°C and a shear rate of 100 / s is higher than 2000 Pa·s, the fluidity of the heat-shrinkable tubing during shrinkage will be low, which may reduce its gap-filling effect and reduce sealing performance.

[0048] In this heat-shrinkable connecting component, the shear viscosity of the sealing material at 250°C and a shear rate of 0.01 / s is preferably 3000 Pa·s or more and 40,000 Pa·s or less. If the shear viscosity at 250°C and a shear rate of 0.01 / s is lower than 3000 Pa·s, the sealing material may flow easily when maintained at high temperatures for long periods, making it difficult to maintain sealing performance. If the shear viscosity at 250°C and a shear rate of 0.01 / s is higher than 40,000 Pa·s, the sealing material's fluidity is low, reducing its gap-filling effect and potentially reducing sealing performance.

[0049] In this heat-shrinkable connecting component, the lower limit of the shear viscosity of the sealing material at 215°C and a shear rate of 0.01 / s is preferably 7000 Pa·s, more preferably 10000 Pa·s, and even more preferably 13000 Pa·s. If the shear viscosity of the sealing material at 215°C and a shear rate of 0.01 / s is lower than 7000 Pa·s, it may become more fluid when maintained at high temperatures for a long period of time, and its sealing properties may not be maintained. On the other hand, the upper limit of the shear viscosity of the sealing material at 215°C and a shear rate of 0.01 / s is preferably 70000 Pa·s, more preferably 60000 Pa·s, and even more preferably 50000 Pa·s. If the shear viscosity of the sealing material at 215°C and a shear rate of 0.01 / s is higher than 70000 Pa·s, its fluidity may be too low, making it unable to sufficiently fill gaps and resulting in reduced sealing properties.

[0050] In this heat-shrinkable connecting component, the shear viscosity of the sealing material at 215°C and a shear rate of 100 / s is preferably 1500 Pa·s or more and 2500 Pa·s or less. If the shear viscosity of the sealing material at 215°C and a shear rate of 100 / s is lower than 1500 Pa·s, the sealing material may soften and change shape during shrinkage of the heat-shrinkable tubing, making gaps more likely to occur, resulting in reduced sealing performance. If the shear viscosity of the sealing material at 215°C and a shear rate of 100 / s is higher than 2500 Pa·s, the sealing material may have reduced fluidity during shrinkage of the heat-shrinkable tubing, reducing its gap-filling effect and reducing sealing performance.

[0051] In the heat-shrinkable connecting part 50, the melting point of the solder material constituting the solder portion 2 is preferably 210°C or higher and 240°C or lower, and more preferably 220°C or higher and 230°C or lower. The softening point of the sealing material constituting the sealing portion 3 is preferably 80°C or higher and 170°C or lower, more preferably 100°C or higher and 150°C or lower, and even more preferably 110°C or higher and 140°C or lower. When the melting point of the solder material is 210°C or higher and 240°C or lower and the softening point of the sealing material is 80°C or higher and 170°C or lower, the combination of the heat-shrinkable tube 1 with the solder material and the sealing material can improve the heat resistance, sealing properties, and insulated wire connectivity of the heat-shrinkable connecting part 50.

[0052] In the heat-shrinkable connecting part 50, the melting point of the sealing material is preferably 110°C or higher and 170°C or lower, and more preferably 120°C or higher and 160°C or lower. When the melting point of the sealing material is 110°C or higher and 170°C or lower, the sealing material has better fluidity and is more effective at filling gaps, thereby further improving sealing performance. If the melting point is lower than 110°C, the sealing material softens during shrinkage of the tube and is more likely to change shape, which may lead to gaps and reduced sealing performance. If the melting point is higher than 170°C, the fluidity during shrinkage is low, which may reduce the gap-filling effect and reduce sealing performance.

[0053] Examples of the sealing material include polyolefin, fluororesin, and fluororubber. High-density polyethylene (HDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ethylene-vinyl acetate copolymer (EVA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methyl methacrylate copolymer (EMMA), polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (THV), vinylidene fluoride rubber (FKM), fluorinated ethylene propylene rubber (FEPM), and tetrafluoroethylene perfluorovinyl ether rubber (FFKM). The sealing material may also contain a colorant, antioxidant, infrared absorber, and lubricant.

[0054] The sealing material can be crosslinked to adjust the shear viscosity. The crosslinking can be performed by irradiation with electron beams such as electron beams or gamma rays, or by chemical crosslinking.

[0055] The sealing material may contain an inorganic filler to adjust the shear viscosity, such as silica, hydrotalcite, clay, or a combination thereof.

[0056] The content of the inorganic filler in the encapsulant is preferably more than 0.2 parts by mass, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, per 100 parts by mass of the resin of the encapsulant. If the content of the inorganic filler is 0.2 parts by mass or less, the effect of sufficiently improving the shear viscosity may not be obtained. On the other hand, the content of the inorganic filler in the encapsulant is preferably less than 5.0 parts by mass, more preferably 4.0 parts by mass or less, and even more preferably 3.5 parts by mass or less. If the content of the inorganic filler exceeds 5.0 parts by mass, the shear viscosity may become too high, resulting in a decrease in sealing properties.

[0057] The solder material may be a metal-based material. Examples of the solder material include Sn, Sb, Pb, Bi, Ag, Cu, Ni, In, Ge, P, and Zn, or a combination thereof. Among these, solder materials containing Sn-Ag, Sn-Cu, Sn-Sb, Sn-Pb, and Pb-In are preferred, as they allow the melting point of the solder material to be adjusted within a favorable range. The solder material may also contain flux.

[0058] In the heat-shrinkable connecting part 50, the transmittance of the sealing material to infrared rays with a wavelength of 1 μm is preferably 1.0% to 30.0%, more preferably 3% to 22%, and even more preferably 5% to 16%. If the infrared transmittance of the sealing material exceeds the upper limit, the heating of the sealing portion 3 during infrared heating is slowed, making it difficult for softening to proceed, which may result in poor sealing performance of the heat-shrinkable connecting part. On the other hand, if the infrared transmittance of the sealing material is below the lower limit, the sealing portion 3 may soften preferentially, which may result in poor sealing performance of the solder material. If the transmittance of the sealing material to infrared rays with a wavelength of 1 μm is within the above range, the infrared absorption of the heat-shrinkable connecting part 50 during infrared heating can be improved, and the sealing performance of the heat-shrinkable connecting part can be improved.

[0059] The heat-shrinkable connecting component includes the heat-shrinkable tube, and therefore has good shrinkage performance, sealing properties, and heat resistance as a heat-shrinkable connecting component.

[0060] <Method of manufacturing heat shrinkable tubing> The method for manufacturing the heat-shrinkable tube includes the steps of extruding a resin composition containing an ethylene-tetrafluoroethylene copolymer as a main component into a tube, crosslinking the tube formed by the extrusion molding process by irradiation, heating the tube after the crosslinking process at a temperature of 250°C or higher and 280°C or lower, and expanding the tube by increasing the pressure inside the tube by 50 kPa or more higher than the pressure outside the tube.

[0061] (Extrusion molding process) First, a resin composition for forming the heat-shrinkable tube is prepared by mixing an ethylene-tetrafluoroethylene copolymer, which is the resin component of the heat-shrinkable tube, with other additives as needed using a melt mixer or the like. In the resin composition, a colorant or a crosslinking aid is added to the ethylene-tetrafluoroethylene copolymer raw material as needed. The melting point and storage modulus can be controlled by selecting the ethylene-tetrafluoroethylene copolymer raw material and adjusting the crosslinking. The melt mixer is not particularly limited, and examples that can be used include an open roll, a Banbury mixer, a pressure kneader, a single-screw mixer, and a multi-screw mixer.

[0062] Next, in this process, a resin composition containing an ethylene-tetrafluoroethylene copolymer as a main component is extruded into a tube. The resin composition is extruded using a melt extruder. Specifically, the resin composition is heated to a temperature above its melting point to melt it, eluted from an extrusion die having a cylindrical space, and cooled to below its melting point with cooling water or the like to solidify it, thereby extruding the resin composition into a tube. The dimensions of the extrusion molded product can be designed depending on the application, etc. The dimensions of the extrusion molded product can be adjusted by the dimensions of the extrusion die and the draw-down ratio. The "draw-down ratio" is the ratio between the cross-sectional area of ​​the extrusion die and the cross-sectional area of ​​the tube after extrusion. To suppress surface roughness during extrusion, a draw-down ratio of 6 or more is preferred, and 10 or more is more preferred.

[0063] (Crosslinking process) In the crosslinking step, the tube formed in the extrusion molding step is crosslinked by irradiation. In this step, the ethylene-tetrafluoroethylene copolymer, which is the base resin of the extrusion molded product, is crosslinked to impart shrinkability (shape memory effect) when heated and shrunk at high temperatures after the expansion step, and shape retention at high temperatures after shrinkage. A preferred method for crosslinking the ethylene-tetrafluoroethylene copolymer is to irradiate the ethylene-tetrafluoroethylene copolymer with radiation. Since molding becomes difficult after the ethylene-tetrafluoroethylene copolymer has been crosslinked by irradiation with radiation, irradiation with radiation (crosslinking) is carried out after the extrusion molding step. By irradiating with radiation after extrusion molding, molding can be carried out reliably and the effects of radiation irradiation can be fully obtained.

[0064] Examples of radiation used for irradiation crosslinking of ethylene-tetrafluoroethylene copolymer include electron beams (β rays), γ rays, etc. Electron accelerators have low running costs, can produce high-power electron beams, and are easy to control, so electron beams are preferred as the radiation.

[0065] The radiation dose is preferably in the range of 30 kGy to 300 kGy. If the radiation dose is less than 30 kGy, the degree of crosslinking will be small, resulting in insufficient strength of the heat-shrinkable connecting part and making it more susceptible to breakage. Furthermore, the shrink performance (shape memory ability) will be reduced, which may result in a decrease in shape retention at high temperatures after shrinkage. On the other hand, if the radiation dose is more than 300 kGy, the degree of crosslinking will be large, which may reduce the flexibility of the heat-shrinkable connecting part and make it more susceptible to breakage during assembly. Furthermore, expansion will be difficult, which may result in quality variations, a decrease in wall thickness deviation, and variations in length change rate.

[0066] (Heating process) In the heating step, the tube after the crosslinking step is heated to a temperature of 250°C or higher and 280°C or lower. This reduces the wall thickness deviation of the expanded tube and increases the expansion speed. This more reliably reduces the manufacturing cost and quality variation of the heat-shrinkable tube. If the heating temperature of the tube is lower than the lower limit, expansion may be insufficient or the linear expansion speed may decrease. Conversely, if the heating temperature of the tube exceeds the upper limit, the tube may be damaged by heat. Note that the tube temperature needs to be heated to a temperature of 250°C or higher and 280°C or lower just before expansion, and heating can be performed in two or more stages to improve heating efficiency and suppress damage due to overheating.

[0067] (Expansion process) In the expansion step, the heated tube is expanded. The expansion of the tube may be performed simultaneously with the heating. The tube can be expanded by any known expansion method commonly used in the manufacture of conventional heat-shrinkable tubes. For example, an extrusion-molded product can be expanded to a predetermined inner diameter by heating the product to a temperature above its melting point and introducing compressed air into the product, or by reducing the pressure from the outside, and then cooled to fix the shape. The heat-shrinkable tube is obtained by fixing the shape of the expanded extrusion-molded product. Examples of such a fixing method include cooling the product to a temperature below the melting point of the base resin component. The heat-shrinkable tube is obtained by expanding the extrusion-molded product and fixing its shape in this way. The tube is expanded (expanded) so that the average inner diameter of the tube becomes approximately 1.4 to 4 times its original size.

[0068] During the expansion process, the tube is expanded by increasing the pressure inside the tube by 50 kPa or more higher than the pressure outside the tube. If the pressure inside the tube is less than 50 kPa higher than the pressure outside the tube, the expansion may be insufficient or the linear expansion speed may decrease. The expansion ratio when used as a heat-shrinkable connecting part is preferably 2.5 times or more, more preferably 3 times or more. The expansion dimension during expansion can be controlled by the size of the expansion die. The expansion die stabilizes expansion by reducing frictional resistance with the tube during expansion, improving the wall thickness deviation and reducing the variation in the length change rate. To reduce frictional resistance, the expansion die can be surface-treated. Surface treatments can include coating with fluororesins such as PTFE and PFA, which have a low friction coefficient, or modifying the surface shape by sandblasting, machining, or electrical discharge machining. Frictional resistance can be reduced by increasing surface roughness or reducing the contact area by creating grooves.

[0069] In the heat-shrinkable tubing manufactured by the method for manufacturing a heat-shrinkable tubing, the lower limit of the storage modulus at 250° C. or higher and 280° C. or lower is 0.8 MPa, preferably 1.0 MPa, and more preferably 1.2 MPa, while the upper limit of the storage modulus is 2.8 MPa, preferably 2.0 MPa, and more preferably 1.6 MPa.

[0070] The lower limit of the melting point of the heat-shrinkable tube is 210°C, more preferably 215°C. Meanwhile, the upper limit of the melting point of the heat-shrinkable tube is 250°C, more preferably 240°C. By setting the storage modulus and melting point within the above ranges, expansion can be stabilized. Furthermore, the heat-shrinkable tube has excellent deformability when heated to a temperature above its melting point, and can be easily and reliably expanded in diameter.

[0071] The thickness deviation of the heat-shrinkable tube is preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more. The lower limit of the length change rate of the heat-shrinkable tube is preferably -15% or more, more preferably -10% or more, and even more preferably -5% or more. The thickness deviation is defined by the following formula:

[0072] Wall thickness deviation rate (%) = Minimum wall thickness / Maximum wall thickness in tube cross section x 100 The upper limit of the length change rate of the heat-shrinkable tube is preferably +15% or less, more preferably +10% or less, and even more preferably +5% or less. The length change rate is defined by the following formula. Length change rate (%) = (tube length after shrinkage - tube length before shrinkage) / tube length before shrinkage x 100

[0073] The inclination angle of the end face of the heat-shrinkable tube during shrinkage is preferably 10° or less, more preferably 8° or less, and even more preferably 5° or less. The inclination angle of the end face is a measure of the degree of deformation that occurs on the longitudinal end face of the heat-shrinkable tube due to heat shrinkage. The inclination angle of the end face is measured using the following procedure. In a longitudinal cross-section of the heat-shrinkable tube cut longitudinally from the tip after heat shrinkage, the distance between a line parallel to the outer diameter passing through the highest point that protrudes from the tip in the longitudinal direction and a line parallel to the outer diameter passing through the lowest point that is recessed from the tip in the longitudinal direction is defined as X mm. When the outer diameter of the heat-shrinkable tube is D mm, the angle θ is the angle that satisfies the following formula: tanθ=X / D

[0074] The inner diameter, wall thickness deviation, length change rate, and end face inclination angle during shrinkage of the heat-shrinkable tube can be controlled by controlling the storage modulus of the heat-shrinkable tube, the heating temperature, the heating method, the expansion conditions such as the pressure difference between the inside and outside of the tube, and the surface treatment of the expansion die.

[0075] According to this method for manufacturing a heat-shrinkable tube, it is possible to manufacture a heat-shrinkable tube having excellent heat resistance and heat-shrinkability for use as a heat-shrinkable connecting part for a highly heat-resistant insulated electric wire. Furthermore, this method for manufacturing a heat-shrinkable tube can reduce variation in quality.

[0076] [Method of manufacturing heat-shrinkable connectors] The method for manufacturing a heat-shrinkable connection part includes the steps of making sealing portions and fixing a pair of sealing portions to the inner circumferential surface of both end sides of a heat-shrinkable tube. Preferably, the method for manufacturing a heat-shrinkable connection part further includes the step of fixing a solder portion to the inner circumferential surface of the heat-shrinkable tube between the pair of sealing portions. The method for manufacturing a heat-shrinkable connection part includes the steps of making sealing portions using a sealing material and fixing a pair of sealing portions to the inner circumferential surface of both end sides of a heat-shrinkable tube, so that a heat-shrinkable connection part with good shrink performance, sealing ability, and heat resistance can be manufactured.

[0077] (Process for producing sealing portion) In this step, a sealing portion is produced using a sealing material. In the sealing portion production step, a sealing portion is produced using a sealing material. First, a sealing material for forming the sealing portion is prepared using a melt mixer or the like. The melt mixer is not particularly limited, and for example, an open roll, a Banbury mixer, a pressure kneader, a single-screw mixer, a multi-screw mixer, or the like can be used.

[0078] Next, the encapsulating material is extruded using a melt extruder. Specifically, the encapsulating material is heated to a temperature equal to or higher than the melting point of the main component resin to melt it, and then extruded from an extrusion die having a cylindrical space. The encapsulating material is then cooled to a temperature equal to or lower than the melting point of the main component resin using cooling water or the like to solidify it, thereby extruding the encapsulating material into a tubular shape. The encapsulating material is then cut to a predetermined length to produce a ring-shaped encapsulation portion.

[0079] (Process for fixing the sealing portion) In this process, a pair of sealing portions is fixed to the inner circumferential surface at both ends of the heat-shrinkable tube. First, a pair of sealing portions composed of the heat-shrinkable tube and a sealing material is disposed on a metal rod. In this process, a solder portion composed of a solder material may also be disposed between the pair of sealing portions. In this process, the entire heat-shrinkable tube disposed on the metal rod is heated to shrink the heat-shrinkable tube, thereby fixing the pair of sealing portions to the inner circumferential surface at both ends of the heat-shrinkable tube. Furthermore, if a solder portion is also disposed between the pair of sealing portions on the metal rod, shrinking the heat-shrinkable tube also fixes the solder portion to the inner circumferential surface between the pair of sealing portions on the heat-shrinkable tube. Examples of the heating method include heating with a heat gun and heating with an infrared heating device. Then, the heat-shrinkable tube with the sealing portions, solder portions, etc. fixed thereto is removed from the metal rod to form a heat-shrinkable connection part.

[0080] The softening point of the sealing material is preferably 80° C. or higher and 170° C. or lower. When the softening point of the sealing material is 80° C. or higher and 170° C. or lower, the sealing material has appropriate fluidity and is more effective in filling gaps, thereby improving sealing properties.

[0081] Other configurations of the method for manufacturing the heat-shrinkable connecting part are as described above.

[0082] [How the heat-shrinkable connector is used] The heat-shrinkable connecting element 50 can be used, for example, as a component for connecting multiple insulated electric wires, as well as a component for attaching an earth wire to the insulated electric wires. As an example of a method for connecting multiple insulated electric wires using the heat-shrinkable connecting element 50, a method for connecting the exposed conductor portions of two insulated electric wires will be described with reference to FIGS. 7 to 11 . Note that the number and configuration of the insulated electric wires are not limited to those shown in FIGS. 7 to 11 . The process for connecting multiple insulated electric wires using the heat-shrinkable connecting element 50 mainly includes a heat-shrinkable connecting element covering step, a heat-shrinkable connecting element heating step, and a heat-shrinkable connecting element cooling step. Below, a use example will be described in which the heat-shrinkable connecting element 50 is used to connect two insulated electric wires 8 and 18 to obtain the electric wire bundle 100 shown in FIG. 11 .

[0083] (Heat-shrinkable connection part coating process) When connecting two insulated wires 8 and 18 using the heat-shrinkable connecting part 50, first, as shown in Fig. 7 , the conductor 6 exposed from the insulating layer 7 of the insulated wire 8 and the conductor 16 exposed from the insulating layer 17 of the insulated wire 18 are inserted through openings at both ends of the heat-shrinkable connecting part 50. Then, as shown in Fig. 8 , the heat-shrinkable connecting part 50 is placed over the two insulated wires 8 and 18 so as to cover the boundary between the exposed portion of the conductor 6 and the insulating layer 7, and the boundary between the exposed portion of the conductor 16 and the insulating layer 17. When the heat-shrinkable connecting part 50 is placed over the two insulated wires 8 and 18, it is preferably positioned so that the conductor connection part 5 around the boundary between the exposed conductor 6 of the insulated wire 8 and the exposed conductor 16 of the insulated wire 18 is covered with the solder part 2.

[0084] (heat shrinkable connection part heating process) In the heat-shrinkable connecting component heating step, the heat-shrinkable connecting component 50 is heated and thermally shrunk. Examples of the heating method include heating the heat-shrinkable connecting component 50 with a heat gun, an infrared heating device, or the like. The heating temperature is determined by the heat-shrinkage temperature of the heat-shrinkable connecting component 50, and is, for example, 200°C or higher and 600°C or lower. The heating time may be any time long enough to cause the heat-shrinkable connecting component 50 to shrink sufficiently, and may be, for example, 1 second or higher and 30 seconds or lower.

[0085] As shown in FIGS. 9 to 11, the shrink behavior of the heat-shrinkable connecting part 50 is preferably such that the heat-shrinkable tube 1 shrinks first, then the sealing part 3 deforms, and finally the solder part 2 melts. When the heat-shrinkable connecting part 50 is heated, the solder material of the solder part 2 flows and spreads. FIG. 11 shows the heat-shrinkable tube 11 after shrinkage, the solder part 12 after melting, and the sealing part 13 after melting in the connected wire bundle 100. The sealing material of the sealing part 3 has a high viscosity and therefore does not spread as much as the solder part 2, and therefore closes the opening of the heat-shrinkable tube 1. This prevents the solder material of the solder part 2 from flowing out of the opening of the heat-shrinkable tube 1. In addition, the solder material of the solder portion 2 covers the exposed portions of the conductor 6 of the insulated wire 8 and the conductor 16 of the insulated wire 18, and penetrates into the inside of the insulating layer 7 from the boundary between the exposed portion of the conductor 6 and the insulating layer 7, while also penetrating into the inside of the insulating layer 17 from the boundary between the exposed portion of the conductor 16 and the insulating layer 17.

[0086] Since atmospheric heating transfers heat from the outside, good assembly is possible by setting the melting point of the solder material of the solder portion 2 to 210°C or higher and 240°C or lower, and the softening point of the sealing material of the sealing portion 3 to 80°C or higher and 170°C or lower. If the melting point of the sealing portion 3 is high and softens slowly, the end of the heat-shrinkable tube 1 cannot be sealed, causing the solder material to dissolve. If the melting point of the sealing portion 3 is low and softens quickly, the sealing material will dissolve. If the melting point of the solder material is high, the insulated wires may not be connected properly by the heat-shrinkable connecting part 50. If the melting point of the solder material is low, the solder material may dissolve because it is not held in place by the sealing portion 3. If the tube shrinks slowly, the sealing portion 3 and solder portion 2 will not be able to melt and be held in place due to the large gaps. By having the melting point of the solder material and the softening point of the sealing material within the above ranges, the heat-shrinkable tube 1 can be combined with the solder material and the sealing material to improve the heat resistance, sealing properties, and connectivity of the insulated wire in the heat-shrinkable connecting part 50.

[0087] When the heat-shrinkable connecting part 50 is shrunk using an infrared heating device, the sealing part 3 is heated by absorbing infrared rays. As described above, the transmittance of the sealing material for infrared rays with a wavelength of 1 μm is preferably 1.0% to 30.0%, more preferably 3% to 22%, and even more preferably 5% to 16%. If the infrared transmittance of the sealing material exceeds the upper limit, the sealing part 3 may be difficult to heat, which may slow down softening. On the other hand, if the infrared transmittance of the sealing material is less than the lower limit, the sealing part 3 may soften preferentially and may dissolve from the heat-shrinkable connecting part 50. If the transmittance of the sealing material for infrared rays with a wavelength of 1 μm is within the above range, the infrared absorption of the heat-shrinkable connecting part 50 during infrared heating can be improved, and the heat-shrinkage behavior can be easily controlled.

[0088] To visually check whether the solder material has been heated sufficiently and melted, a thermochromic paint that disappears above a specified temperature can be applied to the solder material. Alternatively, a bi-alloy solder ring can be used, which has a high-melting-point portion in the center and allows the temperature to be confirmed by the melting of this high-melting-point portion. The high-melting-point portion is for visual confirmation, and does not necessarily need to be completely melted in terms of its characteristics.

[0089] (Heat-shrinkable connection part cooling process) In the heat-shrinkable connecting part cooling step, the heat-shrinkable connecting part 50 is cooled after heat shrinking. The cooling method is not particularly limited, but may be, for example, cooling by leaving it to stand or forced cooling using cold air, etc. This cooling solidifies the solder material and the sealing material, thereby connecting the insulated electric wires together and waterproofing the insulated electric wires.

[0090] [Other embodiments] The embodiments disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is not limited to the configurations of the above-described embodiments, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.

[0091] Another embodiment of the heat-shrinkable connecting component may include the heat-shrinkable tube, a pair of sealing portions disposed on the inner circumferential surface of both ends of the heat-shrinkable tube, and braided solder instead of the solder portion. A heat-shrinkable connecting component 53 according to another embodiment shown in FIG. 5 includes a heat-shrinkable tube 1, a pair of sealing portions 3 disposed on the inner circumferential surface of both ends of the heat-shrinkable tube 1, and braided solder 27. When the solder portion 2 is a braided solder formed by impregnating a braided wire with solder, the metal material constituting the braided wire can be, for example, Cu, Fe, Sn, Sb, Ag, Ni, Al, Zn, or a combination thereof. The metal material constituting the solder material of the braided solder can be the same as the solder material described above. The braided solder 27 can also be combined with the solder portion described above.

[0092] As another example of the heat-shrinkable connecting part, a crimp sleeve may be used instead of the solder portion of the heat-shrinkable connecting part. A heat-shrinkable connecting part 54 according to another embodiment shown in FIG. 6 includes a heat-shrinkable tube 1, a pair of sealing portions 3 disposed on the inner circumferential surface of both ends of the heat-shrinkable tube 1, and a crimp sleeve 28. The crimp sleeve may be made of one or a combination of two or more of Cu, Fe, Sn, Sb, Ag, Ni, Al, or Zn. A coating layer may be formed on the surface to reduce wear and scratch resistance and improve chemical durability. The coating layer may be made of one or a combination of two or more of Cu, Fe, Sn, Sb, Ag, Ni, Al, or Zn. [Example]

[0093] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0094] <Test Example 1> Heat-shrinkable tubes No. 1 to No. 10 in Table 1 were produced through the steps of raw material selection, resin mixing, extrusion, irradiation, and expansion. First, a resin composition was prepared by blending triallyl isocyanurate as a crosslinking aid with an ethylene-tetrafluoroethylene copolymer resin containing the fluorine content listed in Table 1. The resin composition was melt-extruded to form a tube. The extrusion was performed at a die temperature of 280°C, a drawdown ratio of 10, and a linear speed of 20 m / min. The tube was then crosslinked by electron beam irradiation at a dose of 25 kGy to 400 kGy. After irradiation, the tube was heated to 250°C to 280°C and expanded by applying a higher pressure to the inside of the tube than to the outside using an expansion die. The expansion die was coated with a fluororesin. The melting point and high-temperature storage modulus were adjusted by selecting the raw materials and the degree of crosslinking. Shrinkage was performed by heating at 270°C for 10 minutes.

[0095] For the above heat shrinkable tubes No. 1 to No. 10, the melting point of the tube, the storage modulus [MPa] at 250°C to 280°C, the wall thickness deviation [%], and the length change [%] are shown below. The expansion and contraction performance of the tubes were also evaluated on a four-point scale of A to D. The results are shown in Table 1. Note that "-" in the tables below indicates that the corresponding evaluation was not performed.

[0096] The evaluation criteria for the expansion and contraction performance of the tube are shown below, with A to C being levels that present no practical problems. (1) Expansion performance A: The dimensional variation during continuous expansion is particularly small, making it particularly excellent. B: Excellent, with minimal dimensional variation during continuous expansion. C: Stable and continuous expansion is possible. D: Stable continuous expansion is not possible. (2) Shrinkage performance A: The shrinkage time is particularly short and excellent. B: Excellent, short shrinkage time. C: Contraction time is slightly longer. D: Does not shrink to desired size.

[0097] [Table 1]

[0098] As shown in Table 1, by setting the storage modulus at 250°C to 280°C to 0.8 MPa to 2.8 MPa, good expansion and contraction performance and wall thickness deviation were obtained. On the other hand, in Nos. 1 and 9, which had a storage modulus of less than 0.8 MPa, the tube did not shrink to the desired size during contraction, and a sufficient shape memory effect was not obtained. In Nos. 8 and 10, which had a storage modulus of more than 2.8 MPa, stable continuous expansion was difficult.

[0099] <Test Example 2> Heat-shrinkable tubes Nos. 11 to 17 were fabricated in the same manner as in Test Example 1 No. 2, except that the raw materials for the ethylene-tetrafluoroethylene copolymer resin were selected so that the fluorine content in the ethylene-tetrafluoroethylene copolymer was the value shown in Table 2. For No. 18, a PTFE raw material was used. For PTFE, a petroleum-based solvent was added to the raw material and mixed to prepare a preformed ingot. The extruded tube was then paste-extruded, dried, and sintered to produce an extruded tube. The extruded tube was expanded in the same manner as ETFE. For No. 19, a heat-shrinkable tube was fabricated using a PVDF raw material. For PVDF, an extruded tube was fabricated by melt molding in the same manner as ETFE, and then expanded after irradiation. Next, a ring-shaped solder portion was formed in the longitudinal center of a metal rod, and ring-shaped sealing portions were formed at both ends using a heat-shrinkable tube, a solder material (Sn 96.0% by mass, Ag 3.0% by mass, and Cu 1.0% by mass) with a melting point of 223°C, and a sealing material (THV) with a softening point of 110°C. Next, the tip of the lead wire was placed in the solder area, and a heat-shrinkable tube was placed around it. A heat gun was then used to apply hot air at 500°C to the tube, shrinking it to fix the solder and sealing portions. After cooling, the tube was removed from the metal rod to produce a heat-shrinkable connection. The tube length was 20 mm. The sealing material was 2 mm wide and 0.4 mm thick. The solder material was 2.5 mm wide and 0.4 mm thick. A thermomechanical analyzer TMA-50 (Shimadzu Corporation) was used to measure the softening point. The softening point was determined as the temperature at which the thickness of the 0.4 mm sheet was reduced to 50% when the heating rate was 10°C / min, the push rod diameter was 0.5 mm, and the pressure was 5 kPa. Table 2 shows the fluorine content of heat-shrinkable tubes No. 11 to No. 19, their physical properties, and the same expansion performance, wall thickness deviation, and shrinkage performance as in Test Example 1, as well as the evaluation results of the heat-shrinkable connection.

[0100] The performance of the heat-shrinkable connectors was evaluated by placing them on the ETFE wire where the insulation had been removed, applying a voltage in the solution, and determining whether the leakage current was below the threshold. To evaluate heat resistance, the shrunk wire was heated at 200°C for 500 hours, after which the leakage current was evaluated. The immersion solution was a 5% NaCl, 0.5% surfactant solution, and a voltage of 1 kV was applied for 60 seconds to evaluate the leakage current. The evaluation criteria for the performance of heat shrinkable connectors are as follows: A: The pass rate for leakage current testing is over 90%. B: The passing rate of the leakage current test is 80% or more. C: The passing rate of the leakage current test is 75% or more. D: The passing rate of the leakage current test is less than 75%.

[0101] [Table 2]

[0102] As shown in Table 2, when the fluorine content of ETFE was between 58% and 62% by mass, good results were obtained in the evaluation of the tubing and the evaluation of the heat-shrinkable connector. On the other hand, No. 11, which had a fluorine content of less than 58% by mass, had a high melting point, resulting in a high shrinkage temperature. When used as a heat-shrinkable connector, the ETFE-insulated wire to be covered was damaged by heat. No. 17, which had a fluorine content of more than 62% by mass, had a low melting point, resulting in performance inconsistency when used as a heat-shrinkable connector at 200°C. In No. 18, the PTFE melting point was high at 327°C, making expansion difficult without softening the material. Furthermore, the high melting point of PTFE led to a high shrinkage temperature, requiring prolonged heating, which damaged the insulated wire. In No. 19, the PVDF melting point was low at 160°C, making stable expansion difficult due to the material softening at high temperatures. In addition, because PVDF has a low melting point and a low shrinkage temperature, when it is heated to the extent that it melts the solder, the heating conditions are too strong, causing damage to the tube and preventing it from exhibiting good properties as a heat-shrinkable connecting part.

[0103] <Test Example 3> Heat-shrinkable tubes No. 20 to No. 27 were fabricated in the same manner as in Test Example 1, except that raw materials with controlled molecular structures of ethylene-tetrafluoroethylene copolymer resins were used. Next, using the heat-shrinkable tubes listed in Table 3, a solder material (96.5% by mass of Sn and 3.5% by mass of Ag) with a melting point of 223°C, and a sealing material (60% by mass of THV and 40% by mass of FKM) with a softening point of 140°C, a ring-shaped solder material was fixed to the longitudinal center of a metal rod, and ring-shaped sealing portions were fixed to both ends. Next, the tip of a lead wire was placed in the soldered portion area, and a heat-shrinkable tube was attached around the periphery. Then, hot air at 500°C was applied using a heat gun to shrink the tube, fixing the soldered portion and sealing portion. After cooling, the tube was removed from the metal rod, producing a heat-shrinkable connection. The tube length was 20 mm. Table 3 shows the physical properties and evaluation of the tube similar to Test Example 1, and the evaluation results of the heat-shrinkable connecting parts similar to Test Example 2, in relation to the ratio n / m of the number of ethylene units m to the number of tetrafluoroethylene units n in the ethylene-tetrafluoroethylene copolymer.

[0104] [Table 3]

[0105] As shown in Table 3, when the ratio n / m (the number of tetrafluoroethylene units n to the number of ethylene units m in ETFE) was 1.02 or more and 1.20 or less, good results were obtained in the evaluation of the tube and the evaluation of the heat-shrinkable connector. On the other hand, No. 20, which had an n / m ratio of less than 1.02, had a high melting point and a high shrinkage temperature, and when used as a heat-shrinkable connector, the ETFE-insulated electric wire to be covered was damaged by heat. No. 27, which had an n / m ratio of more than 1.20, had a low melting point, so the heat-shrinkable connector did not exhibit stable performance when used at high temperatures and did not meet the 200°C heat resistance requirement.

[0106] <Test Example 4> Heat-shrinkable tubes Nos. 28 to 35 were produced in the same manner as in Test Example 1 No. 2, except that the molecular structure of ETFE and the irradiation dose were controlled so that the storage modulus of the resulting heat-shrinkable tube at 25°C would be the value shown in Table 4. Next, heat-shrinkable connecting parts were produced using the heat-shrinkable tubes shown in Table 4, a solder material (95.0 mass% Sn and 5.0 mass% Sb) with a melting point of 236°C, and a sealing material (60 mass% PVDF and 40 mass% EVA) with a softening point of 80°C, using the same process as in Test Example 2. The storage modulus, strength, and flexibility of heat-shrinkable tubes Nos. 28 to 35 at 25°C were evaluated. The evaluation results are shown in Table 4.

[0107] The strength and flexibility of the heat shrinkable tubes No. 28 to No. 35 were evaluated according to the following criteria. (1) Strength of heat-shrinkable connectors A: No damage occurs during assembly, shrinkage, or use. B: In rare cases, damage may occur during use. C: Damage may occur during use. D: There is a high probability of breakage during use. (2) Flexibility of heat-shrinkable connecting parts A: No damage occurs during assembly. B: In rare cases, damage may occur during assembly. C: Damage may occur during assembly. D: There is a high probability of damage occurring during assembly.

[0108] [Table 4]

[0109] As shown in Table 4, when the storage modulus of ETFE at 25°C is 500 MPa or more and 900 MPa or less, the strength and flexibility of the heat-shrinkable connecting part can be improved. In No. 28, which has a storage modulus of less than 500 MPa at 25°C, the strength of the heat-shrinkable connecting part was insufficient. In No. 35, which has a storage modulus of more than 900 MPa at 25°C, the flexibility of the heat-shrinkable connecting part was low and it was prone to breaking.

[0110] <Test Example 5> Heat-shrinkable tubes Nos. 36 to 43 were produced in the same manner as No. 15 in Test Example 2, except that the draw-down rate during extrusion was controlled so that the arithmetic mean roughness Ra of the surface of the resulting heat-shrinkable tube would be the value shown in Table 5. Heat-shrinkable connecting parts were also produced using the same process as in Test Example 2. The same solder material and sealing material were used as in Test Example 2. Table 5 shows the evaluation results of the arithmetic mean roughness Ra and infrared heating efficiency of heat-shrinkable tubes Nos. 36 to 43, as well as the visibility of the inside of the heat-shrinkable tube. The arithmetic mean roughness Ra of the heat-shrinkable tube was measured using a stylus-type roughness tester.

[0111] The infrared heating efficiency of the heat-shrinkable tube and the visibility of the inside of the heat-shrinkable tube were evaluated according to the following criteria. The evaluation results are shown in Table 5. (1) Heating efficiency of heat shrinkable tubing in infrared rays A: Particularly excellent with heat shrinkable connecting parts with a shrinkage time of 20 seconds or less. B: The shrinkage time of the heat-shrinkable connecting part is 25 seconds or less. C: The shrinkage time of the heat-shrinkable connecting part is 35 seconds or less. D: The shrinkage time of the heat-shrinkable connecting part is 35 seconds or more. (2) Visibility inside the heat shrink tubing A: It is particularly easy to check the state of solder impregnation into the wire, the melting of the sealing material, and the state of the wire coating. B: The state of solder impregnation into the wire, the melting of the sealing material, and the state of the wire coating can be confirmed. C: The state of impregnation of the solder material into the wire and the progress of melting of the sealing material can be confirmed. D: Impregnation of the solder material into the wire and progress of melting of the sealing material cannot be confirmed.

[0112] [Table 5]

[0113] As shown in Table 5, when the arithmetic mean roughness Ra of the tube surface was 0.10 μm or more and 2.00 μm or less, good results were obtained in the evaluation of the tube and the evaluation of the heat-shrinkable connector. On the other hand, No. 36, which had an arithmetic mean roughness Ra of less than 0.10 μm, had high infrared transmittance and low tube heating efficiency. No. 43, which had an arithmetic mean roughness Ra of more than 2.00 μm, had high visible light scattering, which reduced visibility of the inside of the heat-shrinkable tube when checking the condition of the inside of the heat-shrinkable connector.

[0114] <Test Example 6> Heat-shrinkable tubes Nos. 44 to 49 were produced in the same manner as in Test Example 1 No. 2, except that the amount of colorant was controlled so that the infrared transmittance of the resulting heat-shrinkable tube would be the value shown in Table 6. Next, heat-shrinkable connecting parts were produced in the same manner as in Test Example 2, using the heat-shrinkable tubes shown in Table 6, a solder material (62.0 mass% Pb and 38.0 mass% In) with a melting point of 210°C, and a sealing material (50 mass% PVDF and 50 mass% LLDPE) with a softening point of 95°C. Table 6 shows the infrared transmittance of heat-shrinkable tubes Nos. 44 to 49 at a center wavelength of 1 μm in an infrared heating device, the infrared heating efficiency of the heat-shrinkable tubes similar to those in Test Example 5, and the heating efficiency of the sealing material inside the heat-shrinkable connecting parts.

[0115] The heating efficiency of the sealing material was evaluated according to the following criteria. A: The sealing material heats and melts in a particularly short time, allowing heat-shrinkable connection parts to be produced. B: The sealing material is heated and melted in a short time, allowing the creation of heat-shrinkable connection parts. C: The sealing material is heated and melted to create a heat-shrinkable connection part. D: The sealing material does not heat or melt sufficiently.

[0116] [Table 6]

[0117] As shown in Table 6, when the transmittance of the tube for infrared rays with a wavelength of 1 μm was 90.0% or more and 99.0% or less, good results were obtained in the evaluation of the infrared heating efficiency of the heat-shrinkable tubing and the heating efficiency of the sealing material inside the heat-shrinkable connecting part. On the other hand, No. 44, which had an infrared transmittance of less than 90.0%, had a reduced heating efficiency of the sealing material when the heat-shrinkable connecting part was heated, making the sealing material less likely to deform and slowing the shrinkage of the heat-shrinkable connecting part. No. 49, which had an infrared transmittance of more than 99.0%, had a reduced heating efficiency of the heat-shrinkable tubing when the heat-shrinkable connecting part was heated, making it difficult for the heat-shrinkable tubing to shrink.

[0118] <Test Example 7> First, heat-shrinkable tubes No. 50 to No. 57 were produced in the same manner as in No. 2 of Test Example 1. Next, heat-shrinkable connecting parts were produced in the same manner as in Test Example 2 using the heat-shrinkable tubes shown in Table 7, a solder material (67.0 mass% Sn, 32.0 mass% Pb, and 1.0 mass% Cd) with a melting point of 218°C, and a sealing material (70 mass% THV and 30 mass% PVDF) with a softening point of 160°C, except that a sealing material was selected so that the infrared transmittance at a wavelength of 1 μm of the sealing material was the value shown in Table 7. Table 7 shows the infrared transmittance at a wavelength of 1 μm of the sealing material for heat-shrinkable connecting parts No. 50 to No. 57, and the results of performance evaluation of the heat-shrinkable connecting parts in the same manner as in Test Example 2.

[0119] [Table 7]

[0120] As shown in Table 7, when the infrared transmittance of the sealing material of the heat-shrinkable connecting part was 1.0% or more and 30.0% or less at a wavelength of 1 μm, good results were obtained in the performance of the heat-shrinkable connecting part. On the other hand, in No. 50, where the sealing material had an infrared transmittance of less than 1.0%, the infrared heating proceeded quickly, causing the sealing material to soften quickly and reducing the sealing ability of the solder material, resulting in poor performance of the heat-shrinkable connecting part. In No. 57, where the sealing material had an infrared transmittance of more than 30.0%, the sealing material heated slowly, causing the softening to proceed more slowly, resulting in poor performance of the heat-shrinkable connecting part.

[0121] <Test Example 8> First, heat-shrinkable tubes No. 58 to No. 69 were fabricated in the same manner as No. 2 in Test Example 1. Next, one or a mixture of two or more of THV, PVDF, FKM, EVA, LLDPE, and HDPE was used as the sealing material, and two or more of Sn, Ag, Sb, Pb, Bi, and In were used as the solder material, so that the softening point of the sealing material and the melting point of the solder material of the heat-shrinkable connecting parts would be the values ​​shown in Table 8. The softening points of the sealing material and the melting points of the solder material for heat-shrinkable connecting parts No. 58 to No. 69 are shown in Table 8. The performance of the heat-shrinkable connecting parts was evaluated in the same manner as in Test Example 2, and the results are shown in Table 8.

[0122] [Table 8]

[0123] As shown in Table 8, Nos. 61 to 66, which have heat-shrinkable connecting parts with solder melting points of 210°C to 240°C and encapsulating materials with softening points of 80°C to 170°C, achieved good results in the leakage current test. On the other hand, the pass rates of heat-shrinkable connecting parts for No. 60, which has a solder melting point below 210°C, No. 59, which has a encapsulating material softening point below 80°C, No. 58, which has a solder melting point below 210°C and a encapsulating material softening point below 80°C, No. 68, which has a solder melting point above 240°C, No. 67, which has a encapsulating material softening point above 170°C, and No. 69, which has a solder melting point above 240°C and a encapsulating material softening point above 170°C, all showed lower pass rates in the leakage current test.

[0124] <Test Example 9> Heat-shrinkable tubes Nos. 70 to 77 were fabricated in the same manner as in Test Example 1 No. 3. Next, using a heat-shrinkable tube, a solder material (Sn 96.0% by mass, Ag 3.0% by mass, and Cu 1.0% by mass) with a melting point of 223°C, and a sealing material (THV + silica) containing THV with a softening point of 110°C and silica in the amounts listed in Table 9, a ring-shaped solder material was fixed to the longitudinal center of a metal rod, and ring-shaped sealing portions were fixed to both ends. Next, the tip of a lead wire was placed in the soldered portion area, and a heat-shrinkable tube was attached around the periphery. Then, hot air at 500°C was applied with a heat gun to shrink the tube, fixing the soldered portion and sealing portion. After cooling, the tube was removed from the metal rod to fabricate a heat-shrinkable connection. The tube length was 20 mm. The sealing material was 2 mm wide and 0.4 mm thick. The solder material was 2.5 mm wide and 0.4 mm thick. The shear viscosity of the sealing material was adjusted by the amount of silica added. The shear viscosity at 250°C is shown in Table 9.

[0125] The performance of the heat-shrinkable connectors was evaluated by placing them on the ETFE wire where the insulation had been removed, applying a voltage in the solution, and determining whether the leakage current was below the threshold. To evaluate heat resistance, the shrunk wire was heated at 215°C for 750 hours, after which the leakage current was evaluated. The immersion solution was a 5% NaCl, 0.5% surfactant solution, and a voltage of 1 kV was applied for 60 seconds to evaluate the leakage current. The evaluation results of the heat-shrinkable connector performance are shown in Table 9. The evaluation criteria for the performance of the heat shrinkable connectors are as follows: A: The pass rate for leakage current testing is over 90%. B: The passing rate of the leakage current test is 80% or more. C: The passing rate of the leakage current test is 75% or more. D: The passing rate of the leakage current test is less than 75%.

[0126] [Table 9]

[0127] As shown in Table 9, good heat-shrinkable connector properties were obtained when the sealing material's shear viscosity at 250°C and a shear rate of 100 / s was between 1000 and 2000 Pa·s. No. 70, with a shear viscosity below 1000 Pa·s, softened and easily deformed during heat-shrinkable tubing shrinkage, resulting in poor sealing performance and a low pass rate in the leakage current test for heat-shrinkable connectors. On the other hand, No. 77, with a shear viscosity above 2000 Pa·s, had poor fluidity during heat-shrinkable tubing shrinkage, resulting in poor gap-filling performance and a low pass rate in the leakage current test for heat-shrinkable connectors.

[0128] <Test Example 10> Heat-shrinkable tubes Nos. 78 to 89 were fabricated in the same manner as in Test Example 1, No. 2, except that raw materials for the ethylene-tetrafluoroethylene copolymer resin were selected so that the fluorine content in the ethylene-tetrafluoroethylene copolymer would be the value shown in Table 10, and crosslinking was performed by electron beam irradiation at an irradiation dose of 80 kGy. Next, using a heat-shrinkable tube and a solder material (96.0 mass% Sn, 3.0 mass% Ag, and 1.0 mass% Cu) with a melting point of 223°C, and a sealing material with a softening point of 110°C containing 70 mass% THV, 30 mass% FKM, and the silica content shown in the table, a ring-shaped solder material was fixed to the longitudinal center of a metal rod, and ring-shaped sealing portions were fixed to both ends. Next, the tip of a lead wire was placed in the soldered portion area, and a heat-shrinkable tube was attached to its outer periphery. The tube was then shrunk by applying hot air at 500°C using a heat gun to fix the solder and sealing portions, and after cooling, it was removed from the metal rod to produce a heat-shrinkable connection. The tube was 20 mm long. The sealing material was 2 mm wide and 0.4 mm thick. The solder material was 2.5 mm wide and 0.4 mm thick. The shear viscosity of the sealing material was adjusted by the amount of silica added. The shear viscosity at 215°C is shown in the table. The performance of the heat-shrinkable connection was evaluated in the same manner as in Test Example 9.

[0129] [Table 10]

[0130] As shown in Table 10, good results were obtained in the sealing performance of heat-shrinkable connecting parts when the shear viscosity of the sealing material was between 7,000 Pa·s and 70,000 Pa·s at 215°C and a shear rate of 0.01 / s. On the other hand, No. 78, which had a shear viscosity of less than 7,000 Pa·s, tended to flow easily when held at high temperatures for long periods, resulting in a lower pass rate in the leakage current test. No. 89, which had a shear viscosity higher than 70,000 Pa·s, had poor fluidity, making it less effective at filling gaps, resulting in poor sealing and a lower pass rate in the leakage current test.

[0131] <Test Example 11> Heat-shrinkable tubes No. 90 to No. 95 were produced in the same manner as in No. 2 of Test Example 1. Next, heat-shrinkable connecting parts No. 90 to No. 95 were produced in the same manner as in Test Example 9 using heat-shrinkable tubes, solder material (Sn 96.0 mass%, Ag 3.0 mass%, and Cu 1.0 mass%) with a melting point of 223°C, and sealing materials (EVA, PVDF, THV) shown in Table 11. The melting point of the sealing material was determined by selecting the type of resin and adjusting the ratio. The melting points of the sealing materials for heat-shrinkable tubes No. 90 to No. 95 and the evaluation results of the performance of the heat-shrinkable connecting parts similar to those in Test Example 9 are shown in Table 11.

[0132] [Table 11]

[0133] As shown in Table 11, heat-shrinkable connectors No. 91 to No. 94, which had a melting point of 110°C or higher and 170°C or lower, exhibited favorable heat-shrinkable connector properties. No. 90, which had a melting point lower than 110°C, became soft and easily deformed when the heat-shrinkable tubing was shrunk, resulting in poor sealing performance and a low pass rate in the leakage current test for the heat-shrinkable connector. Furthermore, when held at high temperatures for long periods, the tubing became prone to flow, making it difficult to maintain sealing performance, resulting in a low pass rate in the leakage current test for the heat-shrinkable connector. No. 95, which had a melting point higher than 170°C, had poor fluidity when the heat-shrinkable tubing was shrunk, resulting in poor gap-filling effectiveness and poor sealing performance, resulting in a low pass rate in the leakage current test for the heat-shrinkable connector.

[0134] <Test Example 12> Heat-shrinkable connectors No. 96 to No. 103 were fabricated using tubes No. 2 to No. 7 from Test Example 1. Next, a ring-shaped sealing portion was fixed to the longitudinal end of a metal rod using a heat-shrinkable tube and a sealing material with a softening point of 110°C containing 70% by mass of THV, 30% by mass of FKM, and the silica content listed in Table 12. Next, a heat-shrinkable tube was attached to the outer periphery. The sealing portion was fixed by applying hot air at 500°C with a heat gun to shrink the tube. After cooling, the tube was removed from the metal rod to fabricate heat-shrinkable connectors No. 96 to No. 103. The length of the tube was 30 mm. The sealing material was 2 mm wide and 0.4 mm thick. The shear viscosity was adjusted by the amount of silica added. The shear viscosities at 250°C and 215°C are shown in Table 12.

[0135] The performance of the heat-shrinkable connectors was evaluated by placing a crimp sleeve and heat-shrinkable connector in the area where the insulation of the ETFE electric wire had been removed, positioning the lead wire so that the tip of the wire was positioned in the removed area, and then crimping and fixing the crimp sleeve with a crimping tool. The connector was then heated and shrunk. A voltage was applied in the solution to determine whether the leakage current was below the threshold. The crimp sleeve was 15 mm long and had an 8 μm thick nickel plating on a copper base. To evaluate heat resistance, the shrunk electric wires were heated at 215°C for 750 hours, after which the leakage current was evaluated. The immersion solution was a 5% NaCl, 0.5% surfactant solution, and a voltage of 1 kV was applied for 60 seconds to evaluate the leakage current. The results of the heat-shrinkable connector performance evaluation are shown in Table 12. The evaluation criteria for the performance of the heat shrinkable connectors are as follows: A: The pass rate for leakage current testing is over 90%. B: The passing rate of the leakage current test is 80% or more. C: The passing rate of the leakage current test is 75% or more. D: The passing rate of the leakage current test is less than 75%.

[0136] [Table 12]

[0137] As shown in Table 12, heat-shrinkable connecting parts No. 96 to No. 103, in which the heat-shrinkable tubing had a storage modulus of 0.8 MPa or more and 2.8 MPa or less at 250°C or more and 280°C or less, the sealing material had a shear viscosity of 1000 Pa·s or more and 2000 Pa·s or less at 250°C and a shear rate of 100 / s, and the sealing material had a shear viscosity of 7000 Pa·s or more and 70000 Pa·s or less at 215°C and a shear rate of 0.01 / s, showed good sealing performance.

[0138] <Test Example 13> In Test Example 13, heat-shrinkable tubing was evaluated when inorganic substances were added as additives. Heat-shrinkable tubing Nos. 104 to 110 were produced in the same manner as Test Example 1, No. 2, except that the inorganic substances shown in Table 13 were added. These heat-shrinkable tubing Nos. 104 to 110 were evaluated for strength and facility contamination in addition to the expansion and contraction performance in the same manner as Test Example 1. The evaluation results are shown in Table 13.

[0139] Strength and equipment contamination were evaluated by the following methods. (1) Strength The strength was measured by a tensile test at a pulling rate of 50 mm / min in accordance with ASTM D-638, and was evaluated according to the following criteria. A: Particularly excellent. B: Excellent. (2) Facility contamination The equipment contamination was evaluated according to the following criteria for the equipment after the heat shrinkable tube was manufactured. A: No contamination. B: Slightly contaminated. C: Slightly contaminated. D: Severe contamination.

[0140] [Table 13]

[0141] As shown in Table 13, by setting the content of inorganic substances to 1 mass % or less, it is possible to maintain good expansion characteristics, contraction characteristics and strength of the heat shrinkable tube, and also to suppress facility contamination.

[0142] The above results demonstrate that the heat-shrinkable tube has excellent heat resistance and heat-shrinkability when used as a heat-shrinkable connecting part for highly heat-resistant insulated electric wires. [Explanation of symbols]

[0143] 1 heat shrink tubing 2 Soldering section 3 Sealing part 5 Conductor connection 6, 16 conductors 7, 17 Insulation layer 8, 18 Insulated wire 11 Heat shrink tubing after shrinking 12 Solder after melting 13 Sealed part after melting 23 Wire of insulated earthing wire 24 Insulation layer of grounding insulated wire 25 Insulated grounding wire 27 Braid body 28 Crimp sleeve 40, 50, 51, 53, 54 Heat Shrink Connectors 100 Connected wire bundle

Claims

1. A heat-shrinkable connecting part for connecting an insulated electric wire having an element wire covered with an insulating layer, a heat shrinkable tube containing an ethylene-tetrafluoroethylene copolymer as a main component, having a melting point of 210° C. or more and 250° C. or less, and a storage modulus of 0.8 MPa or more and 2.8 MPa or less at 250° C. or more and 280° C. or less; a pair of sealing portions provided on an inner peripheral surface of both ends of the heat shrink tube; and a crimp sleeve. A heat-shrinkable connection part, wherein the sealing material constituting the sealing portion has a shear viscosity of 7000 Pa·s or more and 70000 Pa·s or less at 215° C. and a shear rate of 0.01 / s.

2. 2. The heat-shrinkable connection part according to claim 1, wherein the sealing material constituting the sealing portion has a shear viscosity of 1000 Pa.s or more and 2000 Pa.s or less at 250° C. and a shear rate of 100 / s.

3. 3. The heat-shrinkable connecting part according to claim 1, wherein the melting point of the sealing material is 110° C. or higher and 170° C. or lower.

4. 4. The heat-shrinkable connecting part according to claim 1, wherein the transmittance of the sealing material for infrared rays having a wavelength of 1 μm is 1.0% or more and 30.0% or less.

Citation Information

Patent Citations

  • Cross-linked fluoroplastic heat-shrinkable tube and preparation method thereof

    CN106317598A

  • Fluoropolymer heat-shrinkable sleeve and production method thereof

    CN106700218A

  • Irradiation crosslinking high-temperature-resistance heat-shrinkable sleeve and production method

    CN109337188A

  • Tube and heat contraction tube

    JP1993325692A

  • Fluororesin composition, and tube and thermally shrinkable tube produced therefrom

    JP1995033938A