Photosensitive resin composition

Incorporating onium gallate salts as photoacid generators in photosensitive resin compositions addresses the issues of insulation reliability and patterning properties, enhancing the performance of semiconductor devices by reducing wiring short-circuits.

JP7590807B2Active Publication Date: 2024-11-27SUMITOMO BAKELITE CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2018210849
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-11-08
Publication Date
2024-11-27
Estimated Expiration
2038-11-08

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions, particularly those using triarylsulfonium borate salts, suffer from issues of insulation reliability and patterning properties due to acid-generated corrosion of wiring, leading to increased risk of wiring short-circuits from metal migration.

Method used

Incorporation of an onium gallate salt with a triarylsulfonium cation and a gallate anion as a thermally dissociable photoacid generator to improve the insulation reliability and patterning properties of the resin composition.

Benefits of technology

The use of onium gallate salts enhances insulation reliability and patterning properties, reducing the risk of wiring short-circuits and improving the overall performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590807000028
    Figure 0007590807000028
  • Figure 0007590807000029
    Figure 0007590807000029
  • Figure 0007590807000030
    Figure 0007590807000030
Patent Text Reader

Abstract

To provide a photosensitive resin composition excellent in insulation reliability and patterning properties.SOLUTION: The photosensitive resin composition to be used for a bump protective film contains an epoxy resin, a phenoxy resin, and a photoacid generator. The photoacid generator contains an onium gallate salt having a triarylsulfonium cation and a gallate anion.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition. [Background technology]

[0002] Various developments have been made in the field of photosensitive resin compositions. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes the use of a triarylsulfonium borate salt as a photosensitive acid generator that generates an acid by baking after exposure in a photosensitive resin composition and promotes a curing reaction using the acid (Table 1 in Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-188987 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of investigations by the present inventors, it was found that the photosensitive resin composition described in Patent Document 1 above leaves room for improvement in terms of insulation reliability and patterning properties. [Means for solving the problem]

[0005] In recent years, there has been a trend towards using photoacid generators (PAGs) capable of generating strong acids with high catalytic activity in order to improve resolution. Triarylsulfonium borate salts are a typical example of strong acid PAGs. However, it has been found that when used over time, the acid generated during exposure can cause corrosion of wiring, increasing the risk of wiring shorts due to metal migration.

[0006] In light of these circumstances, the present inventors further investigated PAG and found that PAG has a thermal dissociation property (PAG characteristic) that it is weakly oxidized by heat, and found that the use of this thermally dissociable PAG can suppress wiring shorts. Based on this knowledge, the present inventors further studied and found that the use of an onium gallate salt having a triarylsulfonium cation and a gallate anion as the thermally dissociable PAG can improve the patterning property of the photosensitive resin composition while improving the insulation reliability of the resin film obtained by heat-treating the photosensitive resin composition, and thus completed the present invention.

[0007] According to the present invention, Epoxy resin, Phenoxy resin, A photosensitive resin composition for use in a bump protective film, comprising: There is provided a photosensitive resin composition, wherein the photoacid generator comprises an onium gallate salt having a triarylsulfonium cation and a gallate anion. Effect of the Invention

[0008] According to the present invention, there is provided a photosensitive resin composition having excellent insulation reliability and patterning ability. [Brief description of the drawings]

[0009] [Figure 1] 1 is a vertical cross-sectional view showing an example of the configuration of a semiconductor device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a partial enlarged view of the area enclosed by the dashed line in FIG. [Diagram 3] 2 is a process diagram showing a method for manufacturing the semiconductor device shown in FIG. [Figure 4] 2A to 2C are diagrams for explaining a method for manufacturing the semiconductor device shown in FIG. [Diagram 5] 2A to 2C are diagrams for explaining a method for manufacturing the semiconductor device shown in FIG. [Figure 6]2A to 2C are diagrams for explaining a method for manufacturing the semiconductor device shown in FIG. [Figure 7] 1 is a partial enlarged cross-sectional view showing a first modified example of the semiconductor device according to the embodiment. FIG. [Figure 8] FIG. 11 is a partially enlarged cross-sectional view showing a second modified example of the semiconductor device according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, the same components are given the same reference numerals and the description will be omitted as appropriate. In addition, the drawings are schematic diagrams and do not correspond to the actual dimensional ratio.

[0011] An overview of the photosensitive resin composition of the present embodiment is shown. The photosensitive resin composition of the present embodiment contains an epoxy resin, a phenoxy resin, and a photoacid generator. In the photosensitive resin composition, the photoacid generator contains an onium gallate salt having a triarylsulfonium cation and a gallate anion.

[0012] According to the findings of the present inventors, it has been found that by using an onium gallate salt having a triarylsulfonium cation and a gallate anion as a thermally dissociable PAG, it is possible to improve the patterning ability of a photosensitive resin composition while also improving the insulation reliability of a resin film obtained by heat-treating the photosensitive resin composition.

[0013] According to the photosensitive resin composition of the present embodiment, the insulation reliability and patterning property can be improved, so that a semiconductor device with excellent connection reliability and an electronic device using the same can be realized.

[0014] The resin film of the photosensitive resin composition of the present embodiment is used in electric and electronic devices (electronic devices), for example, as a permanent film, a protective film, an insulating film, a rewiring material, etc. This resin film includes a cured film that has been cured by heating.

[0015] Here, "electrical and electronic equipment" refers to semiconductor chips, semiconductor elements, printed wiring boards, electric circuits, display devices such as television sets and monitors, information and communication terminals, light-emitting diodes, physical batteries, chemical batteries, and other elements, devices, final products that apply electronic engineering technology, as well as other electrical equipment in general.

[0016] Among these, the photosensitive resin composition of the present embodiment can be suitably used, for example, as a photosensitive resin composition for bump protective films. Resin films provided around electrical connection elements such as bumps, lands, and wiring are collectively called "bump protective films." The photosensitive resin composition for bump protective films refers to a resin composition used to form bump protective films.

[0017] Specific examples of the bump protective film include a passivation film provided around an electrical connection element, an overcoat film, an interlayer insulating film, etc. The resin film is provided on the semiconductor chip, but may be provided in the vicinity of the semiconductor chip, or may be provided at a position away from the semiconductor chip, such as a rewiring layer or build-up wiring layer.

[0018] Next, the photosensitive resin composition of the present embodiment will be described in detail. (Epoxy resin) The photosensitive resin composition of the present embodiment contains an epoxy resin, which can improve the film properties and processability of the resin film of the photosensitive resin composition.

[0019] As the epoxy resin, for example, an epoxy resin having two or more epoxy groups in one molecule can be used. As the epoxy resin, a monomer, an oligomer, or a polymer in general can be used, and the molecular weight and molecular structure thereof are not particularly limited. Examples of the epoxy resin include phenol novolac type epoxy resin, cresol novolac type epoxy resin, cresol naphthol type epoxy resin, biphenyl type epoxy resin, biphenyl aralkyl type epoxy resin, phenoxy resin, naphthalene skeleton type epoxy resin, bisphenol A type epoxy resin, bisphenol A diglycidyl ether type epoxy resin, bisphenol F type epoxy resin, bisphenol F diglycidyl ether type epoxy resin, bisphenol S diglycidyl ether type epoxy resin, glycidyl ether type epoxy resin, cresol novolac type epoxy resin, aromatic polyfunctional epoxy resin, aliphatic epoxy resin, aliphatic polyfunctional epoxy resin, alicyclic epoxy resin, polyfunctional alicyclic epoxy resin, etc. The epoxy resin may be used alone or in combination.

[0020] The epoxy resin may include a solid epoxy resin having two or more epoxy groups in the molecule. As the solid epoxy resin, one having two or more epoxy groups and being solid at 25°C (room temperature) may be used. This can improve the mechanical properties of the resin film of the photosensitive resin composition.

[0021] The epoxy resin may also include a polyfunctional epoxy resin having three or more functional groups in the molecule (that is, a polyfunctional epoxy resin having three or more epoxy groups in one molecule).

[0022] The trifunctional or higher polyfunctional epoxy resin preferably contains one or more epoxy resins selected from the group consisting of phenol novolac epoxy resins, cresol novolac epoxy resins, triphenylmethane epoxy resins, dicyclopentadiene epoxy resins, bisphenol A epoxy resins, and tetramethylbisphenol F epoxy resins, and more preferably contains novolac epoxy resins, which can improve the heat resistance of the resin film while realizing an appropriate thermal expansion coefficient.

[0023] The epoxy resin may include a liquid epoxy resin having two or more epoxy groups in the molecule. The liquid epoxy resin functions as a film-forming agent and can improve the brittleness of the resin film of the photosensitive resin composition.

[0024] The liquid epoxy resin can be an epoxy compound that has two or more epoxy groups and is liquid at room temperature of 25° C. The viscosity of this liquid epoxy resin at 25° C. can be, for example, 1 mPa·s to 8000 mPa·s, preferably 5 mPa·s to 1500 mPa·s, and more preferably 10 mPa·s to 1400 mPa·s.

[0025] The liquid epoxy resin may include, for example, one or more selected from the group consisting of bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, alkyl diglycidyl ether, and alicyclic epoxy. These may be used alone or in combination of two or more. Among these, alkyl diglycidyl ether may be used from the viewpoint of reducing cracks after development.

[0026] The epoxy equivalent of the liquid epoxy resin is, for example, 100 g / eq or more and 200 g / eq or less, preferably 105 g / eq or more and 180 g / eq or less, and more preferably 110 g / eq or more and 170 g / eq or less, thereby improving the brittleness of the resin film.

[0027] The lower limit of the content of the liquid epoxy resin is, for example, 5% by mass or more, preferably 10% by mass or more, and more preferably 15% by mass or more, based on the total non-volatile components of the photosensitive resin composition. This can improve the brittleness of the finally obtained cured film. On the other hand, the upper limit of the content of the liquid epoxy resin is, for example, 40% by mass or less, preferably 35% by mass or less, and more preferably 30% by mass or less, based on the total non-volatile components of the photosensitive resin composition. This can balance the film properties of the cured film.

[0028] The lower limit of the content of the epoxy resin is, for example, 40% by mass or more, preferably 45% by mass or more, and more preferably 50% by mass or more, based on the total non-volatile components of the photosensitive resin composition. This can improve the heat resistance and mechanical strength of the finally obtained cured film. On the other hand, the upper limit of the content of the epoxy resin is, for example, 90% by mass or less, preferably 85% by mass or less, and more preferably 80% by mass or less, based on the total non-volatile components of the photosensitive resin composition. This can improve the patterning properties.

[0029] In this embodiment, the non-volatile components of the photosensitive resin composition refer to the remainder excluding volatile components such as water, solvent, etc. When a solvent is included, the content of the non-volatile components of the photosensitive resin composition relative to the total non-volatile components of the photosensitive resin composition refers to the content of the solvent relative to the total non-volatile components of the photosensitive resin composition excluding the solvent.

[0030] The photosensitive resin composition of the present embodiment may contain other thermosetting resins other than the epoxy resin. Examples of other thermosetting resins include resins having a triazine ring, such as urea resins and melamine resins; unsaturated polyester resins; maleimide resins such as bismaleimide compounds; polyurethane resins; diallyl phthalate resins; silicone-based resins; benzoxazine resins; polyimide resins; polyamide-imide resins; cyanate ester resins such as benzocyclobutene resins, novolac-type cyanate resins, bisphenol A-type cyanate resins, bisphenol E-type cyanate resins, and tetramethylbisphenol F-type cyanate resins. These may be used alone or in combination of two or more.

[0031] (Phenoxy resin) The photosensitive resin composition of the present embodiment contains a phenoxy resin, which can increase the flexibility of the resin film of the photosensitive resin composition.

[0032] The weight average molecular weight of the phenoxy resin is not particularly limited, but is preferably 10,000 to 100,000, and more preferably 20,000 to 80,000. By using such a phenoxy resin with a relatively high molecular weight, it is possible to impart good flexibility to the resin film and sufficient solubility in a solvent.

[0033] In the present embodiment, the weight average molecular weight is measured, for example, as a polystyrene equivalent value by gel permeation chromatography (GPC).

[0034] The phenoxy resin may have reactive groups such as epoxy groups at both ends of the molecular chain or inside the molecular chain. The reactive groups in the phenoxy resin are capable of crosslinking with the epoxy groups in the epoxy resin. By using such a phenoxy resin, the solvent resistance and heat resistance of the resin film can be improved.

[0035] The phenoxy resin is preferably a solid at 25° C. Specifically, a phenoxy resin having a non-volatile content of 90% by mass or more is preferably used. By using such a phenoxy resin, the mechanical properties of the cured product can be improved.

[0036] Examples of the phenoxy resin include bisphenol A type phenoxy resin, bisphenol F type phenoxy resin, copolymer phenoxy resin of bisphenol A type and bisphenol F type, biphenyl type phenoxy resin, bisphenol S type phenoxy resin, copolymer phenoxy resin of biphenyl type phenoxy resin and bisphenol S type phenoxy resin, etc., and one or a mixture of two or more of these is used. Among these, bisphenol A type phenoxy resin or copolymer phenoxy resin of bisphenol A type and bisphenol F type is preferably used.

[0037] The lower limit of the content of the phenoxy resin is, for example, 20 parts by mass or more, preferably 25 parts by mass or more, more preferably 30 parts by mass or more, based on the content of the epoxy resin. This can improve flexibility. On the other hand, the upper limit of the content of the phenoxy resin is, for example, 60 parts by mass or less, preferably 55 parts by mass or less, more preferably 50 parts by mass or less. This can improve the solubility of the phenoxy resin and realize a photosensitive resin composition with excellent coatability.

[0038] The photosensitive resin composition of the present embodiment may contain a thermoplastic resin other than the phenoxy resin. Examples of the thermoplastic resin include polyvinyl acetal resin, acrylic resin, polyamide resin (e.g., nylon, etc.), thermoplastic urethane resin, polyolefin resin (e.g., polyethylene, polypropylene, etc.), polycarbonate, polyester resin (e.g., polyethylene terephthalate, polybutylene terephthalate, etc.), polyacetal, polyphenylene sulfide, polyether ether ketone, liquid crystal polymer, fluororesin (e.g., polytetrafluoroethylene, polyvinylidene fluoride, etc.), modified polyphenylene ether, polysulfone, polyether sulfone, polyarylate, polyamide imide, polyether imide, thermoplastic polyimide, etc. These may be used alone or in combination of two or more.

[0039] (Photoacid generator) The photosensitive resin composition of the present embodiment contains a photoacid generator, which can improve processability during patterning, such as sensitivity and resolution. The photosensitive resin composition of the present embodiment is a chemically amplified photosensitive resin composition that utilizes an acid generated from a photoacid generator as a catalyst, and can be used as a negative photosensitive resin composition.

[0040] The photoacid generator contains an onium gallate salt having a triarylsulfonium cation and a gallate anion, which can improve the patterning properties as well as the insulation reliability.

[0041] The triarylsulfonium cation may include at least one compound represented by the following general formula (1).

[0042] [ka]

[0043] In the above general formula (1), R 1 ~R 4 each independently represents an alkyl group, a hydroxy group, an alkoxy group, an alkylcarbonyl group, an arylcarbonyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an arylthiocarbonyl group, an acyloxy group, an arylthio group, an alkylthio group, an aryl group, a heterocyclic hydrocarbon group, an aryloxy group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, a hydroxy(poly)alkyleneoxy group, a group that forms a condensed polycyclic hydrocarbon skeleton by condensing with the benzene ring to which it is bonded, a substituted or unsubstituted silyl group, an amino group, a cyano group, a nitro group, or a halogen atom; and a, b, c, and d are each R 1 ~R 4 a is an integer of 1 to 5, c and d are integers of 0 to 5, and b is an integer of 0 to 4. R 1 ~R 4 The substituents of the above general formula (1) include R 1 ~R 4 As the group, the same groups as those mentioned above can be used.

[0044] In the above general formula (1), R 1 ~R 4In the above formula, examples of the alkyl group include linear alkyl groups having 1 to 18 carbon atoms (methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-octyl, n-decyl, n-dodecyl, n-tetradecyl, n-hexadecyl, n-octadecyl, etc.), branched alkyl groups having 3 to 18 carbon atoms (isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl, isooctadecyl), and cycloalkyl groups having 3 to 18 carbon atoms (cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, 4-decylcyclohexyl, etc.).

[0045] In the above general formula (1), R 1 ~R 4 In the above formula, examples of the alkoxy group include linear alkoxy groups having 1 to 18 carbon atoms, and branched alkoxy groups having 3 to 18 carbon atoms (such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, sec-butoxy, tert-butoxy, hexyloxy, decyloxy, dodecyloxy, and octadecyloxy).

[0046] In general formula (1), R 1 ~R 4 In the above, examples of the aryl group include aryl groups having 6 to 10 carbon atoms (such as phenyl, tolyl, dimethylphenyl, and naphthyl).

[0047] In the general formula (1), the condensed polycyclic hydrocarbon skeleton may have two or more rings, six or less rings, preferably four or less rings, and more preferably three or less rings. The condensed polycyclic hydrocarbon skeleton may be a condensation of cyclic hydrocarbons having different numbers of rings, such as five-membered rings and six-membered rings. Examples of such condensed polycyclic hydrocarbon skeletons include a fluorene skeleton and a derivative of the fluorene skeleton. One or two of the above-mentioned substituents, such as an alkyl group, may be bonded to the 9-position of the phenanthrene skeleton.

[0048] The gallate anion may include a compound represented by the following general formula (5).

[0049] [ka]

[0050] In the above general formula (5), R 13 ~R 16 represents independently a phenyl group or a perfluoroalkyl group substituted with a group selected from the group consisting of a perfluoroalkyl group, a perfluoroalkoxy group, a nitro group, a cyano group, an acyl group, and a halogen atom, or an unsubstituted phenyl group or a perfluoroalkyl group.

[0051] In the above general formula (5), the carbon number of the perfluoroalkyl group is 1 to 8, preferably 1 to 4. Specific examples of the perfluoroalkyl group include linear perfluoroalkyl groups such as trifluoromethyl, pentafluoroethyl, heptafluoropropyl, nonafluorobutyl, perfluoropentyl, and perfluorooctyl; branched perfluoroalkyl groups such as heptafluoroisopropyl, nonafluoroisobutyl, nonafluoro-sec-butyl, and nonafluoro-tert-butyl; and perfluorocycloalkyl groups such as perfluorocyclopropyl, perfluorocyclobutyl, perfluorocyclopentyl, and perfluorocyclohexyl. In the above general formula (5), the number of carbon atoms in the perfluoroalkoxy group is 1 to 8, preferably 1 to 4. Specific examples of the perfluoroalkoxy group include linear perfluoroalkoxy groups such as trifluoromethoxy, pentafluoroethoxy, heptafluoropropoxy, nonafluorobutoxy, perfluoropentyloxy, and perfluorooctyloxy; and branched perfluoroalkoxy groups such as heptafluoroisopropoxy, nonafluoroisobutoxy, nonafluoro-sec-butoxy, and nonafluoro-tert-butoxy. In the above general formula (5), examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. In the above general formula (5), from the viewpoint of cationic polymerization performance, R 13 ~R 16is preferably a phenyl group substituted with at least one selected from the group consisting of a perfluoroalkyl group and a fluorine atom.

[0052] An example of the gallate anion is (C6F5)4Ga - , ((CF3)2C6H3)4Ga - , (CF3C6H4)4Ga - , (C6F5)2GaF2 - , C6F5GaF3 - , (C6H3F2)4Ga - This makes it possible to realize high thermal dissociation properties.

[0053] The onium gallate salt is converted to a gallate anion (Ga - As a specific example, the onium gallate salt can be thermally dissociated by subjecting the resin film of the photosensitive resin composition to a curing treatment by heating. The onium gallate salt according to this embodiment has a relatively high thermal dissociation property when a borate anion, a sulfonate anion, a phosphorus-based anion, or an antimony-based anion is used as the counter anion.

[0054] In a manufacturing process using the photosensitive resin composition of this embodiment, the process compatibility of the photosensitive resin composition can be improved by setting the temperature of the heat treatment (e.g., curing treatment) after exposure to a temperature equal to or higher than the temperature at which thermal dissociation occurs.

[0055] The content of the photoacid generator is, for example, 0.3% by mass to 5.0% by mass, preferably 0.5% by mass to 4.5% by mass, and more preferably 1.0% by mass to 4.0% by mass, based on the total solid content of the photosensitive resin composition. By making the content equal to or more than the lower limit, patterning properties can be improved. On the other hand, by making the content equal to or less than the upper limit, insulation reliability can be improved. In this specification, the symbol "to" indicates that the upper and lower limits are included, unless otherwise specified.

[0056] The content of the onium gallate salt in the entire photoacid generator may be, for example, 70% by mass to 100% by mass, preferably 80% by mass to 100% by mass, and more preferably 90% by mass to 99% by mass, which can improve connection reliability and patterning properties.

[0057] The photosensitive resin composition of the present embodiment may contain a photosensitizer other than the photoacid generator. Examples of the other photosensitizer include onium salt compounds. More specifically, cationic photopolymerization initiators such as diazonium salts, iodonium salts such as diaryliodonium salts, sulfonium salts such as triarylsulfonium salts, triarylpyrilium salts, benzylpyridinium thiocyanates, dialkylphenacylsulfonium salts, and dialkylhydroxyphenylphosphonium salts can be mentioned.

[0058] (Surfactant) The photosensitive resin composition of the present embodiment may contain a surfactant. By containing a surfactant, wettability during coating can be improved, and a uniform resin film and cured film can be obtained. Examples of the surfactant include fluorine-based surfactants, silicone-based surfactants, alkyl-based surfactants, and acrylic-based surfactants.

[0059] The surfactant preferably contains a surfactant containing at least one of a fluorine atom and a silicon atom. This contributes to obtaining a uniform resin film (improved coating properties), improving developability, and also improving adhesive strength. For example, such a surfactant is preferably a nonionic surfactant containing at least one of a fluorine atom and a silicon atom. Commercially available surfactants that can be used include, for example, F-251, F-253, F-281, F-430, F-477, F-551, F-552, F-553, F-554, F-555, F-556, F-557, F-558, F-559, F-560, F-561, F-562, F-563, F-565, F-56 fluorine-containing oligomer structure surfactants such as F-8, F-569, F-570, F-572, F-574, F-575, F-576, R-40, R-40-LM, R-41, R-94, etc.; fluorine-containing nonionic surfactants such as F-tergent 250 and F-tergent 251 manufactured by NEOS Corporation; and silicone surfactants such as the SILFOAM (registered trademark) series manufactured by Wacker Chemie (e.g., SD 100 TS, SD 670, SD 850, SD 860, SD 882).

[0060] The content of the surfactant can be, for example, 0.001 to 1 mass %, and preferably 0.005 to 0.5 mass %, based on the total amount of nonvolatile components of the photosensitive resin composition.

[0061] (Adhesion aid) The photosensitive resin composition of the present embodiment may contain an adhesion aid, which can further improve adhesion to inorganic materials.

[0062] The adhesion aid is not particularly limited, but may be, for example, a silane coupling agent such as aminosilane, epoxysilane, acrylicsilane, mercaptosilane, vinylsilane, ureidosilane, or sulfidosilane. The silane coupling agent may be used alone or in combination of two or more. Among these, it is more preferable to use epoxysilane (i.e., a compound containing both an epoxy moiety and a group that generates a silanol group by hydrolysis in one molecule).

[0063] Examples of amino group-containing coupling agents include bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldiethoxysilane, and N-phenyl-γ-aminopropyltrimethoxysilane. Examples of the epoxy group-containing coupling agent include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and γ-glycidylpropyltrimethoxysilane. Examples of the acrylic group-containing coupling agent or the methacrylic group-containing coupling agent include γ-(methacryloxypropyl)trimethoxysilane, γ-(methacryloxypropyl)methyldimethoxysilane, and γ-(methacryloxypropyl)methyldiethoxysilane. An example of a mercapto group-containing coupling agent is 3-mercaptopropyltrimethoxysilane. Examples of the vinyl group-containing coupling agent include vinyltris(β-methoxyethoxy)silane, vinyltriethoxysilane, and vinyltrimethoxysilane. An example of a ureido group-containing coupling agent is 3-ureidopropyltriethoxysilane. Examples of sulfide group-containing coupling agents include bis(3-(triethoxysilyl)propyl) disulfide, bis(3-(triethoxysilyl)propyl) tetrasulfide, and the like. Examples of the acid anhydride-containing coupling agent include 3-trimethoxysilylpropylsuccinic anhydride, 3-triethoxysilylpropylsuccinic anhydride, and 3-dimethylmethoxysilylpropylsuccinic anhydride.

[0064] Although silane coupling agents are listed here, titanium coupling agents, zirconium coupling agents, etc. may also be used.

[0065] The content of the adhesion aid is, for example, preferably 0.3 to 5 mass %, more preferably 0.4 to 4%, and can be 0.5 to 3 mass %, based on the total amount of non-volatile components of the photosensitive resin composition.

[0066] (Additives) In addition to the above components, the photosensitive resin composition of the present embodiment may contain other additives as necessary, such as antioxidants, fillers such as silica, sensitizers, and film-forming agents.

[0067] (solvent) The photosensitive resin composition of the present embodiment may contain a solvent. The solvent may contain an organic solvent. The organic solvent may be any solvent that can dissolve each component of the photosensitive resin composition and does not chemically react with each component.

[0068] Examples of organic solvents include acetone, methyl ethyl ketone, toluene, propylene glycol methyl ethyl ether, propylene glycol dimethyl ether, propylene glycol 1-monomethyl ether 2-acetate, diethylene glycol ethyl methyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, benzyl alcohol, propylene carbonate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol monomethyl ether acetate, dipropylene glycol methyl-n-propyl ether, butyl acetate, γ-butyrolactone, etc. These may be used alone or in combination.

[0069] The solvent is preferably used so that the total concentration of non-volatile components in the photosensitive resin composition is, for example, 30 to 75% by mass. By setting the concentration in this range, each component can be sufficiently dissolved, and good coating properties can be ensured. In addition, the viscosity of the photosensitive resin composition can be appropriately controlled by adjusting the content of the non-volatile components.

[0070] The viscosity of the varnish-like photosensitive resin composition at 25°C is, for example, 10 cP to 6000 cP, preferably 20 cP to 5000 cP, and more preferably 30 cP to 4000 cP. By setting the viscosity within the above numerical range, the thickness of the coating film can be appropriately controlled. For example, a thickness of 1 μm to 100 μm, preferably 3 μm to 80 μm, and more preferably 5 μm to 50 μm can be achieved.

[0071] Next, the semiconductor device and electronic device of this embodiment will be described.

[0072] Fig. 1 is a vertical cross-sectional view showing an example of a semiconductor device according to the present embodiment. Fig. 2 is a partial enlarged view of a region surrounded by a dashed line in Fig. 1. In the following description, the upper side in Fig. 1 will be referred to as "upper" and the lower side as "lower".

[0073] A semiconductor device 1 shown in FIG. 1 has a so-called package-on-package structure, which includes a through electrode substrate 2 and a semiconductor package 3 mounted thereon.

[0074] The through electrode substrate 2 comprises an insulating layer 21, a plurality of through wirings 221 penetrating from the upper surface to the lower surface of the insulating layer 21, a semiconductor chip 23 embedded inside the insulating layer 21, a lower wiring layer 24 provided on the lower surface of the insulating layer 21, an upper wiring layer 25 provided on the upper surface of the insulating layer 21, and solder bumps 26 provided on the lower surface of the lower wiring layer 24.

[0075] The semiconductor package 3 includes a package substrate 31, a semiconductor chip 32 mounted on the package substrate 31, bonding wires 33 electrically connecting the semiconductor chip 32 and the package substrate 31, a sealing layer 34 in which the semiconductor chip 32 and the bonding wires 33 are embedded, and solder bumps 35 provided on the underside of the package substrate 31.

[0076] Then, the semiconductor package 3 is laminated on the through electrode substrate 2. As a result, the solder bumps 35 of the semiconductor package 3 and the upper wiring layer 25 of the through electrode substrate 2 are electrically connected to each other.

[0077] In such a semiconductor device 1, it is possible to easily achieve a low height because there is no need to use a thick substrate such as an organic substrate including a core layer in the through electrode substrate 2. This can also contribute to miniaturization of electronic devices incorporating the semiconductor device 1.

[0078] In addition, since the through hole electrode substrate 2 and the semiconductor package 3 each having a different semiconductor chip are stacked, the packaging density per unit area can be increased. This makes it possible to achieve both miniaturization and high performance.

[0079] The through electrode substrate 2 and the semiconductor package 3 will be described in further detail below. 2 includes an insulating layer, a wiring layer, a through-hole wiring, etc. As a result, the lower wiring layer 24 and the upper wiring layer 25 include wiring inside and on the surface, and are electrically connected to each other via the through-hole wiring 221 that penetrates the insulating layer 21.

[0080] The wiring layer included in the lower wiring layer 24 is connected to the semiconductor chip 23 and the solder bumps 26. Therefore, the lower wiring layer 24 functions as a rewiring layer for the semiconductor chip 23, and the solder bumps 26 function as external terminals for the semiconductor chip 23.

[0081] 2 is provided to penetrate the insulating layer 21, as described above. This electrically connects the lower wiring layer 24 and the upper wiring layer 25, and enables stacking of the through electrode substrate 2 and the semiconductor package 3, thereby improving the functionality of the semiconductor device 1.

[0082] 2 is connected to the through-wires 221 and the solder bumps 35. Therefore, the upper wiring layer 25 is electrically connected to the semiconductor chip 23 and functions as a rewiring layer for the semiconductor chip 23 and also as an interposer interposed between the semiconductor chip 23 and the package substrate 31.

[0083] The through-hole wiring 221 penetrates the insulating layer 21, thereby providing an effect of reinforcing the insulating layer 21. Therefore, even if the mechanical strength of the lower wiring layer 24 or the upper wiring layer 25 is low, it is possible to avoid a decrease in the mechanical strength of the entire through-hole electrode substrate 2. As a result, the lower wiring layer 24 and the upper wiring layer 25 can be made even thinner, and the semiconductor device 1 can be made even thinner.

[0084] 1 also includes a through-wire 222 provided to penetrate the insulating layer 21 located on the upper surface of the semiconductor chip 23, in addition to the through-wire 221. This allows electrical connection between the upper surface of the semiconductor chip 23 and the upper wiring layer 25.

[0085] The insulating layer 21 is provided so as to cover the semiconductor chip 23. This enhances the effect of protecting the semiconductor chip 23. As a result, it is possible to improve the reliability of the semiconductor device 1. In addition, the semiconductor device 1 can be easily applied to a mounting method such as the package-on-package structure according to this embodiment.

[0086] The diameter W (see FIG. 2) of the through wire 221 is not particularly limited, but is preferably about 1 to 100 μm, and more preferably about 2 to 80 μm. This ensures the conductivity of the through wire 221 without impairing the mechanical properties of the insulating layer 21.

[0087] The semiconductor package 3 shown in Fig. 1 may be a package of any type, such as a Quad Flat Package (QFP), a Small Outline Package (SOP), a Ball Grid Array (BGA), a Chip Size Package (CSP), a Quad Flat Non-leaded Package (QFN), a Small Outline Non-leaded Package (SON), a Lead Flame BGA (LF-BGA), etc.

[0088] The arrangement of the semiconductor chips 32 is not particularly limited, but as an example, multiple semiconductor chips 32 are stacked in Fig. 1. This increases the packaging density. The multiple semiconductor chips 32 may be arranged side by side in the planar direction, or may be stacked in the thickness direction and arranged side by side in the planar direction.

[0089] The package substrate 31 may be any substrate, but is, for example, a substrate including an insulating layer, a wiring layer, and through-wires (not shown). Among these, the solder bumps 35 and the bonding wires 33 can be electrically connected via the through-wires.

[0090] The sealing layer 34 is made of, for example, a known sealing resin material. By providing such a sealing layer 34, the semiconductor chip 32 and the bonding wires 33 can be protected from external forces and the external environment.

[0091] In addition, since the semiconductor chip 23 of the through electrode substrate 2 and the semiconductor chip 32 of the semiconductor package 3 are arranged close to each other, it is possible to enjoy the advantages of high speed and low loss of mutual communication. From this viewpoint, for example, if one of the semiconductor chip 23 and the semiconductor chip 32 is a computing element such as a CPU (Central Processing Unit), a GPU (Graphics Processing Unit), or an AP (Application Processor), and the other is a storage element such as a DRAM (Dynamic Random Access Memory) or a flash memory, these elements can be arranged close to each other in the same device. This makes it possible to realize a semiconductor device 1 that is both highly functional and compact.

[0092] <Method of Manufacturing Semiconductor Device> Next, a method for manufacturing the semiconductor device 1 shown in FIG. 1 will be described.

[0093] Fig. 3 is a process diagram showing a method for manufacturing the semiconductor device 1 shown in Fig. 1. Also, Figs. 4 to 6 are diagrams for explaining the method for manufacturing the semiconductor device 1 shown in Fig. 1.

[0094] The manufacturing method of the semiconductor device 1 includes a chip placement process S1 of obtaining an insulating layer 21 so as to embed the semiconductor chip 23 and the through-wires 221, 222 provided on the substrate 202, an upper wiring layer formation process S2 of forming an upper wiring layer 25 on the insulating layer 21 and the semiconductor chip 23, a substrate peeling process S3 of peeling the substrate 202, a lower wiring layer formation process S4 of forming a lower wiring layer 24, a solder bump formation process S5 of forming solder bumps 26 to obtain the through electrode substrate 2, and a stacking process S6 of stacking a semiconductor package 3 on the through electrode substrate 2.

[0095] Among these, the upper wiring layer formation process S2 includes a first resin film arrangement process S20 of arranging a photosensitive resin varnish 5 (a varnish-like photosensitive resin composition) on the insulating layer 21 and the semiconductor chip 23 to obtain a photosensitive resin layer 2510, a first exposure process S21 of performing an exposure process on the photosensitive resin layer 2510, a first development process S22 of performing a development process on the photosensitive resin layer 2510, a first curing process S23 of performing a curing process on the photosensitive resin layer 2510, and a wiring layer formation process S24 of forming the wiring layer 253. The method includes step S24, a second resin film arrangement step S25 of arranging a photosensitive resin varnish 5 on the photosensitive resin layer 2510 and the wiring layer 253 to obtain a photosensitive resin layer 2520, a second exposure step S26 of subjecting the photosensitive resin layer 2520 to an exposure process, a second development step S27 of subjecting the photosensitive resin layer 2520 to a development process, a second curing step S28 of subjecting the photosensitive resin layer 2520 to a curing process, and a through wiring formation step S29 of forming a through wiring 254 in the opening 424 (through hole).

[0096] Each step will be described below in order. Note that the following manufacturing method is an example and is not intended to be limiting.

[0097] [1] Chip placement process S1 First, as shown in FIG. 4(a), a chip-embedded structure 27 is prepared, which includes a substrate 202, a semiconductor chip 23 and through-wires 221, 222 provided on the substrate 202, and an insulating layer 21 provided so as to embed these.

[0098] The constituent material of the substrate 202 is not particularly limited, but examples thereof include metal materials, glass materials, ceramic materials, semiconductor materials, organic materials, etc. Furthermore, the substrate 202 may be a semiconductor wafer such as a silicon wafer, a glass wafer, or the like.

[0099] The semiconductor chip 23 is bonded onto the substrate 202. In this manufacturing method, as an example, a plurality of semiconductor chips 23 are arranged side by side on the same substrate 202 while being spaced apart from each other. The plurality of semiconductor chips 23 may be of the same type or different types. In addition, the substrate 202 and the semiconductor chip 23 may be fixed to each other via an adhesive layer (not shown) such as a die attach film.

[0100] If necessary, an interposer (not shown) may be provided between the substrate 202 and the semiconductor chip 23. The interposer functions as, for example, a rewiring layer for the semiconductor chip 23. Therefore, the interposer may have pads (not shown) for electrically connecting to electrodes of the semiconductor chip 23, which will be described later. This allows the pad spacing and arrangement pattern of the semiconductor chip 23 to be changed, thereby further increasing the design freedom of the semiconductor device 1.

[0101] For such an interposer, for example, an inorganic substrate such as a silicon substrate, a ceramic substrate, or a glass substrate, or an organic substrate such as a resin substrate, or the like is used.

[0102] The insulating layer 21 may be, for example, a resin film (organic insulating layer) containing a thermosetting resin or a thermoplastic resin such as those listed as components of the photosensitive resin composition, or may be a conventional sealing material used in the semiconductor technology field.

[0103] Examples of materials for the through-wires 221 and 222 include copper or a copper alloy, aluminum or an aluminum alloy, gold or a gold alloy, silver or a silver alloy, nickel or a nickel alloy, and the like.

[0104] It should be noted that the chip-embedded structure 27 may be prepared by a method different from that described above.

[0105] [2] Upper wiring layer formation process S2 Next, an upper wiring layer 25 is formed on the insulating layer 21 and the semiconductor chip 23 .

[0106] [2-1] First resin film placement step S20 First, as shown in Fig. 4(b), a photosensitive resin varnish 5 is applied (placed) on the insulating layer 21 and the semiconductor chip 23. This results in a liquid coating of the photosensitive resin varnish 5 as shown in Fig. 4(c). The photosensitive resin varnish 5 is the photosensitive resin composition of this embodiment, and is a varnish having photosensitivity.

[0107] The photosensitive resin varnish 5 is applied by using, for example, a spin coater, a bar coater, a spray device, an inkjet device, or the like.

[0108] The viscosity of the photosensitive resin varnish 5 is not particularly limited, but is 10 cP to 6000 cP, preferably 20 cP to 5000 cP, and more preferably 30 cP to 4000 cP. When the viscosity of the photosensitive resin varnish 5 is within the above range, a thinner photosensitive resin layer 2510 (see FIG. 4(d)) can be formed. As a result, the upper wiring layer 25 can be made thinner, and the semiconductor device 1 can be easily made thinner.

[0109] The viscosity of the photosensitive resin varnish 5 is, for example, a value measured using a cone-plate type viscometer (TV-25, manufactured by Toki Sangyo Co., Ltd.) at a rotation speed of 100 rpm.

[0110] Next, the liquid coating of the photosensitive resin varnish 5 is dried, thereby obtaining the photosensitive resin layer 2510 shown in FIG.

[0111] The drying conditions for the photosensitive resin varnish 5 are not particularly limited, but may be, for example, heating at a temperature of 80 to 150° C. for 1 to 60 minutes.

[0112] In this step, a process of disposing a photosensitive resin film obtained by forming the photosensitive resin varnish 5 into a film may be adopted instead of the process of applying the photosensitive resin varnish 5. The photosensitive resin film is the photosensitive resin composition of this embodiment and is a resin film having photosensitivity.

[0113] The photosensitive resin film is produced, for example, by applying a photosensitive resin varnish 5 onto a base such as a carrier film by means of various coating devices, and then drying the resulting coating.

[0114] After the photosensitive resin layer 2510 is formed in this manner, a pre-exposure heat treatment is performed on the photosensitive resin layer 2510 as necessary. By performing the pre-exposure heat treatment, the molecules contained in the photosensitive resin layer 2510 are stabilized, and the reaction in the first exposure step S21 described below can be stabilized. On the other hand, by heating under the heating conditions described below, adverse effects of heating on the photoacid generator can be minimized.

[0115] The temperature of the pre-exposure bake treatment is preferably 70 to 130° C., more preferably 75 to 120° C., and even more preferably 80 to 110° C. If the temperature of the pre-exposure bake treatment is below the lower limit, the purpose of stabilizing the molecules by the pre-exposure bake treatment may not be achieved. On the other hand, if the temperature of the pre-exposure bake treatment is above the upper limit, the movement of the photoacid generator becomes too active, and the effect of making it difficult to generate acid even when irradiated with light in the first exposure step S21 described below may become widespread, resulting in a decrease in the processing accuracy of patterning.

[0116] The time of pre-exposure heat treatment is appropriately set according to the temperature of the pre-exposure heat treatment, and is preferably 1 to 10 minutes, more preferably 2 to 8 minutes, and even more preferably 3 to 6 minutes at the above temperature. If the time of pre-exposure heat treatment is below the lower limit, the heating time is insufficient, and the purpose of stabilizing the molecules by the pre-exposure heat treatment may not be achieved. On the other hand, if the time of pre-exposure heat treatment is above the upper limit, the heating time is too long, and even if the temperature of the pre-exposure heat treatment is within the above range, the action of the photoacid generator may be inhibited.

[0117] The atmosphere for the heat treatment is not particularly limited and may be an inert gas atmosphere or a reducing gas atmosphere, but is preferably air in consideration of work efficiency and the like.

[0118] The atmospheric pressure is not particularly limited and may be reduced or increased pressure, but is set to normal pressure in consideration of work efficiency, etc. Normal pressure refers to a pressure of about 30 to 150 kPa, and is preferably atmospheric pressure.

[0119] [2-2] First exposure process S21 Next, the photosensitive resin layer 2510 is subjected to an exposure process.

[0120] 4(d), a mask 412 is placed in a predetermined region on the photosensitive resin layer 2510. Then, light (active radiation) is irradiated through the mask 412. As a result, the photosensitive resin layer 2510 is subjected to an exposure process according to the pattern of the mask 412.

[0121] 4(d) illustrates a case where the photosensitive resin layer 2510 has so-called negative photosensitivity. In this example, the photosensitive resin layer 2510 is provided with solubility in a developer in the region corresponding to the light-shielding portion of the mask 412.

[0122] On the other hand, for example, acid is generated by the action of the photosensitizer in the regions corresponding to the transmitting portions of the mask 412. The generated acid acts as a catalyst for the reaction of the thermosetting resin in a process to be described later.

[0123] The exposure dose in the exposure treatment is not particularly limited, but is preferably 100 to 2000 mJ / cm. 2 is preferably 200 to 1000 mJ / cm 2 This makes it possible to suppress underexposure and overexposure in the photosensitive resin layer 2510. As a result, high patterning accuracy can be finally achieved. Thereafter, if necessary, the photosensitive resin layer 2510 is subjected to post-exposure heat treatment.

[0124] The temperature of the post-exposure heat treatment is not particularly limited, but is preferably 50 to 150° C., more preferably 50 to 130° C., even more preferably 55 to 120° C., and particularly preferably 60 to 110° C. By carrying out the post-exposure heat treatment at such a temperature, the catalytic action of the generated acid is sufficiently enhanced, and the thermosetting resin can be reacted sufficiently in a shorter time. By setting the temperature within the above range, it is possible to suppress a decrease in the processing accuracy of patterning due to the promotion of acid diffusion.

[0125] By setting the temperature of the post-exposure bake treatment to the lower limit or more, the reaction rate of the thermosetting resin can be increased, and the productivity can be improved. On the other hand, by setting the temperature of the post-exposure bake treatment to the upper limit or less, the deterioration of the processing accuracy of the patterning due to the promotion of acid diffusion can be suppressed.

[0126] On the other hand, the time of the post-exposure bake treatment is appropriately set according to the temperature of the post-exposure bake treatment, and is preferably 1 to 30 minutes, more preferably 2 to 20 minutes, and further preferably 3 to 15 minutes at the above temperature. By carrying out the post-exposure bake treatment for such a time, the thermosetting resin can be sufficiently reacted, and the diffusion of the acid can be suppressed, thereby preventing a decrease in the processing accuracy of the patterning.

[0127] The atmosphere for the post-exposure heat treatment is not particularly limited, and may be an inert gas atmosphere or a reducing gas atmosphere, but is preferably air in consideration of work efficiency and the like.

[0128] The atmospheric pressure for the post-exposure heat treatment is not particularly limited and may be reduced pressure or increased pressure, but is set to normal pressure in consideration of work efficiency, etc. This allows the pre-exposure heat treatment to be performed relatively easily. Note that normal pressure refers to a pressure of about 30 to 150 kPa, and is preferably atmospheric pressure.

[0129] [2-3] First development step S22 Next, a development process is performed on the photosensitive resin layer 2510. As a result, openings 423 penetrating the photosensitive resin layer 2510 are formed in the regions corresponding to the light-shielding portions of the mask 412 (see FIG. 5(e)). Examples of the developer include an organic developer and a water-soluble developer.

[0130] [2-4] First curing step S23 After the development process, the photosensitive resin layer 2510 is subjected to a curing process (post-development heat treatment). The conditions for the curing process are not particularly limited, but are set at a heating temperature of about 160 to 250° C. for a heating time of about 30 to 240 minutes. This makes it possible to cure the photosensitive resin layer 2510 while suppressing the thermal effect on the semiconductor chip 23, and obtain the organic insulating layer 251.

[0131] [2-5] Wiring layer formation step S24 Next, the wiring layer 253 is formed on the organic insulating layer 251 (see FIG. 5(f)). The wiring layer 253 is formed by obtaining a metal layer using a vapor phase deposition method such as a sputtering method or a vacuum deposition method, and then patterning the metal layer using a photolithography method and an etching method.

[0132] Prior to forming the wiring layer 253, a surface modification treatment such as a plasma treatment may be performed.

[0133] [2-6] Second resin film placement step S25 5(g), a photosensitive resin layer 2520 is obtained in the same manner as in the first resin film disposing step S20. The photosensitive resin layer 2520 is disposed so as to cover the wiring layer 253.

[0134] Thereafter, if necessary, a pre-exposure heat treatment is performed on the photosensitive resin layer 2520. The treatment conditions are, for example, the conditions described in the first resin film disposing step S20.

[0135] [2-7] Second exposure process S26 Next, an exposure process is performed on the photosensitive resin layer 2520. The process conditions are, for example, the conditions described in the first exposure step S21.

[0136] Thereafter, if necessary, a post-exposure heat treatment is performed on the photosensitive resin layer 2520. The treatment conditions are, for example, the conditions described in the first exposure step S21.

[0137] [2-8]Second development step S27 Next, a development process is performed on the photosensitive resin layer 2520. The process conditions are, for example, the conditions described in the first development step S22. As a result, an opening 424 penetrating the photosensitive resin layers 2510 and 2520 is formed (see FIG. 5(h)).

[0138] [2-9]Second curing step S28 After the development process, the photosensitive resin layer 2520 is subjected to a curing process (post-development heat treatment). The curing conditions are, for example, the conditions described in the first curing step S23. This causes the photosensitive resin layer 2520 to cure, and the organic insulating layer 252 is obtained (see FIG. 6(i)).

[0139] In this embodiment, the upper wiring layer 25 has two layers, the organic insulating layer 251 and the organic insulating layer 252, but may have three or more layers. In this case, after the second curing step S28, a series of steps from the wiring layer forming step S24 to the second curing step S28 may be repeatedly added.

[0140] [2-10]Through wiring formation process S29 Next, the through wiring 254 shown in FIG.

[0141] The through wiring 254 can be formed by a known method, for example, the following method.

[0142] First, a seed layer (not shown) is formed on the organic insulating layer 252. The seed layer is formed on the inner surfaces (side surfaces and bottom surfaces) of the opening 424 and on the upper surface of the organic insulating layer 252.

[0143] The seed layer may be, for example, a copper seed layer, and may be formed by, for example, a sputtering method.

[0144] Furthermore, the seed layer may be made of the same metal as the through-wiring 254 to be formed, or may be made of a different metal.

[0145] Next, a resist layer (not shown) is formed on the seed layer (not shown) in a region other than the opening 424. Then, using this resist layer as a mask, the opening 424 is filled with a metal. For example, electrolytic plating is used for this filling. Examples of the metal to be filled include copper or a copper alloy, aluminum or an aluminum alloy, gold or a gold alloy, silver or a silver alloy, nickel or a nickel alloy, etc. In this way, the conductive material is embedded in the opening 424, and the through wiring 254 is formed.

[0146] Next, the resist layer (not shown) is removed, and further, the seed layer (not shown) on the organic insulating layer 252 is removed. For this purpose, for example, a flash etching method can be used. The location where the through wiring 254 is formed is not limited to the location shown in the figure.

[0147] [3] Substrate peeling process S3 6(j), the substrate 202 is peeled off, thereby exposing the lower surface of the insulating layer 21.

[0148] [4] Lower wiring layer formation step S4 6(k), a lower wiring layer 24 is formed on the lower surface side of the insulating layer 21. The lower wiring layer 24 may be formed by any method, and may be formed, for example, in the same manner as the above-mentioned upper wiring layer forming step S2.

[0149] The lower wiring layer 24 thus formed is electrically connected to the upper wiring layer 25 via the through-wires 221 .

[0150] [5] Solder bump formation process S5 6(L), solder bumps 26 are formed on the lower wiring layer 24. In addition, a protective film such as a solder resist layer may be formed on the upper wiring layer 25 and the lower wiring layer 24, if necessary. In this manner, the through electrode substrate 2 is obtained.

[0151] The through electrode substrate 2 shown in Fig. 6(L) can be divided into a plurality of regions. Therefore, for example, by dividing the through electrode substrate 2 along the dashed line shown in Fig. 6(L), a plurality of through electrode substrates 2 can be efficiently manufactured. For example, a diamond cutter or the like can be used for dividing the substrate.

[0152] [6]Lamination process S6 Next, a semiconductor package 3 is placed on each individual through hole electrode substrate 2. In this way, the semiconductor device 1 shown in FIG.

[0153] Such a manufacturing method for the semiconductor device 1 can be applied to a wafer level process or a panel level process using a large-area substrate, thereby improving the manufacturing efficiency of the semiconductor device 1 and reducing costs.

[0154] <Modifications of the semiconductor device> Next, a modification of the semiconductor device according to the embodiment will be described.

[0155] (First Modification) First, the first modified example will be described. FIG. 7 is a partial enlarged cross-sectional view showing a first modified example of the semiconductor device according to the embodiment. The first modified example will be described below, focusing on the differences from the embodiment shown in Figures 1 and 2, and omitting a description of similar points. Note that the same reference numerals are used in Figure 7 to designate the same components as those in Figures 1 and 2.

[0156] 7 is similar to the semiconductor device 1 shown in FIGS. 1 and 2, except for the structure of the lower wiring layer. That is, the semiconductor device 1A shown in FIG. 7 includes a semiconductor chip 23 provided with lands 231, a lower wiring layer 24A, and solder bumps 26. The structure of the lower wiring layer 24A is different from the structure of the lower wiring layer 24 shown in FIGS.

[0157] 7 includes an organic insulating layer 240 provided on the lower surface of the semiconductor chip 23, and an organic insulating layer 241 provided below the organic insulating layer 240. At least one of the organic insulating layers 240 and 241 is formed using a photosensitive resin composition for bump protective films. The lower surface of the semiconductor chip 23 is covered with the organic insulating layers 240 and 241.

[0158] Moreover, the lower wiring layer 24A shown in FIG. 7 includes a bump adhesion layer 245 that is electrically connected to both the lands 231 and the solder bumps 26.

[0159] In manufacturing such a first modified example, by using a photosensitive resin composition for a bump protective film, it is possible to achieve high patterning accuracy and suppress deterioration of the metals contained in the lands 231 and the bump adhesion layer 245. As a result, a highly reliable semiconductor device 1A can be obtained.

[0160] (Second Modification) Next, a second modified example will be described. FIG. 8 is a partial enlarged cross-sectional view showing a second modified example of the semiconductor device according to the embodiment. The second modified example will be described below, focusing on the differences from the embodiment shown in Figures 1 and 2, and omitting a description of similar points. Note that the same reference numerals are used in Figure 8 to designate the same components as those in Figures 1 and 2.

[0161] The semiconductor device 1B shown in Fig. 8 is similar to the semiconductor device 1 shown in Fig. 1 and 2, except for the structure of the lower wiring layer. That is, the semiconductor device 1B shown in Fig. 8 includes a semiconductor chip 23 provided with lands 231, a lower wiring layer 24B, and solder bumps 26. The structure of the lower wiring layer 24B is different from the structure of the lower wiring layer 24 shown in Figs. 1 and 2.

[0162] 8 includes an organic insulating layer 240 provided on the lower surface of the semiconductor chip 23, an organic insulating layer 241 provided below the organic insulating layer 240, and an organic insulating layer 242 provided below the organic insulating layer 241. At least one of these organic insulating layers 240, 241, and 242 is formed using a photosensitive resin composition for bump protective films.

[0163] 8 includes a wiring layer 243 electrically connected to the land 231, and a bump adhesion layer 245 electrically connected to both the wiring layer 243 and the solder bump 26. Organic insulating layers 240 and 241 are interposed between the semiconductor chip 23 and the wiring layer 243, and the lower surface of the wiring layer 243 is covered with an organic insulating layer 242.

[0164] In manufacturing such a second modified example, by using a photosensitive resin composition for a bump protective film, it is possible to achieve high patterning accuracy and suppress deterioration of the metals contained in the lands 231, the wiring layer 243, and the bump adhesion layer 245. As a result, a highly reliable semiconductor device 1B can be obtained.

[0165] <Electronic equipment> The electronic device according to this embodiment includes the semiconductor device according to this embodiment described above.

[0166] The electronic device according to this embodiment is not particularly limited as long as it is equipped with such a semiconductor device, but examples of the electronic device include information devices such as mobile phones, smartphones, tablet terminals, wearable terminals, personal computers, communication devices such as servers and routers, industrial equipment such as robots and machine tools, and in-vehicle equipment such as vehicle control computers and car navigation systems.

[0167] While the present invention has been described above based on the illustrated embodiments, the present invention is not limited to these.

[0168] For example, the method for manufacturing a semiconductor device of the present invention may include any step added for any purpose to the above-described embodiment.

[0169] Moreover, the photosensitive resin composition, the semiconductor device, and the electronic device of the present invention may be those in which any element is added to the above-mentioned embodiment.

[0170] In addition to semiconductor devices, the photosensitive resin composition can also be used as a bump protective film for MEMS (Micro Electro Mechanical Systems) and various sensors, and as a bump protective film for display devices such as liquid crystal display devices and organic EL devices.

[0171] Furthermore, the form of the package of the semiconductor device is not limited to the form shown in the drawings, and any form may be used. EXAMPLES

[0172] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0173] (Preparation of Photosensitive Resin Composition) The raw materials of each component blended according to Table 1 were dissolved in propylene glycol monomethyl ether acetate (PGMEA) to obtain a mixed solution. The mixed solution was then filtered through a 0.2 μm polypropylene filter to obtain a varnish-like photosensitive resin composition having a viscosity of about 100 cP at 25° C. The viscosity of the photosensitive resin composition was measured using a cone-plate viscometer (TV-25, manufactured by Toki Sangyo Co., Ltd.) at a rotation speed of 100 rpm.

[0174] Details of the raw materials for each component in Table 1 are as follows: (Epoxy resin) Epoxy resin 1: Cresol novolac type epoxy resin (EOCN-1020-55, Nippon Kayaku Co., Ltd., solid at 25°C, n=3-6) [ka]

[0175] (Phenoxy resin) Phenoxy resin 1: Bisphenol A / bisphenol F type phenoxy resin (YP-70, Nippon Steel & Sumikin Chemical Co., Ltd., Mw: approx. 41,000) [ka]

[0176] (Adhesion aid) Adhesion aid 1: 3-glycidoxypropyltrimethoxysilane (silane coupling agent, KBM-403, Shin-Etsu Chemical Co., Ltd.) [ka]

[0177] (Surfactant) ·Surfactant 1: Oligomer containing fluorine-containing group and lipophilic group (R-41, manufactured by DIC)

[0178] (Photoacid generator) [Synthesis Example 1] Synthesis of lithium tetrakis(3,4,5-trifluorophenyl)gallate 360 parts of ultra-dehydrated diethyl ether and 25.6 parts of 1-bromo-3,4,5-trifluorobenzene were charged into a 125 mL four-neck flask that had been thoroughly dried under a nitrogen atmosphere, and the flask was cooled to -78°C using a dry ice / acetone bath. 70 parts of a 2.5 mol / L n-butyllithium hexane solution were added dropwise over 10 minutes, and the mixture was then stirred at -78°C for 30 minutes. 68 parts of a diethyl ether solution in which 5 parts of gallium (III) chloride had been dissolved were added dropwise over 10 minutes, and the mixture was stirred at -78°C for 3 hours. The reaction liquid was stirred while gradually returning to room temperature, and after returning to room temperature, the mixture was stirred for another 5 hours. The precipitated solid was filtered, the reaction liquid was transferred to an evaporator, and the solvent was distilled off to obtain a gray-white product. The product was washed four times with 50 parts of ultra-dehydrated hexane, and then vacuum-dried overnight to obtain lithium tetrakis(3,4,5-trifluorophenyl)gallate. The product was 19 Identification was performed using F-NMR.

[0179] [Synthesis Example 2] Synthesis of lithium tetrakis(pentafluorophenyl)gallate Lithium tetrakis(pentafluorophenyl)gallate was obtained in the same manner as in Synthesis Example 1, except that 25.6 parts of 1-bromo-3,4,5-trifluorobenzene was replaced with 30 parts of bromopentafluorobenzene. 19 Identification was performed using F-NMR.

[0180] [Synthesis Example 3] Synthesis of lithium tetrakis[3,5-bis(trifluoromethyl)phenyl]gallate Lithium tetrakis[3,5-bis(trifluoromethyl)phenyl]gallate was obtained in the same manner as in Synthesis Example 1, except that 25.6 parts of 1-bromo-3,4,5-trifluorobenzene was replaced with 22.5 parts of 1-bromo-3,5-bis(trifluoromethyl)benzene. The product was 19 Identification was performed using F-NMR.

[0181] [Synthesis Example 4] Synthesis of Photoacid Generator (A-1) 2.0 parts of a mixture containing 51% 4-[(2-methylphenyl)sulfinyl]biphenyl and 49% 4-[(2-methylphenyl)thio]biphenyl, 0.24 parts 4-[(2-methylphenyl)thio]biphenyl, 1.2 parts acetic anhydride, 0.72 parts trifluoromethanesulfonic acid, and 6.5 parts acetonitrile were mixed uniformly and reacted at 60°C for 2 hours. The reaction solution was cooled to room temperature (about 25°C), poured into 30 parts ion-exchanged water, extracted with 30 parts dichloromethane, and washed with water until the pH of the aqueous layer became neutral. The organic layer was transferred to a rotary evaporator, the solvent was distilled off, and a product was obtained. 10 parts of ethyl acetate was added to this and dissolved in a water bath at 60°C, and then 30 parts of hexane was added and stirred, and the mixture was left to stand in a refrigerator (about 5°C) for 30 minutes, and the supernatant was removed twice, and the product was washed. This was transferred to a rotary evaporator, and the solvent was distilled off. The residue was dissolved in 27 parts of dichloromethane, and 2.8 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate synthesized in Synthesis Example 1 and 20 parts of ion-exchanged water were added and stirred at room temperature for 1 hour. The aqueous layer was removed, and the organic layer was washed three times with 20 parts of ion-exchanged water. The organic layer was then transferred to a rotary evaporator and the solvent was distilled off to obtain A-1. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0182] [ka]

[0183] [Synthesis Example 5] Synthesis of Photoacid Generator (A-2) A-2 was obtained in the same manner as in Synthesis Example 4, except that 2.8 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 3.5 parts of lithium tetrakis(pentafluorophenyl)gallate synthesized in Synthesis Example 2. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0184] [ka]

[0185] [Synthesis Example 6] Synthesis of photoacid generator (A-3) A-3 was obtained in the same manner as in Synthesis Example 4, except that 2.8 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 4.3 parts of lithium tetrakis[3,5-bis(trifluoromethyl)phenyl]gallate synthesized in Synthesis Example 3. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0186] [ka]

[0187] [Synthesis Example 7] Synthesis of photoacid generator (A-4) A-4 was obtained in the same manner as in Synthesis Example 4, except that 2.0 parts of a mixture containing 51% 4-[(2-methylphenyl)sulfinyl]biphenyl and 49% 4-[(2-methylphenyl)thio]biphenyl was replaced with 2.0 parts of a mixture containing 51% 4-[(2-methoxyphenyl)sulfinyl]biphenyl and 49% 4-[(2-methoxyphenyl)thio]biphenyl. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0188] [ka]

[0189] [Synthesis Example 8] Synthesis of photoacid generator (A-5) A-5 was obtained in the same manner as in Synthesis Example 7, except that 2.8 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 3.5 parts of lithium tetrakis(pentafluorophenyl)gallate synthesized in Synthesis Example 2. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0190] [ka]

[0191] [Synthesis Example 9] Synthesis of photoacid generator (A-6) A-6 was obtained in the same manner as in Synthesis Example 7, except that 2.8 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 4.3 parts of lithium tetrakis[3,5-bis(trifluoromethyl)phenyl]gallate synthesized in Synthesis Example 3. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0192] [ka]

[0193] [Synthesis Example 10] Synthesis of photoacid generator (A-7) A-7 was obtained in the same manner as in Synthesis Example 4, except that 2.0 parts of a mixture containing 51% 4-[(2-methylphenyl)sulfinyl]biphenyl and 49% 4-[(2-methylphenyl)thio]biphenyl was replaced with 2.0 parts of a mixture containing 55% 4-[(phenyl)sulfinyl]biphenyl and 45% 4-(phenylthio)biphenyl. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0194] [ka]

[0195] [Synthesis Example 11] Synthesis of photoacid generator (A-8) A-8 was obtained in the same manner as in Synthesis Example 10, except that 2.8 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 3.5 parts of lithium tetrakis(pentafluorophenyl)gallate synthesized in Synthesis Example 2. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0196] [ka]

[0197] [Synthesis Example 12] Synthesis of photoacid generator (A-9) A-9 was obtained in the same manner as in Synthesis Example 10, except that 2.8 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 4.3 parts of lithium tetrakis[3,5-bis(trifluoromethyl)phenyl]gallate synthesized in Synthesis Example 3. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0198] [ka]

[0199] [Synthesis Example 13] Synthesis of Photoacid Generator (B-1) 2.0 parts of a mixture containing 48% 2-(phenylsulfinyl)-fluorene and 52% 2-(phenylthio)-fluorene, 3.1 parts of acetic anhydride, and 1.6 parts of methanesulfonic acid were mixed uniformly and reacted at 65°C for 3 hours. The reaction solution was cooled to room temperature (about 25°C), poured into 5.0 parts of ion-exchanged water, extracted with 5.0 parts of dichloromethane, and washed with water until the pH of the aqueous layer became neutral. 15 parts of cyclohexane was added to this, stirred, and then allowed to stand for 30 minutes, and the operation of removing the supernatant was performed twice to wash the product. The residue was dissolved in 15.0 parts of dichloromethane, and 2.0 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate synthesized in Synthesis Example 1 and 10 parts of ion-exchanged water were added and stirred at room temperature for 1 hour. The aqueous layer was removed, the organic layer was washed three times with 10 parts of ion-exchanged water, and the organic layer was transferred to a rotary evaporator to distill off the solvent, thereby obtaining B-1. The product is 1 H-NMR, 19 Identification was performed using F-NMR.

[0200] [ka]

[0201] [Synthesis Example 14] Synthesis of Photoacid Generator (B-2) B-2 was obtained in the same manner as in Synthesis Example 13, except that 2.0 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 2.4 parts of lithium tetrakis(pentafluorophenyl)gallate synthesized in Synthesis Example 2. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0202] [ka]

[0203] [Synthesis Example 15] Synthesis of Photoacid Generator (B-3) B-3 was obtained in the same manner as in Synthesis Example 13, except that 2.0 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 3.0 parts of lithium tetrakis[3,5-bis(trifluoromethyl)phenyl]gallate synthesized in Synthesis Example 3. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0204] [ka]

[0205] [Synthesis Example 16] Synthesis of photoacid generator (B-4) B-4 was obtained in the same manner as in Synthesis Example 13, except that 2.0 parts of a mixture containing 48% 2-(phenylsulfinyl)-fluorene and 52% 2-(phenylthio)-fluorene was replaced with 2.0 parts of a mixture containing 48% 2-(phenylsulfinyl)-9,9-dimethylfluorene and 52% 2-(phenylthio)-9,9-dimethylfluorene. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0206] [ka]

[0207] [Synthesis Example 17] Synthesis of photoacid generator (B-5) B-5 was obtained in the same manner as in Synthesis Example 16, except that 2.0 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 2.4 parts of lithium tetrakis(pentafluorophenyl)gallate synthesized in Synthesis Example 2. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0208] [ka]

[0209] [Synthesis Example 18] Synthesis of photoacid generator (B-6) B-6 was obtained in the same manner as in Synthesis Example 16, except that 2.0 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 3.0 parts of lithium tetrakis[3,5-bis(trifluoromethyl)phenyl]gallate synthesized in Synthesis Example 3. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0210] [ka]

[0211] [Synthesis Example 19] Synthesis of photoacid generator (B-7) B-7 was obtained in the same manner as in Synthesis Example 13, except that 2.0 parts of a mixture containing 48% 2-(phenylsulfinyl)-fluorene and 52% 2-(phenylthio)-fluorene was replaced with 2.0 parts of a mixture containing 48% 2-(phenylsulfinyl)-9,9-diethylfluorene and 52% 2-(phenylthio)-9,9-diethylfluorene. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0212] [ka]

[0213] [Synthesis Example 20] Synthesis of photoacid generator (B-8) B-8 was obtained in the same manner as in Synthesis Example 19, except that 2.0 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 2.4 parts of lithium tetrakis(pentafluorophenyl)gallate synthesized in Synthesis Example 2. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0214] [ka]

[0215] [Synthesis Example 21] Synthesis of photoacid generator (B-9) B-9 was obtained in the same manner as in Synthesis Example 19, except that 2.0 parts of lithium tetrakis(3,4,5-trifluorophenyl)gallate was replaced with 3.0 parts of lithium tetrakis[3,5-bis(trifluoromethyl)phenyl]gallate synthesized in Synthesis Example 3. The product was 1 H-NMR, 19 Identification was performed using F-NMR.

[0216] [ka]

[0217] Photoacid generator (C-1): Triarylsulfonium borate salt (San-Apro, CPI-310B)

[0218] [Table 1]

[0219] The obtained photosensitive resin compositions were evaluated based on the following evaluation items.

[0220] <Evaluation of insulation reliability> (Preparation of test specimens for evaluation) A heat-resistant polyvinyl chloride resin sheet was prepared as a substrate. A comb-shaped Cu plating film (Cu electrode) with a width of 30 μm, a pitch of 20 μm, and a thickness of 10 to 15 μm was formed on the substrate to obtain a Cu wiring board. Next, the obtained photosensitive resin composition was spin-coated on the Cu wiring substrate to form a spin-coated film (liquid film). The liquid film was heated at 100°C for 3 minutes and dried to obtain a photosensitive resin film with a thickness of 30 μm. Next, the obtained photosensitive resin film was exposed to 600 mJ / cm 365 nm i-line light using an automatic exposure machine. 2 The entire surface was exposed to an exposure dose of 1000 μg / cm. Next, the Cu wiring substrate was heated on a hot plate in the atmosphere at 70° C. for 5 minutes. Next, the Cu wiring substrate was immersed in PGMEA for 20 seconds. Thereafter, the Cu wiring board was heated in a nitrogen atmosphere at 170° C. for 180 minutes to harden the photosensitive resin film, thereby obtaining a test piece for evaluation.

[0221] (Bias-HAST test (test time: 100 hours)) The evaluation test piece obtained in the above (Preparation of evaluation test piece) was placed in the B-HAST device. Then, the wiring of the B-HAST device and the Cu electrode of the evaluation test were soldered. The B-HAST device is a biased highly accelerated stress test device.

[0222] Next, the temperature inside the device was set to 130°C, the relative humidity inside the device was set to 85%, and a bias of 3.5 V was applied between the Cu electrodes spaced apart from each other. Subsequently, the insulation resistance value between the Cu electrodes was automatically measured at 6-minute intervals from the start of application. Then, the elapsed time from the start of application to the occurrence of leakage (insulation breakdown) (leak occurrence time) was measured. Note that leakage occurs when the measured insulation resistance value reaches 1.0×10 4 This refers to the case where the resistance drops below Ω.

[0223] The measured leak occurrence time was then evaluated based on the following evaluation criteria. The evaluation results are shown in Table 1. Leak time evaluation criteria: ◎: Leak occurrence time is 100 hours or more ○: The leak occurred for 50 hours or more but less than 100 hours. ×: Leak occurrence time is less than 50 hours

[0224] <Evaluation of patterning ability> The obtained photosensitive resin composition was applied onto an 8-inch silicon wafer using a spin coater. After application, the wafer was prebaked at 120° C. for 3 minutes in the atmosphere on a hot plate to obtain a coating film having a thickness of about 9.0 μm. This coating film was irradiated with i-line through a mask (drawn with 1.0-100μm wide patterns) manufactured by Toppan Printing Co., Ltd. An i-line stepper (Nikon Corporation, NSR-4425i) was used for irradiation. After exposure, the wafer was placed on a hot plate and baked in air at 80° C. for 5 minutes. Thereafter, the unexposed areas were dissolved and removed by spray development for 30 seconds using PGMEA as a developer. The cross section of the 100 μm wide via pattern on the obtained coating sample was then observed using a tabletop SEM (Hitachi High-Technologies Corporation) to confirm the presence or absence of undercuts. The evaluation results are shown in Table 1. Evaluation criteria for patterning: 〇: No undercut occurred ×: Undercut occurs

[0225] <Evaluation of tensile elongation> - Preparation of hardened film (1) The photosensitive resin compositions of Examples 1, 8, 12 and Comparative Example 2 were each applied onto a substrate by spin coating so that the film thickness after drying was 10 μm, and then dried at 120° C. for 5 minutes to form a photosensitive resin film. (2) The photosensitive resin film obtained in (1) above is exposed to 600 mJ / cm 2 using an automatic exposure machine. 2 It was fully exposed. (3) After the above (2), the substrate was post-exposure heated on a hot plate at 100° C. for 5 minutes. (4) After the above (3), the coating was cured under nitrogen at 170° C. for 180 minutes to obtain a cured film for evaluation. Elongation measurement A sample was cut out from the cured film for evaluation obtained above, and the measurement sample with a film thickness of 10 μm, width of 6.5 mm, and distance between chucks for fixing the sample of 20 mm was measured with a Tensilon universal material measuring instrument RTA-100 (A & D Co., Ltd.) using a 100 N load cell at a tensile speed of 5 mm / min. In each example, 10 samples were measured, and the average values ​​(%) for the six samples excluding the four samples with the best elongation rate, the second best elongation rate, the worst elongation rate and the second worst elongation rate are shown in Table 2 below.

[0226] [Table 2]

[0227] It was found that the photosensitive resin compositions of Examples 1 to 18 had superior insulation reliability compared to Comparative Example 1. It was also found that the photosensitive resin compositions of Examples 1 to 18 had better patterning properties (pattern shape) compared to Comparative Example 2. It is expected that such photosensitive resin compositions of Examples 1 to 18 can be suitably used for bump protection films such as insulating films for wiring layers. [Explanation of symbols]

[0228] 1 Semiconductor device 1A Semiconductor Device 1B Semiconductor Device 2 Through-hole electrode substrate 3. Semiconductor Package 5. Photosensitive resin varnish 21 Insulating layer 23 Semiconductor Chips 24 Lower wiring layer 24A lower wiring layer 24B Lower wiring layer 25 Upper wiring layer 26 Solder Bumps 27 Chip embedding structure 31 Package substrate 32 Semiconductor Chips 33 Bonding Wire 34 Sealing layer 35 Solder Bumps 202 Substrate 221 Through Wiring 222 Through Wiring 231 rand 240 Organic Insulating Layer 241 Organic Insulating Layer 242 Organic Insulating Layer 243 Wiring layer 245 Bump Adhesion Layer 251 Organic Insulating Layer 252 Organic Insulating Layer 253 Wiring layer 254 Through Wiring 412 Mask 423 Opening 424 Opening 2510 Photosensitive resin layer 2520 Photosensitive resin layer S1 Chip placement process S2 Upper wiring layer formation process S20 First resin film placement process S21 First exposure process S22 1st development process S23 1st curing process S24 Wiring layer formation process S25 Second resin film placement process S26 Second exposure process S27 2nd development process S28 2nd curing process S29 Through-hole wiring formation process S3 Substrate peeling process S4 Lower wiring layer formation process S5 Solder bump formation process S6 Lamination process W diameter

Claims

1. Epoxy resin, Phenoxy resin, A photosensitive resin composition for use in a bump protective film, comprising: the photoacid generator comprises an onium gallate salt having a triarylsulfonium cation and a gallate anion, the epoxy resin comprises one or more epoxy resins selected from the group consisting of phenol novolac epoxy resins and cresol novolac epoxy resins, The photosensitive resin composition, wherein the epoxy resin is a thermosetting resin and the phenoxy resin is a thermoplastic resin.

2. The photosensitive resin composition according to claim 1, The phenoxy resin has a weight average molecular weight of 10,000 to 100,000.

3. The photosensitive resin composition according to claim 1 or 2, The photosensitive resin composition, wherein the triarylsulfonium cation contains at least one compound represented by the following general formula (1): [Formula 1] (In the above general formula (1), R 1 ~R 4 each independently represents an alkyl group, a hydroxy group, an alkoxy group, an alkylcarbonyl group, an arylcarbonyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an arylthiocarbonyl group, an acyloxy group, an arylthio group, an alkylthio group, an aryl group, a heterocyclic hydrocarbon group, an aryloxy group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, a hydroxy(poly)alkyleneoxy group, a group that forms a condensed polycyclic hydrocarbon skeleton by condensing with the benzene ring to which it is bonded, a substituted or unsubstituted silyl group, an amino group, a cyano group, a nitro group, or a halogen atom; 1 ~R 4a is an integer from 1 to 5, c and d are integers from 0 to 5, and b is an integer from 0 to 4.

4. The photosensitive resin composition according to any one of claims 1 to 3, The photosensitive resin composition, wherein the gallate anion contains a compound represented by the following general formula (5): [chemical 2] (In the above general formula (5), R 13 ~R 16 each independently represents a phenyl group or a perfluoroalkyl group which is unsubstituted or substituted with a group selected from the group consisting of a perfluoroalkyl group, a perfluoroalkoxy group, a nitro group, a cyano group, an acyl group, and a halogen atom.

5. The photosensitive resin composition according to any one of claims 1 to 4, A photosensitive resin composition, wherein the content of the photoacid generator is 0.3 mass % or more and 5.0 mass % or less based on the total solid content of the photosensitive resin composition.

6. The photosensitive resin composition according to any one of claims 1 to 5, A photosensitive resin composition comprising a surfactant.

7. The photosensitive resin composition according to any one of claims 1 to 6, A photosensitive resin composition comprising an adhesion aid.

8. The photosensitive resin composition according to any one of claims 1 to 7, A photosensitive resin composition comprising a solvent.

Citation Information

Patent Citations

  • Photosensitive resin composition, photosensitive element, semiconductor device and method for forming resist pattern

    JP2016188987A

  • Photosensitive resin composition, dry film resist, and cured objects obtained therefrom

    WO2019111796A1

  • Photosensitive resin composition for bump protecting films, semiconductor device, method for manufacturing semiconductor device, and electronic device

    WO2019208443A1