Water-based dispersions and release films
An aqueous dispersion of acid-modified polyolefin resin and polyvinylpyrrolidone, combined with a crosslinking agent, addresses the issue of inconsistent mold releasability in release films by ensuring stable resin layer formation and adhesion, even under varying drying conditions.
Patent Information
- Application Number
- JP2020160430
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-27
- Filing Date
- 2020-09-25
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2040-09-25
AI Technical Summary
The existing release films formed with an aqueous dispersion containing acid-modified polyolefin resin and polyvinyl alcohol suffer from poor coating properties and may not achieve optimal mold releasability due to variations in drying temperature and time, leading to inconsistent resin layer formation.
An aqueous dispersion comprising acid-modified polyolefin resin, polyvinylpyrrolidone and/or its copolymer, and a crosslinking agent is used to form a resin layer on a base film, which maintains excellent mold release properties regardless of drying conditions.
The resulting resin layer exhibits superior coating properties, suppresses streak-like defects, and ensures stable adhesion to the base film, maintaining excellent mold releasability even with variations in drying conditions, thereby improving product yield and quality.
Smart Images

Figure 0007591252000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous dispersion and a release film. [Background technology]
[0002] Polyolefin resins are used in large quantities, mainly in the fields of automobiles and electrical appliances, packaging, daily necessities, etc., due to their excellent electrical properties, mechanical properties, chemical properties, recyclability, etc. Furthermore, polyolefin resins are also used as water-based paints after being acid-modified.
[0003] On the other hand, release films are widely used in the medical and industrial fields. For example, in the medical field, they are used as protective films for medical tapes and poultices, and in the industrial field, they are used as process materials for producing printed wiring boards, flexible printed wiring boards, multilayer printed wiring boards, etc., adhesive materials, protective materials for liquid crystal display parts, etc., and molding materials for sheet-like structures such as ion exchange membranes and ceramic green sheets. Patent Document 1 discloses a release film having a resin layer formed by applying an aqueous dispersion containing an acid-modified polyolefin resin, and having good releasability from various adherends. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2014 / 109340 Summary of the Invention [Problem to be solved by the invention]
[0005] The release film described in Patent Document 1 is one in which an aqueous dispersion containing an acid-modified polyolefin resin and polyvinyl alcohol is applied onto a substrate film to form a resin layer. However, the aqueous dispersion may not have good coatability, and the coating film of the aqueous dispersion applied onto the substrate film may not form a resin layer having good release properties depending on the conditions such as temperature and time in the drying process. In view of these problems, the object of the present invention is to provide an aqueous dispersion having good coatability, and to provide a release film that is not affected by the drying temperature or drying time in the resin layer formation process and can exhibit excellent releasability. [Means for solving the problem]
[0006] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that an aqueous dispersion containing an acid-modified polyolefin resin and polyvinylpyrrolidone has good coatability, and that a coating film obtained by applying this dispersion can form a resin layer having excellent release properties without being affected by drying temperature or drying time, thereby arriving at the present invention.
[0007] That is, the gist of the present invention is as follows. (1) an acid-modified polyolefin resin, polyvinylpyrrolidone and / or a copolymer thereof, A cross-linking agent; The present invention is characterized in that it contains an aqueous medium. For forming release layer Aqueous dispersion. (2) The weight average molecular weight of the polyvinylpyrrolidone and / or its copolymer according to (1) is 10,000 to 1,100,000. For forming release layer aqueous dispersion 。 (3 )moreover Polyvinyl alcohol (1) Or (2) Described in For forming release layer Aqueous dispersion. ( 4 ) on at least one side of the base film Demolding A release film having a layer thereon, DemoldingA release film, comprising a layer containing an acid-modified polyolefin resin, polyvinylpyrrolidone and / or a copolymer thereof, and a crosslinking agent. ( 5 ) Demolding The layer further contains polyvinyl alcohol ( 4 ) To The release film described herein. ( 6 ) characterized in that the haze is 5% or less ( 4 )or( 5 ) The release film described in the above. ( 7 ) The weight average molecular weight of polyvinylpyrrolidone and / or its copolymer is 10,000 to 1,100,000. 4 )~( 6 2. The release film according to claim 1 , 。 (8 )the above( 4) A method for producing the release film according to the present invention, comprising the steps of: For forming the release layer according to (1) A method for producing a release film, comprising the step of applying an aqueous dispersion. ( 9 )the above( 5 ) To A method for producing the release film according to the present invention, comprising the steps of: For forming the release layer described in (3) A method for producing a release film, comprising the step of applying an aqueous dispersion. Effect of the Invention
[0008] The aqueous dispersion of the present invention has good coatability, can suppress the occurrence of streak-like defects, and has excellent adhesion to a substrate film, and when it contains a crosslinking agent, it can form a resin layer having excellent releasability without being affected by the drying temperature or drying time in the resin layer formation process. Therefore, even if there is a change in the amount of heat in the process, the release film of the present invention is not affected by the change and can obtain excellent releasability, and the product production yield is not reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below. The aqueous dispersion of the present invention contains an acid-modified polyolefin resin, polyvinylpyrrolidone and / or a copolymer thereof, and an aqueous medium. The release film of the present invention has a resin layer provided on at least one surface of a base film, and the resin layer contains an acid-modified polyolefin resin, polyvinylpyrrolidone and / or a copolymer thereof, and a crosslinking agent.
[0010] <Aqueous dispersion> (Acid-modified polyolefin resin) The aqueous dispersion of the present invention and the resin layer of the release film of the present invention contain an acid-modified polyolefin resin. In the present invention, the acid-modified polyolefin resin is a resin containing an olefin component as a main component and modified with an acid-modifying component. Examples of the olefin component constituting the acid-modified polyolefin resin include ethylene, propylene, and butene. From the viewpoint of releasability of the release film from various adherends, it is preferable that the release film contains propylene. From the viewpoint of further improving releasability from various adherends, the content of propylene in the olefin component is preferably 50% by mass or more, more preferably 80% by mass or more, even more preferably 95% by mass or more, and particularly preferably 99% by mass or more. Furthermore, when transparency is required for the release film of the present invention, for example, when it is used as a protective film and the product is inspected while being attached to the product without being peeled off, or when it is used in a resist application requiring an exposure process, it is preferable that the olefin component of the acid-modified polyolefin resin does not contain butene from the viewpoint of reducing haze.
[0011] The acid-modified component constituting the acid-modified polyolefin resin includes unsaturated carboxylic acid components, specifically acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, crotonic acid, etc., as well as half esters and half amides of unsaturated dicarboxylic acids. Among them, in order to stably disperse the resin in the aqueous dispersion of the resin described later, acrylic acid, methacrylic acid, maleic acid, and maleic anhydride are preferred, and acrylic acid, methacrylic acid, and maleic anhydride are particularly preferred. Two or more of these acid-modified components may be contained in the acid-modified polyolefin resin.
[0012] The proportion of the acid-modified component in the acid-modified polyolefin resin is preferably from 1 to 10% by mass, and more preferably from 2 to 9% by mass. When the acid-modified component is less than 1%, the proportion of polar groups in the acid-modified polyolefin resin contained in the resin layer is small, so the resin layer tends not to have sufficient adhesion to the base film, and the release film may contaminate the adherend released from the resin layer. Furthermore, in the aqueous dispersion of the resin described below, it tends to be difficult to stably disperse the resin. On the other hand, when the proportion of the acid-modified component is more than 10% by mass, the proportion of polar groups is high, so the resin layer has sufficient adhesion to the base film, but the adhesion to the adherend also increases at the same time, so the releasability tends to decrease.
[0013] In addition, the acid-modified polyolefin resin may contain an ethylenically unsaturated component containing an oxygen atom in the side chain, so long as the effect of the present invention is not impaired. Examples of ethylenically unsaturated components containing oxygen atoms in the side chain include esters of (meth)acrylic acid and alcohols having 1 to 30 carbon atoms, and among these, from the viewpoint of availability, esters of (meth)acrylic acid and alcohols having 1 to 20 carbon atoms are preferred. Specific examples of such compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate. A mixture of these may be used. Among these, from the viewpoint of adhesion to the base film, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl acrylate, and octyl acrylate are more preferred, ethyl acrylate and butyl acrylate are even more preferred, and ethyl acrylate is particularly preferred. "(meth)acrylic acid" means "acrylic acid or methacrylic acid". If the amount of ethylenically unsaturated components containing oxygen atoms in the side chain is too large, the properties of the olefin-derived resin may be lost, and the releasability from the adherend may decrease. The proportion of ethylenically unsaturated components containing oxygen atoms in the side chain in the acid-modified polyolefin resin is preferably 40% by mass or less, more preferably 35% by mass or less, even more preferably 30% by mass or less, and particularly preferably 18% by mass or less. Even if an acid-modified polyolefin resin containing an ethylenically unsaturated component containing an oxygen atom in the side chain is used, the adhesion to the substrate film is not impaired.
[0014] The acid-modified polyolefin resin may be copolymerized with a small amount of other monomers, such as dienes, (meth)acrylonitrile, vinyl halides, vinylidene halides, carbon monoxide, and sulfur dioxide.
[0015] The components constituting the acid-modified polyolefin resin may be copolymerized in the acid-modified polyolefin resin in any form, and examples of the copolymerization state include random copolymerization, block copolymerization, and graft copolymerization (graft modification).
[0016] The melting point of the acid-modified polyolefin resin is preferably 80 to 200° C., more preferably 90 to 150° C. If the melting point exceeds 200° C., high-temperature treatment may be required when forming a resin layer on the surface of the substrate film. On the other hand, if the melting point is less than 80° C., the releasability of the resin layer tends to decrease.
[0017] (Polyvinylpyrrolidone and / or its copolymer) The aqueous dispersion of the present invention and the resin layer of the release film of the present invention must contain polyvinylpyrrolidone and / or its copolymer together with the acid-modified polyolefin resin. In the aqueous dispersion or resin layer, polyvinylpyrrolidone and / or its copolymer are dispersed in the acid-modified polyolefin resin, so that the aqueous dispersion has excellent coatability and can form a coating film in which the occurrence of streak-like defects described below is suppressed, and the formed coating film has excellent adhesion to the substrate film. In addition, the aqueous dispersion can form a resin layer that exhibits excellent releasability even when the amount of heat applied to the coating film in the coating film formation process changes.
[0018] The copolymer of polyvinylpyrrolidone may be any copolymer containing vinylpyrrolidone as the main component, and examples of copolymerization components other than vinylpyrrolidone include vinyl alcohol, vinyl acetal, vinyl acetate, styrene-based resin, quaternized dimethylaminoethyl methacrylate, alkylaminoacrylate, vinylcaprolactam, methacrylamide propyl trimethylammonium chloride, methacrylamide, and vinylimidazole. Examples of the copolymerization state include random copolymerization, block copolymerization, and graft copolymerization (graft modification). These may be used alone or in combination of two or more.
[0019] The content of polyvinylpyrrolidone and / or its copolymer is preferably 10 to 1000 parts by mass, more preferably 50 to 900 parts by mass, and even more preferably 50 to 600 parts by mass, relative to 100 parts by mass of the acid-modified polyolefin resin. If the content of polyvinylpyrrolidone and / or its copolymer exceeds 1000 parts by mass, the aqueous dispersion has a high viscosity, which tends to cause coating unevenness, and the resin layer tends to have a low adhesion to the substrate film and a low transparency. On the other hand, if the content of polyvinylpyrrolidone and / or its copolymer is less than 10 parts by mass, the aqueous dispersion has a low viscosity, which tends to cause coating unevenness, which tends to cause coating unevenness.
[0020] The weight-average molecular weight of polyvinylpyrrolidone and / or its copolymer is preferably 10,000 to 1,100,000, more preferably 30,000 to 1,000,000, and even more preferably 100,000 to 800,000. If the weight-average molecular weight of polyvinylpyrrolidone and / or its copolymer is less than 10,000, the resin layer tends to have poor releasability. On the other hand, if the weight-average molecular weight of polyvinylpyrrolidone and / or its copolymer exceeds 1,100,000, the aqueous dispersion has a high viscosity, which reduces the handling properties during the work process, reduces the coatability, and tends to cause streak-like defects, which will be described later, on the surface of the formed resin layer.
[0021] (Crosslinking agent) The aqueous dispersion of the present invention can contain a crosslinking agent, and when used to form a resin layer of a release film, it is necessary to contain a crosslinking agent. By containing the crosslinking agent, the components of the formed resin layer are crosslinked, the cohesive force is improved, and the releasability is improved.
[0022] The content of the crosslinking agent is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 2 to 10 parts by mass, relative to 100 parts by mass of the acid-modified polyolefin resin. If the content of the crosslinking agent is less than 1 part by mass, the cohesive force of the resin layer is likely to be weakened, and the adhesion to the substrate tends to decrease. On the other hand, if the content of the crosslinking agent exceeds 20 parts by mass, the releasability of the resin layer may be poor.
[0023] As the crosslinking agent, a compound having a plurality of functional groups in the molecule that react with a carboxyl group can be used, and examples thereof include polyfunctional epoxy compounds; polyfunctional isocyanate compounds; polyfunctional aziridine compounds; carbodiimide group-containing compounds; oxazoline group-containing compounds; phenolic resins; and amino resins such as urea compounds, melamine resins, and benzoguanamine resins. One of these may be used, or two or more may be used in combination. Among these, polyfunctional isocyanate compounds, melamine compounds, urea compounds, polyfunctional epoxy compounds, carbodiimide group-containing compounds, and oxazoline group-containing compounds are preferred, carbodiimide group-containing compounds and oxazoline group-containing compounds are more preferred, and oxazoline group-containing compounds are even more preferred. By using an oxazoline group-containing compound, it is possible to obtain a resin layer that has excellent adhesion to the substrate film. These crosslinking agents may also be used in combination.
[0024] Specifically, polyepoxy compounds, diepoxy compounds, etc. can be used as the polyfunctional epoxy compounds. For example, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, triglycidyl tris(2-hydroxyethyl)isocyanate, glycerol polyglycidyl ether, and trimethylolpropane polyglycidyl ether can be used as the polyepoxy compounds. For example, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, resorcinol diglycidyl ether, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and polytetramethylene glycol diglycidyl ether can be used as the diepoxy compounds.
[0025] Examples of polyfunctional isocyanate compounds that can be used include tolylene diisocyanate, diphenylmethane-4,4'-diisocyanate, metaxylylene diisocyanate, hexamethylene-1,6-diisocyanate, 1,6-diisocyanatehexane, an adduct of tolylene diisocyanate and hexanetriol, an adduct of tolylene diisocyanate and trimethylolpropane, polyol-modified diphenylmethane-4,4'-diisocyanate, carbodiimide-modified diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, 3,3'-bitrylene-4,4'-diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, and metaphenylene diisocyanate. Blocked isocyanate compounds in which these isocyanate groups are blocked with bisulfites and sulfonic acid group-containing phenols, alcohols, lactams, oximes, active methylene compounds, etc. may also be used. Commercially available polyfunctional isocyanate compounds include, for example, "Basonate HW-100" manufactured by BASF.
[0026] As the polyfunctional aziridine compound, for example, N,N'-hexamethylene-1,6-bis-(1-aziridinecarboxamide), trimethylolpropane-tri-β-aziridinylpropionate, etc. can be used.
[0027] The carbodiimide group-containing compound is not particularly limited as long as it has one or more carbodiimide groups in the molecule. The carbodiimide compound forms an ester with two carboxyl groups in the acid-modified portion of the acid-modified polyolefin resin at one carbodiimide portion to achieve crosslinking. For example, compounds having carbodiimide groups such as p-phenylene-bis(2,6-xylylcarbodiimide), tetramethylene-bis(t-butylcarbodiimide), and cyclohexane-1,4-bis(methylene-t-butylcarbodiimide), and polycarbodiimide, which is a polymer having a carbodiimide group, can be used. One or more of these can be used. Among these, polycarbodiimide is preferred because of its ease of handling. Commercially available polycarbodiimide products include the Carbodilite series manufactured by Nisshinbo Corporation, specifically water-soluble types "SV-02", "V-02", "V-02-L2", and "V-04"; emulsion types "E-01" and "E-02"; organic solution types "V-01", "V-03", "V-07", and "V-09"; and solvent-free type "V-05".
[0028] The oxazoline group-containing compound is not particularly limited as long as it has two or more oxazoline groups in the molecule. In the oxazoline compound, each of the two oxazoline moieties forms an amide ester with one carboxyl group in the acid-modified portion of the acid-modified polyolefin resin to achieve crosslinking. Such a polymer can be prepared by polymerization of an addition-polymerizable oxazoline group-containing monomer alone or with other monomers. Examples of the addition-polymerizable oxazoline group-containing monomer include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline. The addition-polymerizable oxazoline group-containing monomer can be one of these or a mixture of two or more of them. Among these, 2-isopropenyl-2-oxazoline is industrially easily available and is suitable.The other monomer is not limited as long as it is a monomer copolymerizable with the addition-polymerizable oxazoline group-containing monomer, and examples thereof include (meth)acrylic acid esters such as alkyl acrylate and alkyl methacrylate (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, styrenesulfonic acid, and salts thereof (sodium salt, potassium salt, ammonium salt, tertiary amine salt, and the like); unsaturated nitriles such as acrylonitrile and methacrylonitrile; acrylamide, methacrylamide, N-alkane, etc. Examples of the monomer include unsaturated amides such as alkyl acrylamide, N-alkyl methacrylamide, N,N-dialkyl acrylamide, and N,N-dialkyl methacrylate (the alkyl group is a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, a 2-ethylhexyl group, and a cyclohexyl group); vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether and ethyl vinyl ether; α-olefins such as ethylene and propylene; halogen-containing α,β-unsaturated aliphatic monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride; and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. As the other monomer, one or more of these monomers can be used. Among these, oxazoline group-containing polymers are preferred from the viewpoint of ease of handling. Commercially available oxazoline group-containing polymers include the Epocross series manufactured by Nippon Shokubai Co., Ltd., specifically water-soluble types "WS-500" and "WS-700"; emulsion types "K-1010E", "K-1020E", "K-1030E", "K-2010E", "K-2020E", and "K-2030E".
[0029] As the phenolic resin, for example, resol type phenolic resins and / or novolac type phenolic resins prepared using phenol, bisphenol A, alkylphenols such as pt-butylphenol, octylphenol, and p-cumylphenol, p-phenylphenol, cresol, and the like as raw materials can be used.
[0030] As the urea resin, for example, dimethylol urea, dimethylol ethylene urea, dimethylol propylene urea, tetramethylol acetylene urea, 4-methoxy 5-dimethyl propylene urea dimethylol can be used.
[0031] The melamine resin is, for example, a compound having an imino group, a methylol group, and / or an alkoxymethyl group (e.g., a methoxymethyl group, a butoxymethyl group) as a functional group in one molecule. As the melamine resin, imino group-type methylated melamine resin, methylol group-type methylated melamine resin, methylol group-type methylated melamine resin, fully alkylated methylated melamine resin, etc. can be used. Among them, methylolated melamine resin is most preferable. Furthermore, in order to promote the thermal curing of the melamine resin, it is preferable to use an acid catalyst such as p-toluenesulfonic acid.
[0032] As the benzoguanamine resin, for example, trimethylolbenzoguanamine, hexamethylolbenzoguanamine, trismethoxymethylbenzoguanamine, hexakismethoxymethylbenzoguanamine, etc. can be used.
[0033] (aqueous medium) The aqueous medium constituting the aqueous dispersion of the present invention means a solvent containing water and an amphipathic organic solvent and having a water content of 2% by mass or more, and may consist of water alone. An amphipathic organic solvent refers to an organic solvent in which the solubility of water in the organic solvent at 20°C is 5 mass% or more (the solubility of water in organic solvents at 20°C is described in literature such as "Solvent Handbook" (Kodansha Scientific, 10th edition, 1990)). Specific examples of amphipathic organic solvents include alcohols such as methanol, ethanol, n-propanol, and isopropanol; ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone and methyl ethyl ketone; esters such as methyl acetate, n-propyl acetate, isopropyl acetate, methyl propionate, ethyl propionate, and dimethyl carbonate; ethylene glycol derivatives such as ethylene glycol n-butyl ether; organic amine compounds containing ammonia such as diethylamine, triethylamine, diethanolamine, triethanolamine, N,N-dimethylethanolamine, and N,N-diethylethanolamine; and lactams such as 2-pyrrolidone and N-methyl-2-pyrrolidone.
[0034] (Method for producing aqueous dispersion) The aqueous dispersion of the present invention can be prepared, for example, by adding an aqueous solution of polyvinylpyrrolidone and, if necessary, a crosslinking agent, etc. to an aqueous dispersion of an acid-modified polyolefin resin, but is not limited to this method.
[0035] The method for aqueously dispersing the acid-modified polyolefin resin is not particularly limited, and examples thereof include the method described in WO 02 / 055598. The particle size of the acid-modified polyolefin resin dispersed in the aqueous medium is preferably 1 μm or less, more preferably 0.8 μm or less, in terms of stability when mixed with other components and storage stability after mixing. Such a particle size can be achieved by the manufacturing method described in International Publication No. 02 / 055598. The number average particle size of the acid-modified polyolefin resin is measured by dynamic light scattering. The solids concentration of the aqueous dispersion of the acid-modified polyolefin resin is not particularly limited, but in order to maintain the viscosity of the aqueous dispersion at an appropriate level, it is preferably from 1 to 60% by mass, and more preferably from 5 to 30% by mass.
[0036] The solids concentration in the aqueous dispersion containing an acid-modified polyolefin resin, polyvinylpyrrolidone, etc. can be appropriately selected depending on the coating conditions of the aqueous dispersion, the desired thickness and performance of the resin layer, etc., and is not particularly limited. In order to maintain an appropriate viscosity of the aqueous dispersion and form a uniform resin layer, however, the solids concentration is preferably 2 to 30 mass %, and more preferably 3 to 20 mass %. The aqueous dispersion may also contain additives such as antioxidants, ultraviolet absorbers, surfactants, and colorants, provided that the properties of the dispersion are not impaired.
[0037] <Release film> The release film of the present invention comprises a base film and a resin layer provided on at least one surface of the base film. (Base film) Examples of the base film constituting the release film of the present invention include polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), poly(1,4-cyclohexylene dimethylene terephthalate), and polylactic acid (PLA); polyolefin films such as polypropylene; polystyrene films; polyamide 6, poly-p-xylylene adipamide (MXD6 nylon), polyamide 66, polyamide 46, polyamide 4T, polyamide 6T, and polyamide 9T; polycarbonate films; polyacrylonitrile films; polyimide films; and laminates thereof (e.g., polyamide 6 / MXD6 nylon / polyamide 6, polyamide 6 / ethylene-vinyl alcohol copolymer / polyamide 6) or mixtures thereof. Polyester films and polyamide films having mechanical strength and dimensional stability are preferred.
[0038] The intrinsic viscosity of the resin constituting the base film is preferably 0.55 to 0.80, more preferably 0.60 to 0.75. If the intrinsic viscosity is less than the above range, the film is easily cut during film formation, making it difficult to produce stably, and the strength of the obtained film is low. On the other hand, if the intrinsic viscosity exceeds the above range, shear heat is generated during melt extrusion of the resin in the film production process, the load on the extruder is increased, the production speed has to be sacrificed, and it becomes difficult to control the thickness of the film, so that the productivity of the film decreases. In addition, the obtained film has an increased amount of thermal decomposition and gelation, and surface defects, foreign matter, and surface coarse protrusions. In addition, if the intrinsic viscosity is too high, the polymerization time and polymerization process are long, which is also a factor that increases costs.
[0039] The polymerization method of the resin constituting the base film is not particularly limited, and for example, in the case of polyester, examples include transesterification and direct polymerization. Examples of transesterification catalysts include compounds such as oxides and acetates of Mg, Mn, Zn, Ca, Li, Ti, etc. Examples of polycondensation catalysts include compounds such as oxides and acetates of Sb, Ti, Ge, etc. Since the polyester after polymerization contains monomers, oligomers, and by-products such as acetaldehyde, it may be subjected to solid-phase polymerization at a temperature of 200° C. or higher under reduced pressure or in an inert gas stream.
[0040] If necessary, additives such as antioxidants, heat stabilizers, ultraviolet absorbers, antistatic agents, pinning agents, etc. may be added to the base film. Examples of antioxidants include hindered phenol compounds and hindered amine compounds, examples of heat stabilizers include phosphorus compounds, etc., and examples of ultraviolet absorbers include benzophenone compounds and benzotriazole compounds.
[0041] Next, an example of a method for producing a base film will be described using a polyester film as a specific example. First, a sufficiently dried polyester is fed into an extruder, melted at a temperature at which it is sufficiently plasticized and exhibits fluidity, passed through a filter selected as necessary, and then extruded into a sheet through a T-die. This sheet is brought into close contact with a cooling drum whose temperature is adjusted to below the glass transition temperature (Tg) of the polyester, to obtain an unstretched film. The unstretched film thus obtained is uniaxially oriented by a uniaxial stretching method, or biaxially oriented by a biaxial stretching method. The biaxial stretching method is not particularly limited, but may be a sequential biaxial stretching method or a simultaneous biaxial stretching method.
[0042] In the uniaxial stretching method, an unstretched film is stretched in the longitudinal or transverse direction at a stretch ratio of about 2 to 6 times in the temperature range from the Tg of the resin to a temperature 50° C. higher than the Tg. In the simultaneous biaxial stretching method, an unstretched film is biaxially stretched to a stretch ratio of about 2 to 4 times in both the longitudinal and transverse directions in a temperature range of from the Tg of the resin to 50° C. higher than the Tg. Before being introduced into the simultaneous biaxial stretching machine, the unstretched film may be subjected to preliminary longitudinal stretching up to about 1.2 times. In the sequential biaxial stretching method, an unstretched film is heated with a heating roll or infrared rays and stretched in the longitudinal direction to obtain a longitudinally stretched film. The longitudinal stretching is preferably performed at a stretching ratio of 2.5 to 4.0 times in a temperature range of Tg to 40°C higher than Tg of the polyester by utilizing the peripheral speed difference between two or more rolls. The longitudinally stretched film is then continuously subjected to transverse stretching in the width direction, heat setting, and heat relaxation in sequence to obtain a biaxially oriented film. The transverse stretching is started at a temperature of Tg to 40°C higher than Tg of the resin, and the maximum temperature is preferably a temperature (100 to 40)°C lower than the melting point (Tm) of the resin. The transverse stretching ratio is adjusted depending on the required physical properties of the final film, but is preferably 3.5 times or more, further preferably 3.8 times or more, and more preferably 4.0 times or more. After stretching in the longitudinal direction and the width direction, the film can be further stretched again in the longitudinal direction and / or the width direction to increase the elastic modulus and dimensional stability of the film. Following the stretching, it is preferable to heat set the film for several seconds at a temperature (50-10)°C lower than the Tm of the resin, and simultaneously relax the film by 1-10% in the width direction. After the heat setting, the film is cooled to below Tg to obtain a biaxially stretched film.
[0043] Although a single-layer film can be obtained by the above-mentioned production method, the base film constituting the laminated film may be a multilayer film having two or more kinds of layers laminated thereto. The multilayer film can be produced by the above-mentioned production method, in which the resins constituting each layer are melted separately, extruded using a multilayer die, laminated and fused before solidification, and then biaxially stretched and heat-set, or by a method in which two or more resins are melted separately, extruded to form films, and laminated and fused in an unstretched state or after stretching, etc. From the viewpoint of process simplicity, it is preferable to use a multilayer die and laminate and fused before solidification.
[0044] (Resin layer) The resin layer constituting the release film of the present invention contains the above-mentioned acid-modified polyolefin resin, polyvinylpyrrolidone and / or its copolymer, and a crosslinking agent, and preferably further contains polyvinyl alcohol.
[0045] (Polyvinyl alcohol) In the release film of the present invention, the resin layer further contains polyvinyl alcohol, so that the transparency is improved and the haze of the release film can be reduced. By improving the transparency of the release film, for example, the release film attached to a product as a protective film can be inspected without peeling it off. In addition, the release film can be used without peeling it off even in resist applications that require an exposure process.
[0046] When the resin layer contains polyvinyl alcohol, the content is preferably 600 parts by mass or less per 100 parts by mass of the acid-modified polyolefin resin, from the viewpoint of maintaining releasability that is not affected by changes in heat quantity. In addition, from the viewpoints of releasability, residual adhesion rate of the adherend, and transparency, the content of polyvinyl alcohol is preferably 5 to 2000 parts by mass, and more preferably 15 to 700 parts by mass, per 100 parts by mass of polyvinylpyrrolidone and / or its copolymer.
[0047] (lubricant) In the present invention, the resin layer may contain a lubricant within a range that does not impair the effects of the present invention. Examples of the lubricant include inorganic particles such as calcium carbonate, magnesium carbonate, calcium oxide, zinc oxide, magnesium oxide, silicon oxide, sodium silicate, aluminum hydroxide, iron oxide, zirconium oxide, barium sulfate, titanium oxide, tin oxide, antimony trioxide, carbon black, and molybdenum disulfide, organic particles such as acrylic crosslinked polymers, styrene crosslinked polymers, silicone resins, fluororesins, phenolic resins, nylon resins, and polyethylene wax, and surfactants.
[0048] (Production method of release film) The release film of the present invention can be produced by a method including a step of applying an aqueous dispersion containing an acid-modified polyolefin resin, polyvinylpyrrolidone and / or its copolymer, a crosslinking agent, and an aqueous medium to at least one side of a substrate film. The release film can also be produced by adding polyvinyl alcohol to the aqueous dispersion.
[0049] In the present invention, the method for applying the above-mentioned aqueous dispersion to a substrate film may be a known method, such as gravure roll coating, reverse roll coating, wire bar coating, lip coating, air knife coating, curtain flow coating, spray coating, dip coating, brush coating, etc., and in the present invention, the gravure roll coating method is particularly effective.
[0050] In the present invention, the aqueous dispersion may be applied to the substrate film during the above-mentioned production process, or may be applied to the substrate film after the production process is completed and the film has been oriented and stretched. That is, in a method (in-line coating method) in which the aqueous dispersion is applied to a substrate film (unstretched film or uniaxially stretched film) during the manufacturing process, the film coated with the aqueous dispersion is dried, oriented and stretched, and heat-set. In a method (post-coating method) in which the aqueous dispersion is applied to a substrate film that has been oriented and stretched after the manufacturing process is completed, the film coated with the aqueous dispersion is dried.
[0051] In the in-line coating method, the resin layer can be formed in a state where the degree of oriented crystallization on the surface of the substrate film is small compared to the post-coating method, so that the adhesion between the substrate film and the resin layer is improved. In addition, since the resin layer can be heat-treated at a higher temperature while the film is in a tensed state, a resin layer having stable releasability can be formed without degrading the quality of the release film. In the in-line coating method, it is preferable from the viewpoint of simplicity and operation to adopt a sequential biaxial stretching method, coat the aqueous dispersion on the substrate film stretched in a uniaxial direction, dry the film coated with the aqueous dispersion, further stretch in a direction perpendicular to the direction, and heat-treat.
[0052] On the other hand, in the post-coating method, the applied aqueous dispersion may be dried at a relatively low temperature to prevent deterioration of the quality of the substrate film, and the formed resin layer may not exhibit sufficient releasability. However, since the aqueous dispersion of the present invention contains polyvinylpyrrolidone and / or its copolymer, it is possible to form a resin layer with excellent release properties without being affected by the drying temperature or drying time in the resin layer formation process, and it is possible to form a resin layer that exhibits excellent release properties even when used in a post-coating method in which a small amount of heat is applied to the coating film.
[0053] (Release film characteristics) The release film of the present invention has a peel strength between the acrylic adherend and the resin layer of preferably 0.01 to 3.5 N / cm, more preferably 0.01 to 2.5 N / cm, and even more preferably 0.01 to 2.0 N / cm, when the acrylic adherend as the adhesive material is attached to the resin layer and measured. By setting the peel strength between the acrylic adherend and the resin layer to 0.01 to 3.5 N / cm, the release film of the present invention can be practically used as a release film for acrylic adherends. Furthermore, since the release layer of the release film of the present invention has good adhesion to the base film, the acrylic adherend peeled from the resin has a high residual adhesion rate, and the residual adhesion rate of the acrylic adherend is preferably 70% or more, and more preferably 80% or more.
[0054] When the release film of the present invention is used as a protective film to inspect the product without peeling it off, or for resist applications that require an exposure process, it is preferable that the release film has transparency, and the haze is preferably 5% or less, more preferably 4% or less, and even more preferably 3% or less. As a method for making the haze of the release film 5% or less, for example, as described above, a method of using an acid-modified polyolefin resin of the resin layer that does not contain butene in the olefin component, or a method of making the aqueous dispersion used for in-line coating contain polyvinyl alcohol can be mentioned.
[0055] In the present invention, the thickness of the resin layer is preferably 0.01 to 1 μm, more preferably 0.03 to 0.7 μm, and even more preferably 0.05 to 0.5 μm. If the thickness of the resin layer is less than 0.01 μm or exceeds 1 μm, the state of the coating film formation tends to become unstable when the amount of heat applied to the coating film during coating film formation changes. In addition, it is not preferable for the resin layer thickness to exceed 1 μm because it increases costs.
[0056] Since the aqueous dispersion of the present invention has excellent coatability, the resin layer constituting the release film is suppressed from generating streaks and unevenness that can be recognized due to interference of light from a high-brightness light source, and has excellent appearance. That is, the release film of the present invention can have an average value of streak-like defects generated per 1 m of film width observed over the entire width of the film at a total of 10 points, including a point 1 m from one end edge in the longitudinal direction of the film, a point 1 m from the other end edge, and a point obtained by dividing the area between the two points into 9 equal parts, within 3 points, and preferably 0 points. Streak-like defects can be visually confirmed by applying white light (100 lumens) from a fluorescent lamp at an angle of 5 to 45° to the resin layer side surface of the release film.
[0057] The release film of the present invention can be suitably used for protective films for double-sided tapes or adhesive materials, protective materials or process materials when producing liquid crystal display components or printed wiring boards, and for forming sheet-like structures such as ion exchange membranes, ceramic green sheets, and heat dissipation sheets. EXAMPLES
[0058] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The properties of the release film were measured by the following methods.
[0059] (1) Mold releasability A 50 mm wide, 150 mm long acrylic adhesive tape (Nitto Denko No. 31B / acrylic adhesive) was pressed with a rubber roll onto the resin layer side of the release film to prepare a sample. The sample was sandwiched between metal plate / rubber plate / sample / rubber plate / metal plate and left for 20 hours under a load of 2 kPa in an atmosphere of 70°C, after which it was cooled for 30 minutes or more to return to room temperature to obtain a sample for measuring peel strength. The peel strength between the acrylic adhesive tape and the release film of the peel strength measurement sample was measured in a thermostatic chamber at 23° C. using a tensile tester (Shimadzu Corporation, Autograph AGS-100B) under the conditions of a peel angle of 180 degrees and a peel speed of 300 mm / min. For the resin layer not containing a crosslinking agent, the peel strength was measured only for the resin layer of Example 1.
[0060] (2)Residual adhesion rate In the above (1) mold releasability evaluation, an acrylic adhesive tape (manufactured by Nitto Denko Corporation, No. 31B / acrylic adhesive) with a width of 50 mm and a length of 150 mm peeled from the release film surface was attached to a stainless steel plate (SUS304, thickness 1 mm) and left at room temperature for 20 hours under a load of 2 kPa. Thereafter, the peel strength between the acrylic adhesive tape and the stainless steel plate was measured using a tensile tester (Shimadzu Corporation Autograph AGS-100B) in a thermostatic room at 23°C. The peel angle was 180 degrees and the peel speed was 300 mm / min. The peel strength obtained by this measurement was designated as F1. An acrylic adhesive tape (Nitto Denko No. 31B / acrylic adhesive) with a width of 50 mm and a length of 150 mm was attached to a stainless steel plate (SUS304, thickness 1 mm) and left at room temperature for 20 hours under a load of 2 kPa. The peel strength between the acrylic adhesive tape and the stainless steel plate was then measured (peel angle 180 degrees, peel speed 300 mm / min) using a tensile tester (Shimadzu Autograph AGS-100B) in a thermostatic room at 23°C, and the obtained peel strength was designated as F2. The residual adhesion rate of the adhesive tape was calculated using the following formula. Residual adhesion rate (%)=(F1 / F2)×100 If the surface of the adhesive layer of the adhesive tape is contaminated by the release film or if the surface of the adhesive tape becomes significantly rough when peeled off, the re-adhesiveness of the adhesive tape decreases and the performance as an adhesive tape is impaired. Therefore, a high residual adhesion rate is preferable.
[0061] (3) Coatability (suppression of streak-like defects in coating) The surface of the resin layer of the release film obtained by the post-coating method was irradiated with white light (100 lumens) from a fluorescent lamp at an angle of 5 to 45 degrees, and the presence or absence of streaky interference was visually confirmed. Coatability was evaluated according to the following criteria based on the occurrence of streaky defects over the entire width of the following 10 points. ○: No streak defects were observed at any point △: Can be confirmed at one to three locations ×: Streak-like defects can be seen in more than three locations The evaluation points were 10 points in total, including a point 1 m from one edge of the release film in the longitudinal direction, a point 1 m from the other edge, and 9 equal points between these two points. Straight lines were drawn in the width direction (TD) of the film at each point with a black oil-based pen, and streak-like defects intersecting the straight lines were observed across the entire width of the film.
[0062] (4) Adhesion between the base film and the resin layer The resin layer side surface of the release film obtained by the post-coating method was evaluated for adhesion between the base film and the resin layer by the cross-cut method in accordance with JIS K-5600-5-6. In detail, an adhesive tape (TF-12 manufactured by Nichiban Co., Ltd.) was applied to the resin layer surface on which a lattice pattern of 100 sections was formed by cutting, and the tape was vigorously peeled off. "100 / 100" indicates that none of the 100 sections peeled off, which is the best state, and "0 / 100" indicates that all of the 100 sections peeled off, which is the worst state. 100 / 100 to 90 / 100 is considered to be acceptable, with 100 / 100 to 95 / 100 being preferable, and 100 / 100 to 98 / 100 being more preferable.
[0063] (5) Haze of release film Based on JIS K 7136 (2000), the haze value of the release film was measured by irradiating light onto the surface of the resin layer of the release film using a turbidity meter "NDH-4000" manufactured by Nippon Denshoku Industries Co., Ltd.
[0064] The acid-modified polyolefin resin and its aqueous dispersion were produced by the following method. <Production of Acid-Modified Polyolefin Resin A-1> 280g of propylene-butene-ethylene terpolymer (propylene / butene / ethylene=68.0 / 16.0 / 16.0 (mass ratio)) was heated and melted in a four-neck flask under a nitrogen atmosphere, and then 32.0g of maleic anhydride as an unsaturated carboxylic acid and 6.0g of dicumyl peroxide as a radical generator were added over 1 hour while stirring while maintaining the temperature in the system at 170°C, and then reacted for 1 hour. After the reaction was completed, the obtained reaction product was poured into a large amount of acetone to precipitate a resin. This resin was further washed several times with acetone to remove unreacted maleic anhydride, and then dried under reduced pressure in a vacuum dryer to obtain an acid-modified polyolefin resin A-1.
[0065] <Production of Acid-Modified Polyolefin Resins A-2 and A-3> Acid-modified polyolefin resin A-2 was obtained in the same manner as in the production of the above acid-modified polyolefin resin A-1, except that the propylene-butene-ethylene terpolymer (propylene / butene / ethylene = 68.0 / 16.0 / 16.0 (mass ratio)) was changed to a propylene-ethylene copolymer (propylene / ethylene = 99 / 1 (mass ratio)). In addition, acid-modified polyolefin resin A-3 was obtained in the same manner, except that the ethylene-ethyl acrylate copolymer (ethylene / ethyl acrylate=93 / 7 (mass ratio)) was used.
[0066] <Production of Aqueous Dispersion of Acid-Modified Polyolefin Resin A-1> Using a stirrer equipped with a sealable pressure-resistant 1-liter glass container with a heater, 60.0 g of the acid-modified polyolefin resin A-1 produced by the above method, 45.0 g of ethylene glycol-n-butyl ether (boiling point 171 ° C), 6.9 g of N,N-dimethylethanolamine (boiling point 134 ° C, 1.0 times equivalent to the carboxyl group of the maleic anhydride unit in the resin), and 188.1 g of distilled water were charged into the above glass container, and the stirring blade rotation speed was set to 300 rpm and stirred. As a result, no precipitation of the resin was observed at the bottom of the container, and it was confirmed that the resin was in a floating state. Therefore, while maintaining this state, the heater was turned on after 10 minutes and heated. Then, the temperature inside the system was kept at 140 ° C and stirred for another 60 minutes. After that, the mixture was cooled to room temperature (about 25 ° C) by air cooling while stirring at a rotation speed of 300 rpm. Further, pressure filtration (air pressure 0.2 MPa) was performed using a 300 mesh stainless steel filter (wire diameter 0.035 mm, plain weave) to obtain a uniform aqueous dispersion of acid-modified polyolefin resin A-1 (solid content concentration 25% by mass). There was almost no residual resin on the filter.
[0067] <Production of Aqueous Dispersions of Acid-Modified Polyolefin Resins A-2 and A-3> Except for changing the acid-modified polyolefin resins used to A-2 and A-3, aqueous dispersions of acid-modified polyolefin resins A-2 and A-3 (solid content concentration 25% by mass) were obtained in the same manner as described above.
[0068] To prepare the aqueous dispersions, aqueous solutions of polymers of the following vinyl compounds were used: B-1: Polyvinylpyrrolidone, Pitzcol K-30L (weight average molecular weight 45,000) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. B-2: Polyvinylpyrrolidone, Pitzcol K-60L (weight average molecular weight 450,000) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. B-3: Polyvinylpyrrolidone, Pitzcol K-90L (weight average molecular weight 1,200,000) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. B-4: Polyvinyl alcohol-polyvinylpyrrolidone graft copolymer, Pitcol V-7154 manufactured by Daiichi Kogyo Seiyaku Co., Ltd. B-5: Polyvinyl alcohol, Poval JT-05 manufactured by Japan Vinyl Acetate & Poval Corporation B-6: Polyvinyl alcohol, Poval VC-10 manufactured by Nippon Vacuum Acetate & Poval Co., Ltd. B-7: Polyvinylamine, Mitsubishi Rayon PVAM0570B
[0069] The following crosslinking agents were used: C-1: Aqueous solution of an oxazoline group-containing compound, Epocross WS-700 manufactured by Nippon Shokubai Co., Ltd. C-2: Aqueous solution of a compound containing a carbodiimide group, Carbodilite V-02-L2 manufactured by Nisshinbo Chemical Co., Ltd. C-3: Aqueous solution of melamine compound, Beckamin APM manufactured by Dainippon Ink and Chemicals, Inc.
[0070] Example 1 <Preparation of Aqueous Dispersions X and Y> The acid-modified polyolefin resin aqueous dispersion "A-1" and the polyvinylpyrrolidone aqueous solution "B-2" were mixed so that the solid contents were 100 parts by mass and 300 parts by mass, respectively, and then pure water was added to obtain an aqueous dispersion X having a final solid content of 6.0 mass% and an aqueous dispersion Y having a final solid content of 2.7 mass%.
[0071] <Formation of resin layer (in-line coating method)> Polyethylene terephthalate (polymerization catalyst: antimony trioxide, intrinsic viscosity: 0.62, glass transition temperature: 78°C, melting point: 255°C) containing 0.12% by mass of amorphous silica particles with an average particle size of 2.3 μm was melt-extruded at 280°C, and then quenched in close contact with a casting drum using the T-die method and electrostatic pinning method to form an unstretched film with a thickness of 600 μm. This unstretched film was then stretched 3.5 times with a longitudinal stretching roll heated to 90°C. Aqueous Dispersion X was applied at a rate of 5 g / m2 to one side of the longitudinally stretched film using a reverse gravure coater. 2The film was stretched 4.5 times at 120°C in a transverse stretching tenter, then heat-treated at 230°C for 10 seconds, cooled, and wound up. The thickness of the obtained laminated film was 38 μm, and the thickness of the resin layer was approximately 0.08 μm.
[0072] <Formation of resin layer (post-coating method)> In the above in-line coating method, one side of the longitudinally stretched film was not coated with the aqueous dispersion X, and the film was stretched 4.5 times at 120°C in a transverse stretching tenter, heat-treated at 230°C for 10 seconds, cooled, and wound up to obtain a biaxially stretched film (thickness 38 μm, haze 3.0%). The aqueous dispersion Y was applied to the obtained biaxially stretched film using a Mayer bar, and then dried at 120° C. for 20 seconds to form a resin layer. The thickness of the resin layer was approximately 0.08 μm.
[0073] Examples 2 to 4, Comparative Example 1 In order to obtain the compositions shown in Table 1, an aqueous dispersion X having a final solid content of 6.0 mass% and an aqueous dispersion Y having a final solid content of 2.7 mass% were prepared, and in the same manner as in Example 1, a laminate film having a resin layer formed thereon was obtained by an in-line coating method using this aqueous dispersion X and by a post-coating method using the aqueous dispersion Y.
[0074] Example 5 <Preparation of Aqueous Dispersions X and Y> An acid-modified polyolefin resin aqueous dispersion "A-1", an aqueous polyvinylpyrrolidone solution "B-1", and an aqueous solution of an oxazoline compound as a crosslinking agent "C-1" were mixed so that the solid contents were 100 parts by mass, 300 parts by mass, and 7 parts by mass, respectively, and then pure water was added to obtain an aqueous dispersion X having a final solid content of 6.0% by mass and an aqueous dispersion Y having a final solid content of 2.7% by mass.
[0075] <Production of Release Film X (In-line Coating Method)> Polyethylene terephthalate (polymerization catalyst: antimony trioxide, intrinsic viscosity: 0.62, glass transition temperature: 78°C, melting point: 255°C) containing 0.12% by mass of amorphous silica particles with an average particle size of 2.3 μm was melt-extruded at 280°C, and then quenched in close contact with a casting drum using the T-die method and electrostatic pinning method to form an unstretched film with a thickness of 600 μm. This unstretched film was then stretched 3.5 times with a longitudinal stretching roll heated to 90°C. Aqueous Dispersion X was applied at a rate of 5 g / m2 to one side of the longitudinally stretched film using a reverse gravure coater. 2 The film was stretched 4.5 times at 120°C in a transverse stretching tenter, then heat-treated at 230°C for 10 seconds, cooled, and wound up. The thickness of the resulting release film was 38 μm, and the thickness of the resin layer was approximately 0.08 μm.
[0076] <Production of Release Film Y (Post Coating Method)> In the above in-line coating method, one side of the longitudinally stretched film was not coated with the aqueous dispersion X, and the film was stretched 4.5 times at 120°C in a transverse stretching tenter, heat-treated at 230°C for 10 seconds, cooled, and wound up to obtain a biaxially stretched film (thickness 38 μm, haze 3.0%). The above aqueous dispersion Y was applied to the obtained biaxially stretched film using a Mayer bar, and then dried at 120° C. for 20 seconds to obtain a release film with a resin layer thickness of approximately 0.08 μm.
[0077] Examples 6 to 22, Comparative Examples 2 to 6 In order to obtain the compositions shown in Table 1, an aqueous dispersion X having a final solid content of 6.0 mass% and an aqueous dispersion Y having a final solid content of 2.7 mass% were prepared, and in the same manner as in Example 5, the aqueous dispersion X was used to obtain a release film X by an in-line coating method, and the aqueous dispersion Y was used to obtain a release film Y by a post-coating method. In Example 14, a release film was also produced when a commercially available biaxially oriented polyester film was used as the base film. That is, the aqueous dispersion Y was applied to the corona-treated surface of a biaxially oriented polyester film (Unitika Co., Ltd., Emblet S-38, thickness 38 μm) by a post-coating method, and then dried at 120° C. for 20 seconds to form a resin layer, thereby obtaining a release film. The thickness of the resin layer was approximately 0.08 μm.
[0078] The results of various evaluations of the laminated films and release films obtained in the examples and comparative examples are shown in Table 1. Note that, for the release film produced by the post-coating method using a biaxially oriented polyester film (manufactured by Unitika Ltd., Emblet S-38, thickness 38 μm) as the base film in Example 14, the evaluation results of the peel force and cross-cut test are shown in parentheses.
[0079] [Table 1]
[0080] The aqueous dispersions of the examples contain an acid-modified polyolefin resin and polyvinylpyrrolidone and / or its copolymer, and therefore have excellent coatability, and the formed resin layer suppresses the occurrence of streak-like defects and has excellent adhesion to the substrate film. In addition, since the aqueous dispersions of the examples contain polyvinylpyrrolidone and / or its copolymer, even when these are used in a post-coating method that requires less heat during drying, the formed resin layer has a peel strength within a preferred range, and the peeled adherend has a residual adhesion rate within a preferred range. Since the aqueous dispersions of Examples 5 to 17 contained a crosslinking agent, the obtained resin layers had excellent release properties. In particular, the aqueous dispersions of Examples 5 to 6 and 10 to 11 had excellent coatability because the content and weight average molecular weight of polyvinylpyrrolidone and / or its copolymer were in a particularly preferred range. Furthermore, the obtained release layers had particularly excellent release properties that did not change with changes in the amount of heat during drying. In the aqueous dispersions of Examples 13 and 14, the olefin component of the acid-modified polyolefin resin did not contain butene, and therefore the obtained release films had reduced haze, which was within a preferable range. Since the aqueous dispersions of Examples 18 to 22 further contained polyvinyl alcohol, the obtained release films had lower haze, particularly in the in-line coated products, compared to the release film of Example 14, and had excellent visibility. Among them, the aqueous dispersions of Examples 19 to 21 contained 15 to 700 parts by mass of polyvinyl alcohol per 100 parts by mass of polyvinylpyrrolidone and / or its copolymer, and therefore the obtained release films had haze in the most preferable range, and the release properties did not change with the change in heat during drying, which was particularly excellent. The aqueous dispersions containing polyvinyl alcohol instead of polyvinylpyrrolidone and / or its copolymer in Comparative Examples 1 to 4 were inferior in coatability, and streak-like defects occurred in the formed resin layer. Furthermore, when used in the in-line coating method, a resin layer having releasability was formed, but when used in the post-coating method, which uses less heat during drying of the coating film, the formed resin layer had reduced releasability. The aqueous dispersion of Comparative Example 5 contained polyvinylamine instead of polyvinylpyrrolidone and / or its copolymer, and the aqueous dispersion of Comparative Example 6 did not contain an acid-modified polyolefin resin. Therefore, in both cases, the formed resin layer did not exhibit releasability, regardless of the amount of heat applied during drying of the coating film.
Claims
1. An aqueous dispersion for forming a release layer, comprising an acid-modified polyolefin resin, polyvinylpyrrolidone and / or a copolymer thereof, a crosslinking agent, and an aqueous medium.
2. 2. The aqueous dispersion for forming a release layer according to claim 1, wherein the weight average molecular weight of the polyvinylpyrrolidone and / or its copolymer is 10,000 to 1,100,000.
3. The aqueous dispersion for forming a release layer according to claim 1 or 2, further comprising polyvinyl alcohol.
4. A release film comprising a release layer provided on at least one surface of a base film, the release layer comprising an acid-modified polyolefin resin, polyvinylpyrrolidone and / or a copolymer thereof, and a crosslinking agent.
5. The release film as described in claim 4, characterized in that the release layer further contains polyvinyl alcohol.
6. 6. The release film according to claim 4, wherein the haze is 5% or less.
7. 7. The release film according to claim 4, wherein the weight average molecular weight of the polyvinylpyrrolidone and / or its copolymer is 10,000 to 1,100,000.
8. A method for producing the release film according to claim 4, comprising a step of applying the aqueous dispersion for forming a release layer according to claim 1 to at least one surface of a substrate film.
9. A method for producing the release film according to claim 5, comprising a step of applying the aqueous dispersion for forming a release layer according to claim 3 to at least one surface of a substrate film.
Citation Information
Patent Citations
Thermoplastic resin composition
JP2002003731A
Water vapor-permeating film
JP2004161891A
Method for producing fluorinated hydrocarbon
JP2017122069A
Aqueous dispersion
JP2019157066A
Mold release film and production method for same
WO2014109340A1