Cyclic olefin copolymer composition and crosslinked product thereof
A cyclic olefin copolymer composition with a hindered phenol and hindered amine compound addresses the issue of poor heat aging resistance and dielectric property deterioration in crosslinked products, achieving enhanced thermal stability and dielectric performance.
Patent Information
- Application Number
- JP2020190140
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-28
- Filing Date
- 2020-11-16
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-11-16
AI Technical Summary
Crosslinked products made from cyclic olefin copolymers with crosslinkable groups suffer from poor heat aging resistance and deterioration of dielectric properties when exposed to high temperatures, and existing solutions to improve heat resistance, such as increasing the amount of heat stabilizers, lead to a decline in dielectric properties.
A cyclic olefin copolymer composition is developed by incorporating a specific hindered phenol and a hindered amine compound with a piperidyl group in a defined ratio, maintaining excellent dielectric properties while enhancing heat aging resistance.
The composition effectively improves heat aging resistance of cyclic olefin copolymers without compromising their dielectric properties, ensuring long-term stability under high temperatures.
Smart Images

Figure 0007590854000001 
Figure 0007590854000002 
Figure 0007590854000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cyclic olefin copolymer composition and a crosslinked product thereof. [Background technology]
[0002] Cyclic olefin copolymers are used in a variety of fields because of their excellent heat resistance, mechanical properties, transparency, dielectric properties, solvent resistance, moldability, dimensional stability, etc. (see, for example, Patent Documents 1 and 2).
[0003] Furthermore, in recent years, cyclic olefin polymers have begun to be considered as materials for electronic parts such as printed wiring boards because of their excellent balance of heat resistance and dielectric properties (see, for example, Patent Documents 2 and 3).
[0004] Patent Document 2 describes a cyclic olefin copolymer having a crosslinkable group. It describes that the crosslinked product of this cyclic olefin copolymer has excellent stability over time of dielectric properties, and also has excellent heat resistance, transparency, mechanical properties, etc., and can therefore be suitably used for high frequency applications such as high frequency circuit boards.
[0005] Patent Document 3 describes a crosslinkable resin composition comprising a cyclic olefin resin, an organic peroxide, a crosslinking aid, and powdered red phosphorus. It describes that a crosslinked resin molded product obtained by heating and crosslinking this crosslinkable resin composition has dielectric properties and solder heat resistance in the high frequency band, and also has high flame retardancy and mechanical strength, and is therefore suitable for use in applications requiring dielectric properties, heat resistance, flame retardancy, mechanical properties, etc., such as printed wiring boards and computer parts. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2006 / 118261 [Patent Document 2] International Publication No. 2012 / 046443 [Patent Document 3] JP2005-47992A Summary of the Invention [Problem to be solved by the invention]
[0007] According to the study by the present inventors, it has become clear that the dielectric properties of a crosslinked body made of a cyclic olefin copolymer having a crosslinkable group as described in Patent Document 2 are gradually deteriorated by exposure to high temperatures. That is, the crosslinked body made of a cyclic olefin copolymer having a crosslinkable group has poor heat aging resistance. In addition, the crosslinked body made of a cyclic olefin resin as described in Patent Document 3 has poor crosslinking reactivity and leaves room for improvement in terms of heat resistance, since the cyclic olefin resin, which is the main component of the resin composition constituting this crosslinked body, does not have a crosslinkable group. Furthermore, according to the inventors' investigations, it has become clear that when the amount of heat stabilizer blended with the cyclic olefin copolymer is increased in order to improve the heat aging resistance of a crosslinked body composed of a cyclic olefin copolymer having a crosslinkable group as described in Patent Document 2, the dielectric properties may deteriorate. From the above, there is room for improvement in the crosslinked body composed of a cyclic olefin copolymer having a crosslinkable group in terms of improving heat aging resistance while maintaining the excellent dielectric properties of the cyclic olefin copolymer.
[0008] The present invention has been made in consideration of the above circumstances, and provides a cyclic olefin copolymer composition that can improve heat aging resistance while maintaining the excellent dielectric properties of the cyclic olefin copolymer. [Means for solving the problem]
[0009] As a result of intensive research aimed at solving the above problems, the present inventors have found that by mixing a specific hindered phenol (X) and a specific hindered amine compound having a piperidyl group in a specific ratio with a cyclic olefin copolymer having a crosslinkable group, the heat aging resistance of the cyclic olefin copolymer can be improved while maintaining the excellent dielectric properties of the cyclic olefin copolymer, and have completed the present invention.
[0010] The present invention is as follows.
[0011] [1] A cyclic olefin copolymer composition comprising a cyclic olefin copolymer (m), a hindered phenol (X) represented by the following general formula (1), and a hindered amine compound (Y) having a piperidyl group represented by the following general formula (2): The cyclic olefin copolymer (m) is (A) one or more olefin-derived repeating units represented by the following general formula (I), (B) one or more repeating units derived from a cyclic non-conjugated diene represented by the following general formula (III): Rank and (C) one or more repeating units derived from a cyclic olefin represented by the following general formula (V), When the total number of moles of repeating units in the cyclic olefin copolymer (m) is taken as 100 mol %, the content of the repeating unit (A) derived from the olefin is 10 mol % or more and 90 mol % or less, the content of the repeating unit (B) derived from the cyclic non-conjugated diene is 1 mol % or more and 40 mol % or less, and the content of the repeating unit (C) derived from the cyclic olefin is 1 mol % or more and 30 mol % or less, A cyclic olefin copolymer composition, in which the content of the hindered amine compound (Y) in the cyclic olefin copolymer composition is 0.01 parts by mass or more and 5 parts by mass or less when the content of the cyclic olefin copolymer (m) contained in the cyclic olefin copolymer composition is 100 parts by mass. [ka] [In the above general formula (I), R300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. [ka] [In the above general formula (III), u is 0 or 1, v is 0 or a positive integer, and w is 0. or 1, and R 61 ~R 76 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 104 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, t is a positive integer of 0 to 10, and R 75 and R 76 are bonded to each other may form a monocyclic or polycyclic ring.] [ka] [In the above general formula (V), u is 0 or 1, v is 0 or a positive integer, w is 0 or 1, and R 61 ~R 78 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 75 ~R 78 may be bonded to each other to form a monocyclic or polycyclic ring. [ka] (In the above general formula (1), X is an organic group.) [ka] [In the above general formula (2), X is a hydrogen atom, an oxy radical group, an alkyl group, an alkoxy group, an aryl group, or a hydroxy group, and R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom or an alkyl group. [2] the organic group X of the hindered phenol (X) is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a cyclohexyl group, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; The cyclic olefin copolymer composition according to the above [1], wherein the substituents of the alkyl group, the cyclohexyl group, and the aryl group are selected from the group consisting of an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, a hydroxy group, a methoxy group, and an oxadiazole group. [3] The organic group X of the hindered phenol (X) is a methyl group, an ethyl group, an n-propyl group, an n-octyl group, an n-tetradecyl group, an n-hexadecyl group, a 2,4-di-t-butyl group, A group selected from the group consisting of a phenyl group and a 2,4-di-t-pentylphenyl group. The cyclic olefin copolymer composition according to the above [1] or [2]. [4] The cyclic non-conjugated diene constituting the repeating unit (B) derived from the cyclic non-conjugated diene is 5-vinyl-2-norbornene or 8-vinyl-9-methyltetracyclo[4.4.0.1 2,5 .1 7,10 The cyclic olefin copolymer composition according to any one of the above [1] to [3], wherein the cyclic olefin copolymer is 3-dodecene. [5] The cyclic olefin constituting the repeating unit (C) derived from the cyclic olefin is bicyclo[2.2.1]-2-heptene or tetracyclo[4.4.0.1 2,5 .1 7,10 The cyclic olefin compound according to any one of the above [1] to [4], wherein the cyclic olefin compound is 3-dodecene. Copolymer composition. [6] The composition further comprises a cyclic olefin polymer (n) different from the cyclic olefin copolymer (m), The cyclic olefin polymer (n) is a copolymer (n1) of ethylene or an α-olefin and a cyclic olefin (wherein the copolymer (n1) is represented by the following general formula (III) (n2) a ring-opening polymer of a cyclic olefin, When the total amount of the cyclic olefin copolymer (m) and the cyclic olefin polymer (n) is taken as 100 mass%, The cyclic olefin copolymer composition according to any one of [1] to [5] above, wherein the content of the cyclic olefin polymer (m) is 5% by mass or more and 95% by mass or less, and the content of the cyclic olefin polymer (n) is 5% by mass or more and 95% by mass or less. [ka] [In the above general formula (III), u is 0 or 1, v is 0 or a positive integer, and w is 0. or 1, and R 61 ~R 76 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 104 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, t is a positive integer of 0 to 10, and R 75 and R 76 are bonded to each other may form a monocyclic or polycyclic ring.] [7] The cyclic olefin copolymer composition according to any one of the above [1] to [6], wherein the hindered amine compound (Y) has a molecular weight of 1,000 or more. [8] A varnish comprising the cyclic olefin copolymer composition according to any one of the above [1] to [7] and a solvent. [9] A crosslinked product of the cyclic olefin copolymer composition according to any one of [1] to [7] above.
[10] A film or sheet comprising the crosslinked product according to [9] above.
[11] A laminate obtained by laminating the film or sheet according to
[10] above onto a substrate.
[12] A prepreg comprising the cyclic olefin copolymer composition according to any one of [1] to [7] above and a sheet-like fiber substrate.
[13] A metal-clad laminate obtained by laminating at least one selected from the film or sheet according to the above-mentioned
[10] , the laminate according to the above-mentioned
[11] , and the prepreg according to the above-mentioned
[12] , and a metal foil.
[14] A printed wiring board comprising an electrical insulation layer formed from at least one material selected from the film or sheet according to
[10] above, the laminate according to
[11] above, and the prepreg according to
[12] above, and a conductor layer provided on the electrical insulation layer.
[15] An electronic device comprising the printed wiring board according to
[14] above. Effect of the Invention
[0012] According to the present invention, it is possible to provide a cyclic olefin copolymer composition which can improve heat aging resistance while maintaining the excellent dielectric properties of the cyclic olefin copolymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the present invention will be described based on the embodiments. In the present embodiments, "A to B" indicating a numerical range means A or more and B or less unless otherwise specified.
[0014] First, a cyclic olefin copolymer composition according to an embodiment of the present invention will be described. The cyclic olefin copolymer composition according to the present embodiment contains a cyclic olefin copolymer (m), a hindered phenol (X) represented by the following general formula (1), and a hindered amine compound (Y) having a piperidyl group represented by the following general formula (2). When the content of the cyclic olefin copolymer (m) contained in the cyclic olefin copolymer composition according to the present embodiment is 100 parts by mass, the content of the hindered amine compound (Y) in the cyclic olefin copolymer composition is 0.01 parts by mass or more, preferably 0.02 parts by mass or more, more preferably 0.05 parts by mass or more, and particularly preferably 0.08 parts by mass or more. When the content of the hindered amine compound (Y) is the above lower limit or more, the heat aging resistance of the cyclic olefin copolymer composition can be improved. In addition, when the content of the cyclic olefin copolymer (m) contained in the cyclic olefin copolymer composition according to the present embodiment is 100 parts by mass, the content of the hindered amine compound (Y) in the cyclic olefin copolymer composition is 5 parts by mass or less, preferably 2 parts by mass or less, and more preferably 1 part by mass or less. When the content of the hindered amine compound (Y) is the above upper limit or less, deterioration of the dielectric properties of the cyclic olefin copolymer composition can be suppressed. According to the cyclic olefin copolymer composition of this embodiment, it is possible to improve the heat aging resistance while maintaining the excellent dielectric properties of the cyclic olefin copolymer. The reason for this is not entirely clear, but it is believed to be as follows. That is, the hindered phenol (X) captures peroxide radicals, which are among the radical species generated when cyclic olefin resins are exposed to high temperatures for long periods of time, and suppresses oxidative degradation of the resin. In addition, the hindered phenol (X) having a benzoate skeleton has good compatibility with cyclic olefins, and is thought to be highly effective in improving heat aging resistance. On the other hand, the hindered amine compound (Y) efficiently captures alkyl radicals and inhibits the oxidative deterioration of the resin. In particular, the hindered amine compound (Y) having a molecular weight of a certain level or more is highly stable in the cyclic olefin resin and is considered to be effective for a long period of time. By mixing these in a specific ratio, it is possible to obtain a cyclic olefin resin composition that exhibits excellent heat aging resistance over a longer period of time.
[0015] [ka] (In the above general formula (1), X is an organic group.)
[0016] [ka] [In the above general formula (2), X is a hydrogen atom, an oxy radical group, an alkyl group, an alkoxy group, an aryl group, or a hydroxy group, and R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom or an alkyl group.
[0017] The total content of the cyclic olefin polymers contained in the cyclic olefin copolymer composition according to this embodiment is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more, when the entire cyclic olefin copolymer composition is taken as 100% by mass. This can improve the balance of heat resistance, mechanical properties, transparency, dielectric properties, solvent resistance, moldability, dimensional stability, etc. The upper limit of the total content of the cyclic olefin polymers contained in the cyclic olefin copolymer composition according to this embodiment is not particularly limited, but is, for example, less than 100% by mass, preferably 99% by mass or less. Here, the cyclic olefin polymer contained in the cyclic olefin copolymer composition according to this embodiment means the cyclic olefin copolymer (m) and the cyclic olefin copolymer (n) described below.
[0018] Each component will be specifically described below.
[0019] [Cyclic olefin copolymer (m)] The cyclic olefin copolymer (m) according to the present embodiment comprises (A) one or more olefin-derived repeating units represented by the following general formula (I) and (B) a repeating unit represented by the following general formula (III): It contains one or more repeating units derived from a cyclic non-conjugated diene, and (C) one or more repeating units derived from a cyclic olefin represented by the following general formula (V).
[0020] [ka]
[0021] In the above general formula (I), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms.
[0022] [ka]
[0023] In the above general formula (III), u is 0 or 1, and v is 0 or a positive integer, preferably 0. is an integer of 0 or more and 2 or less, more preferably 0 or 1, w is 0 or 1, R 61 ~R 76 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 104is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and t is 0 is a positive integer between 10 and R 75 and R 76 may be bonded to each other to form a monocyclic or polycyclic ring.
[0024] [ka]
[0025] In the above general formula (V), u is 0 or 1, v is 0 or a positive integer, preferably an integer of 0 or more and 2 or less, more preferably 0 or 1, w is 0 or 1, R 61 ~R 78 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 75 ~R 78 may be bonded to each other to form a monocyclic or polycyclic ring.
[0026] In the cyclic olefin copolymer (m), when the total number of moles of repeating units in the cyclic olefin copolymer (m) is taken as 100 mol%, the content of the repeating unit (A) derived from an olefin is 10 mol% to 90 mol%, preferably 15 mol% to 85 mol%, more preferably 20 mol% to 80 mol%, even more preferably 30 mol% to 80 mol%, even more preferably 35 mol% to 80 mol%, and particularly preferably 40 mol% to 80 mol%. The content of the repeating unit (B) derived from a cyclic non-conjugated diene is 1 mol% to 40 mol%, preferably 2 mol% to 35 mol%, even more preferably 3 mol% to 30 mol%, and the content of the repeating unit (C) derived from a cyclic olefin is 1 mol% to 30 mol%, preferably 3 mol% to 25 mol%, and even more preferably 5 mol% to 20 mol%. When the content of each repeating unit in the cyclic olefin copolymer (m) is within the above range, the crosslinked body obtained from the cyclic olefin copolymer composition has excellent stability of dielectric properties over time and excellent heat resistance. Furthermore, the crosslinked body (Q) can be obtained that is excellent in mechanical properties, dielectric properties, transparency and gas barrier properties. In other words, the crosslinked body (Q) can be obtained that has a good balance of these physical properties.
[0027] The olefin monomer, which is one of the copolymerization raw materials for the cyclic olefin copolymer (m), is a monomer that provides the skeleton represented by the above formula (I) through addition copolymerization, and is an olefin represented by the following general formula (Ia).
[0028] [ka]
[0029] In the above general formula (Ia), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. Examples of the olefin represented by the general formula (Ia) include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. From the viewpoint of obtaining a crosslinked body (Q) having better heat resistance, mechanical properties, dielectric properties, transparency, and gas barrier properties, ethylene and propylene are preferred, and ethylene is particularly preferred. Two or more kinds of olefin monomers represented by the above formula (Ia) may be used.
[0030] The cyclic non-conjugated diene monomer, which is one of the copolymerization raw materials of the cyclic olefin copolymer (m), undergoes addition copolymerization to form the constitutional unit represented by the above formula (III). Specifically, A cyclic non-conjugated diene represented by the following general formula (IIIa) corresponding to the above general formula (III) is used.
[0031] [ka]
[0032] In the above general formula (IIIa), u is 0 or 1, v is 0 or a positive integer, preferably is an integer of 0 to 2, more preferably 0 or 1, w is 0 or 1, R 61 ~R 76 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 104 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and t is a positive integer between 0 and 10, and R 75 and R 76 may be bonded to each other to form a monocyclic or polycyclic ring.
[0033] The cyclic non-conjugated diene represented by the above general formula (IIIa) is not particularly limited. Examples of the cyclic non-conjugated dienes are those represented by the following chemical formulas: 2,5 .1 7,10 ]-3-dodecene is preferred, and 5-vinyl-2-norbornene is preferred. is particularly preferred.
[0034] [ka]
[0035] [ka]
[0036] The cyclic non-conjugated diene represented by the above general formula (IIIa) can also be specifically represented by the following general formula (IIIb).
[0037] [ka]
[0038] In the general formula (IIIb), n is an integer of 0 to 10, and R1 is a hydrogen atom or a group having 1 carbon atom. R2 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.
[0039] The cyclic olefin copolymer (m) according to the present embodiment includes a ring represented by the general formula (III). The copolymer is characterized in that it contains a structural unit derived from a non-conjugated diene and thus has a double bond in the side chain portion, i.e., in the portion other than the main chain of the copolymer.
[0040] The cyclic olefin monomer, which is one of the copolymerization raw materials of the cyclic olefin copolymer (m), undergoes addition copolymerization to form the constitutional unit represented by the above formula (V). Specifically, the cyclic olefin monomer represented by the following general formula (Va) corresponding to the above general formula (V) is used.
[0041] [ka]
[0042] In the above general formula (Va), u is 0 or 1, v is 0 or a positive integer, preferably an integer of 0 or more and 2 or less, more preferably 0 or 1, w is 0 or 1, R 61 ~R 78 And R a1 and R b1may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 75 ~R 78 may be bonded to each other to form a monocyclic or polycyclic ring.
[0043] Specific examples of the cyclic olefin represented by the above general formula (Va) include the compounds described in WO 2006 / 118261. Examples of the cyclic olefin represented by the above general formula (Va) include bicyclo[2.2.1]-2-heptene (also called norbornene), tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene (also called tetracyclododecene) is preferred, and tetracyclo[4.4.0.1 2,5 .1 7,10 These cyclic olefins have the advantage that the elastic modulus of the copolymer and crosslinked body is easily maintained because they have a rigid ring structure, and crosslinking can be easily controlled because they do not contain a hetero double bond structure.
[0044] By using the olefin monomer represented by the general formula (Ia) and the cyclic olefin represented by the general formula (Va) as the copolymerization components, the solubility of the cyclic olefin copolymer (m) in a solvent is further improved, resulting in good moldability and improved product yield.
[0045] The cyclic olefin copolymer (m) comprises (A) one or more repeating units derived from olefins represented by general formula (I), (B) repeating units derived from cyclic non-conjugated dienes represented by general formula (III), (C) one or more repeating units derived from a cyclic olefin represented by general formula (V), in addition to the repeating units derived from a cyclic non-conjugated diene represented by general formula (III) and a repeating unit derived from a cyclic olefin represented by general formula (V). The cyclic olefin may be composed of repeating units derived from a cyclic olefin other than the cyclic olefins mentioned above, and / or repeating units derived from a chain polyene. In this case, the copolymerization raw materials for the cyclic olefin copolymer (m) are an olefin monomer represented by the general formula (Ia), a cyclic non-conjugated diene monomer represented by the general formula (IIIa), In addition to the cyclic olefin monomer represented by the general formula (Va), the cyclic olefin monomer represented by the general formula (IIIa) Cyclic non-conjugated diene monomers and cyclic olefin monomers other than the cyclic olefin monomers represented by general formula (Va), and / or linear polyene monomers can be used. Such cyclic olefin monomers and linear polyene monomers are cyclic olefins represented by the following general formula (VIa) or (VIIa), or linear polyenes represented by the following general formula (VIIIa): Two or more different types of these cyclic olefins and linear polyenes may be used.
[0046] [ka]
[0047] In the general formula (VIa), x and d each represent an integer of 0 or 1 or more, preferably 0 or more and 2 or less. is an integer, more preferably 0 or 1, y and z are 0, 1 or 2, R 81 ~R 99 may be the same or different, and each is a hydrogen atom, a halogen atom, an aliphatic hydrocarbon group which is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 15 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or an alkoxy group; R 89 and R 90 and the carbon atom to which R is bonded. 93 or the carbon atom to which R is bonded 91 may be bonded directly or via an alkylene group having 1 to 3 carbon atoms, and when y=z=0, R 95 and R 92 or R 95 and R 99 may be bonded to each other to form a monocyclic or polycyclic aromatic ring.
[0048] [ka]
[0049] In general formula (VIIa), R 100 and R 101 may be the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and f is 1≦f≦18.
[0050] [ka]
[0051] In general formula (VIIIa), R 201 From R 206 may be the same or different, It is a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and P is a linear or branched hydrocarbon group having 1 to 20 carbon atoms, which may contain a double bond and / or a triple bond.
[0052] Specific examples of cyclic olefins represented by general formula (VIa) and general formula (VIIa) The compounds described in paragraphs 0037 to 0063 of WO 2006 / 118261 can be used.
[0053] Specific examples of the chain polyene represented by the general formula (VIIIa) include 1,4-hexadiene. Examples of the polyene include 3-methyl-1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, 4,5-dimethyl-1,4-hexadiene, 7-methyl-1,6-octadiene, DMDT, 1,3-butadiene, and 1,5-hexadiene. Cyclizable polyenes cyclized from polyenes such as 1,3-butadiene and 1,5-hexadiene may also be used.
[0054] The cyclic olefin copolymer (m) is a linear polyene represented by the above general formula (VIIIa). or a cyclic non-conjugated diene represented by general formula (III) and a structural unit derived from Cyclic olefins other than those represented by the general formula (VIa), the general formula In the case where the copolymer contains a repeating unit derived from one or more olefin-derived repeating units represented by the above general formula (I), the content of the repeating units derived from one or more olefin-derived repeating units represented by the above general formula (III) is The amount is usually 0.1 to 100 mol %, preferably 0.1 to 50 mol %, based on the total molar number of repeating units derived from one or more cyclic non-conjugated dienes and one or more repeating units derived from one or more cyclic olefins represented by the above general formula (V).
[0055] By using the olefin monomer represented by the general formula (I), the cyclic olefin represented by the general formula (VIa) or (VIIa), and the chain polyene represented by the general formula (VIIIa) as the copolymerization components, the effects of this embodiment can be obtained, and the solubility of the cyclic olefin copolymer in a solvent is further improved, resulting in good moldability and improved product yield. Among these, the cyclic olefin represented by the general formula (VIa) or (VIIa) These cyclic olefins have the advantage that the elastic modulus of the copolymer and crosslinked body is easily maintained because they have a rigid ring structure, and crosslinking can be easily controlled because they do not contain a heterogeneous double bond structure.
[0056] The comonomer content and glass transition temperature (Tg) of the cyclic olefin copolymer (m) can be controlled by the monomer charging ratio according to the intended use. The Tg of the cyclic olefin copolymer (m) is usually 300°C or less, preferably 250°C or less, more preferably 200°C or less, even more preferably 170°C or less, and particularly preferably 150°C or less. When the Tg is equal to or less than the upper limit, the melt moldability of the cyclic olefin copolymer (m) and its solubility in a solvent when it is made into a varnish are improved.
[0057] The intrinsic viscosity [η] of the cyclic olefin copolymer (m) measured in decalin at 135°C is usually in the range of 0.10 to 15 dl / g, preferably 0.10 to 5 dl / g, more preferably 0.15 to 3 dl / g. When the intrinsic viscosity [η] is equal to or lower than the upper limit, the moldability is improved. When the intrinsic viscosity [η] is equal to or higher than the lower limit, the heat resistance and mechanical properties of the crosslinked body (Q) obtained by crosslinking the cyclic olefin copolymer composition are improved. The intrinsic viscosity [η] of the cyclic olefin copolymer (m) can be controlled by the polymerization conditions such as the polymerization catalyst, the cocatalyst, the amount of H2 added, and the polymerization temperature.
[0058] [Production method of cyclic olefin copolymer (m)] The cyclic olefin copolymer (m) according to this embodiment can be produced, for example, according to the method for producing a cyclic olefin copolymer described in paragraphs 0075 to 0219 of WO 2012 / 046443. Details are omitted here.
[0059] [Hindered phenol (X)] The hindered phenol (X) according to this embodiment is represented by the following general formula (1).
[0060] [ka]
[0061] X in the general formula (1) represents an organic group. The organic group X represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cyclohexyl group, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, and is preferably a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms. Examples of the substituted or unsubstituted alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an n-octyl group, an n-tetradecyl group, an n-hexadecyl group, etc. Examples of the substituted or unsubstituted aryl group having 6 to 20 carbon atoms include a 2,4-di-t-butylphenyl group, a 2,4-di-t-pentylphenyl group, etc. The substituent that the alkyl group, cyclohexyl group, and aryl group represented by the organic group X may have is preferably a group selected from the group consisting of an alkyl group having 1 to 12 carbon atoms, such as a methyl group or an ethyl group; an aryl group having 6 to 12 carbon atoms, such as a phenyl group; a hydroxy group; a methoxy group; and an oxadiazole group.
[0062] The molecular weight of the hindered phenol (X) is preferably from 200 to 2000, more preferably from 200 to 1000. When the molecular weight of the hindered phenol (X) is within the above range, volatilization during processing is small, and it is easily mixed well with other components. The hindered phenol (X) may have a radical scavenging effect. This can capture radicals generated by heat or light during the production or molding of the cyclic olefin copolymer composition according to this embodiment, or in the environment in which the molded product is used, and can suppress oxidative deterioration or thermal decomposition of the cyclic olefin copolymer composition according to this embodiment during the production or molding, or oxidative deterioration or decomposition of the cyclic olefin copolymer composition according to this embodiment in the molded product due to heat or light. In addition, the hindered phenol (X) may have an ultraviolet absorbing effect. This can suppress decomposition of the cyclic olefin copolymer composition according to this embodiment in the molded product due to light. In particular, the hindered phenol (X) has an oxycarbonyl group directly bonded to a benzene ring as shown in general formula (1), which allows the hindered phenol (X) to have good radical scavenging properties.
[0063] The content of the hindered phenol (X) in the resin composition is 0.01 to 5 parts by mass, preferably 0.02 to 2 parts by mass, and more preferably 0.08 to 1 part by mass, relative to 100 parts by mass of the total content of the cyclic olefin copolymers (m) and (n). When the content of the hindered phenol (X) is equal to or higher than the lower limit, the oxidative deterioration of the cyclic olefin copolymer composition can be suppressed and the heat aging resistance can be improved. When the content of the hindered phenol (X) is equal to or lower than the upper limit, the inhibition of the crosslinking reaction of the cyclic olefin copolymer composition by the hindered phenol (X) can be suppressed. When the content of the hindered phenol (X) is at least a certain level, the oxidative deterioration reaction of the cyclic olefin copolymers (m) and (n) in the molded product when exposed to heat or light for a long period of time can be preferably suppressed. When the content of the hindered phenol (X) is at most a certain level, the inhibition of the crosslinking reaction of the cyclic olefin copolymer composition by the hindered phenol (X) can be suppressed. During molding, radicals generated by heat and light received in the environment in which the molded product is used are captured, and oxidative deterioration and thermal decomposition of the cyclic olefin polymer during the production or molding, as well as oxidative deterioration and decomposition of the cyclic olefin polymer in the molded product due to heat and light, can be suppressed.
[0064] [Hindered amine compounds (Y)] The hindered amine compound (Y) according to this embodiment is a compound having a piperidyl group represented by the following general formula (2): The number of piperidyl groups represented by general formula (2) per molecule may be one or more.
[0065] [ka] In the above general formula (2), X is a hydrogen atom, an oxy radical group, an alkyl group, an alkoxy group, an aryl group, or a hydroxy group, preferably a hydrogen atom, a methyl group, or an ethyl group, more preferably a hydrogen atom or a methyl group, and particularly preferably a hydrogen atom. R 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom or an alkyl group, preferably a methyl group or an ethyl group, and more preferably a methyl group.
[0066] In the above general formula (2), when X is an alkyl group, the carbon number is preferably 1 to 12, when X is an alkoxy group, the carbon number is preferably 1 to 12, and when X is an aryl group, the carbon number is preferably 6 to 12. The alkyl group or alkoxy group represented by X is each independently linear or cyclic, and may have a branched chain. The alkyl group, alkoxy group, or aryl group represented by X may each independently have a substituent, and examples of the substituent include a hydroxyl group, a benzoyloxy group, and an acetoxy group.
[0067] Among the piperidyl groups represented by the above general formula (2), R 1 , R 2 , R 3 and R 4 In terms of cost and availability, compounds having a group in which all X are methyl groups are preferred. Also, compounds having a piperidyl group in which X is a methyl group or a hydrogen atom are preferred in terms of cost and availability.
[0068] The hindered amine compound (Y) having a piperidyl group represented by the above general formula (2) is preferably a compound having two or more piperidyl groups in one molecule. In this case, it is preferable that the compound has two or more piperidyl groups bonded via the bond at the 4-position of the piperidyl group represented by the above general formula (1).
[0069] The molecular weight of the hindered amine compound (Y) according to this embodiment is preferably from 140 to 20000. When the molecular weight of the hindered amine compound (Y) is within the above range, volatilization during processing is small, and the compound is easily mixed well with other components, and a decrease in the fluidity of the cyclic olefin copolymer composition according to this embodiment can be suppressed. The hindered amine compound (Y) according to the present embodiment may be either a low molecular weight type or a high molecular weight type. The molecular weight of the low molecular weight type hindered amine compound (Y) is preferably 200 or more and less than 1000, and the molecular weight of the high molecular weight type hindered amine compound (Y) is preferably 1000 or more and 20000 or less, more preferably 1000 or more and 10000 or less. In particular, it is preferable for the hindered amine compound (Y) to have a molecular weight of 1000 or more, since there is less volatilization during processing and the compound is more easily mixed with other components. The molecular weight of the hindered amine compound (Y) can be measured as the relative mass of the molecule, for example, by a mass spectrometer.
[0070] The hindered amine compound (Y) according to the present embodiment may have a radical scavenging action, which may scavenge radicals generated by heat or light during the production or molding of the cyclic olefin copolymer composition according to the present embodiment or in the environment in which the molded product is used, thereby suppressing oxidative deterioration or thermal decomposition of the cyclic olefin polymer during the production or molding, and oxidative deterioration or decomposition of the cyclic olefin polymer in the molded product due to heat or light.
[0071] Examples of the hindered amine compound (Y) according to the present embodiment include, but are not limited to, 2,2,6,6-tetramethyl-4-piperidone; 2,2,6,6-tetramethyl-4-piperidinol; bis-(1,2,2,6,6-pentamethylpiperidyl)-(3',5'-di-t-butyl-4'-hydroxybenzyl)butylmalonate; di-(2,2,6,6-tetramethyl-4-piperidyl)sebacate; N-(2-hydroxyethyl)- Oligomer of 2,2,6,6-tetramethyl-4-piperidinol and succinic acid;Oligomer of cyanuric acid and N,N-di(2,2,6,6-tetramethyl-4-piperidyl)-hexamethylenediamine;Bis-(2,2,6,6-tetramethyl-4-piperidinyl)succinate;Bis-(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl)sebacate;Bis-(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate;Tet Rakis-(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate;N,N'-bis-(2,2,6,6-tetramethyl-4-piperidyl)-hexane-1,6-diamine;N-Butyl-2,2,6,6-tetramethyl-4-piperidinamine;2,2'-[(2,2,6,6-tetramethyl-piperidinyl)-imino]-bis-[ethanol];Poly((6-morpholine-S-triazine-2,4-diyl)(2 ,2,6,6-tetramethyl-4-piperidinyl)-iminohexamethylene-(2,2,6,6-tetramethyl-4-piperidinyl)-imino);5-(2,2,6,6-tetramethyl-4-piperidinyl)-2-cyclo-undecyl-oxazole;1,1'-(1,2-ethane-di-yl)-bis-(3,3',5,5'-tetramethyl-piperazinone);8-acetyl-3-dodecyl-7,7,9,9-tetramethyl-1,3,8-triazaspiro(4.5) Decane-2,4-dione; Polymethylpropyl-3-oxy-[4(2,2,6,6-tetramethyl)-piperidinyl]siloxane; 1,2,3,4-butane-tetracarboxylic acid-1,2,3-tris(1,2,2,6,6-pentamethyl-4-piperidinyl)-4-tridecyl ester; α-methylstyrene-N-(2,2,6,6-tetramethyl-4-piperidinyl)maleimide and N-stearylmaleimide copolymer; 1,2,3,4-butanetetracarboxylic acid, β,β,β',β'-tetramethyl-2,4,8,10-tetramethyl- Polymer with laoxaspiro[5.5]undecane-3,9-diethanol, 1,2,2,6,6-pentamethyl-4-piperidinyl ester; Polymer with 2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diethanol, 1,2,3,4-butanetetracarboxylic acid, 2,2,6,6-tetramethyl-4-piperidinyl ester, β,β,β',β'-tetramethyl-; D-glucitol, 1,3:2,4-bis-o-(2,2,6,6-tetramethyl-4-piperidinylidene)-; 7-oxa-3,20-diaza Oligomers of dispiro[5.1.11.2]-heneicosan-21-one-2,2,4,4-tetramethyl-20-(oxiranylmethyl);Propanedioic acid, [(4-methoxyphenyl)methylene]-, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) ester;Formamide, N,N'-1,6-hexanediylbis[N-(2,2,6,6-tetramethyl-4-piperidinyl;1,3,5-triazine-2,4,6-triamine, N,N'''-[1,2-ethanediylbis[[[4,6-bis[butyl(1,2,2 ,6,6-pentamethyl-4-piperidinyl)amino]-1,3,5-triazin-2-yl]imino]-3,1-propanediyl]]-bis[N',N''-dibutyl-N',N''-bis(1,2,2,6,6-pentamethyl-4-piperidinyl);Poly[6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino];1,5-dioxaspiro(5.5)Undecane 3,3-dicarboxylic acid, bis(2,2,6,6-tetramethyl-4-piperidinyl) ester;1,5-dioxaspiro(5.5)Undecane 3,3-dicarboxylic acid, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) ester;N-2,2,6,6-tetramethyl-4-piperidinyl-N-amino-oxamide;4-acryloyloxy-1,2,2, 6,6-Pentamethyl-4-piperidine;1,5,8,12-Tetrakis[2',4'-bis(1'',2'',2'',6'',6''-pentamethyl-4''-piperidinyl(butyl)amino)-1',3',5'-triazin-6'-yl]-1,5,8,12-tetraazadodecane;3-Dodecyl-1-(2,2,6,6-tetramethyl-4-piperidyl)-pyrrolidine-2 ,5-dione;1,1'-(1,2-ethanediyl)-bis-(3,3',5,5'-tetramethylpiperazinone);1,1'1''-(1,3,5-triazine-2,4,6-triyltris((cyclohexylimino)-2,1-ethanediyl)tris(3,3,5,5-tetramethylpiperazinone);1,1',1''-(1,3,5-triazine-2,4,6-triyltris((cyclohexylimino)-2,1-ethanediyl)tris(3,3,5,5-tetramethylpiperazinone);1,1',1''-(1,3,5-triazine-2,4,6-tri Examples include polycondensates of dibutylamine 1,3,5-triazine·N,N-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine·N-(2,2,6,6-tetramethyl-4-piperidyl)butylamine. Among these, at least one selected from poly[6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino] (e.g., CHIMASSORB944FDL, manufactured by BASF) and a polycondensate of dibutylamine-1,3,5-triazine·N,N-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine·N-(2,2,6,6-tetramethyl-4-piperidyl)butylamine (e.g., CHIMASSORB2020FDL, manufactured by BASF) is preferred.
[0072] [Cyclic olefin polymer (n)] The cyclic olefin copolymer composition according to this embodiment may further contain a cyclic olefin polymer (n) different from the cyclic olefin copolymer (m). Specifically, the cyclic olefin polymer (n) contains at least one selected from a copolymer (n1) of ethylene or an α-olefin with a cyclic olefin and a ring-opening polymer (n2) of a cyclic olefin. The cyclic olefin copolymer composition according to the present embodiment contains the cyclic olefin polymer (n), and thus the dielectric properties of the crosslinked product obtained by crosslinking the cyclic olefin copolymer composition can be further improved. Here, the copolymer (n1) is a cyclic non-conjugated diene-derived copolymer represented by the general formula (III). In this embodiment, the fact that the copolymer (n1) does not contain a repeating unit derived from the cyclic non-conjugated diene represented by the general formula (III) means that the copolymer ( n1) is 100 mol %, the total number of moles of repeating units in the above general formula (III) This means that the content of repeating units derived from a cyclic non-conjugated diene represented by the following formula (I) is 0.05 mol % or less. When the total amount of the cyclic olefin copolymer (m) and the cyclic olefin polymer (n) contained in the cyclic olefin copolymer composition according to this embodiment is taken as 100% by mass, the content of the cyclic olefin copolymer (m) is from 5% by mass to 95% by mass, preferably from 10% by mass to 90% by mass, more preferably from 20% by mass to 80% by mass, and even more preferably from 25% by mass to 75% by mass, and the content of the cyclic olefin polymer (n) is from 5% by mass to 95% by mass, preferably from 10% by mass to 90% by mass, more preferably from 20% by mass to 80% by mass, and even more preferably from 25% by mass to 75% by mass.
[0073] As the copolymer (n1) of ethylene or an α-olefin and a cyclic olefin, for example, the polymers described in paragraphs 0030 to 0123 of WO 2008 / 047468 can be used.
[0074] For example, it is a polymer having an alicyclic structure in at least a portion of the repeating structural units (hereinafter, also simply referred to as a "polymer having an alicyclic structure"), and it is sufficient that at least a portion of the repeating units of the polymer has an alicyclic structure. Specifically, it is preferable to include a polymer having one or more structures represented by the following general formula (3).
[0075] [ka] (In formula (3), x and y represent a copolymerization ratio and are real numbers satisfying 0 / 100≦y / x≦95 / 5. x and y are on a molar basis. n represents the number of substituents Q and is a real number satisfying 0≦n≦2. R a is a 2+n valent group selected from the group consisting of hydrocarbon groups having 2 to 20 carbon atoms. R b is a hydrogen atom or a monovalent group selected from the group consisting of hydrocarbon groups having 1 to 10 carbon atoms. R c is a tetravalent group selected from the group consisting of hydrocarbon groups having 2 to 10 carbon atoms. Q is for COORd (R d is a hydrogen atom or a monovalent group selected from the group consisting of hydrocarbon groups having 1 to 10 carbon atoms. R a , R b , R c and Q may each be one type, or two or more types in any ratio.)
[0076] In addition, in the above general formula (3), R a is preferably one or more divalent groups selected from hydrocarbon groups having 2 to 12 carbon atoms, more preferably a divalent group represented by the following general formula (7) when n=0, and most preferably a divalent group in which p is 0 or 1 in the following general formula (7). a The structure may be used alone or in combination of two or more.
[0077] [ka] In the formula (7), p is an integer of 0 to 2.
[0078] The copolymer (n1) of ethylene or an α-olefin and a cyclic olefin is a cyclic olefin-based copolymer represented by the following general formula (4): For example, it comprises a structural unit (A) derived from ethylene or a linear or branched α-olefin having 3 to 30 carbon atoms, and a structural unit (B) derived from a cyclic olefin.
[0079] [ka] (In formula (4), R a is a divalent group selected from the group consisting of hydrocarbon groups having 2 to 20 carbon atoms. R b is a hydrogen atom or a monovalent group selected from the group consisting of hydrocarbon groups having 1 to 10 carbon atoms. R a and R bmay each be one type, or may contain two or more types in any ratio. x and y represent a copolymerization ratio and are real numbers satisfying 5 / 95≦y / x≦95 / 5, preferably 50 / 50≦y / x≦95 / 5, and more preferably 55 / 45≦y / x≦80 / 20. x and y are on a molar basis.
[0080] The copolymer (n1) of ethylene or α-olefin and cyclic olefin is preferably a copolymer of ethylene and cyclic olefin, and the cyclic olefin is preferably bicyclo[2.2.1]-2-heptene, tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene, 1,4-methano-1,4,4a,9a-tetrahydrofluorene, cyclopentadiene- Preferably, the compound is one or more selected from the group consisting of benzyne adducts and cyclopentadiene-acenaphthylene adducts, and more preferably, bicyclo[2.2.1]-2-heptene and tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene is more preferable. The copolymer (n1) of ethylene or an α-olefin and a cyclic olefin may be a polymer having one or more structures represented by the above general formula (3) or a polymer obtained by subjecting a cyclic olefin copolymer represented by the above general formula (4) to a hydrogenation treatment.
[0081] In addition, as the copolymer (n1) of ethylene or α-olefin and cyclic olefin, a copolymer of an α-olefin having 4 to 12 carbon atoms and a cyclic olefin is also preferred. As the copolymer of α-olefin and cyclic olefin, for example, those described in International Publication No. 2003 / 0133665 and International Publication No. 2003 / 0133665 are described. The polymers described in paragraphs 0056 to 0070 of No. 015 / 178145 can be used. Cyclic olefins that form copolymers of α-olefins with 4 to 12 carbon atoms and cyclic olefins Examples of the cyclic olefin include norbornene and substituted norbornene, and norbornene is preferred. The above cyclic olefins can be used alone or in combination of two or more.
[0082] The substituted norbornene is not particularly limited, and examples of the substituents of the substituted norbornene include halogen atoms and monovalent or divalent hydrocarbon groups. Specific examples of the substituted norbornene include those represented by the following general formula (A).
[0083] [ka] (In the formula, R 1 ~R 12 may be the same or different and are selected from the group consisting of a hydrogen atom, a halogen atom, and a hydrocarbon group; R 9 and R 10 , R 11 and R 12 may combine together to form a divalent hydrocarbon group, R 9 or R 10 And, R 11 or R 12 may form a ring together. n represents 0 or a positive integer, and when n is 2 or more, R 5 ~R 8 may be the same or different in each repeating unit. However, when n=0, R 1 ~R 4 and R 9 ~R 12 At least one of is not a hydrogen atom.)
[0084] The substituted norbornene represented by the general formula (A) will be described. R in the general formula (A) 1 ~R 12 may be the same or different and are selected from the group consisting of a hydrogen atom, a halogen atom, and a hydrocarbon group.
[0085] R 1 ~R 8Specific examples of the alkyl group include a hydrogen atom; a halogen atom such as fluorine, chlorine, or bromine; and an alkyl group having 1 to 20 carbon atoms, and these may be different from each other, may be partially different, or may be the same as one another.
[0086] Also, R 9 ~R 12 Specific examples of the alkyl group include a hydrogen atom; a halogen atom such as fluorine, chlorine, or bromine; an alkyl group having from 1 to 20 carbon atoms; a cycloalkyl group such as a cyclohexyl group; a substituted or unsubstituted aromatic hydrocarbon group such as a phenyl group, a tolyl group, an ethylphenyl group, an isopropylphenyl group, a naphthyl group, or an anthryl group; a benzyl group, a phenethyl group, or another aralkyl group in which an aryl group is substituted on an alkyl group, and the like. These may be different from each other, may be partially different, or may be the same in all.
[0087] R 9 and R 10 , or R 11 and R 12 Specific examples of the divalent hydrocarbon group formed by combining with each other include alkylidene groups such as an ethylidene group, a propylidene group, and an isopropylidene group.
[0088] R 9 or R 10 And, R 11 or R 12 When these rings form a ring, the ring formed may be a monocyclic ring or a polycyclic ring, a polycyclic ring having a bridge, a ring having a double bond, or a ring consisting of a combination of these rings. These rings may have a substituent such as a methyl group.
[0089] Specific examples of the substituted norbornene represented by the general formula (A) include 5-methyl-bicyclo[2.2.1]hept-2-ene, 5,5-dimethyl-bicyclo[2.2.1]hept-2-ene, 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-butyl-bicyclo[2.2.1]hept-2-ene, 5-ethylidene-bicyclo[2.2.1]hept-2-ene, 5-hexyl-bicyclo[2 .2.1]hept-2-ene, 5-octyl-bicyclo[2.2.1]hept-2-ene, 5-octadecyl-bicyclo[2.2.1]hept-2-ene, 5-methylidene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, 5-propenyl-bicyclo[2.2.1]hept-2-ene, and other two-ring cyclic olefins; tricyclo[4.3.0.1]hept-2-ene, 5-octyl-bicyclo[2.2.1]hept-2-ene, 5-octadecyl-bicyclo[2.2.1]hept-2-ene, 5-methylidene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, and 5-propenyl-bicyclo[2.2.1]hept-2-ene; 2,5 ]Deca-3,7-diene (common name: dicyclopentadiene), tricyclo[4.3.0.1 2,5 ]dec-3-ene; tricyclo[4.4.0.1 2,5 ]Undeca-3,7-diene or tricyclo[4.4.0.1 2,5 ]Undeca-3,8-diene or partially hydrogenated products thereof (or an adduct of cyclopentadiene and cyclohexene) 2,5 ]undec-3-ene; three-ring cyclic olefins such as 5-cyclopentyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexenyl-bicyclo[2.2.1]hept-2-ene, and 5-phenyl-bicyclo[2.2.1]hept-2-ene; tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene (also called tetracyclododecene), 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethyltetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-methylidenetetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethylidenetetracyclo[4.4.0.1 2,5 .17,10 ]dodec-3-ene, 8-vinyltetracyclo[4,4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-propenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, a 4-ring cyclic olefin; 8-cyclopentyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-cyclohexyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-cyclohexenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-phenyl-cyclopentyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene;tetracyclo[7.4.1 3,6 .0 1,9 .0 2,7 ]tetradeca-4,9,11,13-tetraene (also called 1,4-methano-1,4,4a,9a-tetrahydrofluorene), tetracyclo[8.4.1 4,7 .0 1,10 .0 3,8 ]Pentadeca-5,10,12,14-tetraene (also called 1,4-methano-1,4,4a,5,10,10a-hexahydroanthracene); Pentacyclo[6.6.1.1 3,6 .0 2,7 .0 9,14 ]-4-Hexadecene, Pentacyclo[6.5.1.1 3,6 .0 2,7 .0 9,13 ]-4-Pentadecene, Pentacyclo[7.4.0.0 2,7 .1 3,6 .1 10,13 ]-4-Pentadecene;Heptacyclo[8.7.0.1 2,9 .1 4,7 .1 11,17 .0 3,8 .0 12,16 ]-5-Eicosene, heptacyclo[8.7.0.1 2,9 .0 3,8 .1 4,7 .012,17 .1 13,l6 ]-14-eicosene; and polycyclic olefins such as a tetramer of cyclopentadiene.
[0090] Among these, alkyl-substituted norbornenes (e.g., bicyclo[2.2.1]hept-2-ene substituted with one or more alkyl groups) and alkylidene-substituted norbornenes (e.g., bicyclo[2.2.1]hept-2-ene substituted with one or more alkylidene groups) are preferred, and 5-ethylidene-bicyclo[2.2.1]hept-2-ene (common name: 5-ethylidene-2-norbornene, or simply ethylidenenorbornene) is particularly preferred.
[0091] A copolymer of an α-olefin having 4 to 12 carbon atoms and a cyclic olefin having 4 to 12 carbon atoms. Examples of the α-olefins having 4 to 12 carbon atoms include α-olefins having 4 to 12 carbon atoms and α-olefins having 4 to 12 carbon atoms and having at least one substituent such as a halogen atom. α-Olefins having prime numbers of 4 to 12 are preferred.
[0092] The α-olefin having 4 to 12 carbon atoms is not particularly limited, and examples thereof include 1-butene, 1-pentene, Examples of the ethylene glycol ether include ethylene glycol ether, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, and 1-dodecene. Among these, 1-hexene, 1-octene, and 1-decene are preferred.
[0093] The copolymer of an α-olefin having 4 to 12 carbon atoms and a cyclic olefin according to this embodiment is When the total number of repeating units contained in the copolymer is taken as 100 mol %, the ratio of repeating units derived from an α-olefin having 4 to 12 carbon atoms is preferably 10 mol % or more and 90 mol % or less. It is more preferably 15 mol % or more and 80 mol % or less, and further preferably 20 mol % or more and 70 mol % or less. In addition, the copolymerization of an α-olefin having 4 to 12 carbon atoms and a cyclic olefin according to this embodiment In the copolymer, when the total number of repeating units contained in the copolymer is taken as 100 mol %, the proportion of repeating units derived from cyclic olefins is preferably 10 mol % or more and 90 mol % or less, more preferably 20 mol % or more and 85 mol % or less, and even more preferably 30 mol % or more and 80 mol % or less.
[0094] A polymerization process for obtaining copolymers of α-olefins having 4 to 12 carbon atoms and cyclic olefins. The conditions for the above are not particularly limited as long as the desired copolymer is obtained, and known conditions can be used, with the polymerization temperature, polymerization pressure, polymerization time, etc. being appropriately adjusted.
[0095] As the cyclic olefin polymer (n), a ring-opening polymer (n2) of a cyclic olefin can be used. Examples of the ring-opening polymer (n2) of a cyclic olefin include a ring-opening polymer of a norbornene-based monomer, a ring-opening polymer of a norbornene-based monomer and another monomer capable of ring-opening copolymerization with the norbornene-based monomer, and hydrogenated products thereof.
[0096] Examples of norbornene monomers include bicyclo[2.2.1]hept-2-ene (common name: norbornene) and its derivatives (those having a substituent on the ring), tricyclo[4.3.01,6.12,5]deca-3,7-diene (common name: dicyclopentadiene) and its derivatives, 7,8-benzotricyclo[4.3.0.12,5]deca-3-ene (common name: methanotetrahydrofluorene, also known as 1,4-methano-1,4,4a,9a-tetrahydrofluorene) and its derivatives, tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene (common name: tetracyclododecene) and its derivatives, etc. The substituents on the rings of these derivatives include alkyl groups, alkylene groups, vinyl groups, alkoxycarbonyl groups, and alkylidene groups. The derivatives may have one or more substituents. Examples of derivatives having a substituent on the ring include 8-methoxycarbonyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-methyl-8-methoxycarbonyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethylidene-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene and the like. These norbornene monomers may be used alone or in combination of two or more.
[0097] A ring-opening polymer of a norbornene-based monomer, or a ring-opening polymer of a norbornene-based monomer and another monomer capable of ring-opening copolymerization therewith, can be obtained by polymerizing the monomer components in the presence of a known ring-opening polymerization catalyst. Examples of the ring-opening polymerization catalyst that can be used include catalysts consisting of a halide of a metal such as ruthenium or osmium, a nitrate or an acetylacetone compound, and a reducing agent; and catalysts consisting of a halide of a metal such as titanium, zirconium, tungsten, or molybdenum, or an acetylacetone compound, and an organoaluminum compound. Examples of other monomers capable of undergoing ring-opening copolymerization with norbornene monomers include monocyclic olefin monomers such as cyclohexene, cycloheptene, and cyclooctene.
[0098] A hydrogenated ring-opening polymer of a norbornene-based monomer or a hydrogenated ring-opening polymer of a norbornene-based monomer and another monomer capable of ring-opening copolymerization with the norbornene-based monomer can usually be obtained by adding a known hydrogenation catalyst containing a transition metal such as nickel or palladium to a polymerization solution of the ring-opening polymer and hydrogenating the carbon-carbon unsaturated bonds.
[0099] In the present embodiment, the cyclic olefin polymer (n) may be used alone or in combination of two or more kinds.
[0100] [Resins other than cyclic olefin polymers] The cyclic olefin copolymer composition according to this embodiment may further contain at least one selected from thermoplastic resins and thermosetting resins other than the cyclic olefin copolymer (m) and the cyclic olefin polymer (n), within the scope not impairing the object of this embodiment. The content of the resin other than the cyclic olefin polymer is preferably 1 part by mass or more and 50 parts by mass or less when the entire cyclic olefin copolymer composition is taken as 100 parts by mass. The resin other than the cyclic olefin polymer is not particularly limited as long as it is a thermoplastic resin or a thermosetting resin, but it is preferable that the resin contains one or more types selected from, for example, a styrene-based elastomer, an ethylene-propylene elastomer, and a diene-based elastomer.
[0101] Examples of styrene-based elastomers include styrene-conjugated diene block copolymer resins (conjugated dienes include butadiene, isoprene, etc.), hydrogenated styrene-conjugated diene block copolymer resins (conjugated dienes include butadiene, isoprene, etc.), styrene-conjugated diene-styrene triblock copolymer resins (conjugated dienes include butadiene, isoprene, etc.), and hydrogenated styrene-conjugated diene-styrene triblock copolymer resins (conjugated dienes include butadiene, isoprene, etc.). Examples of ethylene-propylene elastomers include ethylene-propylene rubber and ethylene-propylene-diene rubber. Examples of diene-based elastomers include polybutadiene, polyisoprene, styrene-butadiene rubber, butadiene rubber, isoprene rubber, chloroprene rubber, and acrylonitrile-butadiene rubber.
[0102] [Additives] The cyclic olefin copolymer composition according to the present embodiment may further contain various additives other than the hindered phenol (X) and the hindered amine compound (Y) depending on the purpose. The amount of the additive added is appropriately selected according to the application within a range that does not impair the purpose of the present embodiment. The additives include one or more additives selected from the group consisting of heat stabilizers, weather stabilizers, radiation resistance agents, plasticizers, lubricants, release agents, nucleating agents, friction and wear improvers, flame retardants, foaming agents, antistatic agents, colorants, antifogging agents, antiblocking agents, impact resistance agents, surface wetting improvers, fillers, hydrochloric acid absorbents, and metal deactivators. The cyclic olefin copolymer composition according to this embodiment may contain a heat stabilizer and a weather stabilizer other than the hindered phenol (X) and the hindered amine compound (Y) within a range that does not significantly impair the effects of this embodiment. The total content of the heat stabilizer and the weather stabilizer other than the hindered phenol (X) and the hindered amine compound (Y) is, for example, 1 mass % or less, preferably 0.5 mass % or less, more preferably 0.3 mass % or less, and particularly preferably 0.1 mass % or less, when the entire cyclic olefin copolymer composition is taken as 100 mass %.
[0103] Examples of the heat stabilizer include tris(2,4-di-tert-butylphenyl)phosphite, bis[2,4-bis(1,1-dimethylethyl)-6-methylphenyl]ethyl ester phosphorous acid, tetrakis(2,4-di-tert-butylphenyl)[1,1-biphenyl]-4,4'-diylbisphosphonite, and bis(2,4-di-t tert-butylphenyl)pentaerythritol diphosphite and other phosphite-based heat stabilizers; lactone-based heat stabilizers such as the reaction product of 3-hydroxy-5,7-di-tert-butyl-furan-2-one and o-xylene; 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(methylene-2,4,6-triyl)tri-p-cresol, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl)benzylbenzene, pentaerythritol tetrakis[3-(3,5-di- Examples of the heat stabilizer include hindered phenol-based heat stabilizers such as octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], sulfur-based heat stabilizers, and amine-based heat stabilizers. These may be used alone or in combination of two or more. Among these, phosphite-based heat stabilizers and hindered phenol-based heat stabilizers are preferred.
[0104] As the weather resistance stabilizer, one or more compounds selected from antioxidants, ultraviolet absorbents, etc. can be used.
[0105] Examples of the antioxidant include phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and thioether-based antioxidants.
[0106] Examples of the phenol-based antioxidant include acrylate-based phenol compounds described in JP-A-63-179953 and JP-A-1-168643, such as 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate and 2,4-di-t-amyl-6-(1-(3,5-di-t-amyl-2-hydroxyphenyl)ethyl)phenyl acrylate; 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-4-ethylphenol, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'- Methylene-bis(4-methyl-6-t-butylphenol), 4,4'-butylidene-bis (6-t-butyl-m-cresol), 4,4'-thiobis(3-methyl-6-t-butyl ethylphenol), bis(3-cyclohexyl-2-hydroxy-5-methylphenyl)methane, 3,9-bis(2-(3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tetrakis(methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenylpropionate)methane [i.e. That is, alkyl-substituted phenolic compounds such as pentaerythritol tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenylpropionate)], triethylene glycol bis(3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate), and tocopherol; 6-(4-hydroxy-3,5-di-t-butylanilino)-2,4-bisoctylthio-1,3,5-triazine, 6-(4-hydroxy-3,5-dimethylanilino)-2,4-bisoctylthio-1,3,5-triazine, triazine group-containing phenolic compounds such as octylthio-1,3,5-triazine, 6-(4-hydroxy-3-methyl-5-t-butylanilino)-2,4-bisoctylthio-1,3,5-triazine, and 2-octylthio-4,6-bis-(3,5-di-t-butyl-4-oxyanilino)-1,3,5-triazine; etc. Among these, acrylate-based phenolic compounds and alkyl-substituted phenolic compounds are preferred, and alkyl-substituted phenolic compounds are particularly preferred.
[0107] Examples of the phosphorus-based antioxidant include triphenyl phosphite, diphenyl isodecyl phosphite, phenyl diisodecyl phosphite, tris(nonylphenyl)phosphite, tris(dinonylphenyl)phosphite, tris(2,4-di-t-butylphenyl)phosphite, tris(2-t-butyl-4-methylphenyl)phosphite, tris(cyclohexylphenyl)phosphite, 2,2-methylenebis(4,6- monophosphite compounds such as di-t-butylphenyl)octyl phosphite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(3,5-di-t-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene; 4,4'-butylidene-bis( 3-Methyl-6-t-butylphenyl-di-tridecyl phosphite), 4,4'-iso Propylidene-bis(phenyl-di-alkyl(C12-C15) phosphite), 4,4'-isopropylidene-bis(diphenyl monoalkyl(C12-C15) phosphite) 1,1,3-tris(2-methyl-4-di-tridecylphosphite-5-t-butylphenyl)butane, tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenyl Examples of the diphosphite compounds include phenylene diphosphite, cyclic neopentane tetrayl bis(isodecyl phosphite), cyclic neopentane tetrayl bis(nonylphenyl phosphite), cyclic neopentane tetrayl bis(2,4-di-t-butylphenyl phosphite), cyclic neopentane tetrayl bis(2,4-dimethylphenyl phosphite), and cyclic neopentane tetrayl bis(2,6-di-t-butylphenyl phosphite). Among these, monophosphite compounds are preferred, and tris(nonylphenyl)phosphite, tris(dinonylphenyl)phosphite, and tris(2,4-di-t-butylphenyl)phosphite are particularly preferred.
[0108] Examples of the sulfur-based antioxidants include dilauryl 3,3-thiodipropionate, dimyristyl 3,3'-thiodipropionate, and distearyl 3,3-thiodipropionate. ester, laurylstearyl 3,3-thiodipropionate, pentaerythritol-tetrakis-(β-lauryl-thio-propionate), 3,9-bis(2-dodecylthioethyl)-2,4,8,10-tetraoxaspiro[5,5]undecane, and the like.
[0109] Examples of the thioether antioxidant include tetrakis{methylene-3-(laurylthio)propionate}methane, bis[methyl-4-{3-n-alkyl(C12 or C14)thiopropioniodyl}-5-t-butylphenyl]sulfide, and ditridecyl-3,3'-thiodipropionate.
[0110] Examples of the ultraviolet absorbing agent include benzophenone-based ultraviolet absorbing agents, salicylic acid-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, acrylate-based ultraviolet absorbing agents, and metal complex salt-based ultraviolet absorbing agents.
[0111] Examples of the benzophenone-based ultraviolet absorbers include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid trihydrate, 2-hydroxy-4-octyloxybenzophenone, 4-dodecaloxy-2-hydroxybenzophenone, 4-benzyloxy-2-hydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone.
[0112] Examples of the salicylic acid-based ultraviolet absorbers include phenyl salicylate, 4-t-butylphenyl-2-hydroxybenzoate, phenyl-2-hydroxybenzoate, 2,4-di-t-butylphenyl-3,5-di-t-butyl-4-hydroxybenzoate, and hexadecyl-3,5-di-t-butyl-4-hydroxybenzoate.
[0113] Examples of the benzotriazole-based ultraviolet absorbers include 2-(2-hydroxy-5-methylphenyl)-2H-benzotriazole, 2-(3-t-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)-2H-benzotriazole, and 5-chloro-2-(3,5-di-t-butyl- 2-Hydroxyphenyl)-2H-benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(2-hydroxy-5-t-octylphenyl)-2H-benzotriazole, 2-(2-hydroxy-4-octylphenyl)-2H-benzotriazole, 2-(2H-benzotriazol-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl)phenol, 2,2'-methylenebis[4-(1,1 ,3,3-tetramethylbutyl)-6-[(2H-benzotriazol-2-yl)phenol]], and the like.
[0114] Examples of the acrylate-based ultraviolet absorber include ethyl-2-cyano-3,3-diphenylacrylate, 2'-ethylhexyl-2-cyano-3,3-diphenylacrylate, Rates, etc.
[0115] As the metal complex salt-based ultraviolet absorber, a complex salt of nickel or cobalt is usually used. Specifically, nickel [2,2'-thiobis(4-t-octyl)phenolate] normal butylamine, nickel dibutyldithiocarbamate, nickel bis[o-ethyl-3,5-(di-t-butyl-4-hydroxybenzyl)]phosphate, cobalt dicyclohexyldithiophosphate, [1-phenyl, 3-methyl, 4-decanoyl, pyrazolate(5)2]nickel, and the like.
[0116] Examples of the radiation-resistant agent include rosin, rosin derivatives (for example, modified rosins such as hydrogenated rosin, disproportionated rosin, polymerized rosin, and modified rosin esters thereof), terpene resins, terpene phenol resins, aromatic modified terpene resins, hydrogenated terpene resins, aliphatic petroleum resins, aromatic petroleum resins, copolymerized petroleum resins, alicyclic petroleum resins, hydrogenated petroleum resins, and alkylphenol resins.
[0117] Examples of the plasticizer include phosphate triester plasticizers such as tricresyl phosphate, trixylyl phosphate, triphenyl phosphate, triethylphenyl phosphate, diphenyl cresyl phosphate, monophenyl dicresyl phosphate, dicresyl monoxylenyl phosphate, aryl alkyl phosphate, diphenyl monoxylenyl phosphate, morphophosphate, trioctyl phosphate, and tris(isopropylphenyl) phosphate; Examples of plasticizers include phthalate ester plasticizers such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diheptyl phthalate, di-n-octyl phthalate, di-2-ethylhexyl phthalate, diisononyl phthalate, octyldecyl phthalate, and butyl benzyl phthalate; fatty acid monobasic acid ester plasticizers such as butyl oleate and glycerin monooleate; dibutyl adipate and di-n-fatty acid dibasic acid ester plasticizers; dihydric alcohol ester plasticizers; and oxyacid ester plasticizers.
[0118] Examples of the lubricant include waxes, oils, capric acids, higher fatty acids such as lauric acid, myristic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, behenic acid, and the like, or metal salts thereof, i.e., lithium salts, calcium salts, sodium salts, magnesium salts, potassium salts, and the like, aliphatic alcohols such as palmityl alcohol, cetyl alcohol, stearyl alcohol, and the like, aliphatic amides such as caproic acid amide, caprylic acid amide, capric acid amide, lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, and the like, esters of fatty acids and alcohols, fluorine compounds such as fluoroalkyl carboxylic acids or metal salts thereof, and fluoroalkyl sulfonic acid metal salts. Examples of the above waxes include mineral waxes such as montan wax, peat wax, ozokerite, ceresin wax, and petroleum wax; polyolefin waxes such as polyethylene wax and polypropylene wax; synthetic waxes such as Fischer-Tropsch wax, chemically modified hydrocarbon wax, and substituted amide wax; vegetable waxes; and animal waxes. Examples of the oil agent include natural and synthetic oils such as aromatic oils, naphthenic oils, paraffinic oils, vegetable oils, silicone oils, etc. As the silicone oil, dimethylpolysiloxane having a viscosity of 10 to 5000 cSt, preferably 500 cSt, can be used.
[0119] Examples of the release agent include lower (C1-4) alcohol esters of higher fatty acids (butyl stearate, etc.), polyhydric alcohol esters of fatty acids (C4-30) (hydrogenated castor oil, etc.), glycol esters of fatty acids, and liquid paraffin.
[0120] Examples of the nucleating agent include sodium-2,2'-methylenebis(4,6-di-t- butylphenyl)phosphate, [phosphate-2,2'-methylenebis(4,6-di-t- butylphenyl)]dihydroxyaluminum, bis[2,2'-methylenebisphosphate Tris[(4,6-di-t-butylphenyl)]hydroxide aluminum, tris[2,2'-methylenebis(4,6-di-t-butylphenyl)]aluminum, sodium Mu-bis(4-t-butylphenyl)phosphate, metal salts of benzoic acid such as sodium benzoate, aluminum pt-butylbenzoate, 1,3:2,4-bis(O-benzylidene)sorbitol, 1,3:2,4-bis(O-methylbenzylidene)sorbitol, 1,3:2,4-bis(O-ethylbenzylidene)sorbitol, 1,3-O-3,4-dimethylbenzylidene-2,4-O-benzylidene sorbitol, 1,3-O-benzylidene -2,4-O-3,4-dimethylbenzylidene sorbitol, 1,3:2,4-bis(O-3,4-dimethylbenzylidene)sorbitol, 1,3-Op-chlorobenzylidene-2,4-O-3,4-dimethylbenzylidene sorbitol, 1,3-O-3,4-dimethylbenzylidene-2,4-Op-chlorobenzylidene sorbitol, 1,3:2,4-bis(Op-chlorobenzylidene)sorbitol, and mixtures thereof.
[0121] Examples of the friction and wear improver include resin fillers such as ultra-high molecular weight polyethylene filler, PTFE filler, and polyimide filler, and inorganic fillers such as boron nitride filler and aluminum nitride filler.
[0122] As the flame retardant, for example, a halogen-based flame retardant, a phosphorus-based flame retardant, a nitrogen-containing flame retardant, or an antimony-based flame retardant can be used. As the halogen-based flame retardant, various chlorine-based and bromine-based flame retardants can be used. From the standpoints of flame retardancy, heat resistance during molding, dispersibility in resin, effect on the physical properties of resin, etc., the following are preferred: pentabromodiphenyl ether, octabromodiphenyl ether, decabromodiphenyl ether, tetrabromobisphenol A, hexabromocyclododecane, hexabromobenzene, pentabromoethylbenzene, hexabromobiphenyl, decabromodiphenyl, hexabromodiphenyl oxide, octabromodiphenyl oxide , decabromodiphenyl oxide, pentabromocyclohexane, tetrabromobisphenol A and its derivatives [e.g., tetrabromobisphenol A-bis(hydroxyethyl ether), tetrabromobisphenol A-bis(2,3-dibromopropyl ether), tetrabromobisphenol A-bis(bromoethyl ether), tetrabromobisphenol A-bis(allyl ether), etc.], tetrabromobisphenol S and its derivatives [e.g., tetrabromobisphenol S-bis(hydroxyethyl ether), diethyl ether), tetrabromobisphenol S-bis(2,3-dibromopropyl ether), etc.], tetrabromophthalic anhydride and its derivatives [e.g., tetrabromophthalimide, ethylene bistetrabromophthalimide, etc.], ethylene bis(5,6-dibromonorbornene-2,3-dicarboximide), tris-(2,3-dibromopropyl-1)-isocyanurate, adducts of Diels-Alder reaction of hexachlorocyclopentadiene, tribromophenyl glycidyl ether, tribromophenyl It is preferable to use brominated flame retardants such as acrylate, ethylene bistribromophenyl ether, ethylene bispentabromophenyl ether, tetradecabromodiphenoxybenzene, brominated polystyrene, brominated polyphenylene oxide, brominated epoxy resin, brominated polycarbonate, polypentabromobenzyl acrylate, octabromonaphthalene, hexabromocyclododecane, bis(tribromophenyl)fumaramide, and N-methylhexabromodiphenylamine; or chlorinated flame retardants such as chlorinated paraffin.
[0123] Examples of the phosphorus-based flame retardant include halogen-containing phosphate ester flame retardants such as tris(chloroethyl)phosphate, tris(2,3-dichloropropyl)phosphate, tris(2-chloropropyl)phosphate, tris(2,3-bromopropyl)phosphate, tris(bromochloropropyl)phosphate, 2,3-dibromopropyl-2,3-chloropropyl phosphate, tris(tribromophenyl)phosphate, tris(dibromophenyl)phosphate, and tris(tribromoneopentyl)phosphate; aliphatic phosphate esters such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, and tributoxyethyl phosphate; non-halogen-based phosphate ester flame retardants such as aromatic phosphate esters such as phenyl phosphate, cresyl diphenyl phosphate, dicresyl phenyl phosphate, tricresyl phosphate, trixylenyl phosphate, xylenyl diphenyl phosphate, tri(isopropylphenyl)phosphate, isopropylphenyl diphenyl phosphate, diisopropylphenyl phosphate, tri(trimethylphenyl)phosphate, tri(t-butylphenyl)phosphate, hydroxyphenyl diphenyl phosphate, and octyl diphenyl phosphate; and aluminum phosphinate-based flame retardants such as aluminum dimethylphosphinate and aluminum diethylphosphinate. Examples of the nitrogen-containing flame retardants include melamine cyanurate, isocyanuric acid, tris(2-hydroxyethyl)isocyanurate, triallyl isocyanurate, tris(2,3-epoxypropyl)isocyanurate, guanidine hydrochloride, guanidine nitrate, guanidine phosphate, guanidine sulfate, guanidine sulfamate, guanidine tetraborate, guanidine carbonate, guanylurea phosphate, guanylurea sulfate, melamine, melamine melam melem, melamine cyanurate, melamine phosphate, melamine pyrophosphate, melamine polyphosphate, melamine melam melem polyphosphate, melamine sulfate, and the like. Examples of the antimony-based flame retardants include antimony oxide, antimony trioxide, antimony pentoxide, antimony tetroxide, and sodium antimonate.
[0124] As the foaming agent, a wide variety of foaming agents generally used in foam molding of rubber can be used. Specifically, inorganic foaming agents such as sodium bicarbonate, sodium carbonate, ammonium bicarbonate, ammonium carbonate, and ammonium nitrite; nitrite foaming agents such as N,N'-dimethyl-N,N'-dinitrosoterephthalamide and N,N'-dinitrosopentamethylenetetramine; azo compounds such as azodicarbonamide, azobisisobutyronitrile, azocyclohexylnitrile, azodiaminobenzene, and barium azodicarboxylate; benzenesulfonyl hydrazide, toluenesulfonyl hydrazide, and p,p'-oxybis( Benzenesulfonylhydrazide), Diphenylsulfone-3,3'-disulfonylhydrazide and azide compounds such as calcium azide, 4,4-diphenyl disulfonyl azide, and p-toluenesulfonyl azide.
[0125] Examples of the antistatic agent and antifogging agent include cationic surfactants, anionic surfactants, amphoteric surfactants, and nonionic surfactants.
[0126] Examples of the cationic surfactant include tetraalkylammonium salts such as lauryltrimethylammonium chloride and stearyltrimethylammonium chloride.
[0127] Examples of the anionic surfactant include sodium decane sulfonate, sodium indecane sulfonate, sodium dodecane sulfonate, sodium tridecane sulfonate, sodium tetradecane sulfonate, sodium pentadecane sulfonate, sodium hexadecanesulfonate, sodium heptadecanesulfonate, sodium octadecanesulfonate, sodium nonadecanesulfonate, sodium heicosane sulfonate, potassium decane sulfonate, potassium undecanesulfonate, potassium dodecanesulfonate, potassium tridecanesulfonate, potassium tetradecanesulfonate, potassium pentadecanesulfonate, and potassium hexadecanesulfonate. Examples of the alkyl benzene sulfonates include potassium benzoate, potassium heptadecanesulfonate, potassium octadecanesulfonate, potassium nonadecanesulfonate, and potassium heicosane deca sulfonate; alkyl benzene sulfonates such as sodium decylbenzenesulfonate, sodium undecylbenzenesulfonate, sodium dodecylbenzenesulfonate, sodium tridecylbenzenesulfonate, sodium tetradecylbenzenesulfonate, sodium pentadecylbenzenesulfonate, sodium hexadecylbenzenesulfonate, sodium heptadecylbenzenesulfonate, and sodium octadecylbenzenesulfonate; and alkyl phosphates.
[0128] Examples of the amphoteric surfactant include betaine compounds such as lauryl betaine, stearyl betaine, lauryl amidopropyl betaine, and stearyl amidopropyl betaine; dimethylamine oxide compounds such as lauryl dimethylamine oxide and stearyl dimethylamine oxide; and alanine compounds such as N-stearyl-α-alaninate and N-lauryl-α-alaninate.
[0129] Examples of the nonionic surfactant include monoglyceride laurate, monoglyceride palmitate, monoglyceride stearate, monoglyceride oleate, monoglyceride behenate, monoglyceride caprylate, monoglyceride coconut fatty acid, diglyceride laurate, diglyceride palmitate, diglyceride stearate, diglyceride oleate, diglyceride behenate, diglyceride caprylate, diglyceride coconut fatty acid, triglyceride laurate, triglyceride palmitate, triglyceride stearate, triglyceride oleate, triglyceride behenate, triglyceride caprylate, triglyceride coconut fatty acid, pentaerythritol monolaurate, pentaerythritol Examples of the fatty acid esters of pentaerythritol include fatty acid esters of pentaerythritol such as pentaerythritol monostearate, pentaerythritol dilaurate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate, and pentaerythritol tetralaurate; fatty acid esters of sorbitol, sorbitol monolaurate, sorbitol monostearate, and sorbitol; fatty acid esters of polyhydric alcohols such as polyethylene glycol monolaurate, polyethylene glycol monostearate, polyethylene glycol monooleate, and polyethylene glycol distearate; and diethanolamides such as lauric acid diethanolamide, stearic acid diethanolamide, and coconut fatty acid diethanolamide.
[0130] As the colorant, for example, various natural and synthetic dyes and various inorganic and organic pigments can be arbitrarily used.
[0131] Examples of the antiblocking agent include fine particle inorganic compounds such as silica, alumina, alumina silicate, and diatomaceous earth, and fine particle organic compounds such as polyethylene, crosslinked polyethylene, polymethyl methacrylate, and crosslinked polymethyl methacrylate.
[0132] As the impact-resistant agent, various agents can be used, such as a (meth)acrylic acid ester-based impact-resistant agent having a core-shell structure.
[0133] Examples of the surface wettability improver include vinyltrimethoxysilane, 3-glycidoxy Examples of the silane coupling agent include silane coupling agents such as propyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-aminopropyltrimethoxysilane.
[0134] Examples of the filler include inorganic fillers and organic fillers. Examples of the inorganic filler include silica, diatomaceous earth, alumina, titanium oxide, magnesium oxide, pumice powder, pumice balloon, aluminum hydroxide, magnesium hydroxide, basic magnesium carbonate, dolomite, calcium sulfate, potassium titanate, barium sulfate, calcium sulfite, talc, clay, mica, asbestos, calcium silicate, montmorillonite, bentonite, graphite, aluminum powder, molybdenum sulfide, etc. These may be used alone or in combination of two or more.
[0135] Examples of the organic filler include starch and its derivatives, cellulose and its derivatives, pulp and its derivatives, paper and its derivatives, wheat flour, soybean pulp pulp, bran, coconut shells, coffee grounds, protein, low molecular weight substances such as phthalic acid, aliphatic polybasic acid, glycerin, citric acid, glycol, and olefin, polyethylene terephthalate fiber, polyethylene naphthalate fiber, and aramid fiber.
[0136] The hydrochloric acid absorbent may be, for example, a higher fatty acid metal salt. Specific examples include sodium stearate, magnesium stearate, calcium stearate, zinc stearate, lithium stearate, barium stearate, aluminum stearate, sodium 12-hydroxystearate, calcium 12-hydroxystearate, magnesium 12-hydroxystearate, zinc 12-hydroxystearate, etc. In addition, examples include epoxy compounds such as epoxidized octyl stearate and epoxidized soybean oil; and inorganic compounds such as magnesium hydroxide, calcium hydroxide, and hydrotalnites.
[0137] Examples of the metal deactivator include N,N'-diphenyloxamide, N-salicide, Ral-N'-salicyloylhydrazine, N,N'-bis(salicyloyl)hydrazine, N,N'-bis(3,5-di-t-butyl-4-hydroxyphenylpropionyl)hydrazine Examples of such compounds include 3-salicyloylamino-1,2,4-triazole, bis(benzylidene)oxalyl dihydrazide, oxanilide, isophthaloyl dihydrazide, sebacoyl bisphenylhydrazide, N,N'-bis(salicyloyl)oxalyl dihydrazide, and N,N'-bis(salicyloyl)thiopropionyl dihydrazide.
[0138] [Method for preparing cyclic olefin copolymer composition] The cyclic olefin copolymer composition according to the present embodiment can be prepared by mixing the cyclic olefin copolymer (m), the hindered phenol (X), the hindered amine compound (Y), and, if necessary, the cyclic olefin polymer (n), the elastomer, and various additives. As a mixing method, a melt blending method using an extruder or the like, or a solution blending method in which the composition is dissolved and dispersed in a suitable solvent, for example, saturated hydrocarbons such as heptane, hexane, decane, and cyclohexane; aromatic hydrocarbons such as toluene, benzene, and xylene, can be adopted.
[0139] [varnish] The cyclic olefin copolymer composition according to this embodiment can be made into a varnish by mixing with a solvent. The solvent for preparing the varnish is not particularly limited as long as it does not impair the solubility or affinity of the cyclic olefin copolymer (m), the hindered phenol (X) and the hindered amine compound (Y).Preferably used solvents include, for example, saturated hydrocarbons such as heptane, hexane, octane, and decane; alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, and decahydronaphthalene; aromatic hydrocarbons such as toluene, benzene, xylene, mesitylene, and pseudocumene; alcohols such as methanol, ethanol, isopropyl alcohol, butanol, pentanol, hexanol, propanediol, and phenol; ketone solvents such as acetone, methyl isobutyl ketone, methyl ethyl ketone, pentanone, hexanone, cyclohexanone, isophorone, and acetophenone; cellosolves such as methyl cellosolve and ethyl cellosolve; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl propionate, and butyl formate; and halogenated hydrocarbons such as trichloroethylene, dichloroethylene, and chlorobenzene. Preferably, heptane, decane, cyclohexane, methylcyclohexane, decahydronaphthalene, toluene, benzene, xylene, mesitylene, and pseudocumene are used. These solvents can be used alone or in combination of two or more in any ratio.
[0140] In this embodiment, the method for preparing the varnish may be carried out by any method, but usually includes a step of mixing the cyclic olefin copolymer composition and the solvent. The mixing order of each component is not limited, and it can be carried out in any manner, such as all at once or in portions. There is also no limitation on the apparatus for preparing the varnish, and it may be carried out by any apparatus capable of stirring and mixing, such as a batch type or a continuous type. The temperature when preparing the varnish can be selected arbitrarily within the range from room temperature to the boiling point of the solvent. The reaction solution obtained when the cyclic olefin copolymer (m) is obtained may be used as a solvent and the hindered phenol (X) and the hindered amine compound (Y) may be dissolved therein to prepare a varnish. Alternatively, the varnish may be prepared by mixing a separately prepared varnish of the hindered amine compound (Y) with the reaction solution obtained when the cyclic olefin copolymer (m) is obtained.
[0141] [Method for producing the crosslinked body (Q)] The crosslinked body (Q) is the crosslinked body of the cyclic olefin copolymer composition according to the present embodiment, and is obtained by crosslinking the cyclic olefin copolymer (m) in the above-mentioned cyclic olefin copolymer composition.The crosslinking method of the cyclic olefin copolymer (m) is not particularly limited, and may be, for example, a method of crosslinking while or after molding into any shape by using a radical polymerization initiator, sulfur, a hydrosilyl group-containing compound, electron beam or other radiation.
[0142] Crosslinking with a radical polymerization initiator can be performed by the same method as that used for polyolefins. That is, a radical polymerization initiator such as dicumyl peroxide is mixed into the cyclic olefin copolymer composition, and the mixture is heated and crosslinked. The mixing ratio of the radical polymerization initiator is not particularly limited, but is usually 0.02 to 20 parts by mass, preferably 0.05 to 10 parts by mass, and more preferably 0.5 to 10 parts by mass per 100 parts by mass of the cyclic olefin copolymer (m). When the mixing ratio of the radical polymerization initiator is equal to or less than the upper limit, the dielectric properties of the crosslinked body (Q) are improved, and when the mixing ratio is equal to or more than the lower limit, the heat resistance and mechanical properties of the crosslinked body (Q) can be improved.
[0143] The radical polymerization initiator may be a known thermal radical polymerization initiator, a photoradical polymerization initiator, or a combination of these. When using a thermal radical polymerization initiator among these radical polymerization initiators, the initiator has a 10-hour half-life temperature of usually 80° C. or higher, preferably 120° C. or higher, from the viewpoint of storage stability. Examples of such initiators include dialkyl peroxides such as dicumyl peroxide, t-butylcumyl peroxide, 2,5-bis(t-butylperoxy)2,5-dimethylhexane, 2,5-bis(t-butylperoxy)2,5-dimethylhexyne-3, di-t-butyl peroxide, isopropylcumyl-t-butyl peroxide, and bis(α-t-butylperoxyisopropyl)benzene; 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclododecane, n-butyl-4,4-bis(t-butylperoxy)valerate, and ethyl-3,3-bis(t-butylperoxy). peroxy ketals such as bis(t-butylperoxy)isophthalate, t-butyl peroxybenzoate, t-butyl peroxyacetate, etc.; hydroperoxides such as t-butyl hydroperoxide, t-hexyl hydroperoxide, cumin hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, diisopropylbenzene hydroperoxide, p-menthane hydroperoxide, etc.; bibenzyl compounds such as 2,3-dimethyl-2,3-diphenylbutane, etc.; 3,3,5,7,7-pentamethyl-1,2,4-trioxepane, etc.
[0144] Among the radical polymerization initiators, specific examples of the photoradical polymerization initiator include benzoin alkyl ether, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzophenone, methylbenzoyl formate, isopropyl thioxanthone, and mixtures of two or more of these. In addition, a sensitizer can be used together with these photoradical polymerization initiators. Examples of the sensitizer include anthraquinone, 1,2-naphthoquinone, 1,4-naphthoquinone, benzanthrone, and p,p'-tetramethyldiaminobenzophenone. Examples of suitable organic solvents include carbonyl compounds such as chloranil, nitro compounds such as nitrobenzene, p-dinitrobenzene, and 2-nitrofluorene, aromatic hydrocarbons such as anthracene and chrysene, sulfur compounds such as diphenyl disulfide, and nitrogen compounds such as nitroaniline, 2-chloro-4-nitroaniline, 5-nitro-2-aminotoluene, and tetracyanoethylene.
[0145] When crosslinking with sulfur or the like, a sulfur-based compound, and if necessary, a vulcanization accelerator and a vulcanization acceleration aid are mixed into the cyclic olefin copolymer composition, and heated to carry out a crosslinking reaction. The amount of the sulfur-based compound is not particularly limited, but it is usually used in the range of 0.1 to 10 parts by mass, preferably 0.3 to 5 parts by mass, per 100 parts by mass of the cyclic olefin copolymer (m) in order to efficiently proceed with the crosslinking reaction, improve the physical properties of the crosslinked product obtained, and from the economical standpoint, and when a vulcanization accelerator or a vulcanization acceleration aid is used in combination, it is usually used in the range of 0.1 to 20 parts by mass, preferably 0.2 to 10 parts by mass. Various known sulfur-based compounds can be used to cause the crosslinking reaction, and examples thereof include sulfur, sulfur monochloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dimethyldithiocarbamate. Various vulcanization accelerators can also be used, including thiazole-based accelerators such as N-cyclohexyl-2-benzothiazole-sulfenamide, N-oxydiethylene-2-benzothiazole-sulfenamide, N,N-diisopropyl-2-benzothiazole-sulfenamide, 2-mercaptobenzothiazole, 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-diethyl-4-morpholinothio)benzothiazole, and benzothiazyl-disulfide; guanidine-based accelerators such as diphenylguanidine, triphenylguanidine, di-ortho-tolylguanidine, ortho-tolyl biguanide, and diphenylguanidine phthalate; acetaldehyde-aniline reaction products; butyraldehyde-aniline condensates; aldehyde amines such as hexamethylenetetramine and acetaldehyde ammonia; and aldehyde-ammonia. ammonium-based compounds; imidazoline-based compounds such as 2-mercaptoimidazoline; thiourea-based compounds such as thiocarbanilide, diethylthiourea, dibutylthiourea, trimethylthiourea, and diorthothylthiourea; thiuram-based compounds such as tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, and dipentamethylenethiuram tetrasulfide; dithioacid salt-based compounds such as zinc dimethyldithiocarbamate, zinc diethylthiocarbamate, zinc di-n-butyldithiocarbamate, zinc ethylphenyldithiocarbamate, zinc butylphenyldithiocarbamate, sodium dimethyldithiocarbamate, selenium dimethyldithiocarbamate, and tellurium diethyldithiocarbamate; and xanthate-based compounds such as zinc dibutylxanthogenate.Examples of vulcanization accelerators include metal oxides such as zinc oxide, active zinc oxide, zinc carbonate, complex zinc oxide, magnesium oxide, litharge, red lead, and basic lead carbonate; fatty acid compounds such as stearic acid, oleic acid, lauric acid, and lead stearate; and organic amines and glycols such as triethanolamine and diethylene glycol.
[0146] The temperature for crosslinking the cyclic olefin copolymer composition with both radical polymerization initiator crosslinking and sulfur crosslinking is usually 100 to 300°C, preferably 120 to 250°C, more preferably 120 to 220°C, and the temperature may be changed stepwise to perform crosslinking. If the temperature is equal to or higher than the lower limit, crosslinking can be sufficiently advanced. If the temperature is equal to or lower than the upper limit, coloring of the crosslinked body obtained can be suppressed and the process can be simplified. For reference, polybutadiene, which is a typical double bond-containing polymer, generally cannot be crosslinked under the above conditions and requires crosslinking conditions at a high temperature such as 300°C.
[0147] The cyclic olefin copolymer composition according to the present embodiment can also be crosslinked using a hydrosilyl group-containing compound having at least two hydrosilyl groups in one molecule. Crosslinking using a hydrosilyl group-containing compound can be carried out, for example, according to the method described in JP-A-2015-193680. Details are omitted here.
[0148] The method of crosslinking using electron beams or other radiation has the advantage that there are no restrictions on temperature or fluidity during molding, and examples of radiation include electron beams, gamma rays, UV rays, and the like.
[0149] In any of the methods using a radical polymerization initiator, sulfur, a hydrosilyl group-containing compound, etc., and the method using radiation, crosslinking can be carried out in the presence of a crosslinking assistant.
[0150] The crosslinking agent is not particularly limited, but examples thereof include p-quinonedioxime, p,p'-dibenzyl oximes such as benzoylquinone dioxime; acrylates or methacrylates such as ethylene dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, cyclohexyl methacrylate, acrylic acid / zinc oxide mixture, and allyl methacrylate; vinyl monomers such as divinylbenzene, vinyltoluene, and vinylpyridine; allyl compounds such as hexamethylenediallylnadimide, diaryl itaconate, diallyl phthalate, diallyl isophthalate, diallyl monoglycidyl isocyanurate, triallyl cyanurate, and triallyl isocyanurate; N,N'-m Examples of the crosslinking aid include maleimide compounds such as N,N'-(4,4'-methylenediphenylene)dimaleimide, and cyclic non-conjugated dienes such as vinylnorbornene, ethylidenenorbornene, and dicyclopentadiene. These crosslinking aids may be used alone or in combination.
[0151] The crosslinking reaction can be carried out by using a mixture of the cyclic olefin copolymer composition and the above-mentioned radical polymerization initiator, sulfur, hydrosilyl group-containing compound, or the like in a molten state, or by using the mixture in a solution state in which the mixture is dissolved or dispersed in a solvent, or by volatilizing the solvent from the solution state in which the mixture is dissolved in a solvent, forming the mixture into any desired shape such as a film or coating, and then allowing the crosslinking reaction to proceed further.
[0152] When the reaction is carried out in a molten state, the mixture of raw materials is melt-kneaded and reacted using a kneading device such as a mixing roll, a Banbury mixer, an extruder, a kneader, a continuous mixer, etc. In addition, the crosslinking reaction can be further carried out after molding by any method.
[0153] When the reaction is carried out in a solution state, the same solvents as those used in the above solution blending method can be used as the solvent.
[0154] When the crosslinking reaction is carried out using electron beams, other radiation, or UV, the reaction can be carried out after shaping by any method.
[0155] [Film or sheet] The crosslinked product of the cyclic olefin copolymer composition according to this embodiment can be formed into a film or sheet and used for various applications. Various known methods can be applied as a method for forming a film or sheet using the cyclic olefin copolymer composition according to this embodiment. For example, a method of forming the film or sheet by applying the above-mentioned varnish to a supporting substrate such as a thermoplastic resin film, drying, and then performing a heat treatment or the like to crosslink the cyclic olefin copolymer composition can be mentioned. The method of applying the varnish to the supporting substrate is not particularly limited, and examples thereof include application using a spin coater, application using a spray coater, and application using a bar coater. Another example is a method in which the cyclic olefin copolymer composition according to this embodiment is melt molded to obtain a film or sheet.
[0156] [Laminate] The film or sheet according to this embodiment can be laminated on a substrate to form a laminate for various applications. As a method for forming the laminate according to this embodiment, various known methods can be applied. For example, a laminate can be produced by laminating the film or sheet produced by the above-mentioned method onto a substrate, and, if necessary, heat curing the laminate by a press or the like. Furthermore, a laminate can be produced by laminating an electrical insulating layer containing the above-mentioned crosslinked body onto a conductor layer.
[0157] [Multi-layer molded body or multi-layer laminated film] The cyclic olefin copolymer composition according to the present embodiment may be formed on the surface layer of various multi-layer molded articles or multi-layer laminated films. In this case, the resin layer formed by the cyclic olefin copolymer composition is preferably 100 μm or less. Examples of various multilayer molded articles or multilayer laminated films include a multilayer molded article for an optical lens in which the cyclic olefin copolymer composition according to this embodiment is formed on the surface of a resin optical lens, and a multilayer gas barrier film in which the cyclic olefin copolymer composition according to this embodiment is formed on the surface of a resin film such as a PET film or a PE film to impart gas barrier properties.
[0158] [Prepreg] The prepreg according to the present embodiment is formed by combining the cyclic olefin copolymer composition according to the present embodiment with a sheet-like fiber substrate. The method for producing the prepreg is not particularly limited, and various known methods can be applied. For example, there is a method including a step of impregnating a sheet-like fiber substrate with the above-mentioned varnish to obtain an impregnated body, and a step of heating the obtained impregnated body to dry the solvent contained in the above-mentioned varnish. The above-mentioned varnish can be impregnated into the sheet-like fiber substrate by, for example, applying a predetermined amount of varnish to the sheet-like fiber substrate by a known method such as spray coating, dip coating, roll coating, curtain coating, die coating, or slit coating, and, if necessary, placing a protective film on top of it and pressing from above with a roller or the like. The process of heating the impregnated body and drying the solvent contained in the varnish is not particularly limited, but examples of the process include drying in air or nitrogen using a blower dryer in a batch process, or drying by passing through a heating furnace in a continuous process. In this embodiment, after the varnish is impregnated into the sheet-like fiber substrate, the obtained impregnated body is heated to a predetermined temperature, whereby the solvent contained in the varnish evaporates and a prepreg is obtained.
[0159] The fibers constituting the sheet-like fiber substrate according to this embodiment can be inorganic and / or organic fibers, and are not particularly limited. For example, organic fibers such as PET (polyethylene terephthalate) fibers, aramid fibers, ultra-high molecular weight polyethylene fibers, polyamide (nylon) fibers, and liquid crystal polyester fibers; inorganic fibers such as glass fibers, carbon fibers, alumina fibers, tungsten fibers, molybdenum fibers, titanium fibers, steel fibers, boron fibers, silicon carbide fibers, and silica fibers; and the like can be mentioned. Among these, organic fibers and glass fibers are preferred, and aramid fibers, liquid crystal polyester fibers, and glass fibers are particularly preferred. Examples of glass fibers include E glass, NE glass, S glass, D glass, H glass, and T glass. The impregnation of the sheet-like fiber substrate with the varnish is carried out, for example, by immersion and coating. The impregnation may be repeated multiple times as necessary. These sheet-like fiber substrates can be used alone or in combination of two or more, and the amount used is selected appropriately as desired, but is usually in the range of 10 to 90 mass%, preferably 20 to 80 mass%, and more preferably 30 to 70 mass% in the prepreg or laminate. If it is in this range, the dielectric properties and mechanical strength of the obtained laminate are highly balanced, which is preferable.
[0160] The thickness of the prepreg according to the present embodiment is appropriately selected depending on the purpose of use, but is usually 0.001 to 10 mm, preferably 0.005 to 1 mm, and more preferably 0.01 to 0.5 mm. This range is preferable because it allows the shapeability during lamination and the properties such as mechanical strength and toughness of the laminate obtained by curing to be fully exhibited.
[0161] [Metal-clad laminate] The film, sheet, laminate or prepreg according to this embodiment may be formed into a metal-clad laminate by laminating a metal foil on at least one surface thereof and heat-curing it using a lamination press or the like. Examples of the metal foil include copper foil, aluminum foil, nickel foil, gold foil, silver foil, and stainless steel foil. The metal-clad laminate of this embodiment can be produced by various known methods. For example, a metal-clad laminate can be produced by laminating a metal foil onto the film, sheet, laminate or prepreg according to this embodiment, and, if necessary, heat curing the laminate using a press or the like.
[0162] The metal-clad laminate of this embodiment uses the cyclic olefin copolymer composition of this embodiment, and therefore has excellent heat aging resistance while satisfying dielectric properties suitable for printed wiring boards. Therefore, the metal-clad laminate according to this embodiment can be suitably used as an insulating layer material for printed wiring boards.
[0163] [Printed wiring board] The cyclic olefin copolymer composition according to this embodiment has excellent dielectric properties, heat resistance, mechanical properties, and the like, and therefore can be suitably used for printed wiring boards. The method for producing a printed wiring board can be a generally known method, and is not particularly limited. For example, the film, sheet, laminate, or prepreg produced by the above-mentioned method is heated and cured by a lamination press or the like to form an electrical insulating layer. Next, a conductor layer is laminated on the obtained electrical insulating layer by a known method to produce a laminate. Thereafter, the conductor layer in the laminate is subjected to circuit processing or the like to obtain a printed wiring board.
[0164] Metals that can be used for the conductor layer include metals such as copper, aluminum, nickel, gold, silver, stainless steel, etc. Methods for forming the conductor layer include, for example, a method in which the metal is made into a foil or the like and heat-fused onto the electrical insulating layer, a method in which the metal is made into a foil or the like and attached to the electrical insulating layer using an adhesive, or a method in which a conductor layer made of the metal is formed on the electrical insulating layer by a method such as sputtering, vapor deposition, plating, etc. The printed wiring board may be either a single-sided board or a double-sided board.
[0165] Such a printed wiring board can be used as an electronic device by mounting electronic components such as semiconductor elements, etc. Electronic devices can be manufactured based on publicly known information. Examples of such electronic devices include ICT infrastructure equipment such as servers, routers, supercomputers, mainframes, and workstations; antennas such as GPS antennas, antennas for wireless base stations, millimeter-wave antennas, and RFID antennas; communication devices such as mobile phones, smartphones, PHS, PDAs, and tablet terminals; digital devices such as personal computers, televisions, digital cameras, digital video cameras, POS terminals, wearable terminals, and digital media players; on-vehicle electronic devices such as electronic control system devices, on-vehicle communication devices, car navigation devices, millimeter-wave radars, and on-vehicle camera modules; semiconductor testing equipment, high-frequency measuring equipment, and the like.
[0166] [Foam] In addition, the cyclic olefin copolymer composition according to the present embodiment can be crosslinked and foamed to form a foam. At this time, the above-mentioned foaming agent may be added to the cyclic olefin copolymer composition.
[0167] [Application] The cyclic olefin copolymer composition and the crosslinked body (Q) according to the present embodiment are excellent in solvent resistance, heat resistance, mechanical strength, and transparency, and thus molded articles made of the crosslinked body can be used in a wide range of applications, including, for example, optical fibers, optical waveguides, optical disk substrates, optical filters, lenses, optical adhesives, optical filters for PDPs, coating materials for organic EL, base film substrates for solar cells in the aerospace field, coating materials for solar cells and thermal control systems, semiconductor elements, light-emitting diodes, electronic elements such as various types of memories, hybrid ICs, MCMs, printed wiring boards, prepregs and laminates used to form insulating layers for printed wiring boards, and display components. The compound can be used for applications such as barrier coating materials or interlayer insulating materials, substrates for liquid crystal displays and solar cells, medical instruments, automobile parts, release agents, resin modifiers, transparent substrates for displays, parts for lithium ion batteries, semiconductor process parts, film capacitors, gas barrier coating materials, electric wire covering materials, automobile parts, aerospace parts, semiconductor process materials, electric wire covering materials, parts for lithium ion batteries, parts for fuel cells, capacitor films, flexible display parts, anchor coating materials, transparent adhesives, modifiers, crosslinking assistants, medical containers, parts for medical catheters, waterproof sealants, release agents, hard coating materials, and foaming modifiers. In particular, since it has excellent stability over time in dielectric properties, and also has excellent solvent resistance, heat resistance, transparency, mechanical properties, etc., it can be suitably used in high frequency applications such as high frequency circuit boards, etc. Furthermore, since it has excellent gas barrier properties, it can be suitably used as a substrate, film, or sheet for liquid crystal displays and solar cells.
[0168] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES
[0169] The present invention will be described in more detail below with reference to Synthesis Examples and Examples, but the present invention is not limited thereto in any way.
[0170] The composition and intrinsic viscosity [η] of the cyclic olefin copolymer (m) used in the Synthesis Examples, Examples, and Comparative Examples were measured by the methods described below.
[0171] composition; 1 H-NMR measurement was performed, and the cyclic non-conjugated diene content was calculated from the intensity of the peak derived from hydrogen directly bonded to the double bond carbon and the peak of other hydrogen.
[0172] Intrinsic viscosity [η]: Measured in decalin at 135°C.
[0173] The films and laminates obtained in the examples and comparative examples were evaluated by the methods described below.
[0174] Dissipation factor rating: The laminated films obtained in the examples and comparative examples were evaluated for dielectric loss tangent at 10 GHz by a cylindrical cavity resonator method.
[0175] Heat aging resistance rating: Heat aging resistance was evaluated based on the change in dielectric tangent before and after heat treatment in an oven at 125° C. for the time period shown in Table 1.
[0176] The following raw materials were used in the experiment:
[0177] Transition metal compounds (1) (Synthesized by the method described in JP 2004-331965 A.)
[0178] [ka]
[0179] MMAO (manufactured by Tosoh Finechem) Toluene (Fujifilm Wako Pure Chemical Industries, Ltd.: Wako special grade) Cyclohexane (Fujifilm Wako Pure Chemical Industries, Ltd.: Wako Special Grade) 5-vinyl-2-norbornene (Tokyo Chemical Industry Co., Ltd.) Tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-Dodecene (Mitsui Chemicals, Inc.) Methanol (Fujifilm Wako Pure Chemical Industries, Ltd.: Wako special grade)
[0180] Cyclic olefin polymers (n): Polymer 1: Ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene copolymer (product name: APEL 6509T, manufactured by Mitsui Chemicals)
[0181] Hindered phenols (X): X-1: KEMISORB114 (Chemipro Chemical Co., Ltd., compound represented by the following formula, molecular weight 474.8) [ka]
[0182] X-2: KEMISORB113 (Chemipro Chemical Co., Ltd., compound represented by the following formula, molecular weight 466.8) [ka]
[0183] X-3: KEMISORB112 (Chemipro Chemical Co., Ltd., compound represented by the following formula, molecular weight 438.7) [ka]
[0184] Hindered amine compounds (Y): Compound (Y)-4: CHIMASSORB 944 FDL (molecular weight 2000-3100) (manufactured by BASF) Compound (Y)-5: CHIMASSORB 2020 FDL (molecular weight 2600-3400) (manufactured by BASF)
[0185] Comparison compound: Compound (R)-1: Irganox 1010 (BASF) Compound (R)-2: Irganox 1076 (BASF)
[0186] Radical polymerization initiator: Crosslinking agent 1: Percumyl D (manufactured by Nippon Oil & Fats Co., Ltd.)
[0187] [Synthesis Example 1] In a 1L stainless steel autoclave that has been thoroughly purged with nitrogen, 450 ml of toluene and 5-Vinyl-2-norbornene (VNB) 30ml, Tetracyclo[4.4.0.1 2,5 .1 7,10 After adding 16 ml of ]-3-dodecene (TD), 0.9 mmol of MMAO (manufactured by Tosoh Finechem Co., Ltd.) in hexane in terms of Al, and 360 ml of hydrogen, ethylene was introduced into the system until the total pressure reached 0.6 MPa. A toluene solution of 0.028 mmol of transition metal compound (1) was added, and polymerization was carried out at 35°C for 180 minutes. The polymerization was then terminated by injecting 1 ml of methanol. The intrinsic viscosity [η] was 0.35 (dL / g), and the composition ratio of the VNB-derived structure in the polymer determined by NMR was 26 mol%, and the composition ratio of the TD-derived structure was 12 mol%. The glass transition temperature measured by DSC was 96°C.
[0188] [Example 1] (Preparation of Varnish 1) The solution of the cyclic olefin copolymer (m) obtained in Synthesis Example 1, polymer 1 as the cyclic olefin polymer (n), crosslinking agent 1 as the radical polymerization initiator, (X)-1 as the hindered phenol (X), compound (Y)-1 as the hindered amine compound (Y), and toluene / cyclohexane mixed solvent as the solvent were weighed according to the composition in Table 1. The weighed sample was stirred until it was fully dissolved, and the desired varnish-like cyclic olefin copolymer composition was obtained. The unit of the blending ratio of each raw material in Table 1 is parts by mass.
[0189] (Film production) The obtained varnish-like cyclic olefin copolymer composition was applied onto a PET film at a speed of 10 mm / sec, and then dried in a nitrogen gas flow drier at 150°C for 4 minutes. Next, two of the obtained films were stacked, pressurized to 3.5 MPa by a vacuum press, heated at a constant rate from room temperature (25°C), and held at 180°C for 120 minutes to obtain a laminated film with a thickness of 70 μm. The obtained laminated film was evaluated in each case. The results are shown in Table 1.
[0190] [Comparative Example 1] A film was produced and evaluated in the same manner as in Example 1, except that the blending composition was changed to that shown in Table 1. That is, a film was produced without adding the hindered amine (X) or the hindered phenol compound (Y), and evaluated in the same manner as in Example 1.
[0191] [Examples 2 to 9 and Comparative Examples 2 to 4] Films were produced and evaluated in the same manner as in Example 1, except that the blending compositions were changed to those shown in Table 1. The results are shown in Table 1.
[0192] [Table 1]
[0193] [Table 2]
Claims
1. A cyclic olefin copolymer (m); A cyclic olefin-based polymer (n) different from the cyclic olefin-based copolymer (m); A hindered phenol (X) represented by the following general formula (1), A hindered amine compound (Y) having a piperidyl group represented by the following general formula (2), A cyclic olefin copolymer composition comprising: The cyclic olefin copolymer (m) is (A) one or more olefin-derived repeating units represented by the following general formula (I), (B) one or more repeating units derived from a cyclic non-conjugated diene represented by the following general formula (III): Rank and (C) one or more repeating units derived from a cyclic olefin represented by the following general formula (V), When the total number of moles of repeating units in the cyclic olefin copolymer (m) is taken as 100 mol%, the content of the repeating unit (A) derived from the olefin is 10 mol% or more and 90 mol% or less, the content of the repeating unit (B) derived from the cyclic non-conjugated diene is 1 mol% or more and 40 mol% or less, and the content of the repeating unit (C) derived from the cyclic olefin is 1 mol% or more and 30 mol% or less, The cyclic olefin polymer (n) comprises at least one selected from a copolymer (n1) of ethylene or an α-olefin with a cyclic olefin (provided that the copolymer (n1) does not contain a repeating unit derived from a cyclic non-conjugated diene represented by the following general formula (III)) and a ring-opening polymer (n2) of a cyclic olefin, When the total amount of the cyclic olefin copolymer (m) and the cyclic olefin polymer (n) is taken as 100 mass%, the content of the cyclic olefin polymer (m) is 5% by mass or more and 95% by mass or less, and the content of the cyclic olefin polymer (n) is 5% by mass or more and 95% by mass or less, The molecular weight of the hindered phenol (X) is 264 to 2000; the content of the hindered phenol (X) is 0.01 to 5 parts by mass relative to 100 parts by mass of the total content of the cyclic olefin copolymer (m) and the cyclic olefin polymer (n), The molecular weight of the hindered amine compound (Y) is 1000 or more, The cyclic olefin copolymer composition has a content of the hindered amine compound (Y) in the cyclic olefin copolymer composition of 0.01 parts by mass or more and 5 parts by mass or less, when the content of the cyclic olefin copolymer (m) contained in the cyclic olefin copolymer composition is taken as 100 parts by mass. 【Chemistry 1】 [In the above general formula (I), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. 【Chemistry 2】 [In the above general formula (III), u is 0 or 1, v is 0 or a positive integer, and w is 0. or 1, R 61 ~R 76 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 104 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, t is a positive integer of 0 to 10, and R 75 and R 76 are bonded to each other may form a monocyclic or polycyclic ring.] 【Chemistry 3】 [In the above general formula (V), u is 0 or 1, v is 0 or a positive integer, w is 0 or 1, R 61 ~R 78 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 75 ~R 78 may be bonded to each other to form a monocyclic or polycyclic ring. 【Chemistry 4】 [In the above general formula (1), X is a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cyclohexyl group, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; The substituents on the alkyl group, the cyclohexyl group, and the aryl group are selected from the group consisting of an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, a hydroxy group, a methoxy group, and an oxadiazole group. 【Chemistry 5】 [In the above general formula (2), X is a hydrogen atom, an oxy radical group, an alkyl group, an alkoxy group, an aryl group, or a hydroxy group, and R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom or an alkyl group.
2. the organic group X of the hindered phenol (X) is a group selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an n-octyl group, an n-tetradecyl group, an n-hexadecyl group, a 2,4-di-t-butylphenyl group, and a 2,4-di-t-pentylphenyl group; The cyclic olefin copolymer composition according to claim 1 .
3. The cyclic non-conjugated diene constituting the repeating unit (B) derived from the cyclic non-conjugated diene is 5-vinyl-2-norbornene or 8-vinyl-9-methyltetracyclo[4.4.0.1 2,5 .1 7,10 3. The cyclic olefin copolymer composition according to claim 1, wherein the cyclic olefin copolymer is 3-dodecene.
4. The cyclic olefin constituting the cyclic olefin-derived repeating unit (C) is bicyclo[2.2.1]-2-heptene or tetracyclo[4.4.0.1 2,5 .1 7,10 4. The cyclic olefin copolymer according to claim 1, wherein the copolymer is 3-dodecene. Body composition.
5. A varnish comprising the cyclic olefin copolymer composition according to any one of claims 1 to 4 and a solvent.
6. A crosslinked product of the cyclic olefin copolymer composition according to any one of claims 1 to 5.
7. A film or sheet comprising the crosslinked product according to claim 6.
8. A laminate comprising the film or sheet according to claim 7 laminated on a substrate.
9. A prepreg comprising the cyclic olefin copolymer composition according to any one of claims 1 to 4 and a sheet-like fiber substrate.
10. A metal-clad laminate obtained by laminating at least one selected from the film or sheet according to claim 7, the laminate according to claim 8, and the prepreg according to claim 9, and a metal foil.
11. A printed wiring board comprising an electrical insulating layer formed from at least one selected from the film or sheet according to claim 7, the laminate according to claim 8, and the prepreg according to claim 9, and a conductor layer provided on the electrical insulating layer.
12. An electronic device comprising the printed wiring board according to claim 11.
Citation Information
Patent Citations
Polyolefin resin composition for agricultural film and agricultural film
JP2003231777A
Crosslinking resin composition, crosslinking resin molding and flame retardant crosslinked resin molding
JP2005047992A
Polyolefin resin composition and molded article using the same
JP2018062565A
Resin composition and crosslinked body of the same
JP2018095786A
&agr -OLEFIN / CYCLOOLEFIN / POLYENE COPOLYMER AND PROCESS FOR PRODUCING THE SAME
WO2006118261A1