How to reuse lithium-ion secondary batteries

By cleaning and heat-treating ceramic electrodes from used lithium ion secondary batteries, the method addresses the challenges of recycling and reuse, enabling efficient reassembly and performance restoration.

JP7591165B2Active Publication Date: 2024-11-27NGK CORP
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
JP2023569241
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-23
Filing Date
2022-12-01
Publication Date
2024-11-27
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

Conventional lithium ion secondary batteries face challenges in recycling and reuse due to the presence of organic binders and conductive additives, leading to complex processes and limited applications, making it difficult to recover and reuse electrodes effectively.

Method used

The method involves cleaning and/or heat treatment of ceramic electrodes from used lithium ion secondary batteries to separate and restore their performance, allowing for reassembly into functional batteries with a simple procedure and low cost.

Benefits of technology

This approach enables the recovery of lithium ion secondary batteries with sufficient performance by removing impurities and optimizing the ceramic electrodes, resulting in improved capacity and charge/discharge efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591165000003
    Figure 0007591165000003
  • Figure 0007591165000004
    Figure 0007591165000004
  • Figure 0007591165000005
    Figure 0007591165000005
Patent Text Reader

Abstract

Provided is a method for recycling a lithium-ion secondary battery, the method making it possible to use a depleted lithium-ion secondary battery to reassemble a lithium-ion secondary battery with sufficiently restored performance through a simple procedure and at low cost. This method includes: a step in which a depleted lithium-ion secondary battery is readied, the battery comprising (i) a battery element that includes a positive electrode, a separator, and a negative electrode, at least the positive electrode or the negative electrode being a ceramic electrode, (ii) an electrolyte, and (iii) a battery container that accommodates the battery element and the electrolyte; a step in which the ceramic electrode is extracted from the lithium-ion secondary battery so as to mutually separate the positive electrode and the negative electrode (the separator may be bonded to the extracted ceramic electrode); a step in which electrode restoration processing that includes cleaning and / or heat processing is applied to the extracted ceramic electrode; and a step in which the ceramic electrode subjected to the electrode restoration processing is returned to the inside of the battery container to assemble the lithium ion secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recycling a lithium ion secondary battery. [Background technology]

[0002] Various methods have been proposed for reusing lithium ion secondary batteries or their components. For example, Patent Document 1 (JP 2014-127417 A) discloses a method for reusing a negative electrode active material layer, and proposes immersing a negative electrode having a negative electrode active material layer containing a non-aqueous binder and a current collector in an aqueous solution, recovering the peeled negative electrode active material layer, and attaching the recovered negative electrode active material layer to the current collector again. Patent Document 2 (JP 2019-145315 A) discloses a method for reusing a lithium ion secondary battery, which includes injecting dry air into the interior of a used lithium ion secondary battery containing a non-aqueous electrolyte. Patent Document 3 (JP Patent No. 5077788 A) discloses a method for recovering cobalt and lithium from battery materials, and proposes dissolving an electrode material in sulfuric acid to obtain a solution in which cobalt ions and lithium ions are dissolved, and separating this solution from insoluble matter. Patent Document 4 (JP Patent No. 5664043) discloses a method for reusing electrolyte from used lithium ion batteries, including recovering electrolyte from the used lithium ion batteries and using the electrolyte as fuel. Patent Document 5 (JP Patent Publication No. 2014-82120) discloses a system for determining whether or not a non-aqueous electrolyte secondary battery can be reused, and the system includes a first acquisition unit that acquires a first measurement value obtained by measuring the amount of lithium fluoride film formed on the positive electrode, a first storage unit that holds a first range of the lithium fluoride film formed on the positive electrode that has been determined in advance, and a first determination unit that determines whether or not the target battery can be reused based on the first measurement value and the first range.

[0003] Meanwhile, many existing lithium ion secondary batteries employ a powder-dispersed type positive electrode (so-called coated electrode) that is prepared by applying and drying a positive electrode mixture that contains a positive electrode active material, a conductive additive, a binder, and the like.

[0004] Generally, a powder-dispersed positive electrode contains a relatively large amount (for example, about 10% by weight) of components (binders and conductive assistants) that do not contribute to capacity, so the packing density of the lithium composite oxide as the positive electrode active material is low. For this reason, the powder-dispersed positive electrode has a large room for improvement in terms of capacity and charge / discharge efficiency. Therefore, attempts have been made to improve the capacity and charge / discharge efficiency by forming the positive electrode or the positive electrode active material layer from a lithium composite oxide sintered plate. In this case, since the positive electrode or the positive electrode active material layer does not contain a binder or conductive assistant (for example, conductive carbon), it is expected that a high capacity and good charge / discharge efficiency can be obtained by increasing the packing density of the lithium composite oxide. For example, Patent Document 6 (Patent Publication No. 6374634) discloses a lithium composite oxide sintered plate such as lithium cobalt oxide LiCoO2 (hereinafter referred to as LCO) used in the positive electrode of a lithium ion secondary battery. This lithium composite oxide sintered plate has a structure in which a plurality of primary particles having a layered rock salt structure are bonded together, and has a porosity of 3 to 40%, an average pore size of 15 μm or less, an open pore ratio of 70% or more, a thickness of 15 to 200 μm, and a primary particle size which is the average particle size of the plurality of primary particles of 20 μm or less. Furthermore, this lithium composite oxide sintered plate is said to have an average angle between the (003) plane of the plurality of primary particles and the plate surface of the lithium composite oxide sintered plate, i.e., an average tilt angle, which is greater than 0° and less than 30°.

[0005] On the other hand, it has also been proposed to use a titanium-containing sintered plate as the negative electrode. For example, Patent Document 7 (Japanese Patent No. 6392493) discloses lithium titanate Li4Ti5O 12 The LTO sintered plate has a structure in which multiple primary particles are bonded together, and is said to have a thickness of 10 to 290 μm, a primary particle size, which is the average particle size of the multiple primary particles, of 1.2 μm or less, a porosity of 21 to 45%, and an open pore ratio of 60% or more. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-127417 A [Patent Document 2] JP 2019-145315 A [Patent Document 3] Patent No. 5077788 [Patent Document 4] Patent No. 5664043 [Patent Document 5] JP 2014-82120 A [Patent Document 6] Patent No. 6374634 [Patent Document 7] Patent No. 6392493 Summary of the Invention

[0007] The reuse of lithium-ion secondary batteries or their components as described above can be broadly divided into recycling and reuse. Battery recycling involves the recovery of materials such as electrodes as active materials or alloys, but is costly due to the complex process. On the other hand, battery reuse involves evaluating the performance of the battery and reusing it for different purposes depending on the degree of deterioration. For example, if the degree of deterioration is small, the battery can be reused for electric vehicles (EVs) or forklifts, and if the degree of deterioration is large, it can be reused for backup power sources.

[0008] Thus, recycling of lithium-ion secondary batteries is complicated and expensive, while reuse has limited applications. For this reason, the reuse of lithium-ion secondary batteries or their components has not progressed much. In particular, conventional lithium-ion secondary batteries, which contain organic binders and conductive additives in the electrodes, have many degradation factors, making it difficult to separate, regenerate, and reuse used electrodes.

[0009] The present inventors have now discovered that by cleaning and / or heat treating a ceramic electrode removed from a used lithium-ion secondary battery, a lithium-ion secondary battery with sufficiently restored performance can be reassembled in a simple procedure at low cost.

[0010] Therefore, an object of the present invention is to provide a method for recycling lithium ion secondary batteries, which enables reassembly of a lithium ion secondary battery with sufficiently restored performance using a used lithium ion secondary battery in a simple procedure at low cost.

[0011] According to the present invention, the following aspects are provided. [Aspect 1] (i) preparing a used lithium ion secondary battery comprising a battery element including a positive electrode, a separator, and a negative electrode, at least one of the positive electrode and the negative electrode being a ceramic electrode, (ii) an electrolyte, and (iii) a battery container that contains the battery element and the electrolyte; removing the ceramic electrode from the lithium ion secondary battery such that the positive electrode and the negative electrode are separated from each other (however, the separator may be bonded to the removed ceramic electrode); subjecting the removed ceramic electrode to an electrode restoration treatment including cleaning and / or heat treatment; returning the ceramic electrode that has been subjected to the electrode restoration treatment into the battery container to assemble a lithium ion secondary battery; A method for reusing a lithium-ion secondary battery, comprising: [Aspect 2] The method for reusing a lithium ion secondary battery according to aspect 1, wherein the electrode revival treatment includes washing the ceramic electrode with a polar solvent to remove impurities contained in and / or attached to the ceramic electrode, followed by drying. [Aspect 3] The ceramic electrode further comprises a positive electrode current collector and / or a negative electrode current collector, The positive and / or negative current collectors are removed before and / or during said cleaning, and 3. The method for reusing a lithium-ion secondary battery according to claim 1, wherein a positive electrode current collector and / or a negative electrode current collector is attached to the ceramic electrode after the electrode revival treatment. [Aspect 4] 4. The method for reusing a lithium ion secondary battery according to aspect 2 or 3, wherein the electrode revival treatment includes heating the washed and dried ceramic electrode at 300 to 1000°C. [Aspect 5] 5. The method for reusing a lithium-ion secondary battery according to claim 4, wherein the electrode restoration treatment includes degreasing the ceramic electrode at 300 to 600° C. and / or firing the ceramic electrode at 650 to 1000° C. [Aspect 6] The method for reusing a lithium ion secondary battery according to any one of aspects 1 to 5, wherein the positive electrode is a ceramic positive electrode, and the ceramic positive electrode is made of a sintered lithium composite oxide. [Aspect 7] The method for reusing a lithium ion secondary battery according to any one of aspects 1 to 6, wherein the positive electrode is a ceramic positive electrode, the ceramic positive electrode is an oriented positive electrode that includes a plurality of primary particles constituted by a lithium composite oxide, and the plurality of primary particles are oriented at an average orientation angle of more than 0° and not more than 30° with respect to a main surface of the positive electrode. [Aspect 8] 8. The method for reusing a lithium ion secondary battery according to aspect 6 or 7, wherein the lithium composite oxide is lithium cobalt oxide. [Aspect 9] The method for reusing a lithium ion secondary battery according to any one of aspects 1 to 8, wherein the negative electrode is a ceramic negative electrode, and the ceramic negative electrode is made of a titanium-containing sintered body. [Aspect 10] 10. The method for reusing a lithium-ion secondary battery according to aspect 9, wherein the titanium-containing sintered body contains lithium titanate or niobium titanium composite oxide. [Aspect 11] 11. The method for reusing a lithium ion secondary battery according to any one of aspects 1 to 10, wherein the separator is a ceramic separator, and the ceramic separator contains at least one selected from the group consisting of MgO, Al2O3, ZrO2, SiC, Si3N4, AlN, and cordierite. [Aspect 12] 12. The method for reusing a lithium ion secondary battery according to any one of aspects 1 to 11, further comprising replacing the electrolyte in the lithium ion secondary battery with fresh electrolyte. [Aspect 13] 13. The method for reusing a lithium ion secondary battery according to any one of aspects 1 to 12, further comprising the step of replacing the battery container with another battery container after removing the ceramic electrode and before returning the ceramic electrode into the battery container. [Aspect 14] The method for reusing a lithium ion secondary battery according to any one of aspects 1 to 13, further comprising a step of replacing a positive electrode or a negative electrode other than the ceramic electrode that has been subjected to the electrode revival treatment with a new positive electrode or a negative electrode equivalent thereto during or before assembling the lithium ion secondary battery. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view of an example of a lithium ion secondary battery used in the method of the present invention. [Diagram 2] 1 is a SEM image showing an example of a cross section perpendicular to the layer surface of an oriented positive electrode layer. [Diagram 3] 3 is an EBSD image of a cross section of the oriented positive electrode layer shown in FIG. 2. [Figure 4] FIG. 4 is a histogram showing the distribution of orientation angles of primary particles in the EBSD image of FIG. 3 on an area basis. [Diagram 5] FIG. 2 is a schematic perspective view showing an example of a honeycomb-type ceramic positive electrode. [Figure 6A] FIG. 1 is a schematic perspective view conceptually showing the configuration of a lithium ion secondary battery provided with a honeycomb-type ceramic positive electrode. [Figure 6B]6B is a cross-sectional view of the lithium-ion secondary battery shown in FIG. 6A taken along line 6B-6B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] How to reuse lithium-ion secondary batteries The used lithium ion secondary battery used in the method of the present invention is a sintered type battery (semi-solid battery) equipped with ceramic electrodes together with an electrolyte. An example of such a lithium ion secondary battery is shown in FIG. 1. The lithium ion secondary battery 10 shown in FIG. 1 is in the form of a coin battery, but the present invention is not limited thereto, and may be a battery in other forms such as a button battery, a cylindrical battery, a prismatic battery, a pack battery, a car battery, or a sheet battery.

[0014] That is, in the method for recycling a lithium ion secondary battery according to the present invention, first, a used lithium ion secondary battery 10 is prepared, which includes a battery element 21, an electrolyte 22, and a battery container 24 that contains the battery element 21 and the electrolyte 22. The battery element 21 includes a positive electrode 12, a separator 20, and a negative electrode 16, and at least one of the positive electrode 12 and the negative electrode 16 is a ceramic electrode. Then, the ceramic electrodes (i.e., the positive electrode 12 and / or the negative electrode 16) are taken out from the lithium ion secondary battery 10 so that the positive electrode 12 and the negative electrode 16 are separated from each other. At this time, the separator 20 may be bonded to the taken-out ceramic electrodes. Next, the taken-out ceramic electrodes are subjected to an electrode restoration process including washing and / or heat treatment. Finally, the ceramic electrodes that have been subjected to the electrode restoration process are returned into the battery container 24, and the lithium ion secondary battery 10 is assembled. In this manner, by performing cleaning and / or heat treatment on the ceramic electrodes (i.e., the positive electrode 12 and / or the negative electrode 16) removed from a used lithium-ion secondary battery 10, a lithium-ion secondary battery 10 with sufficiently restored performance can be reassembled in a simple manner at low cost.

[0015] As described above, recycling of lithium ion secondary batteries involves complicated processes and high costs, while reuse has limited applications. For this reason, the current situation is that the reuse of lithium ion secondary batteries or their components has hardly progressed. In particular, conventional lithium ion secondary batteries that contain organic binders and conductive assistants in the electrodes have many degradation factors, making it difficult to separate, regenerate, and reuse used electrodes. This problem is conveniently solved by the present invention. This is explained as follows.

[0016] First, there are various factors that can be considered as general deterioration factors of conventional lithium-ion secondary batteries. First, when the battery is manufactured or in the early stages of use, the water contained in the electrolyte and the electrolyte anion PF5 - The reaction with the electrolyte, the reaction with the solvent produced by this reaction, the reaction with the electrolyte and the active material, the formation of a carbonate layer or a fluorinated layer on the electrode surface caused by this side reaction, and the generation of gas occur. Next, the use of the battery causes the deterioration and reduction of the active material itself used in the active material layer of the electrode. Repeated charging and discharging causes the cracking of particles due to swelling and shrinkage changes, structural deterioration and destruction due to phase changes and distortion, dissolution of the positive electrode active material, precipitation of the dissolved material at the negative electrode, short circuit between the positive electrode and the negative electrode due to this, reduction of lithium ions, formation of Li dendrites at the negative electrode due to low temperature operation / high current operation, reduction of lithium ions and short circuit between the positive electrode and the negative electrode, and deterioration of the interface. In addition, corrosion of the current collector surface, peeling of the active material from the current collector, reduction in the conductivity of the electrode, change and non-uniformity of the conductive network in the active material layer, deterioration of the binder, clogging of the separator, and an increase in the internal resistance of the cell due to these changes. In addition, depending on the conditions of use, various factors can be cited as causes of capacity degradation, such as a decrease in the reaction amount of the active material due to overcharging or overdischarging, oxidation of the electrolyte, deterioration due to reduction reactions, deterioration of the reaction interface layer, and deterioration due to expansion and contraction of the electrodes during charging and discharging.

[0017] In contrast, the used lithium ion secondary battery used in the present invention is a sintered body type battery that includes a battery element in which at least one of the positive and negative electrodes is a ceramic electrode together with an electrolyte, and has fewer degradation factors than a general lithium ion secondary battery, and is robust because the ceramic electrodes are made of ceramic (sintered body), and the electrolyte 22 can be replaced any number of times to reassemble the battery. Advantageously, the main degradation modes in such a semi-solid battery are only "reaction between the electrolyte and the active material" and "dissolution of the positive electrode active material" among the extremely wide variety of degradation factors described above. That is, the positive electrode 12 and / or the negative electrode 16, which are the ceramic electrodes in the semi-solid battery, are made of ceramic (i.e., sintered body), and therefore do not contain components that are degradation factors such as organic binders (organic binders disappear due to sintering). As a result, ceramic electrodes that do not contain binders, etc., are less likely to deteriorate (there is no deterioration due to the binder). In addition, since the ceramic electrodes are made of ceramics, they can be taken out in their original form even after use, and can be easily handled. Moreover, since this electrode is a ceramic alone (even if a metal foil is attached, it can be removed or peeled off), it can be cleaned, degreased, fired, and other heat treatments. Although degradation occurs due to oxidative decomposition of the electrolyte 22, the ceramic electrode itself is not subject to much degradation, so that the performance of the battery can be restored to a certain extent by simply replacing the electrolyte 22. Therefore, according to the method of the present invention, a lithium ion secondary battery with sufficiently restored performance can be reassembled using a used lithium ion secondary battery in a simple procedure at low cost.

[0018] (1) Prepare used lithium-ion secondary batteries A used lithium ion secondary battery 10 is prepared. This lithium ion secondary battery 10 includes a battery element 21, an electrolyte 22, and a battery container 24 that accommodates the battery element 21 and the electrolyte 22. The battery element 21 includes a positive electrode 12, a separator 20, and a negative electrode 16, and at least one of the positive electrode 12 and the negative electrode 16 is a ceramic electrode. Preferably, both the positive electrode 12 and the negative electrode 16 are ceramic electrodes. That is, the lithium ion secondary battery 10 is a sintered body type battery (semi-solid battery) that includes a ceramic electrode together with an electrolyte. This sintered body type battery is publicly known as disclosed in Patent Documents 6 and 7, and its preferred configuration will be described later. In particular, since the ceramic electrode is made of ceramic (sintered body), the positive electrode 12 and the negative electrode 16 can be handled separately from each other, which is preferable from the viewpoint of improving work efficiency. Therefore, a battery element in which the ceramic positive electrode layer, the ceramic separator, and the ceramic negative electrode layer as a whole form a single integrated sintered body is excluded from the scope of the present invention, since it would be difficult to separate the positive electrode 12 and the negative electrode 16. The battery element may further include a positive electrode current collector 14 and / or a negative electrode current collector 18.

[0019] (2) Removal of the battery element The ceramic electrodes are taken out from the lithium ion secondary battery 10 (specifically, the battery container 24) so ​​that the positive electrode 12 and the negative electrode 16 are separated from each other. At this time, the separator 20 may be bonded to the ceramic electrodes taken out, and a preferred example of such a form is an integrated sintered body of the ceramic electrode / ceramic separator. The battery element 21 may be taken out by removing a part of the battery container 24 (e.g., the negative electrode can 24b) to open the inside of the battery, and taking out the battery element 21 or the ceramic electrode (i.e., the positive electrode 12 and / or the negative electrode 16), which may be appropriately performed depending on the configuration of the battery container 24. After the battery element 21 is taken out as a whole, the positive electrode 12 may be separated from the negative electrode 16, or only the ceramic electrode (which may be bonded to the separator 20) that is the positive electrode 12 or the negative electrode 16 may be taken out while leaving the battery element 21 in the battery container 24. In any case, since the ceramic electrodes are made of ceramic (sintered bodies), the positive electrode 12 and the negative electrode 16 can be handled separately from each other. This is advantageous not only in terms of ease of operation, but also in terms of the ability to perform the electrode restoration process under more appropriate procedures and conditions depending on the type of ceramic electrode (positive electrode 12 or negative electrode 16). In other words, different electrode restoration processes can be performed on the positive electrode 12 and the negative electrode 16. Alternatively, the electrode restoration process may be performed on only one of the positive electrode 12 and the negative electrode 16.

[0020] (3) Electrode restoration treatment The removed ceramic electrodes (i.e., the positive electrode 12 and / or the negative electrode 16) are subjected to an electrode restoration treatment including washing and / or heat treatment. The electrode restoration treatment is not particularly limited as long as it is a washing and / or heat treatment that can improve the deteriorated electrode performance. Typically, the electrode restoration treatment is performed by washing the ceramic electrode with a polar solvent to remove impurities contained in and / or attached to the ceramic electrode, and then drying. The polar solvent may be either a non-aqueous solvent or water. Examples of non-aqueous solvents include NMP (N-methyl-2-pyrrolidone), ethanol, etc. The method of cleaning with a polar solvent is not particularly limited, but it is preferable to immerse the ceramic electrode in the polar solvent and perform ultrasonic cleaning or stirring.

[0021] The ceramic electrode thus washed and dried is preferably heated at 300 to 1000°C in order to further improve the electrode performance. Since the ceramic electrode in the present invention is a ceramic single body (excluding the positive electrode current collector 14 and / or the negative electrode current collector 18), it can be subjected to heat treatment such as degreasing and firing (which cannot be performed with a coated electrode containing an active material or binder). In this case, it is preferable to degrease and / or fire the ceramic electrode, and more preferably, both degreasing and firing are performed. The ceramic electrode can be degreased by heating the ceramic electrode preferably at 300 to 600°C, more preferably at 400 to 600°C, and the preferred holding time in the above temperature range is 0.5 to 20 hours, more preferably 2 to 20 hours. This causes unnecessary components or impurities (such as SEI) remaining in the ceramic electrode to disappear or be burned off, further reducing the amount of the remaining components, and further improving the battery performance. The ceramic electrode may be fired by heating the battery element at preferably 650 to 1000°C, more preferably 700 to 950°C, and the preferred retention time in the above temperature range is 0.01 to 20 hours, more preferably 0.01 to 15 hours. This allows the crystallinity of the material to be restored or improved, and the battery performance to be further improved. In addition, the strength of the electrode active material layer can be improved by further sintering the electrode active material. In addition, by making a lithium compound coexist and / or adopting a lithium-containing atmosphere during heat treatment such as degreasing and firing, it is possible to optimize the lithium content in the electrode active material and promote the recovery of the performance of the positive electrode 12 and / or the negative electrode 16. The above-mentioned degreasing conditions and / or firing conditions can also be applied in the same way when the separator 20 is bonded to the ceramic electrode (typically an integrated sintered body of the ceramic electrode / ceramic separator).

[0022] In addition, when the ceramic electrode further includes a positive electrode current collector 14 and / or a negative electrode current collector 18, it is preferable that the positive electrode current collector 14 and / or the negative electrode current collector 18 are removed before and / or during cleaning, and the positive electrode current collector 14 and / or the negative electrode current collector 18 are attached to the ceramic electrode after the electrode restoration process. In this way, the ceramic electrode alone can be subjected to cleaning and heat treatment as described above. The positive electrode current collector 14 and / or the negative electrode current collector 18 attached to the ceramic electrode after the electrode restoration process is not limited to a new positive electrode current collector 14 and / or a negative electrode current collector 18, and the removed positive electrode current collector 14 and / or the negative electrode current collector 18 may be reused.

[0023] (4) Battery assembly The ceramic electrode that has been subjected to the electrode restoration process is returned into the battery container 24 to assemble the lithium-ion secondary battery 10. The assembly of the lithium-ion secondary battery 10 may be performed by any procedure, and is not particularly limited, as long as the original structure of the lithium-ion secondary battery 10 is reproduced. The components other than the ceramic electrode that has been subjected to the electrode restoration process may be the same as those originally included in the used lithium-ion secondary battery 10, or may be replaced with new ones.

[0024] For example, after the ceramic electrode is removed and before it is returned to the battery container 24, the battery container 24 may be replaced with another battery container 24. Also, during or before assembling the lithium-ion secondary battery 10, the positive electrode 12 or the negative electrode 16 other than the ceramic electrode that has been subjected to the electrode restoration treatment may be replaced with a new or equivalent positive electrode 12 or negative electrode 16. Also, the separator 20 may be replaced with a new or equivalent separator 20.

[0025] The electrolyte 22 in the lithium ion secondary battery 10 (specifically, in the battery container 24) may be replaced with a fresh electrolyte 22. The electrolyte 22 is preferably replaced after the ceramic electrode is removed (for example, during or before the assembly of the battery), but is not limited thereto. For example, when the battery container 24 is replaced, fresh electrolyte 22 may be placed in the replaced battery container 24. The fresh electrolyte 22 may have the same composition as the electrolyte 22 originally used in the lithium ion secondary battery 10, or may have a different composition from the electrolyte 22 originally used, as long as it can exhibit acceptable performance. For example, an electrolyte 22 that provides better performance than the electrolyte 22 originally used may be used. Details of the preferred electrolyte 22 will be described later.

[0026] Lithium-ion secondary battery As shown in Fig. 1, a lithium ion secondary battery 10 includes a positive electrode 12, a negative electrode 16, a separator 20, an electrolyte 22, and a battery container 24. At least one of the positive electrode 12 and the negative electrode 16 is a ceramic electrode, but in the illustrated example, both the positive electrode 12 and the negative electrode 16 are depicted as ceramic electrodes. The separator 20 is interposed between the positive electrode 12 and the negative electrode 16. The electrolyte 22 is impregnated into the positive electrode 12, the negative electrode 16, and the separator 20. The battery container 24 includes a sealed space, and the positive electrode 12, the negative electrode 16, the separator 20, and the electrolyte 22 are accommodated in this sealed space.

[0027] The positive electrode 12 is preferably a ceramic positive electrode. In this case, the ceramic positive electrode 12 is preferably composed of a lithium composite oxide sintered body. The fact that the positive electrode 12 is composed of a sintered body means that the positive electrode 12 does not contain a binder or a conductive assistant. This is because even if the green sheet contains a binder, the binder disappears or is burned away during firing. And, since the positive electrode 12 does not contain a binder, there is an advantage that deterioration of the positive electrode due to the electrolyte 22 can be avoided. In addition, it is particularly preferable that the lithium composite oxide constituting the sintered body is lithium cobalt oxide (typically LiCoO2 (hereinafter, sometimes abbreviated as LCO)). Various lithium composite oxide sintered body plates or LCO sintered body plates are known, and for example, those disclosed in Patent Document 6 (Patent Publication No. 6374634) can be referred to. However, when the negative electrode 16 is a ceramic electrode, the positive electrode 12 does not necessarily have to be a ceramic electrode, and may be a powder-dispersed positive electrode (a so-called coated electrode) prepared by applying and drying a positive electrode mixture containing a positive electrode active material, a conductive assistant, a binder, and the like.

[0028] When the ceramic positive electrode 12 is composed of a lithium composite oxide sintered body, the ceramic positive electrode 12 (i.e., the lithium composite oxide sintered body) is preferably an oriented positive electrode that contains a plurality of primary particles composed of a lithium composite oxide, and the plurality of primary particles are oriented with respect to the main surface of the positive electrode (i.e., the layer surface of the positive electrode layer) at an average orientation angle of more than 0° and not more than 30°. Since the oriented positive electrode is oriented as described above, it is less susceptible to structural damage due to expansion and contraction accompanying charge and discharge, and is particularly suitable for reuse. FIG. 2 shows an example of a cross-sectional SEM image perpendicular to the layer surface of the oriented ceramic positive electrode 12, while FIG. 3 shows an electron backscatter diffraction (EBSD) image of the cross section perpendicular to the main surface of the oriented ceramic positive electrode 12. FIG. 4 shows a histogram showing the distribution of the orientation angles of the primary particles 11 in the EBSD image of FIG. 3 on an area basis. In the EBSD image shown in FIG. 3, discontinuity in the crystal orientation can be observed. In FIG. 3, the orientation angle of each primary particle 11 is shown by a shade of color, and the darker the color, the smaller the orientation angle. The orientation angle is the inclination angle that the (003) plane of each primary particle 11 makes with respect to the main surface direction. In Figures 2 and 3, the areas shown in black inside the oriented ceramic positive electrode 12 are pores.

[0029] The oriented ceramic positive electrode 12 is an oriented sintered body composed of a plurality of primary particles 11 bonded to each other. Each primary particle 11 is mainly plate-shaped, but may also be formed into a rectangular parallelepiped, cubic, spherical, or other shape. The cross-sectional shape of each primary particle 11 is not particularly limited, and may be rectangular, a polygonal shape other than a rectangle, a circle, an ellipse, or any other complex shape.

[0030] Each primary particle 11 is composed of a lithium composite oxide. xAn oxide represented by MO₂ (where 0.05 < x < 1.10, M is at least one transition metal, and M typically includes one or more of Co, Ni, and Mn). The lithium composite oxide has a layered rock salt structure. The layered rock salt structure refers to a crystal structure in which lithium layers and transition metal layers other than lithium are alternately stacked with oxygen layers in between, that is, a crystal structure in which a transition metal ion layer and a lithium single layer are alternately stacked via oxide ions (typically an α-NaFeO₂ type structure, that is, a structure in which transition metals and lithium are regularly arranged in the

[0111] axis direction of the cubic rock salt type structure). Examples of the lithium composite oxide include Li x CoO₂ (lithium cobaltate), Li x NiO₂ (lithium nickelate), Li x MnO₂ (lithium manganate), Li x NiMnO₂ (lithium nickel manganate), Li x NiCoO₂ (lithium nickel cobaltate), Li x CoNiMnO₂ (lithium cobalt nickel manganate), Li x CoMnO₂ (lithium cobalt manganate), etc. are mentioned, and particularly preferably Li x CoO₂ (lithium cobaltate, typically LiCoO₂). The lithium composite oxide may contain one or more elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, Ag, Sn, Sb, Te, Ba, Bi, and W.

[0031] As shown in Figs. 3 and 4, the average value of the orientation angles of the primary particles 11, i.e., the average orientation angle, is more than 0° and not more than 30°. This brings about various advantages as follows. First, since the primary particles 11 lie in a state inclined with respect to the thickness direction, the adhesion between the primary particles can be improved. As a result, the lithium ion conductivity between a certain primary particle 11 and other primary particles 11 adjacent to both sides of the primary particle 11 in the longitudinal direction can be improved, so that the rate characteristics can be improved. Secondly, the rate characteristics can be further improved. This is because, as described above, in the oriented ceramic positive electrode 12, expansion and contraction in the thickness direction is dominant over that in the main surface direction when lithium ions enter and exit, so that the expansion and contraction of the oriented ceramic positive electrode 12 becomes smooth, and accordingly, the entry and exit of lithium ions also becomes smooth. Thirdly, since the expansion and contraction of the oriented ceramic positive electrode 12 due to the entry and exit of lithium ions occurs predominantly in the direction perpendicular to the main surface, stress is less likely to occur at the bonding interface between the oriented ceramic positive electrode 12 and the separator 20, making it easier to maintain good bonding at the interface.

[0032] The average orientation angle of the primary particles 11 is obtained by the following method. First, in an EBSD image of a rectangular region of 95 μm×125 μm observed at a magnification of 1000 times as shown in FIG. 3, three horizontal lines are drawn to divide the oriented ceramic positive electrode 12 into four equal parts in the thickness direction, and three vertical lines are drawn to divide the oriented ceramic positive electrode 12 into four equal parts in the main surface direction. Next, the average orientation angle of the primary particles 11 is obtained by arithmetically averaging the orientation angles of all the primary particles 11 that intersect with at least one of the three horizontal lines and the three vertical lines. From the viewpoint of further improving the rate characteristics, the average orientation angle of the primary particles 11 is preferably 30° or less, more preferably 25° or less. From the viewpoint of further improving the rate characteristics, the average orientation angle of the primary particles 11 is preferably 2° or more, more preferably 5° or more.

[0033] As shown in FIG. 4, the orientation angle of each primary particle 11 may be widely distributed from 0° to 90°, but it is preferable that the majority of the orientation angles are distributed in the region of more than 0° and less than 30°. That is, when the cross section of the oriented sintered body constituting the oriented ceramic positive electrode 12 is analyzed by EBSD, the total area of ​​the primary particles 11 (hereinafter referred to as low-angle primary particles) having an orientation angle of more than 0° and less than 30° with respect to the layer surface of the oriented ceramic positive electrode 12 among the primary particles 11 contained in the analyzed cross section is preferably 70% or more, more preferably 80% or more, of the total area of ​​the primary particles 11 contained in the cross section (specifically, the 30 primary particles 11 used to calculate the average orientation angle). This makes it possible to increase the proportion of primary particles 11 with high mutual adhesion, thereby further improving the rate characteristics. In addition, it is more preferable that the total area of ​​the low-angle primary particles having an orientation angle of 20° or less is 50% or more of the total area of ​​the 30 primary particles 11 used to calculate the average orientation angle. Furthermore, the total area of ​​the low-angle primary particles having an orientation angle of 10° or less is more preferably 15% or more of the total area of ​​the 30 primary particles 11 used to calculate the average orientation angle.

[0034] Since each primary particle 11 is mainly plate-like, as shown in Figs. 2 and 3, the cross section of each primary particle 11 extends in a predetermined direction and is typically approximately rectangular. That is, when the cross section of the oriented sintered body is analyzed by EBSD, the total area of ​​the primary particles 11 having an aspect ratio of 4 or more among the primary particles 11 included in the analyzed cross section is preferably 70% or more, more preferably 80% or more, of the total area of ​​the primary particles 11 included in the cross section (specifically, the 30 primary particles 11 used to calculate the average orientation angle). Specifically, in the EBSD image shown in Fig. 3, this can further improve the mutual adhesion between the primary particles 11, and as a result, the rate characteristics can be further improved. The aspect ratio of the primary particles 11 is the value obtained by dividing the maximum Feret diameter of the primary particles 11 by the minimum Feret diameter. The maximum Feret diameter is the maximum distance between two parallel straight lines when the primary particle 11 is sandwiched between the two parallel straight lines on the EBSD image when the cross section is observed. The minimum Feret diameter is the minimum distance between two parallel lines when the primary particle 11 is sandwiched between the lines on an EBSD image.

[0035] The average particle size of the primary particles constituting the oriented sintered body is preferably 5 μm or more. Specifically, the average particle size of the 30 primary particles 11 used to calculate the average orientation angle is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 12 μm or more. This reduces the number of grain boundaries between the primary particles 11 in the direction in which lithium ions are conducted, improving the overall lithium ion conductivity, and thus improving the rate characteristics. The average particle size of the primary particles 11 is the arithmetic average of the circle-equivalent diameters of the primary particles 11. The circle-equivalent diameter is the diameter of a circle having the same area as each primary particle 11 on an EBSD image.

[0036] It is preferable that the ceramic positive electrode 12 contains pores. When the sintered body contains pores, particularly open pores, the electrolyte can penetrate into the sintered body when the sintered body is incorporated into a battery as a positive electrode, and as a result, the lithium ion conductivity can be improved. This is because the conduction of lithium ions in the sintered body is by far faster through the electrolyte in the pores than through the particles that constitute the sintered body, and through the electrolyte in the pores.

[0037] The ceramic positive electrode 12 (preferably a lithium composite oxide sintered body) preferably has a porosity of 20 to 60%, more preferably 25 to 55%, further preferably 30 to 50%, and particularly preferably 30 to 45%. The pores are expected to provide a stress relief effect and a high capacity, and the mutual adhesion between the primary particles 11 can be improved, thereby further improving the rate characteristics. The porosity of the sintered body is calculated by polishing the cross section of the positive electrode layer with a CP (cross section polisher) and then observing the SEM at a magnification of 1000, and binarizing the obtained SEM image. The average circle equivalent diameter of each pore formed inside the oriented sintered body is not particularly limited, but is preferably 8 μm or less. The smaller the average circle equivalent diameter of each pore, the more the mutual adhesion between the primary particles 11 can be improved, and as a result, the rate characteristics can be further improved. The average circle equivalent diameter of the pores is the arithmetic average of the circle equivalent diameters of 10 pores on the EBSD image. The circle equivalent diameter is the diameter of a circle having the same area as each pore on an EBSD image. Each pore formed inside the oriented sintered body is preferably an open pore that communicates with the outside of the positive electrode 12.

[0038] The average pore size of the ceramic positive electrode 12, i.e., the lithium composite oxide sintered body, is preferably 0.1 to 10.0 μm, more preferably 0.2 to 5.0 μm, and further preferably 0.25 to 3.0 μm. Within the above range, local stress concentration in large pores is suppressed, and stress in the sintered body is easily released uniformly.

[0039] The thickness of the ceramic positive electrode 12 (positive electrode layer) is preferably 60 to 450 μm, more preferably 70 to 350 μm, and further preferably 90 to 300 μm. Within such a range, the active material capacity per unit area is increased to improve the energy density of the lithium-ion secondary battery 10, and deterioration of the battery characteristics (particularly an increase in the resistance value) due to repeated charging and discharging can be suppressed.

[0040] The negative electrode 16 is preferably a ceramic negative electrode. In this case, the ceramic negative electrode 16 is preferably composed of a titanium-containing sintered body. However, when the negative electrode 16 is a ceramic electrode, the negative electrode 16 does not necessarily have to be a ceramic electrode, and may be a powder-dispersed negative electrode (so-called coated electrode) prepared by applying and drying a negative electrode mixture containing a negative electrode active material, a conductive assistant, a binder, and the like.

[0041] When the ceramic negative electrode 16 is made of a titanium-containing sintered body, the ceramic negative electrode 16 (i.e., the titanium-containing sintered body) is made of lithium titanate Li4Ti5O 12 It is preferable that the battery contains Li4Ti5O (hereinafter referred to as LTO) or niobium titanium composite oxide Nb2TiO7, and more preferably contains LTO. Although LTO is typically known to have a spinel structure, it can also adopt other structures during charging and discharging. For example, LTO is Li4Ti5O 12 (spinel structure) and Li7Ti5O 12 The reaction proceeds in the coexistence of two phases, i.e., spinel and tetrahydrofuran (rock salt structure). Therefore, LTO is not limited to a spinel structure.

[0042] The ceramic negative electrode 16 being made of a sintered body means that the negative electrode 16 does not contain a binder or a conductive additive. This is because even if the green sheet contains a binder, the binder will disappear or be burned away during firing. Since the negative electrode layer does not contain a binder, the packing density of the negative electrode active material (e.g., LTO or Nb2TiO7) becomes high, and a high capacity and good charge / discharge efficiency can be obtained. The LTO sintered body can be manufactured according to the method described in Patent Document 7 (Japanese Patent No. 6392493).

[0043] The ceramic negative electrode 16 (preferably a titanium-containing sintered body) has a structure in which a plurality (i.e., a large number) of primary particles are bonded together. Therefore, it is preferable that these primary particles are composed of LTO or Nb2TiO7.

[0044] The thickness of the ceramic negative electrode 16 (negative electrode layer) is preferably 70 to 500 μm, more preferably 85 to 400 μm, and more preferably 95 to 350 μm. The thicker the negative electrode 16, the easier it is to realize a battery with a high capacity and high energy density. The thickness of the negative electrode 16 can be obtained, for example, by measuring the distance between layer surfaces observed to be approximately parallel when a cross section of the negative electrode 16 is observed by SEM (scanning electron microscope).

[0045] The primary particle size, which is the average particle size of the multiple primary particles constituting the ceramic negative electrode 16, is preferably 1.2 μm or less, more preferably 0.02 to 1.2 μm, and further preferably 0.05 to 0.7 μm. Within such a range, it is easy to achieve both lithium ion conductivity and electronic conductivity, which contributes to improving the rate performance.

[0046] It is preferable that the ceramic negative electrode 16 contains pores. When the sintered body contains pores, particularly open pores, and is incorporated into a battery as a negative electrode layer, the electrolyte can penetrate into the sintered body, thereby improving the lithium ion conductivity. This is because the conduction of lithium ions in the sintered body is by far faster than the conduction through the electrolyte in the pores, although there are two types of conduction: through the constituent particles of the sintered body and through the electrolyte in the pores.

[0047] The porosity of the ceramic negative electrode 16 is preferably 20 to 60%, more preferably 30 to 55%, and further preferably 35 to 50%. Within such a range, it is easy to achieve both lithium ion conductivity and electronic conductivity, which contributes to improving the rate performance.

[0048] The average pore size of the ceramic negative electrode 16 is 0.08 to 5.0 μm, preferably 0.1 to 3.0 μm, and more preferably 0.12 to 1.5 μm. Within such a range, it is easy to achieve both lithium ion conductivity and electronic conductivity, which contributes to improving the rate performance.

[0049] The separator 20 is preferably a ceramic separator. The separator 20 is a microporous film made of ceramic. The ceramic separator 20 is advantageous in that it can be manufactured as a single integral sintered plate together with either the positive electrode 12 or the negative electrode 16 as a whole, as well as being excellent in heat resistance. The ceramic contained in the ceramic separator 20 is preferably at least one selected from MgO, Al2O3, ZrO2, SiC, Si3N4, AlN, and cordierite, and more preferably at least one selected from MgO, Al2O3, and ZrO2. The thickness of the ceramic separator 20 is preferably 3 to 40 μm, more preferably 5 to 35 μm, and even more preferably 10 to 30 μm. The porosity of the ceramic separator 20 is preferably 30 to 85%, and more preferably 40 to 80%. Alternatively, the separator 20 may be a polymer microporous film. In this case, the separator 20 is preferably made of polyolefin, polyimide, polyester (for example, polyethylene terephthalate (PET)), or cellulose. Examples of polyolefin include polypropylene (PP), polyethylene (PE), and combinations thereof.

[0050] The electrolyte solution 22 is not particularly limited, and may be a commercially available electrolyte solution for lithium batteries, such as a solution in which a lithium salt (e.g., LiPF6) is dissolved in a non-aqueous solvent such as an organic solvent (e.g., a mixed solvent of ethylene carbonate (EC) and methyl ethyl carbonate (MEC), a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC), or a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC)).

[0051] In order to obtain a lithium ion secondary battery having excellent heat resistance, the electrolyte 22 is preferably a non-aqueous solvent containing lithium borofluoride (LiBF4). In this case, the preferred non-aqueous solvent is at least one selected from the group consisting of γ-butyrolactone (GBL), ethylene carbonate (EC) and propylene carbonate (PC), more preferably a mixed solvent of EC and GBL, a single solvent of PC, a mixed solvent of PC and GBL, or a single solvent of GBL, and particularly preferably a mixed solvent of EC and GBL or a single solvent of GBL. The non-aqueous solvent contains γ-butyrolactone (GBL) to increase the boiling point and significantly improve the heat resistance. From this viewpoint, the volume ratio of EC:GBL in the non-aqueous solvent containing EC and / or GBL is preferably 0:1 to 1:1 (GBL ratio 50 to 100 volume%), more preferably 0:1 to 1:1.5 (GBL ratio 60 to 100 volume%), even more preferably 0:1 to 1:2 (GBL ratio 66.6 to 100 volume%), and particularly preferably 0:1 to 1:3 (GBL ratio 75 to 100 volume%). Lithium borofluoride (LiBF4) dissolved in the non-aqueous solvent is an electrolyte with a high decomposition temperature, which also brings about a significant improvement in heat resistance. The concentration of LiBF4 in the electrolytic solution 22 is preferably 0.5 to 2 mol / L, more preferably 0.6 to 1.9 mol / L, even more preferably 0.7 to 1.7 mol / L, and particularly preferably 0.8 to 1.5 mol / L.

[0052] The electrolyte solution 22 may further contain vinylene carbonate (VC) and / or fluoroethylene carbonate (FEC) and / or vinyl ethylene carbonate (VEC) as an additive. Both VC and FEC have excellent heat resistance. Therefore, by including such an additive in the electrolyte solution 22, an SEI film having excellent heat resistance can be formed on the surface of the negative electrode 16.

[0053] The battery container 24 has a sealed space, and the positive electrode 12, the negative electrode 16, the separator 20, and the electrolyte 22 are accommodated in this sealed space. The battery container 24 may be appropriately selected according to the type of the lithium ion secondary battery 10. For example, when the lithium ion secondary battery is in the form of a coin-shaped battery as shown in FIG. 1, the battery container 24 typically includes a positive electrode can 24a, a negative electrode can 24b, and a gasket 24c, and the positive electrode can 24a and the negative electrode can 24b are crimped via the gasket 24c to form a sealed space. The positive electrode can 24a and the negative electrode can 24b may be made of a metal such as stainless steel, and are not particularly limited. The gasket 24c may be a ring-shaped member made of an insulating resin such as polypropylene, polytetrafluoroethylene, or PFA resin, and are not particularly limited.

[0054] The lithium ion secondary battery 10 preferably further includes a positive electrode current collector 14 and / or a negative electrode current collector 18. The positive electrode current collector 14 and the negative electrode current collector 18 are not particularly limited, but are preferably metal foils such as copper foil and aluminum foil. The positive electrode current collector 14 is preferably disposed between the positive electrode 12 and the battery container 24 (e.g., the positive electrode can 24a), and the negative electrode current collector 18 is preferably disposed between the negative electrode 16 and the battery container 24 (e.g., the negative electrode can 24b). In addition, a positive electrode side carbon layer 13 is preferably provided between the positive electrode 12 and the positive electrode current collector 14 from the viewpoint of reducing contact resistance. Similarly, a negative electrode side carbon layer 17 is preferably provided between the negative electrode 16 and the negative electrode current collector 18 from the viewpoint of reducing contact resistance. Both the positive electrode side carbon layer 13 and the negative electrode side carbon layer 17 are preferably made of conductive carbon, and may be formed, for example, by applying a conductive carbon paste by screen printing or the like.

[0055] Honeycomb-type secondary battery The ceramic positive electrode 12 or the ceramic negative electrode 16 may have a honeycomb structure. In this way, a three-dimensional structure suitable for high capacity and high output, capable of accommodating a plurality of negative electrodes 16 or positive electrodes 12 inside the honeycomb structure, can be realized. FIG. 5 shows an example of a honeycomb-type ceramic positive electrode 12'. The honeycomb-type ceramic positive electrode 12' has a columnar honeycomb structure. This columnar honeycomb structure has a first end face 12a, a second end face 12b parallel to the first end face 12a, and an outer peripheral side face 12c perpendicular to the first end face 12a and the second end face 12b. In addition, the columnar honeycomb structure has a plurality of holes 12d extending from the first end face 12a toward the second end face 12b, and these holes 12d are partitioned by partition walls 12e.

[0056] The honeycomb ceramic positive electrode 12' is preferably made of a lithium composite oxide sintered body, and more preferably made of an oriented lithium composite oxide sintered body. In this case, when the central axis of the columnar honeycomb structure parallel to the outer peripheral side surface 12c or an axis parallel thereto is defined as the z-axis, it is preferable that the primary particles are oriented in the z-axis direction (for example, at an average orientation angle of more than 0° and not more than 30° with respect to the z-axis). In addition, when the columnar honeycomb structure is viewed in a plan view in the z-axis direction and one direction of the lattice-like partition wall 12e is assigned to the x-axis and the other direction to the y-axis, it is preferable that the primary particles constituting the partition wall 12e in the x-axis direction are oriented in the x-axis direction (for example, at an average orientation angle of more than 0° and not more than 30° with respect to the x-axis), and the primary particles constituting the partition wall 12e in the y-axis direction are oriented in the y-axis direction (for example, at an average orientation angle of more than 0° and not more than 30° with respect to the y-axis). In this way, the primary particles are oriented in all directions of the x-axis, y-axis, and z-axis of the columnar honeycomb structure, so that the resistance is reduced not only in the z-axis direction (the length direction of the columnar honeycomb structure) but also in the x-axis and y-axis directions (i.e., the xy plane direction), which is believed to promote lithium ion conduction and electron conduction, resulting in improved battery characteristics (e.g., discharge rate characteristics) in the secondary battery 10.

[0057] 6A and 6B show a lithium ion secondary battery 10' with a honeycomb-type ceramic positive electrode 12'. For convenience of explanation, these figures show only a part cut out into a rectangular column from a columnar honeycomb structure. The secondary battery 10' includes a honeycomb-type ceramic positive electrode 12', a plurality of negative electrodes 16', a separator 20', an electrolyte (not shown), and a battery container (not shown). The plurality of negative electrodes 16' are inserted into the holes of the honeycomb-type ceramic positive electrode 12', and the ends of the negative electrodes 16' extend from the first end surface 12a or the second end surface 12b. The separator 20' is interposed between the honeycomb-type ceramic positive electrode 12' and the negative electrode 16'.

[0058] The lithium ion secondary battery 10' having the honeycomb type ceramic positive electrode 12' may be manufactured by any manufacturing method. For example, the separator 20' may be formed in advance on the surface of the negative electrode 16', and the negative electrode 16' covered with the separator 20' may be inserted into the hole 12d of the honeycomb type ceramic positive electrode 12'. In this case, the separator 20' may be formed on the surface of the negative electrode 16' by applying a slurry containing ceramic powder (e.g., MgO powder), a binder, a dispersion medium, etc. (e.g., by dip coating) to the negative electrode 16' and drying it. Alternatively, the separator 20' may be formed in advance on the surface of the partition wall 12e of the honeycomb type ceramic positive electrode 12', and the rod-shaped negative electrode 16' may be inserted into the hole 12d. In this case, instead of inserting the rod-shaped negative electrode 16', a slurry containing a negative electrode active material (e.g., graphite slurry) may be poured into the hole 12d to form the negative electrode 16'.

[0059] The method for recycling a lithium ion secondary battery according to the present invention can also be preferably applied to the honeycomb type secondary battery 10' described above. In this case, too, the honeycomb type ceramic positive electrode 12' and the negative electrode 16' can be separated and the electrode restoration treatment can be performed. For example, when the negative electrode 16' is rod-shaped, the rod-shaped negative electrode 16' can be pulled out from the honeycomb type ceramic positive electrode 12' to separate the positive electrode 12' and the negative electrode 16'. Furthermore, when the negative electrode 16' is formed of a slurry (e.g., graphite slurry) containing a negative electrode active material poured into the holes 12d of the honeycomb type ceramic positive electrode 12', the positive electrode 12' and the negative electrode 16' may be separated by dissolving the negative electrode active material slurry using a solvent (e.g., NMP (N-methyl-2-pyrrolidone)). Even when the negative electrode is a honeycomb type ceramic and the positive electrode is a rod-shaped or slurry-shaped positive electrode, unlike the above configuration, the positive electrode and the negative electrode can be separated by the same method as above and the electrode restoration treatment can be performed. EXAMPLES

[0060] The present invention will be described more specifically with reference to the following examples. In the following examples, LiCoO2 is abbreviated as "LCO" and Li4Ti5O 12 shall be abbreviated as "LTO."

[0061] Example 1 (1) Preparation of LCO green sheet (positive electrode green sheet) First, Co3O4 powder (manufactured by Seido Chemical Industry Co., Ltd.) and Li2CO3 powder (manufactured by Honjo Chemical Co., Ltd.) were mixed so that the molar ratio of Li / Co was 1.01, and then the mixture was kept at 780°C for 5 hours. The obtained powder was pulverized in a pot mill so that the volumetric D50 was 0.4 μm to obtain a powder consisting of LCO plate-like particles. 100 parts by weight of the obtained LCO powder, 100 parts by weight of a dispersion medium (toluene: isopropanol = 1:1), 10 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di (2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The obtained mixture was stirred under reduced pressure to defoam it, and the viscosity was adjusted to 4000 cP to prepare an LCO slurry. The viscosity was measured using a Brookfield LVT viscometer. The slurry thus prepared was formed into a sheet on a PET film by a doctor blade method to form an LCO green sheet. The thickness of the LCO green sheet was adjusted to 60 μm after firing.

[0062] (2) Preparation of LTO green sheet (negative electrode green sheet) First, 100 parts by weight of LTO powder (volume-based D50 particle size 0.06 μm, manufactured by Sigma-Aldrich Japan LLC), 100 parts by weight of dispersion medium (toluene: isopropanol = 1:1), 20 parts by weight of binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of plasticizer (DOP: Di (2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The obtained negative electrode raw material mixture was stirred and degassed under reduced pressure, and the viscosity was adjusted to 4000 cP to prepare an LTO slurry. The viscosity was measured with an LVT type viscometer manufactured by Brookfield. The slurry thus prepared was formed into a sheet shape on a PET film by the doctor blade method to form an LTO green sheet. The thickness of the LTO green sheet was set so that the thickness after firing was 70 μm.

[0063] (3) Preparation of MgO green sheet (separator green sheet) Magnesium carbonate powder (manufactured by Konoshima Chemical Co., Ltd.) was heat-treated at 900°C for 5 hours to obtain MgO powder. The obtained MgO powder and glass frit (manufactured by Nippon Frit Co., Ltd., CK0199) were mixed at a weight ratio of 4:1. 100 parts by weight of the obtained mixed powder (volume-based D50 particle size 0.4 μm), 100 parts by weight of a dispersion medium (toluene: isopropanol = 1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di (2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The obtained raw material mixture was stirred under reduced pressure to defoam it, and the viscosity was adjusted to 4000 cP to prepare a slurry. The viscosity was measured with a Brookfield LVT type viscometer. The slurry thus prepared was formed into a sheet on a PET film by a doctor blade method to form a separator green sheet, the thickness of which was adjusted to 25 μm after firing.

[0064] (4a) Preparation of positive electrode / separator sintered plate The LCO green sheet (positive electrode green sheet) is stacked with the MgO green sheet (separator green sheet), and the resulting laminate is subjected to CIP (cold isostatic pressing) at 200 kgf / cm 2 The green sheets were pressed together with a press. The laminate thus pressed was punched out into a disk shape with a diameter of 10 mm using a punching die. The obtained disk-shaped laminate was degreased at 600°C for 5 hours, and then heated to 800°C at a rate of 1000°C / h and held there for 10 minutes for firing, after which it was cooled. In this way, a positive electrode / separator integrated sintered plate was obtained, which included two layers: a positive electrode layer (LCO sintered body layer) and a ceramic separator (MgO separator).

[0065] (4b) Preparation of negative electrode layer (LTO sintered layer) The LTO green sheet (negative electrode green sheet) was punched out into a disk shape with a diameter of 10 mm using a punching die. The obtained disk was degreased at 600°C for 5 hours, then heated to 800°C at 1000°C / h and held there for 10 minutes for firing, and then cooled. In this way, a sintered plate of the negative electrode layer (LTO sintered body layer) was obtained.

[0066] (5) Fabrication of lithium-ion secondary batteries A coin-type lithium-ion secondary battery 10 as shown in FIG. 1 was fabricated as follows.

[0067] (5a) Bonding the negative electrode layer and negative electrode current collector with conductive carbon paste Acetylene black and polyimide amide were weighed out to a mass ratio of 3:1, and mixed with an appropriate amount of NMP (N-methyl-2-pyrrolidone) as a solvent to prepare a conductive carbon paste as a conductive adhesive. The conductive carbon paste was screen-printed on an aluminum foil as a negative electrode current collector. The negative electrode sintered plate prepared in (4b) above was placed so that the negative electrode layer was contained within the undried printing pattern (i.e., the area coated with the conductive carbon paste), and the negative electrode sintered plate was vacuum-dried at 60°C for 30 minutes to prepare a structure in which the negative electrode layer and the negative electrode current collector were bonded via the negative electrode-side carbon layer. The thickness of the negative electrode-side carbon layer was set to 10 μm.

[0068] (5b) Preparation of positive electrode current collector with carbon layer Acetylene black and polyimide amide were weighed out to a mass ratio of 3:1 and mixed with an appropriate amount of NMP (N-methyl-2-pyrrolidone) as a solvent to prepare a conductive carbon paste. The conductive carbon paste was screen-printed on an aluminum foil as a positive electrode current collector, and then vacuum-dried at 60°C for 30 minutes to prepare a positive electrode current collector with a positive electrode carbon layer formed on the surface. The thickness of the positive electrode carbon layer was 5 μm.

[0069] (5c) Coin Cell Battery Assembly Between the positive electrode can and the negative electrode can that constitute the battery case, the positive electrode current collector, the positive electrode side carbon layer, the positive electrode / separator integrated sintered plate (LCO positive electrode layer and MgO separator), the negative electrode sintered plate, the negative electrode side carbon layer, and the negative electrode current collector were stacked in this order from the positive electrode can to the negative electrode can, and after filling with electrolyte, the positive electrode can and the negative electrode can were crimped via a gasket to seal. In this way, a coin cell type lithium ion secondary battery 10 with a diameter of 12 mm and a thickness of 1.0 mm was produced. At this time, the electrolyte used was a solution obtained by dissolving LiBF4 to a concentration of 1.5 mol / L in an organic solvent in which ethylene carbonate (EC) and γ-butyrolactone (GBL) were mixed in a volume ratio of 1:3.

[0070] (6) Measurement of capacity retention rate after storage The post-storage capacity retention rate of the battery was measured by the following procedure. First, the battery was charged at a constant voltage of 2.7 V in a 25° C. environment, and then discharged at a discharge rate of 0.2 C to measure the initial capacity. Next, the battery was held for 50 days in a 60° C. environment with a voltage of 2.7 V applied. Finally, the battery was charged at a constant voltage of 2.7 V, and then discharged at 0.2 C to measure the post-storage capacity. The measured post-storage capacity was divided by the initial capacity and multiplied by 100 to obtain the post-storage capacity retention rate (%).

[0071] (7) Dismantling, cleaning and reassembling the battery after storage A battery in a discharged state after storage was prepared, and the sealing part where the positive electrode can and the negative electrode can were crimped was opened. Next, the negative electrode can and the gasket were removed from the battery, and the positive electrode current collector, the positive electrode / separator integrated sintered body plate, the negative electrode sintered body plate, and the negative electrode current collector were taken out from inside. The positive electrode current collector was removed from the taken out positive electrode / separator integrated sintered body plate. The positive electrode / separator integrated sintered body plate and the negative electrode sintered body plate to which the negative electrode current collector was attached were immersed in an appropriate amount of NMP (N-methyl-2-pyrrolidone) and stirred for 60 minutes. In this way, the positive electrode side carbon layer attached to the positive electrode / separator integrated sintered body plate, the negative electrode side carbon layer attached to the negative electrode sintered body plate, and impurities such as electrolyte decomposition products attached to the positive electrode / separator integrated sintered body plate and the negative electrode sintered body plate were dissolved and removed, and at the same time, the negative electrode current collector was peeled off. The same procedure was repeated twice, and the positive electrode / separator integrated sintered body plate and the negative electrode sintered body plate from which impurities had been removed were vacuum-dried for 12 hours at 120° C. The vacuum-dried positive electrode / separator integrated sintered body plate and negative electrode sintered body plate were reassembled into a coin-type battery by the above steps (5a), (5b), and (5c).

[0072] (8) Capacity retention rate of reassembled batteries The capacity retention rate of the reassembled battery was measured by the following procedure. First, the battery was charged at a constant voltage of 2.7 V in a 25° C. environment, and then discharged at a discharge rate of 0.2 C to measure the capacity after reassembly. The measured capacity after reassembly was divided by the initial capacity and multiplied by 100 to obtain the capacity retention rate after reassembly (%).

[0073] Example 2 The reassembled battery was evaluated in the same manner as in Example 1, except that the vacuum-dried positive electrode / separator integrated sintered body plate and the negative electrode sintered plate were degreased by heating them at 600°C for 5 hours and then used to reassemble the battery.

[0074] Example 3 The reassembled battery was evaluated in the same manner as in Example 2, except that the degreased positive electrode / separator integrated sintered body plate and the negative electrode sintered plate were each fired at 800° C. for 10 minutes and then used to reassemble the battery.

[0075] Example 4 The reassembled battery was evaluated in the same manner as in Example 2, except that only the vacuum-dried positive electrode / separator integrated sintered body plate was degreased (that is, the negative electrode sintered plate was not degreased).

[0076] Example 5 The reassembled battery was evaluated in the same manner as in Example 3, except that only the vacuum-dried positive electrode / separator integrated sintered body plate was degreased and fired (i.e., the negative electrode sintered plate was not degreased or fired).

[0077] Example 6 The reassembled battery was evaluated in the same manner as in Example 3, except that the electrode restoration process (cleaning, drying, degreasing, and firing) was performed only on the vacuum-dried positive electrode / separator integrated sintered body plate (i.e., the negative electrode sintered plate was not subjected to the electrode restoration process).

[0078] Example 7 (comparison) The reassembled battery was evaluated in the same manner as in Example 1, except that the positive and negative electrodes were not subjected to electrode restoration treatment (cleaning and drying) after disassembly of the battery, and only the electrolyte was replaced.

[0079] Example 8 (comparison) A battery was produced in the same manner as in Example 1, except that a) a commercially available LCO coated electrode (manufactured by Hosen Co., Ltd.) was used as the positive electrode instead of the LCO sintered body layer, b) a carbon coated electrode on a negative electrode current collector produced by the procedure shown below was used as the negative electrode and negative electrode current collector, and c) a cellulose separator was used as the separator. In addition, the battery was evaluated in the same manner as in Example 1, except that the charging voltage and the applied voltage during storage were 4.2 V.

[0080] (Preparation of carbon-coated electrodes) A paste containing a mixture of graphite as an active material and polyvinylidene fluoride (PVDF) as a binder was applied to the surface of a negative electrode current collector (aluminum foil) and then dried to produce a carbon-coated electrode with a carbon layer 280 μm thick.

[0081] Evaluation results Table 1 shows the evaluation results of Examples 1 to 8.

[0082] [Table 1]

[0083] As can be seen from the results shown in Table 1, in Examples 1 to 6, the capacity retention rate was significantly restored due to the effect of removing impurities by the electrode restoration treatment. On the other hand, in Example 7, which is a comparative example in which only the electrolyte was replaced, no significant improvement in the capacity retention rate was observed. In addition, in Example 8, a comparative example in which a coated electrode (containing a binder, etc.) was used, deterioration occurred due to the detachment of the active material during the washing process.

[0084] Example 9 (1) Preparation of the positive electrode A honeycomb-type ceramic positive electrode was prepared by the following procedure.

[0085] (1a) Preparation of molding materials Co3O4 powder (manufactured by Seido Chemical Industry Co., Ltd.) and Li2CO3 powder (manufactured by Honjo Chemical Co., Ltd.) were mixed so that the molar ratio of Li / Co was 1.01, and then the mixture was kept at 780°C for 5 hours. The resulting powder was pulverized and crushed in a pot mill so that the volume standard D50 was 0.4 μm to obtain LiCoO2 raw material powder. 100 parts by weight of this LiCoO2 raw material powder, 30 parts by weight of a dispersion medium (toluene: isopropanol = 1:1), 10 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di (2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed to obtain a clay-like molding raw material.

[0086] (1b) Molding The obtained molding raw material was extruded to obtain a honeycomb molded body. The die dimensions were as follows: The honeycomb shape was formed with a wall thickness of 100 μm and a pitch of 2.0 mm. The area of ​​the die was approximately 20 × 20 mm. The obtained honeycomb molded body was cut into a length of 50 mm.

[0087] (1c) Firing The honeycomb molded body was heated to 600°C at a heating rate of 200°C / h and degreased for 3 hours, and then placed in an alumina sheath (Nikkato Corporation). The temperature was raised to 920°C at 200°C / h in the sealed sheath and held for 4 hours. The honeycomb structure was densely sintered to obtain a honeycomb-type oriented ceramic positive electrode with a wall thickness of 100 μm and a pitch of 2.0 mm.

[0088] (2) Preparation of the negative electrode 100 parts by weight of artificial graphite (SCMG-CF manufactured by Showa Denko K.K.) and 10 parts by weight of PTFE (Polyflon D-1E manufactured by Daikin Industries, Ltd.) were mixed with 30 parts by weight of isopropanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and extruded through a die measuring 1.9 x 1.9 mm to obtain a rectangular parallelepiped negative electrode. This was dried under reduced pressure (-95 kPa, 80°C, 16 h) and cut to a length of 50 mm to produce a rectangular parallelepiped negative electrode.

[0089] (3) Preparation of the separator Magnesium carbonate powder (manufactured by Konoshima Chemical Co., Ltd.) was heat-treated at 900°C for 5 hours to obtain MgO powder. 100 parts by weight of this powder, 100 parts by weight of a dispersion medium (toluene: isopropanol = 1:1), 20 parts by weight of a binder (polyvinyl butyral: product number BM-2, manufactured by Sekisui Chemical Co., Ltd.), 4 parts by weight of a plasticizer (DOP: Di (2-ethylhexyl) phthalate, manufactured by Kurogane Kasei Co., Ltd.), and 2 parts by weight of a dispersant (product name Rheodol SP-O30, manufactured by Kao Corporation) were mixed. The above-mentioned rectangular parallelepiped negative electrode was dip-coated with the obtained paint up to 49 mm out of the 50 mm in the length direction, and then vacuum dried (-95 kPa, 100°C, 2 h) to form a separator film on the surface of the rectangular parallelepiped negative electrode.

[0090] (4) Preparation of conductive adhesive Acetylene black and polyimide amide were weighed out to a mass ratio of 3:1, and mixed with an appropriate amount of NMP (N-methyl-2-pyrrolidone) as a solvent to prepare a conductive carbon paste as a conductive adhesive.

[0091] (5) Battery construction A rectangular parallelepiped negative electrode with an MgO separator formed thereon is inserted into each of the holes with a 2.0 mm pitch formed in the honeycomb ceramic positive electrode. The insertion into the honeycomb ceramic positive electrode is limited to the 49 mm portion where the separator is formed. Next, a 10 μm thick copper foil is attached to the end face of the negative electrode at the 1 mm portion protruding from the honeycomb structure using the conductive adhesive. In addition, a 15 μm thick aluminum foil is attached to the end face of the honeycomb ceramic positive electrode where the negative electrode does not protrude using a conductive adhesive. This structure is enclosed in a glass cell provided with a current collector, and an electrolyte is poured and sealed to form a battery. As the electrolyte, LiPF6 is dissolved in an organic solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 3:7 to a concentration of 1.0 mol / L, and vinylene carbonate is further added as an additive to make 2 parts by weight.

[0092] (6) Measurement of capacity retention rate after storage The post-storage capacity retention rate of the battery was measured by the following procedure. First, the battery was charged at a constant voltage of 4.2 V in a 25° C. environment, and then discharged at a discharge rate of 0.2 C to measure the initial capacity. Next, the battery was held for 50 days in a 50° C. environment with a voltage of 4.2 V applied. Finally, the battery was charged at a constant voltage of 4.2 V, and then discharged at 0.2 C to measure the post-storage capacity. The measured post-storage capacity was divided by the initial capacity and multiplied by 100 to obtain the post-storage capacity retention rate (%).

[0093] (7) Dismantling, cleaning and reassembling the battery after storage A battery in a discharged state after storage was prepared, and the sealed part of the glass cell was opened. The honeycomb structure was removed from the glass cell. The rectangular parallelepiped negative electrode inserted into the honeycomb-type ceramic positive electrode was pulled out, and the honeycomb-type ceramic positive electrode and the rectangular parallelepiped negative electrode were separated. The removed honeycomb-type ceramic positive electrode was immersed in an appropriate amount of NMP (N-methyl-2-pyrrolidone) and stirred for 20 minutes to remove the aluminum foil and conductive adhesive attached to the positive electrode. The separated honeycomb-type ceramic positive electrode was immersed in NMP again and stirred for 60 minutes to dissolve and remove impurities such as electrolyte decomposition products attached to the honeycomb-type ceramic positive electrode. The same operation was repeated twice, and the honeycomb-type ceramic positive electrode from which the impurities had been removed was vacuum-dried at 120°C for 12 hours. The vacuum-dried honeycomb-type ceramic positive electrode was heated at 600°C for 5 hours to degrease it, and then fired at 900°C for 1 hour. The removed rectangular parallelepiped negative electrode was inserted into the fired honeycomb ceramic positive electrode, and the resulting glass cell was reassembled in the same manner as in (5) above (including replacement of the electrolyte).

[0094] Example 10 (comparison) In the above (7), the reassembled battery was evaluated in the same manner as in Example 8, except that the electrode restoration treatment (cleaning and drying) after disassembly of the battery was not performed and only the electrolyte was replaced.

[0095] [Table 2]

Claims

1. (i) preparing a used lithium ion secondary battery comprising a battery element including a positive electrode, a separator, and a negative electrode, at least one of the positive electrode and the negative electrode being a ceramic electrode, (ii) an electrolyte, and (iii) a battery container that contains the battery element and the electrolyte; removing the ceramic electrode from the lithium ion secondary battery such that the positive electrode and the negative electrode are separated from each other (however, the separator may be bonded to the removed ceramic electrode); subjecting the removed ceramic electrode to an electrode restoration treatment including cleaning and / or heat treatment; returning the ceramic electrode that has been subjected to the electrode restoration treatment into the battery container to assemble a lithium ion secondary battery; A method for reusing a lithium-ion secondary battery, comprising:

2. 2. The method for reusing a lithium ion secondary battery according to claim 1, wherein the electrode revival treatment includes washing the ceramic electrode with a polar solvent to remove impurities contained in and / or attached to the ceramic electrode, and then drying the ceramic electrode.

3. The ceramic electrode further comprises a positive electrode current collector and / or a negative electrode current collector, The positive and / or negative current collectors are removed before and / or during said cleaning, and The method for reusing a lithium ion secondary battery according to claim 1 or 2, wherein a positive electrode current collector and / or a negative electrode current collector is attached to the ceramic electrode after the electrode restoration treatment.

4. The method for reusing a lithium ion secondary battery according to claim 2, wherein the electrode revival treatment includes heating the washed and dried ceramic electrode at 300 to 1000°C.

5. The method for reusing a lithium ion secondary battery according to claim 4, wherein the electrode revival treatment includes degreasing the ceramic electrode at 300 to 600 ° C. and / or firing the ceramic electrode at 650 to 1000 ° C.

6. 3. The method for recycling a lithium ion secondary battery according to claim 1, wherein the positive electrode is a ceramic positive electrode, and the ceramic positive electrode is made of a sintered lithium composite oxide.

7. 3. The method for reusing a lithium ion secondary battery according to claim 1, wherein the positive electrode is a ceramic positive electrode, the ceramic positive electrode is an oriented positive electrode that includes a plurality of primary particles composed of a lithium composite oxide, and the plurality of primary particles are oriented at an average orientation angle of more than 0° and not more than 30° with respect to a main surface of the positive electrode.

8. 7. The method for recycling a lithium ion secondary battery according to claim 6, wherein the lithium composite oxide is lithium cobalt oxide.

9. 3. The method for recycling a lithium ion secondary battery according to claim 1, wherein the negative electrode is a ceramic negative electrode, and the ceramic negative electrode is made of a titanium-containing sintered body.

10. The method for reusing a lithium ion secondary battery according to claim 9 , wherein the titanium-containing sintered body contains lithium titanate or niobium titanium composite oxide.

11. The separator is a ceramic separator, and the ceramic separator is made of MgO, Al 2 O 3 , ZrO 2 , SiC, Si 3 N 4 3. The method for recycling a lithium ion secondary battery according to claim 1 or 2, wherein the lithium ion secondary battery contains at least one selected from the group consisting of CrN, AlN, and cordierite.

12. 3. The method for reusing a lithium ion secondary battery according to claim 1, further comprising the step of replacing the electrolyte in the lithium ion secondary battery with fresh electrolyte.

13. 3. The method for reusing a lithium ion secondary battery according to claim 1, further comprising the step of replacing the battery container with another battery container after removing the ceramic electrode and before returning the ceramic electrode into the battery container.

14. 3. The method for reusing a lithium ion secondary battery according to claim 1 or 2, further comprising a step of replacing a positive electrode or a negative electrode other than the ceramic electrode that has been subjected to the electrode revival treatment with a new or equivalent positive electrode or negative electrode during or before assembling the lithium ion secondary battery.