Coating method and coating material set
By employing multiple coating materials with binders and colored aggregates, the method addresses the issue of monochromaticity in decorative coatings, achieving a visually appealing surface with blended color tones and natural shading.
Patent Information
- Application Number
- JP2020162208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-28
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-09-28
AI Technical Summary
Existing methods for forming decorative coatings on building and civil engineering structures using colored emulsion paints tend to result in monochromatic films due to mixing of different color tones, leading to a loss of aesthetic appeal.
A method involving the use of at least two types of coating materials, each comprising a binder, colored aggregate, and optionally a colored pigment, applied to form a film surface with controlled color mixing and blending effects.
This approach allows for the creation of a highly aesthetically pleasing coating surface with distinct color tones that blend naturally, enhancing visual appeal through controlled color transitions and shading.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a coating surface that can be applied to the decorative surfaces of interior and exterior walls of buildings, civil engineering structures, etc. [Background technology]
[0002] Conventionally, coatings having various patterns have been formed on the wall surfaces of buildings, civil engineering structures, etc. One example of such a coating is one in which a pattern in which different color tones are mixed is formed using a plurality of coating materials.
[0003] Patent Document 1 discloses a method of forming a patterned coating by sequentially applying two or more colored emulsion paints having different color tones and then pressing the coating while the coating is in a fluid state. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-263565 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in Patent Document 1, a colored emulsion paint containing a resin emulsion and a colored pigment as main components is used. Therefore, while two or more colored emulsion paints are in a fluid state, they tend to mix with each other, and there is a risk that the formed coating will become monochromatic.
[0006] The present invention has been made in consideration of such problems, and has an object to provide a method by which a highly aesthetic coating surface having a mixture of different color tones can be easily formed. [Means for solving the problem]
[0007] Means of the Invention As a result of extensive research into solving the above problems, the present inventors came up with the idea of using at least two specific coating materials, and thus completed the present invention.
[0008] That is, the present invention has the following features. 1. A coating method for forming a coating surface having a mixture of different color tones using at least two different color coating materials, Each of the coating materials includes a binder and a colored aggregate, The binder contains 100 to 4,000 parts by weight of colored aggregate per 100 parts by weight of solid content. At least one of the coating materials further contains a color pigment; Contains 0.001 to 150 parts by weight of color pigment for 100 parts by weight of binder solids. , For the coated surface, (1) a step of applying at least two of the above coating materials to form a coating surface; (2) A process of drying the coated surface; A coating forming method comprising the steps of: 2. The method for forming a coating according to 1., characterized in that in the step (1), water and / or a solvent is supplied to the coating surface. 3 A coating material set for forming a coating surface with a mixture of different colors, The coating set includes at least two different color coatings, Each of the at least two coating materials includes a binder and a colored aggregate, The binder contains 100 to 4,000 parts by weight of colored aggregate per 100 parts by weight of solid content. At least one of the above coating materials further contains a color pigment. The binder contains 0.001 to 150 parts by weight of color pigment per 100 parts by weight of solid content. , A coating material set comprising: Effect of the Invention
[0009] According to the present invention, it is possible to easily form a coating surface having a high aesthetic appearance and including a mixture of different color tones. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described in detail.
[0011] The present invention is a coating method for forming a coating surface having a mixture of different color tones using at least two different color coating materials.
[0012] [Coating material] In the present invention, at least two types of coating materials, i.e., a coating material set, are used. Each of these coating materials contains a binder and a colored aggregate. At least one of these coating materials contains a color pigment in addition to the binder and the colored aggregate. In the present invention, by using such at least two types of coating materials, a highly aesthetic coating surface with a mixture of different color tones can be easily formed.
[0013] The reason for this effect is not limited to the following, but when a painted surface is formed by applying multiple coating materials, multiple colored regions are produced in a mixed state based on the color development of the color aggregates and color pigments of each coating material, and near the boundaries between the coating materials, color changes are mitigated by the bleeding action of the color pigments, etc., resulting in a visually blurred state of the boundaries. In the present invention, it is believed that such visual effects result in natural changes in shading, improving the aesthetic appearance.
[0014] The binder in the coating material is a component that plays a role in fixing colored aggregates, colored pigments, etc. As the binder, a water-soluble resin and / or a water-dispersible resin (resin emulsion) is preferable. Examples of the type of resin include cellulose, polyvinyl alcohol, ethylene resin, vinyl acetate resin, polyester resin, alkyd resin, vinyl chloride resin, epoxy resin, acrylic resin, urethane resin, acrylic silicone resin, fluororesin, etc., or composites thereof. These can be used alone or in combination of two or more. In addition, these binders may be either those having crosslinking reactivity or those not having crosslinking reactivity.
[0015] The colored aggregate is a component that imparts color to the coating material. As the colored aggregate, aggregate that can be visually recognized in some color can be used. The color of the colored aggregate may be, for example, of natural origin or may be artificially imparted. In the present invention, the use of such colored aggregate makes it possible to realize the effect of juxtaposition color mixing (when viewed from a certain distance or more, multiple colors placed side by side appear to be mixed together without being individually distinguished) by coloring due to the aggregation of small dots of the colored aggregate, unlike the case where only a general color pigment is used, and to impart texture, naturalness, fineness, etc. In addition, the use of the colored aggregate can also suppress monochromatization when multiple coating materials are mixed.
[0016] Examples of colored aggregates include crushed materials of marble, granite, serpentine, granite, fluorite, kansuiite, feldspar, silica stone, silica sand, etc., crushed ceramics, crushed ceramics, crushed glass, glass beads, crushed resins, resin beads, metal particles, etc., or materials having a colored coating on the surface thereof, etc. These can be used alone or in combination of two or more types depending on the desired color.
[0017] The colored aggregate desirably has a larger average particle size than the colored pigment described below. The average particle size of the colored aggregate is preferably 0.05 mm to 3 mm, more preferably 0.06 mm to 1 mm, and even more preferably 0.07 mm to 0.5 mm. The average particle size is a value obtained by sieving the aggregate using a metal mesh sieve specified in JIS Z8801-1:2000 and calculating the average weight distribution.
[0018] The mixing ratio of the colored aggregate is preferably 100 to 4000 parts by weight, more preferably 200 to 3000 parts by weight, and further preferably 300 to 2000 parts by weight, relative to 100 parts by weight of the solid content of the binder.
[0019] At least one of the above coating materials contains a color pigment. Examples of color pigments include titanium oxide, zinc oxide, carbon black, graphite, black iron oxide, copper chrome black, cobalt black, copper manganese iron black, red iron oxide, molybdate orange, permanent red, permanent carmine, anthraquinone red, perylene red, quinacridone red, yellow iron oxide, titanium yellow, fast yellow, benzimidazolone yellow, chrome green, cobalt green, phthalocyanine green, ultramarine blue, Prussian blue, cobalt blue, phthalocyanine blue, quinacridone violet, dioxazine violet, aluminum pigment, and pearl pigment. These can be used alone or in combination of two or more. The average particle size of the color pigment is preferably 2 μm or less, more preferably 0.01 μm or more and 1 μm or less. The average particle size of the color pigment is a value measured by a laser diffraction type particle size distribution measuring device.
[0020] When the coating material contains a color pigment, the mixing ratio of the color pigment is 200 parts by weight or less, preferably 0.001 to 150 parts by weight, more preferably 0.005 to 100 parts by weight, and further preferably 0.01 to 90 parts by weight, relative to 100 parts by weight of the solid content of the binder. By mixing the color pigment at such a ratio, the color effect such as the change in shade near the boundary between the coating materials can be sufficiently improved, which is preferable in terms of improving the effects of the present invention.
[0021] The coating materials may contain components other than those mentioned above, so long as they do not significantly impair the effects of the present invention. Examples of such components include thickeners, film-forming assistants, leveling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, defoamers, adsorbents, extender pigments, fibers, water repellents, hydrophilizing agents, crosslinking agents, ultraviolet absorbers, light stabilizers, antioxidants, catalysts, etc.
[0022] Among these, examples of the extender pigment include heavy calcium carbonate, light calcium carbonate, kaolin, clay, china clay, diatomaceous earth, hydrous fine silica, talc, baryte powder, barium sulfate, precipitated barium sulfate, barium carbonate, magnesium carbonate, silica powder, aluminum hydroxide, etc., and one or more of these can be used. The average particle size of the extender pigment is preferably less than 50 μm, more preferably 0.5 μm or more and 40 μm or less. The average particle size of the extender pigment is a value measured by a laser diffraction type particle size distribution measuring device.
[0023] The coating material of the present invention can be produced by uniformly mixing the above-mentioned binder, colored aggregate, colored pigment, and, if necessary, each of the above-mentioned components, in a conventional manner.
[0024] The viscosity of the coating material is preferably 5 to 150 Pa·s, more preferably 10 to 120 Pa·s, and further preferably 20 to 100 Pa·s. By setting the coating material to such a viscosity, it is possible to prevent the formed coating from becoming monochromatic and improve the aesthetics while ensuring the coating material's coating workability. Note that the viscosity referred to here is the viscosity at 20 rpm (guideline value at the fourth rotation) measured with a BH type viscometer at a temperature of 23°C.
[0025] The coating material set of the present invention is composed of at least two coating materials of different colors. In the present invention, the color tones of the at least two coating materials need only be visually distinguishable, and the color difference (ΔE) between them is preferably 1 or more, and more preferably 2 or more. The color tone of each coating material can be appropriately set, for example, by mixing color aggregates and color pigments. When the coating material set is composed of two coating materials, it is sufficient that the color tones of the coating materials are different from each other. When the coating material set is composed of three or more coating materials, it is sufficient that at least one of the other coating materials is a different color from one reference coating material.
[0026] In the present invention, a coating surface with subtle changes in color can be formed by setting the color difference of each coating material to a relatively small value (e.g., a color difference of 1 to 10). On the other hand, a coating surface in which the color shading, etc., is clearly visible can be formed by setting the color difference of each coating material to a relatively large value (e.g., a color difference of more than 10).
[0027] In the present invention, the color difference (ΔE) is a value measured by a colorimeter for the dry coating film of each coating material (formed on a standard white paper with a dry thickness of 1 mm). * Value, a * Value, b * It can be calculated using the following formula from the value (average value of 10 or more measurement points). <Formula>△E={(L * 1-L * 2) 2 +(a * 1-a * 2) 2 +(b * 1-b * 2) 2} 0.5 (In the formula, L * 1, a * 1, b * 1 is the L of one standard coating material * , a * , b * .L * 2, a * 2, b * 2 is the L of other coating materials * , a * , b * )
[0028] The coating material set of the present invention comprises at least two coating materials that satisfy the above-mentioned conditions. At least one of these coating materials contains a color pigment. When such a coating material set comprises two coating materials, the embodiment thereof is as follows: One coating material contains color pigments, and the other coating material does not contain color pigments. Both coating materials contain color pigments. etc.
[0029] In addition, when the coating material set is composed of three or more types of coating materials, the embodiment is as follows: One coating material contains color pigments, and the other coating material does not contain color pigments. Two or more coating materials contain color pigments, and the other coating materials do not contain color pigments. Three or more coating materials all contain color pigments etc.
[0030] In the coating material set of the present invention, it is desirable that the average particle size of the colored aggregate contained in each coating material is approximately the same. The absolute value of the difference between the average particle sizes of the colored aggregate contained in each coating material is preferably 0.1 mm or less, more preferably 0.05 mm or less.
[0031] [Film formation method] In the present invention, a coating is formed using at least two different color coating materials as described above. (1) A process for applying at least two types of coating materials to form a coating surface; (2) A process of drying the coated surface; Do the following.
[0032] Examples of the surface to be coated include those constituting the interior and exterior walls of buildings, civil engineering structures, etc. Examples of the substrate constituting the surface to be coated include concrete, mortar, porcelain tile, fiber-mixed cement board, cement calcium silicate board, slag cement perlite board, cement board, ALC board, siding board, gypsum board, plywood, extrusion molding board, steel board, plastic board, etc. The surface of these substrates may be one that has been subjected to some kind of surface treatment (for example, treatment with putty, sealer, surfacer, filler, etc.), one that already has a coating film formed thereon, one that has wallpaper, etc., attached thereto, etc.
[0033] In step (1), at least two types of coating materials are applied to such a substrate to form a coated surface. In step (1), each coating material is applied to the substrate so that the coating materials are mixed on the substrate, and the coating surface is formed by spreading the coating materials. This makes it possible to form a coating surface with a mixture of different color tones. The coating amount of the coating material (total coating amount of each coating material) is preferably 0.1 to 5 kg / m. 2 , more preferably 0.2 to 4 kg / m 2 It is.
[0034] When applying each coating material to the substrate, tools such as a sprayer, roller, trowel, spatula, etc. may be used. Each coating material may be applied to the substrate so that each coating material is mixed and applied to the same substrate before drying. For example, each coating material may be applied in a scattered state, adjacent state, or overlapping state on the substrate. The shape and amount of each coating material applied to the substrate may be appropriately set according to the desired finish state, aesthetics, etc.
[0035] When spreading the coating material, for example, a roller, a trowel, a spatula, etc. can be used. When a trowel, a spatula, etc. is used when spreading the coating material, it is easier to obtain a flat coating surface by leveling the coating surface.
[0036] In step (1), water and / or a solvent can be supplied to the coating surface. For example, water can be applied to a tool such as a trowel or spatula, or a spray can be used to supply water and / or a solvent to the coating surface. This allows color effects such as natural changes in shade to be sufficiently imparted, and the aesthetic appearance can be further improved. This effect is believed to be achieved by the bleeding action of the color pigment on the coating surface before drying, which makes it easier for the boundaries between the coating materials to become visually blurred.
[0037] The type of water and / or solvent to be supplied to the coating surface may be appropriately selected depending on the coating material to be used. Examples of the solvent include alcohol-based solvents, ether-based solvents, and ester-based solvents. When an aqueous coating material is used as the coating material, water or a mixture of water and a solvent may be used. The amount and timing of supplying water and / or solvent to the coating surface may be appropriately set in consideration of the drying property, aesthetics, etc. of the coating surface.
[0038] In the step (2), the coating surface obtained by the above method is dried. The drying temperature is preferably 0° C. or higher and 40° C. or lower (room temperature), and can be heated as necessary. The drying time is preferably 2 hours or longer.
[0039] By the above method, a coating surface having different colors and excellent aesthetics can be obtained. The color tone of the coating surface formed by the present invention is based on the color tone of at least two coating materials, but partial mixing of the coating materials and bleeding of color pigments can produce color effects such as gradation and blurring, and natural changes in shade can be imparted. For example, by using white and gray coating materials, a coating surface exhibiting aesthetics such as mortar and concrete can be formed. The shape of the coating surface formed by the present invention can be flat, but various uneven patterns can also be imparted. EXAMPLES
[0040] The following examples will be given to clarify the features of the present invention, but the present invention is not limited to these examples.
[0041] (Manufacturing of coating materials) The following raw materials were used to manufacture the coating material: Binder: Acrylic resin emulsion (solid content 50% by weight, glass transition temperature 30°C) Colored aggregate A: White silica sand (average particle size 150 μm) Colored aggregate B: Gray silica sand (average particle size 150 μm) Color pigment A: Black pigment dispersion (20% by weight dispersion of carbon black (average particle size 0.05 μm)) Color pigment B: Yellow pigment dispersion (50% by weight dispersion of yellow iron oxide (average particle size 0.5 μm)) Color pigment C: Red pigment dispersion (50% by weight dispersion of red iron oxide (average particle size 0.2 μm)) Color pigment D: White pigment dispersion (60% by weight dispersion of titanium oxide (average particle size 0.3 μm)) · Extender pigment: Ground calcium carbonate (average particle size 8μm) Fiber: Pulp fiber (average fiber length 0.5 mm) Dispersant: Polycarboxylic acid dispersant Coalescence agent: Ether-based coalescence agent Thickener: Hydroxyethylcellulose 3% by weight aqueous solution Defoamer: Silicone-based defoamer
[0042] Example 1 -Production of coating material 1 Coating material 1 (white, viscosity 40 Pa s) was produced by mixing and stirring 200 parts by weight of binder, 900 parts by weight of colored aggregate A, 50 parts by weight of colored aggregate B, 200 parts by weight of extender pigment, 10 parts by weight of fiber, 100 parts by weight of water, 150 parts by weight of thickener, 3 parts by weight of dispersant, 15 parts by weight of film-forming agent, and 2 parts by weight of defoamer in a conventional manner.
[0043] -Production of coating material 2 Coating material 2 (gray, viscosity 40 Pa s) was produced by mixing and stirring 200 parts by weight of binder, 50 parts by weight of colored aggregate A, 900 parts by weight of colored aggregate B, 0.5 parts by weight of colored pigment A, 200 parts by weight of extender pigment, 10 parts by weight of fiber, 100 parts by weight of water, 150 parts by weight of thickener, 3 parts by weight of dispersant, 15 parts by weight of film-forming aid, and 2 parts by weight of defoamer in a conventional manner.
[0044] As a result, a coating material set consisting of coating material 1 and coating material 2 was obtained. The color difference between coating material 1 and coating material 2 was 14.
[0045] A slate board that had been previously coated with a white sealer was prepared as the coating surface. Coating material 1 and coating material 2 were applied to this coating surface with a trowel so that they were interspersed or adjacent to each other, and then immediately spread and smoothed with the trowel to form a coating surface (coating amount of coating material 1: 0.5 kg / m2). 2 , coating amount of coating material 2 is 0.5 kg / m 2 ) Next, water was sprayed onto the surface of the coating, the surface was smoothed again with a trowel, and then it was left to dry for 24 hours. This method resulted in the formation of a mortar-like coating surface with a mixture of white and gray areas, and visible changes in shade due to the intermediate color tones between these two.
[0046] Example 2 -Production of coating material 3 Coating material 3 (light gray, viscosity 38 Pa s) was produced by mixing and stirring 200 parts by weight of binder in a conventional manner with 950 parts by weight of colored aggregate A, 0.2 parts by weight of colored pigment A, 0.2 parts by weight of colored pigment B, 0.1 parts by weight of colored pigment C, 70 parts by weight of colored pigment D, 200 parts by weight of extender pigment, 10 parts by weight of fiber, 40 parts by weight of water, 160 parts by weight of thickener, 3 parts by weight of dispersant, 15 parts by weight of film-forming aid, and 2 parts by weight of defoamer.
[0047] -Production of coating material 4 Coating material 4 (dark gray, viscosity 37 Pa s) was produced by mixing and stirring 200 parts by weight of binder in a conventional manner with 950 parts by weight of colored aggregate A, 20 parts by weight of colored pigment A, 20 parts by weight of colored pigment B, 12 parts by weight of colored pigment C, 35 parts by weight of colored pigment D, 200 parts by weight of extender pigment, 10 parts by weight of fiber, 20 parts by weight of water, 160 parts by weight of thickener, 3 parts by weight of dispersant, 15 parts by weight of film-forming aid, and 2 parts by weight of defoamer.
[0048] As a result, a coating material set consisting of coating material 3 and coating material 4 was obtained. The color difference between coating material 3 and coating material 4 was 16.
[0049] On the same substrate as in Example 1, coating material 3 and coating material 4 were applied with a trowel so that they were adjacent to each other and partially overlapped, and then immediately spread and smoothed with a trowel to form a coated surface (coating amount of coating material 3: 0.5 kg / m2).2 , coating amount of coating material 4 is 0.5 kg / m 2 ) and then dried for 24 hours. Through the above method, a mortar-like coating surface was formed, with a mixture of light gray and dark gray areas, and visible changes in shade due to intermediate colors between these two.
[0050] Example 3 -Production of coating material 5 Coating material 5 (pale orange, viscosity 40 Pa s) was produced by mixing and stirring 200 parts by weight of binder, 950 parts by weight of colored aggregate A, 1.5 parts by weight of colored pigment B, 2 parts by weight of colored pigment C, 70 parts by weight of colored pigment D, 200 parts by weight of extender pigment, 10 parts by weight of fiber, 20 parts by weight of water, 160 parts by weight of thickener, 3 parts by weight of dispersant, 15 parts by weight of film-forming aid, and 2 parts by weight of defoamer in a conventional manner.
[0051] -Production of coating material 6 Coating material 6 (dark orange, viscosity 41 Pa s) was produced by mixing and stirring 200 parts by weight of binder in a conventional manner with 950 parts by weight of colored aggregate A, 1 part by weight of colored pigment A, 40 parts by weight of colored pigment B, 60 parts by weight of colored pigment C, 35 parts by weight of colored pigment D, 200 parts by weight of extender pigment, 10 parts by weight of fiber, 160 parts by weight of thickener, 3 parts by weight of dispersant, 15 parts by weight of film-forming aid, and 2 parts by weight of defoamer.
[0052] As a result, a coating material set consisting of coating material 5 and coating material 6 was obtained. The color difference between coating material 5 and coating material 6 was 20.
[0053] On the same substrate as in Example 1, coating material 5 and coating material 6 were applied with a trowel so that they were adjacent to each other and partially overlapped, and then immediately spread and smoothed with a trowel to form a coated surface (coating amount of coating material 5: 0.5 kg / m 2 , coating amount of coating material 6 is 0.5 kg / m 2 ) and then dried for 24 hours. Through the above process, an orange coating surface was formed in which light orange and dark orange areas were mixed, and in which intermediate tones of these colors were visible.
Claims
1. A coating method for forming a coating surface having a mixture of different color tones using at least two different color coating materials, comprising the steps of: Each of the coating materials contains a binder and a colored aggregate, and contains 100 to 4000 parts by weight of the colored aggregate per 100 parts by weight of the solid content of the binder; At least one of the coating materials further contains a color pigment, and contains 0.001 to 150 parts by weight of the color pigment per 100 parts by weight of the solid content of the binder; For the coated surface, (1) a step of applying the at least two types of coating materials to form a coating surface; (2) A step of drying the coated surface; A coating forming method comprising the steps of:
2. 2. The method for forming a coating film according to claim 1, wherein water and / or a solvent is supplied to the coating surface in the step (1).
3. A coating material set for forming a coating surface having a mixture of different color tones, The coating set includes at least two different color coatings, Each of the at least two coating materials contains a binder and a colored aggregate, and contains 100 to 4000 parts by weight of the colored aggregate per 100 parts by weight of the solid content of the binder; At least one of the coating materials further contains a color pigment, and contains 0.001 to 150 parts by weight of the color pigment per 100 parts by weight of the solid content of the binder. A coating material set comprising:
Citation Information
Patent Citations
Method for forming coating layer like natural stone
JP1992202264A
Stone-patterned decorative panel
JP1998238072A
Decorative material for surface finishing of building or structure and manufacture thereof
JP2001003544A
Method for forming pattern coating film
JP2002263565A
Method of forming decorative face
JP2004249268A