Dielectric and Ceramic Electronic Components

A perovskite-based dielectric material with a +2 valence Eu proportion of 21% or more, combined with specific atomic concentration ratios, addresses reliability issues in ceramic components by improving lifespan and reliability under high electric field loads.

JP7591411B2Active Publication Date: 2024-11-28TAIYO YUDEN KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021003742
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-13
Publication Date
2024-11-28
Estimated Expiration
2041-01-13

Smart Images

  • Figure 0007591411000003
    Figure 0007591411000003
  • Figure 0007591411000004
    Figure 0007591411000004
  • Figure 0007591411000005
    Figure 0007591411000005
Patent Text Reader

Abstract

To provide a dielectric, a ceramic electronic component, a manufacturing method of the dielectric, and a manufacturing method of the ceramic electronic component that can improve reliability.SOLUTION: A dielectric contains, as a main phase, perovskite containing at least Ba in the A site and at least Ti in the B site, and contains Eu, and the proportion of +2 valences of Eu is 21% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to Dielectric and Ceramic Electronic Components Regarding. [Background technology]

[0002] In high-frequency communication products, such as mobile phones, ceramic electronic components such as multilayer ceramic capacitors are used to eliminate noise. In such products, there is a demand for smaller (thinner) and larger-capacity ceramic electronic components. There is also a demand for highly reliable ceramic electronic components with high rated voltages, such as in-vehicle components. In order to meet these needs, a highly reliable dielectric material is required that can ensure reliability even when the electric field load applied to one dielectric layer increases. Therefore, a technology for adding rare earth elements to perovskite has been disclosed (see, for example, Patent Document 1). The effects of Eu as a rare earth element have been disclosed (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] WO 2008 / 105240 [Patent Document 2] JP 2016-169130 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, due to the increased load on the dielectric, the reliability improved by these methods is becoming insufficient, and there is a demand for means for further improving reliability.

[0005] The present invention has been made in consideration of the above problems, and is capable of improving reliability. Dielectric and Ceramic Electronic Components The purpose is to provide. [Means for solving the problem]

[0006] The dielectric material according to the present invention is characterized in that it contains, as a main phase, a perovskite containing at least Ba in the A site and at least Ti in the B site, and contains Eu, the proportion of the +2 valence of the Eu being 21% or more.

[0007] In the dielectric, the proportion of Eu with a valence of +2 may be 80% or less.

[0008] In the perovskite of the dielectric, the atomic concentration ratio of the A site / the B site may be 0.980 or less.

[0009] In the perovskite of the dielectric, the atomic concentration ratio of the A site / the B site may be 0.920 or more.

[0010] In the dielectric, the atomic concentration ratio of Eu / B site may be 0.001 or more.

[0011] In the dielectric, the atomic concentration ratio of Eu / B site may be 0.100 or less.

[0012] A ceramic electronic component according to the present invention is characterized in that it has a laminated structure in which a plurality of dielectric layers made of any one of the above dielectric materials and a plurality of internal electrode layers are alternately laminated.

[0013] The method for producing a dielectric material according to the present invention includes a firing step of firing a dielectric material in which Eu is added to a powder of perovskite containing at least Ba in the A site and at least Ti in the B site, and an annealing step of annealing at a temperature and at a lower oxygen partial pressure than those in the firing step, and is characterized in that the conditions of the annealing step are adjusted so that the proportion of the +2 valence of Eu is 21% or more.

[0014] The method for producing a ceramic electronic component according to the present invention includes a firing step of firing a laminate formed by stacking a sheet of a dielectric material in which Eu has been added to powder of perovskite containing at least Ba in the A site and at least Ti in the B site, and a pattern of a metal conductive paste, and an annealing step of annealing the laminate at a lower temperature and at a lower oxygen partial pressure than those in the firing step, and is characterized in that the conditions of the annealing step are adjusted so that the proportion of the +2 valence of Eu is 21% or more. Effect of the Invention

[0015] According to the present invention, it is possible to provide a ceramic electronic component and a dielectric material that can improve reliability. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a partial cross-sectional perspective view of a multilayer ceramic capacitor. [Diagram 2] 2 is a cross-sectional view taken along line AA in FIG. 1. [Diagram 3] FIG. 2 is a cross-sectional view taken along line BB in FIG. [Figure 4] 1A to 1C are diagrams illustrating a flow of a method for manufacturing a multilayer ceramic capacitor. [Diagram 5] 1 is a XANES spectrum near the L3 absorption edge of Eu for Example 2. [Figure 6] 13 is a XANES spectrum near the Eu L3 absorption edge for Example 5. [Figure 7] FIG. 1 is a graph showing the relationship between the +2 valence rate of Eu and the lifetime. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment will be described with reference to the drawings.

[0018] (Embodiment) FIG. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to an embodiment. FIG. 2 is a cross-sectional view taken along line AA in FIG. 1. FIG. 3 is a cross-sectional view taken along line BB in FIG. 1. As illustrated in FIGS. 1 to 3, the multilayer ceramic capacitor 100 includes a laminated chip 10 having a substantially rectangular parallelepiped shape, and external electrodes 20a, 20b provided on any two opposing end faces of the laminated chip 10. Of the four faces of the laminated chip 10 other than the two end faces, the two faces other than the top and bottom faces in the stacking direction are referred to as side faces. The external electrodes 20a, 20b extend on the top, bottom and two side faces in the stacking direction of the laminated chip 10. However, the external electrodes 20a, 20b are spaced apart from each other.

[0019] The laminated chip 10 has a configuration in which dielectric layers 11 containing a ceramic material that functions as a dielectric and internal electrode layers 12 containing a base metal material are alternately laminated. The edges of the internal electrode layers 12 are alternately exposed to the end face on which the external electrode 20a of the laminated chip 10 is provided and the end face on which the external electrode 20b is provided. As a result, each internal electrode layer 12 is alternately conductive to the external electrode 20a and the external electrode 20b. As a result, the laminated ceramic capacitor 100 has a configuration in which a plurality of dielectric layers 11 are laminated via the internal electrode layers 12. In addition, in the laminate of the dielectric layers 11 and the internal electrode layers 12, the internal electrode layers 12 are arranged on the outermost layer in the lamination direction, and the upper and lower surfaces of the laminate are covered by the cover layer 13. The cover layer 13 is mainly composed of a ceramic material. For example, the material of the cover layer 13 is the same as that of the dielectric layers 11 and the ceramic material.

[0020] The size of the multilayer ceramic capacitor 100 is, for example, 0.25 mm in length, 0.125 mm in width, and 0.125 mm in height, or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 3.2 mm in length, 1.6 mm in width, and 1.6 mm in height, or 4.5 mm in length, 3.2 mm in width, and 2.5 mm in height, but is not limited to these sizes.

[0021] The internal electrode layers 12 are mainly composed of base metals such as Ni (nickel), Cu (copper), Sn (tin), etc. The internal electrode layers 12 may be made of precious metals such as Pt (platinum), Pd (palladium), Ag (silver), Au (gold), etc., or alloys containing these metals.

[0022] The dielectric layer 11 has a main phase made of a ceramic material having a perovskite structure represented by the general formula ABO3. 3-α In this embodiment, the ceramic material contains at least Ba (barium) in the A site and at least Ti (titanium) in the B site. The B site may contain Zr (zirconium).

[0023] 2, a region where the internal electrode layer 12 connected to the external electrode 20a and the internal electrode layer 12 connected to the external electrode 20b face each other is a region that generates capacitance in the multilayer ceramic capacitor 100. Therefore, the region that generates capacitance is referred to as a capacitance region 14. In other words, the capacitance region 14 is a region where adjacent internal electrode layers 12 connected to different external electrodes face each other.

[0024] The region where the internal electrode layers 12 connected to the external electrode 20a face each other without an internal electrode layer 12 connected to the external electrode 20b being interposed therebetween is referred to as the end margin 15. The region where the internal electrode layers 12 connected to the external electrode 20b face each other without an internal electrode layer 12 connected to the external electrode 20a being interposed therebetween is also the end margin 15. In other words, the end margin 15 is a region where the internal electrode layers 12 connected to the same external electrode face each other without an internal electrode layer 12 connected to a different external electrode being interposed therebetween. The end margin 15 is a region that does not generate capacitance.

[0025] 3, in the laminated chip 10, the regions extending from the two side surfaces of the laminated chip 10 to the internal electrode layers 12 are referred to as side margins 16. That is, the side margins 16 are regions provided to cover the ends of the multiple internal electrode layers 12 stacked in the above-mentioned laminated structure that extend to the two side surfaces. The side margins 16 are also regions that do not generate electrical capacitance.

[0026] In order to improve the reliability of the dielectric layer 11, it is conceivable to add a rare earth element to the dielectric layer 11. However, rare earth elements such as Ho (holmium), Dy (dysprosium), and Y (yttrium) tend to dissolve more in the B site than in the A site. When a rare earth element dissolves more in the B site, it becomes an acceptor excess, which introduces oxygen defects that cause deterioration of the life due to the electrically neutral condition, and therefore the effect of improving the life is limited.

[0027] Therefore, the inventors investigated rare earth elements having a large ionic radius that are likely to form a solid solution by substitution at the A site of BaTiO3, and found that by adding Eu (europium), the high temperature load life of the dielectric layer 11 is improved by about one order of magnitude compared to rare earth elements such as Ho, Dy, and Y.

[0028] Rare earth elements usually have a valence of +3. Eu may also be used as a +3 rare earth to modify perovskite. However, Eu has a feature not found in other rare earth elements in that it may have a stable valence of +2 other than +3. As a result of intensive research, the present inventors have found that the high temperature load life of the dielectric layer 11 is dramatically improved by increasing the +2 valence of Eu. The reason why +2 valence Eu brings about a large life improvement effect is not yet clear, but +2 valence Eu ions have the largest ion size among rare earth elements that are solid-dissolved in the A site, so it is possible that they greatly distort the perovskite lattice and reduce the energy (activation energy) required for the movement of oxygen defects, which are considered to be the main cause of life deterioration. In fact, the same life improvement effect was not obtained using the method of the present invention with rare earth elements other than Eu that cannot have a stable valence of +2.

[0029] Table 1 shows the ionic radius of each rare earth element with six coordinations. The source of Table 1 is "RD Shannon, Acta Crystallogr., A32, 751 (1976)". [Table 1]

[0030] Through intensive research by the present inventors, it has been found that when 21% or more of the Eu added to the dielectric layer 11 has a valence of +2, the life and reliability of the dielectric layer 11 are improved. This is believed to be because a large amount of Eu can be dissolved in the A site.

[0031] From the viewpoint of further improving the reliability of the dielectric layer 11, the ratio of Eu having a valence of +2 (+2 valence rate) to the Eu added to the dielectric layer 11 is preferably 21% or more, and more preferably 26% or more.

[0032] In order to increase the +2 valence rate of Eu, it is required to reduce many +3 valence Eu. However, during the period in which many +3 valence Eu are reduced in the annealing process for reducing to +2 valence Eu, grain growth may occur in the dielectric layer 11. If grain growth occurs, the life of the dielectric layer 11 may be reduced. Therefore, if grain growth occurs in the dielectric layer 11, the life reduction effect due to grain growth may offset the life improvement effect of the Eu valence, and the grain growth may cause the internal electrode layer 12 to lose its structure, resulting in a short circuit. Therefore, it is preferable to set an upper limit on the +2 valence rate of Eu. For example, in the dielectric layer 11, the +2 valence rate of Eu is preferably 80% or less, more preferably 70% or less, and even more preferably 59% or less.

[0033] In addition, when the A site is deficient in the perovskite constituting the main phase of the dielectric layer 11, sufficient vacancies are formed in the A site, and Eu with a valence of +2, which has a large ionic radius, is easily dissolved in the A site. Therefore, it is preferable that the A site is deficient. For example, in the perovskite constituting the main phase of the dielectric layer 11, the atomic concentration ratio of the A site / B site is preferably 0.980 or less, more preferably 0.970 or less, and even more preferably 0.960 or less. In addition, if the A site element is only Ba and the B site element is only Ti, the atomic concentration ratio of the A site / B site is the atomic concentration ratio of Ba / Ti. If the A site element is only Ba and the B site element is only Ti and Zr, the atomic concentration ratio of the A site / B site is the atomic concentration ratio of Ba / (Ti+Zr).

[0034] If the atomic concentration ratio of the A site / B site is too low, the tetragonality decreases, and the dielectric constant of the dielectric layer 11 may decrease. Therefore, it is preferable to set a lower limit for the atomic concentration ratio of the A site / B site. For example, in the perovskite constituting the main phase of the dielectric layer 11, the atomic concentration ratio of the A site / B site is preferably 0.920 or more, more preferably 0.940 or more, and even more preferably 0.950 or more.

[0035] The perovskite constituting the main phase of the dielectric layer 11 can obtain an effect of maintaining insulation by including Zr in the B site. From the viewpoint of obtaining the effect sufficiently, it is preferable to set a lower limit to the Zr / Ti ratio (atomic concentration ratio). For example, the Zr / Ti ratio is preferably 0.01 or more, more preferably 0.02 or more, and further preferably 0.04 or more.

[0036] When Zr is contained in the B site of the perovskite constituting the main phase of the dielectric layer 11, if the amount of Zr is too large, grain growth occurs during firing of the dielectric layer 11, and the life may not be achieved. Therefore, it is preferable to set an upper limit to the Zr / Ti ratio. For example, the Zr / Ti ratio is preferably 0.14 or less, more preferably 0.10 or less, and even more preferably 0.08 or less.

[0037] If the amount of Eu added in the dielectric layer 11 is too small, a sufficient life may not be obtained. Therefore, it is preferable to set a lower limit on the amount of Eu added. For example, in the dielectric layer 11, the atomic concentration ratio of Eu / B site, which is the ratio of the amount of Eu to the amount of B-site elements, is preferably 0.001 or more, more preferably 0.005 or more, and even more preferably 0.010 or more. If the B-site element is only Ti, the atomic concentration ratio of Eu / B site is the atomic concentration ratio of Eu / Ti. If the B-site element is only Ti and Zr, the atomic concentration ratio of Eu / B site is the atomic concentration ratio of Eu / (Ti+Zr).

[0038] If the amount of Eu added to the dielectric layer 11 is too large, the insulating properties may be reduced, and a sufficient life may not be obtained. Therefore, it is preferable to set an upper limit on the amount of Eu added. For example, in the dielectric layer 11, the atomic concentration ratio of Eu / B site is preferably 0.100 or less, more preferably 0.060 or less, and even more preferably 0.040 or less.

[0039] If the amount of rare earth elements other than Eu added to the dielectric layer 11 is too large, the effect of improving the lifespan by Eu is weakened, and there is a risk that a sufficient lifespan cannot be obtained. Therefore, it is preferable to set an upper limit on the amount of rare earth elements other than Eu added. Specifically, it is preferable to make the amount of rare earth elements other than Eu added less than the amount of Eu added. When there are multiple types of rare earth elements other than Eu, it is preferable to make the total amount of the multiple types of rare earth elements added less than the amount of Eu added.

[0040] Next, a description will be given of a method for manufacturing the multilayer ceramic capacitor 100. FIG.

[0041] (Raw powder production process) First, a dielectric material for forming the dielectric layer 11 is prepared. The A-site elements and B-site elements contained in the dielectric layer 11 are usually contained in the dielectric layer 11 in the form of a sintered body of ABO3 particles. For example, BaTiO3 is a tetragonal compound having a perovskite structure and exhibits a high dielectric constant. This BaTiO3 can generally be obtained by synthesizing barium titanate by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate. Various methods have been known so far as a method for synthesizing the main component ceramic of the dielectric layer 11, such as a solid-phase method, a sol-gel method, a hydrothermal method, and the like. In this embodiment, any of these methods can be adopted.

[0042] To the obtained ceramic powder, a predetermined additive compound is added according to the purpose. The additive compound may be oxides of Zr (zirconium), Mg (magnesium), Mn (manganese), V (vanadium), Cr (chromium), Eu (europium), and oxides or glasses of Co (cobalt), Ni (nickel), Li (lithium), B (boron), Na (sodium), K (potassium), and Si (silicon). If necessary, oxides of rare earth elements other than Eu (Sc (scandium), Y (yttrium), La (lanthanum), Ce (cerium), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (lutetium)) may be added.

[0043] For example, a compound containing an additive compound is wet-mixed with a ceramic raw material powder, and then dried and pulverized to prepare a ceramic material. For example, the ceramic material obtained as described above may be pulverized as necessary to adjust the particle size, or may be combined with a classification process to adjust the particle size. Through the above steps, a dielectric material is obtained.

[0044] (Lamination process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained dielectric material and wet mixed. The obtained slurry is used to coat a strip-shaped dielectric green sheet, for example, 0.5 μm or more thick, on a substrate by, for example, a die coater method or a doctor blade method, and then dried.

[0045] Next, a metal conductive paste for forming an internal electrode containing an organic binder is printed on the surface of the dielectric green sheet by screen printing, gravure printing, or the like to arrange an internal electrode layer pattern that is alternately drawn to a pair of external electrodes with different polarities. Ceramic particles are added to the metal conductive paste as a co-material. The main component of the ceramic particles is not particularly limited, but is preferably the same as the main component ceramic of the dielectric layer 11. For example, BaTiO3 with an average particle size of 50 nm or less may be uniformly dispersed.

[0046] Thereafter, the dielectric green sheet on which the internal electrode layer pattern is printed is punched out to a predetermined size, and the punched dielectric green sheet is laminated by a predetermined number of layers (for example, 100 to 1000 layers) with the base material peeled off so that the internal electrode layers 12 and the dielectric layers 11 are alternately arranged, and the edges of the internal electrode layers 12 are alternately exposed at both end faces in the length direction of the dielectric layers 11 and alternately drawn out to a pair of external electrodes 20a, 20b with different polarities. Cover sheets for forming the cover layer 13 are pressure-bonded to the top and bottom of the laminated dielectric green sheets, and the laminated dielectric green sheets are cut to a predetermined chip size (for example, 1.0 mm x 0.5 mm).

[0047] (Firing process) The ceramic laminate thus obtained was subjected to a binder removal treatment in an N2 atmosphere, after which a metal paste that would become the undercoat layers of the external electrodes 20a and 20b was applied thereto by a dipping method. -12 MPa~10 -9 The mixture is fired in a reducing atmosphere at 1160°C to 1280°C under reduced pressure of MPa for 5 to 10 minutes.

[0048] (Annealing process) After that, the temperature is changed to a lower temperature and a stronger reducing atmosphere than that of the firing process, and annealing is performed. -14 MPa~10 -13 Annealing is performed for 1 to 2 hours in a strong reducing atmosphere at 1100° C. to 1150° C. under a pressure of 200 MPa. The holding temperature in the annealing step is preferably about 50° C. lower than the maximum temperature in the firing step.

[0049] By performing the annealing step in a more strongly reducing atmosphere than the firing step, it is possible to reduce +3 Eu to +2 Eu. The conditions of the annealing step should be adjusted so that the +2 valence rate of Eu is 21% or more.

[0050] In principle, Eu can be reduced by setting the firing process to a strong reducing atmosphere like the annealing process. However, in this case, there is a risk that barium titanate, which is the main phase of the dielectric layer 11, is reduced, generating a large amount of oxygen defects and electrons. Since oxygen defects are the main factor that reduces the life of the dielectric layer 11, they actually reduce the reliability. In fact, if the atmosphere is set to sufficiently make Eu +2, the barium titanate itself is strongly reduced and becomes an n-type semiconductor. In addition, if it is held at high temperature for a long time in a strong reducing atmosphere, the barium titanate grains grow, causing the internal electrode layer 12 to break, and it is not negligible that this leads to a decrease in capacity. For this reason, although it is possible to achieve both the reduction resistance of barium titanate and Eu reduction by strictly designing the conditions for high-temperature firing and precisely controlling the atmosphere in the furnace, it is difficult to make it a general-purpose process suitable for mass production of multilayer ceramic capacitors. Therefore, although there is no particular restriction on the process for reducing Eu, in order to reliably obtain the effect of improving the life, it is recommended to provide the above-mentioned strong reduction annealing in the temperature decreasing process. Note that the method for increasing the +2 valence rate of Eu is not limited to the above.

[0051] (Reoxidation treatment process) In order to return oxygen to the barium titanate, which is the partially reduced main phase of the dielectric layer 11 fired in a reducing atmosphere, heat treatment may be performed in a mixed gas of N2 and water vapor at about 1000°C or in the air at 500°C to 700°C, to the extent that the internal electrode layer 12 is not oxidized. This process is called a reoxidation process. However, when such a general reoxidation process is performed, Eu reduced to +2 may be oxidized to +3.

[0052] Therefore, in this embodiment, the reoxidation process is performed, for example, in an N2 gas atmosphere at about 900° C. By performing the reoxidation process under such weak oxidation conditions, it is possible to return oxygen to barium titanate while maintaining a high +2 valence rate of Eu.

[0053] (Plating process) Thereafter, the underlayers of the external electrodes 20a, 20b are coated with a metal such as Cu, Ni, Sn, etc. by plating. Through the above steps, the multilayer ceramic capacitor 100 is completed.

[0054] The +2 valence rate of Eu in the dielectric layer 11 can be evaluated, for example, by X-ray Absorption Near Edge Structure (XANES). Specifically, a spectrum near the L3 absorption edge (6977 eV) of Eu is obtained by a fluorescence method using a synchrotron light source. The +2 valence rate (%) can be calculated from the ratio of the peak area of ​​+2 valence and the peak area of ​​+3 valence after removing the background. The peak area ratio can be expressed as in the following formula (1). (+2 charge peak area) / {(+2 charge peak area)+(+3 charge peak area)}×100(%) (1)

[0055] The sample form for measuring the +2 valence rate of Eu may be in the form of a multilayer ceramic capacitor, or may be a powder of a multilayer ceramic capacitor that has been ground into a shape suitable for evaluation. A bulk body may also be obtained by forming a dielectric material into a disk or square plate shape and co-firing it with a multilayer ceramic capacitor. EXAMPLES

[0056] The multilayer ceramic capacitor according to the embodiment was fabricated and its characteristics were examined.

[0057] Example 1 Barium titanate powder was prepared as the dielectric material. Additives such as ZrO2, Eu oxide, MnCO3, and SiO2 were added to the barium titanate powder, and the mixture was mixed and ground with φ0.5mm zirconia beads to obtain the dielectric material. 1.0 mol of Eu was added per 100 mol of the main phase (BaTiZrO3). 0.5 mol of MnCO3 was added per 100 mol of the main phase (BaTiZrO3). 1.0 mol of SiO2 was added per 100 mol of the main phase (BaTiZrO3). Ba / (Ti+Zr) was set to 0.960.

[0058] Dielectric green sheets were prepared by adding an organic binder and a solvent to the dielectric material using the doctor blade method. Polyvinyl butyral (PVB) was used as the organic binder, and ethanol, toluene, etc. were added as the solvent. Plasticizers, etc. were also added.

[0059] Next, a metal conductive paste for forming the internal electrode containing Ni as the main component metal of the internal electrode layer 12, a co-material, a binder (ethyl cellulose), a solvent, and other auxiliary agents as necessary, was prepared using a planetary ball mill.

[0060] A metal conductive paste for forming an internal electrode was screen-printed on the dielectric green sheet. The sheet member on which the metal conductive paste was printed was placed on the dielectric green sheet, and a cover sheet was laminated on the top and bottom of the sheet. After that, a laminate was obtained by thermocompression bonding, and the laminate was cut into a predetermined shape.

[0061] After the obtained laminate was debindered in a N2 atmosphere, a metal conductive paste containing a metal filler mainly composed of Ni, a co-material, a binder, a solvent, etc. was applied to both ends and each side of the laminate as a base layer, and then dried. -10 The firing process was carried out at 1200°C and 10 MPa for 10 minutes. The oxygen partial pressure was set to a mixture ratio of N2-H2-H2O gas. After that, the temperature was increased to 1140°C and the oxygen partial pressure was increased to 10 -13 The annealing process was then carried out by switching the pressure to MPa and holding the pressure for two hours. After that, a reoxidation process was carried out in a N2 gas atmosphere at about 900°C.

[0062] The size of the obtained multilayer ceramic capacitor was 1005 size (length 1.0 mm, width 0.5 mm, height 0.5 mm). The thickness of each dielectric layer was 2 μm. The number of laminated internal electrode layers was 100.

[0063] Example 2 In Example 2, the temperature of the annealing step was set to 1150° C. The other conditions were the same as those in Example 1.

[0064] Example 3 In Example 3, the temperature of the annealing step was set to 1160° C. The other conditions were the same as those in Example 1.

[0065] Example 4 In Example 4, the oxygen partial pressure in the annealing step was set to 10 -14 The other conditions were the same as those in Example 1.

[0066] Example 5 In Example 5, the annealing temperature was 1150° C. and the oxygen partial pressure was 10 -14 The other conditions were the same as those in Example 1.

[0067] Example 6 In Example 6, the annealing temperature was 1160° C. and the oxygen partial pressure was 10 -14 The other conditions were the same as those in Example 1.

[0068] Example 7 In Example 7, the annealing temperature was set to 1150° C., and Ba / (Ti+Zr) was set to 0.940. The other conditions were the same as those in Example 1.

[0069] Example 8 In Example 8, the annealing temperature was 1150° C., and Ba / (Ti+Zr) was 0.920. The other conditions were the same as those in Example 1.

[0070] Example 9 In Example 9, the annealing temperature was 1150° C., and Ba / (Ti+Zr) was 0.980. The other conditions were the same as those in Example 1.

[0071] Comparative Example 1 In Comparative Example 1, the annealing step was not performed. The other conditions were the same as those in Example 1.

[0072] Comparative Example 2 In Comparative Example 2, the baking process was carried out for 20 minutes. The other conditions were the same as those in Example 9.

[0073] Comparative Example 3 In Comparative Example 3, La was used instead of Eu. The other conditions were the same as in Example 2.

[0074] Comparative Example 4 In Comparative Example 4, Gd was used instead of Eu. The other conditions were the same as in Example 2.

[0075] Comparative Example 5 In Comparative Example 5, Dy was used instead of Eu. The other conditions were the same as in Example 2.

[0076] Comparative Example 6 In Comparative Example 6, Ho was used instead of Eu. The other conditions were the same as in Example 2.

[0077] Comparative Example 7 In Comparative Example 7, Er was used instead of Eu. The other conditions were the same as in Example 2.

[0078] (Valence evaluation) The +2 valence rate of Eu in the dielectric layer was evaluated for each of Examples 1 to 9 and Comparative Examples 1 and 2. The +2 valence rate of Eu was evaluated by XANES. FIG. 5 is a XANES spectrum near the L3 absorption edge (6977 eV) of Eu for Example 2. In addition to the +3 valence, a +2 valence peak is clearly observed. From the results of FIG. 5, the +2 valence rate was 26% in Example 2. FIG. 6 is a XANES spectrum near the L3 absorption edge (6977 eV) of Eu for Example 5. From the results of FIG. 6, the +2 valence rate was 43% in Example 5.

[0079] The +2 valence rate of Example 1 was 21%. The +2 valence rate of Example 3 was 29%. The +2 valence rate of Example 4 was 32%. The +2 valence rate of Example 6 was 59%. The +2 valence rate of Example 7 was 28%. The +2 valence rate of Example 8 was 27%. The +2 valence rate of Example 9 was 24%. These results are shown in Table 1. It can be seen that the +2 valence rate increases when the reducing property is strengthened by increasing the temperature of the atmosphere in the annealing process or decreasing the oxygen partial pressure. [Table 1]

[0080] (Life evaluation method) For each of Examples 1 to 9 and Comparative Examples 1 to 7, the mean time to failure in a high-temperature accelerated life test (125°C, 50V / μm) was measured as the life. The life of the sample (Comparative Example 1) produced under normal firing conditions with Eu added was taken as 1.0, and the life ratio of each sample of Examples 1 to 9 and Comparative Examples 2 to 7 was measured. The results are shown in Table 1. If the measured ratio was 5 times or more, the life was sufficiently long and the sample was judged to pass. If the measured ratio was less than 5, the life was not sufficiently long and the sample was judged to fail.

[0081] Fig. 7 is a diagram showing the relationship between the Eu +2 valence rate and the lifespan. As shown in Fig. 7, if the +2 valence rate is 21% or more, the lifespan is 5 times or more longer than that of Comparative Example 1. Also, if the +2 valence rate is 26% or more, the lifespan is 10 times or more longer than that of Comparative Example 1.

[0082] In contrast, no long life was obtained in Comparative Examples 3 to 7. These results show that rare earth elements other than Eu cannot withstand a high load of 125°C and 50V / m. This is thought to be because all rare earth elements other than Eu have a stable valence of +3 and cannot assume a valence of +2.

[0083] In addition, when Examples 7 and 8 are compared with Example 2, it is found that the effect of improving the life is greater in Examples 7 and 8. This is believed to be because the Ba / (Ti+Zr) in Examples 7 and 8 is smaller than the Ba / (Ti+Zr) in Example 2, which increases the number of vacant A sites and increases the amount of Eu in solid solution.

[0084] (Dielectric constant evaluation) The dielectric constant and tan δ were measured for each of Examples 1 to 9 and Comparative Examples 1 to 7. The results are shown in Table 1. Comparing Comparative Example 1 with Example 1, there is no significant difference in dielectric constant and tan δ. This shows that the annealing step does not cause any significant structural changes such as grain growth. Comparing Comparative Example 1 with Example 2, there is no significant difference in dielectric constant and tan δ. This shows that the annealing step of Example 2 does not cause any significant structural changes such as grain growth.

[0085] In Example 6, the dielectric constant and tan δ tended to increase, and there were signs of grain growth. Proceeding the reduction treatment beyond that of Example 6 may cause a change in the structure. Therefore, it is found that the +2 valence rate of Eu is preferably 59% or less.

[0086] Comparing Example 7 and Example 8, it is found that the dielectric constant begins to decrease in Example 8. This means that even if a long life can be secured, there is a risk of capacity decrease. Therefore, it is found that Ba / (Ti+Zr) is preferably 0.940 or more.

[0087] Comparing Example 1 and Comparative Example 2, there is no significant difference in the +2 valence rate, but the relative life of Comparative Example 2 did not reach 5.0 or more. In Comparative Example 2, the dielectric constant and tan δ are increased compared to Example 1. This is considered to mean that the grain growth of barium titanate occurs, and the life-reducing effect due to the grain growth offsets the effect of the +2 valence rate. The reason for this is considered to be that the reactivity of barium titanate increases rapidly as Ba / (Ti+Zr) approaches 1.000, which is the stoichiometric composition. Therefore, it is found that Ba / (Ti+Zr) is preferably 0.960 or less.

[0088] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0089] 10 Stacked Chip 11 Dielectric layer 12 Internal electrode layer 13 Cover Layer 14 Capacity area 15 End Margin 16 Side Margin 20a,20b external electrode 100 Multilayer ceramic capacitors

Claims

1. The perovskite includes, as a main phase, at least Ba in the A site and at least Ti in the B site; Contains Eu, A dielectric material characterized in that the proportion of Eu with a valence of +2 is 21% or more and 43% or less.

2. 2. The dielectric material according to claim 1, wherein the proportion of Eu having a valence of +2 is 80% or less.

3. 3. The dielectric material according to claim 1, wherein in the perovskite, the atomic concentration ratio of the A site / the B site is 0.980 or less.

4. 4. The dielectric material according to claim 1, wherein in the perovskite, the atomic concentration ratio of the A site / the B site is 0.920 or more.

5. 5. The dielectric material according to claim 1, wherein the atomic concentration ratio of Eu / B site is 0.001 or more.

6. 6. The dielectric material according to claim 1, wherein the atomic concentration ratio of Eu to the B site is 0.100 or less.

7. 7. A ceramic electronic component having a laminated structure in which a plurality of dielectric layers made of the dielectric material according to claim 1 and a plurality of internal electrode layers are alternately laminated.

Citation Information

Patent Citations

  • Laminated ceramic electronic component

    JP2012129508A

  • Dielectric ceramic composition and ceramic electronic component

    JP2016169130A

  • Dielectric ceramic and layer-built ceramic capacitor

    WO2008105240A1