Spot welding method
A two-step energization process for spot welding steel and aluminum alloy plates stabilizes the welding by melting steel first and then transferring heat to melt aluminum, addressing spatter and thickness issues, achieving strong joints.
Patent Information
- Application Number
- JP2020171405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-09
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-10-09
AI Technical Summary
Existing spot welding methods for joining steel and aluminum alloy plates face issues such as spatter, electrode welding, thickness reduction, and joint strength degradation due to direct resistance heating of aluminum alloy plates, leading to unstable welds.
A two-step energization process is employed, where the first step melts the steel plates without melting the aluminum alloy, followed by a second step that heats and melts the aluminum alloy through heat transfer from the steel plates, using controlled current values to stabilize the welding process.
This method suppresses spatter and thickness reduction, ensuring stable joint strength by forming intermetallic compounds, resulting in a welded product with desired strength.
Smart Images

Figure 0007590849000001 
Figure 0007590849000002 
Figure 0007590849000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a spot welding method and the like. [Background technology]
[0002] Car bodies, aircraft bodies, and the like are manufactured by joining multiple plate materials (joined materials) at multiple points by spot welding. Spot welding is a type of resistance welding that utilizes Joule heating, and is performed by passing a large current for a short period of time from an electrode that is pressed against the outer surfaces of overlapping plate materials. Generally, this current flow forms a molten pool near the contact interface (joined portion) between the overlapping plate materials (usually steel plates), which then cools and solidifies to become a weld (nugget). In this way, multiple steel plates are joined at multiple points by spot-shaped nuggets to form a structure (welded object).
[0003] Incidentally, not only spot welding between steel plates, but also spot joining between lightweight aluminum alloy plates and steel plates (these are also simply referred to as "spot welding"). Proposals regarding such spot welding are made, for example, in the following patent documents. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2006-289452 [Patent Document 2] Patent Publication No. 2008-105087 [Patent Document 3] Patent Publication No. 2013-78804 [Patent Document 4] Patent Publication No. 2013-27890 Summary of the Invention [Problem to be solved by the invention]
[0005] In Patent Documents 1 to 3, a plate assembly consisting of two overlapping plate materials, one steel plate and one aluminum alloy plate, is spot welded. In all of these patent documents, a large current (15 to 30 kA) is applied in one welding process, which is large enough to melt the aluminum alloy plate, which has a low specific resistance, by resistance heating alone.
[0006] In Patent Document 4, a pre-pressurizing process, a pre-heating process, a cooling process, and a welding process are carried out in that order, and a sheet assembly in which three sheets of plate material, a non-plated steel sheet, a zinc-plated steel sheet, and an aluminum alloy sheet, are stacked in that order, is spot-welded (
[0036] to
[0054] , Table 1, Figure 6, etc.).
[0007] The preheating process is performed with a current value of 2 kA within a range in which the plates do not melt (
[0041] ). In the subsequent welding process, a large current (12.5 to 15 kA) is passed all at once (
[0057] ,
[0067] , Figures 7 and 8). The electrode used in Patent Document 4 has a cylindrical portion (D2): φ16 mm (nominal diameter), a spherical portion (R) of the shoulder: 5 mm (radius of curvature), and a tip portion (D1): φ6 mm (
[0039] ). The tip portion (tip area: π×6×6 / 4 ≒ 28.3 mm 2 The current density through the 2 (Figure 3) The tip area is the projected area (circular area) of the tip.
[0008] In Patent Document 4, a current of a large density is passed through which the aluminum alloy sheet can be melted by resistance heating alone. In this single welding process, the vicinity of the contact interface between the non-plated steel sheet and the plated steel sheet and the vicinity of the contact interface between the plated steel sheet and the aluminum alloy sheet are melted simultaneously, and these are joined at the same time (
[0044] to
[0048] ).
[0009] According to the inventor's research, when a large current is applied so that the aluminum alloy plate is directly melted only by resistance heating as in Patent Document 4, dust (explosions, spatters) are generated between the steel plates or between the aluminum alloy plate and the steel plate, and adhesion is easily caused between the aluminum alloy plate and the electrode. In addition, when a large current is applied so that an aluminum alloy plate with a high conductivity (electrical conductivity, electrical conductivity) is melted only by resistance heating, the aluminum alloy plate is suddenly softened as a whole, and a large depression (depression) is formed on the electrode side where the plate is pressed. The remaining thickness (plate thickness other than the welded part) of such an aluminum alloy plate after welding is too small, and the plate is easily destroyed starting from the welding spot (especially the aluminum alloy plate part), making it difficult to ensure the joint strength of the welded product.
[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide a new method etc. by which spot welding of steel plates and aluminum alloy plates can be stably and appropriately performed. [Means for solving the problem]
[0011] As a result of intensive research to solve this problem, the inventor came up with the idea of performing at least two stages of current application process when spot joining two steel sheets and an aluminum alloy sheet. In the first current application process, only the space between the steel sheets is melted without melting the aluminum alloy sheet. In the second current application process, the aluminum alloy sheet is melted by current application within a range where the aluminum alloy sheet does not melt by resistance heating alone, utilizing heat transfer from the steel sheet side. In this way, it was newly discovered that spot welding, which is a joining of dissimilar metals, can also be performed stably. By developing this result, the present invention described below has been completed.
[0012] <Spot welding method> The present invention is a spot welding method for joining a plurality of stacked plate materials by resistance heating by passing a current through a pair of opposing electrodes pressed against both outer surfaces of the plate set, the plate set being composed of at least a first steel plate, a second steel plate, and an aluminum alloy plate stacked in that order, the spot welding method comprising a first current passing step for generating a molten pool between opposed surfaces of the first steel plate and the second steel plate without melting the aluminum alloy plate, and a second current passing step for generating a melting reaction between opposed surfaces of the second steel plate and the aluminum alloy plate after the first current passing step, the first steel plate and the second steel plate being joined via a first nugget, and the second steel plate and the aluminum alloy plate being joined via a second nugget containing an intermetallic compound produced by the melting reaction.
[0013] According to the present invention, a spot welding method (also simply referred to as a "welding method" or "joining method") for steel sheets and aluminum alloy sheets can be stably performed while suppressing the generation of spatter (dust) between sheets, adhesion between the sheets and electrodes, reduction in thickness or depression of the sheets, etc.
[0014] The reason why such an excellent effect is obtained is considered to be as follows: In the first current application step, a current in a range that does not substantially melt the aluminum alloy plate is applied, and melting occurs mainly between the first steel plate and the second steel plate. Since this first current application step is performed with a suppressed current value, spatter is unlikely to occur not only between the second steel plate and the aluminum alloy plate, but also between the first steel plate and the second steel plate.
[0015] In the second current application process, not only the aluminum alloy plate is resistance heated, but also the molten pool or its solidified portion already formed between the first and second steel plates is resistance heated. Therefore, the aluminum alloy plate is heated and melted by its own resistance heating and heat transfer from the second steel plate (see Figure 7). Therefore, even an aluminum alloy plate with a high electrical conductivity can be melted by applying current with a suppressed current value, and the generation of spatter between the plates is suppressed in the second current application process.
[0016] Furthermore, in the second current flow process, it is possible to pass current at a lower value than before, which prevents overheating of the aluminum alloy sheet itself, and thus avoids excessive softening, deformation (such as depressions caused by the electrode), and reduction in remaining thickness of the aluminum alloy sheet. In this way, even when spot welding dissimilar metal sheets, a weldment with the desired strength is obtained. During the second current flow process, the molten pool or solidified part already formed between the first and second steel sheets is also heated and grows and increases. This can further improve the joint strength of the weldment. The molten pool or solidified part formed in the first current flow process becomes the "first nugget" after the second current flow process.
[0017] <Spot welded object, spot welding control device or control program> The present invention can also be understood as a spot welded product obtained by the above-mentioned method. The present invention can also be understood as a spot welding control device or a control program thereof that at least controls the supply of current to the above-mentioned electrode.
[0018] In addition, in the components of the control device and the control program, for example, the component "step" of the above-mentioned method can be interpreted as "means" or "part." Furthermore, the "step" can be interpreted as "step," and the present invention can be understood as a control method for executing a control program by a computer.
[0019] "others" (1) The first current value passed in the first current passing step and the second current value passed in the second current passing step are adjusted within a predetermined range according to the workpieces (composition, thickness, surface condition, etc. of each plate material), other welding conditions (electrode specifications, pressure, current passing time, etc.), and the required strength of the welded workpiece. However, the second current value (average value) is usually larger than the first current value (average value). In addition, the second current value is preferably smaller than the melting current value that can melt the aluminum alloy plate by resistance heating alone.
[0020] (2) For ease of explanation, the term "first" will be attached to the term relating to the first current flow process or on the first steel plate side, and the term "second" will be attached to the term relating to the second current flow process or on the aluminum alloy plate side, as appropriate.
[0021] (3) Unless otherwise specified, "x to y" in this specification includes a lower limit value x and an upper limit value y. Any numerical value included in the various numerical values or numerical ranges described in this specification may be used as a new lower limit or upper limit value to create a new range such as "a to b". Furthermore, unless otherwise specified, "x to ykA" in this specification means xkA to ykA. Other unit systems (A / mm 2 The same applies to (etc.). [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a schematic diagram showing an overview of spot welding. [Diagram 2] 4 is an example of a time chart relating to spot welding. [Figure 3A] 1 is a photomicrograph showing a cross section of a spot-welded plate assembly (weld). [Figure 3B] 1 is a photomicrograph showing a cross section in the vicinity of a bonding interface between an aluminum alloy plate and a second steel plate. [Figure 4] 1 is a schematic diagram of an evaluation test of bonding strength and a data table showing evaluation examples. [Diagram 5] 10 is a graph showing an example of the relationship between a second current value in a second current passing step and a second nugget diameter or a sheet thickness reduction rate of an aluminum alloy sheet. [Figure 6] 13 is a list of photographs summarizing the influence of the second current value or the tip diameter of the electrode on the welding of the aluminum alloy plate and the electrode. [Figure 7] 1 is a schematic diagram showing a progress process of spot welding. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] One or more components selected arbitrarily from this specification may be added to the above-mentioned components of the present invention. The contents described in this specification may also be applied to a control device, a control program, etc., as well as a welding method or a resultant product (such as a welded product). Which embodiment is best depends on the target, the required performance, etc.
[0024] 《Plate materials / board assembly》 A plate assembly in which at least two steel plates (a first steel plate and a second steel plate) and an aluminum alloy plate (simply referred to as an "Al alloy plate") are stacked is spot welded. The number of steel plates on at least one side of the Al alloy plate may be three or more. Also, there may be at least one steel plate on the other side of the Al alloy plate. There may also be multiple Al alloy plates. Each plate material may have a portion that is joined without relying on spot welding. It is also possible to join one steel plate and one Al alloy plate by the welding method of the present invention. In this case, it is preferable that the one steel plate replacing the two steel plates has a plate thickness of 1.5 times or more than that of the Al alloy plate.
[0025] The steel sheets may be of the same or different plate materials having the same composition, surface treatment state (presence or absence of plating, etc.), plate thickness, etc. Examples of the steel sheets include cold-rolled steel sheets, hot-rolled steel sheets, high-strength steel sheets, and hot-stamped steel sheets.
[0026] The steel plate may be surface-treated. For example, the second steel plate to be joined to the Al alloy plate may have a metal layer (simply referred to as a "low melting point metal layer") having a lower melting point than the Al alloy plate at least on the Al alloy plate side. The low melting point metal layer melts prior to (preferentially) the base material (Al alloy) of the Al alloy plate during the second current application step, and wets and spreads between the joined surfaces of the Al alloy plate and the second steel plate. This expands the joining area of the second nugget, improving the joining strength between the plates.
[0027] Galvanization is a typical surface treatment for steel sheets. Galvanized steel sheets include, for example, hot-dip galvanized steel sheets, electrogalvanized steel sheets, and alloyed hot-dip galvanized steel sheets. The alloyed hot-dip galvanized steel sheets may be aluminum-zinc alloy-plated steel sheets (so-called Galvalume Steel Sheet (registered trademark)). The metal layer (galvanized layer, etc.) is usually present on both sides of the steel sheet, but may be present on only one side. The first steel sheet may be surface-treated (coated steel sheet, etc.) or may not be surface-treated (non-coated steel sheet, etc.).
[0028] For the Al alloy plate, 2000 series to 8000 series, particularly 5000 series or 6000 series, are usually used. For example, for the 5000 series, Al alloy plates corresponding to A5052, A5083, A5005, etc., specified in JIS are often used. For the 6000 series, Al alloy plates corresponding to A6022, A6016, A6N01, etc., specified in JIS are often used. In addition, the Al alloy plate referred to in this specification may also include A1000 series.
[0029] The thickness of each plate material may be the same or different. The thickness of the steel plate is, for example, 0.4 to 2.5 mm, or 0.6 to 1.8 mm. The thickness of the Al alloy plate is, for example, 0.8 to 3 mm, or 1 to 2 mm.
[0030] 《First energization process》 (1) In the first current application step, a molten pool and its solidification portion are generated between the facing first steel sheet and the facing second steel sheet. When a direct current is applied, the (first) current value is, for example, 4 to 10 kA, 6 to 9.5 kA, or even 7 to 9.0 kA. The (first) current density is, for example, 10 to 200 A / mm 2 Furthermore, 25~100A / mm 2 If the current value or current density is too low, it becomes difficult to form a sufficient molten pool or solidified zone between the steel sheets, and thus to form a first nugget. If the current value or current density is too high, splashing, adhesion, and the like are likely to occur.
[0031] When the current value changes, the integral value of the current value (absolute value) with respect to the current flow time is divided by the current flow time to obtain an average value, which is adopted as the "(first) current value". The current density is calculated by dividing the current value by the tip area of the electrode. For example, if the tip of a substantially cylindrical or columnar electrode is flat or radiused, the tip area of the electrode is calculated as the circular area (area equivalent to the tip diameter: D1) projected onto the tip. The tip area of the electrode can be substituted by the area of the indentation (contact area between the plate material and the electrode) formed on the plate material after spot welding. The first current density is calculated by, for example, dividing the first current value by the tip area (first tip area) of the electrode (first electrode) on the first steel plate side. These will be described later in the second current flow process (second current value, second current density, second tip area of the second electrode). ) The same applies to.
[0032] (2) The pressure in the first current application step is, for example, 2 to 6 kN, or further 3 to 5 kN. The current application time is, for example, 25 to 200 ms, or further 50 to 150 ms. If the pressure or current application time is too small, the formation of the molten pool (solidified portion) between the steel sheets or the first nugget becomes unstable, and spattering is likely to occur in the second current application step. If the pressure is too large, deep dents (dents, depressions) may occur in the plate material (especially the Al alloy plate). If the current application time is too long, the second nugget formed in the second current application step becomes too large, and spattering is likely to occur.
[0033] Incidentally, the molten pool or solidified portion formed in the first current flow process may be large enough to become a heating source by heat transfer of the Al alloy plate in the second current flow process. Even if the molten pool or solidified portion is small at the end of the first current flow process, it can grow to become a sufficient first nugget in the second current flow process. Therefore, the (first) current flow time in the first current flow process may be shorter than the (second) current flow time in the second current flow process.
[0034] (3) A pre-current process may be performed before the first current process, in which the temperature of the sheet pair is increased to allow the contact state between the sheets to become familiar. The pre-current process may be performed by current flow that does not generate a molten pool for the sheet pair to which the electrodes are pressed. For example, the pre-current process is performed by current flowing at a pre-current value (time average value) smaller than the first current value. The pre-current value is, for example, 0.5 to 3 kA, or 1 to 2 kA.
[0035] 《Second energization process》 (1) The second current application step causes a melting reaction between the facing surfaces of the second steel sheet and the Al alloy sheet to produce a second nugget. When a direct current is applied, the (second) current value is, for example, 11 to 15 kA, 11.5 to 14.5 kA, or even 12 to 14 kA. The second current value is usually set to be larger than the first current value (for example, 2 to 6 kA, or even 3 to 5 kA larger). The (second) current density is, for example, 50 to 300 A / mm 2 Furthermore, 100~250A / mm 2 If the current value or current density is too small, melting of the Al alloy plate and generation of the second nugget between the second steel plate and the Al alloy plate are insufficient. If the current value or current density is too large, sputtering from between the plates and welding between the plates and the electrode are likely to occur. As described above, the second current density is calculated, for example, by dividing the second current value by the tip area (second tip area) of the electrode (second electrode) on the Al alloy plate side.
[0036] (2) The pressure in the second current application step is, for example, 2 to 6 kN, or further 3 to 5 kN. The current application time is, for example, 50 to 500 ms, or further 150 to 400 ms. If the pressure is too small, dust is likely to be generated between the Al alloy sheet and the second steel sheet. If the pressure is too large, deep dents (depressions) are likely to be formed in the Al alloy sheet. If the current application time is too short, melting of the Al alloy sheet and formation of the second nugget between the Al alloy sheet and the second steel sheet are insufficient. If the current application time is too long, adhesion or wear of the electrodes (especially on the Al alloy sheet side) is likely to occur, and productivity may also decrease.
[0037] (3) After the first current-passing step and before the second current-passing step, a cooling step may be performed to lower the temperature of the sheet assembly. The cooling step is usually performed through an electrode that is pressed against the sheet assembly. The cooling step may be performed by cutting off the current to the electrodes, or by passing a current value smaller than that in the first current-passing step.
[0038] The cooling step reduces the electrical resistance of the sheet assembly to within a desired range, which makes it possible to prevent spattering or the like occurring at least between the second steel sheet and the Al alloy sheet when a large second current value is applied in the second current application step.
[0039] <Heat treatment process> The plate assembly joined after the second current passing step may be further subjected to heat treatment such as annealing or tempering. The heat treatment adjusts the structure of each joint (nugget) or its vicinity (heat-affected zone) and removes residual stress.
[0040] The heating temperature in the heat treatment step is, for example, 120 to 250° C., or 150 to 200° C. The heating time is, for example, 10 to 180 minutes, or 30 to 120 minutes. The heating method may be, for example, furnace heating or electric current heating. The heating range may be the entire joined plate assembly, or may be the spot-welded local area.
[0041] "electrode" (1) Form The electrodes for spot welding may be either detachable from the shank (cap tip type) or integral with the shank (integral type). Usually, cap tip type electrodes (also called "tips") are used to reduce costs.
[0042] The electrode (tip) has, for example, a bottomed, generally cylindrical tip portion and a generally cylindrical body portion continuing from the tip portion. The outer surface (pressure contact surface) of the tip portion may be convex or concave. The size of the electrode is not important. The outer diameter (nominal diameter / D2) of the body portion is, for example, φ10 to 20 mm, or φ12 to 18 mm. The tip diameter (D1) is, for example, φ6 to 14 mm, or φ8 to 12 mm.
[0043] The electrode is preferably introduced with a coolant (cooling liquid / cooling water) in the inner cylinder at the tip of the electrode. The coolant is forced to circulate. R This makes it possible to stably suppress the temperature rise of the electrodes and cool the plate material through the electrodes.
[0044] Many basic shapes of the tip of electrodes (especially convex electrodes) are specified in JIS C9304 (1999). For example, there are flat type (F type), radius type (R type), dome type (D type), dome radius type (DR type), truncated cone type (CF type), truncated cone radius type (CR type), etc. For spot welding of steel plates and Al alloy plates, it is recommended to use electrodes of DR type or R type, for example, from the viewpoint of versatility.
[0045] (2)Material The electrode (at least the tip) is preferably made of a material having excellent thermal conductivity, electrical conductivity, strength, etc. For example, an electrode made of a copper alloy having an electrical conductivity of 75 to 95% IACS, or even 80 to 90% IACS, is used. Examples of copper alloys include chromium copper, zirconium copper, chromium-zirconium copper, alumina-dispersed copper, and beryllium copper.
[0046] The electrode in contact with the steel plate and the electrode in contact with the Al alloy plate may be the same or different in form (shape, size (diameter)) and material.
[0047] "others" The current value (current density) and / or pressure may be changed during or between current passing steps. For example, at the start of each current passing step, an upslope process in which the current flow rate is gradually increased may be provided to prevent the generation of spatter due to a sudden increase in the current value. Also, at the end of each current passing step, a downslope process in which the current flow rate is gradually decreased may be provided to prevent weld cracks (solidification cracks associated with solidification shrinkage of the molten pool, hot cracks that may occur near the recrystallization temperature, etc.) due to a sudden drop in the current value.
[0048] The pressure may be changed for each step, during each step, or between steps. However, the pressure should be such that the thickness of the Al alloy sheet is not excessively reduced due to indentation by the electrodes. Usually, it is sufficient to keep the pressure constant during or between steps. EXAMPLES
[0049] The present invention will be specifically described with reference to an example in which a sheet assembly in which two steel sheets and an Al alloy sheet are stacked in order is joined by spot welding.
[0050] "overview" An overview of spot welding according to this embodiment is shown in Fig. 1. The material to be welded is a sheet assembly in which a first steel plate, a second steel plate, and an Al alloy plate are laminated in this order. Spot welding is performed by clamping both outer sides of the assembly with a pair of electrodes and passing current through them.
[0051] (1) Board material The first steel plate was a non-coated cold-rolled steel plate (440 MPa grade / plate thickness: 1.4 mm), the second steel plate was a galvannealed steel plate (270 MPa grade / plate thickness: 0.8 mm), and the Al alloy plate was a wrought material equivalent to JIS A6022 / plate thickness: 1.2 mm). The galvanized steel plate had a galvanized layer (metal layer) of approximately 8 μm in thickness. The melting point of the galvanized layer itself is approximately 420°C, and the melting point of the Al alloy plate is approximately 650°C.
[0052] Each plate material was used for spot welding as it was, without surface polishing, etc. Also, each plate material was cut into strips (30 mm x 100 mm) before use.
[0053] (2) Electrode The first electrode on the first steel plate side and the second electrode on the Al alloy plate side used the same DR type (JIS C9304) commercially available tip (OBARA Corporation). The tip was forcibly cooled by supplying forcedly circulated cooling water (flow rate: 4 L / min) to the inside (inner cylindrical part). The electrode was made of chromium copper (Cr: 1 mass%, Cu: balance), and its electrical conductivity was 80% IACS.
[0054] The size of the electrode was as shown in the enlarged view of Figure 1, with a tip diameter (nominal diameter D2) of φ16 mm, a thickness at the bottom of the tip of 12 mm, a radius of curvature (R) at the tip shoulder of 8 mm, a radius of curvature (R1) at the tip surface of 40 mm, and a tip diameter (D1) of either 8 mm, 10 mm, or 12 mm. Unless otherwise specified, an electrode with a tip diameter (D1) of 12 mm was used.
[0055] (3) Welding conditions The spot welding was performed using a servo pressure spot welding machine (ARO PA235KVAMF) according to the current pattern shown in FIG. 2. Specifically, current was controlled by DC current, and the current value was constant during each current process except for the transition period at the start and end of current. The pressure (F) was 4 kN (constant). In the first current process, the first current value (I1) was 9 kA, and the current time was 100 ms. In the second current process, the second current value (I2) was 10 to 20 kA, and the current time was 300 ms. If pre-current is performed before the first current process to allow the plates or the electrodes and the plates to blend together, the quality (joint strength) of the welded product can be stabilized even during mass production.
[0056] In addition, a cooling process was provided before the start of the second current application process. In the cooling process, the current was not applied for 200 ms after the end of the first current application process. This allows the plate assembly to be cooled through both electrodes, and the electrical resistance between each plate (particularly between the second steel plate and the Al alloy plate) falls to a predetermined range. This cooling process allows the subsequent second current application process to be carried out stably.
[0057] "observation" (1) The above plate assembly is spot welded (second current value: 13 kA, electrode tip diameter: φ12 mm, current density: 115 A / mm 2A photograph of the cross section of the joint obtained by welding (100% pure steel) was observed with an inverted metallurgical microscope (GX53 manufactured by Olympus Corporation) and shown in FIG. 3A. As is clear from FIG. 3A, it was confirmed that the first steel plate and the second steel plate were joined via the first nugget located between the opposing surfaces of the first steel plate and the second steel plate, and that the second steel plate and the Al alloy plate were joined via the second nugget located between the opposing surfaces of the second steel plate and the second steel plate. From FIG. 3A, it can be seen that the first nugget was formed by melting both the first steel plate and the second steel plate and then solidifying. Also from FIG. 3A, it can be seen that the second nugget was formed mainly by melting and solidifying the Al alloy plate.
[0058] As can be seen from Fig. 3A, both the first and second nuggets had sufficient size (diameter) and thickness (length in the sheet thickness direction). It was also found that the indentation (dent, depression) on the Al alloy sheet side by the electrode was only about 0.3 mm deep (sheet thickness reduction: about 25%).
[0059] (2) Figure 3B shows a photograph of the structure near the bonding interface between the second steel plate and the Al alloy plate, observed with a scanning electron microscope (S-3600N, Hitachi High-Tech Corporation). When the structure was observed with an energy dispersive X-ray spectrometer (EDX) attached to the microscope, several types of intermetallic compounds were observed, such as the Fe2Al5 phase, FeAl3 phase, Fe-Al-Zn phase (mainly Fe2Al5 with Zn solid solution) or Al-Zn phase. If we had to say, there was a lot of Al5Fe2 phase (or Fe-Al-Zn phase) on the second steel plate side, and Al3Fe phase was confirmed on the Al alloy plate side.
[0060] Generally, it is said that an intermetallic compound layer (interface reaction layer) is fragile and therefore its thickness is preferably 1 to 2 μm or less. However, the thickness of the intermetallic compound layer in this example was about 4.3 μm, but as described later, sufficient bonding strength was ensured.
[0061] 《Join strength》 (1) As shown in Figure 4, spot welding (second current value: 13 kA, electrode tip diameter: φ12 mm, current density: 115 A / mm 2 Two types of test pieces were prepared using the above method, and their bonding strengths were evaluated.
[0062] (2) As shown in Figure 4(a), the tensile shear strength (average of five tests) was 4430N. As shown in Figure 4(b), the cross tensile strength (average of five tests) was 1150N. In both cases, it was confirmed that sufficient joint strength was ensured. Note that the joint strength shown in Figure 4 is the load at break.
[0063] Second current value (1) As shown in Fig. 5, spot welding (electrode tip diameter: φ12 mm) was performed by changing the second current value in various ways. The cross section of each obtained weld was observed with the above-mentioned microscope (see Fig. 3A), and the size of the second nugget (simply referred to as "second nugget diameter (d2)") and the sheet thickness reduction rate (b / t) of the Al alloy sheet were measured. Here, d2 is the minimum width of the second nugget, and b is the thickness obtained by subtracting the thickness of the second nugget from the minimum thickness part of the Al alloy sheet. Note that t was set to 1.2 mm (constant).
[0064] (2) As can be seen from Fig. 5, when the second current value was 16 kA or more (over 15 kA), spatter was generated between the Al alloy sheet and the second steel sheet. After that, even if the second current value increased, the second nugget diameter (d2) hardly increased, and the remaining thickness of the Al alloy sheet (thickness other than the second nugget) rapidly decreased.
[0065] Welded (1) As shown in Figure 6, spot welding was performed by changing the second current value and the electrode tip diameter in various ways. Spot welding was performed at five points at one second intervals. The welding spot interval was 35 mm. The tip surface of the electrode on the Al alloy plate side after spot welding was observed. Photographs of each electrode are shown in Figure 6. In Figure 6, the second current value is shown as a function of the electrode tip area (πD1 2 The current density calculated by dividing the current density by 1 / 4) is also shown.
[0066] (2) As can be seen from Fig. 6, when the second current value was 16 kA or more (over 15 kA), adhesion of the Al alloy to the tip surface of the copper alloy electrode was observed even with only five spot welding points. However, it was also found that the adhesion level could be reduced by increasing the tip diameter of the electrode and decreasing the current density.
[0067] On the other hand, it was also found that when the second current value was 13 kA (15 kA or less), welding could be suppressed regardless of the tip diameter of the electrode (current density).
[0068] As described above, it was found that the sheet combination consisting of the first steel sheet, the second steel sheet, and the Al alloy sheet can be well spot welded by performing the first current flow process and the second current flow process. It was also found that it is preferable to set the second current value to 15 kA or less in order to suppress the generation of spatter and the welding of the electrodes.
Claims
1. A spot welding method in which a plurality of overlapping plate materials are joined together by resistance heating by passing current through a pair of opposing electrodes that are pressed against both outer surfaces of a plate assembly, the method comprising the steps of: The plate assembly is formed by stacking at least a first steel plate, a second steel plate, and an aluminum alloy plate in this order, a first current application step of generating a molten pool between the first steel plate and the second steel plate without melting the aluminum alloy plate; A second current application step is provided after the first current application step, in which a melting reaction occurs between the second steel plate and the aluminum alloy plate, The first current application step is performed by applying a direct current of 4 to 10 kA for 25 to 150 ms, The second current passing step is performed by passing a direct current of 15 kA or less, which is smaller than a melting current value that can melt the aluminum alloy plate by resistance heating alone, for a longer time than that of the first current passing step, the first steel plate and the second steel plate are joined via a first nugget, A spot welding method in which the second steel plate and the aluminum alloy plate are joined via a second nugget containing an intermetallic compound produced by the melting reaction.
2. 2. The spot welding method according to claim 1, wherein the second current application step is performed by applying a direct current of 10 to 15 kA for 150 to 500 ms.
3. In the second current application step, a second current density calculated by dividing the current value by the tip area of the electrode in contact with the aluminum alloy plate is set to 50 to 300 A / mm 2 The spot welding method according to claim 1 or 2,
4. The spot welding method according to any one of claims 1 to 3, further comprising a cooling step of, after the first current passing step and before the second current passing step, not passing current or passing a current value smaller than that in the first current passing step to the sheet pair in contact with the electrodes, thereby lowering a temperature of the sheet pair.
5. The spot welding method according to any one of claims 1 to 4, further comprising a heat treatment step of annealing or tempering the plate assembly joined after the second current passing step.
6. The spot welding method according to any one of claims 1 to 5, wherein the second steel plate has a metal layer having a lower melting point than the aluminum alloy plate at least on the aluminum alloy plate side.
7. The spot welding method according to claim 6, wherein the metal layer is a zinc plating layer.
Citation Information
Patent Citations
Joint body of different materials by steel material and aluminum material
JP2006289452A
Joining method of iron member with aluminum member, and iron-aluminum joined structure
JP2008105087A
Joint body of aluminum alloy plate material to plated steel plate material
JP2013027890A
Dissimilar metal bonding method
JP2013078804A
Method for spot welding high-strength steel plate
JP2015093282A