Niobium oxide powder

Niobium oxide powder with a D50 ratio of 5 or less, achieved through ultrasonic treatment, addresses the issue of poor fluidity and aggregation, enhancing its suitability for thin film forming materials and optical products.

JP7591001B2Active Publication Date: 2024-11-27MITSUI MINING & SMELTING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022044331
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-31
Filing Date
2022-03-18
Publication Date
2024-11-27
Estimated Expiration
2042-03-18

AI Technical Summary

Technical Problem

Conventional niobium oxide powders exhibit poor fluidity due to low bulk density, leading to aggregation and reduced mixability, which affects their suitability as raw materials for thin film forming materials and optical products.

Method used

The development of niobium oxide powder with a specific D50 ratio of 5 or less, achieved through ultrasonic treatment, resulting in a fused particle structure that suppresses aggregation and enhances fluidity.

Benefits of technology

The niobium oxide powder demonstrates excellent fluidity and mixability, making it suitable for applications such as sputtering targets and fine ceramics, with improved reactivity when mixed with lithium carbonate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591001000004
    Figure 0007591001000004
  • Figure 0007591001000005
    Figure 0007591001000005
  • Figure 0007591001000001
    Figure 0007591001000001
Patent Text Reader

Abstract

To provide a niobium oxide powder that has excellent flowability and is suitable as a thin film-forming material such as a sputtering target, an optical product, or raw material for fine ceramic and the like.SOLUTION: A niobium oxide powder has the ratio between D50 (N) and D50 (U), D50 (N) / D50 (U), of 5 or less where D50 (N) denotes a median diameter of niobium oxide particles and D50 (U) denotes a median diameter of the ultrasound-irradiated niobium oxide particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to niobium oxide powder. [Background technology]

[0002] Niobium oxide powder is widely used as a raw material for thin film forming materials such as lithium niobate (LN) single crystals, deposition pellets, and sputtering targets, optical products, and fine ceramics. Niobium oxide powder is required to have good fluidity and uniform mixability. Except for some applications, it is also required to be easy to sinter at low temperatures and to react with powders other than niobium oxide powder at low temperatures.

[0003] Conventionally, niobium oxide powders used for the above-mentioned applications have been, for example, powders having an average particle size of 2.0 μm or less and a BET specific surface area of ​​5.0 m 2 / g or more, a niobium oxide powder having a relatively small particle size and a large specific surface area has been used (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-103814 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the niobium oxide powder disclosed in Patent Document 1 had a bulk density (TD) of 0.5 g / mL or less, and was therefore very bulky (low bulk density), prone to aggregation, and had an unsatisfactory level of fluidity.

[0006] In view of the above problems, the present invention provides a niobium oxide powder having excellent fluidity. [Means for solving the problem]

[0007] The niobium oxide powder of the present invention, which has been made to solve the above problems, is characterized in that the ratio D50(N) / D50(U) of the median diameter D50(N) of niobium oxide particles to the median diameter D50(U) obtained by irradiating the niobium oxide particles with ultrasound is 5 or less. First, niobium oxide in the present invention is represented by the general formula Nb2O5 (niobium pentoxide), but also includes various oxides having different oxidation numbers, and may include the compound alone, its hydrate, or its ammonium salt. When the ratio D50(N) / D50(U) (also referred to as the D50 ratio) of the median diameter D50(N) of the niobium oxide particles to the median diameter D50(U) obtained by irradiating the niobium oxide particles with ultrasonic waves is 5 or less, the change in average particle size due to the presence or absence of ultrasonic treatment is small, and the niobium oxide particles have a structure in which they are fused to each other. When the primary particles have a fused structure (see FIG. 1) in which they are fused to each other, aggregation is suppressed, and as a result, the D50 ratio approaches the lower limit of 1, that is, a state in which there is no dispersion of aggregates by ultrasonic dispersion. By having such a fused structure, the formation of aggregates is suppressed and the fluidity is excellent, making it suitable as a raw material for thin film formation materials such as sputtering targets, optical products, or fine ceramics. Therefore, the D50 ratio is preferably 1 or more and 5 or less. Here, a D50 ratio of 1 indicates an ideal state in which there is no dispersion of aggregates by ultrasonic dispersion, so the closer the D50 ratio is to 1, the better, and it may be, for example, 1.1 or more or 1.2 or more. Also, the D50 ratio is more preferably 3 or less, even more preferably 2 or less, and particularly preferably 1.5 or less. On the other hand, if the D50 ratio exceeds 5, the above-mentioned fused structure cannot be sufficiently formed, and excessive aggregates that are largely dispersed by ultrasonic irradiation are formed, resulting in a decrease in fluidity.

[0008] Here, D50 indicates the particle diameter that reaches 50% in terms of volume fraction. In the present invention, the particle size distribution is evaluated by a dynamic light scattering method conforming to JIS Z 8828:2019 using a laser diffraction / scattering particle size distribution measuring device (manufactured by Microtrack Bell Co., Ltd.: MT3300EXII). In addition, filtering is not performed, and a dispersion treatment using ultrasonic waves as follows is performed.

[0009] Specifically, the median diameter D50(N) of niobium oxide particles is the median diameter of niobium oxide powder subjected to particle size evaluation without undergoing ultrasonic dispersion treatment. The median diameter D50(N) of niobium oxide particles also includes the median diameter D50 of niobium oxide particles subjected to ultrasonic dispersion treatment at a frequency and time shorter than the ultrasonic irradiation time described below. On the other hand, the median diameter D50(U) obtained by irradiating niobium oxide particles with ultrasonic waves is the median diameter of niobium oxide powder subjected to particle size evaluation immediately after undergoing ultrasonic dispersion treatment. Specifically, the procedure for ultrasonic dispersion treatment is as follows. First, as a pretreatment for ultrasonic dispersion treatment, 1 mg of sample powder, pure water 20 mL of the solution is placed in a 50 mL wide-mouth PP bottle, which is then placed in an ultrasonic cleaner (VS-100III, manufactured by AS ONE Corp.). The inside of the cleaner is then filled with pure water up to 5 cm above the floor, and ultrasonic dispersion treatment is carried out for 60 minutes at a frequency of 28 kHz and an output of 100 W.

[0010] In addition, in the niobium oxide powder of the present invention, the specific surface area SSA of the niobium oxide particles is 1 m 2 / g or less. The specific surface area (SSA) of niobium oxide particles is 1m 2 / g or less, the niobium oxide particles are fused to each other, so the specific surface area (SSA) tends to be small, especially at 1 m 2 / g or less is preferable in terms of improving fluidity since the adhesive force between particles is further reduced and the formation of aggregates can be suppressed. Here, the specific surface area SSA of the niobium oxide particles is measured in accordance with "6.2 Fluidization method (3.5) Single point method" of JIS R 1626-1996 (Method of measuring specific surface area of ​​fine ceramic powder by gas adsorption BET method). At that time, a mixed gas of helium as a carrier gas and nitrogen as an adsorbate gas is used. The lower limit of the specific surface area SSA of the niobium oxide particles is 0 m 2 The specific surface area (SSA) of the niobium oxide particles becomes smaller as the niobium oxide particles form more fused structures. For example, 2 / g or 0.2m 2 / g.

[0011] In addition, the niobium oxide powder of the present invention has a specific surface area SSA of 0.4 m 2 / g or less. The specific surface area (SSA) of niobium oxide particles is 0m 2 / g excess 0.4m 2 When the specific surface area SSA of the niobium oxide particles is 0.3 m / g or less, the flowability is further improved, as described above. 2 It is more preferable that the ratio is 1 / g or less.

[0012] The niobium oxide powder of the present invention is characterized in that the degree of compression calculated based on the loose bulk density AD and the compacted bulk density TD is 25% or less. The niobium oxide powder of the present invention is characterized in that the degree of compression is 20% or less. The smaller the degree of compression calculated based on the loose bulk density AD and the hardened bulk density TD, the less likely the niobium oxide powder of the present invention will aggregate when loaded into a hopper even under pressure, and the less likely it will stick to the wall of the hopper, so that high fluidity can be maintained, which is preferable. Specifically, the degree of compression is preferably 25% or less, more preferably 20% or less, and even more preferably 18% or less. Here, the theoretically ideal degree of compression is 0%, but it may be 10% or more, or 15% or more.

[0013] Here, the method for measuring the compacted bulk density TD is to measure the compacted bulk density in accordance with "Part 12: Apparent density or apparent specific volume - Section 2: Tamp method" of JIS K 5101-12-2:2004 (Methods for measuring pigments). The method for measuring the loose bulk density AD is to measure the loose bulk density in accordance with "Part 12: Apparent density or apparent specific volume - Section 1: Static method" of JIS K 5101-12-1:2004 (Methods for measuring pigments). The compressibility calculated based on the loose bulk density AD and the compacted bulk density TD is calculated by the following formula: Compressibility (%) = ([Compacted bulk density] - [Loose bulk density] / [Compacted bulk density]) x 100.

[0014] Furthermore, the compacted bulk density TD is preferably 1.5 g / mL or more. Niobium oxide powder having a compacted bulk density TD of 1.5 g / mL or more is preferred in that it has a small degree of compression. Furthermore, the compacted bulk density TD is more preferably 2.0 g / mL or more, even more preferably 2.1 g / mL or more, particularly preferably 2.3 g / mL or more, and particularly preferably 2.5 g / mL or more. Furthermore, the compacted bulk density TD is preferably 4.0 g / mL or less, and more preferably 3.0 g / mL or less. On the other hand, the loose bulk density AD is preferably 0.7 g / mL or more. Niobium oxide powder having a loose bulk density AD of 0.7 g / mL or more is preferred in that it has a small degree of compression. Furthermore, the loose bulk density AD is more preferably 1.0 g / mL or more, even more preferably 1.5 g / mL or more, and particularly preferably 1.6 g / mL or more. Also, the loose bulk density AD is preferably 3.0 g / mL or less, and more preferably 2.0 g / mL or less.

[0015] The niobium oxide powder of the present invention is characterized in that the median diameter D50(U) is 5 μm or more and 120 μm or less. The niobium oxide powder of the present invention is preferred in that if it has a fused structure in the particle size range of the median diameter D50(U) of 5 μm or more and 120 μm or less, it tends to be difficult to reduce the diameter by the above-mentioned dispersion treatment.

[0016] The niobium oxide powder of the present invention described above is generally produced as follows. First, raw materials such as ores, alloys, or scraps containing niobium are prepared, and the raw materials are put into a vibration mill to be pulverized. The pulverized product obtained is treated with an alkaline aqueous solution and washed with a mineral acid, thereby dissolving the niobium in the raw materials with hydrofluoric acid to obtain a solution containing niobium. Then, a niobium extraction solution adjustment solution is obtained by adjusting the concentration of hydrofluoric acid and the concentration of mineral acids other than hydrofluoric acid (e.g., sulfuric acid) in the solution containing niobium. This niobium extraction solution adjustment solution is separated and refined by solvent extraction using an organic solvent of 4-methyl-2-pentanone to obtain a niobium fluoride solution (hereinafter referred to as a niobium purified solution). Next, ultrapure water is added to the niobium purified solution to obtain a niobium diluted solution. Furthermore, the niobium diluted solution and the ammonia water are mixed by a reverse neutralization method in which the niobium diluted solution is added to ammonia water to obtain a precipitate slurry containing niobium. The obtained precipitated slurry is subjected to solid-liquid separation, and the precipitated slurry obtained by the solid-liquid separation is washed with a washing liquid and ultrapure water, and then squeezed to obtain a precipitated cake. The precipitated cake is then roasted, and the roasted product is pulverized to obtain the niobium oxide powder of the present invention.

[0017] When the above-mentioned niobium refined liquid is subjected to solvent extraction, the organic solvent used in the solvent extraction is preferably tributyl phosphate in addition to 4-methyl-2-pentanone. Note that 4-methyl-2-pentanone can be used without dilution, but tributyl phosphate is often used after being diluted with a diluent such as a petroleum-based hydrocarbon.

[0018] The niobium fluoride solution thus separated and purified by solvent extraction has a niobium concentration of 50 g / L to 500 g / L, more preferably 70 g / L to 400 g / L, calculated as niobium oxide (Nb2O5). When the niobium concentration in the solution is 50 g / L to 500 g / L, calculated as niobium oxide (Nb2O5), the amount of wastewater can be kept within an appropriate amount, and unnecessary costs and labor are not required for wastewater treatment, and the heat generated when the niobium fluoride solution is mixed with a precipitant in the subsequent process can be suppressed, and the temperature during precipitation can be kept below a predetermined temperature. The niobium in the niobium fluoride solution is considered to be H2NbOF5 or H2NbOF7. Here, in the case of the niobium fluoride solution obtained by the solvent extraction method, since there is little excess hydrofluoric acid, most of the niobium in the niobium fluoride solution is considered to be H2NbOF5.

[0019] The process for obtaining the above-mentioned niobium-containing precipitate slurry, i.e., the mixing and precipitation process, is characterized in that ultrapure water is added to a niobium purified solution obtained by solvent extraction of a solution in which niobium is dissolved, and the obtained niobium diluted solution is added to an alkaline aqueous solution by a reverse neutralization method to generate a niobium-containing precipitate slurry. The above-mentioned mixing and precipitation step uses a reverse neutralization method in which a niobium dilute solution is added to an alkaline aqueous solution, for example, ammonia water, and therefore, since an acidic niobium dilute solution is added to an alkaline ammonia water, niobium hydroxide can be produced while maintaining a high pH. Here, an alkaline aqueous solution of ammonia water is used as a precipitant used to produce the precipitation slurry. Although ammonia in gaseous, liquid, or aqueous form can be used, an aqueous ammonia solution (ammonia water) is more preferable in terms of ease of handling. Specifically, the ammonia water used as the precipitant is preferably 10% by weight or more, more preferably 25% by weight or more. In addition to ammonia water, other neutralizing agents such as caustic soda and ammonium hydrogen carbonate may also be used, and ammonia water may also be used in combination with other neutralizing agents such as caustic soda and ammonium hydrogen carbonate.

[0020] In the mixing and precipitation process, the pH of the alkaline aqueous solution to which the niobium dilution solution is added is preferably 10 or more. The pH of the alkaline aqueous solution is always 10 or more, that is, niobium hydroxide can be generated while maintaining the alkalinity, which is advantageous in that niobium oxide with a large average particle size can be easily formed. Here, if the pH of the alkaline aqueous solution is less than 10, it is difficult to form a structure in which the niobium oxide particles are fused together, and the amount of niobium remaining in the solution increases, and the yield of the precipitate decreases, that is, the yield of the niobium oxide decreases. On the other hand, if the pH of the alkaline aqueous solution exceeds 11, the particle size of the niobium oxide particles becomes too large, which may hinder the uniformity of the mixture mixed and reacted with other powders. The process of washing and squeezing the generated precipitate slurry becomes difficult. In addition, in the positive neutralization method in which an alkaline aqueous solution is added to an acidic niobium dilution solution, niobium hydroxide is generated while the pH of the mixture of the niobium dilution solution and the alkaline aqueous solution changes from acidic to alkaline, so the average particle size of the niobium oxide formed is unlikely to become large. The pH is measured by placing a tabletop pH meter (Horiba, Ltd.: F-71S: Standard ToupH electrode) in the precipitation tank, and measuring the mixture of the diluted niobium solution and the alkaline aqueous solution during the addition of the diluted niobium solution and during stirring for 10 minutes after the addition. The pH is measured after confirming that the temperature of the solution has stabilized at 25°C. Furthermore, during the mixing and precipitation process, the temperature of the mixture of the diluted niobium solution and the alkaline aqueous solution may be adjusted to 100°C or lower. The temperature of the mixture is preferably adjusted to 80°C or lower, more preferably 50°C or lower, and even more preferably to room temperature. Here, in order to adjust the temperature to the above-mentioned range, heating with steam or a heater, or cooling with a heat exchanger or a cooling unit may be performed.

[0021] The precipitated slurry after solid-liquid separation can be washed with a washing liquid and ultrapure water to reduce the amount of remaining fluorine. For example, when filtering using a filter, the precipitated slurry can be washed by passing a washing liquid through the filter, or by feeding the filter cake and the washing liquid into a washing tank equipped with a stirring means, stirring the mixture, and filtering again. When a filter is not used and a supernatant liquid is extracted after settling of the precipitate, the washing is performed by a method in which the supernatant liquid is extracted, the washing liquid is added, the mixture is thoroughly stirred, stirring is stopped, the precipitate is allowed to settle, and the supernatant liquid is extracted. Such a series of washing operations is performed multiple times.

[0022] The cleaning liquid is preferably an ammoniacal aqueous solution, which is an aqueous solution containing ammonia or ammonium ions and is the same type of aqueous solution as the precipitant. Specifically, ammonia water of 5.0% by weight or less is preferable, ammonia water of 4.0% by weight or less is more preferable, ammonia water of 3.0% by weight or less is even more preferable, and ammonia water of 2.5% by weight is particularly preferable. With ammonia water of 5.0% by weight or less, ammonia and ammonium ions are suitable for fluorine, and unnecessary cost increases can be avoided. Furthermore, as the water for cleaning after cleaning with ammonia water, ultrapure water is suitable because the fewer impurities the better.

[0023] The precipitated slurry washed with the above-mentioned washing liquid is fed into a press and squeezed to obtain a precipitated cake.

[0024] The precipitate cake obtained by squeezing is placed in a stationary furnace and fired at a predetermined heating temperature. The heating temperature is preferably 500°C or more and 2,000°C or less. When the heating temperature is 500°C or more and 2,000°C or less, it is a temperature sufficient for the growth of niobium oxide particles, and the firing cost can be suppressed, and the fired product obtained by firing does not become a hard lump, so that the labor and cost increase of crushing can be avoided. Furthermore, the heating temperature is more preferably 700°C or more and 1,500°C or less, and even more preferably 900°C or more and 1,500°C or less. Furthermore, the firing time is preferably 0.5 hours to 72 hours. When the firing time is 0.5 hours to 72 hours, it is a time sufficient for the growth of niobium oxide particles, and unnecessary costs can be suppressed. Furthermore, the firing time is more preferably 0.5 hours to 50 hours, and even more preferably 0.5 hours to 30 hours.

[0025] The calcined niobium oxide is used as it is as niobium oxide powder. The calcined product may be pulverized and used as niobium oxide powder. Regardless of whether it is pulverized or not, the calcined product may be classified using a sieve or the like, and the undersize (fine particle side) obtained may be used as niobium oxide powder. The oversize (coarse particle side) may be pulverized again and classified for use. It is also possible to combine pulverization and classification using a vibrating sieve into which iron balls coated with nylon or fluororesin are charged as pulverization media. By combining classification and pulverization in this way, even if there are niobium oxide particles that are too large after roasting, they can be removed. Specifically, when classifying using a sieve, it is preferable to use one with an opening of 150 μm to 1,000 μm. If it is 150 μm to 1,000 μm, the proportion of oversize particles will not be too high, so that re-pulverization will not be repeated, and niobium oxide powder that needs re-pulverization will not be classified to the undersize.

[0026] The niobium oxide powder produced by the above-mentioned method for producing niobium oxide powder according to the present invention has a structure in which primary particles of niobium oxide are fused to each other. In this way, the structure in which primary particles of niobium oxide are fused to each other increases the average particle size, so that the gravity acting on the primary particles of niobium oxide increases and the degree of compression decreases. In other words, this shows that the niobium oxide powder of the present invention is a powder that is difficult to crush, and even under conditions of pressure, a powder with high fluidity that is difficult to form aggregates can be obtained. Specifically, a niobium oxide powder in which the ratio D50(N) / D50(U) of the median diameter D50(N) of the niobium oxide particles to the median diameter D50(U) obtained by irradiating the niobium oxide particles with ultrasonic waves is 5 or less, and a niobium oxide powder in which the specific surface area SSA of the niobium oxide particles is 1 m 2 / g or less, and 0.4m 2 / g or less, a niobium oxide powder having a compressibility calculated based on the loose bulk density AD and the compacted bulk density TD of 25% or less, and further 20% or less, and a niobium oxide powder having the median diameter D50(U) of 5 μm or more and 120 μm or less are preferred.

[0027] In addition, when the niobium oxide powder according to the present invention is mixed with lithium carbonate powder to produce lithium niobate powder, it is well mixed, a uniform reaction product is obtained, and it has excellent reactivity. A specific method for evaluating this reactivity is as follows. First, niobium oxide powder and lithium carbonate powder are weighed so that the molar ratio of the two is 1:1, and the mixture (total weight 30 g) is mixed and crushed in a ball mill, and the resulting mixed powder is fired in an air atmosphere at a firing temperature of 1,000°C to 1,800°C for a firing time of 1 hour to 8 hours to produce lithium niobate powder. Next, this lithium niobate powder is crushed in an agate mortar, and powder X-ray diffraction measurement using CuKα rays is performed according to the powder X-ray diffraction measurement conditions described later to obtain an X-ray diffraction pattern. Then, if the obtained X-ray diffraction pattern is only a Bragg peak derived from lithium niobate, it is evaluated that the reactivity for the production of lithium niobate powder is good. Effect of the Invention

[0028] The niobium oxide powder of the present invention has excellent flowability and is suitable as a thin film forming material such as a sputtering target, an optical product, or a raw material for fine ceramics. [Brief description of the drawings]

[0029] [Figure 1] 1 is a scanning electron microscope (SEM) photograph of Example 1 of a niobium oxide powder according to an embodiment of the present invention. [Diagram 2] 1 is a scanning electron microscope (SEM) photograph of Comparative Example 1 of a niobium oxide powder according to an embodiment of the present invention. BEST MODE FOR CARRYING OUT THEINVENTION

[0030] Hereinafter, the niobium oxide powder according to the embodiment of the present invention will be described in accordance with the manufacturing method thereof. The niobium oxide powder according to the embodiment of the present invention is an ore, an alloy, a scrap, or the like containing niobium (hereinafter referred to as a raw material).

[0031] Preparation of niobium fluoride solution First, the above-mentioned raw material, for example, ore containing niobium, was put into a vibration mill and pulverized, and the obtained pulverized product was treated with an alkaline aqueous solution and washed with a mineral acid, after which the niobium in the raw material was dissolved with hydrofluoric acid to obtain a solution containing niobium. Then, the concentration of hydrofluoric acid in the solution containing niobium and the concentration of mineral acids other than hydrofluoric acid (for example, sulfuric acid) were adjusted to obtain a niobium extraction solution adjustment. This niobium extraction solution adjustment was separated and refined by a solvent extraction method using an organic solvent of 4-methyl-2-pentanone to obtain a niobium fluoride solution (hereinafter referred to as a niobium refined solution). Here, the niobium concentration in the obtained niobium fluoride solution was 320 g / L (grams / liter) when converted to niobium oxide (Nb2O5). Hereinafter, all niobium concentrations in the niobium fluoride solution are concentrations converted to niobium oxide.

[0032] Example 1The niobium purified solution obtained as described above was diluted to a niobium concentration of 60 g / L calculated as niobium oxide by adding ultrapure water to obtain a niobium diluted solution. Next, the niobium diluted solution was mixed with the ammonia water by a reverse neutralization method in which 47 L of the obtained niobium diluted solution was added over 30 minutes while stirring 25 L of 25 wt% ammonia water (13.2 mol / L) in a precipitation tank, and a precipitated slurry containing niobium was obtained (hereinafter referred to as the mixing / precipitation step). Here, the ammonia water in the precipitation tank was at room temperature (20°C).

[0033] Here, the pH of the ammonia water in the precipitation tank during the addition of the niobium diluted solution was always 10 or more. The pH of the obtained precipitation slurry containing niobium was also 10 or more. Furthermore, the niobium diluted solution to be added to the ammonia water in the precipitation tank was cooled to about 5°C by passing through a heat exchanger, and added to the ammonia water. A cooling tube made of fluororesin was installed in the precipitation tank, and cooling water with a tube inlet temperature of about 5°C was circulated to cool the precipitation tank. As a result of cooling in this way, the maximum temperature of the mixture of the niobium diluted solution and the ammonia water was 29°C from the start of the addition of the niobium diluted solution to the end of the precipitation of the precipitation slurry. The pH was measured by installing a tabletop pH meter (Horiba, Ltd.: F-71S: Standard ToupH electrode) in the precipitation tank, and the mixture of the niobium diluted solution and the alkaline aqueous solution in the precipitation tank during the addition of the niobium diluted solution and during stirring for 10 minutes after the addition. The pH was measured after confirming that the liquid temperature was stable at 25°C. After the addition of the diluted niobium solution was completed, stirring was continued for an additional 30 minutes, and after stirring was completed, the mixture was left to stand for 3 hours to allow the precipitate to settle, thereby obtaining a precipitate slurry containing niobium.

[0034] After removing the supernatant liquid from the precipitation tank, the precipitated slurry in the precipitation tank was taken out and separated into solid and liquid by a filter press. The precipitated slurry after solid-liquid separation was then transferred to a washing tank, where washing water was added and stirred for 30 minutes, and the tank was left to stand for 3 hours. The washing liquid (2.5% by weight of ammonia water) was then removed. This series of operations was repeated several times until the fluoride ion concentration in the washing liquid after washing became 100 mg / L or less.

[0035] After removing the washing liquid whose fluoride ion concentration was reduced to 100 mg / L or less, ultrapure water was added to wash the precipitated slurry, and the precipitated cake was obtained by squeezing the slurry. The precipitated cake was then collected and placed in a static furnace and calcined in air at a heating temperature of about 1,000°C for 3 hours (hereinafter referred to as the calcination process).

[0036] After firing, the obtained roasted powder was pulverized in a ball mill to obtain a powder form. Here, the ball mill media used was urethane-coated with a diameter of about 15 mm. Further, the mixture was sieved through a mesh with an opening of 200 μm, and the powder that fell through the sieve was collected to obtain the niobium oxide powder according to Example 1.

[0037] Example 2 This example is the same as Example 1 except that the diluted niobium solution was diluted so that the niobium concentration was 40 g / L calculated as niobium oxide, and therefore a description thereof will be omitted.

[0038] Example 3 This embodiment is the same as embodiment 1 except that in the mixing and precipitation step, the ammonia water in the precipitation tank was set to 10 wt % (5.9 mol / L) and the volume was set to 50 L, and therefore a description thereof will be omitted.

[0039] Example 4 This example is the same as Example 1 except that the diluted niobium solution was diluted so that the niobium concentration was 20 g / L calculated as niobium oxide, and therefore a description thereof will be omitted.

[0040] Example 5 This example is the same as Example 1 except that the time for adding the diluted niobium solution was 90 minutes, so a detailed explanation will be omitted.

[0041] Example 6This embodiment is the same as Example 1 except that the niobium diluted solution was diluted to a niobium concentration of 20 g / L calculated as niobium oxide, and the ammonia water in the precipitation tank was adjusted to 10 wt % (5.9 mol / L) and the volume was adjusted to 50 L, so a description thereof will be omitted.

[0042] Comparative Example 1 In this comparative example, the niobium diluted solution was diluted so that the niobium concentration was 90 g / L in terms of niobium oxide. In addition, contrary to the reverse neutralization method of Example 1, the niobium diluted solution and the ammonia water were mixed by a forward neutralization method in which 63 L of the niobium diluted solution in the precipitation tank was stirred while 30 L of 25 wt % ammonia water (13.2 mol / L) was added over 10 minutes to obtain a precipitation slurry containing niobium. The pH of the obtained precipitation slurry containing niobium was 9.5. Other conditions were the same as those of Example 1, so a description will be omitted.

[0043] Comparative Example 2 In this comparative example, similar to Comparative Example 1, the niobium dilution liquid and the ammonia water were mixed by the positive neutralization method to obtain a precipitation slurry containing niobium. Furthermore, similar to Example 1, the obtained precipitation slurry was washed and pressed to obtain a precipitation cake. Then, prior to the firing process, the obtained precipitation cake was placed in a static furnace and fired in the air at a heating temperature of about 100 to 200°C for 12 hours (hereinafter referred to as the preliminary drying process). Prior to the firing process, the preliminary dried precipitation cake was classified by a turbo screener. The classification conditions of the turbo screener were mesh opening: 32 μm, and rotation frequency: 90 Hz. Other conditions were the same as those of Example 1, so a description will be omitted.

[0044] The production conditions for the niobium oxide powders of the above-mentioned Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 1 below.

[0045] [Table 1]

[0046] The following physical properties were measured for the niobium oxide powders obtained in Examples 1 to 6 and Comparative Examples 1 and 2. The measured physical properties and the methods for measuring the physical properties are shown below, and the measurement results are shown in Table 2.

[0047] Particle size distribution The particle size distribution was evaluated by dynamic light scattering in accordance with JIS Z 8828:2019 using a laser diffraction / scattering particle size distribution analyzer (Microtrack Bell Corporation: MT3300EXII). No filtering was performed, and dispersion processing using ultrasonic waves, which will be described later, was performed. D50 indicates the particle size that reaches 50% by volume fraction.

[0048] Ultrasonic treatment: D50(N) is the median diameter of niobium oxide powder when particle size evaluation was performed without performing ultrasonic dispersion treatment. On the other hand, D50(U) is the median diameter of niobium oxide powder when particle size evaluation was performed immediately after performing ultrasonic dispersion treatment. Specifically, the procedure for ultrasonic dispersion treatment is as follows. First, as a pretreatment for ultrasonic dispersion treatment, 1 mg of sample powder, pure water 20 mL of the solution was poured into a 50 mL wide-mouth PP bottle, and the PP bottle was set in an ultrasonic cleaner (VS-100III, manufactured by AS ONE Corporation). Next, in a state where the inside of the cleaner was filled with pure water up to 5 cm above the floor surface, ultrasonic dispersion treatment was carried out for 60 minutes at a frequency of 28 kHz and an output of 100 W.

[0049] Tumbled bulk density (TD) The compacted bulk density was measured in accordance with "Part 12: Apparent density or apparent specific volume - Section 2: Tamp method" of JIS K 5101-12-2:2004 (Methods for measuring pigments).

[0050] Loose bulk density (AD) The loose bulk density was measured in accordance with "Part 12: Apparent density or apparent specific volume - Section 1: Static method" of JIS K 5101-12-1:2004 (Methods for measuring pigments).

[0051] Compression Degree The compression ratio was calculated according to the following formula (1).

[0052]

number

[0053] Specific surface area (SSA) The measurement was performed in accordance with "6.2 Flow method (3.5) Single point method" of JIS R 1626-1996 (Method of measuring specific surface area of ​​fine ceramic powder by gas adsorption BET method). A mixture of helium as carrier gas and nitrogen as adsorbate gas was used.

[0054] PFT slope The PFT slope is the slope of the approximation curve obtained by linear fitting the measurement data plotted on the graph with the uniaxial collapse strength (unit: kPa) on the vertical axis and the major principal consolidation stress (unit: kPa) on the horizontal axis by the least squares method. The measurement of the uniaxial collapse strength and the maximum principal consolidation stress was performed using a powder flow tester (manufactured by Brookfield, PET) in accordance with the measurement conditions of the Standard Flow Function Test. The range of the maximum principal consolidation stress was 1 kPa to 25 kPa, and the slope was calculated from the plot of five points. Here, the slope of the uniaxial collapse strength / maximum principal consolidation stress of the powder flow tester means how little force is required to break up a powder mass whose one end has been solidified by pressure, and a powder with a small slope is easy to flow even if it has solidified by pressure, so that it has the effect of being less likely to cause so-called "clogging" in a hopper, etc. A hopper is a device that temporarily holds powders such as ready-mix concrete and soil and pours them into the desired location; it is a container shaped like an inverted cone or an inverted pyramid.

[0055] Void presenceThe presence or absence of voids (air bubbles) formed on the surface of the primary particles of the niobium oxide powder was observed by observing five SEM images (20 μm × 20 μm) at a magnification of 5,000 times under the condition of an acceleration voltage of 1 kV with a scanning electron microscope (SEM), and the presence or absence of voids with a circumscribed circle diameter of 1 μm or less was observed. Under the above observation conditions, the case where no voids were observed on the surface of the primary particles was evaluated as "○", and the case where one or more voids were observed on the surface of the primary particles was evaluated as "×". Here, a scanning electron microscope (SEM) photograph of Example 1 of the niobium oxide powder according to the embodiment of the present invention is shown in FIG. 1, which shows a structure in which the primary particles of the niobium oxide powder according to Example 1 are fused to each other. On the other hand, a scanning electron microscope (SEM) photograph of Comparative Example 1 of the niobium oxide powder according to the embodiment of the present invention is shown in FIG. 2, which shows a structure in which the primary particles of the niobium oxide powder according to Comparative Example 1 are not fused to each other.

[0056] Hopper clogging test A 20 L hopper was attached to a small powder filling machine (RD703-T+SU01, manufactured by Naomi Co., Ltd.), niobium oxide powder was fed into the hopper at 5 kg / min, and the presence or absence of clogging during 60 minutes of continuous operation was evaluated. Specifically, when the discharge rate of the fed niobium oxide powder from the hopper continued to be maintained at a rate exceeding 4 kg / min, it was determined that no clogging had occurred in the hopper and the niobium oxide powder continued to flow, and was evaluated as "○". On the other hand, when the discharge rate of the fed niobium oxide powder from the hopper became 4 kg / min or less, it was determined that clogging had occurred in the hopper and the niobium oxide powder had stopped flowing, and was evaluated as "×".

[0057] Reactivity TestingA lithium niobate powder produced by mixing niobium oxide powder and lithium carbonate powder was used as a sample, and a powder X-ray diffraction measurement using CuKα radiation was performed according to the following powder X-ray diffraction measurement conditions, and the obtained X-ray diffraction pattern was confirmed to evaluate the reactivity. The lithium niobate powder sample was produced as follows. First, niobium oxide powder and lithium carbonate powder (manufactured by Wako Pure Chemical Industries, Ltd.) were weighed so that the molar ratio of the two was 1:1, and the mixture (total weight 30 g) was mixed and crushed in a ball mill, and the resulting mixed powder was fired in an air atmosphere at a firing temperature of 1,600°C to 1,800°C for a firing time of 8 hours to produce lithium niobate powder. Next, this lithium niobate powder was crushed in an agate mortar, and a powder X-ray diffraction measurement using CuKα radiation was performed according to the following powder X-ray diffraction measurement conditions to obtain an X-ray diffraction pattern. When the obtained X-ray diffraction pattern only had Bragg peaks derived from lithium niobate, it was judged that the niobium oxide powder and the lithium carbonate powder were well mixed and had good reactivity for producing lithium niobate powder, and was evaluated as "○". On the other hand, when the obtained X-ray diffraction pattern contained at least one peak other than the Bragg peak derived from lithium niobate, for example, a peak derived from niobium pentoxide (2θ=22.7°±0.5°, 32.7°±0.5°, and / or 36.5°±0.5°), it was judged that the niobium oxide powder and the lithium carbonate powder were poorly mixed, unreacted niobium oxide and lithium carbonate remained, and the reactivity for producing lithium niobate powder was poor, and was evaluated as "×".

[0058] = Powder X-ray diffraction measurement conditions = Diffraction equipment: MiniFlex2 (Rigaku Corporation) ·X-ray tube: Cu Tube voltage / current: 30kV, 15mA ·Slit: DS-SS; 1.25 degree, RS; 0.3mm ·Graphite Monochromator Measurement interval: 0.01 degree Counting method: Constant counting method

[0059] [Table 2]

[0060] As shown in Table 2, when the niobium oxide powders of Examples 1 to 6 had a D50 ratio, i.e., D50(N) / D50(U), of 5 or less, the primary particles of the niobium oxide powder of Example 1 had a structure in which they were fused to each other as shown in FIG. 1, so that the formation of agglomerates was suppressed, and as shown by the results of the hopper clogging test, a niobium oxide powder with high fluidity was obtained.

[0061] The niobium oxide powders according to Examples 1 to 6 have a specific surface area (SSA) of 1 m 2 At a molecular weight of 1000 to 1000 g / g or less, the adhesive force between niobium oxide particles was further reduced, the formation of agglomerates was suppressed, and a niobium oxide powder with high fluidity was obtained, as shown by the results of the hopper clogging test.

[0062] The niobium oxide powders of Examples 1 to 6 had a compression rate of 25% or less, calculated based on the loose bulk density AD and the compacted bulk density TD, which indicated that the niobium oxide powders of Examples 1 to 6 were powders that were difficult to crush, and niobium oxide powders with high fluidity and little tendency to agglomerate were obtained even when placed in a hopper and subjected to pressure.

[0063] The niobium oxide powders of Examples 1 to 6, when their median particle size D50(U) was 5 μm or more and 120 μm or less, as determined by particle size evaluation immediately after ultrasonic dispersion treatment, tended to be larger than the niobium oxide powders of Comparative Examples 1 and 2, which were largely dispersed by ultrasonic dispersion treatment.

[0064] The slope of the uniaxial collapse strength / maximum principal consolidation stress of the powder flow tester for the niobium oxide powders of Examples 1 to 6 is significantly smaller than that of the niobium oxide powders of Comparative Examples 1 and 2, and the powder lumps in the niobium oxide powders of Examples 1 to 6 are easily broken down with a small force.

[0065] In addition, the niobium oxide powder of the present embodiment is produced through a reverse neutralization method, and has a structure in which the primary particles are fused to each other, so that the particle size increases, and the degree of compression is small, so that agglomerates are not easily formed even under conditions of applied pressure, and the powder has excellent fluidity.

[0066] Furthermore, the niobium oxide powders according to Examples 1 to 6 are well mixed with lithium carbonate powder, and a uniform lithium niobate powder is obtained, and therefore the reactivity is also excellent.

[0067] The inventions disclosed in this specification include, in addition to the configurations of each invention or embodiment, those that are specified by changing these partial configurations to other configurations disclosed in this specification, to the extent applicable, or those that are specified by adding other configurations disclosed in this specification to these configurations, or those that are specified as higher-level concepts by deleting these partial configurations to the extent that partial action and effects are obtained. [Industrial Applicability]

[0068] The niobium oxide powder according to the present invention has excellent fluidity and is therefore suitable as a thin film forming material such as a sputtering target, an optical product, or a raw material for fine ceramics.

Claims

1. a ratio D50(N) / D50(U) of a median diameter D50(N) of the niobium oxide particles to a median diameter D50(U) obtained by irradiating the niobium oxide particles with ultrasonic waves under conditions of a frequency of 28 kHz, an output of 100 W, and a time period of 60 minutes is 5 or less; The niobium oxide particles have a specific surface area SSA of 0.4 m 2 / g or less; The degree of compression calculated based on the loose bulk density (AD) and the compacted bulk density (TD) is 25% or less; The niobium oxide powder has a median diameter D50 (U) of 5 μm or more and 120 μm or less.

2. 2. The niobium oxide powder according to claim 1, characterized in that the degree of compression is 20% or less.

3. A method for producing the niobium oxide powder according to claim 1 or 2, comprising the steps of: A method for producing niobium oxide powder, comprising the steps of: subjecting a solution in which niobium is dissolved to a solvent extraction; adding ultrapure water to the resulting niobium purified solution; and adding the resulting niobium diluted solution to an alkaline aqueous solution by a reverse neutralization method to produce a precipitate slurry containing niobium.

4. 4. The method for producing niobium oxide powder according to claim 3, wherein the alkaline aqueous solution to which the diluted niobium solution is added has a pH of 10 or more.

5. 4. The method for producing niobium oxide powder according to claim 3, wherein the alkaline aqueous solution is ammonia water.

Citation Information

Patent Citations

  • Dielectric ceramic composition and manufacturing method thereof

    JP1994103814A

  • Regeneration method of organic solvent in separation purification of tantalum and / or niobium by solvent extraction

    JP2004143009A

  • Niobium oxide and its manufacturing method

    JP2004292234A

  • Niobium oxide powder

    JP2005247601A

  • Powder of oxide of tantalum or niobium

    JP2005289692A