Manufacturing method of electret
By dispersing a metastable zirconia phase in alumina and applying a polarization process, the electret achieves high heat resistance and stable polarization, addressing the limitations of existing piezoelectric materials.
Patent Information
- Application Number
- JP2020211649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-21
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Existing piezoelectric materials lack sufficient heat resistance and are prone to polarization relaxation, making them unsuitable for long-term applications at high temperatures.
A ceramic material is produced by dispersing a metastable zirconia phase in an alumina phase, with a polarization process involving heating and voltage application to create an electret with strong and stable polarization characteristics.
The resulting electret exhibits high heat resistance and maintains strong polarization, suitable for high-temperature applications.
Smart Images

Figure 0007590863000002 
Figure 0007590863000003 
Figure 0007590863000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an electret and an electret. [Background technology]
[0002] In some dielectric materials, such as permanent magnets, the dielectric polarization may remain after the electric field disappears. Such materials are called electrets in contrast to magnets, and are used in filters for dust collectors, microphones, etc.
[0003] For example, Patent Document 1 discloses a polymer composite piezoelectric material obtained by converting a compound having a polyimide resin and ferroelectric ceramic particles into an electret. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-287448 Summary of the Invention [Problem to be solved by the invention]
[0005] Patent Document 1 discloses that the piezoelectric material can be used for a long period of time even at high temperatures of about 150° C. However, the heat resistance of the piezoelectric material described in Patent Document 1 is still insufficient, and furthermore, the viscoelasticity of the polymer causes relaxation of polarization, making it difficult to maintain polarization for a long period of time.
[0006] The present invention has been made to solve the above problems, and an object of the present invention is to provide an electret which has high heat resistance and is less susceptible to polarization relaxation, and a method for producing the same. [Means for solving the problem]
[0007] The method for producing an electret of the present invention is characterized by having a polarization step of polarizing a ceramic material in which a first phase made of zirconia is dispersed and scattered in a second phase made of alumina, and the first phase includes a metastable phase whose crystal system is metastable at room temperature.
[0008] A ceramic material in which a first phase containing metastable zirconia that is metastable at room temperature is dispersed and scattered in a second phase made of alumina is easily polarized due to the dielectric properties of the metastable zirconia contained in the first phase. Therefore, by using the electret manufacturing method of the present invention, which includes a polarization step for polarizing such a ceramic material, it is possible to manufacture an electret that is highly heat resistant and is less susceptible to relaxation of polarization.
[0009] In the method for producing an electret of the present invention, the zirconia preferably contains a tetragonal crystal system that is metastable at room temperature and a monoclinic crystal system that is stable at room temperature. Tetragonal zirconia, whose crystal system is metastable at room temperature, exhibits excellent polarization properties. When zirconia contains tetragonal crystals, whose crystal system is metastable at room temperature, and monoclinic crystals, whose crystal system is stable at room temperature, it becomes an electret with excellent polarization properties.
[0010] In the method for producing an electret of the present invention, the first phase preferably does not contain a stabilizer. If the first phase does not contain a stabilizer, the volume change from the metastable phase to the stable phase upon cooling after sintering is maximized, maximizing the interaction with the second phase and making it easier for the metastable phase to remain, thereby enhancing the electret effect.
[0011] In the method for producing an electret of the present invention, the first phase further contains a stabilizer, and the content of the stabilizer in the first phase is preferably 5 mol % or less. If the content of the stabilizer in the first phase is 5 mol % or less, the volume change from the metastable phase to the stable phase upon cooling after sintering becomes larger, which increases the interaction with the second phase and makes it easier for the metastable phase to remain, thereby enhancing the electret effect.
[0012] In the method for producing an electret of the present invention, the polarization step preferably includes a heating step of sandwiching the ceramic material between a pair of electrodes and heating the ceramic material at 700°C to 1000°C while a voltage is applied to the pair of electrodes, and a cooling step of cooling the ceramic material while a voltage is applied to the pair of electrodes. By setting the heating temperature in the polarization process to 700°C or higher, the dipoles of the first phase can be sufficiently oriented, resulting in excellent polarization characteristics. Also, by setting the heating temperature in the polarization process to 1000°C or lower, polarization can be achieved while maintaining the internal stress, without causing a phase change from the metastable phase at room temperature to a stable phase due to internal stress.
[0013] In the method for producing an electret of the present invention, the voltage applied to the pair of electrodes in the heating step is preferably 1 kV to 10 kV. When the voltage applied to the pair of electrodes in the heating step is in the above range, the ceramic material can be sufficiently polarized. If the voltage is 1 kV or more, the ceramic material can be sufficiently polarized, whereas if the voltage is 10 kV or less, dielectric breakdown is unlikely to occur in the space or the ceramic material, and the electretization treatment can be stably performed.
[0014] The electret of the present invention is characterized in that a first phase made of zirconia is dispersed and scattered in a second phase made of alumina, and the first phase has a ceramic material having a crystal system including a metastable phase that is metastable at room temperature, and the first phase is polarized.
[0015] The electret of the present invention is excellent in heat resistance because it is made of zirconia and alumina. Also, the electret of the present invention has excellent polarization characteristics because the first phase, which includes a metastable phase that is metastable at room temperature, is polarized.
[0016] In the electret of the present invention, the maximum value of the surface potential of the ceramic material is preferably 100V to 10 kV. When the maximum value of the surface potential of the ceramic material is within the above range, it can be said to exhibit excellent properties as an electret.
[0017] In the electret of the present invention, it is preferable that the surface potential of the ceramic material is non-uniform. If the surface potential of a ceramic material is non-uniform, a high potential is generated locally, and this high potential can be utilized positively, for example, to increase sensitivity as a sensor.
[0018] In the electret of the present invention, the surface of the ceramic material is preferably exposed. When the surface of the ceramic material is exposed, a high potential can be obtained without averaging out uneven polarization that occurs within the surface.
[0019] In the electret of the present invention, the shape of the ceramic material is a plate having a first main surface and a second main surface opposed to each other in the thickness direction, and it is preferable that the surface potential of the edge portion of at least one of the first main surface and the second main surface is lower than that of the center of the main surface. If the surface potential of the edge portion is lower than that of the center, a high potential can be obtained at the center portion of the main surface, which is easily usable when fabricating various devices, etc., and the substrate can be suitably used as an electronic component. Effect of the Invention
[0020] According to the method for producing an electret of the present invention, a step of polarizing a ceramic material in which a first phase made of zirconia containing a metastable phase whose crystal system is metastable at room temperature is dispersed and scattered in a second phase is provided. Therefore, an electret having high heat resistance and strong polarization that is likely to remain can be produced. According to the electret of the present invention, the first phase made of zirconia contains a metastable phase whose crystal system is metastable at room temperature, so that the polarization is likely to remain strong and it can be suitably used as a material for electrets. In addition, since it is formed only of ceramic materials that are stable up to high temperatures, it has excellent heat resistance that allows it to be used at high temperatures. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a ceramic material. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates an example of the polarization step. [Diagram 3] FIG. 3 is a diagram showing XRD patterns of the electrets according to Examples 1 and 3 and Comparative Example 1. [Figure 4] FIG. 4 is an SEM photograph of a cross section of the electret according to Example 1. [Diagram 5] FIG. 5 is an SEM photograph of a cross section of the electret according to Example 2. [Figure 6] FIG. 6 is an SEM photograph of a cross section of the electret according to Example 3. [Figure 7A] FIG. 7A is a diagram showing the distribution of surface potential on the surface (+ side) of the electret according to Example 1. FIG. [Figure 7B] FIG. 7B is a diagram showing the distribution of the surface potential on the surface (-side) of the electret according to Example 1. [Figure 8A] FIG. 8A is a diagram showing the distribution of surface potential on the surface (+ side) of the electret according to Example 2. [Figure 8B] FIG. 8B is a diagram showing the distribution of the surface potential on the surface (-side) of the electret according to Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The electret and the method for producing the electret of the present invention will be described in detail below, but the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention. The present invention also includes an appropriate combination of the preferred embodiments of the present invention.
[0023] [Method of manufacturing electret] The method for producing an electret of the present invention is characterized by having a polarization step of polarizing a ceramic material in which a first phase made of zirconia is dispersed and scattered in a second phase made of alumina, and the first phase includes a metastable phase whose crystal system is metastable at room temperature.
[0024] A ceramic material in which a first phase made of zirconia is dispersed and scattered in a second phase made of alumina, and the first phase contains a metastable phase whose crystal system is metastable at room temperature, is easily polarized due to the dielectric properties of the metastable phase zirconia contained in the first phase. Therefore, by using the electret manufacturing method of the present invention, which includes a polarization step for polarizing such a ceramic material, it is possible to manufacture an electret that is highly heat resistant and is less susceptible to relaxation of polarization.
[0025] First, the ceramic material used in the polarization step will be briefly described.
[0026] The ceramic material used in the polarization step is composed of a first phase made of zirconia dispersed and scattered within a second phase made of alumina. The first phase includes a metastable phase whose crystal system is metastable at room temperature. In this specification, room temperature is 25°C.
[0027] The first phase consists of zirconia. Examples of the crystal system of zirconia include monoclinic zirconia, which is a stable phase at room temperature, and tetragonal zirconia and cubic zirconia, which are metastable phases at room temperature.
[0028] The stable phase is monoclinic zirconia. The metastable phase is preferably tetragonal zirconia. When the metastable phase is tetragonal zirconia, the polarization tends to remain strong and it can be suitably used as a material for an electret.
[0029] The zirconia preferably has a crystal system containing tetragonal crystals, which are metastable at room temperature, and monoclinic crystals, which are stable at room temperature. Tetragonal zirconia, whose crystal system is metastable at room temperature, exhibits excellent polarization properties. When zirconia contains tetragonal crystals, whose crystal system is metastable at room temperature, and monoclinic crystals, whose crystal system is stable at room temperature, it becomes an electret with excellent polarization properties.
[0030] The type of crystal system constituting zirconia can be confirmed by comparing the peak positions in a diffraction pattern obtained by X-ray diffraction (XRD) with those of a known measurement sample.
[0031] When zirconia is heated, the stable phase changes from monoclinic to tetragonal at 1170°C. When the phase changes from monoclinic to tetragonal, a volumetric shrinkage of about 4% occurs, so the first phase heated to a temperature of 1170°C or higher rapidly decreases in volume. On the other hand, when cooled, the tetragonal phase attempts to change to monoclinic, but this is accompanied by a volume expansion of about 4%. In the electret of the present invention, the first phase made of zirconia is dispersed and scattered in the second phase made of alumina, so that the first phase and the second phase form a composite material. Therefore, they exert a mechanical interaction with each other, and the second phase, alumina, exerts a strong restraining force on the first phase, zirconia, restraining the volume expansion and allowing the metastable phase, tetragonal, to remain even at room temperature. Furthermore, it is considered that the strong restraining force of the second phase makes it difficult for the dipoles inside the metastable phase to rotate easily, and strong polarization can be maintained.
[0032] The content of zirconia in the ceramic material is preferably 5 wt % to 15 wt %. When the zirconia content is 5wt% or more, it can exert a sufficient polarization effect and act as an electret.When the zirconia content is 15wt% or less, it can receive a strong compressive stress from the second phase and maintain polarization. The content of zirconia does not take into consideration the weight of the stabilizer.
[0033] The first phase may or may not contain a stabilizing agent. The stabilizer contained in zirconia is not particularly limited, but metal oxides can be used. For example, CaO, Y2O3, CeO2, etc. can be used, and zirconia with the addition of CaO is called CaO stabilized zirconia (CSZ), and zirconia with the addition of Y2O3 is called Y2O3 stabilized zirconia (YSZ). Among them, zirconia with the addition of Y2O3 can be used stably even at high temperatures. The above-mentioned polarization effect is not observed in stabilized zirconia that becomes a tetragonal crystal even at room temperature due to the addition of the above-mentioned stabilizer, but the above-mentioned polarization effect is observed in partially stabilized zirconia in which a stable phase and a metastable phase are mixed at room temperature due to the addition of the above-mentioned stabilizer, and in zirconia that does not substantially contain a stabilizer. Therefore, the first phase containing partially stabilized zirconia or zirconia that does not substantially contain a stabilizer is subjected to a strong compressive stress from the second phase at or below the phase transition temperature, so that the dipole of the zirconia that constitutes the first phase can be maintained in a fixed state, and an electret with strong residual polarization can be obtained. On the other hand, if the first phase does not contain a stabilizer, the volume change during cooling after sintering is maximized, which maximizes the interaction with the second phase and makes it easier for the metastable phase to remain, thereby enhancing the electret effect.
[0034] When the first phase contains a stabilizer, the content of the stabilizer in the first phase is preferably 5 mol % or less, more preferably 0.5 mol % or less, and even more preferably the first phase is substantially free of stabilizer. If the content of the stabilizer in the first phase is 5 mol% or less, the volume change from the metastable phase to the stable phase during cooling becomes larger, so that the interaction with the second phase becomes larger and the metastable phase is more likely to remain, so that the electret effect can be strengthened. This effect can be more effectively expressed when Y2O3 is added. Therefore, Y2O3 is particularly preferable as an additive.
[0035] In the ceramic material, at least a part of the first phase is preferably present in a flat shape, and the flat shapes are preferably oriented in the same direction. It is believed that if the first phase has a flat shape, it is more likely to receive stress equally from the second phase, making it easier to maintain the metastable phase. In addition, since the orientation direction of the flat shapes is uniform, it can be strongly polarized in the polarization process.
[0036] The maximum length of the flat shape is preferably 0.2 μm to 10 μm. When the maximum length of the flat shape is 0.2 μm or more, the direction of the compressive stress from the first phase is aligned, and the restoring force of the dipoles can be more strongly restricted. When the maximum length of the flat shape is 10 μm or less, the internal stress is less likely to concentrate, and destruction due to the interaction between the first phase and the second phase is less likely to occur. In the ceramic material 1 shown in FIG. 1, the maximum length of the first phase 10 is the length in the x direction. The maximum length of the flat shape is the maximum value of the major axis of the first phase that can be confirmed within the field of view in an image of a cross section of a ceramic material observed with an SEM (magnification: 1000 times to 10000 times).
[0037] The second phase consists of alumina. Alumina is stable up to the temperature range where zirconia becomes an electret, and can continue to bind the dipoles of zirconia during the cooling process. In addition, since alumina is unlikely to form a mixture with zirconia, the interface between the first and second phases is clearly formed, making the interaction stronger.
[0038] In the cross section of the ceramic material, the area ratio of the first phase is preferably 3.5% to 10%. If the area ratio of the first phase is 3.5% or more, sufficient polarization is obtained and the material can be suitably used as an electret. If the area ratio of the first phase is 10% or less, the first phase can be maintained in a dispersed and scattered state in the second phase, and the material can be easily subjected to compressive stress by the second phase. The area ratio of the first phase in the cross section of the ceramic material is determined as the ratio of the total area of the first phase to the total area in the field of view of the cross section of the ceramic material observed with an SEM (magnification 1000 times to 10000 times).
[0039] The porosity of the ceramic material is preferably 0.01% to 0.5%. When the porosity is 0.5% or less, the compressive stress from the second phase can be efficiently transmitted to the first phase, and the function as an electret can be further enhanced. The porosity of the ceramic material can be adjusted by adjusting the molding pressure when molding the ceramic material. The higher the molding pressure, the smaller the porosity. The porosity of a ceramic material can be determined from the pore volume and pore size distribution measured using mercury intrusion porosimetry. The pore volume and pore size distribution of a ceramic material are measured by setting the surface tension and contact angle of mercury to 485 mN / m and 130°, respectively, and injecting mercury at a pressure ranging from atmospheric pressure to 200 MPa.
[0040] FIG. 1 is a cross-sectional view that illustrates an example of a ceramic material. 1, the ceramic material 1 contains a first phase 10 made of zirconia and a second phase 20 made of alumina. The first phase 10 is dispersed and scattered within the second phase 20. Moreover, the first phase 10 contains a metastable phase whose crystal system is metastable at room temperature. The shape of the first phase 10 shown in Fig. 1 is a flat shape in which the length in the x direction is longer than the length in the y direction. In Fig. 1, the first phase 10 can be said to be oriented along the x direction.
[0041] In a state where the first phase 10 is dispersed and scattered in the second phase 20, the periphery of the first phase 10 is covered with the second phase 20. Therefore, when the ceramic material 1 is cooled after being heated, the first phase 10 receives a compressive stress from the second phase 20. Since the volume expansion of the first phase 10 is restricted by this compressive stress, the phase transition from the metastable phase to the stable phase, which would result in a volume expansion of about 4%, is prevented, and the metastable phase is generated even at room temperature.
[0042] In addition, when specifying the shape of the first phase, the shape is specified by regarding the first phase surrounded by the second phase as one unit, rather than the shape of the zirconia particles or the shape of the crystallites that constitute the first phase.
[0043] Next, a method for producing the above-mentioned ceramic material will be described. As a method for producing the ceramic material, for example, a method in which a mixture of zirconia, alumina and an organic binder is formed into a predetermined shape, and then degreased and fired (also called sintered) can be mentioned.
[0044] The average particle size of the zirconia is not particularly limited, but is preferably 0.1 μm to 10 μm.
[0045] The average particle size of the alumina is not particularly limited, but is preferably 0.05 μm to 1 μm.
[0046] The average particle size of zirconia and alumina is the cumulative volume 50% particle size D50 determined by laser diffraction method.
[0047] The weight ratio of zirconia to the total weight of zirconia and alumina in the mixture is preferably 5% to 15%.
[0048] Moreover, the ratio of the volume of zirconia to the total volume of zirconia and alumina in the mixture is preferably 3.5% to 10%. The volume ratio of zirconia is calculated from the mass and true density of the raw materials (zirconia and alumina before mixing) used, and the volume ratio is compared. By setting the volume ratio at the raw material stage, it is possible to obtain a sintered body with the desired volume ratio of the first and second phases, even if raw materials with different true densities are used.
[0049] The content of the organic binder is preferably 20% by weight to 50% by weight relative to the total of the zirconia and alumina, 100% by weight. Examples of the organic binder include acrylic organic binders such as polymethyl methacrylate, polyvinyl alcohol, and paraffin.
[0050] In addition to the zirconia, alumina, and organic binder, additives may be added to the mixture as appropriate. Examples of additives include plasticizers, solvents, and dispersants, and these can be used as appropriate depending on the properties of the mixture. Examples of the solvent include 1-butanol, toluene, and isopropyl alcohol. Among the above solvents, those that have low solubility in the organic binder (poor solvents) are preferred. An example of a poor solvent for the acrylic organic binder is butanol.
[0051] In addition, when the first phase is zirconia containing a stabilizer, zirconia containing the stabilizer from the beginning may be used, or when mixing alumina and an organic binder, zirconia and the stabilizer may be prepared separately, mixed in advance, and then mixed with alumina in a two-stage method. In this case, in the first stage of mixing zirconia and the stabilizer, it is preferable to perform dry mixing that is less likely to cause aggregation so that they are mixed uniformly. On the other hand, it is preferable to mix with alumina by making it into a paste and then performing wet mixing. By preparing the mixture in this manner, it is possible to obtain a structure in which zirconia and the stabilizer are mixed uniformly and the first phase is dispersed and scattered throughout the second phase.
[0052] Alternatively, the first phase may be precipitated from a mixture in which the first phase and the second phase are uniformly mixed. Specifically, for example, alumina and zirconia are dispersed in a solution in which an organic binder and a poor solvent are mixed, and as the poor solvent evaporates, the organic binder is precipitated by spinodal decomposition, and the aggregation of zirconia, which has a high affinity with the organic binder, is promoted. Since zirconia is aggregated at the raw material stage, a flat first phase is obtained by subsequent molding, and the polarization characteristics can be improved.
[0053] Examples of methods for forming the mixture into a predetermined shape include a method in which the mixture is formed into a sheet shape and then laminated, and a method in which the mixture is directly pressure molded or extrusion molded. In uniaxial pressing, which can be molded into a plate, the material is crushed so that the first phase is oriented along a plane perpendicular to the pressing direction, whereas in extrusion molding, the first phase is oriented along the extrusion direction.
[0054] When the mixture is molded, it is preferable to apply uniaxial pressure to the molded body. By applying uniaxial pressure to the green body, the orientation of the first phase in the green body can be aligned and the green body can be flattened. This operation produces a ceramic material in which the first phase can be strongly polarized.
[0055] The obtained molded body is degreased and sintered to obtain a ceramic material. The degreasing can be carried out, for example, by heating the compact at a temperature of about 1000°C. Prior to the degreasing, the solvent may be dried from the molded body.
[0056] The degreased compact is then sintered. The sintering temperature is preferably 1300°C to 1500°C. If the sintering temperature is 1300°C or higher, the first phase zirconia, which was monoclinic zirconia in the raw material stage, can be transformed into tetragonal zirconia, which is a metastable phase. Also, if the sintering temperature is 1500°C or lower, the particles are less likely to coarsen, resulting in a fine structure that is more likely to be polarized.
[0057] Since the solid-state reaction rate between zirconia and alumina is extremely slow, the first and second phases are hardly mixed during sintering under the above conditions, and a dispersed state of the first phase is formed that corresponds to the agglomerated state of the mixture. Therefore, the zirconia first phase is fixed in a dispersed and scattered state in the alumina second phase by sintering.
[0058] In the sintering, it is preferable to apply uniaxial pressure to the compact. In particular, when uniaxial pressure is not applied to the green body in the compacting step, it is preferable to apply uniaxial pressure to the green body during sintering. The surface pressure of the uniaxial press is preferably 15 MPa to 150 MPa. By applying uniaxial pressure during sintering, the orientation state of the first phase in the compact can be fixed while sintering proceeds, resulting in a ceramic material in which the first phase can be strongly polarized. In addition, by sintering under a surface pressure of 15 MPa or more, a strong second phase can be formed that can suppress expansion when the first phase transitions from a metastable phase to a stable phase during cooling. Furthermore, even if the sintering temperatures of the first and second phases are different, they can be sintered simultaneously at the lower sintering temperature due to the action of pressure.
[0059] The flat first phase can be formed not only during the molding stage but also during the sintering stage. In order to form a flat shape during the sintering stage, hot pressing using a uniaxial mold, SPS, etc. can be used. In addition, by applying pressure at the same time as sintering, the phase transition to the stable phase of zirconia at the phase transition temperature can be suppressed.
[0060] By the above procedure, a ceramic material can be obtained in which a first phase containing metastable zirconia, which is metastable at room temperature, is dispersed and scattered in a second phase made of alumina.
[0061] [Polarization process] The method for producing an electret of the present invention includes a polarization step of polarizing the above-mentioned ceramic material. The method for polarizing the ceramic material is not particularly limited, but examples include a method of heating the ceramic material while applying a voltage to it (also known as thermal electret treatment), a method of irradiating it with radiation, or a method of applying corona discharge.
[0062] The thermal electret treatment preferably includes, for example, a heating step in which the ceramic material is sandwiched between a pair of electrodes and heated at 700°C to 1000°C while a voltage is applied to the pair of electrodes, and a cooling step in which the ceramic material is cooled while a voltage is applied to the pair of electrodes.
[0063] Moreover, the electrodes may not only be sandwiched but also formed on the surface of the ceramic material. Methods for forming a pair of electrodes include, for example, a method in which an electrode paste containing metal particles and a solvent is applied to the surface of a ceramic material and then dried, a method in which a metal layer is formed on the surface of a ceramic material by a method such as vapor deposition, and a plating method.
[0064] Examples of metals constituting the electrodes include Pt, Au, Cu, Ni, and stainless steel.
[0065] The pair of electrodes is preferably formed on two opposing surfaces. When the ceramic material has a plate shape, it is preferable that the two surfaces are opposed to each other in the thickness direction. In this case, the thickness of the ceramic material is preferably 0.1 mm to 5 mm.
[0066] In the heating step, the ceramic material is heated to 700°C to 1000°C while a voltage is applied to the pair of electrodes. The atmosphere during heating is not particularly limited, but when a metal that easily forms an oxide film is used for the electrode, a non-oxidizing atmosphere is preferable so that the metal is not oxidized. The ceramic material can be heated in a muffle furnace.
[0067] In the heating step, the voltage applied to the ceramic material is preferably 1 kV to 10 kV. When the applied voltage is within the above range, the ceramic material can be sufficiently polarized while preventing dielectric breakdown. When the applied voltage is 1 kV or more, the ceramic material can be sufficiently polarized, whereas when the applied voltage is 10 kV or less, dielectric breakdown is unlikely to occur in the ceramic material or space, and the electretization treatment can be stably performed.
[0068] In the cooling process, the ceramic material that has completed the heating process is cooled while a voltage is still applied to the pair of electrodes. The cooling may be natural cooling in which the supply of heat from the heat source used in the heating step is stopped, or may be forced cooling in which air is blown against the ceramic material.
[0069] An example of the polarization step will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view that illustrates a schematic example of the polarization step. In the polarization step shown in Fig. 2, a pair of electrodes 30a and 30b are formed on the opposing surfaces 1a and 1b of the ceramic material 1, and the ceramic material 1 is heated to 700°C to 1000°C using a muffle furnace 100, while a voltage is applied between the pair of electrodes 30a and 30b. By applying a voltage while heating to a predetermined temperature, the metastable phase contained in the first phase 10 can be polarized. The direction in which the first phase 10 is polarized is the opposite direction to the direction of the voltage applied to the ceramic material 1. Polarization occurs at the surfaces of the crystallites of the metastable phase. Thus, when the first phase 10 has a flat shape and is oriented along the x direction, as in the ceramic material 1 shown in Figure 1, it can be strongly polarized in the y direction.
[0070] In the method for producing an electret of the present invention, since electrodes are formed on the surface of the ceramic material, it is preferable to further include an electrode removing step of removing the pair of electrodes after the cooling step. The part that exhibits electret properties through polarization is the part of the ceramic material where the electrodes were formed. Therefore, by removing a pair of electrodes in the electrode removal process, the surface of the electret can be effectively utilized.
[0071] [Electret] The electret of the present invention is characterized in that a first phase made of zirconia is dispersed and scattered in a second phase made of alumina, and the first phase has a ceramic material having a crystal system including a metastable phase that is metastable at room temperature, and the first phase is polarized.
[0072] The electret of the present invention has a first phase made of zirconia dispersed and scattered in a second phase made of alumina, and the first phase contains a metastable phase whose crystal system is metastable at room temperature, and therefore exhibits the properties of an electret.
[0073] The electret of the present invention corresponds to a material obtained by polarizing the ceramic material produced by the method for producing an electret of the present invention. Therefore, the configuration of the ceramic material constituting the electret of the present invention is the same as the configuration of the ceramic material that is subjected to the polarization step in the manufacturing method of the electret of the present invention. Therefore, hereinafter, the configuration of the ceramic material constituting the electret of the present invention will be omitted.
[0074] In the electret of the present invention, the maximum value of the surface potential of the ceramic material is preferably 100V to 10 kV. The surface potential of the ceramic material can be measured by a surface potential meter.
[0075] In the electret of the present invention, the surface potential of the ceramic material may be either uniform or non-uniform, but it is preferable that the surface potential of the ceramic material is non-uniform. If the surface potential is non-uniform, a high potential can be generated locally, and this high potential can be utilized positively, for example, to increase sensitivity as a sensor.
[0076] In the electret of the present invention, it is preferable that the surface of the ceramic material is exposed. The exposed surface on which the surface of the ceramic material is exposed may be one that has been exposed since the stage at which the ceramic material is manufactured, or may be one on which the surface of the ceramic material is exposed by removing a pair of electrodes formed in the polarization process.
[0077] In the electret of the present invention, the ceramic material has a plate shape having a first main surface and a second main surface opposed to each other in the thickness direction, and it is preferable that the surface potential of the edge portion of at least one of the first main surface and the second main surface is lower than that of the center of the main surface. If the surface potential of the edge portion is lower than that of the center, a high potential can be obtained in the easily accessible center portion, making it suitable for use as an electronic component. EXAMPLES
[0078] EXAMPLES Hereinafter, examples that more specifically disclose the present invention will be described, however, the present invention is not limited to only the following examples.
[0079] Example 1 (Ceramics Material Preparation) A mixture was obtained by mixing 0.480 parts by weight of alumina, 0.053 parts by weight of zirconia, 0.182 parts by weight of an acrylic organic binder, 0.027 parts by weight of an adipate ester plasticizer (bis(2-ethylhexyl) adipate), 0.008 parts by weight of a plasticizer, FLOWLEN G-700 (a carboxyl group-containing polymer composition), and 0.246 parts by weight of a solvent, 1-butanol, in a ball mill.
[0080] The resulting mixture was formed into a sheet by a doctor blade method and dried at 100° C. for 2 hours.
[0081] The obtained green body was heated at 1000° C. for 1 hour to degrease the green body.
[0082] The degreased green body was heated at 1450°C for 3 hours while applying uniaxial pressure of 40 MPa using a hot press, to obtain a plate-shaped ceramic material with a thickness of 1 mm.
[0083] (Polarization process) Pt electrodes were formed on the front and back surfaces of the obtained ceramic material, and it was placed in a muffle furnace. While applying a voltage of 4 kV between a pair of Pt electrodes formed on the surface of the ceramic material, the ceramic material was heated to 900°C in a non-oxidizing atmosphere in a muffle furnace and held for 3 hours. The muffle furnace was then turned off and the material was cooled to room temperature, thereby obtaining an electret according to Example 1.
[0084] Example 2 An electret according to Example 2 was obtained in the same manner as in Example 1, except that 0.246 parts by weight of 1-butanol was changed to 0.246 parts by weight of toluene.
[0085] Example 3 An electret according to Example 3 was obtained in the same manner as in Example 2, except that 0.053 parts by weight of zirconia was changed to 0.053 parts by weight of partially stabilized zirconia (p-YSZ) to which 6 mol % of Y2O3 was added.
[0086] Comparative Example 1 An electret according to Comparative Example 1 was obtained in the same manner as in Example 1, except that zirconia was not added and the amount of alumina added was changed to 0.533 parts by weight.
[0087] Comparative Example 2 An electret according to Comparative Example 2 was obtained in the same manner as in Example 1, except that no alumina was added and the amount of zirconia added was changed to 0.533 parts by weight.
[0088] Comparative Example 3 An electret according to Comparative Example 3 was obtained in the same manner as in Comparative Example 2, except that the zirconia was changed to stabilized zirconia (YSZ) to which 10 mol % of Y2O3 was added.
[0089] (Crystalline Measurement) The electrets according to each of the examples and comparative examples were subjected to X-ray diffraction (XRD) measurement, and the obtained diffraction patterns were compared with those of known compounds to identify the crystal system of the zirconia contained in the electrets. The results are shown in Table 1. FIG. 3 is a diagram showing XRD patterns of the electrets according to Examples 1 and 3 and Comparative Example 1.
[0090] (Observation of the dispersion state and shape of the first phase) The cross section of the electret was observed by SEM to observe the dispersion state of the first phase relative to the second phase and the shape of the first phase. At this time, the orientation direction of the first phase and the maximum length of the first phase were also obtained. The results are shown in Table 1. In addition, SEM photographs of Examples 1 to 3 are shown in Figures 4 to 6. Figure 4 is an SEM photograph of the cross section of the electret according to Example 1, Figure 5 is an SEM photograph of the cross section of the electret according to Example 2, and Figure 6 is an SEM photograph of the cross section of the electret according to Example 3.
[0091] (Checking the polarization state) The polarization state of the electrets according to each example and comparative example was confirmed by changing the location with a surface potential meter Model 1344 manufactured by Trek Japan, and the overall polarization state was confirmed. The difference between the maximum value of the surface potential (voltage) of the surface on the positive potential side and the minimum value of the surface potential (voltage) of the surface on the negative potential side was taken as the polarization voltage. The polarization states of the electrets according to Examples 1 and 2 are shown in Figs. 7A, 7B, 8A, and 8B. Fig. 7A is a diagram showing the distribution of the surface potential of the surface (+ side) of the electret according to Example 1, Fig. 7B is a diagram showing the distribution of the surface potential of the surface (- side) of the electret according to Example 1, Fig. 8A is a diagram showing the distribution of the surface potential of the surface (+ side) of the electret according to Example 2, and Fig. 8B is a diagram showing the distribution of the surface potential of the surface (- side) of the electret according to Example 2. The vertical axis in Figs. 7A, 7B, 8A, and 8B indicates the surface potential, and the two axes perpendicular to this indicate the position (coordinates) of the electret surface. As shown in Figures 7A, 7B, 8A, and 8B, the polarization voltage of the surface was nonuniform in the electrets according to Examples 1 and 2. Although not shown, the surface potential of the electret surface was also nonuniform in the electret according to Example 3.
[0092] [Table 1]
[0093] The polarization voltages of the electrets according to Examples 1 and 2 were 1061.9 V (maximum value: +959.9 V, minimum value: -102.0 V) and 175.9 V (maximum value: +103.8 V, minimum value: -72.1 V), respectively. Therefore, it can be said that they have excellent properties as electrets. On the other hand, slight polarization was observed on the surface of the electret according to Example 3. For this reason, it can be said that it has some electret properties, although only slightly. On the other hand, on the surfaces of the electrets according to Comparative Examples 1 to 3, no polarization was observed.
[0094] When Example 1 and Example 2 are compared, the polarization in Example 1 is larger, which is believed to be due to the particle shape of the zirconia before sintering. 1-butanol was used as the solvent in Example 1. It is believed that because 1-butanol is a poor solvent with low solubility for the organic binder, aggregation of zirconia and the organic binder occurred during the drying process, resulting in flat-shaped zirconia particles. On the other hand, toluene was used as the solvent in Example 2. Because toluene is a good solvent with high solubility for the organic binder, it is believed that the zirconia and the organic binder did not aggregate during the drying process, and flat zirconia particles were not obtained. In the electret according to Example 3, it is believed that the polarization of the first phase was alleviated by the addition of the stabilizer.
[0095] The reason why Comparative Example 1 did not show polarization is believed to be because zirconia, which acts as a dielectric, was not included. The reason why Comparative Example 2 did not show polarization is believed to be that the zirconia that serves as a dielectric was not dispersed and scattered throughout the alumina, and therefore there was no interference with the transition of the zirconia crystal system from tetragonal to monoclinic. The reason why Comparative Example 3 did not show polarization is believed to be because it behaved as a conductor of oxygen ions. It is believed that Comparative Example 3 did not show polarization because the polarization was alleviated by the movement of oxygen ions. [Industrial Applicability]
[0096] Since the electret of the present invention can maintain its polarization even at high temperatures, it can control plasma at high temperatures and collect particles, and can be suitably used as a component for semiconductor manufacturing equipment such as a susceptor, a plasma etching component, or a dummy wafer. [Explanation of symbols]
[0097] 1. Ceramic materials 1a, 1b Ceramic surface 10 Phase 1 20 Phase 2 30a, 30b Electrodes 100 Muffle Furnace
Claims
1. A method for producing an electret having a ceramic material in which a first phase made of zirconia is dispersed and scattered in a second phase made of alumina, and the first phase has a crystal system including a metastable phase that is metastable at room temperature, A polarization step of polarizing the ceramic material, The first phase does not contain a stabilizer or the content of the stabilizer is 5 mol % or less, A method for producing an electret, characterized in that the content of the zirconia in the ceramic material is 5 wt % to 15 wt %.
2. The method for producing an electret according to claim 1, wherein the zirconia contains a tetragonal crystal system that is metastable at room temperature and a monoclinic crystal system that is stable at room temperature.
3. The polarization step includes sandwiching the ceramic material between a pair of electrodes, a heating step of heating the pair of electrodes at 700° C. to 1000° C. while applying a voltage to the pair of electrodes; a cooling step of cooling the pair of electrodes while applying a voltage to the pair of electrodes; The method for producing the electret according to claim 1 or 2, comprising:
4. The method for producing an electret according to claim 3, wherein in the heating step, a voltage applied to the pair of electrodes is 1 kV to 10 kV.
Citation Information
Patent Citations
massager
JP1984025748A
Alumina-zirconia compounded sintered material
JP1991223159A
High molecular composite piezoelectric material and its production
JP1994287448A
Production of ceramics sintered compact
JP1995291722A
Electret and electrostatic induction type conversion device
JP2009253050A