Glass sphere

A glass composition with increased potassium oxide content in a soda lime base addresses the mechanical strength and cost issues of conventional glass bulbs, providing high-strength, cost-effective blasting materials suitable for both wet and dry blasting.

JP7591259B2Active Publication Date: 2024-11-28UNITIKA GLASS BEADS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020214135
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-23
Publication Date
2024-11-28
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

Conventional blasting materials using glass bulbs, such as soda lime-based glass, suffer from poor mechanical strength and high cost, while those with high zirconia content are expensive. Borosilicate glass spheres offer excellent mechanical strength but are costly.

Method used

A glass composition with a soda lime composition containing 2% or more potassium oxide (K2O), 60-75% silicon dioxide (SiO2), 5-17% sodium oxide (Na2O), 5-15% calcium oxide (CaO), and 0-5% aluminum oxide (Al2O3) is developed, which is manufactured by increasing the potassium oxide content through contact with a molten salt containing potassium nitrate, resulting in glass spheres with enhanced mechanical strength.

Benefits of technology

The glass spheres exhibit high compressive strength, enabling their use as low-cost blasting materials with improved durability and suitability for both wet and dry blasting applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591259000001
    Figure 0007591259000001
  • Figure 0007591259000002
    Figure 0007591259000002
  • Figure 0007591259000003
    Figure 0007591259000003
Patent Text Reader

Abstract

To provide a glass ball having excellent mechanical strength, and a blast material including the glass ball.SOLUTION: A glass ball has a glass composition containing K2O of 2 mass% or more, SiO2 of 60-75 mass%, Na2O of 5-17 mass%, CaO of 5-15 mass%, and Al2O of 0-5 mass%. There is also provided a blast material including the glass ball.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to glass spheres having excellent mechanical strength, and to a blasting material using said glass spheres. [Background technology]

[0002] Conventionally, blasting materials using glass spheres have been used. For example, Patent Document 1 discloses an abrasive for sandblasting, which is used for forming partition walls and electrodes of flat panel displays by sandblasting, and is a ceramic powder and / or ceramic beads and / or glass beads containing 60% or more of zirconia having an average particle size of 5 μm to 50 μm. When sandblasting is performed under the same conditions as for forming partition walls and electrodes of flat panel displays, this abrasive can increase the processing speed and reduce wear of the abrasive, and stable processing can be performed.

[0003] However, the abrasive material for sandblasting in Patent Document 1 contains a large amount of zirconia, and has the problem of being expensive.

[0004] On the other hand, blasting media using glass materials available on the market are soda-lime-based glass, which is widely produced commercially. By manufacturing glass spheres using soda-lime-based glass, it is possible to provide blasting media in large quantities and at low cost. However, glass spheres with soda-lime-based glass have the disadvantage that they are inferior in mechanical strength and are easily consumed when used as blasting media. In addition, borosilicate glass spheres have excellent mechanical strength and can meet the required characteristics of blasting media, but have the disadvantage that they are expensive. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-50327 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide glass beads having excellent mechanical strength, and a blasting material using said glass beads. [Means for solving the problem]

[0007] The present inventors conducted extensive research to solve the above problems and found that glass spheres with a rich K2O content, which have a glass composition containing 2 mass% or more K2O, 60-75 mass% SiO2, 5-17 mass% Na2O, 5-15 mass% CaO, and 0-5 mass% Al2O3, have excellent mechanical strength and can be suitably used as a blasting material. The inventors also found that the glass spheres can be obtained by contacting glass spheres of a soda-lime composition with a KNO3 molten salt to make the K2O content 2 mass% or more. The present invention was completed based on these findings and through further research.

[0008] That is, the present invention provides the following aspects. Item 1. Glass spheres having a glass composition containing 2 mass% or more of K2O, 60 to 75 mass% of SiO2, 5 to 17 mass% of Na2O, 5 to 15 mass% of CaO, and 0 to 5 mass% of Al2O3. Item 2. The glass sphere according to item 1, containing 2 to 15 mass% K2O. Item 3. The glass beads according to item 1 or 2, wherein the weight ratio of K2O / Na2O is 0.2 to 2.5. Item 4. The glass spheres according to any one of Items 1 to 3, having an average particle size of 50 to 500 μm. Item 5. Compressive strength is 100kgf / mm 2 The glass sphere according to any one of items 1 to 4, which is as described above. Item 6. A blasting material comprising the glass spheres according to any one of items 1 to 5. Item 7. A method for producing glass spheres according to any one of items 1 to 5, A manufacturing method comprising the step of contacting glass spheres having a glass composition containing 0-1.5 mass% K2O, 60-75 mass% SiO2, 10-20 mass% Na2O, 5-15 mass% CaO, and 0-5 mass% Al2O3 with a molten salt containing potassium nitrate, thereby increasing the K2O content to 2 mass% or more. Effect of the Invention

[0009] The glass spheres of the present invention have high compressive strength and excellent mechanical strength, and can be suitably used as blasting materials. In addition, the glass spheres of the present invention can be produced from recycled glass of soda-lime composition as a raw material, and therefore can be supplied in large quantities at low cost. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The glass spheres of the present invention are characterized by having a glass composition containing 2 mass% or more of K2O, 60 to 75 mass% of SiO2, 5 to 17 mass% of Na2O, 5 to 15 mass% of CaO, and 0 to 5 mass% of Al2O3. The glass spheres of the present invention will be described in detail below.

[0011] [Glass composition] The glass composition of the glass spheres of the present invention is a specific soda lime-based composition with 2 mass% or more of K2O. While normal soda lime-based glass has a K2O content of 1.5 mass% or less, the glass spheres of the present invention have a soda lime-based composition with a high K2O content of 2 mass% or more, which makes it possible to provide them with excellent mechanical strength.

[0012] The term "soda-lime-based composition" in this specification includes not only a glass composition that corresponds to soda-lime glass (containing 70 to 73 mass% SiO2, 12 to 15 mass% Na2O, 7 to 12 mass% CaO, and 1 to 5 mass% MgO) specified in JIS Z 8901 "Test Powder 2 Instruction Manual," but also a glass composition containing SiO2, Na2O, and CaO as main components.

[0013] Specifically, the glass composition of the glass spheres of the present invention contains 2 mass% or more K2O, 60 to 75 mass% SiO2, 5 to 17 mass% Na2O, 5 to 15 mass% CaO, and 0 to 5 mass% Al2O3.

[0014] In the glass beads of the present invention, K2O is a component that plays a role in improving mechanical strength. The content of K2O in the glass beads of the present invention may be 2% by mass or more, but from the viewpoint of providing even better mechanical strength, it is preferably 2 to 15% by mass, preferably 2 to 12% by mass, more preferably 2 to 10% by mass, even more preferably 2 to 8.5% by mass, even more preferably 2 to 5% by mass, and even more preferably 2.5 to 3.5% by mass. The glass composition of the glass beads of the present invention has a higher content of K2O than conventional soda lime-based compositions, which is one of the reasons why it is possible to provide excellent mechanical strength.

[0015] In the glass beads of the present invention, SiO2 is a component that plays a role in forming a glass network structure. The SiO2 content in the glass beads of the present invention may be 60 to 75 mass%, preferably 65 to 73 mass%, more preferably 68 to 73 mass%. By making the SiO2 content fall within the above range, the glass beads can be provided with excellent mechanical strength while improving the moldability of the glass beads and the uniformity of the glass composition.

[0016] In the glass beads of the present invention, Na2O is a component that plays a role of enhancing melting property, etc. The Na2O content in the glass beads of the present invention may be 5 to 17 mass%, preferably 7 to 15 mass%, and more preferably 10 to 13 mass%. When the Na2O content satisfies the above range, the glass beads can be provided with excellent mechanical strength and excellent water resistance, and can be suitably used as a blasting material that can be used continuously in wet blasting, for example.

[0017] In the glass beads of the present invention, the weight ratio of K2O / Na2O may be within the range corresponding to the above-mentioned contents of K2O and Na2O, but from the viewpoint of providing even better mechanical strength, it is 0.1 to 2.5, preferably 0.1 to 0.5, and more preferably 0.15 to 0.3.

[0018] In the glass spheres of the present invention, CaO is a component that plays a role in increasing meltability and decreasing viscosity during melting. The CaO content in the glass spheres of the present invention may be 5 to 15 mass%, preferably 6 to 12 mass%, more preferably 7 to 10 mass%. By having the CaO content satisfy the above range, the glass spheres can have excellent mechanical strength and good shape uniformity.

[0019] The Al2O3 content in the glass beads of the present invention is 0 to 5 mass%. That is, the glass beads of the present invention may not contain Al2O3, and even if they contain Al2O3, the content is 5 mass% or less. The Al2O3 content in the glass beads of the present invention is preferably 0.5 to 3 mass%, more preferably 1 to 2 mass%.

[0020] The glass beads of the present invention may contain MgO. The MgO content in the glass beads of the present invention is, for example, 0 to 7 mass%, preferably 1 to 7 mass%, and more preferably 2 to 5 mass%.

[0021] Furthermore, in addition to the above components, the glass spheres of the present invention may contain components such as SO3, Fe2O3, F, Cl, B2O3, Li2O, ZnO, ZrO2, La2O3, WO3, Nb2O5, Y2O3, MoO3, TiO2, and As2O3. These components may be derived as unavoidable impurities from, for example, glass raw materials, glass composition manufacturing equipment, and glass composition molding equipment. In the glass spheres of the present invention, the content of each of these components is, for example, 0 to 1 mass%, preferably 0 to 0.5 mass%.

[0022] [Particle size] The average particle size of the glass spheres of the present invention is not particularly limited, but from the viewpoint of suitably providing the above-mentioned glass composition, it is 50 to 500 μm, preferably 50 to 300 μm, more preferably 50 to 200 μm, and even more preferably 50 to 150 μm.

[0023] In the present invention, the "average particle size of glass beads" is a value measured as follows: First, 30,000 or more glass beads are collected and passed through a JIS test sieve with an auxiliary dimension of 300 μm described in Table 2 of JIS K 8801-1:2019. If all the glass beads pass through the sieve, the average particle size is measured using the method (1) below. Otherwise, the average particle size is measured using the method (2) below.

[0024] Method (1) The average particle size of glass spheres is the volume-based median diameter (D) measured according to the method (Coulter counter method) in the "Method of measuring particle size distribution - Electrical detection zone method" specified in JIS Z 8832:2010. 50 )

[0025] Method (2) The particle size distribution is determined by measuring according to the manual dry sieving method described in the "Sieving test method for chemical products" specified in JIS K 0069:1992. Specifically, all sieves with the auxiliary dimension series described in Tables 1 and 2 of JIS K 8801-1:2019 are prepared as test sieves. 100.0 g of the measurement sample is weighed out using a balance that can measure up to 0.1 g. Sieving is continued until no sample passes through the test sieve. If the sample adheres to the bottom of the sieve, it is sieved down using a beating stick, and if the sample is clogged in the sieve, it is removed from the bottom of the sieve with a brush and the remaining sample is sieved up (residual). The largest test sieve used for sieving has an opening that allows the entire amount to pass through, and the smallest test sieve has an opening that does not allow the entire amount to pass through. Weigh out the residue on each test sieve using a balance capable of measuring to 0.1 g, and calculate the particle size distribution by calculating the percentage A of the mass of the residue on the sieve corresponding to each particle size range relative to the total weight (100.0 g). Round the figure to one decimal place.Here, each particle size range is in accordance with the above JIS K The range determined by the sieve of the auxiliary dimension series of apertures listed in Table 1 and Table 2 of 8801-1:2019, i.e., 125mm~106mm, 106mm~90mm, 90mm~75mm, 75mm~63mm, 63mm~53mm, 53mm~45mm, 45mm~37.5mm, 37.5mm~31.5mm, 31.5mm~26.5mm, 26.5mm~22.4mm, 22.4mm~19mm, 19~16mm, 16mm~13.2mm, 13.2mm~11.2mm, 11.2mm~9.5mm, 9.5mm~8mm, 8mm~6.7mm, 6.7mm~5.6mm, 5.6mm~4.75mm, 4.75mm~4mm, 4mm~3.35m m, 3.35mm~2.8mm, 2.8mm~2.36mm, 2.36mm~2mm, 2mm~1.7mm, 1.7mm~1.4mm, 1.4mm~1.18mm , 1.18mm~1mm, 1000μm~710μm, 710μm~600μm, 600μm~500μm, 500μm~425μm, 425μm~355μm, 3 55 μm to 300 μm, 300 μm to 250 μm, 250 μm to 212 μm, 212 μm to 180 μm, 180 μm to 150 μm, 150 μm to 125 μm, 125 μm to 106 μm, 106 μm to 90 μm, 90 μm to 75 μm, 75 μm to 63 μm, 63 μm to 53 μm, 53 μm to 45 μm, and 45 μm to 38 μm. Then, the sum of the maximum and minimum values ​​in each particle size range is divided by 2 (for example, in the case of a particle size range of 125 mm to 106 mm, (125,000 μm + 106,000 μm) / 2 = 115,500 μm), multiplied by the percentage A / 100 of the mass of the sieve residue corresponding to the particle size range calculated above with respect to the total amount (100.0 g), and the value obtained by integrating this for all particle size ranges is defined as the average particle size.

[0026] Furthermore, there are no particular limitations on the particle size distribution of the glass spheres of the present invention, but it is desirable that glass spheres with particle sizes within ±50% of the average particle size account for 70% or more of all glass spheres, preferably 80% or more, more preferably 90% or more, even more preferably 95% or more, and particularly preferably 100%.

[0027] [Physical properties] (Compressive strength) The glass spheres of the present invention are characterized by their high mechanical strength. In one embodiment of the glass spheres of the present invention, the compressive strength is 100 kgf / mm 2 More than 110kgf / mm 2 More preferably, 120kgf / mm 2 The upper limit of the compressive strength of the glass spheres of the present invention is not particularly limited, but is, for example, 200 kgf / mm 2 Less than 150kgf / mm 2 Less than or equal to 135kgf / mm 2 Less than or equal to 130kgf / mm 2 The following are included:

[0028] The compressive strength is a value measured by the following method.

[0029] The glass spheres to be measured are those selected under a microscope so that the particle size is within the range of the average particle size ±1%. The average cross-sectional area of ​​the glass spheres to be measured is calculated according to the following formula.

number

[0030] Next, the breaking strength of the glass spheres to be measured is measured in accordance with "Compression method B (displacement control in which the displacement is increased at a constant rate)" described in "Method for measuring breaking strength and deformation strength of microparticles" specified in JIS Z 8844:2019. Specifically, when the average particle diameter is 300 μm or less, a flat plate made of S45C-H material is placed as the lower jig on the measurement table of the tension compression tester, and a pressing jig (cylindrical with a diameter of 5 mm) made of SKH / hardened and tempered material is placed as the upper jig under the crosshead of the tension compression tester. The glass sphere is placed on the lower jig in line with the center of the upper jig, and a compression test is performed with the load range set to 100 N and the test speed set to 0.1 mm / min, and the load at which the glass sphere breaks is obtained as the breaking strength (kgf). The breaking strength is measured for 25 glass spheres, and the average value is calculated. The average value of the breaking strength is divided by the average cross-sectional area to obtain the compressive strength (kgf / mm 2 In addition, when the average particle size is more than 300 μm and 1000 μm or less, the compressive strength (kgf / mm ) is calculated under the same conditions as for glass spheres with an average particle size of 300 μm or less, except that a flat plate made of SKH / quenched and tempered material is used as the lower jig, and a pressing jig (cylindrical with a diameter of 20 mm) made of SKH / quenched and tempered material is used as the upper jig, and the load range is set to 2000 N and the test speed to 0.1 mm / min. 2 In addition, when the average particle size exceeds 1000μm, the compressive strength (kgf / mm2) is measured under the same conditions as for glass spheres with an average particle size of 300μm or less, except that a flat plate made of SKH / quenched and tempered material is used as the lower jig, and a pressing jig (cylindrical with a diameter of 20mm) made of SKH / quenched and tempered material is used as the upper jig, and the load range is set to 2000N and the test speed to 1mm / min. 2 ) is required.

[0031] (Elasticity Modulus) In one embodiment of the glass sphere of the present invention, the elastic modulus is 4700 N / mm 2 More than 4800N / mm 2 More preferably, 5000N / mm 2The upper limit of the elastic modulus of the glass sphere of the present invention is not particularly limited, but is, for example, 6500 N / mm 2 Less than 6000N / mm 2 Less than or equal to 5500N / mm 2 Less than or equal to 5300N / mm 2 The following are included:

[0032] The elastic modulus is a value obtained by the following method. From the measured data of the compressive strength, the elastic gradient (N / mm) was calculated by the linear least squares method from the displacement (mm) from the load from 0 kgf to the breaking strength and the breaking strength (kgf), and the elastic modulus (N / mm) was calculated according to the following formula: 2 ) is calculated.

number

[0033] (Vickers hardness) In addition, one embodiment of the glass spheres of the present invention has a Vickers hardness (HV) of 540 or more, preferably 580 or more, and more preferably 590 or more. The upper limit of the Vickers hardness (HV) of the glass spheres of the present invention is not particularly limited, but may be, for example, 700 or less, preferably 650 or less, more preferably 630 or less or 620 or less.

[0034] The Vickers hardness (HV) is a value measured by setting the test force to 25 gf and the test force holding time to 10 seconds according to the method described in "Vickers Hardness Test - Test Method" specified in JIS Z 2244:2009, and the specific measurement method is as follows. First, the glass spheres are selected under a microscope so that the particle diameter is within the range of the average particle diameter ±1% and are used as the measurement object. Next, adhesive is applied to a glass plate to a thickness that does not bury the glass sphere, and one glass sphere is placed on it and bonded. The glass plate with the glass sphere fixed is placed on the measurement table of the tester, and the test force is set to 25 gf and the test force holding time is set to 10 seconds, and the hardness of the center of the glass sphere is measured with a regular square pyramid diamond indenter. The Vickers hardness (HV) of 10 glass spheres is measured and the average value is calculated.

[0035] [Application] The use of the glass spheres of the present invention is not particularly limited, and examples thereof include blasting materials, spacers, fillers, etc., and a suitable example is blasting materials. When the glass spheres of the present invention are used as blasting materials, they can be applied to either wet blasting or dry blasting.

[0036] [Manufacturing method] The method for producing the glass spheres of the present invention is not particularly limited as long as it has the above-mentioned composition. A suitable example is a production method including a step of contacting glass spheres of a normal soda lime composition (i.e., a soda lime composition having a K2O content of 1.5 mass% or less) with a molten salt containing potassium nitrate to increase the K2O content to 2 mass% or more.

[0037] More specifically, the method for producing glass spheres of the present invention includes a process that includes a step of contacting glass spheres having a glass composition containing 0-1.5 mass% K2O, 60-75 mass% SiO2, 10-20 mass% Na2O, 5-15 mass% CaO, and 0-5 mass% Al2O3 (hereinafter sometimes referred to as "raw glass spheres") with a molten salt containing potassium nitrate to increase the K2O content to 2 mass% or more.

[0038] When the raw glass spheres come into contact with the molten salt containing potassium nitrate, some of the Na2O is replaced with K2O, so the glass composition of the raw glass spheres is as described in the [Glass composition] section above, except for the Na2O and K2O contents (i.e., the SiO2, CaO, and Al2O3 contents, and components that may be contained as necessary).

[0039] In the raw glass spheres, the Na2O content may be 10 to 20 mass %, preferably 10 to 17 mass %, and more preferably 12 to 15 mass %.

[0040] The content of K2O in the raw glass spheres is 0 to 1.5% by mass. That is, the glass composition of the raw glass spheres does not need to contain K2O, and even if K2O is contained, the content is 1.5% by mass or less. The content of K2O in the raw glass spheres is preferably 0 to 1.5% by mass, more preferably 0.5 to 1.5% by mass.

[0041] An example of the glass composition of the raw glass spheres is soda-lime glass (containing 70-73 mass% SiO2, 12-15 mass% Na2O, 7-12 mass% CaO, and 1-5 mass% MgO) specified in JIS Z 8901 "Test Powder 2 Instruction Manual."

[0042] In this manufacturing method, a part of Na2O is replaced with K2O by contact with the molten salt containing potassium nitrate, so if the particle size of the raw glass spheres is too large, it is difficult to increase the proportion of K2O in the entire glass sphere, and the K2O content tends to not reach 2 mass%. Therefore, it is desirable that the particle size of the raw glass spheres is small enough that the K2O content is easily increased to 2 mass% or more by contact with the molten salt containing potassium nitrate, and specifically, the average particle size is 50 to 500 μm, preferably 50 to 300 μm, more preferably 50 to 200 μm, and even more preferably 50 to 150 μm. In the present invention, the "average particle size of the raw glass spheres" is a value measured by the same method as the average particle size of the glass spheres of the present invention described above.

[0043] In addition, it is desirable that the particle size distribution of the raw glass spheres be such that glass spheres with particle diameters within ±50% of the average particle diameter account for at least 70% of the total glass spheres, preferably at least 80%, more preferably at least 90%, even more preferably at least 95%, and particularly preferably 100%.

[0044] The raw glass spheres can be produced by using raw materials satisfying the above glass composition by a method such as a levitation method, a droplet method, a marble formation method, a direct press method, a mold press method, a reheat press method, etc. A suitable example of a method for producing raw glass spheres is the levitation method disclosed in JP-A-11-199249.

[0045] The raw material for producing the raw glass spheres is not particularly limited as long as it has the above-mentioned glass composition, and may be a glass composition such as recycled glass or glass frit, or may be a raw material (for example, a melted mineral or oxide raw material) that is a source of SiO2, Na2O, Al2O3, CaO, etc. Among them, recycled glass of a soda-lime composition is available in large quantities at low cost, and is suitable as a raw material for producing the raw glass spheres.

[0046] Furthermore, commercially available glass spheres having the above glass composition can also be used as the raw glass spheres.

[0047] The raw glass spheres are preferably subjected to a heat treatment (pre-heating treatment) before contacting with the molten salt containing potassium nitrate. By carrying out the heat treatment, when the raw glass spheres are brought into contact with the molten salt, the raw glass spheres are subjected to a thermal shock due to the temperature difference between the raw glass spheres and the molten salt, and the surface of the raw glass spheres is prevented from cracking or breaking. The temperature condition of the heat treatment is, for example, 100°C or higher, preferably 100 to 500°C, more preferably 150 to 400°C, further preferably 340 to 500°C, and particularly preferably 380 to 460°C. The heat treatment time is, for example, 15 minutes or more, 30 to 120 minutes.

[0048] The molten salt containing potassium nitrate may be any salt that is used in the production of chemically strengthened glass, and the KNO content in the molten salt is, for example, 50 mass% or more, preferably 90 to 100 mass%, and more preferably 98 to 100 mass%.

[0049] In addition, the molten salt may contain inorganic salts such as K2CO3, Na2CO3, KHCO3, NaHCO3, K3PO4, Na3PO4, K2SO4, Na2SO4, KOH, and NaOH, in addition to KNO3, as necessary.

[0050] In order to bring the raw glass spheres into contact with the molten salt containing potassium nitrate, the raw glass spheres may be immersed in a tank containing the molten salt.

[0051] The temperature of the molten salt containing potassium nitrate when the raw glass spheres are brought into contact with the molten salt is, for example, 340 to 500°C, and preferably 380 to 460°C.

[0052] The time for which the raw glass spheres are brought into contact with the molten salt containing potassium nitrate may be set in a range in which the final KO content is 2 mass% or more depending on the composition and temperature of the molten salt, the particle size of the raw glass spheres, etc., and may be, for example, 1 hour or more, preferably 2 to 24 hours, and more preferably 3 to 12 hours.

[0053] Thus, by contacting the raw glass spheres with a molten salt containing potassium nitrate, a portion of the Na2O in the raw glass spheres is replaced with K2O, resulting in the glass spheres of the present invention having a K2O content of 2 mass% or more.

[0054] In the step of contacting the raw glass spheres with a molten salt containing potassium nitrate, the K2O increase relative to the raw glass spheres is, for example, 1 to 10 mass%, preferably 1.2 to 3.0 mass%, and more preferably 1.5 to 3.0 mass%. Here, the "K2O increase" refers to the value obtained by subtracting the K2O content of the raw glass spheres from the K2O content of the glass spheres obtained after contacting the raw glass spheres with a molten salt containing potassium nitrate.

[0055] The glass spheres after contact with the molten salt containing potassium nitrate may be cooled by standing to cool as necessary, and then subjected to a cleaning process to remove the molten salt adhering to the surface. The cleaning process may use pure water, ion-exchanged water, or the like as a cleaning liquid. From the viewpoint of cleaning efficiency, the temperature of the cleaning water during the cleaning process is preferably 70°C or higher. The cleaning process may be performed by a method of placing the glass spheres in a container containing cleaning water and stirring the mixture, a method of ultrasonic cleaning using cleaning water, or a combination of these methods. The glass spheres after the cleaning process may be dried as necessary. EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0057] Measurement method The methods for measuring the component contents, average particle diameters, compressive strengths, elastic moduli, and Vickers hardness (HV) of the glass spheres of Examples 1 to 5, Comparative Examples 1 to 10, and Reference Examples 1 to 6 are described below. The component contents and average particle diameters of the raw glass spheres A to H used as the manufacturing raw materials were also measured by the methods described below.

[0058] [Ingredient content] The glass spheres of Examples 1 to 5, Comparative Examples 1 to 10, and Reference Examples 1 to 6, the raw glass spheres A to H, and 5.0 g of the standard sample were crushed for 3 minutes in a crusher (TI-100, manufactured by CMT Corporation), and the crushed products were packed tightly into a 30 mm PVC ring for powder samples (manufactured by Rigaku Corporation, outer diameter 38 mm × inner diameter × height 5 mm) and pressure molded at 20 MPa to prepare a measurement sample. The sample was analyzed with a wavelength dispersive X-ray fluorescence analyzer (ZSX PrimusII, manufactured by Rigaku Corporation) to determine the component contents. The standard samples, glass spheres of Examples 1 to 5 and Comparative Examples 1 to 10 and raw glass spheres A to E, were valued according to the method of "analysis of soda-lime glass" specified in JIS R3101:1995, and the glass spheres of Reference Examples 1 to 6 and raw glass spheres F, G, and H were valued according to the method of "analysis of borosilicate glass" specified in JIS R3105:1995. Analysis using an X-ray fluorescence analyzer was performed in accordance with the quantitative analysis method specified in "General rules for X-ray fluorescence analysis" specified in JIS K0119:2008.

[0059] [Average particle size] The average particle diameters of the glass beads of Examples 1 to 5, Comparative Examples 1 and 2, Reference Examples 1 to 4, and the raw glass beads A, B, F, and G were measured according to the method described in "Method of Measuring Particle Size Distribution - Electrical Detection Zone Method" specified in JIS Z 8832: 2010. Specifically, 30,000 or more glass beads were collected, and the aperture diameter was set to 280 μm and the number of measurements was set to 20,000 using a Coulter counter (Multisizer 4 manufactured by BECKMAN COULTER). The volume-based median diameter (D 50 ) was measured.

[0060] The glass beads of Comparative Examples 3 to 10, Reference Examples 5 and 6, and raw glass beads C, D, E, and H were measured according to the manual sieving method of dry sieving described in the "Sieving test method for chemical products" specified in JIS K 0069:1992 to obtain the particle size distribution. Specifically, all sieves with the auxiliary dimension series described in Tables 1 and 2 of JIS K 8801-1:2019 were prepared as test sieves. 100.0 g of the measurement sample was weighed using a balance capable of measuring up to 0.1 g. The sieving was continued until no sample passed through the test sieve. If the sample adhered to the bottom of the sieve net, it was sieved under using a beating rod, and if it was clogged in the sieve net, it was removed from the bottom of the sieve net with a brush and sieved over (residual). The largest test sieve used for sieving has a mesh size that allows the entire amount to pass through, and the smallest test sieve has a mesh size that does not allow the entire amount to pass through. The residue on each test sieve was weighed using a balance that can measure to 0.1 g, and the percentage A of the mass of the sieve residue corresponding to each particle size range relative to the total amount (100.0 g) was calculated as the particle size distribution. The numbers were rounded to one decimal place.Here, each particle size range is in accordance with the above JIS K The range determined by the sieve of the auxiliary dimension series of apertures listed in Table 1 and Table 2 of 8801-1:2019, i.e., 125mm~106mm, 106mm~90mm, 90mm~75mm, 75mm~63mm, 63mm~53mm, 53mm~45mm, 45mm~37.5mm, 37.5mm~31.5mm, 31.5mm~26.5mm, 26.5mm~22.4mm, 22.4mm~19mm, 19~16mm, 16mm~13.2mm, 13.2mm~11.2mm, 11.2mm~9.5mm, 9.5mm~8mm, 8mm~6.7mm, 6.7mm~5.6mm, 5.6mm~4.75mm, 4.75mm~4mm, 4mm~3.35m m, 3.35mm~2.8mm, 2.8mm~2.36mm, 2.36mm~2mm, 2mm~1.7mm, 1.7mm~1.4mm, 1.4mm~1.18mm , 1.18mm~1mm, 1000μm~710μm, 710μm~600μm, 600μm~500μm, 500μm~425μm, 425μm~355μm, 3 55 μm to 300 μm, 300 μm to 250 μm, 250 μm to 212 μm, 212 μm to 180 μm, 180 μm to 150 μm, 150 μm to 125 μm, 125 μm to 106 μm, 106 μm to 90 μm, 90 μm to 75 μm, 75 μm to 63 μm, 63 μm to 53 μm, 53 μm to 45 μm, and 45 μm to 38 μm. The sum of the maximum and minimum values ​​in each particle size range was divided by 2 (for example, in the case of a particle size range of 125 mm to 106 mm, (125,000 μm + 106,000 μm) / 2 = 115,500 μm), and multiplied by the percentage A / 100 of the mass of the sieve residue corresponding to each particle size range relative to the total amount (100.0 g), and the value obtained by integrating this for all particle size ranges was defined as the average particle size.

[0061] [Compressive strength] The glass spheres used in the measurement of compressive strength were selected using a microscope. Specifically, the glass spheres used in the measurement of compressive strength were selected using a microscope so that the particle size was within the range of the average particle size ±1%.

[0062] The glass spheres of Examples 1 to 5, Comparative Examples 1 to 2, and Reference Examples 1 to 4 were measured for compressive strength by the following method. A flat plate made of S45C-H (Rockwell hardness 55, surface roughness Ra 0.16) was placed as the lower jig on the measurement table of a tension and compression tester (SDT-503NB-200R3, manufactured by Imada Seisakusho Co., Ltd.), and a pressing jig made of SKH / quenched and tempered (Rockwell hardness 60, cylindrical shape with a diameter of 5 mm) was placed as the upper jig under the crosshead of the tension and compression tester. The glass sphere was placed on the lower jig in alignment with the center of the upper jig, and a compression test was performed with a load range set to 100 N and a test speed set to 0.1 mm / min, and the load at which the glass sphere broke was calculated as the breaking strength (kgf). The breaking strength was measured for 25 pieces of glass, and the average value was calculated. The average value of the breaking strength was divided by the average cross-sectional area calculated from the average particle diameter to obtain the compressive strength (kgf / mm 2 ) was sought.

[0063] For the glass spheres of Comparative Examples 3 to 10 and Reference Examples 5 to 6, the compressive strength (kgf / mm) was measured under the same conditions as above, except that a flat plate (Rockwell hardness 60) made of SKH / quenched and tempered material was used as the lower jig, and a pressing jig (Rockwell hardness 60, cylindrical shape with a diameter of 20 mm) made of SKH / quenched and tempered material was used as the upper jig, and the load range was set to 2000 N and the test speed was set to 1 mm / min. 2 ) was sought.

[0064] Elasticity Modulus From the measured data of the compressive strength, the elastic gradient (N / mm) was calculated by the linear least squares method from the displacement (mm) from the load from 0 kgf to the maximum load and the breaking strength (kgf), and the elastic modulus (N / mm) was calculated according to the following formula: 2 ) was calculated.

number

[0065] [Vickers hardness (HV)] The glass spheres used for the Vickers hardness (HV) measurement were selected using a microscope. Specifically, the glass spheres used for the Vickers hardness (HV) measurement were selected using a microscope so that the particle size was within the range of the average particle size ±1%.

[0066] Vickers hardness (HV) was measured according to the method described in "Vickers hardness test-test method" specified in JIS Z 2244:2009, using a micro Vickers hardness tester (Future Tech Co., Ltd. product name FM-ARS9000), with a test force of 25 gf and a test force holding time of 10 seconds. Specifically, first, a glass plate made of soda lime glass was coated with an instant adhesive (Tough DXF, Cemedine Co., Ltd.) using a bar coater (number No. 80) to a thickness that did not bury the glass ball, and one glass ball was placed on it and bonded to fix it. Next, the glass plate with the glass ball fixed was placed on the measuring table of the tester, and the test force was set to 25 gf and the test force holding time was set to 10 seconds, and the hardness of the center of the glass ball was measured using a regular pyramidal diamond indenter (code No. M-013, for HV). The Vickers hardness (HV) of 10 glass spheres was measured and the average value was calculated.

[0067] Test Example 1 1. Manufacturing of glass spheres [Example 1] Recycled glass with a soda-lime composition was crushed and sieved, and the fine glass powder was blown together with air into a heat forming zone in a gas burner frame to produce glass spheres. The resulting glass spheres were sieved to obtain raw glass spheres (hereinafter referred to as raw glass spheres A) with particle sizes in the range of 90 to 125 μm and an average particle size of 107 μm. The results of analyzing the composition of raw glass spheres A are shown in Table 1.

[0068] [Table 1]

[0069] 10 kg of potassium nitrate (Otsuka Chemical Co., Ltd., Super Tablet, melting point 333°C, potassium nitrate content 99.0 or more) was added to a cylindrical container made of SUS316 (thickness 3 mm, inner diameter 200 mm, internal height 500 mm). The container containing the potassium nitrate was placed in a chemical strengthening furnace (Kyoei Denki Co., Ltd., Ecohot-M size), and the atmospheric temperature in the chemical strengthening furnace was set to 380°C and heated for 8 hours to prepare potassium nitrate molten salt.

[0070] Next, the raw glass spheres A were heat-treated (preheated) in an electric furnace (GME Tanaka Corporation, 200V, 1φ, 10KW) at an atmospheric temperature of 380° C. for 60 minutes.

[0071] 30 g of the heat-treated raw glass spheres A were placed in a container (10 mm x 80 mm x 110 mm) made of a SUS304 mesh with a mesh size of 62 μm, and the container containing the raw glass spheres A was immersed in molten potassium nitrate at 380°C for 6 hours to carry out ion exchange. The temperature of the molten potassium nitrate was measured by inserting a thermocouple (K sheath thermocouple, manufactured by Motoyama Co., Ltd.) in the molten potassium nitrate. The container was then removed from the molten potassium nitrate, and the glass spheres were allowed to cool.

[0072] 2L of purified water and a stirrer were placed in a glass beaker, and the mixture was stirred while being heated with a hot stirrer (Pasolina Hot Stirrer CT-5HA, manufactured by AS ONE Corporation). The container removed from the potassium nitrate molten salt was washed at 70°C for 40 minutes. The glass spheres were transferred to another glass beaker, 300mL of purified water was added, and the container was washed at 28kHz for 10 minutes using an ultrasonic cleaner (VSF-100, manufactured by AS ONE Corporation). The purified water in the glass beaker was discarded, 300ml of fresh purified water was added, and ultrasonic cleaning was performed again under the same conditions. Next, the purified water was discarded, and the glass spheres were collected by suction filtration, and then dried at 110°C for 2 hours using a constant temperature incubator (DK-43, manufactured by Yamato Scientific Co., Ltd.) to obtain glass spheres.

[0073] [Example 2] Glass spheres were produced under the same conditions as in Example 1, except that the temperature of the potassium nitrate molten salt and the atmospheric temperature of the preliminary heat treatment were changed to 400°C.

[0074] [Example 3] Glass spheres were produced under the same conditions as in Example 1, except that the temperature of the potassium nitrate molten salt and the atmospheric temperature of the preliminary heating treatment were changed to 460°C.

[0075] [Example 4] Recycled glass with a soda-lime composition was crushed and sieved, and the fine glass powder was blown together with air into a heat forming zone in a gas burner frame to produce glass spheres. The resulting glass spheres were sieved to obtain raw glass spheres (hereinafter referred to as raw glass spheres B) with particle sizes in the range of 212-300 μm and an average particle size of 250 μm. The results of analyzing the composition of raw glass spheres B are shown below. 2 As shown in.

[0076] [Table 2]

[0077] Under the same conditions as in Example 2, the preparation of molten potassium nitrate, the heat treatment of the raw glass spheres (preliminary heating treatment), the immersion of the heat-treated raw glass spheres in the molten potassium nitrate, washing, and drying were carried out to obtain glass spheres.

[0078] [Example 5] Glass spheres were produced under the same conditions as in Example 4, except that the atmospheric temperature in the preliminary heating treatment was changed to 460°C, and the temperature of the potassium nitrate molten salt was changed to 460°C.

[0079] [Comparative Example 1] Raw glass spheres A (glass spheres that had not been subjected to heat treatment or immersion in a molten potassium nitrate salt) used in the production of the glass spheres in Example 1 were prepared.

[0080] [Comparative Example 2] Raw glass spheres B (glass spheres that had not been subjected to heat treatment or immersion in a molten potassium nitrate salt) used in the production of the glass spheres in Example 4 were prepared.

[0081] [Comparative Example 3] Recycled glass with a soda-lime composition was crushed and sieved, and the resulting glass fine powder was fed into a rotating SUS pipe heated to above the softening point of the glass to produce raw glass spheres. The resulting glass spheres were sieved to obtain raw glass spheres (hereinafter referred to as raw glass spheres C) with particle sizes of 850 to 1250 μm and an average particle size of 1000 μm. The results of analyzing the composition of raw glass spheres C are shown in Table 3.

[0082] [Table 3]

[0083] Molten potassium nitrate was prepared under the same conditions as in Example 1, and the raw glass spheres C were heat-treated (preheated). Next, the heat-treated raw glass spheres C were immersed in molten potassium nitrate under the same conditions as in Example 1, except that a container (10 mm x 80 mm x 110 mm) made of a SUS304 mesh with a mesh size of 283 μm was used as the container for immersing the heat-treated raw glass spheres C in the molten potassium nitrate. After that, washing and drying were performed under the same conditions as in Example 1 to obtain glass spheres.

[0084] [Comparative Example 4] Glass spheres were produced under the same conditions as in Comparative Example 3, except that the temperature of the potassium nitrate molten salt was changed to 400°C and the atmospheric temperature of the preliminary heating treatment was changed to 460°C.

[0085] [Comparative Example 5] Glass spheres were produced under the same conditions as in Comparative Example 3, except that the temperature of the potassium nitrate molten salt was changed to 440°C and the atmospheric temperature of the preliminary heating treatment was changed to 460°C.

[0086] [Comparative Example 6] Raw glass spheres C (glass spheres that had not been subjected to heat treatment or immersion in a molten potassium nitrate salt) used in the production of the glass spheres of Comparative Example 3 were prepared.

[0087] [Comparative Example 7] Recycled glass with a soda-lime composition was crushed and sieved, and the resulting glass fine powder was fed into a rotating SUS pipe heated to above the softening point of the glass to produce raw glass spheres. The resulting glass spheres were sieved to obtain raw glass spheres (hereinafter referred to as raw glass spheres D) with particle sizes of 1700 to 2360 μm and an average particle size of 2091 μm. The results of analyzing the composition of raw glass spheres D are shown in Table 4.

[0088] [Table 4]

[0089] Under the same conditions as in Example 2, the preparation of molten potassium nitrate, the heat treatment of the raw glass spheres (preliminary heating treatment), the immersion of the heat-treated raw glass spheres in the molten potassium nitrate, washing, and drying were carried out to obtain glass spheres.

[0090] [Comparative Example 8] Raw glass spheres D (glass spheres that had not been subjected to heat treatment or immersion in a molten potassium nitrate salt) used in the production of the glass spheres of Comparative Example 7 were prepared.

[0091] [Comparative Example 9] Recycled glass with a soda-lime composition was crushed and sieved, and the resulting glass fine powder was fed into a rotating SUS pipe heated to above the softening point of the glass to produce raw glass spheres. The resulting glass spheres were sieved to obtain raw glass spheres (hereinafter referred to as raw glass spheres E) with particle sizes of 2800 to 4000 μm and an average particle size of 3172 μm. The results of analyzing the composition of raw glass spheres E are shown in Table 5.

[0092] [Table 5]

[0093] Under the same conditions as in Example 2, the preparation of molten potassium nitrate, the heat treatment of the raw glass spheres (preliminary heating treatment), the immersion of the heat-treated raw glass spheres in the molten potassium nitrate, washing, and drying were carried out to obtain glass spheres.

[0094] [Comparative Example 10] Raw glass spheres E (glass spheres that had not been subjected to heat treatment or immersion in a molten potassium nitrate salt) used in the production of the glass spheres of Comparative Example 9 were prepared.

[0095] 2. Evaluation results of glass spheres The evaluation results of each glass sphere of Examples 1 to 5 are shown in Table 6, and the evaluation results of each glass sphere of Comparative Examples 1 to 10 are shown in Table 7. The glass spheres obtained by contacting raw glass spheres of soda lime composition with an average particle size of 100 μm and raw glass spheres of soda lime composition with an average particle size of 250 μm with potassium nitrate molten salt had a K2O content of 2 mass% or more, and had improved compressive strength, elastic modulus, and Vickers hardness (HV) compared to the glass spheres not contacted with potassium nitrate molten salt. In addition, the glass spheres obtained by contacting raw glass spheres of soda lime composition with an average particle size of 1000 μm, 2091 μm, and 3172 μm with potassium nitrate molten salt did not have a K2O content of 2 mass% or more, and had insufficient compressive strength. In the production of glass spheres in Examples 1 to 5 and Comparative Examples 3 to 5, 7 and 9, there was almost no change in the average particle size and particle size distribution between the raw glass spheres before contact with the molten potassium nitrate and the glass spheres after contact with the molten potassium nitrate. In addition, in all of the glass spheres in Examples 1 to 5 and Comparative Examples 1 to 10, glass spheres with particle sizes within ±50% of the average particle size accounted for 100% of the total glass spheres.

[0096] From the above results, it became clear that glass spheres having a soda-lime-based composition with a K2O content of 2 mass% or more have excellent mechanical strength.

[0097] [Table 6]

[0098] [Table 7]

[0099] Reference test example 1 1. Manufacturing of glass spheres [Reference example 1] Glass raw material with borosilicate glass composition was crushed and sieved, and the fine glass powder was blown together with air into the heat forming zone in the frame of a gas burner to produce glass spheres. The obtained glass spheres were sieved to obtain raw glass spheres (hereinafter referred to as raw glass spheres F) with an average particle size of 107 μm and 80 mass % or more of glass spheres with a particle size of 90 to 125 μm. The results of analyzing the composition of raw glass spheres F are shown in Table 8.

[0100] [Table 8]

[0101] Raw glass spheres F were used and subjected to heat treatment, contact with molten potassium nitrate, and washing under the same conditions as in Example 2 to obtain glass spheres.

[0102] [Reference example 2] Raw glass spheres F (glass spheres that had not been subjected to heat treatment or immersion in a molten potassium nitrate salt) used in the production of the glass spheres of Reference Example 1 were prepared.

[0103] 2. Evaluation results of glass spheres The evaluation results of each glass sphere of Reference Examples 1 and 2 are shown in Table 9. As a result, in the glass spheres of borosilicate composition containing almost no Na2O, there was almost no change in compressive strength, elastic modulus, and Vickers hardness (HV) even when they were brought into contact with molten potassium nitrate.

[0104] [Table 9]

[0105] Reference test example 2 1. Manufacturing of glass spheres [Reference example 3] The recycled glass with borosilicate composition was crushed and sieved, and the glass fine powder was blown together with air into the heat forming zone in the frame of a gas burner to produce glass spheres. The obtained glass spheres were sieved to obtain raw glass spheres (hereinafter referred to as raw glass spheres G) with particle sizes in the range of 90 to 125 μm and an average particle size of 106 μm. The results of analyzing the composition of raw glass spheres G are shown in Table 10.

[0106] [Table 10]

[0107] Under the same conditions as in Example 2, the preparation of molten potassium nitrate, the heat treatment of the raw glass spheres (preliminary heating treatment), the immersion of the heat-treated raw glass spheres in the molten potassium nitrate, washing, and drying were carried out to obtain glass spheres.

[0108] [Reference example 4] Raw glass spheres G (glass spheres that had not been subjected to heat treatment or immersion in a molten potassium nitrate salt) used in the production of the glass spheres of Reference Example 3 were prepared.

[0109] [Reference example 5] The recycled glass with borosilicate composition was crushed and sieved, and the obtained glass fine powder was fed into a rotating SUS pipe heated to above the softening point of the glass to produce raw glass spheres. The obtained glass spheres were sieved to obtain raw glass spheres (hereinafter referred to as raw glass spheres H) with particle sizes of 850 to 1180 μm and an average particle size of 1028 μm. The results of analyzing the composition of raw glass spheres H are shown in Table 11.

[0110] [Table 11]

[0111] Under the same conditions as in Example 2, the preparation of molten potassium nitrate, the heat treatment of the raw glass spheres (preliminary heating treatment), the immersion of the heat-treated raw glass spheres in the molten potassium nitrate, washing, and drying were carried out to obtain glass spheres.

[0112] [Reference example 6] Raw glass spheres H (glass spheres that had not been subjected to heat treatment or immersion in a molten potassium nitrate salt) used in the production of the glass spheres of Reference Example 5 were prepared.

[0113] 2. Evaluation results of glass spheres The evaluation results of each of the glass spheres of Reference Examples 3 to 6 are shown in Table 12.

[0114] [Table 12]

Claims

1. K 2 O is 2 mass% or more, SiO 2 65 to 75 mass% of Na 2 O is 5 to 17 mass%, CaO is 5 to 15 mass%, Al 2 A glass sphere having a glass composition containing 0 to 2 mass % of O3 and 0 to 0.5 mass % of B2O3, Glass spheres having an average particle size of 50 to 300 μm.

2. K 2 The glass sphere according to claim 1, containing 2 to 15 mass % O.

3. K 2 O / Na 2 The glass sphere according to claim 1 or 2, wherein the weight ratio of O is 0.1 to 2.

5.

4. Compressive strength is 100 kgf / mm 2 The glass sphere according to any one of claims 1 to 3.

5. A blasting material comprising the glass spheres according to any one of claims 1 to 4.

6. A method for producing glass spheres according to any one of claims 1 to 4, K 2 O 0 to 1.5 mass %, SiO 2 65 to 75 mass% of Na 2 O is 10 to 20 mass%, CaO is 5 to 15 mass%, Al 2 The glass spheres having a glass composition containing 0 to 2 mass % of O3 and 0 to 0.5 mass % of B2O3 are brought into contact with a molten salt containing potassium nitrate, thereby obtaining a glass composition containing potassium nitrate. 2 The method includes a step of adjusting the O content to 2 mass% or more.

Citation Information

Patent Citations

  • Tempered glass bead

    JP1985122734A

  • Manufacture of glassy beads

    JP1986295241A

  • Novel bioactive glasses and their uses

    JP1998512227A

  • Abrasive for sand blasting, treatment method for sand blasting chip and partition wall formation method

    JP2004050327A

  • Tempered glass spacer

    JP2013508250A