Surface shaping method and surface shaping device
The use of X-ray lasers with controlled wavelengths and energy densities addresses the complexity of lithography, enabling direct and efficient surface modeling for precise features like pores and patterns at high resolution.
Patent Information
- Application Number
- JP2020195528
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-28
- Filing Date
- 2020-11-25
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-11-25
AI Technical Summary
Current surface modeling technologies, such as lithography, require multiple complex steps and are not suitable for mass production and cost-effective manufacturing at resolutions of 10 nm or less.
A surface modeling method using X-ray lasers with wavelengths between 1 nm and 200 nm and pulse widths of 1×10^-18 to 1×10^-10 seconds, along with precise control of irradiation energy density and wavelength selection, to directly shape surfaces without the need for multiple lithography processes.
This method allows for simpler and more direct surface modeling, enabling the formation of precise features like pores, holographic patterns, and lattice patterns with reduced rim formation and improved accuracy.
Smart Images

Figure 0007590708000001 
Figure 0007590708000002 
Figure 0007590708000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface shaping method and a surface shaping apparatus. [Background technology]
[0002] Currently, surface modeling technology with a resolution of 10 nm or less is realized by lithography using a so-called low-strength, low-temperature modeling process. Summary of the Invention [Problem to be solved by the invention]
[0003] However, since the lithography process involves many steps from exposure to development to create a pattern, direct precision processing technology (in other words, a surface modeling method) using simpler processes is needed to achieve further mass production and lower costs. [Means for solving the problem]
[0004] In order to solve the above problems, a surface shaping method according to a first aspect of the present invention includes a wavelength selection step of selecting an irradiation wavelength, which is the wavelength of an X-ray laser to be irradiated to a target surface, from a range of 1 nm to 200 nm inclusive in accordance with a wavelength corresponding to an inner shell absorption edge of a material constituting the surface of the target, an irradiation density selection step of selecting an irradiation energy density, which is the energy density of the X-ray laser, in accordance with an aspect of surface shaping to be performed on the surface, and a laser having the irradiation wavelength and the irradiation energy density and having a pulse width of 1×10 -18 1×10 seconds or more -10 and irradiating the surface with an X-ray laser for a period in the range of 1000 to 2000 s.
[0005] According to the above configuration, the irradiation wavelength is in the range of 1 nm to 200 nm, and the pulse width is 1×10 -18 1×10 seconds or more -10By irradiating a surface of a target with an X-ray laser having a wavelength in the range of 1000 nm to 1500 nm and an irradiation energy density appropriately selected, surface shaping can be performed on the surface. This surface shaping method does not require multiple processes as in conventional lithography processes, and is therefore a simpler and more direct surface shaping method compared to lithography processes.
[0006] A surface shaping method according to a second aspect of the present invention, in addition to the configuration of the surface shaping method according to the first aspect described above, adopts a configuration in which, when the surface shaping mode is the formation of pores, the wavelength selection step selects as the irradiation wavelength a wavelength shorter than the wavelength corresponding to the inner shell absorption edge, and the irradiation density selection step selects as the irradiation energy density an energy density exceeding a predetermined processing threshold.
[0007] According to the above-mentioned configuration, a pore can be formed in which the generation of a rim portion is suppressed near the outer edge of the irradiation area irradiated with the X-ray laser on the surface of the target. In this specification, the rim portion refers to a raised portion that may be generated in a ring shape near the outer edge of the pore, that is, a portion having an unintended structure caused by heat influence. The portion having an unintended structure caused by heat influence is sometimes called a HAZ (Heat Affected Zone).
[0008] A surface shaping method according to a third aspect of the present invention, in addition to the configuration of the surface shaping method according to the first aspect described above, further includes a diffraction step of obtaining a diffracted X-ray laser from the X-ray laser by passing through a diffractive optical element such as a slit when the surface shaping aspect is the formation of a holographic pattern, the wavelength selection step selects a wavelength shorter than a wavelength corresponding to the inner shell absorption edge as the irradiation wavelength, the irradiation density selection step selects an energy density exceeding 90% of a predetermined processing threshold as the irradiation energy density, and the irradiation step selects an irradiation wavelength and an irradiation energy density and a pulse width of 1×10 -18 1×10 seconds or more -10The surface is irradiated with the diffracted x-ray laser having a wavelength in the sub-second range.
[0009] According to the above configuration, a holographic pattern can be formed in the area of the target surface that is irradiated with the X-ray laser.
[0010] A surface shaping method according to a fourth aspect of the present invention has the same configuration as the surface shaping method according to the first aspect described above, and in addition, when the aspect of the surface shaping is the formation of a lattice pattern, the wavelength selection step selects a wavelength shorter than a wavelength corresponding to the inner shell absorption edge as the irradiation wavelength, the irradiation density selection step selects an energy density below a predetermined processing threshold as the irradiation energy density, and the irradiating step selects a pulse having the irradiation wavelength and the irradiation energy density and having a pulse width of 1×10 -18 1×10 seconds or more -10 The surface is irradiated with multiple shots of the X-ray laser, the duration of which is in the range of 1 / 2 second or less.
[0011] According to the above configuration, a lattice pattern can be formed in the area of the surface of the target that is irradiated with the X-ray laser.
[0012] A surface shaping method according to a fifth aspect of the present invention employs, in addition to the configuration of any one of the first to fourth aspects described above, a configuration in which the material is silicon or silicon nitride.
[0013] Thus, silicon or silicon nitride is suitable as the target material.
[0014] In order to solve the above problems, a surface shaping apparatus according to a sixth aspect of the present invention is a surface shaping apparatus that irradiates an X-ray laser onto a surface of a target, the surface shaping apparatus comprising: a wavelength selection unit that selects an irradiation wavelength, which is the wavelength of the X-ray laser, from a range of 1 nm to 200 nm inclusive in accordance with a wavelength corresponding to an inner shell absorption edge of a material that constitutes the surface; an irradiation density selection unit that selects an irradiation energy density, which is the energy density of the X-ray laser, in accordance with an aspect of surface shaping to be performed on the surface; and a laser beam shaping unit that has the irradiation wavelength and the irradiation energy density and has a pulse width of 1×10 -18 1×10 seconds or more -10 and an irradiation mechanism for irradiating the surface with an X-ray laser having a wavelength in the range of 1000 nm to 1000 nm.
[0015] According to the above configuration, the same effects as those of the surface shaping method according to the first aspect of the present invention are achieved.
[0016] A surface shaping apparatus according to a seventh aspect of the present invention has, in addition to the configuration of the surface shaping apparatus according to the sixth aspect described above, a configuration in which, when the surface shaping mode is the formation of pores, the wavelength selection unit selects as the irradiation wavelength a wavelength shorter than the wavelength corresponding to the inner shell absorption edge, and the irradiation density selection unit selects as the irradiation energy density an energy density exceeding a predetermined processing threshold.
[0017] According to the above configuration, the same effects as those of the surface shaping method according to the second aspect of the present invention are achieved.
[0018] A surface shaping apparatus according to an eighth aspect of the present invention, in addition to the configuration of the surface shaping apparatus according to the sixth aspect described above, further comprises a slit for obtaining a diffracted X-ray laser by passing the X-ray laser when the surface shaping aspect is the formation of a holographic pattern, the wavelength selection unit selects a wavelength shorter than a wavelength corresponding to the inner shell absorption edge as the irradiation wavelength, the irradiation density selection unit selects an energy density exceeding 90% of a predetermined processing threshold as the irradiation energy density, and the irradiation mechanism has the irradiation wavelength and the irradiation energy density and has a pulse width of 1×10 -18 1×10 seconds or more -10The surface is irradiated with the diffracted x-ray laser having a wavelength in the sub-second range.
[0019] According to the above configuration, the same effects as those of the surface shaping method according to the third aspect of the present invention can be achieved.
[0020] A surface shaping apparatus according to a ninth aspect of the present invention has the same configuration as the surface shaping apparatus according to the sixth aspect described above, and further comprises: when the aspect of the surface shaping is the formation of a lattice pattern, the wavelength selection unit selects a wavelength shorter than a wavelength corresponding to the inner shell absorption edge as the irradiation wavelength; the irradiation density selection unit selects an energy density below a predetermined processing threshold as the irradiation energy density; and the irradiation mechanism has the irradiation wavelength and the irradiation energy density, and has a pulse width of 1×10 -18 1×10 seconds or more -10 The surface is irradiated with multiple shots of the X-ray laser, the duration of which is in the range of 1 / 2 second or less.
[0021] According to the above configuration, the same effects as those of the surface shaping method according to the fourth aspect of the present invention can be achieved.
[0022] A surface shaping device according to a tenth aspect of the present invention, in addition to the configuration of the surface shaping device according to any one of the sixth to ninth aspects described above, further comprises an X-ray laser light source that generates the X-ray laser, a light source control unit that controls the X-ray laser light source, and an X-ray filter, wherein the light source control unit controls the X-ray laser light source so that the wavelength of the X-ray laser becomes the irradiation wavelength, and the X-ray filter reduces the intensity of the X-ray laser so that the energy density of the X-ray laser approaches the irradiation energy density.
[0023] The scope of the present invention includes a surface shaping device that includes such an X-ray laser light source.
[0024] A surface shaping apparatus according to an eleventh aspect of the present invention has the same configuration as the surface shaping apparatus according to any one of the sixth to tenth aspects described above, and further comprises: the X-ray laser light source is a tunable laser light source capable of varying the wavelength of the X-ray laser at least in a range of 1 nm to 200 nm; and the X-ray filter adjusts the energy density in an irradiation spot on the surface to at least 10 mJ / cm. 2 A configuration is adopted in which the voltage is changed within the above range.
[0025] According to the above configuration, surface shaping can be performed on targets whose surfaces are made of various materials. Effect of the Invention
[0026] According to one aspect of the present invention, there is provided a surface shaping method and apparatus that is simpler and more direct compared to lithography processes. [Brief description of the drawings]
[0027] [Figure 1] 1 is a schematic diagram of a surface shaping apparatus according to an embodiment of the present invention; [Diagram 2] FIG. 1A is a front view of the four-quadrant slit in a fully open state, and FIG. 1B is a front view of the four-quadrant slit in a state in which the lower barrier is closed. [Diagram 3] 2 is a functional block diagram of a control unit included in the surface shaping apparatus shown in FIG. 1. [Figure 4] FIG. 1 is a schematic diagram of a target whose surface is irradiated with an X-ray laser. [Diagram 5] 13 is a flowchart of a surface shaping method according to a modified example of the present invention. [Figure 6] Graphs (a) to (f) show the wavelength dependence of the absorption coefficient of silicon, silicon nitride, silicon carbide, sapphire, carbon, and PMMA, respectively. [Figure 7]Graphs (a) to (g) show the wavelength dependence of the absorption coefficient of platinum, gold, aluminum, copper, iron, nickel, and zirconium, respectively. [Figure 8] FIG. 1A is a perspective view of a silicon target obtained according to a first embodiment of the present invention. FIG. 1B is a cross-sectional view of the silicon target shown in FIG. 1A. FIG. 1C and FIG. 1D are perspective views of silicon targets obtained according to a first comparative example and a second comparative example of the present invention, respectively. [Figure 9] 1 is a graph showing wavelength dependence of processing threshold in thermal processing and non-thermal processing. [Figure 10] (a) and (b) are a plan view and a perspective view of a silicon target obtained according to a second embodiment of the present invention, (c) and (d) are a plan view and a perspective view of a silicon target obtained according to a third embodiment of the present invention, and (e) and (f) are a plan view and a perspective view of a silicon target obtained according to a fourth embodiment of the present invention. [Figure 11] FIG. 13 is a plan view of a silicon nitride target obtained according to a fifth embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] [Surface modeling device] A surface shaping device 10 according to an embodiment of the present invention will be described with reference to Figs. 1 to 4. Fig. 1 is a schematic diagram of the surface shaping device 10. Fig. 2(a) is a front view of the four-quadrant slit 12 in a fully open state. Fig. 2(b) is a front view of the four-quadrant slit in a state in which the lower barrier 123 is closed. Fig. 3 is a schematic diagram of a target T whose surface is irradiated with an X-ray laser L generated by an X-ray laser light source 11 provided in the surface shaping device 10. Fig. 4 is a functional block diagram of a control unit 18 provided in the surface shaping device 10.
[0029] As shown in FIG. 1, the surface profiling apparatus 10 includes an X-ray laser light source 11, a quadrant slit 12, a gas energy monitor 13, a K-B mirror 14, an X-ray filter 15, and a personal computer PC. The quadrant slit 12, the gas energy monitor 13, the K-B mirror 14, and the X-ray filter 15 constitute an irradiation mechanism 10A. The irradiation mechanism 10A has an irradiation wavelength selected by a wavelength selection unit 161 shown in FIG. 3 and an irradiation energy density selected by an irradiation density selection unit 162, and has a pulse width of 1×10 -18 seconds or more and 1×10 -10 seconds or less, and irradiates the surface of the target T with an X-ray laser L included in this range. The control unit 16 including the wavelength selection unit 161 and the irradiation density selection unit 162 will be described later with reference to FIG. 3.
[0030] The surface profiling apparatus 10 can perform fine surface profiling on the surface of the target T. Examples of the surface profiling modes include formation of pores, formation of holographic patterns, and formation of lattice patterns.
[0031] In the present embodiment, a single crystal of p-type silicon with a (100) orientation is employed as the target T irradiated with the X-ray laser L. However, the material constituting the target T is not limited to silicon. Other materials constituting the target include, for example, silicon nitride, silicon carbide, sapphire, carbon, polymethylmethacrylate (PMMA), platinum, gold, aluminum, copper, iron, nickel, and zirconium. The form of carbon is not limited, and it may be graphite, graphene, carbon nanofiber, or diamond. PMMA is an example of a resist material used in a lithography process. The material constituting the target T may be a resist material other than PMMA. Note that as the material constituting the target T, silicon or silicon nitride is preferable.
[0032] <X-ray laser light source> The X-ray laser light source 11 has a wavelength in the range of 1 nm to 200 nm and a pulse width of 1×10 -18 1×10 seconds or more -10 A soft X-ray laser source that produces X-rays L in the sub-second range.
[0033] The X-ray laser light source 11 is preferably a wavelength-variable laser light source that can change the wavelength of the X-ray laser L at least in the range of 1 nm or more and 200 nm or less.
[0034] In this embodiment, SACLA (SPring-8 Angstrom Compact Free Electron Laser), which is an example of an X-ray free electron laser (XFEL), is used as the X-ray laser light source 11. The surface shaping device 10 focuses the X-ray laser L generated by the X-ray laser light source 11 and irradiates it onto the surface of the target T. In this embodiment, the pulse width of the X-ray laser L is set to 70×10 -15 seconds (70 femtoseconds). The pulse width of the X-ray laser L is defined using the half-width of the pulse. In this embodiment, the X-ray laser light source 11 is configured so that the polarization direction of the X-ray laser L is parallel to the horizontal plane. However, the polarization direction of the X-ray laser L is not limited to the direction parallel to the horizontal plane.
[0035] However, in one embodiment of the present invention, the X-ray laser source 11 is not limited to SACLA, and may be any source having a wavelength in the range of 1 nm to 200 nm and a pulse width of 1×10 -18 1×10 seconds or more -10 The wavelength of the X-ray laser light source 11 may be appropriately selected from among laser light sources that generate X-ray laser L having a wavelength in the range of 100 s or less. For example, the X-ray laser light source 11 may be an X-ray laser light source using plasma, or an X-ray laser light source that generates an X-ray laser having the above-mentioned wavelength by using high-order harmonics.
[0036] <4-quadrant slit> The quadrant slit 12 is disposed between the X-ray laser light source 11 and a gas energy monitor 13, which will be described later. The quadrant slit 12 has four obstacles 121, 122, 123, and 124 that move independently of each other. The quadrant slit 12 is an example of a slit. The quadrant slit 12 shown in (a) and (b) of FIG. 2 shows a state of being viewed from the front from the X-ray laser light source 11 side. The obstacles 121, 122, 123, and 124 are the upper, right, lower, and left obstacles, respectively. The position of the quadrant slit 12 may be located upstream of the KB mirror 14, which will be described later (X-ray laser light source 11 side), and may be located between the gas energy monitor 13, which will be described later, and the KB mirror, which will be described later.
[0037] The barriers 121 and 123 are arranged so that the long sides of the adjacent sides are spaced apart. In the state shown in FIG. 1, the barriers 121 and 123 can move independently in the vertical direction, so that the interval between the long sides of the barriers 121 and 123 on the adjacent sides (the interval between the slits in the vertical direction) and the position of the slits in the vertical direction can be appropriately changed. Similarly, the barriers 122 and 124 are arranged so that the long sides of the adjacent sides are spaced apart. In the state shown in FIG. 1, the barriers 122 and 124 can move independently in the horizontal direction, so that the interval between the long sides of the barriers 122 and 124 on the adjacent sides (the interval between the slits in the horizontal direction) and the position of the slits in the horizontal direction can be appropriately changed. For example, FIG. 2(a) illustrates the four-quadrant slit 12 in a state in which the barriers 121, 122, 123, and 124 are fully open. 2(b) illustrates the four-quadrant slit 12 with the barrier 123 closed. By closing the barrier 123, the lower half of the X-ray laser L is blocked. As a result, by passing through the four-quadrant slit 12, the X-ray laser L is diffracted by the long side of the barrier 123 on the barrier 121 side. Hereinafter, this diffracted X-ray laser light is referred to as a diffracted X-ray laser.
[0038] In addition, in the present embodiment, the positions of the barriers 121, 122, 123, and 124 of the quadrant slit 12 are controlled by a personal computer PC described later. However, the quadrant slit 12 may be configured to be manually controlled.
[0039] <Gas energy monitor> The gas energy monitor 13 detects the energy of each shot of the X-ray laser L. The energy of the X-ray laser L detected by the gas energy monitor 13 is supplied to the personal computer PC.
[0040] <K-B mirror> The K-B (Kirkpatrick-Baez) mirror 14 focuses the X-ray laser L generated by the X-ray laser light source 11 on the surface of the target T.
[0041] <X-ray filter> The X-ray filter 15 reduces the intensity of the X-ray laser L. In the present embodiment, the X-ray filter 15 is configured using at least one of a plate-like member made of zirconium and a plate-like member made of silicon. The X-ray filter 15 can change the transmittance of the X-ray laser L by appropriately adjusting the number of plate-like members made of zirconium and plate-like members made of silicon having various film thicknesses. As a result, the X-ray filter 15 can adjust the intensity of the X-ray laser L to a desired intensity, so that the energy density at the irradiation spot on the surface of the target T can be adjusted to a desired energy density. Note that the X-ray filter 15 can change the energy density at the irradiation spot within a range of at least 10 mJ / cm 2 It is preferable that the combination of the film thickness and the number of the plate-like members is configured so as to be changeable within the above range.
[0042] As described above, in this embodiment, a (100)-oriented p-type silicon single crystal is used as the target T to be irradiated with the X-ray laser L. The p-type silicon single crystal is arranged on the optical axis of the X-ray laser L so that its main surface is perpendicular to the optical axis. In addition, the X-ray laser L is focused on the main surface of the target T by the above-mentioned KB mirror 14.
[0043] <PC> The personal computer PC includes a control unit 16 that controls the surface shaping device 10. As shown in Fig. 1, the control unit 16 controls each of the X-ray laser light source 11 and the four-quadrant slit 12. The control unit 16 also acquires the energy of the X-ray laser L detected by the gas energy monitor 13 and displays it on the display unit. Specific functional blocks included in the control unit 16 will be described below with reference to Fig. 3.
[0044] As shown in FIG. 3, the control unit 16 includes a wavelength selection unit 161, an irradiation density selection unit 162, a slit control unit 163, and a light source control unit 164.
[0045] (Wavelength selection section) The wavelength selection unit 161 selects the irradiation wavelength, which is the wavelength of the X-ray laser L, from the range of 1 nm to 200 nm in accordance with the wavelength corresponding to the inner shell absorption edge of the material (silicon in this embodiment) constituting the surface of the target T.
[0046] In this embodiment, the L-shell absorption edge of silicon is used as the inner-shell absorption edge used by the wavelength selection unit 161 to select the irradiation wavelength, and 10.3 nm is used as the irradiation wavelength.
[0047] (Irradiation density selection section) The irradiation density selection unit 162 selects the irradiation energy density, which is the energy density of the X-ray laser, in accordance with the mode of surface shaping to be performed on the surface of the target T. Specific examples of the mode of surface shaping will be described later.
[0048] When the irradiation density selection unit 162 selects the irradiation energy density, it refers to a predetermined processing threshold and selects the irradiation energy density to be above or below this processing threshold according to the mode of the surface shaping. This processing threshold can be determined experimentally by irradiating the surface of the target T with the X-ray laser L while changing the energy density of the X-ray laser L.
[0049] (Slit control unit) The slit control unit 163 adjusts the interval and position of the slits in the vertical direction and the interval and position of the slits in the horizontal direction by controlling the positions of the barriers 121, 122, 123, 124 provided in the four-quadrant slit 12. For example, the slit control unit 163 controls the state of the four-quadrant slit 12 as shown in FIGS. 2(a) and 2(b).
[0050] (Light source control unit) The light source control unit 164 controls the X-ray laser light source 11 so that the wavelength of the X-ray laser L becomes the irradiation wavelength.
[0051] <Interaction between X-ray laser and target> The surface shaping apparatus 10 configured as described above can irradiate the surface of the target T with the X-ray laser L in a focused state. FIG. 4 schematically shows the target T irradiated with the X-ray laser L on its surface.
[0052] When the target T is laser processed by irradiating the target T with the X-ray laser L, as shown in FIG. 4, the primary interaction region R 1 and the secondary interaction region R 2 are generated. The primary interaction region R 1 is a region corresponding to the irradiation spot where the X-ray laser L is irradiated on the surface of the target T, and is a region where the X-ray laser L directly interacts with the material constituting the target T. On the other hand, the secondary interaction region R 2 is not a region directly irradiated with the X-ray laser L, and the primary interaction region R 1This is an area that may be affected by heat generated in the
[0053] Conventionally, infrared lasers with wavelengths in the infrared range have been widely used as laser light for laser processing. When a continuous wave infrared laser or an infrared laser with a relatively long pulse width (for example, a pulse width on the order of nanoseconds) is used, the first interaction region R 1 The secondary interaction region R 2 However, in this case, structures that the user did not intend, such as deterioration, a bulge at the outer edge of the opening (hereinafter referred to as a rim portion), and cracks, occurred, resulting in a deterioration in processing accuracy.
[0054] On the other hand, it is known that the generation of the above-mentioned unintended structures is suppressed when an infrared laser having a pulse width on the order of femtoseconds is used. However, in order to perform finer surface modeling, it is necessary to shorten the irradiation wavelength of the X-ray laser L. One aspect of the present invention is based on such a technical idea.
[0055] (pore formation) For example, when the surface shaping is the formation of pores, the wavelength selection unit 161 selects a wavelength shorter than the wavelength corresponding to the core absorption edge as the irradiation wavelength, and the irradiation density selection unit 162 selects an energy density exceeding a predetermined processing threshold as the irradiation energy density. The irradiation mechanism 10A has the irradiation wavelength and the irradiation energy density, and has a pulse width of 1×10 -18 1×10 seconds or more -10 An X-ray laser L in the range of less than 1 / 2 second is irradiated onto the surface of a target T.
[0056] In this embodiment, as described above, the L-shell absorption edge of silicon is adopted as the inner shell absorption edge used by the wavelength selection unit 161 to select the irradiation wavelength, and 10.3 nm is adopted as the irradiation wavelength.
[0057] As a result, in the vicinity of the outer edge of the irradiation area on the surface of the target T irradiated with the X-ray laser L, a pore in which the generation of a rim portion is suppressed is formed, as shown in (a) and (b) of FIG.
[0058] The processing threshold for silicon is 106 mJ / cm when the irradiation wavelength is 10.3 nm. 2 and 418 mJ / cm when the irradiation wavelength is 13.5 nm. 2 This processing threshold can be experimentally determined and can also be determined for materials other than silicon. For example, for silicon nitride, the processing threshold is 200 mJ / cm when the irradiation wavelength is 10.3 nm. 2 When the irradiation wavelength is 13.5 nm, the processing threshold is 400 mJ / cm 2 In addition, in the case of lithium fluoride, when the irradiation wavelength is 10.3 nm and 13.5 nm, the processing threshold value is 10 mJ / cm2, although there is some fluctuation. 2 More than 20mJ / cm 2 Included within the following range:
[0059] In this embodiment, even when the surface modeling form is a holographic pattern or a lattice pattern, the L shell absorption edge of silicon is used as the inner shell absorption edge used by the wavelength selection unit 161 to select the irradiation wavelength, 10.3 nm is used as the irradiation wavelength, and 106 mJ / cm is used as the processing threshold. 2 Therefore, 90% of the processing threshold is 95.4 mJ / cm 2 It is.
[0060] (Holographic pattern formation) Furthermore, for example, when the mode of surface modeling is the formation of a holographic pattern, the slit control unit 163 controls the four-quadrant slit 12 to close the obstruction 123 of the four-quadrant slit 12 as shown in (b) of Fig. 2. As a result, the X-ray laser L passes through the four-quadrant slit 12, thereby obtaining a diffracted X-ray laser.
[0061] Then, the wavelength selection unit 161 selects a wavelength shorter than the wavelength corresponding to the core absorption edge as the irradiation wavelength, and the irradiation density selection unit 162 selects an energy density exceeding 90% of a predetermined processing threshold as the irradiation energy density. The irradiation mechanism 10A has the irradiation wavelength and the irradiation energy density, and has a pulse width of 1×10 -18 1×10 seconds or more -10 A diffracted X-ray laser in the sub-second range is irradiated onto the surface of the target T.
[0062] As a result, a holographic pattern as shown in FIG. 10 is formed in the area of the surface of the target T that is irradiated with the X-ray laser L.
[0063] (Formation of a grid pattern) For example, when the surface modeling mode is the formation of a lattice pattern, the wavelength selection unit 161 selects a wavelength shorter than the wavelength corresponding to the inner shell absorption edge as the irradiation wavelength, and the irradiation density selection unit 162 selects an energy density below a predetermined processing threshold as the irradiation energy density. The irradiation mechanism 10A has the irradiation wavelength and the irradiation energy density, and has a pulse width of 1×10 -18 1×10 seconds or more -10 The surface of the target T is irradiated with a multi-shot X-ray laser L within a range of 100 s or less. In this embodiment, the number of shots of the X-ray laser L irradiated to the surface is 100 shots.
[0064] As a result, a lattice pattern as shown in Fig. 11 is formed in the irradiation area of the surface of the target T irradiated with the X-ray laser L. The polarization direction of the X-ray laser L is set to be parallel to the up-down direction in Fig. 11. On the other hand, referring to Fig. 11, it can be seen that the rows and columns of the lattice pattern formed on the surface of the target T are tilted from the polarization direction of the X-ray laser L described above.
[0065] [Modifications] A surface shaping method M10 according to a modified example of the present invention will be described with reference to Fig. 5. Fig. 5 is a flowchart of the surface shaping method M10.
[0066] The surface shaping method M10 is a method that expresses the surface shaping apparatus 10 shown in Fig. 1. Therefore, the surface shaping method M10 corresponds to the surface shaping apparatus 10. Therefore, in this modification, the corresponding relationship between the surface shaping method M10 and the surface shaping apparatus 10 is mainly shown, and detailed explanations of each process are omitted. Note that, as in the case of the surface shaping apparatus 10, the material that constitutes the target T is preferably silicon or silicon nitride.
[0067] As shown in FIG. 5, the surface shaping method M10 includes a wavelength selection step S11, an irradiation density selection step S12, a slit control step S13, and an irradiation step S14.
[0068] <Wavelength selection process> The wavelength selection step S11 corresponds to the wavelength selection unit 161 of the control unit 16. That is, the wavelength selection step S11 selects an irradiation wavelength, which is the wavelength of an X-ray laser to be irradiated onto the surface of the target T, from a range of 1 nm to 200 nm inclusive, in accordance with a wavelength corresponding to an inner shell absorption edge of a material constituting the surface of the target T.
[0069] When the surface shaping is the formation of pores, a holographic pattern, or a lattice pattern, the wavelength selection step S11 selects an irradiation wavelength that is shorter than the wavelength corresponding to the core absorption edge.
[0070] <Irradiation density selection process> The irradiation density selection step S12 corresponds to the irradiation density selection unit 162 of the control unit 16. That is, the irradiation density selection step S12 selects the irradiation energy density, which is the energy density of the X-ray laser, depending on the aspect of the surface shaping to be performed on the surface of the target T.
[0071] When the surface shaping mode is the formation of fine holes, the irradiation density selection step S12 selects an energy density that exceeds a predetermined processing threshold as the irradiation energy density. When the surface shaping mode is the formation of a holographic pattern, the irradiation density selection step S12 selects an energy density that exceeds 90% of the predetermined processing threshold as the irradiation energy density. When the surface shaping mode is the formation of a lattice pattern, the irradiation density selection step S12 selects an energy density that is below the predetermined processing threshold as the irradiation energy density.
[0072] <Slit control process> The slit control process S13 corresponds to the slit control unit 163. That is, the slit control process S13 adjusts the intervals and positions of the slits in the up-down direction and the intervals and positions of the slits in the left-right direction by controlling the positions of the obstacles 121, 122, 123, and 124 of the four-quadrant slit 12 shown in Fig. 1.
[0073] When the mode of surface modeling is the formation of a holographic pattern, the slit control step S13 controls the four-quadrant slit 12 so as to close the obstruction 123 of the four-quadrant slit 12, as shown in (b) of Fig. 2. As a result, a diffracted X-ray laser is obtained by the X-ray laser L passing through the four-quadrant slit 12.
[0074] On the other hand, when the surface shaping mode is the formation of fine holes and a lattice pattern, the slit control step S13 controls the four-quadrant slit 12 so as to be fully opened, as shown in FIG. 2(a).
[0075] <Irradiation process> The irradiation step S14 corresponds to the irradiation mechanism 10A shown in FIG.
[0076] That is, when the surface modeling mode is a pore, the irradiation step S14 has an irradiation wavelength selected in the wavelength selection step S11 and an irradiation energy density selected in the irradiation density selection step S12, and a pulse width of 1×10 -18 1×10 seconds or more -10An X-ray laser L having a wavelength in the range of less than 1 / 2 s is irradiated onto the surface of a target T.
[0077] In addition, when the surface modeling is to form a holographic pattern, the irradiation step S14 has an irradiation wavelength selected in the wavelength selection step S11 and an irradiation energy density selected in the irradiation density selection step S12, and a pulse width of 1×10 -18 1×10 seconds or more -10 A diffracted X-ray laser in the sub-second range is irradiated onto the surface of the target T.
[0078] In addition, when the surface modeling mode is the formation of a lattice pattern, the irradiation step S14 has an irradiation wavelength selected in the wavelength selection step S11 and an irradiation energy density selected in the irradiation density selection step S12, and a pulse width of 1×10 -18 1×10 seconds or more -10 The surface is irradiated with multiple shots of an X-ray laser L within the range of 1 / 2 seconds or less.
[0079] [Target materials and their inner shell absorption edges]
[0080] The materials constituting the target T and the inner shell absorption edge of each material will be described with reference to Figures 6 and 7. This item is common to both the surface shaping apparatus 10 and the surface shaping method M10.
[0081] As described above in the description of the surface shaping apparatus 10, materials constituting the target T include, for example, silicon, silicon nitride, silicon carbide, sapphire, carbon, polymethylmetha crylate (PMMA), platinum, gold, aluminum, copper, iron, nickel, and zirconium.
[0082] Figures 6(a) to 6(f) are graphs showing the wavelength dependence of the absorption coefficient of silicon, silicon nitride, silicon carbide, sapphire, carbon, and PMMA, respectively. Figures 7(a) to 7(b) are graphs showing the wavelength dependence of the absorption coefficient of platinum, gold, aluminum, copper, iron, nickel, and zirconium, respectively. In Figures 6 and 7, the position of the wavelength corresponding to the core absorption edge of each material is indicated by an arrow.
[0083] As described above, in the surface shaping device 10 and the surface shaping method M10, a predetermined inner shell absorption edge among the K shell, L shell, M shell, N shell, and O shell of each material is adopted as the inner shell absorption edge used by the wavelength selection unit 161 and the wavelength selection process S11 to select the irradiation wavelength. In Figures 6 and 7, the inner shell absorption edge used by the wavelength selection unit 161 and the wavelength selection process S11 to select the irradiation wavelength is surrounded by a dashed line. That is, in one aspect of the present invention, (1) when the material is silicon, silicon nitride, or silicon carbide, the L-shell absorption edge of silicon is adopted as the inner shell absorption edge, (2) when the material is sapphire, the L-shell absorption edge of aluminum is adopted as the inner shell absorption edge, (3) when the material is carbon or PMMA, the K-shell absorption edge of carbon is adopted as the inner shell absorption edge, (4) when the material is platinum or gold, the N-shell absorption edge and the O-shell absorption edge of each material are adopted as the inner shell absorption edge, (5) when the material is aluminum or copper, the L-shell absorption edge of each material is adopted as the inner shell absorption edge, and (6) when the material is iron, nickel, or zirconium, the M-shell absorption edge of each material is adopted as the inner shell absorption edge. When the material is silicon carbide, the K-shell absorption edge of carbon can be adopted as the inner shell absorption edge instead of the L-shell absorption edge of silicon.
[0084] [First Example and Comparative Example] A first embodiment and a comparative example of the surface shaping apparatus 10 and the surface shaping method M10 will be described with reference to FIG. 8. FIG. 8(a) is a perspective view of a silicon target T obtained by the first embodiment. FIG. 8(b) is a cross-sectional view of the silicon target T shown in FIG. 8(a). FIG. 8(c) and FIG. 8(d) are perspective views of silicon targets obtained by the first and second comparative examples of the present invention, respectively. Note that in FIG. 8(b), the center of the target T shown in FIG. 8(a) is set as the origin. FIG. 9 is a graph showing the wavelength dependence of the processing threshold in thermal processing and non-thermal processing.
[0085] In the first embodiment, a single crystal of p-type silicon with a (100) orientation is used as the target T, 10.3 nm, which is a wavelength shorter than the wavelength corresponding to the L-shell absorption edge, is used as the irradiation wavelength, and 107 mJ / cm, which exceeds the predetermined processing threshold, is used as the irradiation energy density. 2 The pulse width of the X-ray laser L is 70×10. -15 In the first comparative example, the second comparative example, and the second to fifth examples described later, the pulse width of the X-ray laser L was commonly set to 70×10 -15 Seconds.
[0086] In the first comparative example, a single crystal of p-type silicon with a (100) orientation was used as the target T, 13.5 nm, which is longer than the wavelength corresponding to the L-shell absorption edge, was used as the irradiation wavelength, and 294 mJ / cm, which is below the predetermined processing threshold, was used as the irradiation energy density. 2 was adopted.
[0087] In the second comparative example, a single crystal of p-type silicon with a (100) orientation was used as the target T, 13.5 nm, which is longer than the wavelength corresponding to the L-shell absorption edge, was used as the irradiation wavelength, and 460 mJ / cm, which exceeds the predetermined processing threshold, was used as the irradiation energy density. 2 was adopted.
[0088] Referring to Figures 8(a) and (b), it was found that in the target T subjected to the first embodiment, a pore without a rim was formed near the outer edge of the irradiation area irradiated with the X-ray laser L.
[0089] Referring to (c) of Figure 8, it was found that although the target T subjected to the first comparative example had traces of the area irradiated with the X-ray laser L having been melted once, no pores were formed.
[0090] Referring to (d) of Figure 8, it was found that in the target T subjected to the second comparative example, a pore with a rim portion was formed near the outer edge of the irradiation area irradiated with the X-ray laser L.
[0091] In addition, the processed shapes of the target T obtained by each of the first embodiment and the second comparative example were compared with theoretical model calculations using a molecular dynamics calculation code incorporating the behavior of atoms and electrons due to X-ray absorption. Figure 9 illustrates the wavelength dependence of processing thresholds in thermal processing and non-thermal processing of silicon, and each of the first embodiment and the second comparative example.
[0092] 9, it was found that the laser processing performed on the target T by the first embodiment was included in the non-thermal processing region, and the laser processing performed on the target T by the second comparative example was included in the thermal processing region. This result is consistent with the fact that the target T subjected to the first embodiment had a pore without a rim portion, and the target T subjected to the second comparative example had a pore with a rim portion.
[0093] [Second to fourth embodiments] Second to fourth embodiments of the surface shaping apparatus 10 and the surface shaping method M10 will be described with reference to Fig. 10. Fig. 10(a) and (b) are a plan view and a perspective view of a silicon target obtained by the second embodiment. Fig. 10(c) and (d) are a plan view and a perspective view of a silicon target obtained by the third embodiment. Fig. 10(e) and (f) are a plan view and a perspective view of a silicon target obtained by the fourth embodiment.
[0094] In the second embodiment, a single crystal of p-type silicon with a (100) orientation is used as the target T, and the X-ray laser L is converted into a diffracted X-ray laser by closing the barrier 123 of the four-quadrant slit 12 as shown in FIG. 2(b). The irradiation wavelength is 10.3 nm, which is shorter than the wavelength corresponding to the L shell absorption edge, and the irradiation energy density is 98.5 mJ / cm, which is higher than 90% of the predetermined processing threshold. 2 The 90% of the predetermined processing threshold is 95.4 mJ / cm 2 It is.
[0095] In each of the third and fourth examples, the same conditions as in the second example were adopted, and the irradiation energy density was set to 183 mJ / cm, which is higher than 90% of the predetermined processing threshold. 2 and 218 mJ / cm 2 was adopted.
[0096] Referring to FIG. 10, it was found that a holographic pattern was formed on the target T on which each of the second to fourth embodiments was implemented.
[0097] Fifth Example A fifth embodiment of the surface shaping apparatus 10 and surface shaping method M10 will be described with reference to Fig. 11. Fig. 11 is a plan view of a silicon nitride target obtained by the fifth embodiment.
[0098] In the fifth embodiment, a polycrystalline silicon nitride film (thickness 50 nm) is used as the target T, 10.3 nm, which is shorter than the wavelength corresponding to the L shell absorption edge, is used as the irradiation wavelength, and 162 mJ / cm, which is below the predetermined processing threshold, is used as the irradiation energy density. 2 was adopted, and the number of shots of the X-ray laser L irradiated onto the surface of the target T was set to 100. The polarization direction of the X-ray laser L was set to be parallel to the up-down direction in FIG.
[0099] 11, it was found that a lattice pattern was formed on the target T to which the fifth embodiment was applied. Also, with reference to FIG. 11, it was found that the rows and columns of the lattice pattern formed on the surface of the target T were tilted from the polarization direction of the X-ray laser L described above.
[0100] [Additional Notes] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. [Explanation of symbols]
[0101] 10 Surface modeling device 10A irradiation mechanism 11 X-ray laser light source 12 4-quadrant slit (slit) 15 X-ray filter 16 Control section 161 Wavelength selection unit 162 Irradiation density selection unit 163 Slit control section 164 Light source control unit T Target PC M10 surface modeling method S11 Wavelength selection process S12 Irradiation density selection process S13 Slit control process S14 Irradiation process
Claims
1. a wavelength selection step of selecting an irradiation wavelength, which is the wavelength of an X-ray laser to be irradiated onto the surface of the target, from a range of 1 nm to 200 nm inclusive in accordance with a wavelength corresponding to an inner shell absorption edge of a material constituting the surface of the target; an irradiation density selection step of selecting an irradiation energy density, which is the energy density of the X-ray laser, according to a mode of surface shaping to be performed on the surface; The irradiation wavelength and the irradiation energy density are set as above, and the pulse width is 1×10 -18 sec or more 1 x 10 -10 and irradiating the surface with an X-ray laser in the range of 1000 to 2000 s. A surface shaping method comprising:
2. When the surface shaping is performed by forming pores, the wavelength selection step includes selecting a wavelength shorter than a wavelength corresponding to the core absorption edge as the irradiation wavelength; The irradiation density selection step selects an energy density exceeding a predetermined processing threshold as the irradiation energy density. The method of claim 1 .
3. When the surface shaping is performed by forming a holographic pattern, The method further includes a diffraction step of obtaining a diffracted X-ray laser from the X-ray laser by passing the X-ray laser through a slit; the wavelength selection step includes selecting a wavelength shorter than a wavelength corresponding to the core absorption edge as the irradiation wavelength; The irradiation density selection step includes selecting an energy density exceeding 90% of a predetermined processing threshold as the irradiation energy density; The irradiation step has the irradiation wavelength and the irradiation energy density, and has a pulse width of 1×10 -18 sec or more 1 x 10 -10 irradiating the surface with the diffracted x-ray laser in the range of 1000 to 15000 sec; The method of claim 1 .
4. When the surface shaping is a lattice pattern, the wavelength selection step includes selecting a wavelength shorter than a wavelength corresponding to the core absorption edge as the irradiation wavelength; The irradiation density selection step includes selecting an energy density below a predetermined processing threshold as the irradiation energy density, The irradiation step has the irradiation wavelength and the irradiation energy density, and has a pulse width of 1×10 -18 sec or more 1 x 10 -10 irradiating the surface with the X-ray laser for multiple shots in the range of 1000 to 2000 s; The method of claim 1 .
5. The material is silicon or silicon nitride. The surface shaping method according to any one of claims 1 to 4.
6. A surface shaping device that irradiates an X-ray laser onto a surface of a target, a wavelength selection unit that selects an irradiation wavelength, which is the wavelength of the X-ray laser, from a range of 1 nm to 200 nm inclusive in accordance with a wavelength corresponding to an inner shell absorption edge of a material that constitutes the surface; an irradiation density selection unit that selects an irradiation energy density, which is the energy density of the X-ray laser, in accordance with a mode of surface shaping to be performed on the surface; The irradiation wavelength and the irradiation energy density are set as above, and the pulse width is 1×10 -18 sec or more 1 x 10 -10 and an irradiation mechanism for irradiating the surface with an X-ray laser having a wavelength in the range of 100 nm to 150 nm. A surface shaping apparatus comprising:
7. When the surface shaping is performed by forming pores, The wavelength selection unit selects a wavelength shorter than a wavelength corresponding to the core absorption edge as the irradiation wavelength, The irradiation density selection unit selects an energy density exceeding a predetermined processing threshold as the irradiation energy density. The surface shaping apparatus of claim 6 .
8. When the surface shaping is performed by forming a holographic pattern, a slit through which the X-ray laser passes to obtain a diffracted X-ray laser; The wavelength selection unit selects a wavelength shorter than a wavelength corresponding to the core absorption edge as the irradiation wavelength, The irradiation density selection unit selects an energy density exceeding 90% of a predetermined processing threshold as the irradiation energy density, The irradiation mechanism has the irradiation wavelength and the irradiation energy density, and has a pulse width of 1×10 -18 sec or more 1 x 10 -10 irradiating the surface with the diffracted x-ray laser in the range of 1000 to 15000 sec; The surface shaping apparatus of claim 6 .
9. When the surface shaping is a lattice pattern, The wavelength selection unit selects a wavelength shorter than a wavelength corresponding to the core absorption edge as the irradiation wavelength, The irradiation density selection unit selects an energy density below a predetermined processing threshold as the irradiation energy density, The irradiation mechanism has the irradiation wavelength and the irradiation energy density, and has a pulse width of 1×10 -18 sec or more 1 x 10 -10 irradiating the surface with the X-ray laser for multiple shots in the range of 1000 to 2000 s; The surface shaping apparatus of claim 6 .
10. an X-ray laser source for generating the X-ray laser; a light source control unit for controlling the X-ray laser light source; an X-ray filter; the light source control unit controls the X-ray laser light source so that the wavelength of the X-ray laser becomes the irradiation wavelength; the X-ray filter reduces the intensity of the X-ray laser so that the energy density of the X-ray laser approaches the irradiation energy density; The surface shaping apparatus according to any one of claims 6 to 9.
11. the X-ray laser light source is a wavelength-variable laser light source that can change the wavelength of the X-ray laser at least in a range of 1 nm to 200 nm, The X-ray filter provides an energy density at an illumination spot on the surface of at least 10 mJ / cm 2 Change within the above range, The surface shaping apparatus of claim 10.
Citation Information
Patent Citations
Lighting system for EUV projection lithography
DE102014226917A1
Laser processing method and laser processing equipment
JP2016215269A