Polymer Electrolytes

A polymer electrolyte with a high oxyethylene content and grafted polysiloxane compound addresses capacity leakage in lithium ion batteries, enhancing stability and performance.

JP7590585B2Active Publication Date: 2024-11-26UMICORE(BE)
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023539032
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-24
Filing Date
2021-12-23
Publication Date
2024-11-26
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

Existing PEO-based polymer electrolytes in lithium ion secondary batteries suffer from capacity leakage due to electronic conductivity, leading to current leakage from the anode to the cathode.

Method used

A polymer electrolyte comprising at least 70.0 mol% oxyethylene units, 0.0 to 10.0 mol% oxypropylene units, and 1.00 to 4.0 mol% of specific repeating units derived from monomers, with a polysiloxane compound grafted onto the polymer through hydrosilylation, reducing electronic conductivity and enhancing stability.

Benefits of technology

The proposed polymer electrolyte significantly reduces capacity leakage, improving the electrochemical performance and stability of lithium ion secondary batteries, especially under high voltage and temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590585000027
    Figure 0007590585000027
  • Figure 0007590585000001
    Figure 0007590585000001
  • Figure 0007590585000002
    Figure 0007590585000002
Patent Text Reader

Abstract

A polymer electrolyte suitable for use in lithium-ion secondary batteries is obtained by reacting at least one polyether polymer (P), the polymer (P) comprising at least 70.0 mol % oxyethylene units, 0.0 to 10.0 mol % oxypropylene units, and 1.00 to 4.0 mol % repeat units derived from at least one monomer, with at least one polysiloxane compound, which is grafted to the at least one polymer (P) via reaction of at least a portion of the —CH═CH2 moieties of the monomer (M) with the H—Si moieties of the polysiloxane compound.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polymer electrolytes suitable for use in lithium-ion secondary batteries. [Background technology]

[0002] Polymer electrolytes are an interesting alternative to liquid electrolytes in batteries. In this context, polyethylene oxide (PEO)-based electrolytes have been extensively studied in the literature.

[0003] For example, Ruoyuan Tao et al. in J. Appl. Electrochem. 35, 163-168 (2005) disclose a positive electrode comprising poly(ethylene oxide) and lithium bis(trifluoromethanesulfonyl)imide (Li(N(SOCF)), also called LiTFSI). PEO and LiTFSI were dissolved in acetonitrile to prepare an electrolyte solution. The positive electrode active material was added to the electrolyte solution.

[0004] US Patent No. 7,585,934 (B2) discloses the use of EO / PO / AGE and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, Li(N(SOCF))) as a solid polymer electrolyte membrane. This document discloses in the examples a copolymerization procedure of EO, PO, and AGE. In particular, LiTFSI was added as a Li salt to a polyether polymer composition containing the EO / PO / AGE copolymer in an amount such that the ratio of (moles of lithium atoms in the electrolyte salt) / (moles of oxygen atoms in the polyether polymer) was 0.05.

[0005] Despite recent advances in this field, capacitive leakage remains a problem when PEO-based solid electrolytes are used in batteries, a phenomenon in which the electrolyte acquires electronic conductivity and leaks electronic current from the anode to the cathode. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] U.S. Patent No. 7,585,934 [Non-patent literature]

[0007] [Non-Patent Document 1] J.Appl.Electrochem.35,p.163-168(2005) Summary of the Invention [Problem to be solved by the invention]

[0008] Thus, there is a need for improved polymer electrolytes, particularly polymer electrolytes that reduce capacitive leakage when used in batteries. [Means for solving the problem]

[0009] The present inventors have surprisingly found that it is possible to provide improved polymer electrolytes which meet the above-mentioned needs.

[0010] The main object of the present invention is to provide a polymer electrolyte suitable for use in lithium ion secondary batteries, i. at least one polyether polymer (hereinafter polymer (P)), said polymer (P) comprising: a) at least 70.0 mol % oxyethylene units (EO); b) 0.0 to 10.0 mol % of oxypropylene units (PO), and c) 1.00 to 4.0 mol % of a compound represented by general formula (I) or general formula (II):

[0011] [ka]

[0012] or

[0013] [ka]

[0014] (In the formula, Each of R1 and R2 is the same or different from each other, and in each occurrence, 1-6 The C is an alkanediyl. 1-6 Alkanediyl is a halide, C 1-4 Alkyl, C 3-6 cycloalkyl, CF, OR, each R being the same or different from each other and each occurrence independently selected from hydrogen and C 1-4 alkyl, n is an integer 0 or 1 or 2; Each X is a leaving group selected from the group consisting of halide, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate, and methanesulfonate) [hereinafter, monomer (M)] At least one polyether polymer comprising ii.Formula (III):

[0015] [ka]

[0016] (In the formula, Each of R3, R4, R5, R6, and R7 is the same or different from each other, and in each occurrence, independently represents 1-6 Alkyl, C 3-6 Cycloalkyl, aryl, C 1-6 alkoxy, heterocyclyl, 1-6 Alkyl, C 3-6 Cycloalkyl, aryl, C 1-6 Alkoxy, heterocyclyl, halide, C 1-4 Alkyl, C 3-6cycloalkyl, CF3, OR9, each of which is the same or different from each other and, at each occurrence, is independently selected from hydrogen, C 1-4 is selected from the group consisting of alkyl, and hydroxyl protecting groups; and m is an integer of at least 3; The at least one polysiloxane compound having formula (III) is grafted to the at least one polymer (P) via reaction of at least a portion of the -CH=CH2 moieties of the monomer (M) with the H-Si moieties of the polysiloxane compound having formula (III). [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 shows GPC elution curves of a polymer electrolyte, a polymer (P), and a polysiloxane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Polymer Electrolytes The term "comprising" as used in the present specification and claims should not be interpreted as being limited to the means recited thereafter, and does not exclude other elements or steps. It should be interpreted as specifying the presence of the mentioned features, integers, steps, or components as mentioned, but does not exclude the presence or addition of one or more other features, integers, steps, or components, or groups thereof. Thus, the scope of the expression "a composition comprising components A and B" should not be limited to a composition consisting of components A and B only. It means that in the context of the present invention, the only relevant components of the composition are A and B. Thus, the terms "comprising" and "including" encompass the more restrictive terms "consisting essentially of" and "consisting of".

[0019] As used herein, "optional" or "optionally" means that the event or circumstance described thereafter may or may not occur, and the description includes instances where the event or circumstance occurs and instances where the circumstance does not occur.

[0020] The inventors have surprisingly found that when the polymer electrolyte according to the present invention is used in batteries, in particular solid-state lithium-ion batteries, the capacitance leakage is reduced, resulting in batteries with improved performance, as demonstrated in the examples.

[0021] In the context of the present invention, the expression "at least one polyether polymer (hereinafter polymer (P))" is intended to mean one or more polymers (P). Similarly, the expression "at least one polysiloxane compound having formula (III)" is intended to mean one or more polysiloxane compounds having formula (III).

[0022] In the remainder of the text, the expressions "polymer (P)" and "polysiloxane compound having formula (III)" are to be understood for the purposes of the present invention both in the plural and in the singular.

[0023] As used herein, the term "alkyl" has its broadest meaning as generally understood in the art and can include moieties that are linear or branched, or combinations thereof.

[0024] The term "alkyl", alone or in combination, means a straight or branched chain alkane derived radical, e.g., C F-G Alkyl defines a straight or branched alkyl group having F to G carbon atoms, for example C 1-4Alkyl defines a straight or branched chain alkyl group having 1 to 4 carbon atoms, for example, methyl, ethyl, 1-propyl, 2-propyl (isopropyl), 1-butyl, 2-butyl, 2-methyl-2-propyl (tert-butyl), 2-methyl-1-propyl (isobutyl), and the like.

[0025] The term “cycloalkyl”, alone or in combination, means a cyclic alkane derived radical, e.g., C L-M Cycloalkyl defines a cyclic alkyl group having L to M carbon atoms, for example, C 3-6 Cycloalkyl defines cyclic alkyl groups having 3 to 6 carbon atoms, for example, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and the like.

[0026] The term "aryl", alone or in combination, means phenyl, naphthyl, or anthracenyl, optionally carbocyclically fused with a cycloalkyl or heterocyclyl, preferably a 5- to 7-membered ring, more preferably a 5- to 6-membered ring, and / or substituted with 1 to 5 groups or substituents. The aryl may be optionally substituted whereby a substituent is attached at one point to the aryl or a substituent is attached at two points to the aryl to form a bicyclic system, e.g., benzodioxole, benzodioxane, benzimidazole.

[0027] The term "heterocyclyl," alone or in combination, means a cyclic alkane derived group in which at least one carbon atom is replaced by a heteroatom independently selected from the group consisting of oxygen, nitrogen, and sulfur (e.g., pyrrolidine, piperidine, or morpholine, etc.).

[0028] The term "alkoxy", alone or in combination, means a radical derived from a straight or branched chain alkane, in which the carbon atom carrying the radical is replaced by an oxygen atom. An alkoxy moiety is an -OR x having the structure: xis alkyl.

[0029] The term "alkanediyl", alone or in combination, means a divalent radical derived from a straight or branched chain alkyl.

[0030] As mentioned above, the polymer (P) a) at least 70.0 mole % of repeating oxyethylene units (EO); b) 0.0 to 10.0 mol % of oxypropylene units (PO), and c) 1.00 to 4.0 mol % of a compound represented by general formula (I) or general formula (II):

[0031] [ka]

[0032] or

[0033] [ka]

[0034] (In the formula, Each of R1 and R2 is the same or different from each other, and in each occurrence, 1-6 The C is an alkanediyl. 1-6 Alkanediyl is a halide, C 1-4 Alkyl, C 3-6 cycloalkyl, CF, OR, each R being the same or different from each other and each occurrence independently selected from hydrogen and C 1-4 alkyl, n is an integer 0 or 1 or 2; Each X is a leaving group selected from the group consisting of halide, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate, and methanesulfonate) (hereinafter, monomer (M)).

[0035] Thus, at least 70.0 mol %, preferably at least 80.0 mol %, preferably at least 85.0 mol %, preferably at least 90.0 mol %, more preferably at least 92.0 mol %, more preferably at least 94.0 mol % of the repeat units of the polymer (P) are oxyethylene repeat units (EO).

[0036] It is further understood that at most 99.0 mol %, more preferably at most 98.5 mol %, more preferably at most 98.0 mol % of the repeat units of the polymer (P) are EO units.

[0037] In a preferred embodiment, the polymer (P) comprises at least 80.0 mol% and at most 99.0 mol%, preferably at least 90.0 mol% and at most 98.5 mol%, preferably at least 92.0 mol% and at most 98.5 mol% of EO units, preferably at least 94.0 mol% and at most 98.5 mol% of EO units.

[0038] When oxypropylene repeat units (PO) are present in the polymer (P), at most 10.0 mol %, more preferably at most 6.0 mol %, even more preferably at most 5.0 mol %, even more preferably at most 4.0 mol %, even more preferably at most 3.0 mol % of the repeat units of the polymer (P) are PO units.

[0039] Advantageously, said polymer (P) comprises at least 0.1 mol %, or at least 0.5 mol %, or at least 1.0 mol % of PO units.

[0040] In a preferred embodiment, the polymer (P) comprises at least 0.5 mol% and at most 6.0 mol%, or at least 0.5 mol% and at most 5.0 mol%, or at least 0.5 mol% and at most 4.0 mol%, or at least 1.0 mol% and at most 4.0 mol%, or at least 1.0 mol% and at most 3.0 mol% of PO units.

[0041] The presence of PO units makes it possible to reduce the crystallinity of the polymer (P), which improves its ionic conductivity.

[0042] For the purposes of the present invention, the term "oxypropylene (PO)" is intended to refer to the formula -O-CH2-CH2-CH2- or -O-CH2-CH(CH3)-, preferably -O-CH2-CH(CH3)-.

[0043] Preferably, at least 1.2 mol %, or at least 1.5 mol %, or at least 1.8 mol %, or at least 2.2 mol % of the repeat units of the polymer (P) are repeat units derived from monomer (M) of general formula (I) or general formula (II) as detailed above.

[0044] It is further understood that at most 4.0 mol %, more preferably at most 3.5 mol %, even more preferably at most 3.0 mol % of the repeat units of the polymer (P) are repeat units derived from monomer (M) of general formula (I) or general formula (II) as detailed above.

[0045] In a preferred embodiment, the polymer (P) comprises at least 1.2 mol % and at most 4.0 mol %, preferably at least 1.5 mol % and at most 3.5 mol %, preferably at least 1.5 mol % and at most 3.0 mol % of repeat units derived from at least one monomer (M) of general formula (I) or general formula (II) as detailed above.

[0046] When the repeat units in the polymer (P) are derived from monomers (M) of general formula (II), it is understood that the repeat units are the result of ring-opening polymerization of epoxide moieties.

[0047] It will be appreciated that when the repeat units in polymer (P) are derived from monomer (M) of general formula (I) where X is an acyl chloride or acyl bromide, the repeat units can form ester moieties by being the result of a reaction between monomer (M) and, for example, a terminal OH group of an EO or PO unit of a dihydroxy-terminated polyethylene oxide (or PEO-co-PPO copolymer).

[0048] When the repeat units in polymer (P) are derived from monomer (M) of general formula (I) where X is trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate, or methanesulfonate, the repeat units can be the result of a Williamson-type reaction between said monomer (M) and, for example, the terminal OH groups of the EO or PO units of a dihydroxy-terminated polyethylene oxide (or PEO-co-PPO copolymer) in the presence of a strong base such as NaH to form ether moieties via alcoholate formation and subsequent displacement of the X moiety of monomer (M).

[0049] These polymerization reactions are known in the art and are described, inter alia, by H.-Q. Xie, J.-S. Guo, G.-Q. Yu, and J. Zu, in Journal of Applied Polymer Science 2001, 80, 2446.

[0050] Preferably, each X in the monomer (M) of general formula (I) is a halide, more preferably a halide selected from the group consisting of chloride, bromide, and iodide.

[0051] According to a preferred embodiment of the polymer electrolyte suitable for use in lithium ion secondary batteries, the monomer (M) is represented by the formula (II)

[0052] [ka]

[0053] (In the formula, Each of R1 and R2 is the same or different from each other, and in each occurrence, 1-2 alkanediyl, where n is an integer 0 or 1, preferably n is 1.

[0054] In another preferred embodiment of the polymer electrolyte suitable for use in lithium ion secondary batteries, the monomer (M) according to the invention is represented by the formulas (IA) to (IF) and (IIA) to (IIE):

[0055] [ka]

[0056] [ka]

[0057] [ka]

[0058] [ka]

[0059] [ka]

[0060] [ka]

[0061] [ka]

[0062] [ka]

[0063] [ka]

[0064] [ka]

[0065] [ka]

[0066] wherein X is selected from the group consisting of halides, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate, and methanesulfonate, acyl chloride, and bromoacyl bromide. Preferably, X is a halide, more preferably a halide selected from the group consisting of chloride, bromide, and iodide. Even more preferably, X is a bromide.

[0067] More preferably, the monomer (M) according to the invention is a compound selected from among those of formulae (IA) to (IF).

[0068] Most preferably, the monomer (M) is a compound of formula (IA).

[0069] According to a preferred embodiment of the polymer electrolyte suitable for use in lithium-ion secondary batteries, the polymer (P) essentially consists of a) 94.0 to 98.5 moles of EO repeat units; b) 0.5 to 3.0 mol % of PO repeating units; c) 1.0 to 3.0 mol % of a compound of general formula (II):

[0070] [ka]

[0071] wherein each of R1 and R2 is the same or different from the other and in each occurrence is a C1-2 alkanediyl, and n is an integer 0 or 1, preferably n is 1. It is understood that chain defects or very small amounts of other units may be present, and that these latter do not substantially alter the properties of the polymer (P).

[0072] Preferably, said polymer (P) as detailed above has a Mw (weight average molecular weight) of at least 10000 g / mol, more preferably at least 20000 g / mol, even more preferably at least 40000 g / mol, even more preferably at least 50000 g / mol.

[0073] It is understood that the polymer (P), as detailed above, preferably has a Mw of at most 150000 g / mol, more preferably at most 100000 g / mol.

[0074] In a preferred embodiment, the polymer (P) has a Mw, as detailed above, of at least 10000 g / mol and at most 150000 g / mol, preferably at least 20000 g / mol and at most 150000 g / mol, more preferably at least 40000 g / mol and at most 100000 g / mol, even more preferably at least 50000 g / mol and at most 100000 g / mol.

[0075] According to the present invention, Mw is measured by GPC using calibration with PEO standards, therefore the Mw stated is the PEO equivalent weight.

[0076] Alternatively and more preferably, the polymer (P) as detailed above has a Mn (number average molecular weight) of at least 10000 g / mol, more preferably at least 20000 g / mol, even more preferably at least 40000 g / mol, even more preferably at least 50000 g / mol.

[0077] It is understood that the polymer (P), as detailed above, preferably has a Mn of at most 150 000 g / mol, more preferably at most 100 000 g / mol.

[0078] In a preferred embodiment, the polymer (P) has a Mn, as detailed above, of at least 10000 g / mol and at most 150000 g / mol, preferably at least 20000 g / mol and at most 150000 g / mol, more preferably at least 40000 g / mol and at most 100000 g / mol, even more preferably at least 50000 g / mol and at most 100000 g / mol.

[0079] According to the present invention, Mn is measured by GPC using calibration with PEO standards, therefore the Mn referred to is the PEO equivalent.

[0080] Preferably, the polymer (P) according to the invention is a random or block copolymer, more preferably a random copolymer.

[0081] Preferably, the polymer (P) according to the invention is linear or branched, more preferably linear.

[0082] Particularly preferred polymers (P) have a main chain which is in particular of formula (IV):

[0083] [ka]

[0084] (wherein the ratio of o to q (o / q) in formula (IV) of polymer (P) is 25 to 100, or 35 to 75, or 40 to 60.) The ratio of p to q (p / q) in formula (IV) of polymer (P) is advantageously 0.05 to 1.50, preferably 0.10 to 1.00, and preferably 0.20 to 0.60.

[0085] Such polymers (P) are in particular commercially available under the trade names Alkox® CP-A series from Meisei Chemical works ltd.

[0086] As described above, the compound of formula (III):

[0087] [ka]

[0088] (In the formula, Each of R3, R4, R5, R6, and R7 is the same or different from each other, and in each occurrence, independently represents 1-6 Alkyl, C 3-6 Cycloalkyl, aryl, C 1-6 alkoxy, heterocyclyl, 1-6 Alkyl, C 3-6 Cycloalkyl, aryl, C 1-6 Alkoxy, heterocyclyl, halide, C 1-4 Alkyl, C 3-6 cycloalkyl, CF3, OR9, each of which is the same or different from each other and, at each occurrence, is independently selected from hydrogen, C 1-4 is selected from the group consisting of alkyl, and hydroxyl protecting groups; m is an integer of at least 3, Through reaction of at least a portion of the -CH=CH2 moieties of monomer (M) with the H-Si moieties of the polysiloxane compound having formula (III), as detailed above, it is grafted onto the polymer (P).

[0089] Preferably, each of R3 and R4 is the same or different from each other, and in each occurrence, independently represents 1-6More preferably, each of R3 and R4 is the same or different from each other and, at each occurrence, is methyl, ethyl, propyl, or isopropyl; even more preferably, each of R3 and R4 is the same or different from each other and, at each occurrence, is methyl.

[0090] Preferably, each of R5 and R6 is the same or different from each other, and in each occurrence, independently represents 1-4 alkyl or phenyl, 1-4 Alkyl is a halide, C 1-4 More preferably, each of R5 and R6 is the same or different from each other and is methyl, ethyl, propyl, or isopropyl at each occurrence; and even more preferably, each of R5 and R6 is the same or different from each other and is methyl at each occurrence.

[0091] Preferably, each R7 is C 1-6 alkyl, and more preferably each R7 is C 1-4 It is alkyl, for example, methyl, ethyl, n-propyl, iso-propyl, n-butyl, iso-butyl, or tert-butyl.

[0092] Preferably, m is an integer of at least 5, more preferably at least 7, and even more preferably at least 8.

[0093] It is further understood that m is preferably an integer of at most 1000, more preferably at most 500, even more preferably at most 100, even more preferably at most 20, and even more preferably at most 15.

[0094] In preferred embodiments of the invention, m is an integer of at least 5 and at most 1000, preferably at least 5 and at most 500, more preferably at least 5 and at most 100, even more preferably at least 5 and at most 20, even more preferably at least 7 and at most 20, even more preferably at least 8 and at most 15.

[0095] Within the context of the present invention, it is understood that the -CH=CH2 moiety of the monomer (M) can react with the H-Si moiety of the polysiloxane compound having formula (III) to obtain a covalent bond between both moieties, as detailed above. Such a reaction is generally referred to as a hydrosilylation reaction. It is further understood that the reaction can involve the formation of one or more intermediates, including metal complexes and sigma complexes.

[0096] As detailed above, several techniques known in the art can be successfully used to react at least a portion of the -CH=CH2 moieties of monomer (M) with the H-Si moieties of the polysiloxane compound having formula (III) detailed above.

[0097] The polymer (P) detailed above and the polysiloxane having the formula (III) detailed above can in particular be reacted in the molten state, for which purpose melt compounders such as extruders, melt kneaders or other devices can be advantageously used.

[0098] The polymer (P) as detailed above and the polysiloxane having formula (III) as detailed above can be reacted in particular in solution, and according to this embodiment, the polymer (P) and the polysiloxane having formula (III) as detailed above are at least partially dissolved in a solvent. Dissolution can be obtained at room temperature or upon heating, preferably to at least 70°C, more preferably to at least 80°C, even more preferably at the reflux temperature of the solvent. The choice of this solvent is not critical, as long as it effectively solvates both the polymer (P) and the polysiloxane having formula (III), as detailed above, and does not interfere with the hydrosilylation reaction. Generally, an organic solvent is preferably selected. Among these organic solvents, mention may be made in particular of benzene, toluene, xylene, cymene, etc.

[0099] Furthermore, the polymer (P) as detailed above and the polysiloxane having the formula (III) as detailed above can in particular be reacted in the presence of a catalyst, in particular a hydrosilylation catalyst.

[0100] Such hydrosilylation catalysts are known in the art and may include, inter alia, ruthenium, platinum, or rhodium based catalysts such as Karstedt's catalyst, Wilkinson's catalyst, Speier's catalyst, and mixtures thereof.

[0101] In the context of the present invention, the expression "through the reaction of at least a portion of the -CH=CH2 of the monomer (M) with the H-Si moiety of the polysiloxane compound having formula (III)" means that only a portion or all of the -CH=CH2 of the monomer (M) can react with the H-Si moiety of the polysiloxane compound having formula (III).

[0102] Preferably, the polysiloxane compound having formula (III) as detailed above is grafted to the polymer (P) as detailed above via reaction of at least 10 mol%, more preferably at least 15 mol%, even more preferably at least 20 mol%, even more preferably at least 25 mol%, even more preferably at least 30 mol%, even more preferably at least 35 mol%, even more preferably at least 40 mol%, even more preferably at least 45 mol% of the -CH=CH2 moieties of the monomer (M) with the H-Si moieties of the polysiloxane compound having formula (III).

[0103] It is further understood that the polysiloxane compound having formula (III) as detailed above can be grafted to the polymer (P) as detailed above via reaction of 100 mol%, preferably at most 95 mol%, more preferably at most 90 mol%, even more preferably at most 85 mol%, even more preferably at most 80 mol%, even more preferably at most 75 mol%, even more preferably at most 70 mol%, even more preferably at most 65 mol%, even more preferably at most 60 mol% of the -CH=CH2 moieties of the monomer (M) with the H-Si moieties of the polysiloxane compound having formula (III).

[0104] In a preferred embodiment, the polysiloxane compound having formula (III) as detailed above is grafted to the polymer (P) as detailed above via reaction of at least 10 mol % and at most 90 mol %, more preferably at least 30 mol % and at most 70 mol %, even more preferably at least 40 mol % and at most 60 mol % of the -CH=CH2 moieties of the monomer (M) with the H-Si moieties of the polysiloxane compound having formula (III).

[0105] The reaction can be carried out in particular by GPC or 1 It can be monitored by using known analytical methods, such as using 1 H-NMR techniques.

[0106] Preferably, the polymer electrolyte is obtained by reaction between the at least one polymer (P) and at least 6% by weight, or at least 7% by weight, or at least 8% by weight, of the at least one polysiloxane compound relative to the total amount of the at least one polymer (P) and the at least one polysiloxane compound.

[0107] Preferably, the polymer electrolyte is obtained by reaction between the at least one polymer (P) and at most 27% by weight, or at most 25% by weight, or at most 22% by weight, of the at least one polysiloxane compound relative to the total amount of the at least one polymer (P) and the at least one polysiloxane compound.

[0108] In a preferred embodiment, the polymer electrolyte is obtained by reaction between the at least one polymer (P) and at least 6% by weight and at most 27% by weight, or at least 7% by weight and at most 25% by weight, or at least 8% by weight and at most 22% by weight, of the at least one polysiloxane compound, relative to the total amount of the at least one polymer (P) and the at least one polysiloxane compound.

[0109] [Example] The following examples are intended to further clarify the invention, but are not intended to limit the scope of the invention.

[0110] 1. Example 1 1.1. Materials and methods Unless otherwise stated, the following materials were used as described below.

[0111] The random polymer (P) was purchased from Meisei Chemical Industry Co., Ltd. under the trade name CP-A of the CP series. Alternatively, the polymer (P) can be prepared by the following procedure disclosed in H.-Q. Xie, J.-S. Guo, G.-Q. Yu, and J. Zu, Journal of Applied Polymer Science 2001, 80, 2446.

[0112] Monohydride-terminated polydimethylsiloxane (SiH-terminated PDMS, M w = 850 g / mol) was purchased from Gelest, Inc.

[0113] The silica-supported Karstedt-type catalyst was prepared according to Q. J. Miao, Z.-P. Fang, and G. P. Kai, Catalysis Communications 2003, 4, 637-639.

[0114] LiTFSI (lithium bis(trifluoromethanesulfonyl)imide salt, 99.95% trace metals basis) was purchased from Sigma-Aldrich.

[0115] 99.8 wt % anhydrous acetonitrile was purchased from Sigma-Aldrich.

[0116] Timcal Super P is a conductive carbon black powder (CAS number 1333-86-4) manufactured by Imerys Graphite & Carbon.

[0117] Polyethylene oxide (1,000,000 M w The PEO having the formula (I) was purchased from Alfa Aesar.

[0118] 1 H spectra were recorded on a JEOL JNM ECZ 500 MHz NMR spectrometer at room temperature. Polymer samples were dissolved in CDCl3 and the internal standard was optimized using tetramethylsilane (TMS).

[0119] Inductively Coupled Plasma (ICP) measurements were performed using an Agilent 720 ICP-OES (Agilent Technologies, https: / / www.agilent.com / cs / library / brochures / 5990-6497EN%20720-725_ICP-OES_LR.pdf). One gram of powder sample is dissolved in 50 mL of high-purity hydrochloric acid (at least 37 wt% HCl with respect to the total weight of the solution) in an Erlenmeyer flask. The flask is covered with a watch glass and heated on a hot plate at 380 °C until the powder is completely dissolved. After cooling to room temperature, the solution from the Erlenmeyer flask is poured into a first 250 mL volumetric flask. The first 250 mL volumetric flask is then filled up to the mark with deionized water, followed by a complete homogenization procedure (first dilution). Pipette an appropriate amount of the solution from the first volumetric flask and transfer it to a second 250 mL volumetric flask for the second dilution, fill the second volumetric flask up to the 250 mL mark with the internal standard and 10% hydrochloric acid, then homogenize. Finally, use this solution for ICP measurement.

[0120] 1.2. Preparation of polymer electrolyte Polymer (P), a random linear copolymer whose characteristics are shown in Table 1, is reacted with monohydride-terminated polydimethylsiloxane (SiH-terminated PDMS) by hydrosilylation according to the following procedure.

[0121] [Table 1]

[0122] A mixture containing 2.0 g of polymer (P) and 0.36 g of SiH-terminated PDMS is added to 50 mL of benzene containing 20 mg of silica-supported Karstedt-type catalyst and heated at 90° C. for 48 hours under nitrogen atmosphere.

[0123] The heated mixture was filtered through Celite to remove the solid catalyst and then placed under reduced pressure to remove the solvent.PDMS was grafted to the polymer (P) via the reaction of -CH=CH2 of 50 mol% of the AGE units with the H-Si moieties of PDMS.

[0124] The success of grafting is 1 The results were confirmed by H-NMR and GPC (gel permeation chromatography).

[0125] Polymer (P): 1 H-NMR (TMS, CDCl3, 500 MHz): δ (ppm) 1.2 (d, CH3 of PO unit), 4 (m, -OCH2-CH=CH2 of AGE unit), 5.2 (m, CH2=CH- of AGE unit), 5.8 (m, -CH=CH2 of AGE unit).

[0126] Monohydride PDMS: 1 H-NMR (TMS, CDCl3, 500MHz): δ(ppm) 0.5(m,-Si-CH2-CH2-), 0.9(t,CH3-CH2-), 1.3(br,-Si-CH2-CH2-CH2-CH3), 4.8(m,H-Si-).

[0127] Polymer electrolyte: 1 H-NMR (TMS, CDCl3, 500 MHz): δ (ppm): 0.5 (br, -Si-CH2-CH2- of PDMS), 0.9 (br, CH3-CH2- of PDMS), 1.1 (d, CH3 of PO units), 1.2 (br, -Si-CH2-CH2-CH2-CH3 of PDMS), 1.4 (br, -OCH2-CH2-CH2-Si-).

[0128] The presence of a broad peak at 1.4 ppm and the absence of peaks assigned to H-Si in the 1H-NMR spectrum of the polyelectrolyte indicates successful hydrosilylation.

[0129] FIG. 1 shows the GPC elution curves of the above prepared polymer electrolyte, polymer (P), and polysiloxane.

[0130] The shorter elution time of the polymer electrolyte compared to the polymer (P) indicates that the polymer electrolyte has a higher molecular weight than the polymer (P) and therefore PDMS was successfully grafted onto the polymer (P).

[0131] 1.3. Preparation of positive electrode active material Measured by ICP, the general formula Li 1.010 (Ni 0.621 Mn 0.224 Co 0.155 ) 0.990 O 2.00 A lithium transition metal composite oxide having the formula: is prepared as a positive electrode active material according to the following process.

[0132] Step 1) Preparation of transition metal oxide-hydroxide precursors: Metal composition measured by ICP: Ni 0.621 Mn 0.224 Co 0.155 Nickel-based transition metal oxide hydroxide powder (TMH1) having the formula (I) is prepared by co-precipitation in a large-scale continuous stirred tank reactor (CSTR) with mixed nickel manganese cobalt sulfate, sodium hydroxide, and ammonia.

[0133] Step 2) First Mixing: TMH1 prepared in step 1) is mixed with Li2CO3 in an industrial blender to obtain a first mixture with a lithium to metal ratio of 0.85.

[0134] Step 3) First calcination: The first mixture from step 2) is calcined at 900°C for 10 hours in a dry air atmosphere to obtain a first calcined cake. The first calcined cake is pulverized to obtain a first calcined powder.

[0135] Step 4) Second mixing: The first calcined powder from step 3) is mixed with LiOH in an industrial blender to obtain a second mixture with a lithium to metal ratio of 1.01.

[0136] Step 5) Second calcination: The second mixture from step 4) is calcined at 930°C for 10 hours in dry air, followed by grinding (bead milling) and sieving process to obtain the second calcined powder.

[0137] Step 6) Third Mixing: The second calcined powder from step 5) is mixed with 1.5 mol% LiOH with respect to the total molar content of Ni, Mn, and Co in an industrial blender to obtain a third mixture.

[0138] Step 7) Third calcination: The third mixture from step 6) is calcined at 750° C. for 10 hours in dry air to obtain a positive electrode active material.

[0139] 1.4. Preparation of the positive electrode A positive electrode comprising the positive electrode active material prepared according to section 1.3 and the polymer electrolyte prepared according to section 1.2 is prepared according to the following procedure.

[0140] Step 1), preparing a polymer electrolyte solution comprising the polymer electrolyte according to section 1.1 and LiTFSI in 99.8 wt % anhydrous acetonitrile, the polymer electrolyte solution having a polymer electrolyte:LiTFSI weight ratio of 74:26.

[0141] Step 2) Mix the polymer electrolyte solution prepared in step 1), the cathode active material prepared according to section 1.2, and carbon black powder (Timcal Super P carbon black) in acetonitrile solution in a weight ratio of 21:75:4 to prepare a slurry mixture. Mixing is performed by a homogenizer at 5000 rpm for 45 minutes.

[0142] Step 3) Casting the slurry mixture from step 2) onto one side of a 20 μm thick aluminum foil with a coater gap of 100 μm.

[0143] Step 4) The foil on which the slurry was cast was dried at 30° C. for 12 hours and then punched out to obtain a positive electrode with a diameter of 14 mm.

[0144] 1.5. Preparation of solid polymer electrolyte (SPE) A PEO-based solid polymer electrolyte (SPE) is prepared according to the following process.

[0145] Step 1) Mix polyethylene oxide (PEO with a molecular weight of 1,000,000) and LiTFSI (purchased from Soulbrain Co., Ltd., not Sigma Aldrich) in 99.8% by weight anhydrous acetonitrile using a mixer at 2,000 revolutions per minute (rpm) for 30 minutes. The molar ratio of ethylene oxide to lithium is 20.

[0146] Step 2) Pour the mixture from step 1) into a Teflon dish and dry at 25° C. for 12 hours.

[0147] Step 3) Remove the dried SPE from the dish and punch out the dried SPE to obtain an SPE disk with a thickness of 300 μm and a diameter of 19 mm.

[0148] 1.6. Polymer cell assembly Assemble a coin-shaped polymer cell in an argon-filled glove box in the following order from bottom to top: 2032 coin cell can, positive electrode prepared according to section 1.4, SPE polymer electrolyte prepared according to section 1.5, gasket, Li anode, spacer, wave spring, and cell cap. The coin cell is then completely sealed to prevent electrolyte leakage.

[0149] 2. Comparative Example 2.1. Polymer electrolytes Instead of a polymer electrolyte according to the invention, poly(ethylene oxide) (PEO) powder (Mw of 1,000,000 g / mol) purchased from Alfa Aesar is used.

[0150] 2.2. Preparation of the positive electrode A positive electrode comprising the positive electrode active material prepared according to section 1.3 and the polymer electrolyte according to section 2.1 is prepared according to the following procedure.

[0151] Step 1) Prepare a polymer electrolyte solution comprising the polymer electrolyte according to section 2.1 and lithium LiTFSI in 99.8 wt% anhydrous acetonitrile, the polymer electrolyte solution having a polymer electrolyte:LiTFSI weight ratio of 74:26.

[0152] Step 2) Mix the prepared polymer electrolyte solution from step 1), the positive electrode active material prepared according to section 1.3, and carbon black powder (Timcal Super P carbon black) in acetonitrile solution in a weight ratio of 21:75:4 to prepare a slurry mixture. Mixing is performed by a homogenizer at 5000 rpm for 45 minutes.

[0153] Step 3) Casting the slurry mixture from step 2) onto one side of a 20 μm thick aluminum foil with a coater gap of 100 μm.

[0154] Step 4) The foil on which the slurry was cast was dried at 30° C. for 12 hours and then punched out to obtain a positive electrode with a diameter of 14 mm.

[0155] 2.3. Polymer cell assembly Assemble a coin-shaped polymer cell in an argon-filled glove box from bottom to top: 2032 coin cell can, the prepared positive electrode from section 2.2, the prepared SPE from section 1.5, a gasket, a Li anode, a spacer, a wave spring, and a cell cap. The coin cell is then completely sealed to prevent electrolyte leakage.

[0156] 3. Comparison and Testing Methods (Qtotal) The leakage capacity (Qtotal) was measured for the coin cells prepared in Section 2.3 and Section 1.6, the coin cells prepared in Section 2.3 containing a polymer electrolyte according to the current art and the coin cells prepared in Section 1.6 containing a polymer electrolyte according to the present invention.

[0157] Each coin-shaped polymer cell was placed in a Toscat-3100 computer-controlled constant current cycling station (Toyo Systems, http: / / www.toyosystem.com / image / menu3 / toscat / TOSCAT-3100.pdf) and cycle at 80°C. The coin cell test procedure uses a 1C current definition of 160mA / g over the 4.4~3.0V / Li metal window range according to the schedule below.

[0158] Step 1) Charge in constant current mode at a C rate of 0.05 with an end condition of 4.4V, followed by a 10 minute rest.

[0159] Step 2) Discharge in constant current mode at a C rate of 0.05 with an end condition of 3.0 V, followed by a 10 minute rest.

[0160] Step 3) Charge in constant current mode at a C rate of 0.05 with an end condition of 4.4V.

[0161] Step 4) Switch to constant voltage mode and maintain 4.4V for 60 hours.

[0162] Step 5) Discharge in constant current mode at a C rate of 0.05 with an end condition of 3.0V.

[0163] Q total Q is defined as the total leakage capacitance at high voltage and temperature in step 4) according to the described test method. total A small value of indicates that the positive electrode active material powder has high stability during high temperature operation.

[0164] [Table 2]

[0165] Table 2 shows the Q values ​​of the polymer batteries containing the positive electrodes prepared in Section 1.6 of Example 1 and Section 2.3 of the Comparative Example. total According to Table 2, the polymer battery containing the polymer electrolyte according to the present invention (Example 1) has a significantly lower Q than the polymer battery containing the polymer electrolyte according to Comparative Example 2. total This indicates that the use of the polymer electrolyte according to the present invention results in better electrochemical performance than the use of the conventional polymer electrolyte, PEO. total A small value of indicates that the stability of the lithium ion secondary battery is high when a high voltage is applied at a high temperature.

Claims

1. A positive electrode for a lithium ion secondary battery comprising a positive electrode active material and a polymer electrolyte, The polymer electrolyte is i. at least one polyether polymer, hereinafter polymer (P), comprising: a) at least 70.0 mol % oxyethylene units (EO); b) 0.0 to 10.0 mole % of oxypropylene units (PO), and c) 1.00 to 4.0 mol % of a compound represented by general formula (I) or general formula (II): 【Chemistry 1】 or 【Chemistry 2】 (In the formula, R 1 and R 2 are the same or different from each other, and in each occurrence, C 1-6 alkanediyl, 1-6 Alkanediyl is a halide, C 1-4 Alkyl, C 3-6 Cycloalkyl, CF 3 , OR 8 and R 8 are the same or different from one another and, in each occurrence, independently represent hydrogen and C 1-4 alkyl, n is an integer 0 or 1 or 2; Each X is a leaving group selected from the group consisting of halide, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate, and methanesulfonate. A repeating unit derived from at least one monomer of the formula (hereinafter, referred to as monomer (M)). A polymer (P) comprising ii. Formula (III): 【Chemistry 3】 (In the formula, R 3 , R 4 , R 5 , R 6 , and R 7 are the same or different from one another, and each occurrence independently represents 1-6 Alkyl, C 3-6 Cycloalkyl, aryl, C 1-6 alkoxy, heterocyclyl, 1-6 Alkyl, C 3-6 Cycloalkyl, aryl, C 1-6 Alkoxy, heterocyclyl are halide, C 1-4 Alkyl, C 3-6 Cycloalkyl, CF 3 , OR 9 and R 9 are the same or different from one another and, in each occurrence, independently represent hydrogen, C 1-4 is selected from the group consisting of alkyl, and hydroxyl protecting groups; and m is an integer of at least 3; The at least one polysiloxane compound having the formula (III) is a monomer (M) having the -CH=CH 2 1. A positive electrode for a lithium ion secondary battery, comprising at least one polymer (P) grafted thereto via reaction of at least a portion of said moieties with the H-Si moieties of said polysiloxane compound having formula (III):

2. 2. The positive electrode for a lithium ion secondary battery according to claim 1, wherein 80.0 mol % to 99.0 mol % of the repeating units of the polymer (P) are EO units.

3. 3. The positive electrode for a lithium ion secondary battery according to claim 1, wherein 0.5 mol % to 5.0 mol % of the repeating units of the polymer (P) are PO units.

4. The repeating units of the polymer (P) are each represented by the general formula (I) or the general formula (II) (wherein R 1 , R 2 4. The positive electrode for a lithium ion secondary battery according to claim 1, wherein n is a repeating unit derived from the monomer (M) of the formula (I), ...

5. The monomer (M) is represented by the formula (II) 【Chemistry 4】 (In the formula, R 1 and R 2 are the same or different from each other, and in each occurrence, C 1-2 The positive electrode for a lithium ion secondary battery according to any one of claims 1 to 4, wherein n is an integer of 0 or 1.

6. The positive electrode for a lithium ion secondary battery according to any one of claims 1 to 5, wherein the polymer (P) is a random copolymer having a Mn (number average molecular weight) of at least 10,000 g / mol and at most 150,000 g / mol.

7. R 3 , R 4 , and R 7 are the same or different from one another, and each occurrence independently represents 1-6 alkyl, R 5 and R 6 are the same or different from one another, and each occurrence independently represents 1-4 alkyl or phenyl, 1-4 Alkyl is halide, C 1-4 Alkyl or CF 3 and m is an integer of at least 5 and at most 1000.

8. The positive electrode for a lithium ion secondary battery according to any one of claims 1 to 7, wherein the polymer (P) and the polysiloxane compound having the formula (III) are at least partially dissolved in an organic solvent selected from the group consisting of benzene, toluene, xylene, and cymene.

9. The positive electrode for lithium ion secondary batteries according to any one of claims 1 to 8, wherein the polysiloxane compound having the formula (III) is grafted to the polymer (P) in the presence of a catalyst.

10. The positive electrode for lithium ion secondary batteries according to any one of claims 1 to 9, wherein the polysiloxane compound having the formula (III) is grafted to the polymer (P) in the presence of a hydrosilylation catalyst selected from among Karstedt's catalyst, Wilkinson's catalyst, Speyer's catalyst, or a mixture thereof.

11. The polysiloxane compound having the formula (III) is a monomer (M) having the -CH=CH 2 11. The positive electrode for a lithium ion secondary battery according to claim 1, wherein at least 10 mol % and at most 90 mol % of the moiety is grafted to the polymer (P) via reaction with the H-Si moiety of the polysiloxane compound having the formula (III).

Citation Information

Patent Citations

  • Lithium low-conductive polyelectrolyte

    JP1991190960A

  • Silicone-group-containing polyoxyalkylene compound

    JP1996165349A

  • Gel electrolyte for lithium secondary battery

    JP2000154254A

  • Cross-linked polymer solid electrolyte and battery