Polyester staple fiber for wet-laid nonwoven fabric, wet-laid nonwoven fabric containing same, and method for producing same

By employing a titanium-based catalyst to produce polyester fibers with controlled properties, the issues of safety, spinnability, and thermal stability are addressed, resulting in high-quality nonwoven fabrics for water purifiers and food filters.

JP7591156B2Active Publication Date: 2024-11-27TORAY ADVANCED MATERIALS KOREA INC
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
JP2023548165
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-19
Filing Date
2021-10-15
Publication Date
2024-11-27
Estimated Expiration
2041-10-15

AI Technical Summary

Technical Problem

Existing polyester fibers produced using antimony and germanium catalysts pose safety, health, and environmental concerns, while those using titanium catalysts suffer from poor spinnability and thermal stability, making them unsuitable for wet-laid nonwoven fabrics used in applications like water purifiers and food filters.

Method used

The use of a titanium-based compound as a polymerization catalyst to produce polyester short fibers with specific fineness, dispersibility, and average fiber length, combined with a binder fiber, to create a wet-laid nonwoven fabric with improved spinning workability and uniform mechanical strength.

Benefits of technology

The solution results in polyester fibers with enhanced dispersibility and spinning workability, producing nonwoven fabrics with consistent mechanical strength and improved safety, suitable for applications requiring high quality and hygiene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591156000001
    Figure 0007591156000001
  • Figure 0007591156000002
    Figure 0007591156000002
  • Figure 0007591156000003
    Figure 0007591156000003
Patent Text Reader

Abstract

The present invention relates to polyester staple fibers for wetlaid nonwoven fabrics, which are produced using a titanium-based compound as a polymerization catalyst, and to wetlaid nonwoven fabrics containing the same. The polyester staple fibers have excellent dispersibility due to significantly less formation of defects, and therefore, it is possible to provide wetlaid nonwoven fabrics having excellent mechanical strength and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester staple fiber for wetlaid nonwoven fabric, a wetlaid nonwoven fabric containing the same, and a method for producing the same. [Background technology]

[0002] Polyester is a commercially very important polymeric material, being used not only for the most widely used synthetic fiber in recent years, but also for various plastic products, due to its excellent mechanical properties, chemical stability, and high melting point. A lot of research is being conducted to expand the range of applications of PET, and in particular, there are steady efforts being made to synthesize PET with a high degree of polymerization and low carboxyl group content in a shorter time to improve various properties and increase productivity.

[0003] The polyester resin undergoes, for example, esterification reaction and then melt polycondensation reaction, and in the polycondensation reaction, antimony compounds or germanium compounds are generally used as polymerization catalysts on an industrial scale.The polyester resin produced using antimony compounds as polymerization catalysts has a unique black color, but has problems in terms of safety and hygiene due to the toxicity of antimony compounds, and environmental considerations.In addition, polyester resins catalyzed by germanium compounds are suitable from the viewpoints of transparency, safety and hygiene, but germanium compounds themselves are very expensive, and economic disadvantages are unavoidable, so there is a strong demand for the emergence of alternative polycondensation catalysts.

[0004] In order to solve the above problems, many compounds have been proposed as catalysts to replace antimony compounds and germanium compounds, and among them, various types of titanium compounds have been proposed because they are inexpensive and have no problems with safety and hygiene. However, polyester resins produced using titanium compounds as polymerization catalysts have a peculiar yellowish color, are poor in thermal stability, and have the disadvantage of producing a large amount of acetaldehyde by-product derived from decomposition reactions during polycondensation and melt molding, for example.

[0005] In particular, wet-laid nonwoven fabrics are used as components of water purifier filters or food filters for tea bags, but polyester fibers produced using antimony catalysts and wet-laid nonwoven fabrics made from them can leach antimony into drinking water, making them unsuitable from the standpoint of safety and hygiene.

[0006] As an example of this, Japanese Patent Publication No. 2002-194618 discloses fibers for nonwoven fabrics produced using an antimony catalyst. However, as mentioned above, when the nonwoven fabric is used for wet-laid nonwoven fabrics, there is a problem that it is not suitable from the viewpoint of safety and hygiene.

[0007] In addition, polyester fibers produced using titanium-based compounds have poor spinnability, and therefore form defects when dispersed in water, making them unsuitable for use as nonwoven fabrics for papermaking and filters.

[0008] In addition, fine polyester fibers have the characteristics of low spinning output and high draw ratio, so that spinnability is often poor, and the physical properties of wet-laid nonwoven fabrics containing them are also poor, and research on this issue is urgently needed. Summary of the Invention [Problem to be solved by the invention]

[0009] In order to solve the above problems, the present invention provides a method for producing polyester staple fibers for wetlaid nonwoven fabrics using a titanium-based compound as a polymerization catalyst, and a wetlaid nonwoven fabric containing the same and a method for producing the same. [Means for solving the problem]

[0010] The polyester staple fiber for wetlaid nonwoven fabrics of the present invention may have a fineness of 0.3 to 3.0 de (denier).

[0011] In a preferred embodiment of the present invention, the polyester staple fiber may have a dispersibility of 10 ppm or less as measured by the following Relation 1:

[0012] [Equation 1] TIFF0007591156000001.tif16161

[0013] In the above Relational Formula 1, the number of undispersed fibers is determined by adding 3 g of polyester staple fibers for wetlaid nonwoven fabrics having a moisture content of 25% by weight to 1 L of water at 25°C, stirring the mixture at 600 rpm for 10 minutes, and then leaving the mixture for 1 minute, after which the number of undispersed fibers is measured.

[0014] In a preferred embodiment of the present invention, the polyester staple fiber includes a spun material obtained by spinning a polymerization product, and the polymerization product is a reaction product obtained by polymerizing an ester reaction product, and the ester reaction product may be a reaction product obtained by reacting a mixture including an ester reactant, a heat stabilizer, and a titanium-based compound represented by the following Chemical Formula 1:

[0015] [Chemical formula 1] TIFF0007591156000002.tif36161

[0016] In the above chemical formula 1, R 1 and R 2 are each independently a linear alkylene group having 1 to 5 carbon atoms or a branched alkylene group having 3 to 5 carbon atoms.

[0017] In a preferred embodiment of the present invention, the polyester staple fibers may have an average fiber length of 3 to 12 mm.

[0018] In another aspect of the present invention, a wetlaid nonwoven fabric may comprise the polyester staple fiber for wetlaid nonwoven fabric; and a binder staple fiber.

[0019] In a preferred embodiment of the present invention, the nonwoven fabric may contain the binder staple fibers and the polyester staple fibers in a weight ratio of 1:1.20 to 1:1.90.

[0020] In a preferred embodiment of the present invention, the nonwoven fabric may have a MD (Machine direction) tensile strength of 150 to 300 N / 15 mm.

[0021] In a preferred embodiment of the present invention, the nonwoven fabric may have a standard deviation of MD (Machine direction) tensile strength that satisfies the following Relational Expression 2.

[0022] [Equation 2] TIFF0007591156000003.tif20160

[0023] In the above Relational Formula 2, N is the number of equal regions of the test piece obtained by cutting the nonwoven fabric into 150 mm x 100 mm, N = 10, and i is the MD tensile strength of the central part of the i-th region, μ is the average MD tensile strength of N equal parts, The file is TIFF0007591156000004.tif2746.

[0024] In a preferred embodiment of the present invention, the binder short fibers may have a fineness of 0.3 to 3.0 de and an average fiber length of 3 to 12 mm.

[0025] In yet another aspect of the present invention, the method for producing the nonwoven fabric may include a step of mixing polyester staple fibers for wetlaid nonwoven fabrics and binder staple fibers to produce a handsheet; a step of drying the handsheet to produce a papermaking paper; and a step of applying at least one selected from heat and pressure to the papermaking paper to perform calendaring to produce a wetlaid nonwoven fabric.

[0026] In a preferred embodiment of the present invention, the polyester staple fiber may be produced by the steps of: Step 1-1: obtaining an ester reactant by reacting an acid component and a diol component; Step 1-2: preparing a polyester resin by mixing and reacting a polymerization reactant including the ester reactant, a heat stabilizer and a titanium-based compound; Step 1-3: spinning the polyester resin to prepare a spun material; and Step 1-4: drawing the spun material to prepare a polyester staple fiber.

[0027] In a preferred embodiment of the present invention, the polymerization may be performed with the temperature raised to a final temperature of 275 to 285°C.

[0028] In a preferred embodiment of the present invention, the titanium-based compound may be contained in an amount of 10 to 20 ppm based on elemental titanium in the total weight of the polymerization reactant. Effect of the Invention

[0029] By using a titanium-based compound as a polymerization catalyst according to the present invention, it is possible to produce polyester staple fibers for wetlaid nonwoven fabrics having excellent spinnability and improved dispersibility, and it is possible to produce wetlaid nonwoven fabrics containing the same and having uniform mechanical strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The present invention will be described in more detail below based on a method for producing a wetlaid nonwoven fabric.

[0031] The method for producing a wetlaid nonwoven fabric of the present invention may include a step of mixing polyester staple fibers for wetlaid nonwoven fabrics and binder staple fibers to produce a handsheet; a step of drying the handsheet to produce papermaking paper; and a step of applying at least one selected from heat and pressure to the papermaking paper to perform calendaring to produce a wetlaid nonwoven fabric.

[0032] First, a one-step polyester staple fiber can be produced by the steps of: step 1-1, in which an acid component and a diol component are reacted to obtain an ester reactant; step 1-2, in which the ester reactant, a heat stabilizer, and a polymerization reactant including a titanium-based compound are mixed and reacted to produce a polyester resin; step 1-3, in which the polyester resin is spun to produce a spun material; and step 1-4, in which the spun material is stretched to produce a polyester staple fiber.

[0033] Specifically, the esterification reaction in step 1-1 can be carried out under esterification reaction conditions commonly used in the art. In a preferred example, the esterification reaction can be carried out at 200-260°C for 150-240 minutes at a rotation speed of 40-80 rpm, and more preferably at 210-250°C for 180-210 minutes at a rotation speed of 50-70 rpm.

[0034] The acid component and the diol component may be contained in a molar ratio of 1:1.0 to 1:1.5, and preferably in a molar ratio of 1:1.0 to 1:1.3. If the diol component is contained in a molar ratio of less than 1.0, the acidity during polymerization may become excessively high, promoting side reactions, and if the molar ratio exceeds 1.5, the degree of polymerization may not be increased.

[0035] In this case, the acidic component includes terephthalic acid, and may further include an aromatic polycarboxylic acid having 6 to 14 carbon atoms, an aliphatic polycarboxylic acid having 2 to 14 carbon atoms, and / or a metal salt of sulfonate.

[0036] The aromatic polycarboxylic acid having 6 to 14 carbon atoms may be any known acid component used for producing polyesters without any limitation, but may be preferably any one or more selected from the group consisting of dimethyl terephthalate, isophthalic acid, and dimethyl isophthalate.

[0037] The aliphatic polycarboxylic acid having 2 to 14 carbon atoms may be any known acid component used for producing polyesters without any limitation, and non-limiting examples thereof may include any one or more selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, citric acid, pimelic acid, azelaic acid, sebacic acid, nonanoic acid, decanoic acid, dodecanoic acid, and hexadecanoic acid.

[0038] The diol component may include ethylene glycol and a component represented by the following Chemical Formula 2:

[0039] [Chemical formula 2] TIFF0007591156000005.tif15159

[0040] Next, the 1-2 stage polymerization can be carried out by gradually reducing the pressure so that the final pressure becomes 0.5 torr while raising the temperature to a final temperature of 275 to 285°C, preferably 277 to 283°C.

[0041] If the final heating temperature of the polymerization is less than 275°C or exceeds 285°C, the dispersion of fibers becomes excessively high, and not only the tensile strength of the nonwoven fabric decreases, but also the thickness uniformity of the nonwoven fabric becomes poor, and the touch feeling of the surface of the nonwoven fabric becomes poor.

[0042] The heat stabilizer may be a commonly used heat stabilizer in the art, and preferably may be one or a mixture of two or more selected from the group consisting of trimethylphosphate, triethylphosphate, tributyl phosphate, tributoxyethyl phosphate, tricresyl phosphate, isopropylated triarylphosphate, and hydroquinone bis-(diphenyl phosphate).

[0043] The heat stabilizer may be contained in an amount of 10 to 30 ppm, preferably 15 to 25 ppm, based on the amount of phosphorus (P) element in the total weight of the polymerization reaction product.

[0044] The polymerization reaction product may further include a color complementing agent, which may be a mixture of blue and red dyes. The dye is a substitute for cobalt compounds, which induce pulmonary interstitial fibrosis and are classified as carcinogenic to humans, and is harmless to the human body.

[0045] The color complementing agent may be contained in the polymerization reaction product in an amount of 1 to 10 ppm, and preferably in an amount of 3 to 7 ppm.

[0046] In addition, the titanium-based compound may act as a polymerization catalyst and may be a titanium-based compound represented by the following Chemical Formula 1, and preferably may be a titanium chelate-based compound represented by the following Chemical Formula 1.

[0047] [Chemical formula 1] TIFF0007591156000006.tif36161

[0048] In the above chemical formula 1, R1 and R 2 may each independently be a linear alkylene group having 1 to 5 carbon atoms or a branched alkylene group having 3 to 5 carbon atoms, and preferably a linear alkylene group having 1 to 3 carbon atoms or a branched alkylene group having 3 to 4 carbon atoms.

[0049] In addition, the titanium-based compound represented by the above formula 1 is stable even in the presence of water molecules, so it is not inactivated even when added before the esterification reaction in which a large amount of water is produced as a by-product. As a result, the esterification reaction and polycondensation reaction can be carried out in a shorter time than before, and coloring can be suppressed. In addition, the titanium-based compound has excellent polymerization reactivity even at low polymerization temperatures, and the generation of carboxyl groups (-COOH) at the ends of polyester resins produced with a relatively high degree of polymerization is reduced, which reduces contamination of the nozzle surface by oligomers and monomers during the spinning process and reduces the number of times the nozzle surface needs to be cleaned, thereby improving production yield and reducing the defective rate. In addition, this makes it possible to produce polymers that are compatible with the human body and have a reduced content of acetaldehyde.

[0050] The titanium-based compound may be contained in an amount of 10 to 20 ppm, preferably 12 to 18 ppm, and more preferably 14 to 16 ppm based on the titanium element in the total weight of the polymerization reaction product. If the amount is less than 10 ppm, the b value (b * If the concentration is too high, the dyeability and dyeing rate of the fiber will be poor, and the amount of acetaldehyde generated will increase, making it impossible to produce a polymer that is safe for the human body. If the concentration exceeds 20 ppm, the amount of carboxyl groups (COOH) generated at the ends of the polyester resin will increase excessively.

[0051] In addition, a color complementing agent may be further included in the preparation of the polyester staple fiber of the present invention. The color complementing agent is used for color tone adjustment to make the color tone of the dye to be dyed in the dyeing process carried out after spinning into fibers stronger and better. Any color complementing agent known in the field of fibers may be added, and non-limiting examples thereof include starting dyes, pigments, dry flame-dyeing pigments, disperse dyes, organic pigments, etc. However, a mixture of blue and red dyes may be used. This is because cobalt compounds, which are commonly used as color complementing agents, are highly harmful to the human body and therefore not preferred, whereas a color complementing agent containing blue and red dyes mixed therein is preferred because it is harmless to the human body. In addition, when blue and red dyes are mixed and used, there is an advantage that the color tone can be finely controlled. Examples of the blue dye include solvent blue 104, solvent blue 122, and solvent blue 45, and examples of the red dye include solvent red 111, solvent red 179, and solvent red 195. In addition, the blue dye and the red dye can be mixed in a weight ratio of 1:1.0 to 3.0, which is advantageous in achieving a remarkable effect in controlling the desired fine color tone.

[0052] The color complementing agent may be included in an amount of 1 to 10 ppm based on the total weight of the polymerization reactant. If the amount is less than 1 ppm, it is difficult to achieve a desired level of color complementing properties, and if the amount is more than 10 ppm, the L value decreases, transparency decreases, and a dark color may appear.

[0053] The polyester resin may have an intrinsic viscosity of 0.60 to 0.80 dl / g, and preferably 0.63 to 0.77 dl / g.

[0054] The polyester resin may have 30 to 40 carboxy groups, and preferably 33 to 39 carboxy groups, as measured by the PHOL method.

[0055] Next, the spinning in steps 1 to 3 can be performed through a spinneret (nozzle), which may preferably be O-shaped, at a temperature of 270 to 300°C and a spinning speed of 1,300 to 1,700 mpm (meter per minute), preferably at a temperature of 275 to 295°C and a spinning speed of 1,400 to 1,600 mpm.

[0056] Next, the stretching in stages 1 to 4 can be carried out at a stretch ratio of 2.0 to 4.0, and preferably at a stretch ratio of 2.5 to 3.5.

[0057] The polyester staple fiber for wetlaid nonwoven fabric produced as above is a base fiber for the wetlaid nonwoven fabric, and may be a fiber that embodies the shape, strength, etc. of the wetlaid nonwoven fabric.

[0058] The polyester staple fiber may include a spun product obtained by spinning a polymerization product, the polymerization product being a reaction product obtained by polymerizing an ester reaction product, and the ester reaction product may be a reaction product obtained by reacting a mixture containing an ester reaction product, a heat stabilizer, and a titanium-based compound.

[0059] In addition, the polyester staple fiber may have a fineness of 0.3 to 3.0 de, preferably 0.4 to 1.5 de. If the fineness of the polyester staple fiber is less than 0.3 de, there may be a problem of poor spinnability, and if it exceeds 3.0 de, there may be a problem of excessively high air permeability of the nonwoven fabric.

[0060] In addition, the polyester staple fiber may have an average fiber length of 3 to 12 mm, and preferably 4 to 6 mm. If the average fiber length is less than 3 mm, the strength of the nonwoven fabric may be excessively low, and if it exceeds 12 mm, the occurrence of defects in papermaking containing such polyester staple fibers may increase significantly.

[0061] The polyester short fibers may have a dispersibility measured by the following relational expression 1 of 10 ppm or less, preferably 0.1 to 8.0 ppm, and more preferably 1.0 to 6.0 ppm.

[0062] [Equation 1] TIFF0007591156000007.tif16161

[0063] The number of undispersed fibers was measured by adding 3 g of polyester staple fibers having a moisture content of 25% by weight to 1 L of water at 25° C., stirring the mixture at 600 rpm for 10 minutes, and then leaving the mixture for 1 minute, after which the number of undispersed fibers was measured.

[0064] If the dispersibility according to Relation 1 exceeds 10 ppm, the wetlaid nonwoven fabric made with such polyester staple fiber has a reduced uniformity of mechanical strength, and the number of polyester staple fibers that become aggregated when dispersed in water at a temperature of 25° C. or higher increases significantly, and the nonwoven fabric realized through this may have a reduced feel and may have poor mechanical strength due to an increase in defects in the nonwoven fabric. In addition, when observing papermaking with the naked eye, the beauty of appearance and feel are very important, and even if the water acidity changes by a few decimal points, the defects can increase significantly, so that management of the water acidity to two decimal places or less is very important for product quality.

[0065] The binder staple fiber, which is separate from the polyester staple fiber, is a fiber that is uniformly dispersed with the polyester staple fiber and then thermally bonds the polyester staple fiber with the binder staple fiber and / or between the binder staple fibers, and can be used by itself as a fiber that ensures the shape and mechanical strength of the wetlaid nonwoven fabric.

[0066] The binder short fibers may include one or more fibers selected from the group consisting of polyethylene terephthalate (PET) fibers and polybutylene terephthalate (PBT) fibers, and are preferably polyethylene terephthalate (PET) fibers.

[0067] The binder staple fiber may be produced by a method including the steps of: subjecting an acid component and a diol component to an ester reaction to obtain an ester reactant; subjecting the ester reactant to a polycondensation reaction to prepare a polyester binder resin; and spinning the polyester binder resin to produce the binder staple fiber.

[0068] To explain this in detail, first, the acid component can be any known acid component without any limitations, and preferably, the acid component may include one or more selected from TPA (Terephthalic acid), IPA (Isophthalic acid) and AA (Arachidonic acid), and more preferably, the acid component may include one or more selected from TPA (Terephthalic acid) and IPA (Isophthalic acid).

[0069] The diol component can be any known diol component without any restrictions. Preferably, the diol component contains one or more selected from EG (Ethylene glycol), PEG (Poly(ethylene glycol)) and NPG (Neopentyl glycol), and more preferably, the diol component contains one or more selected from EG (Ethylene glycol) and PEG (Poly(ethylene glycol).

[0070] The acid component and the diol component may be contained in a molar ratio of 1:1.0 to 1:1.5, and preferably in a molar ratio of 1:1.0 to 1:1.3.

[0071] Next, the polymerization can be carried out by gradually reducing the pressure so that the final pressure becomes 0.5 torr while increasing the temperature to 275 to 285°C, and preferably to 277 to 283°C.

[0072] The binder resin produced as above may have an intrinsic viscosity of 0.60 to 0.80 dl / g, and preferably 0.63 to 0.77 dl / g.

[0073] Next, the spinning can be performed through a spinneret (nozzle), which may preferably be round-shaped, and can be performed at a spinning speed of 1,700 to 2,100 mpm (meter per minute) at 270 to 300°C, and preferably at a spinning speed of 1,800 to 2,000 mpm at 275 to 295°C.

[0074] The binder short fibers produced as described above may be undrawn yarns that have not been subjected to a drawing step.

[0075] The binder short fibers may have a fineness of 0.5 to 3.0 de, and preferably 0.8 to 1.8 de.

[0076] The binder short fibers may have an average fiber length of 3 to 12 mm, and preferably 4 to 6 mm.

[0077] The one-step handsheet can be produced by uniformly dispersing the polyester staple fibers and binder staple fibers prepared above in a dispersion medium, which may be a known dispersion medium such as water. The fibers mixed in the dispersion medium may further undergo a blending process for uniform mixing, and may further contain various other substances such as a pH adjuster, a forming aid, a surfactant, and an antifoaming agent to improve dispersibility.

[0078] The hand paper can be produced using a paper machine, and is not limited to a specific type of paper machine, such as a Fourdrinier paper machine or a ring wire paper machine, and can be modified according to the purpose.

[0079] In this case, the binder staple fiber and the polyester staple fiber may be contained in a weight ratio of 1:1.20 to 1:1.90, preferably in a weight ratio of 1:1.30 to 1:1.80, and more preferably in a weight ratio of 1:1.40 to 1:1.70. If the polyester staple fiber is contained in a weight ratio of less than 1.20, the touch of the nonwoven fabric may become hard, and if it is contained in a weight ratio of more than 1.90, the strength of the nonwoven fabric may become low.

[0080] In addition, a process of draining the dispersion medium may be further carried out before the two-stage drying process.

[0081] After the drainage step, the handsheet may be further dewatered by vacuum or other pressure. The handsheet may then be dried and dewatered to evaporate the remaining dispersion medium in a dryer, oven, or similar device known in the art for drying paper, to produce paper.

[0082] Next, the two-stage drying can be carried out at 90 to 110°C, preferably at 95 to 105°C.

[0083] Next, the three-stage calendaring can be performed by applying at least one of heat and pressure to the paper produced above, and the heat treatment can be performed at 210 to 270°C, preferably at 220 to 260°C.

[0084] In addition, a preliminary compression step may be performed before the calendering step, and the heat and / or pressure may be performed simultaneously by heating a roller and applying pressure, or may be performed in separate steps. However, the heat treatment may be performed by any heating method, such as by contacting the paper with a metal roll or other high-temperature surface, and may be achieved by a conventional method, such as infrared radiation or high-temperature air heating in an oven. The applied heat may be determined in consideration of the thermal properties of the polyester staple fiber and the binder staple fiber, and the present invention is not particularly limited thereto.

[0085] The wetlaid nonwoven fabric produced as above may have an average MD (machine direction) tensile strength of 150 to 300 N / 15 mm, preferably 150 to 200 N / 15 mm.

[0086] The nonwoven fabric may be a staple fiber nonwoven fabric.

[0087] The nonwoven fabric has a basis weight of 60 to 90 g / m 2 Preferably, the thickness is 65 to 85 g / m 2 may be also possible.

[0088] The nonwoven fabric may have an average thickness of 0.050 to 0.10 mm, and preferably 0.070 to 0.090 mm.

[0089] Moreover, the nonwoven fabric can have a standard deviation of MD (Machine direction) tensile strength that satisfies the following Relational Expression 2.

[0090] [Equation 2] TIFF0007591156000008.tif20160

[0091] In the above Relational Formula 2, σ means standard deviation, N is the number of equal areas into which the test piece obtained by cutting the nonwoven fabric into 150 mm × 100 mm is divided, N = 10, and l iis the central MD tensile strength of the i-th region, μ is the average MD tensile strength of the N equally divided regions, The file is TIFF0007591156000009.tif2746.

[0092] In this case, the value of the above relational expression 2 may be preferably 0.05 to 0.8 N / mm. If the value of the above relational expression 2 exceeds 1.0 N / 15 mm, the mechanical strength of the nonwoven fabric may be non-uniform, which may cause a problem in using the nonwoven fabric in products.

[0093] The nonwoven fabric may be a wet-laid nonwoven fabric.

[0094] The wetlaid nonwoven fabric of the present invention can be formed into paper and filters, preferably reverse osmosis filters.

[0095] The present invention will be described in more detail based on the following examples. However, the following examples are not intended to limit the scope of the present invention, and should be understood as being merely to aid in the understanding of the present invention.

[0096] [Example] Example 1-1: Production of polyester staple fiber for wet-laid nonwoven fabric (1) Manufacture of polyester resin An ester reaction tank was charged with 100 mol% terephthalic acid (TPA) as an acid component and 100 mol% ethylene glycol (EG) as a diol component, and reacted at 250°C and 1,140 torr pressure to obtain an ester reaction product. The acid component and the diol component were charged in a molar ratio of 1:1.2.

[0097] The ester reactant was then transferred to a polycondensation reactor.

[0098] Next, the ester reactant, the heat stabilizer and the polymerization reactant containing the titanium-based compound were mixed and polymerized to prepare a polyester resin.

[0099] The polymerization reaction was carried out by gradually reducing the pressure to a final pressure of 0.5 torr and raising the temperature to a final temperature of 280°C.

[0100] In this case, the heat stabilizer was prepared by containing triethyl phosphate in an amount of 25 ppm based on phosphorus element based on the total weight of the polymerization reactants.

[0101] The titanium-based compound is represented by the following formula 1-1, and is added to the polymerization reaction product in an amount of 15 ppm based on the titanium element, and is contained in the polymerization reaction product in an amount of 300 ppm.

[0102] [Chemical formula 1-1] TIFF0007591156000010.tif36161

[0103] In the above chemical formula 1-1, R 1 and R 2 are each independently an alkyl group having one carbon atom.

[0104] (2) Manufacture of polyester staple fibers The polyester resin was spun through a round spinneret at 285° C. and a spinning speed of 1,500 ppm to produce a spun material.

[0105] The spun material was then drawn at a draw ratio of 3.0 to produce polyester staple fibers.

[0106] In this case, the polyester staple fibers have an average fiber length of 5 mm and a fineness of 1.2 de.

[0107] Example 1-2 to Example 1-9 to Comparative Example 1-1 to Comparative Example 1-8: Production of polyester staple fiber for wet-laid nonwoven fabric Polyester staple fibers were produced in the same manner as in Example 1-1, but the polymerization temperature (final heating temperature), the amount of titanium-based compound added (based on Ti element), the fineness of the staple fibers, or the average fiber length of the staple fibers were changed as shown in Tables 1 to 3 below, to carry out Examples 1-2 to 1-9 and Comparative Example 1-1 to Comparative Preparatory Example 1-8.

[0108] Comparative Examples 1-9 to 1-12: Production of polyester staple fibers for wet-laid nonwoven fabrics Comparative Examples 1-9 to 1-12 were carried out by producing polyester staple fibers in the same manner as in Example 1-1, but changing the polymerization temperature (final heating temperature), the type of polymerization catalyst, or the amount of catalyst added (based on Ti element) as shown in Table 4 below.

[0109] Example 2-1: Production of binder short fibers Terephthalic acid (TPA) 100 mol % as an acid component and ethylene glycol (EG) 100 mol % as a diol component were charged into an ester reaction tank and reacted at 250° C. and 1,140 torr pressure to obtain an ester reaction product. The acid component and the diol component were charged in a molar ratio of 1:1.2.

[0110] The ester reactant was then transferred to a polycondensation reactor.

[0111] Next, the ester reactant was subjected to a polycondensation reaction in which the pressure was gradually reduced to a final pressure of 0.5 torr while the temperature was raised to 280° C. to produce a polyester binder resin.

[0112] Next, the polyester binder resin was spun through a round spinneret at 285° C. and a spinning speed of 1,900 ppm to produce binder staple fibers.

[0113] In this case, the polyester binder short fibers had an average fiber length of 5 mm and a fineness of 1.2 de.

[0114] Experimental Example 1: Evaluation of the physical properties of polyester resin and polyester short fiber The polyester resins (intermediate products) and polyester staple fibers for wet-laid nonwoven fabrics produced in Examples 1-1 to 1-9 and Comparative Preparative Examples 1-1 to 1-12 were evaluated for physical properties by the following methods, and the results are shown in Tables 1 to 4 below.

[0115] (1) Intrinsic viscosity (IV) The polyester resin was dissolved in ortho-chlorophenol solvent at a concentration of 2.0 g / 25 ml at 110°C for 30 minutes, and then incubated at 25°C for 30 minutes. The intrinsic viscosity was measured using an automatic viscosity measuring device connected to a Canon viscometer.

[0116] (2) Quantitative determination of carboxyl end groups The number of carboxyl groups in the polyester resin was measured by the PHOL method. Specifically, 0.1250 g of the polymerization product powder crushed to a size of 20 mesh was precisely weighed and placed in a test tube, 5 ml of benzyl alcohol was added, and the mixture was heated and dissolved at 210°C for about 135 seconds while stirring with a micro stirrer. Immediately after dissolution, the test tube was immersed in water at 25°C for 6 seconds to rapidly cool, and the contents were poured into a 50 ml beaker containing 10 ml of chloroform. An additional 5 ml of benzyl alcohol was added to the test tube and stirred for 60 seconds to completely rinse the remaining resin solution, which was then immediately added to the beaker and used as the titrant. The content of carboxyl groups was neutralized by titration using 0.1 N sodium hydroxide benzyl alcohol solution with a microsyringe (100 μl capacity) using phenol red (0.1% benzyl alcohol solution) as an indicator, and the titration determination value was corrected by the basic test result for the titrant, and calculated according to the following relational equation 3.

[0117] [Equation 3] TIFF0007591156000011.tif15160

[0118] where f is the concentration coefficient of 0.1N sodium hydroxide benzyl alcohol solution.

[0119] (3) Evaluation of spinning workability The spinning workability was evaluated by counting the number of drips (meaning clumps formed by irregular fusion of fiber strands after the fiber strands passing through the spinneret are partially fused or broken) generated during the spinning process of polyester staple fibers using a drip detector, and the number of drips generated in the remaining Examples and Comparative Examples was expressed as a relative percentage based on the number of drips generated in Example 1-1 being 100.

[0120] (4) Measurement of wiping cycle (number of times) In the polyester staple fiber manufacturing process, we calculated how many times a spinneret is wiped per day. It was determined that the larger the wiping cycle, the more likely it is that the spinneret is contaminated or has foreign matter trapped inside.

[0121] (5) b value (b * ) Measurement

[0122] The polyester staple fiber was analyzed for hue using a colorimeter to measure the b value. The measurement method was based on spectroscopy, and the chromaticity coordinates were calculated using the CIE standard illuminant and standard observer.

[0123] (6) Measurement of dispersibility The dispersibility was calculated according to the following formula 1.

[0124] [Equation 1] TIFF0007591156000012.tif16161

[0125] The number of undispersed fibers was measured by adding 3 g of polyester staple fibers having a moisture content of 25% by weight to 1 L of water at 25° C., stirring the mixture at 600 rpm for 10 minutes, and then leaving the mixture for 1 minute, after which the number of undispersed fibers was measured.

[0126] At this time, it was judged that the higher the dispersibility, the greater the number of undispersed fibers, and thus the result was judged to be poor.

[0127] [Table 1]

[0128] [Table 2]

[0129] [Table 3]

[0130] [Table 4]

[0131] Referring to Tables 1 to 4, it can be seen that Examples 1-1 to 1-9 have excellent physical properties. Meanwhile, Comparative Example 1-1, in which the final heating temperature (polymerization temperature) is less than 275°C, has a problem of dispersibility exceeding 10 ppm, compared with Example 1-2, in which the final heating temperature (polymerization temperature) is 275°C.

[0132] In addition, in Comparative Example 1-2, in which the final heating temperature (polymerization temperature) exceeded 285°C, more than 40 carboxyl groups were measured in the resin, indicating high contamination, compared with Example 1-3, in which the final heating temperature (polymerization temperature) was 285°C. Not only was the dispersion of the fibers significantly increased, but the spinneret was easily contaminated, shortening the wiping cycle, and the b value (b*) was high, resulting in yellowish fibers.

[0133] In addition, in Comparative Example 1-3, in which the titanium (Ti) element content of the titanium-based compound is less than 10 ppm, the b value is too high compared to Example 1-4, in which the titanium (Ti) element content of the titanium-based compound is 10 ppm, making commercial use of the nonwoven fabric impossible, and the dispersibility also exceeds 10 ppm.

[0134] In addition, in Comparative Example 1-4, in which the titanium (Ti) element content of the titanium-based compound exceeds 20 pm, the resin had excessively high carboxyl groups measured, the number of wipings due to contamination increased significantly, and the dispersibility was excessively high, compared to Example 1-5, in which the titanium (Ti) element content of the titanium-based compound was 20 ppm.

[0135] In addition, Comparative Example 1-5, in which the polyester staple fiber fineness is less than 0.3 de, showed the most frequent wiping cycle compared to Example 1-6, in which the polyester staple fiber fineness is 0.3 de. This is presumably a problem that occurs as the fiber becomes excessively fine.

[0136] In addition, in Comparative Examples 1-9 to 1-12, in which an antimony-based catalyst was used instead of a titanium-based compound, an excessively large amount of carboxyl groups was detected, and not only was the b value high, but the dispersibility was also excessively high, making it impossible to use the resulting wetlaid nonwoven fabric.

[0137] Manufacturing Example 1: Manufacturing of wet-laid nonwoven fabric The polyester staple fiber for wetlaid nonwoven fabric produced in Example 1-1 and the binder staple fiber produced in Example 2-1 were prepared.

[0138] Next, the binder staple fiber and polyester staple fiber were dispersed in water in a weight ratio of 1:1.50, the water was drained, and the mixture was dried at 100°C and calendered at 240°C to obtain a grammage of 75 g / m2. 2 A wet-laid nonwoven fabric having an average thickness of 0.08 mm was produced.

[0139] Production Examples 2 to 11 and Comparative Production Examples 1 to 14: Production of Wet-Laid Nonwoven Fabrics Wetlaid nonwoven fabrics were produced in the same manner as in Production Example 1, but Production Examples 2 to 11 and Comparative Production Examples 1 to 14 were carried out by using the polyester staple fibers for wetlaid nonwoven fabrics produced in Examples 1-2 to 1-9 or Comparative Examples 1-1 to 1-12, or by changing the weight ratios of the binder staple fibers and the polyester staple fibers as shown in Tables 5 to 9 below.

[0140] Experimental Example 2: Evaluation of the physical properties of wet-laid nonwoven fabric The wetlaid nonwoven fabrics produced in Production Examples 1 to 11 and Comparative Production Examples 1 to 14 were cut to 150 mm x 100 mm to produce test pieces. Next, the test pieces were subjected to the following experiments, and the results are shown in Tables 5 to 9 below.

[0141] (1) Measurement of average MD (machine direction) tensile strength The MD tensile strength was measured by subjecting the test piece to 10 tests at a temperature of 25° C. and a speed of 20 mm / min using a tensile strength tester (HZ-1007E, MMS), and the average value was taken as the average tensile strength.

[0142] (2) Measurement of standard deviation of MD (machine direction) tensile strength The standard deviation of the MD tensile strength was calculated according to the following formula 2-1.

[0143] [Equation 2-1] TIFF0007591156000017.tif20158

[0144] In the above Relational Formula 2-1, σ means standard deviation, N is the number of equal areas into which a test piece of the nonwoven fabric cut to 150 mm × 100 mm is divided, N = 10, and l i is the MD tensile strength of the central part of the i-th region, μ is the average MD tensile strength of N equal parts, The file is TIFF0007591156000018.tif2747.

[0145] (4) Evaluation of surface touch (touch) A panel of eight people performed a sensory evaluation of the texture by hand and gave a relative rating as follows: (1: very soft, 2: normal, 3: hard or rough)

[0146] [Table 5]

[0147] [Table 6]

[0148] [Table 7]

[0149] [Table 8]

[0150] [Table 9]

[0151] Referring to Tables 5 to 9, it was found that Preparation Examples 1 to 11 were nonwoven fabrics with excellent physical properties, whereas Comparative Preparation Examples 1 to 14 were found to have nonwoven fabrics with tensile strengths less than 150N / 15mm, standard deviations of tensile strengths exceeding 1.0N / 15mm, or poor touch of the nonwoven fabric surface.

[0152] Although one embodiment of the present invention has been described above, the concept of the present invention is not limited to the examples presented in this specification, and a person skilled in the art who understands the concept of the present invention can easily propose other examples by adding, changing, deleting, or adding components within the scope of the same concept, which can also be said to fall within the concept of the present invention.

Claims

1. A spun product obtained by spinning a polyester resin, The polyester resin is a polymerization product obtained by polymerizing a polymerization reactant including an ester reactant, a heat stabilizer, and a titanium-based compound represented by the following Chemical Formula 1: The ester reactant is a reaction product obtained by an esterification reaction of an acid component and a diol component, The titanium-based compound is contained in an amount of 10 to 20 ppm based on titanium element in the total weight of the polymerization reactant, The polyester resin has 33 to 39 carboxy groups, A polyester staple fiber for wet-laid nonwoven fabrics, characterized in that the fiber size is 0.3 to 3.0 de and the average fiber length is 3 to 12 mm: 【Chemistry 1】 In the above chemical formula 1, R 1 and R 2 are each independently a linear alkylene group having 1 to 5 carbon atoms or a branched alkylene group having 3 to 5 carbon atoms.

2. A polyester staple fiber for wet-laid nonwoven fabric according to claim 1; and a binder staple fiber; The wetlaid nonwoven fabric contains the binder staple fiber and the polyester staple fiber in a weight ratio of 1:1.20 to 1:1.

90.

3. The wet-laid nonwoven fabric according to claim 2, wherein the nonwoven fabric has a tensile strength in a machine direction (MD) of 150 to 300 N / 15 mm.

4. The nonwoven fabric according to claim 2, characterized in that the standard deviation of MD (machine direction) tensile strength satisfies the following relationship 2: [0010] In the above Relational Formula 2, N is the number of regions into which a test piece obtained by cutting the nonwoven fabric into 150 mm x 100 mm is equally divided, N = 10, l i is the MD tensile strength of the central part of the i-th region, μ is the average value of the MD tensile strengths of the N equally divided regions, [0025] It is.

5. 3. The wetlaid nonwoven fabric according to claim 2, wherein the binder short fibers have a fineness of 0.3 to 3.0 de and an average fiber length of 3 to 12 mm.

6. A step of producing hand-made paper by mixing polyester staple fibers for wet-laid nonwoven fabrics having an average fiber length of 3 to 12 mm and binder staple fibers; drying the handsheet to produce a papermaking paper; and The step of calendering the paper by applying at least one selected from heat and pressure to the paper to produce a wet-laid nonwoven fabric; The polyester staple fiber is prepared by reacting an acid component with a diol component to obtain an ester reaction product in step 1-1; Step 1-2: preparing a polyester resin by mixing and reacting the ester reactant, a heat stabilizer, and a titanium-based compound represented by the following Chemical Formula 1 at a final temperature of 275 to 285°C; Steps 1-3: spinning the polyester resin to prepare a spinning product; The spun material is stretched to produce polyester staple fibers having a fineness of 0.3 to 3.0 de (steps 1 to 4); The titanium-based compound in step 1-1 is contained in an amount of 10 to 20 ppm based on titanium element in the total weight of the polymerization reactant; The method for producing a wetlaid nonwoven fabric is characterized in that the polyester resin has 33 to 39 carboxy groups. 【Chemistry 2】 In the above Chemical Formula 1, R 1 and R 2 are each independently a linear alkylene group having 1 to 5 carbon atoms or a branched alkylene group having 3 to 5 carbon atoms.