Hydrotalcite and fiber composite fiber and products containing same
A composite fiber of hydrotalcite and fiber, synthesized with controlled copper content, addresses the lack of deodorizing, antibacterial, and antiallergenic properties in existing fibers, offering effective deodorization and microbial inactivation for various products.
Patent Information
- Application Number
- JP2020087832
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-20
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-05-20
AI Technical Summary
Existing composite fibers do not effectively provide deodorizing, antibacterial, antiviral, and antiallergenic properties, and there is a need for an efficient method to produce such fibers.
A composite fiber of hydrotalcite and fiber is created by controlling the amount of copper added, with hydrotalcite containing copper and zinc, covering 15% or more of the fiber surface, and having a copper content of 10 to 40% by weight, which is synthesized using a coprecipitation reaction with controlled temperature and pH.
The composite fiber exhibits excellent deodorizing, antibacterial, antiviral, and antiallergenic properties, making it suitable for products like masks, wipers, and adsorbents, with high ash content and effective odor reduction and bacterial/viral inactivation.
Smart Images

Figure 0007590817000003 
Figure 0007590817000004 
Figure 0007590817000005
Abstract
Description
Technical Field
[0001] The present invention relates to a composite fiber of inorganic particles and fibers and a product containing the same.
Background Art
[0002] Generally, hydrotalcite has the general formula [M 2+ 1-x M 3+ x (OH)2][A n- x / n ·mH2O] (wherein M 2+ represents a divalent metal ion, M 3+ represents a trivalent metal ion, A n- x / n represents an interlayer anion. Also, 0 < x < 1, n is the valence of A, and 0 ≦ m < 1), and is one of the compounds represented by, and is a substance used as a catalyst, a pharmaceutical, an additive for resins, etc. (Patent Documents 1 to 3).
[0003] Hydrotalcite is a metal hydroxide having a layered crystal structure similar to talc and smectite, and each crystal piece of hydrotalcite is often flaky or scaly. As hydrotalcite, manasseite which is a polytype of hydrotalcite, pyroaurite and sjgrenite in which the metals contained in the hydroxide sheet are magnesium and iron, and further green rust having divalent and trivalent iron in the hydroxide sheet are known. Since the main skeleton is a double hydroxide, it is also called a layered double hydroxide (LDH). Hydrotalcite is also produced naturally, but since the production amount is small, mainly synthetic products are used, and various synthetic methods are known.
[0004] Patent Document 4 proposes a deodorant fabric in which a metal hydroxide such as hydrotalcite is supported on a polyurethane fiber or the like, and Patent Document 5 describes a method for fixing hydrotalcite to a fiber.
Prior Art Documents
[0005] [Patent Document 1] JP 2015-193000 A [Patent Document 2] JP 2013-085568 A [Patent Document 3] JP 2009-143798 A [Patent Document 4] JP 2012-144829 A [Patent Document 5] International Publication WO2018 / 030521 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention aims to provide a composite fiber (composite) of hydrotalcite and fiber that can be suitably used as a raw material for products that require deodorizing, antibacterial, antiviral, and antiallergen effects, and to provide a method for efficiently producing the composite fiber of hydrotalcite and fiber. [Means for solving the problem]
[0007] As a result of intensive research into the above-mentioned problems, the present inventors discovered that by controlling the amount of copper added, a composite fiber (composite) of hydrotalcite and fiber having excellent deodorizing, antibacterial, antiviral, and antiallergen properties can be obtained, and thus completed the present invention.
[0008] The present invention includes, but is not limited to, the following aspects. [1] A composite fiber having hydrotalcite containing copper and zinc fixed to the fiber, wherein 15% or more of the fiber surface is covered with hydrotalcite, and the copper content in the hydrotalcite is 10 to 40% by weight. [2] The composite fiber according to [1], wherein the molar ratio of copper to zinc contained in the hydrotalcite is 2:4 to 5:1. [3] The composite fiber according to [1] or [2], wherein the fiber is a cellulose fiber. [4] The composite fiber according to any one of [1] to [3], wherein the average primary particle size of the hydrotalcite is 1 μm or less. [5] A product containing the composite fiber described in any one of [1] to [4]. [6] The product according to [5], which is in the form of a sheet, pulp mold, or granules. [7] The product according to [5] or [6], wherein the product is a nonwoven fabric or paper. [8] A product according to any one of [5] to [7] for use in hygiene products. [9] The product according to any one of [5] to [8] for use in a mask, wiper, or adsorbent.
[10] The product according to any one of [5] to [9], which is used for deodorizing, antibacterial or antiviral purposes.
[11] The product described in any of [5] to
[10] , having an antibacterial activity value of 2.0 or more for any one of Escherichia coli, Staphylococcus aureus, Klebsiella pneumoniae, MRSA, Pseudomonas aeruginosa, and Moraxella, measured based on JIS L 1902:2015.
[12] A product according to any of [5] to
[11] , in which the odor component reduction rate measured based on the deodorizing test method of the SEK Mark textile product certification standard (JEC301) is equal to or greater than the standard value specified in JEC301 for any one of ammonia, hydrogen sulfide, methyl mercaptan, acetic acid, isovaleric acid, indole, and nonenal.
[13] The product described in any of [5] to
[12] , having an antiviral activity value (Mv) against influenza virus or feline calicivirus of 2.0 or more as measured based on JIS L 1922:2016.
[14] The product according to [5] to
[13] , having a copper content of 7.0% by weight or less.
[15] The product according to any one of [5] to
[14] , having a zinc content of 1.0% by weight or more. Effect of the Invention
[0009] According to the present invention, it is possible to provide a composite fiber of hydrotalcite and fiber, which can be suitably used as a raw material for products that require deodorizing, antibacterial, antiviral, anti-allergenic, and adsorption effects. In particular, the composite fiber according to the present invention has deodorizing, antibacterial, antiviral, anti-allergenic, and adsorption effects, and is suitable for sanitary materials such as masks and wiper sheets, and adsorbents (for removing impurities, deodorizing, dehumidifying, etc.).
Brief Description of the Drawings
[0010] [Figure 1] Figure 1 is a schematic diagram of the synthesis apparatus used in the examples. [Diagram 2] Figure 2 is an electron micrograph of the composite fiber according to Sample 2 (left: 500 times, right: 10,000 times). [Diagram 3] Figure 3 is an electron micrograph of the composite fiber according to Sample 4 (left: 500 times, right: 10,000 times).
Embodiments for Carrying Out the Invention
[0011] Hydrotalcite (HT) Generally, hydrotalcite is represented by the general formula [[M 2+ 1-x M 3+ x (OH)2][A n- x / n ·mH2O] (where M 2+ represents a divalent metal ion, M 3+ represents a trivalent metal ion, and A n- x / n represents an interlayer anion. Also, 0 < x < 1, n is the valence of A, and 0 ≤ m < 1). Here, M 2+ as the divalent metal ion is, for example, Mg 2+ , Co 2+ , Ni 2+ , Zn 2+ , Fe 2+ , Ca 2+ , Ba 2+ , Cu 2+ , Mn 2+ etc., and M 3+ as the trivalent metal ion is, for example, Al3+ , Fe 3+ , Cr 3+ , Ga 3+ etc., A is an interlayer anion n- For example, OH - , Cl - , CO3 - , SO4 - Examples of n-valent anions include, where x is generally in the range of 0.2 to 0.33. Among these, examples of divalent metal ions include Mg 2+ , Zn 2+ , Fe 2+ , Mn 2+ The crystal structure is a laminated structure consisting of a two-dimensional basic layer in which positively charged octahedral brucite units are arranged and a negatively charged intermediate layer. The hydrotalcite according to the present invention contains copper and zinc, and the copper content in the hydrotalcite is 10 to 40% by weight.
[0012] Taking advantage of its anion exchange function, hydrotalcite has been developed into various applications, for example, as an ion exchange material, adsorbent, deodorant, etc. In addition, by taking advantage of the combination of constituent metal ions, hydrotalcite in which the constituent metal ions are in a good mixed state can be heated and dehydrated, or further heated and calcined, to easily obtain composite oxides of uniform composition, which can be used for catalytic applications, etc.
[0013] Hydrotalcite and fiber composite fiber In the present invention, a composite fiber of hydrotalcite and fiber is produced by synthesizing hydrotalcite in a solution in the presence of fiber.
[0014] The ratio of hydrotalcite in the composite fiber of the present invention can be 10% or more, can be 20% or more, and can be preferably 40% or more. The ash content of the composite fiber of hydrotalcite and fiber can be measured according to JIS P 8251:2003. In the present invention, the ash content of the composite fiber of hydrotalcite and fiber can be 10% or more, can be 20% or more, and can be preferably 40% or more. In addition, the composite fiber of hydrotalcite and fiber of the present invention preferably contains magnesium, iron, manganese or zinc in the ash content of 10% or more, more preferably 40% or more. The magnesium or zinc content in the ash content can be quantified by fluorescent X-ray analysis.
[0015] The present invention relates to a composite fiber of hydrotalcite and fibers, and in a preferred embodiment, 15% or more of the fiber surface is covered with hydrotalcite. In a preferred embodiment, the composite fiber of the present invention has a fiber coverage (area ratio) of hydrotalcite of 25% or more, more preferably 40% or more, but according to the present invention, it is also possible to produce composite fibers with a coverage of 60% or more or 80% or more. Furthermore, in a preferred embodiment, it has been revealed from the results of electron microscope observation that the hydrotalcite is not only fixed on the outer surface of the fiber and inside the lumen, but is also formed inside the microfibrils in the composite fiber of hydrotalcite and fibers according to the present invention.
[0016] The composite fiber with inorganic particles is preferably used in an amount such that 15% or more of the fiber surface is covered with the inorganic particles. For example, the weight ratio of the fiber to the inorganic particles can be 5 / 95 to 95 / 5, or it can be 10 / 90 to 90 / 10, 20 / 80 to 80 / 20, 30 / 70 to 70 / 30, or 40 / 60 to 60 / 40.
[0017] When hydrotalcite and fibers are made into a composite fiber according to the present invention, not only is the hydrotalcite more likely to be retained in the product compared to when the hydrotalcite is simply mixed with fibers, but a product can be obtained in which the hydrotalcite is uniformly dispersed without agglomeration. That is, according to the present invention, the yield of the composite fiber of hydrotalcite and fibers in the product (the weight ratio of the added hydrotalcite that remains in the product) can be 65% or more, and can also be 70% or more, or 85% or more.
[0018] The hydrotalcite can be synthesized by a known method. For example, the fibers are immersed in a carbonate aqueous solution containing carbonate ions constituting the intermediate layer and an alkaline solution (such as sodium hydroxide) in a reaction vessel, then an acid solution (a metal salt aqueous solution containing divalent metal ions and trivalent metal ions constituting the basic layer) is added, and the temperature, pH, etc. are controlled to synthesize hydrotalcite by a coprecipitation reaction. Alternatively, the fibers can be immersed in an acid solution (a metal salt aqueous solution containing divalent metal ions and trivalent metal ions constituting the basic layer) in a reaction vessel, then an aqueous carbonate solution containing carbonate ions constituting the intermediate layer and an alkaline solution (such as sodium hydroxide) are dropped, and the temperature, pH, etc. are controlled to synthesize hydrotalcite by a coprecipitation reaction. Although the reaction at normal pressure is common, there is also a method of obtaining hydrotalcite by a hydrothermal reaction using an autoclave or the like (JP Patent Publication 60-6619).
[0019] In the present invention, various chlorides, sulfides, nitrates, and sulfates of magnesium, zinc, barium, calcium, iron, copper, cobalt, nickel, and manganese can be used as sources of divalent metal ions constituting the basic layer, and various chlorides, sulfides, nitrates, and sulfates of aluminum, iron, chromium, and gallium can be used as sources of trivalent metal ions constituting the basic layer.
[0020] In the present invention, water is used for preparing the suspension, etc., and as the water, ordinary tap water, industrial water, groundwater, well water, etc. can be used. In addition, ion-exchanged water, distilled water, ultrapure water, industrial wastewater, and water obtained during the production process can also be suitably used.
[0021] In the present invention, carbonate ions, nitrate ions, chloride ions, sulfate ions, phosphate ions, etc. can be used as the interlayer anions. When carbonate ions are used as the interlayer anions, sodium carbonate is used as the supply source. However, sodium carbonate can be replaced with a gas containing carbon dioxide (carbonic acid gas), and may be substantially pure carbon dioxide gas or a mixture with other gases. For example, exhaust gas discharged from an incinerator, a coal boiler, a heavy oil boiler, etc. in a paper factory can be suitably used as the carbon dioxide-containing gas. In addition, the carbon dioxide generated from the lime burning process can be used to carry out the carbonation reaction.
[0022] When producing the composite fiber of the present invention, various known auxiliary agents can be further added. For example, a chelating agent can be added to the neutralization reaction, and specific examples thereof include polyhydroxycarboxylic acids such as citric acid, malic acid, and tartaric acid, dicarboxylic acids such as oxalic acid, sugar acids such as gluconic acid, aminopolycarboxylic acids such as iminodiacetic acid and ethylenediaminetetraacetic acid, and alkali metal salts thereof, alkali metal salts of polyphosphoric acids such as hexametaphosphoric acid and tripolyphosphoric acid, amino acids such as glutamic acid and aspartic acid, and alkali metal salts thereof, ketones such as acetylacetone, methyl acetoacetate, and allyl acetoacetate, sugars such as sucrose, and polyols such as sorbitol. In addition, as a surface treatment agent, saturated fatty acids such as palmitic acid and stearic acid, unsaturated fatty acids such as oleic acid and linoleic acid, alicyclic carboxylic acids, resin acids such as abietic acid, their salts, esters and ethers, alcohol-based surfactants, sorbitan fatty acid esters, amide-based and amine-based surfactants, polyoxyalkylene alkyl ethers, polyoxyethylene nonylphenyl ether, sodium alpha-olefin sulfonate, long-chain alkyl amino acids, amine oxides, alkylamines, quaternary ammonium salts, aminocarboxylic acids, phosphonic acids, polyvalent carboxylic acids, condensed phosphoric acids, etc. can be added. In addition, a dispersant can be used as necessary. Examples of the dispersant include sodium polyacrylate, sucrose fatty acid esters, glycerin fatty acid esters, acrylic acid-maleic acid copolymer ammonium salts, methacrylic acid-naphthoxy polyethylene glycol acrylate copolymers, methacrylic acid-polyethylene glycol monomethacrylate copolymer ammonium salts, polyethylene glycol monoacrylate, etc. These can be used alone or in combination. In addition, the timing of addition may be before or after the neutralization reaction. Such additives can be added in an amount of preferably 0.001 to 20%, more preferably 0.1 to 10%, based on the hydrotalcite.
[0023] (Reaction conditions) In the present invention, the temperature of the synthesis reaction can be, for example, 30 to 100° C., preferably 40 to 80° C., more preferably 50 to 70° C., and particularly preferably about 60° C. If the temperature is too high or too low, the reaction efficiency tends to decrease and the cost tends to increase.
[0024] In the present invention, the neutralization reaction can be a batch reaction or a continuous reaction. In general, it is preferable to carry out a batch reaction process because of the convenience of discharging the residue after the neutralization reaction. The scale of the reaction is not particularly limited, but the reaction may be carried out on a scale of 100 L or less, or on a scale of more than 100 L. The size of the reaction vessel may be, for example, about 10 L to 100 L, or about 100 L to 1000 L.
[0025] Furthermore, the neutralization reaction can be controlled by monitoring the pH of the reaction suspension, and depending on the pH profile of the reaction, the carbonation reaction can be carried out until it reaches, for example, a pH below 9, preferably below pH 8, and more preferably around pH 7.
[0026] On the other hand, the neutralization reaction can also be controlled by monitoring the conductivity of the reaction solution. It is preferable to carry out the carbonation reaction until the conductivity falls to 100 mS / cm or less. Furthermore, the synthesis reaction can be controlled by the reaction time, specifically, by adjusting the residence time of the reactants in the reaction tank. In addition, in the present invention, the reaction can also be controlled by stirring the reaction solution in the reaction tank or by making the neutralization reaction a multi-stage reaction.
[0027] In the present invention, the composite fiber, which is the reaction product, is obtained as a suspension, and therefore, if necessary, it can be stored in a storage tank, concentrated, dehydrated, pulverized, classified, aged, dispersed, and other processes. These can be performed by known processes, and may be appropriately determined in consideration of the application, energy efficiency, and the like. For example, the concentration and dehydration process is performed using a centrifugal dehydrator, a sedimentation concentrator, and the like. Examples of this centrifugal dehydrator include a decanter and a screw decanter. When a filter or dehydrator is used, there is no particular limitation on the type, and a general one can be used, but for example, a pressurized dehydrator such as a filter press, a drum filter, a belt press, or a tube press, or a vacuum drum dehydrator such as an Oliver filter, and the like can be suitably used to produce a calcium carbonate cake. Examples of the grinding method include a ball mill, a sand grinder mill, an impact mill, a high-pressure homogenizer, a low-pressure homogenizer, a dyno mill, an ultrasonic mill, a kanda grinder, an attritor, a stone mill, a vibration mill, a cutter mill, a jet mill, a disintegrator, a beater, a single-screw extruder, a twin-screw extruder, an ultrasonic agitator, a household juicer mixer, etc. Examples of the classification method include a sieve such as a mesh, an outward or inward slit or round-hole screen, a vibration screen, a heavy foreign matter cleaner, a light foreign matter cleaner, a reverse cleaner, a sieving tester, etc. Examples of the dispersion method include a high-speed disperser, a low-speed kneader, etc.
[0028] The composite fiber obtained by the present invention can be blended with a filler or pigment in the form of a suspension without being completely dehydrated, or can be dried to form a powder. There are no particular limitations on the dryer used in this case, and for example, a flash dryer, band dryer, spray dryer, etc. can be suitably used.
[0029] The composite fiber obtained by the present invention can be treated with a weak acid such as dilute hydrochloric acid or dilute nitric acid to intercalate chloride ions, nitrate ions, etc. as interlayer ions. An anionic substance can be used as an intercalating compound, such as a copper or silver thiosulfato complex. The intercalation method can be a known method, such as adding a solution containing an anionic substance to a composite fiber of hydrotalcite and fiber and mixing it.
[0030] The composite fiber obtained by the present invention can be modified by known methods. For example, in one embodiment, the surface can be made hydrophobic to enhance compatibility with resins, etc.
[0031] fiber In the present invention, hydrotalcite and fibers are made into a composite fiber. The fibers constituting the composite fiber are not particularly limited, and examples thereof include natural fibers such as cellulose, synthetic fibers artificially synthesized from raw materials such as petroleum, regenerated fibers (semi-synthetic fibers) such as rayon and lyocell, and inorganic fibers such as ceramics, without any restrictions. In addition to the above, natural fibers include protein-based fibers such as wool, silk thread, and collagen fibers, and complex carbohydrate-based fibers such as chitin / chitosan fibers and alginic acid fibers.
[0032] Examples of cellulosic raw materials include pulp fiber (wood pulp and non-wood pulp) and bacterial cellulose, and wood pulp can be produced by pulping a wood raw material. Examples of wood raw materials include coniferous trees such as red pine, black pine, Abies sachalinensis, Yezo spruce, red pine, larch, fir, hemlock, cedar, cypress, larch, Shirabe, spruce, hiba, Douglas fir, hemlock, white fir, spruce, balsam fir, cedar, pine, Merkusima pine, and radiata pine, and mixtures thereof, and broad-leaved trees such as beech, birch, alder, oak, tabu, chinquapin, white birch, cottonwood, poplar, ash, Japanese knotweed, eucalyptus, mangrove, lauan, and acacia, and mixtures thereof.
[0033] The method for pulping the wood raw material is not particularly limited, and examples include pulping methods commonly used in the paper manufacturing industry. Wood pulp can be classified by pulping method, and examples include chemical pulp cooked by methods such as the Kraft method, the sulfite method, the soda method, and the polysulfide method; mechanical pulp obtained by pulping using mechanical forces such as a refiner or grinder; semi-chemical pulp obtained by pretreatment with chemicals and then pulping using mechanical forces; waste paper pulp; and deinked pulp. Wood pulp may be in an unbleached state (before bleaching) or in a bleached state (after bleaching).
[0034] Examples of non-wood-derived raw materials include cotton, hemp, sisal, Manila hemp, flax, straw, bamboo, bagasse, kenaf, sugar cane, corn, rice straw, paper mulberry, and mitsumata.
[0035] The pulp fibers may be either unbeaten or beaten, and the choice may be made depending on the physical properties of the composite fiber sheet, but it is preferable to beat the pulp fibers, which is expected to improve the sheet strength and promote the fixation of calcium carbonate.
[0036] Examples of synthetic fibers include polyester, polyamide, polyolefin, acrylic, nylon, acrylic, vinylon, and ceramic fibers. Examples of semi-synthetic fibers include rayon and acetate. Examples of inorganic fibers include glass fibers, carbon fibers, and various metal fibers.
[0037] Furthermore, these cellulose raw materials can be further treated to be used as powdered cellulose, chemically modified cellulose such as oxidized cellulose, and cellulose nanofibers: CNF (microfibrillated cellulose: MFC, TEMPO-oxidized CNF, phosphoric acid esterified CNF, carboxymethylated CNF, mechanically crushed CNF, etc.). As the powdered cellulose used in the present invention, for example, a crystalline cellulose powder having a certain particle size distribution and a rod shape produced by purifying and drying the undecomposed residue obtained after acid hydrolysis of selected pulp, followed by crushing and sieving may be used, or a commercially available product such as KC Flock (Nippon Paper Industries Co., Ltd.), Ceolas (Asahi Kasei Chemicals Co., Ltd.), or Avicel (FMC Co., Ltd.) may be used. The degree of polymerization of cellulose in the powdered cellulose is preferably about 100 to 1500, the degree of crystallinity of the powdered cellulose as measured by an X-ray diffraction method is preferably 70 to 90%, and the volume average particle size as measured by a laser diffraction particle size distribution measuring device is preferably 1 μm or more and 100 μm or less. The oxidized cellulose used in the present invention can be obtained by, for example, oxidation in water using an oxidizing agent in the presence of a compound selected from the group consisting of N-oxyl compounds, and bromides, iodides, or mixtures thereof. For the cellulose nanofibers, a method of defibrating the above-mentioned cellulose raw material is used. For example, a method of defibrating an aqueous suspension of chemically modified cellulose such as cellulose or oxidized cellulose by mechanical grinding or beating using a refiner, high-pressure homogenizer, grinder, single-shaft or multi-shaft kneader, bead mill, or the like can be used. The cellulose nanofibers may be produced by one or a combination of a plurality of the above methods. The fiber diameter of the produced cellulose nanofibers can be confirmed by observation under an electron microscope, and is, for example, in the range of 5 nm to 1000 nm, preferably 5 nm to 500 nm, and more preferably 5 nm to 300 nm. When producing the cellulose nanofibers, any compound can be further added and reacted with the cellulose nanofibers before and / or after defibrating and / or pulverizing the cellulose to obtain a hydroxyl group-modified cellulose nanofiber.The functional groups to be modified include an acetyl group, an ester group, an ether group, a ketone group, a formyl group, a benzoyl group, an acetal, a hemiacetal, an oxime, an isonitrile, an allene, a thiol group, a urea group, a cyano group, a nitro group, an azo group, an aryl group, an aralkyl group, an amino group, an amide group, an imide group, an acryloyl group, a methacryloyl group, a propionyl group, a propioloyl group, a butyryl group, a 2-butyryl group, a pentanoyl group, a hexanoyl group, a heptanoyl group, an octanoyl group, a nonanoyl group, a decanoyl group, an undecanoyl group, a dodecanoyl group, a myristoyl group, a palmitoyl group, a sucrose ... Examples of the alkyl groups include acyl groups such as thiaroyl, pivaloyl, benzoyl, naphthoyl, nicotinoyl, isonicotinoyl, furoyl, and cinnamoyl groups, isocyanate groups such as 2-methacryloyloxyethylisocyanoyl groups, alkyl groups such as methyl, ethyl, propyl, 2-propyl, butyl, 2-butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, myristyl, palmityl, and stearyl groups, oxirane, oxetane, oxyl, thiirane, and thietane groups. Hydrogen in these substituents may be replaced with functional groups such as hydroxyl and carboxyl groups. In addition, a part of the alkyl group may be an unsaturated bond. Compounds used to introduce these functional groups are not particularly limited, and examples thereof include compounds having a group derived from phosphoric acid, compounds having a group derived from carboxylic acid, compounds having a group derived from sulfuric acid, compounds having a group derived from sulfonic acid, compounds having an alkyl group, and compounds having a group derived from amine. Compounds having a phosphoric acid group are not particularly limited, and examples thereof include phosphoric acid, lithium salts of phosphoric acid such as lithium dihydrogen phosphate, dilithium hydrogen phosphate, trilithium phosphate, lithium pyrophosphate, and lithium polyphosphate. Further examples thereof include sodium salts of phosphoric acid such as sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium pyrophosphate, and sodium polyphosphate. Further examples thereof include potassium salts of phosphoric acid such as potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, and potassium polyphosphate.Further examples of the ammonium salt of phosphoric acid include ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium polyphosphate. Among these, from the viewpoint of high efficiency of phosphoric acid group introduction and easy industrial application, phosphoric acid, sodium salt of phosphoric acid, potassium salt of phosphoric acid, and ammonium salt of phosphoric acid are preferred, and sodium dihydrogen phosphate and disodium hydrogen phosphate are more preferred, but are not particularly limited. Examples of compounds having a carboxyl group include, but are not particularly limited to, dicarboxylic acid compounds such as maleic acid, succinic acid, phthalic acid, fumaric acid, glutaric acid, adipic acid, and itaconic acid, and tricarboxylic acid compounds such as citric acid and aconitic acid. Examples of acid anhydrides of compounds having a carboxyl group include, but are not particularly limited to, acid anhydrides of dicarboxylic acid compounds such as maleic anhydride, succinic anhydride, phthalic anhydride, glutaric anhydride, adipic anhydride, and itaconic anhydride. Examples of derivatives of compounds having a carboxyl group include, but are not particularly limited to, imidized products of acid anhydrides of compounds having a carboxyl group, and derivatives of acid anhydrides of compounds having a carboxyl group. The imide of the acid anhydride of the compound having a carboxyl group is not particularly limited, and includes the imide of a dicarboxylic acid compound such as maleimide, succinimide, and phthalimide. The derivative of the acid anhydride of the compound having a carboxyl group is not particularly limited. For example, at least some hydrogen atoms of the acid anhydride of the compound having a carboxyl group, such as dimethylmaleic anhydride, diethylmaleic anhydride, and diphenylmaleic anhydride, are substituted with a substituent (e.g., an alkyl group, a phenyl group, etc.). Among the compounds having a group derived from the above carboxylic acid, maleic anhydride, succinic anhydride, and phthalic anhydride are preferred because they are easily applied industrially and easily gasified, but are not particularly limited. In addition, the cellulose nanofibers may be modified in a form in which the modifying compound is physically adsorbed to the cellulose nanofibers without being chemically bonded. Examples of the physically adsorbing compound include surfactants, and any of anionic, cationic, and nonionic surfactants may be used.If the above-mentioned modifications are carried out before defibrating and / or pulverizing the cellulose, these functional groups can be eliminated after defibrating and / or pulverizing, and the original hydroxyl groups can be restored. By carrying out the above-mentioned modifications, it is possible to promote the defibration of the cellulose nanofibers and to make the cellulose nanofibers easier to mix with various substances when they are used.
[0038] The fibers listed above may be used alone or in combination. Among them, it is preferable to use wood pulp or a combination of wood pulp and non-wood pulp and / or synthetic fibers, and more preferable to use only wood pulp.
[0039] In a preferred embodiment, the fibers constituting the composite fiber of the present invention are pulp fibers. For example, fibrous materials recovered from wastewater from paper mills may be used in the present invention. By supplying such materials to a reaction tank, various composite particles can be synthesized, and fibrous particles can be synthesized in terms of shape.
[0040] The fiber length of the composite fiber is not particularly limited, but may be, for example, an average fiber length of about 0.1 μm to 15 mm, or may be 10 μm to 12 mm, 50 μm to 10 mm, or 200 μm to 8 mm. Among these, in the present invention, an average fiber length of more than 50 μm is preferable because dehydration and sheeting are easy. An average fiber length of more than 1 mm is even more preferable because dehydration and sheeting can be performed using a wire (filter) mesh for dehydration and / or papermaking used in a normal papermaking process.
[0041] The fiber diameter of the composite fiber is not particularly limited, but may be, for example, an average fiber diameter of about 1 nm to 100 μm, and may be 10 nm to 100 μm, 0.15 μm to 100 μm, 1 μm to 90 μm, 3 to 50 μm, 5 to 30 μm, etc. Among these, in the present invention, an average fiber diameter of more than 500 nm is preferable because it is easy to dehydrate and form into a sheet. An average fiber diameter of more than 20 μm is even more preferable because it is possible to dehydrate and form into a sheet using a dehydration method or a wire (filter) mesh for papermaking used in a normal papermaking process.
[0042] Products containing composite fibers Using the composite fiber according to the present invention, it is also possible to manufacture products such as molded articles (bodies) as appropriate. For example, when the composite fiber obtained by the present invention is made into a sheet, a sheet with a high ash content can be easily obtained. Examples of papermaking machines (papermaking machines) used for sheet production include Fourdrinier papermaking machines, cylinder papermaking machines, gap formers, hybrid formers, multi-layer papermaking machines, and known papermaking machines combining the papermaking methods of these machines. The press line pressure in the papermaking machine and the calendar line pressure in the case of performing a calendar treatment in the subsequent stage can both be determined within a range that does not impair the operability or the performance of the composite fiber sheet. In addition, starch, various polymers, pigments, and mixtures thereof may be imparted to the formed sheet by impregnation or coating.
[0043] The copper content is preferably 0.1 to 7.0% in products containing composite fibers, but the copper content can also be 0.1 to 6.9%, 0.15 to 6.8%, or 0.2 to 6.7%. The copper content is measured by fluorescent X-ray analysis. If the copper content is less than 0.2%, the deodorizing performance will be below the standard value set by SEK, the antibacterial activity value of JIS L 1902:2015 will be 2.0 or less, and the antiviral activity value (Mv) of JIS L 1922:2016 will be 2.0 or less. If the copper content is more than 7.0%, the control test of JIS L 1922:2016 will be unsuccessful, and the antiviral test will be unsuccessful.
[0044] The zinc content is preferably 0.1-5.0% in products containing composite fibers, but the zinc content can also be 0.1-4.8%, 0.2-4.7%, or 0.5-4.5%. The zinc content is measured by X-ray fluorescence analysis. If the zinc content is less than 0.5%, a hydrotalcite-like compound having a layered structure cannot be obtained, and the adsorption performance decreases. If the zinc content is more than 4.5%, the copper content in the hydrotalcite-like compound becomes 2.5% or less, and the deodorizing, antibacterial, antiviral, and antiallergen performance decreases.
[0045] The product according to the present invention is suitable as a product that requires deodorizing, antibacterial, antiviral, and antiallergen effects. An allergen is a substance that can be a cause of allergies, such as an antigen that reacts specifically with the antibodies of a person with an allergic disease. Representative allergens include pollen (such as cedar and cypress) that causes hay fever, and mites and indoor dust (house dust) that cause perennial allergic rhinitis, bronchial asthma, and atopic dermatitis.
[0046] When forming the sheet, a wet and / or dry strength agent (paper strength enhancer) can be added. This can improve the strength of the composite fiber sheet. Examples of strength agents include urea formaldehyde resin, melamine formaldehyde resin, polyamide, polyamine, epichlorohydrin resin, vegetable gum, latex, polyethyleneimine, glyoxal, gum, mannogalactan polyethyleneimine, polyacrylamide resin, polyvinylamine, polyvinyl alcohol, and other resins; composite polymers or copolymers consisting of two or more types selected from the above resins; starch and modified starch; carboxymethylcellulose, guar gum, urea resin, and the like. The amount of strength agent added is not particularly limited.
[0047] In addition, polymers and inorganic substances can be added to promote the fixation of the filler to the fibers and to improve the retention of the filler and the fibers. For example, as the coagulant, polyethyleneimine and modified polyethyleneimine containing tertiary and / or quaternary ammonium groups, polyalkyleneimine, dicyandiamide polymer, polyamine, polyamine / epichlorohydrin polymer, as well as cationic polymers such as dialkyldiallyl quaternary ammonium monomer, dialkylaminoalkyl acrylate, dialkylaminoalkyl methacrylate, dialkylaminoalkyl acrylamide and polymer of dialkylaminoalkyl methacrylamide and acrylamide, polymers of monoamines and epihalohydrin, polyvinylamine and polymers having vinylamine moieties, and mixtures thereof, can be used. In addition, cationic rich amphoteric polymers in which anionic groups such as carboxyl groups and sulfonic groups are copolymerized in the molecule of the polymer, mixtures of cationic polymers and anionic or amphoteric polymers can be used. In addition, as the retention agent, cationic or anionic, amphoteric polyacrylamide-based substances can be used. In addition, a so-called dual polymer retention system, which uses at least one cationic or anionic polymer in combination, may be applied, or a multi-component retention system may be used in combination with at least one inorganic fine particle such as anionic bentonite, colloidal silica, polysilicic acid, polysilicic acid or polysilicate microgel, and aluminum-modified products thereof, or organic fine particles with a particle size of 100 μm or less, called micropolymers, in which acrylamide is cross-linked and polymerized. In particular, when the polyacrylamide-based substance used alone or in combination has a weight average molecular weight of 2 million Daltons or more as measured by the intrinsic viscosity method, a good retention rate can be obtained, and when the acrylamide-based substance has a weight average molecular weight of 5 million Daltons or more, and more preferably 10 million Daltons or more but less than 30 million Daltons, a very high retention rate can be obtained. The form of this polyacrylamide-based substance may be an emulsion type or a solution type.The specific composition is not particularly limited as long as the substance contains an acrylamide monomer unit as a structural unit, and examples thereof include a copolymer of a quaternary ammonium salt of an acrylic acid ester and acrylamide, or an ammonium salt obtained by copolymerizing acrylamide and an acrylic acid ester and then quaternizing the copolymer. The cationic charge density of the cationic polyacrylamide-based substance is not particularly limited.
[0048] In addition, depending on the purpose, examples of additives include drainage improvers, internal sizing agents, pH adjusters, defoamers, pitch control agents, slime control agents, bulking agents, calcium carbonate, kaolin, talc, silica and other inorganic particles (so-called fillers), etc. The amount of each additive used is not particularly limited.
[0049] It is also possible to use molding methods other than sheeting. For example, molded products with various shapes can be obtained by pouring the raw material into a mold, which is called pulp molding, and then suction dehydrating and drying it, or by spreading it on the surface of a molded product such as resin or metal, drying it, and then peeling it off from the base material. It can also be molded like a plastic by mixing it with resin, or molded like a ceramic by adding minerals such as silica or alumina and firing it. In the blending, drying, and molding described above, only one type of composite fiber can be used, or two or more types of composite fibers can be mixed and used. When using two or more types of composite fibers, they can be mixed in advance, or they can be blended, dried, molded, and then mixed later.
[0050] When a molded product (body) is produced using the composite fiber according to the present invention, various organic substances such as polymers, various inorganic substances such as pigments, and various fibers such as pulp fibers may be added. Also, various organic substances such as polymers, various inorganic substances such as pigments, and various fibers such as pulp fibers may be added later to a molded product of the composite fiber.
[0051] The composite fiber obtained by the present invention can be used for various applications, such as paper, nonwoven fabric, fiber, cellulose composite material, filter material, paint, plastic and other resins, rubber, elastomer, ceramic, glass, tire, building material (asphalt, asbestos, cement, board, concrete, brick, tile, plywood, fiberboard, etc.), various carriers (catalyst carrier, pharmaceutical carrier, agricultural chemical carrier, microorganism carrier, etc.), adsorbent (impurity removal, deodorization, dehumidification, etc.), wrinkle prevention agent, clay, abrasive, modifier, repair material, heat insulation material. It can be widely used in a wide range of applications, including moisture-proofing materials, water-repellent materials, water-resistant materials, light-shielding materials, sealants, shielding materials, insect repellents, adhesives, inks, cosmetics, medical materials, paste materials, food additives, tablet excipients, dispersants, shape-retaining agents, water-retaining agents, filtration aids, oil refining materials, oil treatment agents, oil modifiers, radio wave absorbing materials, insulating materials, sound-proofing materials, vibration-proofing materials, semiconductor encapsulating materials, radiation shielding materials, cosmetics, fertilizers, feed, fragrances, additives for paints, adhesives, and resins, discoloration prevention agents, conductive materials, heat transfer materials, and sanitary products (disposable diapers, sanitary napkins, incontinence pads, breast pads). It can also be used as various fillers and coating agents in the above applications. Among these, adsorbents (for removing impurities, deodorizing, dehumidifying, etc.), hygiene products (masks, wiper sheets, nursing sheets, disposable diapers, sanitary napkins, incontinence pads, breast pads, pet toilets), filters, paper, cardboard, nonwoven fabrics, and packaging materials are preferred.
[0052] The composite fiber of the present invention may be applied to papermaking applications, such as printing paper, newspaper, inkjet paper, PPC paper, kraft paper, fine paper, coated paper, lightly coated paper, wrapping paper, tissue paper, colored fine paper, cast coated paper, non-carbon paper, label paper, thermal paper, various fancy papers, water-soluble paper, release paper, processing paper, wallpaper base paper, non-flammable paper, flame-retardant paper, laminated board base paper, printed electronics paper, battery separator, cushion paper, tracing paper, impregnated paper, ODP paper, building material paper, decorative paper, envelope paper, tape paper, heat exchange paper, synthetic fiber paper, sterilized paper, waterproof paper, oil-resistant paper, heat-resistant paper, photocatalytic paper, decorative paper (such as grease removal paper), various sanitary papers (toilet paper, tissue paper, wipers, diapers, sanitary products, etc.), tobacco paper, paperboard (liner, core base paper, white paperboard, etc.), paper plate base paper, cup base paper, baking paper, abrasive paper, synthetic paper, etc. EXAMPLES
[0053] The present invention will be described in more detail below with reference to specific experimental examples, but the present invention is not limited to the following experimental examples. In addition, unless otherwise specified in this specification, concentrations, parts, etc. are based on weight, and numerical ranges are described as including their endpoints.
[0054] 1. Sample Preparation for Experiment To synthesize copper-zinc-based or magnesium-based hydrotalcite compounds (HT), the aqueous solutions shown in Table 1 were prepared. The chemicals used were NaOH (Fujifilm Wako Pure Chemicals), Na2CO3 (Fujifilm Wako Pure Chemicals), Al2(SO4)3 (Fujifilm Wako Pure Chemicals), CuSO4·5H2O (Fujifilm Wako Pure Chemicals), ZnSO4·7H2O (Fujifilm Wako Pure Chemicals), and MgSO4·7H2O (Fujifilm Wako Pure Chemicals).
[0055] [Table 1]
[0056] 1-1. Sample 1 (Example) Copper-zinc hydrotalcite compound (Cu2Zn4Al2(OH) 16 We produced a sheet that combined a composite fiber of cellulose acetate (CO3·4H2O) and pulp fiber with synthetic fiber.
[0057] Cellulose fibers were used as the composite fiber. Specifically, pulp fibers were used that were made from bleached softwood kraft pulp (NBKP, Nippon Paper Industries Co., Ltd.) and had their Canadian standard freeness adjusted to 600 ml using a single disc refiner (SDR).
[0058] Cellulose fibers were added to an alkaline solution (solution A) to prepare an aqueous suspension containing cellulose fibers (pulp fiber concentration: 2.5%, pH: 12.5). This aqueous suspension (pulp solid content 100 g) was placed in a 10 L reaction vessel, and while stirring the aqueous suspension, solution B (a mixed acid solution of three types of reagents) was dropped as an acid solution to synthesize composite fibers of hydrotalcite microparticles and fibers. Using an apparatus such as that shown in Figure 1, the reaction temperature was 50°C, the dropping speed was 5 to 15 ml / min, and the dropping was stopped when the pH of the reaction solution reached about 7. After the dropping was completed, the reaction solution was stirred for 30 minutes, and the solution was washed with 10 times the amount of water to remove salt, to obtain composite fibers.
[0059] Then, an aqueous suspension containing 60% by weight of composite fiber and 40% by weight of PET fiber (Teijin Frontier, Ecopet) cut to a fiber length of 5 mm was prepared, and the suspension was spun using an 80-mesh wire in accordance with JIS P 8222:1998 to a basis weight of 30 g / m 2 Hand-made sheets were produced.
[0060] 1-2. Sample 2 (Example, FIG. 2) A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as Sample 1, except that solution C (a mixed acid solution of three types of reagents) was used as the acid solution, and a sheet was produced by blending this composite fiber with chemical fibers.
[0061] 1-3. Sample 3 (Example) Copper-zinc hydrotalcite compound (Cu4Zn2Al2(OH) 16A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as sample 1, except that solution D (a mixed acid solution of three types of reagents) was used as the acid solution, and a sheet was manufactured that combined this composite fiber with chemical fibers.
[0062] 1-4. Sample 4 (Example, FIG. 3) A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as Sample 1, except that solution E (a mixed acid solution of three types of reagents) was used as the acid solution, and a sheet was produced by blending this composite fiber with chemical fibers.
[0063] 1-5. Sample 5 (Example) A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as Sample 4, except that 48% by weight of composite fiber and 52% by weight of PET fiber were used when producing the handsheet, and a sheet was produced by blending this composite fiber with chemical fibers.
[0064] 1-6. Sample 6 (Example) A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as Sample 4, except that 40% by weight of composite fiber and 60% by weight of bleached hardwood kraft pulp (LBKP, Nippon Paper Industries, adjusted to a Canadian standard freeness of 300 ml using SDR) were used in the production of the hand-made sheet. 2 The resulting hand-made sheets were
[0065] 1-7. Sample 7 (Example) A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as in Sample 4. Then, an aqueous suspension containing 60% by weight of the composite fiber and 40% by weight of NBKP (Canadian Standard Freeness was adjusted to 600 ml using SDR) was prepared. The aqueous suspension was then poured into a Büchner funnel in which a filter paper (Advantec, standard filter paper No. 5B, diameter 90 mm) was set. After leaving it to stand for 10 seconds, the wet paper obtained by suction filtration was dried to a basis weight of 500 g / m 2A pulp mold (thickness: approximately 1.5 mm) was produced.
[0066] 1-8. Sample 8 (Example) A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as in Sample 4. Then, 40% by weight of the composite fiber and 60% by weight of LBKP (moisture content: about 70%) were put into a Plosser Mixer (WB type, Pacific Machinery Works, Ltd.) and stirred at room temperature. Next, steam was put into the Plosser Mixer to raise the temperature inside the device to 80°C or higher, and the mixture was dried while stirring. After drying until the moisture content reached about 10%, the mixture was granulated while adding water (finished particle size after granulation: about 0.5 mm, moisture content after granulation: about 50%). Finally, granules with a particle size of 0.5 mm or less were produced using a sieve with a mesh size of 0.5 mm or less.
[0067] 1-9. Sample 9 (Comparative Example) Made entirely from polyester fibre, with a basis weight of 30g / m 2 That is, an aqueous suspension containing PET fibers (Teijin Frontier, Ecopet) cut to a fiber length of 5 mm was prepared, and a hand-made sheet with a basis weight of 30 g / m was produced using an 80-mesh wire in accordance with JIS P 8222:1998. 2 The resulting hand-made sheets were
[0068] 1-10. Sample 10 (Comparative Example) A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as sample 1, except that F solution (a mixed acid solution of three types of reagents) was used as the acid solution, and a sheet was produced by blending this composite fiber with chemical fibers.
[0069] 1-11. Sample 11 (Comparative Example) A composite fiber of hydrotalcite microparticles and fibers was synthesized in the same manner as sample 1, except that solution G (a mixed acid solution of three types of reagents) was used as the acid solution, and a sheet was produced by blending this composite fiber with chemical fibers.
[0070] 1-12. Sample 12 (Comparative Example) Magnesium hydrotalcite compound (Mg6Al2(OH) 16 They synthesized composite fibers from cellulose acetate (CO3·4H2O) and pulp fibers, and produced a sheet that combined the composite fibers with chemical fibers. Specifically, a composite fiber of hydrotalcite fine particles and fibers was synthesized and a sheet was produced in the same manner as in Sample 1, except that an H solution (a mixed acid solution of two types of reagents) was used as the acid solution.
[0071] 1-13. Sample 13 (Comparative Example) Copper-zinc hydrotalcite compound (CuMg5Al2(OH) 16 A composite fiber was synthesized from water-soluble carbon dioxide (CO3·4H2O) and pulp fiber, and a sheet was manufactured by combining the composite fiber with chemical fibers.
[0072] Specifically, a composite fiber of hydrotalcite fine particles and fibers was synthesized and a sheet was produced in the same manner as in Sample 1, except that Solution I (a mixed acid solution of three types of reagents) was used as the acid solution.
[0073] Experiment 2. Sample Evaluation 2-1. Observation using an electron microscope The composite fibers were observed using a scanning electron microscope (SEM) and it was confirmed that the particles were composited on the surface of the pulp fibers.
[0074] 2 and 3 are electron microscope photographs (500x and 10,000x) of the surfaces of the composite fibers of Sample 2 and Sample 4, respectively. The composite fibers had a coverage rate of 70-90% of the pulp fibers with fine particles (particle diameter: 100-1000 nm, average particle diameter: approximately 200 nm).
[0075] 2-2. Weight ratio of inorganic particles The weight percentage of inorganic particles was calculated based on the ash content. The ash content of the composite fiber was calculated from the ratio of the weight of the remaining ash to the original solid content after heating the composite fiber at 525°C for about 2 hours (JIS P 8251:2003). However, since the ashing process at 525°C causes a weight loss due to decarbonation of hydrotalcite and removal of interlayer water, the weight percentage of inorganic particles contained in the composite fiber was calculated based on the weight loss from the actual weight measured after the ashing process.
[0076] The weight percentage of Cu, Zn or Mg was determined by quantifying the amount of Cu, Zn or Mg contained in the ash heated at 525°C for approximately 2 hours using an energy dispersive X-ray fluorescence analyzer (EDX-7000, manufactured by Shimadzu Corporation), and calculating the weight percentage (%) of Cu, Zn or Mg contained in the composite fiber from the quantitative value and the ash content value.
[0077] 2-3. Evaluation of deodorizing properties The deodorizing properties were evaluated for the samples produced in Experiment 1. The amounts of samples used in the deodorizing test were as follows: Nonwoven fabric and paper (samples 1-6 and samples 9-13): 200 cm 2 Pulp mold and granules (samples 7-8): 1.0g The deodorization test was carried out based on the method of SEK Mark Textile Product Certification Standard (JEC301) established by the Japan Textile Evaluation Technology Council (SEK), and the odor reduction rate was calculated. Ammonia, hydrogen sulfide, methyl mercaptan, and acetic acid were quantified using the detector tube method. Isovaleric acid, indole, and nonenal were quantified using the gas chromatography method.
[0078] 2-4. Evaluation of antibacterial properties The antibacterial properties of the samples produced in Experiment 1 were evaluated. The amount of sample used in the antibacterial test was 0.4 g. The antibacterial test was performed using the bacterial liquid absorption method specified in JIS L 1902:2015, and the antibacterial activity value was calculated. The following six types of bacteria were tested. ·Staphylococcus aureus NBRC 12732 ·Escherichia coil NBRC 3301 ·Klebsiella pneumoniae NBRC 13277 ·MRSA(Staphylococcus aureus IID 1677) ·Pseudomonas aeruginosa NBRC 3080 Moraxella osloensis ATCC 19976 2-5. Evaluation of antiviral properties The antiviral properties of the samples produced in Experiment 1 were evaluated. The amount of sample used in the antiviral test was 0.4 g. The antiviral test was performed according to JIS L 1922:2016, and the antiviral activity value was calculated. The following two types of viruses were used as test viruses. Note that no results were obtained from the antiviral test for Sample 11. Influenza virus (H3N2, ATCC VR-1679) Feline calicivirus (Strain: F-9 ATCC VR-782) 2-6. Anti-allergen properties The anti-allergen properties were evaluated for the samples produced in Experiment 1. The anti-allergen properties were evaluated based on the inactivation and removal effect of cedar pollen allergen (Cry j1).
[0079] A test solution was prepared by dissolving purified Cry j1 (manufactured by Seikagaku Biobusiness Co., Ltd.) in phosphate buffered saline (PBS) containing 0.05% Tween 20 to a concentration of 100 ng / mL. At room temperature, 0.2 g of sample was placed in a 15 mL plastic tube and 1 mL of the test solution was contacted. After leaving the sample to stand for 1 hour, the test solution was extracted by squeezing with fingers and centrifuged at 10,000 x g for 3 minutes, and the allergen concentration (Cry j1 concentration) in the supernatant was measured by sandwich ELISA. As a comparative control, the test solution alone was also measured.
[0080] The allergen concentration (Cry j1 concentration) was measured by sandwich ELISA under the following conditions. n=2 (2 wells) per sample Measuring equipment: MULTISKAN FC (Thermo) ·Measurement wavelength: 405nm The inactivation removal rate (%) was calculated from the following formula: The inactivation removal rate was calculated using sample 9 as a control. "Inactivation removal rate (%)" = [1 - (amount of allergen remaining in test sample) / (amount of allergen remaining in control sample)] x 100
[0081] [Table 2]
[0082] As is clear from the table, it was found that the samples of the examples have high deodorizing, antibacterial, antiviral and antiallergenic effects. In particular, it was found that samples 2 to 8 have excellent deodorizing, antibacterial, antiviral and antiallergenic effects. Therefore, it was found that it is possible to obtain a composite fiber of hydrotalcite and fiber having high deodorizing, antibacterial, antiviral and antiallergenic effects by a single-stage treatment.
[0083] On the other hand, no deodorizing, antibacterial, antiviral or antiallergen effects could be confirmed in comparative samples 9 and 12. Sample 11 showed excellent deodorizing, antibacterial and antiallergen effects, but its ammonia deodorizing effect was below the SEK standard. Sample 13 showed excellent deodorizing effects (odor components other than ammonia), antibacterial and anti-feline calicivirus effects, but no anti-influenza virus or anti-allergen effects could be confirmed.
Claims
1. A composite fiber having hydrotalcite containing copper and zinc attached to the fiber, The above composite fiber, wherein 60% or more of the fiber surface is covered with hydrotalcite, the copper content in the hydrotalcite is 22.6 to 40% by weight, and the molar ratio of copper / zinc contained in the hydrotalcite is 3 / 3 to 5 / 1.
2. A composite fiber as described in claim 1, wherein 80% or more of the fiber surface is covered with hydrotalcite.
3. The composite fiber according to claim 1 or 2, wherein the fibers are cellulose fibers.
4. A product comprising the composite fiber according to any one of claims 1 to 3.
5. 5. The product of claim 4 in the form of a sheet, a pulp mold, or granules.
6. The product according to claim 4 or 5, wherein the product is a nonwoven fabric or paper.
7. A product according to any one of claims 4 to 6 for use in hygiene products.
8. The product according to any one of claims 4 to 7 for use in a mask or wiper, or an adsorbent.
9. The product according to any one of claims 4 to 8, which is used for deodorizing, antibacterial or antiviral purposes.
10. The product according to any one of claims 4 to 9, wherein the antibacterial activity value measured based on JIS L 1902:2015 is 2.0 or more for any one of Escherichia coli, Staphylococcus aureus, Klebsiella pneumoniae, MRSA, Pseudomonas aeruginosa, and Moraxella.
11. The product according to any one of claims 4 to 10, wherein the odor component reduction rate measured based on the deodorizing test method of the SEK Mark textile product certification standard (JEC301) is equal to or greater than the standard value specified in JEC301 for any one of ammonia, hydrogen sulfide, methyl mercaptan, acetic acid, isovaleric acid, indole, and nonenal.
12. The product according to any one of claims 4 to 11, having an antiviral activity value (Mv) against influenza virus or feline calicivirus of 2.0 or more as measured based on JIS L 1922:2016.
13. 13. The product according to claims 4 to 12, wherein the copper content is less than or equal to 7.0% by weight.
14. A product according to any one of claims 4 to 13, having a zinc content of at least 1.0% by weight.
Citation Information
Patent Citations
Carbon fiber compound nano copper cobalt alloy catalyst for low-carbon alcohol synthesis and preparation method of catalyst
CN104549283A
Deodorant and deodorizing filter and deodorizing device therewith
JP1998052478A
Deodorant and fiber product using it
JP2003047647A
Method for producing nanocrystal hydrotalcite compound
JP2009143798A
Deodorant fabric