New polymer binder composition for negative electrodes of secondary batteries
The π-conjugated bisiminoacenaphthenequinone polymer binder with polyacrylic acid forms a self-healing matrix, addressing conductivity and volume change issues in silicon electrodes, enhancing the stability and capacity of lithium-ion batteries.
Patent Information
- Application Number
- JP2020083527
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-11
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-05-11
AI Technical Summary
Conventional binders for silicon-based negative electrodes in lithium-ion batteries face issues with conductivity, volume changes due to lithium ion intercalation and deintercalation, leading to electrode degradation and reduced capacity, as well as the need for conductive additives that decrease active material content.
A π-conjugated bisiminoacenaphthenequinone (BIAN) polymer binder, combined with polyacrylic acid or phytic acid, is used to form a self-healing matrix that enhances adhesion, conductivity, and stability, minimizing volume fluctuations and maintaining electrode integrity.
The new binder composition improves the cycle stability and discharge capacity of silicon-based electrodes, achieving high reversible capacity and maintaining coulombic efficiency even after numerous cycles.
Smart Images

Figure 0007590748000027 
Figure 0007590748000028 
Figure 0007590748000029
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel polymer binder composition for the negative electrode of a secondary battery. [Background technology]
[0002] Chemical batteries that generate electricity through chemical reactions between materials are broadly classified into disposable primary batteries, secondary batteries that can be repeatedly charged and discharged, and fuel cells. Of these, secondary batteries that can be repeatedly charged and discharged are used for a variety of purposes, including mobile devices and emergency storage batteries. Here, secondary batteries are sometimes called storage batteries or rechargeable batteries.
[0003] Traditionally, nickel-cadmium secondary batteries have been used for a long time, but small, lightweight, and high-power nickel-lithium secondary batteries (hereafter sometimes referred to as "lithium-ion batteries") have been developed and have become the mainstream power source for mobile phones, laptops, etc. Nickel-ion batteries generally use "lithium cobalt oxide" as the positive electrode material, graphite as the negative electrode material, and an organic electrolyte. Discharging and charging are achieved by the movement of lithium ions (positive ions) contained in the lithium nickel cobalt oxide. Lithium-ion batteries have many advantages, including high voltage and energy density, no memory effect, and the ability to be packaged compactly, and therefore are currently the mainstream type of secondary battery in general use.
[0004] Among the components that make up secondary batteries, the positive electrode, negative electrode, and electrolyte have always been in the spotlight, and active basic research has been conducted on them. On the other hand, polyvinylidene fluoride (hereinafter sometimes abbreviated as "PVDF") has long been widely used as a binder for lithium-ion secondary batteries (Figure 1), but although the number of papers on new binders has increased in recent years, it cannot be said that they have been sufficiently studied. In addition, a cross-linked polyacrylic acid binder for high-capacity silicon-based anodes for next-generation lithium-ion batteries is known (Organic Square 55, 2016).
[0005] In addition, graphite has been used for many years as the active material for the negative electrode of conventional commercial lithium-ion secondary batteries, but its discharge capacity is at most 300 mAhg. -1 On the other hand, the theoretical capacity of silicon is about 10 times that of graphite, which is currently the main negative electrode active material (4200 mAhg -1 ), and it is expected that graphite anodes will be replaced with silicon anodes. As such a technology, a technology using a binder such as polyacrylic acid has been proposed (see Non-Patent Document 1, hereinafter referred to as "Prior Art 1").
[0006] Furthermore, in lithium-ion batteries, it is known that binders play a role in "adhering electrode active materials". In the negative electrode, the binder binds the carbon material and other active materials to the copper foil and other metal foils that serve as the current collector. As such a binder, vinylidene fluoride resin has long been used. It is known that binders play an important role in forming a coating (Solid Electrolyte Interphase, hereinafter sometimes referred to as "SEI") on the negative electrode surface, and it has also been reported that conjugated polymers are used as binders for silicon negative electrodes (see Non-Patent Document 2, hereinafter referred to as "Prior Art 2"). [Prior art documents] [Non-patent literature]
[0007] [Non-Patent Document 1] Review article: DOI: 10.1039 / c7cs00858a [Non-Patent Document 2] S. G Pa111aik, R. Vedarajan, N. Matswni, J. Mater. Chem. A, 5, 17909-17919 (2017) Summary of the Invention [Problem to be solved by the invention]
[0008] Prior Art 1 provides a detailed introduction of the chemical structures of polymer binders that are candidates for improving the shortcomings of conventional binders (such as PVDF) caused by the volume change (300%) during lithiation and delithiation of silicon negative electrodes. However, it does not provide a solution to the following issues that have been problematic when using silicon as a negative electrode material:
[0009] The first problem is that pure silicon has low electrical conductivity and cannot be used as a battery material. For this reason, it has been proposed to use silicon monoxide or silicon dioxide, or to dope silicon to give it electrical conductivity, making it an impurity semiconductor (n or p type). To compensate for the low electrical conductivity of silicon, carbon-based materials are mainly used as conductive additives.
[0010] Since the battery volume is determined by the standard, an increase in the amount of conductive additive directly leads to a decrease in the amount of active material, which leads to a decrease in battery capacity. In order to avoid this problem, it is necessary to attach the conductive additive to all silicon particles and to construct a structure in which the distance between the conductive additives is minimized so that they come into contact with each other. At present, no system has been found that can industrially provide a stable, high-capacity charge / discharge cycle, and the industrial stage is still at the stage of adding 10-20wt% silicon to graphite to achieve 400-500mAhg-l.
[0011] Prior Art 2 is an excellent invention in that it provides a bisiminoacenaphthenequinone (BIAN)-fluorene polymer as a binder, which has significantly improved electrochemical performance in output, cycling behavior, and specific capacity compared to electrodes containing conventional PVDF binders. However, there is still room for improvement in order to solve the problems caused by the volume change of the silicon electrode as described above. The second problem is that the insertion and extraction of lithium ions causes the silicon particles to expand and contract, causing the volume of the electrode to change. Although the change in the volume of the electrode occurs even when a graphite-based negative electrode is used, the degree of change is greater when a silicon-based negative electrode is used, and repeated charging and discharging can cause problems such as the silicon particles being crushed, the conductive network of the negative electrode being cut off, or the negative electrode peeling off from the current collector.
[0012] To solve these problems, new binder materials are needed. In designing such materials, it is necessary to consider various properties such as good miscibility with the electrode active material, high film-forming ability on the current collector, ability to form a film with high adhesion, low interfacial resistance with the electrode active material, electrochemical stability, and ability to assist in the formation of a good solid electrolyte interface (SEI).
[0013] Therefore, there has been a strong social demand for realizing a system that can industrially provide a stable, high-capacity charge / discharge cycle, and for a new binder material having the above-mentioned properties required for this purpose. [Means for solving the problem]
[0014] Under the above circumstances, the inventors of the present invention have conducted intensive research and synthesized a π-conjugated polymer having a bisiminoacenaphthequinone (hereinafter sometimes abbreviated as "BIAN") structure as a new binder material, thereby completing the present invention. That is, one aspect of the present invention is a compound represented by the following formula (I): Polyacrylic acid or phytic acid and , containing either graphite or reduced graphene oxide, and silicon. A polymer binder composition for a negative electrode of a secondary battery.
[0015] [ka]
[0016] In the above formula (I), R1 and R2 each represent a hydrogen atom, a group having 1 to 10 carbon atoms, 8Saturated hydrocarbons Chains? and n is any substituent selected from the group consisting of 7 ~ 17 Represents an integer.
[0017] The compound represented by the formula (I) is preferably any compound selected from the group consisting of compounds represented by the following formula (II):
[0018] [ka]
[0019] In the above formula, R1 and R2 are each a hydrogen atom, a methyl group, an ethyl group, a propyl group, and Isopropyl Base n is any group selected from the group consisting of 7 ~ 17 Represents an integer.
[0020] The compound represented by the formula (I) or (II) may be represented by the following formula (III) to (VII) and the compound represented by the following formula (III) to (VII) In the compound represented by the formula: 7 ~ 17 Represents an integer.
[0021] [ka]
[0022] [ka]
[0023] [ka]
[0024] [ka]
[0025] [ka]
[0027] The polyacid is preferably polyacrylic acid or phytic acid, and the polyacrylic acid is preferably a compound having a number average molecular weight of 3,000 to 500,000. (VII) is preferably a polymer of a dihalide compound having a bisiminoacenaphthequinone skeleton and a diethynylfluorene derivative. The number average molecular weight of these compounds is preferably 3,500 to 4,500.
[0028] Another aspect of the present invention is a negative electrode for a secondary battery, which is produced by dispersing and mixing the above-mentioned polymer binder composition for a negative electrode of a secondary battery, a negative electrode active material, and a conductive material in a solvent to prepare a slurry, and then coating the slurry on a current collector and drying it.
[0029] Here, the negative electrode for secondary batteries is 45 % by weight of silicon, which is a negative electrode active material, and 10 to 20 Acetylene black, a conductive material, weight percent and 10 to 35 weight percent of graphite or reduced graphene oxide. It is preferable that the silicon anode comprises:
[0030] The silicon negative electrode preferably further contains the above-mentioned polymerized π-conjugated polymer and polyacrylic acid, and preferably contains graphite:silicon:acetylene black:the above-mentioned polymerized π-conjugated polymer:polyacrylic acid=28-32:23-27:18-22:18-22:1-9 (wt %).
[0031] Yet another aspect of the present invention is a self-repairing matrix formed in a negative electrode by preparing a slurry containing the above-mentioned polymer binder composition for a negative electrode of a secondary battery. Here, the self-repairing matrix is preferably a compound having hydrogen bonds represented by the following formula (IX). In this specification, "self-repairing" is defined as the ability to repair mechanically caused structural damage by re-forming a bond network with water.
[0032] [ka]
[0033] Yet another aspect of the present invention is a secondary battery comprising the above-mentioned negative electrode. Here, the secondary battery preferably comprises a polymer binder composition for a negative electrode of a secondary battery in the negative electrode. Effect of the Invention
[0034] According to the binder composition of the present invention, the π-conjugated polymer having a bisiminoacenaphthequinone (BIAN) structure contained in the binder composition exhibits particularly advantageous effects compared to conventional binders in terms of the interaction with graphite, solubility in NMP, interaction with the current collector, and the like, which are required of a binder.
[0035] The binder composition of the present invention also provides a self-repairing matrix for protecting the negative electrode, which allows the self-repair of the conductive network that is broken by the volumetric fluctuation of the silicon electrode. [Brief description of the drawings]
[0036] [Figure 1] FIG. 1 shows the three-dimensional structure of poly(BIAN)-poly(acrylic acid), a hydrogen-bonded polymer used as a binder (A), and the structures of the components of the polymer, poly(BIAN) (B) and polyacrylic acid (hereinafter sometimes abbreviated as "PAA") (C). [Diagram 2]Figure 2 is a schematic diagram showing four possibilities for the metal electrode: (I) surface plating with Li metal, (II) supersaturation with Li, (III) equilibrium alloy formation, and (IV) electrochemical lithiation of the Li-metal alloy. [Diagram 3] FIG. 3 is a graph (Nyquist plot) showing the CV and EIS profiles of performing cells having BP-copolymer (compound represented by formula (III) above) / PAA binder.
[0037] [Figure 4] FIG. 4 is a graph showing the CV profile of an anode half-cell containing BP-copolymer / PAA as the binder. [Diagram 5] Figure 5 is a graph showing the discharge capacity of a graphite-silicon composite with poly(BIAN)-PAA as a binder (cell 1): (A) normal discharge capacity and (B) calculated discharge capacity based on the silicon content in the active anode material. [Figure 6] 6 is a graph showing a comparison of the profiles for cell 1 using only PAA as the binder and using the BIAN-PAA binder. (A) is the normal discharge capacity, (B) is the calculated discharge capacity based on the silicon content in the active anode material.
[0038] [Figure 7] FIG. 7 is an electron microscope image (part 1) showing the surface of the negative electrode before cycling ((A1) to (A3)) and after 335 cycles ((B1) to (B3)). [Figure 8] FIG. 8 is an electron microscope image (part 2) showing the surface of the negative electrode before cycling ((A1) to (A3)) and after 335 cycles ((B1) to (B3)). [Figure 9]Figure 9 is a graph (part 1) showing the discharge capacity of a graphite-silicon composite with poly(BIAN)-PAA as a binder (cell 2): (A) normal discharge capacity, (B) calculated discharge capacity based on silicon content in the active anode material.
[0039] [Figure 10] Figure 10 shows the discharge capacity (part 2) of an electrode (cell 2) containing a graphite-silicon composite with poly(BIAN)-PAA as the binder. (A) is the normal discharge capacity, (B) is the calculated discharge capacity based on the silicon content in the active anode material. [Figure 11] FIG. 11 is an electron microscope image (part 1) showing the surface of the negative electrode at position 1 before cycling ((A1) to (A3)) and after 320 cycles ((B1) to (B3)). [Figure 12] FIG. 12 is an electron microscope image (part 2) showing the surface of the negative electrode at position 1 before cycling ((A1) to (A3)) and after 320 cycles ((B1) to (B3)).
[0040] [Figure 13] FIG. 13 shows FT-IR chromatograms (part 1) of the electrode materials after coating the BP-copolymer and GSiBP_PAA slurries on copper foil. [Figure 14] FIG. 14 shows the FT-IR chromatogram (part 2) of the electrode material after coating the BP-copolymer and GSiBP_PAA slurries on copper foil. [Figure 15] FIG. 15 shows the EIS profile and CV of the anode half-cell after fabrication. [Figure 16] FIG. 16 is the CV profile of the anode half-cell containing BP-copolymer / PAA as the binder.
[0041] [Figure 17]Figure 17 shows the discharge capacity of a rGO-silicon composite electrode containing poly(BIAN)-PAA as a binder: (A) normal discharge capacity and (B) calculated discharge capacity based on the silicon content in the active anode material. [Figure 18] Figure 18 shows the profiles of PAA-only and BIAN-PAA binders in a rGO-Si system: (A) normal discharge capacity and (B) calculated discharge capacity based on the silicon content in the active anode material.
[0042] [Figure 19] FIG. 19 shows the EIS and CV profiles of the anode half-cell after fabrication.
[0043] [Figure 20] FIG. 20 shows the CV profile of an anode half-cell containing BP-copolymer / PAA binder. [Figure 21] 21 is a graph showing the discharge capacity of a graphite-silicon electrode containing BIAN-PAA and phytic acid as binders: (A) normal discharge capacity and (B) calculated discharge capacity based on the silicon content in the active anode material. [Figure 22] 22 shows a graph comparing the profiles of PAA-only and BIAN-PAA binders for a phytic acid-based system: (A) normal discharge capacity and (B) calculated discharge capacity based on silicon content in the active anode material.
[0044] [Diagram 23] 23 shows a graph of the performance evaluation results of a high silicon content cell containing BIAN-PAA as a binder: (A) normal discharge capacity and (B) calculated discharge capacity based on the silicon content in the active anode material. [Figure 24]24 is a graph showing the performance evaluation of silicon-only cells (no graphite) containing BIAN-PAA as a binder: (A) normal discharge capacity and (B) calculated discharge capacity based on the silicon content in the active anode material. [Diagram 25] 25 shows a graph of the performance evaluation of low BIAN-PAA binder content (15 wt %) cells: (A) normal discharge capacity and (B) calculated discharge capacity based on silicon content in the active anode material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045] The present invention will now be described in further detail with reference to the drawings as necessary. The present invention relates to a compound represented by the following formula (I): Polyacrylic acid or phytic acid and , containing either graphite or reduced graphene oxide, and silicon. A polymer binder composition for a negative electrode of a secondary battery.
[0046] [ka]
[0047] In the above formula (I), R1 and R2 each represent a hydrogen atom, a group having 1 to 10 carbon atoms, 8 Saturated hydrocarbons Chains? and n is any substituent selected from the group consisting of 7 ~ 17 Represents an integer. The compound represented by formula (I) is preferably any compound selected from the group consisting of compounds represented by the following formula (II), because when a negative electrode is produced, the negative electrode has high performance and is prevented from decreasing in capacity due to a volume change.
[0048] [ka]
[0049] In the above formula, R1 and R2 are each a hydrogen atom, a methyl group, an ethyl group, a propyl group, and Isopropyl Base n is any group selected from the group consisting of 7 ~ 17 Represents an integer. The compound represented by the formula (I) or (II) may be a compound represented by the following formula (III) (VII) It is preferable that the compound is any compound selected from the group consisting of compounds represented by the following formula (III) (hereinafter, sometimes referred to as "polymerized π-conjugated polymer"), because when a negative electrode is produced, the compound has high performance and is capable of preventing a decrease in capacity due to a volume change of the negative electrode. (VII) In the compound represented by the formula: 7 ~ 17 Represents an integer.
[0050] [ka]
[0051] [ka]
[0052] [ka]
[0053] [ka]
[0054] [ka]
[0056] The polyacid is preferably polyacrylic acid or phytic acid because it can effectively form hydrogen bonds, and the polyacrylic acid preferably has a number average molecular weight of 3,000 to 500,000 because it provides sufficient mechanical properties.
[0057] The formula (I) (VII) The compound represented by any one of the formulas (I) to (C) is preferably a polymer of a dihalide compound having a bisiminoacenaphthequinone skeleton and a diethynylfluorene derivative. (VII) The number average molecular weight of the compound represented by any one of the following formulas is preferably 3,500 to 4,500.
[0058] The polymer binder composition for the negative electrode of the secondary battery of the present invention, the negative electrode active material, and the conductive material are dispersed and mixed in a solvent to prepare a slurry, which is then applied to a current collector and dried to prepare a negative electrode for the secondary battery. In order to adjust the viscosity of the slurry to a desired value, a thickener such as methyl cellulose, carboxymethyl cellulose (CMC), or the like may be appropriately added within a range that does not impair the properties of the binder of the present invention.
[0059] As the solvent, for example, organic solvents such as N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as "NMP"), N,N-dimethylformamide, dimethylacetamide, dimethylsulfoxide, hexamethylsulfoxide, hexamethylsulfolamide, and methyl ethyl ketone can be used alone or in combination. In addition, various dispersants, surfactants, stabilizers, etc. may be added as necessary.
[0060] The negative electrode active material is preferably a silicon-based compound, since the battery capacity per weight is significantly larger than that of graphite. In this specification, the term "silicon-based negative electrode active material" refers to silicon and silicon compounds that react with lithium ions during charging and discharging. Examples of such materials include metallurgical grade silicon (silicon produced by reducing silicon dioxide with carbon), industrial grade silicon (silicon in which the metallurgical grade silicon is subjected to acid treatment or unidirectional solidification or other treatment to reduce impurities), and high-purity crystalline silicon (silicon produced from silane obtained by reacting silicon, which is known to have various crystalline states such as single crystal, polycrystalline, and amorphous).
[0061] Here, the negative electrode for secondary batteries is 45 % by weight of silicon, which is a negative electrode active material, and 10 to 20 Acetylene black, a conductive material, weight percent and 10 to 35 weight percent of graphite or reduced graphene oxide. In particular, a silicon negative electrode containing the above is preferable since it can realize a high discharge capacity and improved electrical conductivity.
[0062] The silicon negative electrode preferably further contains the above-mentioned polymerized π-conjugated polymer and polyacrylic acid from the viewpoint of the conductivity of the negative electrode matrix and durability based on the self-repairing ability.The silicon negative electrode preferably contains graphite:silicon:acetylene black:the above-mentioned polymerized π-conjugated polymer:polyacrylic acid in a ratio of 28-32:23-27:18-22:18-22:1-9 (wt%), which further improves the conductivity of the negative electrode matrix and durability based on the self-repairing ability.
[0063] The negative electrode containing the binder of the present invention can be prepared as follows. For example, graphite or reduced type cations are mixed in a desired ratio in an N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as "NMP") solvent. OxidationThe composite material can be produced by dispersing a composition containing graphene (hereinafter sometimes abbreviated as "rGO"), silicon nanopowder, the above-mentioned BIAN-p-phenylene copolymer binder, PAA binder, and acetylene black into a slurry, which is then coated onto the desired metal foil.
[0064] The ratio of each compound contained in the composition may be, for example, about 25 to about 35 wt% graphite or rGO, about 10 to about 20 wt% silicon nanopowder, about 15 to about 25 wt% BIAN-p-phenylene copolymer binder, about 2 to 7 wt% PAA binder, and about 15 to about 25 wt% acetylene black. As the metal foil constituting the current collector, foils of aluminum, copper, zinc, nickel, titanium, stainless steel, etc. may be used.
[0065] Coating of the foil can be carried out by a gravure method, a reverse roll method, a direct roll method, a doctor blade method, a knife method, an extrusion method, or the like. It is preferable to adopt a doctor blade method, since it can coat a plate of uniform thickness. In order to completely remove the NMP solvent from the electrode of uniform thickness obtained by coating, the electrode is dried in a vacuum, for example, at about 80 to about 95°C for about 10 to 15 hours, and then roll pressed to a desired thickness, for example, about 60 to about 90 μm, for example, at about 70 to about 90°C. The electrode thus obtained is punched out into a disk of a desired size using a punch, and a separator is sandwiched between the electrode and a previously prepared positive electrode, and the electrode is stored in a case to prepare a coin-type battery for electrochemical testing.
[0066] In the present invention, the polymer binder composition for the negative electrode of the secondary battery is prepared, dispersed in the above-mentioned solvent to form a slurry, and the slurry is used to form a negative electrode, thereby forming a self-repairing matrix in the negative electrode. Here, as the solvent, for example, NMP can be preferably used because of its good solubility and high dispersibility of the components. As the foil to which the slurry is applied, the above-mentioned foil can be used, but it is preferable to use copper foil from the viewpoint of cost.
[0067] The matrix having self-repairing properties of the present invention is formed, for example, at the same time as forming the negative electrode containing the binder of the present invention prepared as described above. The self-repairing matrix is preferably a compound having hydrogen bonds represented by the following formula (IX), since this gives the negative electrode matrix electrical conductivity and durability based on the self-repairing ability. The formation of the self-repairing matrix prevents the negative electrode surface from becoming rough due to volume change of the negative electrode using silicon, and the number of cycles of a cell equipped with a negative electrode containing the binder of the present invention can be improved.
[0068] [ka]
[0069] Example 1: Preparation of a graphite-silicon composite anode half-cell The above half-cells using N-paraphenylene-PAA (20 wt%-5 wt%) polymer as the binder were fabricated as follows. (1) Preparation of slurry Ultrafine powder of graphite (manufactured by Merk) was used as the electrode active material. Battery-grade acetylene black (hereinafter sometimes abbreviated as "AB") with an average particle size of 40 nm was used as the conductive additive. A total weight of 100 g of the negative electrode composition was prepared. The ratio of each component contained in this composition was 30 wt% graphite, 25 wt% silicon nanopowder (particle size less than 100 nm), 20 wt% BIAN-p-phenylene copolymer binder, 5 wt% PAA binder, and 20 wt% acetylene black. 50 g of this composition was suspended in 100 mL of N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as "NMP") solvent to prepare a slurry. Slurries having the compositions shown in Table 1 below were also prepared in the same manner.
[0070] [Table 1] *1:Reduced type Oxidation Graphene *2: Acetylene black
[0071] (2) Preparation of negative electrode Next, the above slurry was applied to one side of an electrolytic copper foil having a width of 220 mm and a thickness of 20 μm using a doctor blade to a coating width of 200 mm and a coating thickness of 70 μm to prepare an electrode. The electrode was dried in vacuum at 90°C for 12 hours to completely remove the NMP solvent. The electrode was then roll-pressed at 80°C to a thickness of 70 μm, and punched into a small disk (diameter 15 mm) to obtain the negative electrode of the present invention. This negative electrode was immediately subjected to measurement after preparation.
[0072] (3) Preparation of positive electrode Metallic lithium was used as the positive electrode. It was then punched out into a disk of the same size as the negative electrode to prepare the positive electrode.
[0073] (4) Preparation of non-aqueous electrolyte In a glove box filled with argon gas, LiPF6 was dissolved in a mixed solution of ethylene carbonate:diethyl carbonate=1:1 (v / v) to a concentration of 1.0 M to prepare a non-aqueous electrolyte solution.
[0074] (5) Fabrication of lithium-ion secondary batteries (coin cells) A coin-type lithium ion secondary battery (non-aqueous electrolyte secondary battery) for performance evaluation was produced using the negative electrode, positive electrode, non-aqueous electrolyte solution, and a 30 μm-thick polypropylene microporous film separator prepared as described above.
[0075] (6) Calculation of charge in lithium-silicon alloy (6-1) Electrochemically Driven Amorphous Solids Li 21 The theoretical maximum capacity of Si5 alloy silicon is 4200 mAhg -1 It has been reported that the electrochemical solid-state amorphization of lithium-silicon alloys is possible at room temperature (P. Limthongkul et al. / Acta Materialia 51 (2003) 1103-1113 Huggins RA, Nix WD. Ionics 2000;6:57). It has also been confirmed that the electrochemical solid-state amorphization of lithium-silicon alloys is possible at room temperature (P. Limthongkul et al. reported in 2003). Therefore, the charge amount of an electrode having the composition (Li / Si molar ratio) shown in Table 2 below was measured.
[0076] [Table 2]
[0077] (6-2) Theoretical charging capacity expected when using the binder composition of the present invention The theoretical charge capacity of the graphite / silicon composite using the poly(BIAN)-PAA polymer binder of the present invention is 372 mAhg, which is the theoretical charge capacity of graphite (LiC6). -1Based on the above, Li 15 Si4 alloy: 3569 mAhg -1 Therefore, the theoretical charge capacity of the electrode is 1423 mAhg -1 , or (0.333 × 3569) + (0.666 × 372).
[0078] Example 2: Performance evaluation of performing cells (1) EIS profile using performing cells Using the coin-type secondary battery (working cell) produced in Example 1, cyclic voltammetry (CV) and electrochemical impedance spectroscopy (hereinafter sometimes abbreviated as "EIS") profiles were measured.
[0079] The EIS of the negative / negative symmetrical model cell was measured using a VSP potentiostat (Bio-Logic Science Instruments). The frequency range was 65 kHz to 10 mHz, the amplitude voltage was ±5 mV, and the ambient temperature was 25°C. The results are shown in Figure 3. As shown in FIG. 3, the measurement results showed a linear increase after drawing an arc on the Nyquist plot both after mounting and after CV.
[0080] (2) CV profile using performing cells Next, the electrochemical properties of the poly(BIAN)-PAA-based binder (the binder of the present invention) for silicon-graphite-based negative electrodes were evaluated by cyclic voltammetry testing. A VSP potentiostat (Bio-Logic Science Instruments) was used for the cyclic voltammetry testing. Figure 4 shows the cyclic voltammogram. Irreversible electrode decomposition was observed in cycle 1. In addition, peaks corresponding to delithiation from graphite and delithiation by Li+ dealloying from silicon were observed in cycles 2 to 4.
[0081] (3) Measurement of discharge capacity and coulombic efficiency using performing cells Next, the charge-discharge characteristics, including the Coulombic efficiency, were evaluated using an Electrofield ABE 1024. The results are shown in Figure 5(A). As a result, the graphite-silicon composite electrode containing the poly(BIAN)-PAA binder had a reversible capacity of 230 mAhg after 335 cycles. -1 The coulombic efficiency was almost constant at around 100%. This indicates that when the negative electrode of the present invention is used, the amount of discharged electricity that can be effectively extracted is large relative to the amount of electricity (Ah) required for charging. In addition, the reversible capacity after 335 cycles (Figure 5(B)) relative to the amount of silicon as the active material was 470 mAhg -1 It was.
[0082] (Example 3) Performance evaluation using cells - 1 (1) Measurement of discharge amount and coulomb efficiency The discharge capacity and coulombic efficiency of the cell containing the poly(BIAN)-PAA binder were measured with respect to the cell containing only PAA as a control. The measurement conditions were the same as in Example 2. The results are shown in Figure 6(A). The decrease in discharge capacity after 25 cycles was clearly different from that of the cell containing the poly(BIAN)-PAA binder. The same tendency was also observed in the discharge amount relative to the amount of silicon as an active material (Figure 6(B)).
[0083] (2) Changes in the electrode surface before and after cycling The changes in the electrode surface before and after cycling are shown in Figure 7. Electron microscope images showing the state of the electrode surface of the three cells before cycling are shown as (A1) to (A3). Electron microscope images showing the state after 335 cycles used for the evaluation in (1) above are shown as (B1) to (B3). The magnifications are 300x for (A3) and (B3), 600x for (A2) and (B2), and 2,000x for (A1) and (B1). The electrode surface after cycling (position 1) showed a significant change due to the change in the capacity of the control electrode compared to the negative electrodes (A1) and (B1) containing the binder of the present invention ((A2), (A3) and (B2), (B3) in Figure 7).
[0084] In addition, for other positions on the electrode surface, electron microscope images showing the states before and after cycling (before cycling and after 335 cycles) were obtained in the same manner as in Fig. 7 (see Figs. 8(A1) to (B3)). These electron microscope images also showed the same results as in Fig. 7.
[0085] (Example 4) Performance evaluation using cells - 2 (1) Measurement of discharge amount and coulomb efficiency A similar performance evaluation was carried out using another cell as in Example 3 above. The results are shown in Figure 9. For this cell, the reversible capacity after 325 cycles was 510 mAhg -1 (Figure 9(A)). In addition, the reversible capacity relative to the amount of silicon used as the active material was 1122 mAhg after 325 cycles. -1 (FIG. 9(B)). In addition, FIG. 10 shows the results of comparing the control (cell containing a binder containing only PAA) with the cell containing the poly(BIAN)-PAA binder. The same tendency as in Example 3 was observed.
[0086] (2) Changes in the electrode surface before and after cycling The changes in the electrode surface before and after cycling are shown in Figures 11 and 12. In both figures, (A1) to (A3) show electron microscope images of the electrode surface state before cycling for the three cells. (B1) to (B3) show electron microscope images of the state after 320 cycles used for the evaluation in (1) above. The magnification of each image is the same as in Figure 7. It was observed that the electrode surface after cycling at both (position 1) and (position 2) had changed significantly.
[0087] (3) FT-IR results of BP-copolymer and electrode material when the slurry was applied to copper foil Figures 13 and 14 show the FT-IR results of the BP-copolymer and electrode material when the slurry was coated on copper foil. Figure 13 shows the FT-IR result of polyBIAN, and Figure 14 shows the FT-IR result of PAA. CN stretching was observed in polyBIAN, whereas C=O stretching was observed in PAA.
[0088] (Example 5) Study of binder composition-1 Half-cells were fabricated with graphite-silicon composites (hereinafter sometimes referred to as “rGO-Si composites”) containing a negative electrode containing BIAN-paraphenylene-PAA (20 wt% - 5 wt%) polymer as a binder, and their performance was evaluated.
[0089] (1) EIS profile measurement The negative electrode was fabricated in the same manner as above, except that rGO was used instead of graphite. The EIS profiles after fabrication and after CV were measured under the same conditions as in Example 2 above, and the results are shown in Figure 15. There was a large difference between the profiles after fabrication and after CV, and an improvement in the interfacial resistance after cycling was observed.
[0090] The CV profile was also measured under the same conditions as in Example 2. The results (cyclic voltammograms) are shown in Figure 16. Irreversible decomposition of the electrode and partial decomposition of the electrode were observed in cycle 1. Moreover, almost the same voltammograms were obtained in cycles 2 to 4.
[0091] (2) Measurement of discharge capacity and coulombic efficiency The discharge capacity and coulombic efficiency of the rGO-Si composite containing poly(BIAN)-PAA as a binder were measured in the same manner as in Example 3. The results are shown in Figure 17. The discharge capacity of the rGO-Si composite electrode containing poly(BIAN)-PAA as a binder was 750 mAhg after 330 cycles. -1 (Figure 17(A)). The discharge capacity relative to the amount of silicon used as the active material was 1,500 mAhg after 330 cycles. -1 (Figure 17(B)).
[0092] The discharge capacity and coulombic efficiency of the cell using the binder containing only PAA in the rGO-Si system and the cell using the binder containing BIAN-PAA are shown in Figure 18. The cell using the binder containing BIAN-PAA showed a higher discharge capacity.
[0093] (Example 6) Study of binder composition-2 A half cell was fabricated in the same manner as above, except that a graphite-silicon composite containing BIAN-paraphenylene-PAA (20wt%-5wt%) polymer and phytic acid was used as the negative electrode, and its performance was measured.
[0094] (1) EIS profile and CV The EIS profile of the cell containing BP-copolymer / PAA binder is shown in Figure 19, which indicates an improvement in the interfacial resistance, and the CV results are shown in Figure 20.
[0095] (2) Measurement of discharge capacity and coulombic efficiency Under the same conditions as above, the discharge capacity of a graphite-silicon electrode containing BIAN-PAA and phytic acid as binders was measured. The discharge capacity after 400 cycles was 750 mAhg -1 In addition, the discharge capacity relative to the amount of silicon used as the active material was 1,600 mAhg after 400 cycles. -1 It exceeded that.
[0096] (3) Comparison of discharge capacity with PAA as a control As a control, a negative electrode using a binder containing only PAA was used. The negative electrode containing poly(BIAN) and phytic acid showed high discharge capacity (Figure 21(A)). The discharge capacity versus the amount of silicon as active material is shown in Figure 21(B). The profile was similar to that shown in Figure 21(A).
[0097] (4) Examination of silicon content in negative electrode - 1 The discharge capacity and coulombic efficiency of a negative electrode containing 45 wt% Si, 10 wt% graphite, 25 wt% binder, and 20 wt% acetylene black were measured in the same manner as above. The results are shown in Figures 22(A) and (B). The coulombic efficiency was maintained at around 100%, and the discharge capacity was 500 mAhg for up to 300 cycles. -1 The results were as above (FIG. 22(A)). The same was true for the discharge capacity versus the amount of silicon as the active material (FIG. 22(B)).
[0098] (5) Examination of silicon content in negative electrode - 2 The discharge capacity and coulombic efficiency of a negative electrode containing 55 wt% Si, 25 wt% binder, and 20 wt% acetylene black were measured in the same manner as above. The results are shown in Figures 23(A) and (B). The coulombic efficiency was maintained at around 100%, and the discharge capacity was 400 mAhg for up to 120 cycles. -1 The results were as above (FIG. 23(A)). The same was true for the discharge capacity versus the amount of silicon as the active material (FIG. 23(B)).
[0099] (6) Examination of silicon content in negative electrode - 3 The discharge capacity and coulombic efficiency of a negative electrode containing 40 wt% Si, 25 wt% graphite, 20 wt% acetylene black, and 15 wt% binder were measured in the same manner as above. The results are shown in Figures 24(A) and (B). The coulombic efficiency was maintained at around 100%, and the discharge capacity was 400 mAhg for up to 210 cycles. -1 The results were as above (FIG. 24(A)). The same was true for the discharge capacity versus the amount of silicon as the active material (FIG. 24(B)).
[0100] (6) Anode using binder containing only BP-copolymer The discharge capacity and coulombic efficiency of the negative electrode using a binder containing only BP-copolymer were measured in the same manner as above. The results are shown in Figures 25(A) and (B). The coulombic efficiency was maintained at around 100%, and the discharge capacity was 1,000 mAhg for up to 200 cycles. -1 The results were as above (Figure 25(A)). The same was true for the discharge capacity versus the amount of silicon as the active material (Figure 25(B)).
[0101] From the above, it has been demonstrated that by using the binder of the present invention, a negative electrode having a high discharge capacity and good coulombic efficiency can be produced. [Industrial Applicability]
[0102] The present invention is useful in the field of secondary batteries.
Claims
1. A polymer binder composition for a negative electrode of a secondary battery, comprising a compound represented by the following formula (I), either polyacrylic acid or phytic acid, either graphite or reduced graphene oxide, and silicon: [Formula 1] In the above formula (I), R 1 and R 2 represents a substituent selected from the group consisting of a hydrogen atom and a saturated hydrocarbon chain having 1 to 8 carbon atoms, and n represents an integer of 7 to 17.
2. 2. The polymer binder composition for a negative electrode of a secondary battery according to claim 1, wherein the compound represented by formula (I) is any compound selected from the group consisting of compounds represented by the following formula (II): [chemical 2] In the above formula, R 1 and R 2 represents any group selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a propyl group, and an isopropyl group, and n represents an integer of 7 to 17.
3. The polymer binder composition for a negative electrode of a secondary battery according to claim 1 or 2, characterized in that the compound represented by formula (I) or (II) is any compound selected from the group consisting of compounds represented by the following formulas (III) to (VII): [C3] [C4] [C5] [C6] [C7] In the compounds represented by the above formulas (III) to (VII), n represents an integer of 7 to 17.
4. 2. The polymer binder composition for a negative electrode of a secondary battery according to claim 1, wherein the polyacrylic acid has a number average molecular weight of 3,000 to 500,000.
5. The polymer binder composition for a negative electrode of a secondary battery according to claim 3, wherein the compound represented by any one of formulas (I) to (VII) has a number average molecular weight of 3,500 to 4,500.
6. A negative electrode for a secondary battery, the negative electrode comprising the polymer binder composition for a secondary battery according to any one of claims 1 to 5, a negative electrode active material, and a conductive material, which are dispersed and mixed in a solvent to prepare a slurry, and the slurry is applied onto a current collector and dried to produce a negative electrode for a secondary battery.
7. 7. The negative electrode for a secondary battery according to claim 6, wherein the negative electrode for a secondary battery is a silicon negative electrode containing 20 to 45% by weight of a negative electrode active material, 10 to 20% by weight of acetylene black as a conductive material, and 10 to 35% by weight of graphite or reduced graphene oxide, and further containing a binder material.
8. The negative electrode for secondary batteries according to claim 7, wherein the silicon negative electrode further comprises a polymerized π-conjugated polymer represented by any one of the above formulas (III) to (VII) and polyacrylic acid.
9. 9. The negative electrode for secondary batteries according to claim 8, wherein the silicon negative electrode comprises graphite or reduced graphene oxide:silicon:acetylene black:the polymerized π-conjugated polymer:polyacrylic acid=28-32:23-27:18-22:18-22:1-9 (wt %).
10. A self-repairing matrix formed in a negative electrode of a secondary battery by preparing a slurry containing the polymer binder composition for a negative electrode of the secondary battery according to any one of claims 1 to 5 and using the slurry.
11. The self-repairing matrix according to claim 10, characterized in that the self-repairing matrix is a compound having a hydrogen bond represented by the following formula (IX): [C8]
12. A secondary battery comprising the negative electrode according to any one of claims 6 to 9.
13. The secondary battery according to claim 12, wherein the secondary battery comprises a polymer binder composition for a negative electrode of a secondary battery in a negative electrode.
Citation Information
Patent Citations
Negative electrode binder for secondary battery, negative electrode for secondary battery, and secondary battery
JP2017045517A
Negative electrode composition, method for manufacturing a negative electrode, and lithium ion battery
JP2018538675A
Electrolyte, lithium ion secondary battery, and compound
JP2020021656A
Manufacturing method for negative electrode
JP2020027746A
Negative-electrode active material and lithium ion secondary battery using same
WO2017150311A1