Film forming method and laminated body

A film forming method using a first and second coating material with specific polyol and polyisocyanate components addresses plasticizer migration and adhesion issues, resulting in a durable and aesthetically pleasing laminate for building surfaces.

JP7590879B2Active Publication Date: 2024-11-27F CONSULTANT
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021010244
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-06
Filing Date
2021-01-26
Publication Date
2024-11-27
Estimated Expiration
2041-01-26

AI Technical Summary

Technical Problem

Plasticizer migration and adhesion issues in plasticizer-containing coating materials used on building and civil engineering structures, leading to deterioration of appearance and surface contamination.

Method used

A film forming method involving a first coating material and a second coating material, where the second material contains a polyol component with a higher hydroxyl value than the first, using polyether polyols and polyisocyanate components to form a laminate that prevents plasticizer migration and enhances adhesion.

Benefits of technology

The method achieves excellent plasticizer migration prevention and adhesion, forming a durable film with improved resistance to contaminants and maintaining aesthetic qualities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590879000001
    Figure 0007590879000001
  • Figure 0007590879000002
    Figure 0007590879000002
Patent Text Reader

Abstract

To provide a film formation method in which a second coating material containing a specific polyol component (A) is applied to a first coating material containing a polyol component, a polyisocyanate component and a plasticizer to form a film.SOLUTION: In the film formation method, a first coating material and a second coating material are applied. The first coating material contains a plasticizer, and the first coating material and the second coating material contain polyol components (A) and polyisocyanate components (B) as resin components. The second coating material contains a polyol component (A2) larger in hydroxyl value than a polyol component (A1) contained in the first coating material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel method for forming a coating. [Background technology]

[0002] Conventionally, the surfaces of buildings, civil engineering structures, etc. have been covered with urethane resin coating materials containing a plasticizer ("plasticizer-containing coating materials"). Such plasticizer-containing coating materials contain a polyol component, a polyisocyanate component, and a plasticizer. In addition, a coating material may be laminated on the surface of the plasticizer-containing coating material for protection, design, etc. However, the plasticizer may migrate into the coating material over time, and the aesthetics or adhesion may be reduced due to the adhesion of contaminants to the coating material surface.

[0003] In response to this, for example, Patent Document 1 proposes a non-migratory polymer plasticizer, which is described as not migrating to the surface due to its high molecular weight. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-226442 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, generally, low molecular weight plasticizers are widely used in plasticizer-containing coating materials, and there is a demand for the development of a coating formation method that can be applied to such plasticizer-containing coating materials. [Means for solving the problem]

[0006] In order to solve these problems, the present inventors discovered that by applying a second coating material containing a specific polyol component (A) to the surface of a first coating material containing a polyol component, a polyisocyanate component, and a plasticizer to form a coating, it is possible to form a coating that is excellent in preventing plasticizer migration and has excellent adhesion, and thus completed the present invention.

[0007] That is, the present invention has the following features. 1. A coating forming method for applying a first coating material and a second coating material, the first coating material containing a plasticizer, the first coating material and the second coating material containing a polyol component (A) and a polyisocyanate component (B) as resin components, The first coating material and the second coating material each contain a polyether polyol (Ax) as the polyol component (A), and the second coating material contains a polyether polyol (Ax2) having a hydroxyl value larger than that of the polyether polyol (Ax1) of the first coating material. A method for forming a coating comprising the steps of: 2. The polyether polyol (Ax2) is characterized in that it contains a polyether polyol having a hydroxyl value of 50 mgKOH / g or more. To The coating forming method described above. 3. A laminate having a first coating formed from a first coating material and a second coating formed from a second coating material, The first coating material includes a plasticizer, The first and second coating materials each contain a polyol component (A) and a polyisocyanate component (B) as a resin component, The first coating material and the second coating material each contain a polyether polyol (Ax) as the polyol component (A), and the second coating material contains a polyether polyol (Ax2) having a hydroxyl value larger than that of the polyether polyol (Ax1) of the first coating material. A laminate comprising: 4. 4. The laminate according to claim 3, wherein the polyether polyol (Ax2) contains a polyether polyol having a hydroxyl value of 50 mgKOH / g or more. Effect of the Invention

[0008] The present invention relates to a coating formation method for applying a first coating material and a second coating material, wherein the first coating material contains a plasticizer, the first coating material and the second coating material contain a polyol component (A) and a polyisocyanate component (B) as resin components, and the second coating material contains a polyol component (A2) having a hydroxyl value greater than that of the polyol component (A1) of the first coating material, thereby making it possible to form a coating that is excellent in preventing plasticizer migration and has excellent adhesion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below based on the embodiments.

[0010] The present invention relates to a method for forming a coating film by applying a first coating material and a second coating material in this order. Both the first coating material and the second coating material in this invention contain a polyol component (A) and a polyisocyanate component (B) as resin components. The second coating material contains a polyol component (A2) having a higher hydroxyl value than the polyol component (A1) of the first coating material. Common points between the first coating material and the second coating material (hereinafter, both are also collectively referred to simply as "coating materials") will be described first.

[0011] The coating material of the present invention contains a polyol component (A) and a polyisocyanate component (B), and forms a coating film by reaction between them.

[0012] Examples of the polyol component (A) of the present invention (hereinafter also referred to as "component (A)") include polyether polyol, polyester polyol, castor oil, castor oil modified polyol, epoxy modified polyol, silicone modified polyol, fluorine modified polyol, acrylic polyol, polycarbonate polyol, polylactone polyol, polybutadiene polyol, polypentadiene polyol, and the like. The coating material of the present invention preferably contains one or more selected from polyether polyols and acrylic polyols. These polyols are preferably liquid at 20°C, and can be used in the form of a solvent-soluble type, a nonaqueous dispersion (NAD) type, and the like.

[0013] The polyether polyol (Ax) (hereinafter also referred to as "(Ax) component") is obtained by addition polymerization of polyhydric alcohols such as trimethylolpropane, glycerin, hexanetriol, pentaerythritol derivatives, sorbitol, neopentyl glycol, etc., with alkylene oxides such as ethylene oxide and propylene oxide. In the present invention, a polymer obtained by addition polymerization of the above-mentioned polyhydric alcohols with ethylene oxide and / or propylene oxide is preferred, and one having ethylene oxide and / or propylene oxide added to the terminal can also be used. Furthermore, in the present invention, it is preferable that the (Ax) component contains a polyether polyol having three or more functional groups (hydroxyl groups) having active hydrogen atoms (functional group number 3 or more). In this case, the crosslink density of the formed coating can be increased, and the effects of the present invention can be fully exhibited.

[0014] The acrylic polyol (Ay) (hereinafter also referred to as "(Ay) component") contains as constituents an alkyl (meth)acrylate ester, a hydroxyl group-containing monomer, and other monomers as necessary, and a polymer of these can be used. The alkyl (meth)acrylate ester is a compound having a (meth)acryloyl group and an alkyl group. In the present invention, the alkyl acrylate ester and the alkyl methacrylate ester are collectively referred to as alkyl (meth)acrylate ester. The monomer is a general term for a compound having a polymerizable unsaturated double bond.

[0015] Examples of such (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, t-pentyl (meth)acrylate, 1-ethylpropyl (meth)acrylate, 2-methylbutyl (meth)acrylate, and 1-methylpropyl (meth)acrylate. Examples of such acrylates include 3-methylbutyl acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, 2-methylpentyl (meth)acrylate, 4-methylpentyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-undecyl (meth)acrylate, and n-lauryl (meth)acrylate. These can be used alone or in combination of two or more.

[0016] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylate esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc. These can be used alone or in combination of two or more.

[0017] Examples of the other monomers include aromatic monomers, carboxyl group-containing monomers, amino group-containing monomers, pyridine-based monomers, nitrile group-containing monomers, amide group-containing monomers, epoxy group-containing monomers, carbonyl group-containing monomers, alkoxysilyl group-containing monomers, fluorine-containing monomers, ultraviolet absorbing group-containing monomers, photostable group-containing monomers, etc. These can be used alone or in combination of two or more.

[0018] Furthermore, in the present invention, a polyester-containing acrylic polyol containing an acrylic polyol and a polyester can also be used as the component (Ay). The polyester-containing acrylic polyol can be obtained, for example, by reacting a polyester resin having a polymerizable unsaturated group, an alkyl (meth)acrylate ester, a hydroxyl group-containing monomer, and, if necessary, other polymerizable monomers.

[0019] The polyester resin having a polymerizable unsaturated group can be obtained by using a part of the polybasic acid and / or polyhydric alcohol having a polymerizable unsaturated group when obtaining a polyester resin by condensation reaction of a polybasic acid and a polyhydric alcohol. The polyester resin having a polymerizable unsaturated group can also be obtained by reacting a monomer capable of reacting with a hydroxyl group or a carboxyl group in the polyester resin, specifically maleic acid, (meth)acrylic acid, glycidyl (meth)acrylate, etc., with the polyester resin.

[0020] The hydroxyl value of the above component (A) is preferably 1 to 1000 mgKOH / g (more preferably 3 to 900 mgKOH / g). By including such a component (A), the effects of the present invention can be fully exhibited. The hydroxyl value referred to here is a value expressed in mg of potassium hydroxide equivalent to the moles of hydroxyl groups contained in 1 g of solid content (KOH mg / g). In the present invention, "α to β" is synonymous with "α or more and β or less".

[0021] The polyisocyanate component (B) in the coating material of the present invention (hereinafter also referred to as "component (B)") is a component that undergoes a curing reaction with the component (A). In the present invention, such a curing reaction exerts sufficient effects in terms of adhesion, prevention of plasticizer migration, etc.

[0022] Examples of the component (B) include toluene diisocyanate (TDI), 4,4-diphenylmethane diisocyanate (pure-MDI), polymeric MDI, xylylene diisocyanate (XDI), hexamethylene diisocyanate (HMDI), isophorone diisocyanate (IPDI), hydrogenated XDI, hydrogenated MDI, and the like, as well as derivatives thereof which have been allophanated, biurated, dimerized (uretidione), trimerized (isocyanurated), adducted, or carbodiimidized; and blocked isocyanates which have been blocked with alcohols, phenols, ε-caprolactam, oximes, active methylene compounds, or the like. One or more selected from these may be used.

[0023] In the present invention, it is preferable that component (B) contains hexamethylene diisocyanate (HMDI) and / or its derivatives (hereinafter also referred to as "HMDIs"). The content of the HMDIs is preferably 90% by weight or more (more preferably 95% by weight or more) based on the total amount (solid content) of component (B). Also suitable is an embodiment in which component (B) consists only of HMDIs. Moreover, a biuret body is suitable as the derivative. In such a case, the formed coating has excellent curing properties, and it is possible to improve adhesion, plasticizer migration prevention, etc.

[0024] The NCO content of component (B) is preferably 10 to 35% by weight (more preferably 13 to 32% by weight, and even more preferably 15 to 30% by weight). In such a case, the adhesion can be improved. The NCO content refers to the weight % of NCO contained in component (B).

[0025] The above components (A) and (B) are mixed in such a ratio that the NCO / OH equivalent ratio of components (A) and (B) is preferably 0.6 to 3.5 (more preferably 1 to 3.0, and even more preferably 1.1 to 2.5). In such a case, the curability is excellent and the effects of the present invention can be fully exhibited.

[0026] In the present invention, a curing catalyst that promotes the reaction between the (A) component and the (B) component can be used in combination. A curing catalyst is a substance that promotes the reaction and curing of an isocyanate group. Examples of the curing catalyst include various types of amine catalysts, organometallic catalysts, and inorganic catalysts. For example, examples of the amine catalyst include ethylenediamine, triethylenediamine, triethylamine, ethanolamine, diethanolamine, and hexamethylenediamine, or their derivatives or mixtures with solvents. Examples of the organometallic catalyst include organometallic compounds such as dibutyltin dilaurate and dibutyltin diacetate; and organometallic salts such as potassium acetate, zinc stearate, calcium stearate, lead stearate, aluminum stearate, and tin octoate. Examples of the inorganic catalyst include tin chloride. These can be used alone or in combination, and can also be used by mixing with a solvent. In the present invention, it is particularly preferable to include an organometallic catalyst. In this case, curing is accelerated and sufficient effects in terms of adhesion, prevention of plasticizer migration, etc. are exhibited from the initial stage of film formation.

[0027] In addition to the above-mentioned components, various other components can be blended into the coating material of the present invention within the range that does not significantly impair the effects of the present invention. Examples of such components include color pigments, extender pigments, flame retardants, foaming agents, carbonizing agents, thickeners, plasticizers, preservatives, antifungal agents, anti-algae agents, defoamers, leveling agents, pigment dispersants, antiskinning agents, driers, matting agents, UV absorbers, light stabilizers, antioxidants, anti-pollution agents, catalysts, etc.

[0028] In the present invention, such a coating material (first coating material and second coating material) is applied (painted) to a substrate to form a coating. In the present invention, it is preferable to apply the first coating material to the substrate, dry the coating (first coating), and then apply the second coating material. The substrate constitutes the surface of a building, a civil engineering structure, etc. Specifically, the substrate can be applied to various substrates such as walls, pillars, floors, beams, roofs, stairs, ceilings, and doors. Applicable substrates include, for example, concrete, mortar, siding boards, extruded boards, gypsum boards, perlite boards, bricks, plastics, wood, metals, steel frames (steel materials), glass, and porcelain tiles. These substrates may have a coating already formed on their surfaces, may have been subjected to some kind of surface treatment (rust prevention treatment, flame retardant treatment, etc.), or may have wallpaper attached thereto.

[0029] The second coating material can be applied directly to the first coating, or through some other layer (e.g., undercoat layer, intermediate coating layer, etc.). In the present invention, it is preferable to apply the second coating material directly to the first coating. This can provide sufficient effects in terms of preventing plasticizer migration and adhesion. Such a second coating material is effective as a coating material for preventing plasticizer migration.

[0030] Next, the characteristics of the first coating material and the second coating material will be described. The first and second coating materials contain the polyol component (A) as a resin component. Furthermore, the present invention is characterized in that the second coating material contains a polyol (A2) having a hydroxyl value greater than the polyol component (A1) of the first coating material. That is, the first coating material contains a polyol component (A1) having a relatively small hydroxyl value, and the second coating material contains a polyol component (A2) having a relatively large hydroxyl value. In the present invention, by using the first and second coating materials of such a configuration, it is possible to obtain excellent plasticizer migration prevention properties and sufficient adhesion.

[0031] In the present invention, the difference in hydroxyl value between the polyol component (A1) and the polyol component (A2) is preferably 5 mgKOH / g or more (more preferably 10 mgKOH / g or more, even more preferably 50 mgKOH / g or more, particularly preferably 100 mgKOH / g or more, and most preferably 150 mgKOH / g or more). In such a case, excellent plasticizer migration prevention properties can be exhibited. Specifically, the hydroxyl value of the polyol component (A1) is preferably 1 to 200 mgKOH / g (more preferably 3 to 150 mgKOH / g). Also, the hydroxyl value of the polyol component (A2) is preferably 30 to 1000 mgKOH / g (more preferably 35 to 900 mgKOH / g). When either or both of the first and second coating materials contain multiple polyol components, it is sufficient that at least one polyol component (A1) of the first coating material and at least one polyol component (A2) of the second coating material satisfy the above conditions.

[0032] The first and second coating materials preferably contain a polyether polyol (Ax) as the polyol component (A), and the second coating material preferably contains a polyether polyol (Ax2) having a hydroxyl value greater than that of the polyether polyol (Ax1) of the first coating material. Specifically, the hydroxyl value of the polyether polyol component (Ax1) contained in the first coating material is preferably 1 to 200 mgKOH / g (more preferably 3 to 180 mgKOH / g, even more preferably 5 to 150 mgKOH / g, particularly preferably 8 to 100 mgKOH / g, and most preferably 10 to 35 mgKOH / g). The hydroxyl value of the polyether polyol (Ax2) contained in the second coating material is preferably 50 mgKOH / g or more (more preferably 100 mgKOH / g or more, even more preferably 150 mgKOH / g or more, particularly preferably 200 mgKOH / g or more, and most preferably 250 mgKOH / g or more). The upper limit is not particularly limited, but is preferably 1000 mgKOH / g or less (more preferably 800 mgKOH / g or less). In this case, the effect of the present invention can be further improved.

[0033] Furthermore, it is preferable that the second coating material contains a polyether polyol (Ax2) having a smaller molecular weight than the polyether polyol (Ax1) of the first coating material. That is, it is preferable that the first coating material contains a polyether polyol (Ax1) having a relatively large molecular weight, and the second coating material contains a polyether polyol (Ax2) having a relatively small molecular weight. This can further improve the plasticizer migration prevention property and adhesion.

[0034] The difference in molecular weight between the polyether polyol (Ax1) and the polyether polyol (Ax2) is preferably 2000 or more (more preferably 3000 or more, even more preferably 4000 or more, particularly preferably 6000 or more, and most preferably 6500 or more). In such a case, excellent plasticizer migration prevention properties can be exhibited. Specifically, the molecular weight of the polyether polyol (Ax1) is preferably 1000 or more (more preferably 3000 or more, even more preferably 5000 or more, particularly preferably 6000 or more, and most preferably 6500 or more), and the upper limit is preferably 18000 or less (more preferably 15000 or less, and even more preferably 12000 or less). The molecular weight of the polyether polyol (Ax2) is preferably 4000 or less (more preferably 2000 or less, even more preferably 1000 or less, particularly preferably 900 or less, and most preferably 600 or less), and the lower limit is preferably 50 or more (more preferably 100 or more, and even more preferably 150 or more). By using such an (Ax2) component, the plasticizer migration prevention property can be improved. In the present invention, the molecular weight of the polyol component is a number average molecular weight (Mn), which is a so-called polystyrene equivalent molecular weight determined by gel permeation chromatography using a polystyrene polymer as a reference.

[0035] When either or both of the first coating material and the second coating material contain multiple polyether polyols (Ax), it is sufficient that at least one polyether polyol component (Ax1) of the first coating material and at least one polyether polyol component (Ax2) of the second coating material satisfy the above condition, and it is more preferable that all of the polyether polyols (Ax2) of the second coating material satisfy the above condition for all of the polyether polyols (Ax1) of the first coating material.

[0036] In the first coating material, the solid content of the polyether polyol (Ax1) in the solid content of the component (A1) is preferably 50% by weight or more (more preferably 80% by weight or more, and even more preferably 90% by weight or more). There is no particular upper limit, and the component (A1) may be only the polyether polyol (Ax1). In such a case, the effects of the present invention can be fully exhibited.

[0037] On the other hand, the second coating material preferably further contains an acrylic polyol (Ay2) as the polyol component (A2). In this case, the hydroxyl value of the acrylic polyol (Ay2) is preferably 1 to 200 KOHmg / g (more preferably 3 to 100 KOHmg / g, and even more preferably 5 to 80 KOHmg / g). If the hydroxyl value of the acrylic polyol (Ay2) is within such a range, it has excellent plasticizer migration prevention properties and is also advantageous in terms of improving adhesion. In addition, the weight ratio (solid content) of the polyether polyol (Ax2) to the acrylic polyol (Ay2) is preferably 90:10 to 10:90 (more preferably 80:20 to 20:80, and even more preferably 70:30 to 50:50). In such a case, it has excellent plasticizer migration prevention properties and is also advantageous in terms of improving adhesion.

[0038] In the present invention, the solid content (total) of the polyether polyol (Ax2) and the acrylic polyol (Ay2) in the solid content of the component (A2) is preferably 50% by weight or more (more preferably 80% by weight or more, and even more preferably 90% by weight or more). There is no particular upper limit, and the component (A2) may be only the polyether polyol (Ax2) and the acrylic polyol (Ay2). In such a case, the effect of the present invention can be fully exhibited.

[0039] The first coating material of the present invention contains a plasticizer as an essential component in addition to the above-mentioned resin component. Such a first coating material is not particularly limited as long as it is a material containing a plasticizer in the above-mentioned resin component, and examples thereof include coating materials, sheets, sealing materials, plastisols, etc., which may have various functionalities (for example, waterproofness, flame retardancy, heat resistance, etc.).

[0040] The plasticizer is not particularly limited, and examples thereof include phthalate ester compounds such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diheptyl phthalate, dihexyl phthalate, di-2-ethylhexyl phthalate, dioctyl phthalate, diisononyl phthalate, diisodecyl phthalate, diundecyl phthalate, and butyl benzyl phthalate; diethyl adipate, dibutyl adipate, diisobutyl adipate, dihexyl adipate, di-2-ethylhexyl adipate, dioctyl adipate, diisononyl adipate, and diisodecyl adipate; aliphatic dibasic acid ester compounds such as bis(butyl diglycol) adipate, diethyl sebacate, dibutyl sebacate, dihexyl sebacate, and di-2-ethylhexyl sebacate; adipic acid polyester compounds such as 1,3-butylene glycol adipate polyester and 1,2-propylene glycol adipate polyester; maleic acid ester compounds such as dimethyl maleate, diethyl maleate, dibutyl maleate, dihexyl maleate, di-2-ethylhexyl maleate, diisononyl maleate, and diisodecyl maleate;

[0041] Examples of the phosphate ester compounds include triethyl phosphate, tributyl phosphate, tri-2-ethylhexyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, and 2-ethylhexyl diphenyl phosphate; trimellitic acid ester compounds such as tris-2-ethylhexyl trimellitate; ricinoleic acid ester compounds such as methyl acetyl lysinolate; epoxy ester compounds such as di-2-ethylhexyl epoxyhexahydrophthalate, diepoxystearyl epoxyhexahydrophthalate, epoxidized fatty acid butyl, epoxidized fatty acid 2-ethylhexyl, epoxidized soybean oil, and epoxidized linseed oil; benzoic acid ester compounds such as benzoic acid glycol ester; chlorinated paraffin; aromatic hydrocarbon compounds such as 1-phenyl-1-xylylethane and 1-phenyl-1-ethylphenylethane; lactones such as γ-butyrolactone; and mixtures of petroleum resins (polymers of aromatic hydrocarbon fractions having 8 to 10 carbon atoms) and styrylxylene. These may be used alone or in combination.

[0042] In the present invention, it is preferable that the first coating material contains one or more selected from a phthalate ester compound, an aliphatic dibasic acid ester compound, a phosphate ester compound, and a chlorinated paraffin. In this case, the effect of the present invention can be fully exhibited. In addition, in the present invention, even if a relatively low molecular weight plasticizer having a molecular weight of 1000 or less (preferably 100 to 800) is contained, the effect of the present invention can be fully exhibited. Note that the molecular weight of the plasticizer is a value calculated from the molecular formula.

[0043] The content of the plasticizer in the first coating material is preferably 5 to 200 parts by weight (more preferably 10 to 150 parts by weight) relative to 100 parts by weight of the total solid content of the polyol component (A1) and the polyisocyanate component (B1) (hereinafter also referred to as "resin component (solid content)"). Thus, even when a relatively large amount of plasticizer is contained, sufficient effects can be obtained in terms of plasticizer migration prevention and adhesion in the coating forming method of the present invention.

[0044] Furthermore, the first coating material may contain functional powders for imparting various functions. As the functional powder, for example, a powder that exhibits a desired function such as a heat insulation imparting powder, a heat resistance imparting powder, a UV shielding powder, or an infrared shielding powder may be used. By including such a functional powder, it is possible to impart a desired performance to the coating. As such functional powder, for example, a heat insulation imparting powder, a heat resistance imparting powder, an UV shielding powder, or the like may be mentioned. These may be used alone or in combination of two or more.

[0045] The first coating material of the present invention preferably contains a heat resistance imparting powder as a functionality imparting powder. Such a first coating material is suitable as a foamable fireproof coating material applied to surface coating of structures such as buildings and civil engineering structures. The heat resistance imparting powder may be any powder that exhibits at least one of the following effects at high temperatures: dehydration and cooling effect, non-combustible gas generation effect, binder carbonization promotion effect, carbonized heat insulation layer formation effect, and the like, and has a combustion suppressing effect, and examples of such powder include foaming agents, carbonizing agents, and flame retardants.

[0046] Specifically, examples of the foaming agent include melamine and its derivatives, dicyandiamide and its derivatives, azobistetrazole and its derivatives, azodicarbonamide, urea, and thiourea. These can be used alone or in combination of two or more. The content of the foaming agent is preferably 10 to 200 parts by weight (more preferably 20 to 150 parts by weight) per 100 parts by weight of the resin component (solid content). The foaming agent of the present invention imparts a foaming action to the coating due to a temperature rise during a fire or the like, and specifically, imparts a foaming action when the temperature of the coating surface is preferably 200°C or higher.

[0047] Examples of the carbonizing agent include pentaerythritol, dipentaerythritol, trimethylolpropane, starch, and casein. These can be used alone or in combination of two or more. In the present invention, pentaerythritol and dipentaerythritol are particularly preferred because they have excellent dehydration and cooling effects and carbonized heat insulating layer forming effects. The content of the carbonizing agent is preferably 10 to 200 parts by weight (more preferably 20 to 120 parts by weight) per 100 parts by weight of the resin component (solid content). The carbonizing agent of the present invention imparts the effect of forming a carbonized heat insulating layer by carbonizing the resin component and dehydrating and carbonizing it due to a temperature rise during a fire or the like.

[0048] Examples of the flame retardant include organic phosphorus compounds such as tricresyl phosphate and diphenyl cresyl phosphate; chlorine compounds such as chlorinated polyphenyl, chlorinated polyethylene, diphenyl chloride, triphenyl chloride, chlorinated paraffin, pentachlorinated fatty acid ester, perchloropentacyclodecane, chlorinated naphthalene, and tetrachlorophthalic anhydride; antimony compounds such as antimony trioxide and antimony pentachloride; phosphorus compounds such as phosphorus trichloride, phosphorus pentachloride, ammonium phosphate, ammonium polyphosphate, melamine phosphate, melamine polyphosphate, melam polyphosphate, melem polyphosphate, boron phosphate, boron polyphosphate, aluminum phosphate, and aluminum polyphosphate; and inorganic compounds such as zinc borate and sodium borate. These can be used alone or in combination of two or more. The content of the flame retardant is preferably 100 to 1000 parts by weight (more preferably 200 to 800 parts by weight) relative to 100 parts by weight of the resin component (solid content).

[0049] Furthermore, the first coating material may contain a filler, fiber, etc. Examples of the filler include talc, calcium carbonate, sodium carbonate, aluminum oxide (alumina), titanium oxide, zinc oxide, silica, clay, clay, shirasu, mica, silica sand, silica stone powder, quartz powder, barium sulfate, aluminum hydroxide, magnesium hydroxide, etc. These can be used alone or in combination of two or more. Examples of the fiber include organic fibers such as acrylic fiber, acetate fiber, aramid fiber, cuprammonium fiber (cupra), nylon fiber, novoloid fiber, pulp fiber, viscose rayon, vinylidene fiber, polyester fiber, polyethylene fiber, polyvinyl chloride fiber, polychlar fiber, boronosic fiber, polypropylene fiber, and cellulose fiber, and inorganic fibers such as carbon fiber, rock wool fiber, glass fiber, silica fiber, alumina fiber, silica-alumina fiber, slag wool fiber, ceramic fiber, carbon fiber, and silicon carbide fiber. These can be used alone or in combination of two or more.

[0050] The second coating material of the present invention preferably contains a powder component such as a color pigment, an extender pigment, etc., in addition to the resin component. This enhances the cohesive force during coating formation, and provides better effects in terms of adhesion, etc. In order to obtain such effects, a desirable embodiment contains 1 to 200 parts by weight (preferably 5 to 150 parts by weight) of the powder component per 100 parts by weight of the total solid content of the polyol component (A2) and the polyisocyanate component (B2). Examples of color pigments include titanium oxide, zinc oxide, carbon black, graphite, black iron oxide, iron-manganese composite oxide, iron-copper-manganese composite oxide, iron-chromium composite oxide, iron-chromium-cobalt composite oxide, copper-chromium composite oxide, copper-manganese-chromium composite oxide, copper-magnesium composite oxide, bismuth-manganese composite oxide, red iron oxide, molybdate orange, permanent red, permanent carmine, anthraquinone red, perylene red, quinacridone red, yellow iron oxide, titanium yellow, fast yellow, benzimidazolone yellow, chrome green, cobalt green, phthalocyanine green, ultramarine blue, Prussian blue, cobalt blue, phthalocyanine blue, quinacridone violet, dioxazine violet, aluminum pigments, and pearl pigments. These can be used alone or in combination of two or more. Examples of extender pigments include heavy calcium carbonate, clay, kaolin, talc, precipitated barium sulfate, barium carbonate, white carbon, and diatomaceous earth.

[0051] The coating material of the present invention may be applied by mixing the base agent containing the polyol component (A) and the curing agent containing the polyisocyanate component (B) immediately before coating. The solvent may be contained in either the base agent or the curing agent, or in both. In addition, in the present invention, a solvent may be mixed as a diluent at the time of coating, in addition to the base agent and the curing agent. In particular, the solvent of the second coating material is preferably contained in an amount of 5 to 500 parts by weight (preferably 10 to 400 parts by weight, more preferably 20 to 300 parts by weight) relative to 100 parts by weight of the total solid content of the (A) component and the (B) component. If the content of the solvent is within such a range, it is preferable in terms of preventing plasticizer migration, the finish of the topcoat material, and the like. In particular, it is preferable that the solid content of the coating material of the present invention after dilution is 25 to 90% by weight (more preferably 30 to 85% by weight). If it is within such a range, the above-mentioned effect can be further enhanced.

[0052] The coating material of the present invention can be applied by various methods, such as brush coating, roller coating, spray coating, etc. The amount of coating and the number of coats when applying the first coating material may be set according to the functionality of each coating material. The amount of coating when applying the first coating material is preferably 0.5 to 5.0 kg / m 2 (More preferably 0.8 to 3.0 kg / m 2 The first coating material is preferably applied once or twice. On the other hand, the amount of the second coating material applied is preferably 30 to 500 g / m 2 (More preferably 50 to 300 g / m 2 The number of coats of the second coating material may be appropriately determined depending on the surface condition of the film formed by the first coating material, and is preferably 1 to 2 coats. Note that the coating material of the present invention can sufficiently exhibit plasticizer migration prevention properties even when coated once.

[0053] In the present invention, in order to protect the coating film formed by the above-mentioned coating material (first coating material and second coating material), a topcoat material can be applied as necessary. Such a topcoat material can be formed by applying a known topcoat material. As the topcoat material, for example, any of clear type or colored type, glossy type or matte type, hard type or elastic type, thin film type or thick film type can be used. In addition, it may be either water-based or solvent-based, and can be appropriately selected according to the desired purpose.

[0054] The topcoat material of the present invention preferably contains a resin component. Examples of the form of such resin include solvent-soluble resin, non-aqueous dispersion resin, solventless resin, water-dispersed resin, water-soluble resin, etc. Examples of the type of resin include acrylic resin, urethane resin, epoxy resin, vinyl chloride resin, vinyl acetate resin, acrylic silicone resin, fluororesin, silicon resin, polyvinyl alcohol, cellulose derivatives, etc., or composites thereof. These can be used in one or more types. In the present invention, it is particularly preferable to include one or more types selected from urethane resin, epoxy resin, acrylic resin, acrylic silicone resin, and fluororesin.

[0055] Furthermore, the resin component may have crosslinking reactivity. When the resin component is a crosslinking reaction type resin, the water resistance, durability, and adhesion of the formed coating are improved, and the occurrence of swelling and peeling of the coating due to rainfall, condensation, etc. can be suppressed. Furthermore, when the first coating material contains a functional powder, various functionalities (for example, heat resistance, etc.) can be stably maintained. Such a crosslinking reaction type resin may be either one that causes a crosslinking reaction by itself or one that causes a crosslinking reaction by a crosslinking agent that is mixed separately. Such crosslinking reactivity can be imparted by combining reactive functional groups such as a hydroxyl group and an isocyanate group, a carbonyl group and a hydrazide group, an epoxy group and an amino group, an aldo group and a semicarbazide group, a keto group and a semicarbazide group, alkoxyl groups, a carboxyl group and a metal ion, a carboxyl group and a carbodiimide group, a carboxyl group and an epoxy group, a carboxyl group and an aziridine group, or a carboxyl group and an oxazoline group. Among these, it is preferable to contain a crosslinking reactive resin which generates one or more crosslinking reactions selected from the group consisting of a hydroxyl group and an isocyanate group, a carbonyl group and a hydrazide group, and an epoxy group and an amino group.

[0056] As components other than the resin component of the above-mentioned topcoat material, for example, color pigments, extender pigments, aggregates, etc. can be mixed. By appropriately blending such components, it is possible to express the desired color and texture. The amount of color pigments, extender pigments, aggregates, etc. to be mixed is not particularly limited as long as it is within a range that does not inhibit the effect of the above-mentioned coating material, but is preferably 1 to 2000 parts by weight (more preferably 5 to 1000 parts by weight) relative to 100 parts by weight of the solid content of the resin component.

[0057] In the present invention, it is particularly preferable to use pigments having infrared reflectivity and / or infrared transmittance as the color pigments and extender pigments, which can further increase the durability of the formed coating.

[0058] Examples of pigments having infrared reflectivity include aluminum flakes, titanium oxide, barium sulfate, zinc oxide, iron oxide, calcium carbonate, silicon oxide, magnesium oxide, zirconium oxide, yttrium oxide, indium oxide, alumina, iron-chromium composite oxide, manganese-bismuth composite oxide, manganese-yttrium composite oxide, black iron oxide, iron-manganese composite oxide, iron-copper-manganese composite oxide, iron-chromium-cobalt composite oxide, copper-chromium composite oxide, copper-manganese-chromium composite oxide, and the like, and one or more of these can be used.

[0059] Examples of pigments having infrared transmittance include perylene pigments, azo pigments, yellow lead, titanium red, cadmium red, quinacridone red, isoindolinone, benzimidazolone, phthalocyanine green, phthalocyanine blue, cobalt blue, indanthrene blue, ultramarine, and Prussian blue, and one or more of these can be used.

[0060] Furthermore, the topcoat material can also contain various additives that can be used in normal paints. Examples of such additives include thickeners, film-forming assistants, leveling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, defoamers, adsorbents, ultraviolet absorbers, light stabilizers, antioxidants, fibers, low-pollution agents, hydrophilizing agents, water repellents, coupling agents, catalysts, etc.

[0061] The topcoat material may be applied by a known application method, for example, by using various methods such as brush coating, roller coating, spray coating, etc. The amount of coating is preferably 30 to 5000 g / m 2 (More preferably 50 to 3000 g / m 2 The number of coats of the topcoat material may be set appropriately, but is preferably 1 to 2 times. Drying is preferably performed at room temperature.

[0062] According to the present invention, a laminate having a first coating formed by the first coating material and a second coating formed by the second coating material can be obtained. The laminate of the present invention is excellent in preventing migration of plasticizers and can exhibit excellent adhesion. Furthermore, the laminate of the present invention has a topcoat layer formed by a topcoat material on the second coating, so that it is excellent in preventing migration of plasticizers and has excellent adhesion, and can also improve aesthetics and weather resistance. EXAMPLES

[0063] The following examples will clarify the features of the present invention, but the present invention is not limited to these examples.

[0064] <Coating material> (Main ingredient 1-15) According to the formulation shown in Table 1, component (A), color pigment, curing catalyst, and additives were mixed in a conventional manner to prepare a base resin. The following raw materials were used:

[0065] Polyol (A) Polyether polyol (Ax) (Ax-1) Polyether polyol (hydroxyl value 17 mg KOH / g, functionality 3, number average molecular weight 10,000, solid content 100% by weight) (Ax-2) Polyether polyol (hydroxyl value 24 mg KOH / g, functionality 3, number average molecular weight 7000, solid content 100% by weight) (Ax-3) Polyether polyol (hydroxyl value 55 mg KOH / g, functionality 3, number average molecular weight 3000, solid content 100% by weight) (Ax-4) Polyether polyol (hydroxyl value 160 mg KOH / g, functionality 3, number average molecular weight 1000, solid content 100% by weight) (Ax-5) Polyether polyol (hydroxyl value 230 mg KOH / g, functionality 3, number average molecular weight 700, solid content 100% by weight) (Ax-6) Polyether polyol (hydroxyl value 400 mg KOH / g, functionality 3, number average molecular weight 400, solid content 100% by weight) Acrylic polyol (Ay) (Ay-1) Acrylic polyol (hydroxyl value 40 KOHmg / g, solid content 50% by weight, medium: aromatic hydrocarbon compound, ester compound) (Ay-2) Polyester-containing acrylic polyol (hydroxyl value 40 KOHmg / g, polyester ratio 10% by weight, solid content 50% by weight, medium: aromatic hydrocarbon compound, ester compound) The above component (A) is a liquid at 20°C.

[0066] Plasticizer 1: Diisononyl phthalate (molecular weight 419) Plasticizer 2: Diisononyl adipate (molecular weight 399) Functional powders: flame retardants, foaming agents, carbonizing agents, etc. Color pigment: Titanium dioxide, average particle size 0.3 μm ·Curing catalyst: Organometallic catalyst Additives 1: Dispersants, defoamers, etc. Additive 2: Dilution solvent (aromatic hydrocarbon)

[0067] (Hardening agent 1) A curing agent was prepared by mixing 80 parts by weight of polyisocyanate (B) (biuret type hexamethylene diisocyanate, NCO content 23.5%) and 20 parts by weight of a dilution solvent (aromatic hydrocarbon).

[0068] (Preparation of coating material) The base materials 1 to 15 and the curing agent shown in Table 1 were mixed so that the NCO / OH equivalent ratio of the polyol component and the polyisocyanate component was 1.2, to obtain coating materials 1 to 15.

[0069] [Table 1]

[0070] <Top coat material> The main agent was prepared by uniformly mixing and stirring 100 parts by weight of acrylic polyol (hydroxyl value 20 KOHmg / g, solid content 50% by weight, medium: aliphatic hydrocarbon compound), 40 parts by weight of titanium dioxide, and 10 parts by weight of additives (thickener, defoamer) in a conventional manner. Next, 50 parts by weight of polyisocyanate (adduct type hexamethylene diisocyanate, NCO content 12%) and 50 parts by weight of dilution solvent (aliphatic hydrocarbon) were mixed to prepare the hardener. The main agent and hardener were mixed so that the NCO / OH equivalent ratio of the polyol component and the polyisocyanate component was 1.0, respectively, to prepare the topcoat material.

[0071] (Examples 1 to 12, Comparative Examples 1 to 3) The following evaluations were carried out for each coating material, and the results are shown in Table 2.

[0072] Preparation of test specimen [I] The first coating material is applied at 1.5 kg / m to a 150 mm x 70 mm steel plate. 2 The coating was then sprayed at a rate of 100 g / m2 and left to cure for 7 days. 2 The test specimen [I] was prepared by brushing and curing for 24 hours. The combination of the first and second coating materials is shown in Table 2. The painting and curing were all carried out under standard conditions (temperature 23°C and relative humidity 50%). <Evaluation of plasticizer migration prevention> The prepared specimen [I] was left in an incubator at 50°C or 80°C for one week. The specimen was removed from the incubator, placed horizontally and black silica sand was sprinkled on it. The specimen was then immediately stood upright and the black silica sand was allowed to fall naturally. The extent of the black silica sand that had adhered was visually confirmed to evaluate the plasticizer migration prevention properties. The evaluation was done on a four-point scale (A>B>C>D), with "A" being for samples with almost no black silica sand adhering and "D" being for samples with significant black silica sand adhering.

[0073] <Adhesion Evaluation 1> The prepared specimen [I] was evaluated for adhesion to the surface of the plasticizer-containing material by the cross-cut tape method in accordance with JIS K 5600-5-6. The evaluation criteria were as follows: A: Defect area is less than 10% B: The area of ​​the defect is 10% or more but less than 25% C: Defective area is 25% or more but less than 50% D: Defective area is 50% or more

[0074] [Table 2]

[0075] In Examples 1 to 12, good plasticizer migration prevention properties were obtained and a coating film having good adhesion was formed. In particular, in Examples 6 to 11, excellent plasticizer migration prevention properties were exhibited, and further, in Examples 5 to 11, a coating film having excellent adhesion was formed.

[0076] Next, the following evaluations were carried out for Examples 6 to 11. The results are shown in Table 2. - Preparation of test specimen [II] The first coating material is applied at 1.5 kg / m to a 150 mm x 70 mm steel plate. 2 The coating was then sprayed at a rate of 100 g / m2 and left to cure for 7 days. 2 The coating was applied with a brush and left to cure for 24 hours. The combination of the first and second coating materials is shown in Table 2. Next, apply the topcoat at a rate of 0.3 kg / m 2 The coating and curing were all carried out under standard conditions (temperature 23°C and relative humidity 50%).

[0077] <Adhesion evaluation 2> The prepared specimen [II] was evaluated for adhesion to the coating material and topcoat material using the cross-cut tape method in accordance with JIS K 5600-5-6. The evaluation criteria were the same as those for Adhesion Evaluation 1 above.

[0078] <Heat resistance protection evaluation> The prepared specimen [II] was left in an incubator at 80°C for one week, and then the foaming ratio and the steel plate backside temperature were measured when radiant heat of 50 kW / m2 was radiated onto the surface of the specimen for 15 minutes using an electric heater (CONEIII, manufactured by Toyo Seiki Co., Ltd.) based on the ISO 5660-1 cone calorimeter method. The evaluation criteria are as follows. The results are shown in Table 2. (Expansion Ratio) AA: Expansion ratio over 35 times A: Expansion ratio: 25 times or more and 35 times or less B: Expansion ratio: 20 times or more and 25 times or less C: Foaming ratio more than 15 times and less than 20 times D: Expansion ratio 15 times or less (backside temperature) AA: Less than 430℃ A: 430℃ or higher and less than 470℃ B: 470℃ or higher and less than 500℃ C: 500℃ or higher but lower than 550℃ D: 550℃ or more

[0079] In Examples 6 to 11, a carbonized heat insulating layer was formed with excellent foaming properties, and heat-resistant protection of the substrate was obtained.

Claims

1. A coating forming method for applying a first coating material and a second coating material, the first coating material containing a plasticizer, the first coating material and the second coating material containing a polyol component (A) and a polyisocyanate component (B) as resin components, the first coating material and the second coating material each contain a polyether polyol (Ax) as the polyol component (A), and the second coating material contains a polyether polyol (Ax2) having a hydroxyl value larger than the polyether polyol (Ax1) of the first coating material.

2. 2. The method for forming a coating film according to claim 1, wherein the polyether polyol (Ax2) contains a polyether polyol having a hydroxyl value of 50 mg KOH / g or more.

3. A laminate having a first coating formed of a first coating material and a second coating formed of a second coating material, the first coating material contains a plasticizer, the first coating material and the second coating material contain a polyol component (A) and a polyisocyanate component (B) as resin components, the first coating material and the second coating material each contain a polyether polyol (Ax) as the polyol component (A), and the second coating material contains a polyether polyol (Ax2) having a hydroxyl value larger than the polyether polyol (Ax1) of the first coating material.

4. The laminate described in Claim 3, characterized in that the polyether polyol (Ax2) contains a polyether polyol having a hydroxyl value of 50 mg KOH / g or more.

Citation Information

Patent Citations

  • Method for Anti-staining finishing of coating face using sealing material

    JP1997262539A

  • Surface finishing coating material composition and its performing method

    JP1998067964A

  • Waterproof structure and forming method thereof

    JP1999077940A

  • Polymeric plasticizer

    JP2001226442A

  • Urethane waterproof structure and environment-responsive type topcoat material using therefor

    JP2007000720A