Polyolefin-based multilayer elastic film

A multilayer elastic film with specific ethylene/alpha-olefin block copolymers and ethylene-based copolymers addresses elasticity and roll blocking issues, ensuring film performance and reducing additive-related drawbacks.

JP7591565B2Active Publication Date: 2024-11-28DOW GLOBAL TECHNOLOGIES LLC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022515735
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-08-26
Publication Date
2024-11-28
Estimated Expiration
2040-08-26

AI Technical Summary

Technical Problem

Multilayer films used in personal care articles face challenges with elasticity and roll blocking, where additives for reducing migration of low molecular weight polyolefin elastomers can negatively impact film performance and processing.

Method used

A multilayer elastic film composition with a core layer and outer layers comprising specific ethylene/alpha-olefin block copolymers and ethylene-based copolymers, eliminating the need for anti-blocking additives, while maintaining elasticity and preventing surface migration.

Benefits of technology

The film achieves improved elasticity and reduced roll blocking over time, maintaining film performance without the use of anti-blocking additives, and exhibits similar or enhanced elasticity compared to films with additives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591565000001
    Figure 0007591565000001
  • Figure 0007591565000002
    Figure 0007591565000002
  • Figure 0007591565000003
    Figure 0007591565000003
Patent Text Reader

Abstract

According to at least one embodiment of the present disclosure, a multilayer elastic film includes a core layer, a first outer layer, and a second outer layer. The core layer comprises at least 75% by weight of a polyolefin elastomer, such as an ethylene / alpha-olefin block copolymer or a propylene-based plastomer. The first outer layer and the second outer layer each comprise at least 75% by weight of an ethylene-based copolymer selected from the group consisting of: (I) greater than 50% by weight ethylene, 5-16% by weight of an α,β-ethylenically unsaturated C3-C8 carboxylic acid, and optionally, 0.5-10% by weight of an alkyl acrylate; (II) 86-95% by weight ethylene, and 5-14% by weight of an alkyl acrylate; and (III) combinations thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 908,114, filed September 30, 2019, the entire disclosure of which is incorporated herein by reference.

[0002] FIELD OF THE DISCLOSURE Embodiments of the present disclosure relate generally to multilayer films, and specifically to multilayer elastic films comprising polyolefins. [Background technology]

[0003] Multilayer films can be utilized in a variety of applications including personal care articles such as diapers, training pants, adult incontinence products, and hygiene products, among others. The elasticity of such multilayer films can affect the fit of the product, particularly by accommodating the movements of the individual wearing the product.

[0004] To reduce roll blocking behavior, slip and / or anti-blocking additives can be added to the film, but such additives may adversely affect post-processing of the film, such as hot melt adhesive lamination. Additionally or alternatively, low molecular weight polyolefin elastomers that can provide enhanced elasticity may migrate to the surface of the film and cause long-term blocking problems. Additives can be added to the film to prevent migration of these elastomers, but such additives may result in reduced elastic performance and increased stiffness of the film.

[0005] Thus, there remains a need for multilayer elastic films that have suitable elasticity and low roll blocking. Summary of the Invention

[0006] The present composition meets these needs by providing a film having a heat resistant layer to prevent shrinkage or distortion during heat sealing and a tie layer that adheres the heat resistant layer to inks, sealant layers, and / or other polyethylene films without the need for lamination adhesives.

[0007] According to at least one embodiment of the present disclosure, a multilayer elastic film includes a core layer, a first outer layer, and a second outer layer. The core layer includes at least 75% by weight of an ethylene / alpha-olefin block copolymer having a density of 0.850 g / cc to 0.890 g / cc and a melt index (I2) of 0.5 g / 10 min to 5.0 g / 10 min. The first outer layer and the second outer layer each include at least 75% by weight of an ethylene-based copolymer selected from the group consisting of: (I) greater than 50% by weight of ethylene, 5 to 16% by weight of an α,β-ethylenically unsaturated C3-C8 carboxylic acid, and optionally, 0.5 to 10% by weight of an alkyl acrylate; (II) 86 to 95% by weight of ethylene, and 5 to 14% by weight of an alkyl acrylate; and (III) combinations thereof.

[0008] According to another embodiment of the present disclosure, the ethylene / alpha-olefin block copolymer has a melting temperature of 115°C to 125°C.

[0009] According to another embodiment of the present disclosure, the ethylene / alpha-olefin block copolymer has a molecular weight distribution (MWD=Mw / Mn) of 2-3.

[0010] According to another embodiment of the present disclosure, the ethylene / alpha-olefin block copolymer has an I2 of 0.5-2.0 g / 10 min.

[0011] According to another embodiment of the present disclosure, the core layer comprises 75-100 wt % ethylene / alpha-olefin block copolymer.

[0012] According to another embodiment of the present disclosure, a multilayer elastic film includes a core layer, a first outer layer, and a second outer layer. The core layer includes at least 75% by weight of a propylene-based plastomer having a density of 0.860 g / cc to 0.90 g / cc and a melt flow rate (MFR) of 0.5 g / 10 min to 5.0 g / 10 min. The first outer layer and the second outer layer each include at least 75% by weight of an ethylene-based copolymer selected from the group consisting of: (I) greater than 50% by weight of ethylene, 5 to 16% by weight of an α,β-ethylenically unsaturated C3-C8 carboxylic acid, and optionally, 0.5 to 10% by weight of an alkyl acrylate; (II) 86 to 95% by weight of ethylene, and 5 to 14% by weight of an alkyl acrylate; and (III) combinations thereof.

[0013] According to another embodiment of the present disclosure, the first outer layer and the second outer layer each comprise at least 75 weight percent ethylene-based copolymer.

[0014] According to another embodiment of the present disclosure, the first outer layer and the second outer layer each comprise 75 to 100 weight percent ethylene-based copolymer.

[0015] According to another embodiment of the present disclosure, the ethylene-based copolymer of the first outer layer, the second outer layer, or both, has a melt index (I2) from 4.0 g / 10 min to 20.0 g / 10 min.

[0016] According to another embodiment of the present disclosure, the ethylene-based copolymer of the first outer layer, the second outer layer, or both, has greater than 80 weight percent ethylene and from 7 to 11 weight percent α,β-ethylenically unsaturated C3-C8 carboxylic acid.

[0017] According to another embodiment of the present disclosure, the ethylene-based copolymer of the first outer layer, the second outer layer, or both, has 88 to 94 weight percent ethylene and 6 to 12 weight percent alkyl acrylate.

[0018] According to another embodiment of the present disclosure, the ethylene-based copolymer of the first outer layer, the second outer layer, or both, has a density from 0.920 g / cc to 0.950 g / cc.

[0019] According to another embodiment of the present disclosure, the multilayer elastic film comprises less than 1 wt. % of an anti-blocking or slip additive.

[0020] According to another embodiment of the present disclosure, the multilayer elastic film is a blown film or a cast film.

[0021] According to another embodiment of the present disclosure, the multilayer elastic film is a cast film, the cast film having an unwind force of less than 1 N / 50 mm after 12 weeks at a length ranging from 10 m to 50 m.

[0022] These and other embodiments are described in more detail in the Detailed Description below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Specific embodiments of the present application will now be described. However, the present disclosure may be embodied in different forms and should not be construed as being limited to the embodiments set forth in this disclosure. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present subject matter to those skilled in the art.

[0024] definition The term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether the monomers are the same or different types. Thus, the generic term polymer encompasses the term "homopolymer," which is commonly used to refer to a polymer prepared from only one type of monomer, and "copolymer," which refers to a polymer prepared from two or more different monomers. As used herein, the term "interpolymer" refers to a polymer prepared by polymerization of at least two different types of monomers. Thus, the generic term interpolymer includes copolymers and polymers prepared from three or more different types of monomers, such as terpolymers.

[0025] By "multilayer film" is meant any structure having multiple layers. For example, a multilayer structure may have 2, 3, 4, 5, or more layers. A multilayer film may be described as having layers designated by letters. For example, a three-layer structure having a core layer B and two outer layers A and C may be designated as A / B / C. Similarly, a structure having two core layers B and C and two outer layers A and D may be designated as A / B / C / D. Additionally, one skilled in the art will know that additional layers E, F, G, etc. may also be incorporated into this structure.

[0026] As used herein, "polyolefin" refers to an olefin-based polymer. As used herein, "olefin," sometimes referred to as "alkene," refers to a linear, branched, or cyclic compound that contains carbon and hydrogen and has at least one double bond. As used herein, when a polymer or copolymer, such as a polyolefin elastomer, is referred to as containing an olefin, the olefin present in the polymer or copolymer is the polymerized form of the olefin. For example, when a polyolefin elastomer is stated to have an ethylene content of 75% to 85% by weight, it is understood that the polymer units in the polyolefin elastomer are derived from ethylene in a polymerization reaction, and the derived units are present at 75% to 85% by weight, based on the total weight of the polyolefin elastomer.

[0027] As used herein, "elastomer" refers to a material that substantially recovers its original shape after being stretched. For example, upon application of a stretching force, an elastomer can stretch in at least one direction, such as the cross machine direction, and upon release of the stretching force, contracts / returns to approximately its original dimensions. For example, an exemplary elastomer is an extensible material that has an elongated length that is at least 50% greater than its relaxed, unstretched length, and upon release of the stretching force, recovers to within at least 50% of its elongated length. A hypothetical example would be a 1 inch sample of material that can be stretched to at least 1.50 inches, and upon release of the stretching force, recovers to a length of 1.25 inches or less.

[0028] As used herein, the term "ethylene / alpha-olefin block copolymer" refers to a polymer comprising ethylene and an alpha-olefin having 3 or more carbon atoms. Ethylene may constitute the majority mole fraction of the ethylene / alpha-olefin block copolymer. For example, ethylene may constitute at least 50 mol%, at least 60 mol%, at least 70 mol%, at least 80 mol%, or at least 90 mol% of the ethylene / alpha-olefin block copolymer, with the remainder of the ethylene / alpha-olefin block copolymer being at least one other comonomer, such as an alpha-olefin having 3 or more carbon atoms.

[0029] A "propylene-based plastomer" is a propylene / ethylene copolymer having 3 wt%, or 4 wt%, or 5 wt%, or 6 wt%, or 7 wt% to 8 wt%, or 9 wt%, or 10 wt%, or 11 wt%, or 12 wt%, or 13 wt%, or 14 wt%, or 15 wt% ethylene comonomer (based on the total weight of the plastomer). The propylene-based plastomer has a heat of fusion of less than 100 J / g and a Mw / Mn of less than 3.5. The propylene-based plastomer has a heat of fusion of less than 40 J / g when the ethylene comonomer content is 10 wt%, or 11 wt%, or 12 wt% to 13 wt%, or 14 wt%, or 15 wt%.

[0030] Reference will now be made in detail to embodiments of the multilayer films of the present disclosure which exhibit improved elasticity and reduced roll blocking as compared to other films.

[0031] Blocking is the adhesion between two contacting parts of a film, for example between layers or sheets. Without wishing to be bound by theory, blocking may occur due to van der Waals forces between the two contacting parts of the film and / or the presence of relatively low molecular weight components of the film that migrate toward the film surface. For many applications, blocking may be an undesirable property, as it may increase the friction between the two contacting parts.

[0032] Various embodiments include a multilayer film comprising a core layer adjacent to a first outer layer and a second outer layer. For example, the core layer can be formed between the first outer layer and the second outer layer, for example in contact. The outer layers can have the same composition as each other. However, in some embodiments, the first outer layer can have a different composition than the composition of the second outer layer.

[0033] Core layer The core layer comprises at least 75 weight percent (wt%) polyolefin elastomer, based on the total weight of the core layer. For example, the core layer may comprise 75 wt% to 100 wt% polyolefin elastomer, based on the total weight of the core layer. All individual values ​​and subranges between 75 wt% and 100 wt% are included. For example, the core layer may comprise a lower limit of 75 wt%, 76 wt%, 77.5 wt%, or 80 wt% polyolefin elastomer, to an upper limit of 100 wt%, 99.5 wt%, 99 wt%, 97 wt%, or 95 wt%, based on the total weight of the core layer.

[0034] In various embodiments, the polyolefin elastomer can include an olefin block copolymer, such as an ethylene / alpha-olefin block copolymer. Commercially available examples of ethylene / alpha-olefin block copolymers include resins available under the trade name INFUSE™ available from The Dow Chemical Company (Midland, MI).

[0035] In various embodiments, the ethylene / alpha-olefin copolymer may comprise ethylene in polymerized form and one or more copolymerizable alpha-olefins, characterized by multiple blocks or segments of two or more polymerized monomer units with different chemical or physical properties. The polyolefin elastomer may be a multi-block copolymer. In one or more embodiments, the multi-block copolymer may be represented by the formula (AB)n, where n is an integer of at least 1, preferably greater than 1, such as 2, 3, 4, 5, 10, 15, 20, 30, 40, 50, 60, 70, 80, 90, 100, or more, and "A" represents the hard block and "B" represents the soft block. In embodiments, A and B are linked in a substantially linear fashion, as opposed to a substantially branched or substantially star-shaped fashion. In one or more embodiments, the A and B blocks are randomly distributed along the polymer chain and do not have a structure such as the following: AAA-AA-BBB-BB. In some embodiments, the block copolymer does not have a third type of block comprising a different comonomer. In embodiments, block A and block B each have monomers or comonomers substantially randomly distributed within the block such that neither block A nor block B comprises two or more subsegments of distinct composition, such as tip segments, having a substantially different composition than the remainder of the block.

[0036] Ethylene / alpha-olefin block copolymers can include various amounts of "hard" and "soft" blocks. "Hard" blocks refer to blocks of polymerized units in which ethylene is present in an amount of more than about 95% by weight, and preferably more than about 98% by weight, based on the weight of the polymer. In other words, the comonomer content in the hard blocks, i.e., the content of monomers other than ethylene, is less than about 5% by weight, and preferably less than about 2% by weight, based on the weight of the polymer. In one or more embodiments, the hard blocks contain all or substantially all ethylene. "Soft" blocks, on the other hand, refer to blocks of polymerized units in which the comonomer content, i.e., the content of monomers other than ethylene, is greater than about 5% by weight. For example, the comonomer content can be greater than about 5% by weight, greater than about 8% by weight, greater than about 10% by weight, or greater than about 15% by weight, based on the weight of the polymer. In various embodiments, the comonomer content in the soft blocks can be greater than about 20% by weight, greater than about 25% by weight, greater than about 30% by weight, greater than about 35% by weight, greater than about 40% by weight, greater than about 45% by weight, greater than about 50% by weight, or greater than about 60% by weight based on the weight of the polymer.

[0037] In various embodiments, the soft block is present in the ethylene / alpha-olefin block copolymer in an amount of about 1% to about 99% by weight of the total weight of the polyolefin elastomer. For example, the soft segment may be present in the ethylene / alpha-olefin block copolymer in an amount of about 5% to about 95% by weight, about 10% to about 90% by weight, about 15% to about 85% by weight, about 20% to about 80% by weight, about 25% to about 75% by weight, about 30% to about 70% by weight, about 35% to about 65% by weight, about 40% to about 60% by weight, or about 45% to about 55% by weight of the total weight of the polyolefin elastomer. Conversely, the hard flocs may be present in a similar range. The weight percentages of the soft and hard blocks may be calculated based on data obtained from DSC or NMR. Such methods and calculations are disclosed in U.S. Patent Application Publication No. 2006 / 0199930.

[0038] Examples of alpha-olefin comonomers that can be used to form ethylene / alpha-olefin block copolymers include, by way of example and not limitation, propylene, isobutylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecent, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 4,6-dimethyle-1-heptene, 4-vinylcyclohexene, vinylcyclohexane, norbornadiene, ethylidenenorbornene, cyclopentene, cyclohexene, dicyclopentadiene, cyclooctene, C4-C6 40 Dienes, other C4-C 40 In further embodiments, the alpha-olefin comonomer may include a C3-C8 comonomer. Comonomer content may be determined using any suitable technique, such as techniques based on nuclear magnetic resonance ("NMR") spectroscopy, and as described, for example, in U.S. Pat. No. 7,498,282, which is incorporated herein by reference. 13 It can be measured by C NMR analysis.

[0039] In various embodiments, the ethylene / alpha-olefin block copolymer has a melt index (I2) of about 0.5 to about 30.0 g / 10 min, as determined according to ASTM D1238 (190° C., 2.16 kg). For example, the polyolefin elastomer can have a melt index (I2) of 0.5 to 30.0 g / 10 min, 0.5 to 15 g / 10 min, 0.5 g / 10 min to 5.0 g / 10 min, or 0.5 g / 10 min to 2.0 g / 10 min.

[0040] In various embodiments, the ethylene / alpha-olefin block copolymer has a density from 0.850 g / cc to 0.890 g / cc, all individual values ​​and subranges between 0.850 g / cc and 0.890 g / cc are included herein and disclosed herein, for example, the density of the ethylene / alpha-olefin block copolymer can be from a lower limit of 0.850 g / cc, 0.855 g / cc, 0.860 g / cc, 0.865 g / cc, or 0.870 g / cc to an upper limit of 0.890 g / cc, 0.885 g / cc, 0.880 g / cc, or 0.875 g / cc.

[0041] Ethylene / alpha-olefin block copolymers have a melting temperature (T m ) (DSC). All individual values ​​and subranges from 115°C to 125°C are included herein and disclosed herein, for example, the melting point of the ethylene / alpha-olefin block copolymer can be from a lower limit of 115°C, 116°C, 117°C, 118°C, 119°C, or 120°C to an upper limit of 125°C, 124°C, 123°C, 122°C, or 121°C.

[0042] In some embodiments, the ethylene / alpha-olefin block copolymer has a molecular weight distribution (MWD) of 3.5 or less. The molecular weight distribution (MWD) is defined as the weight average molecular weight (Mw) divided by the number average molecular weight (Mn). For example, the ethylene / alpha-olefin block copolymer of some embodiments has an MWD of 2 to 3. Techniques for determining molecular weight (Mn and Mw) and MWD can be found in U.S. Patent No. 4,540,753, which is incorporated herein by reference.

[0043] The ethylene / alpha-olefin block copolymers can be formed utilizing known polymerization processes, such as those described in PCT Application No. PCT / US2005 / 008915, PCT Application No. PCT / US2005 / 008916, and PCT Application No. PCT / US2005 / 008917, each of which is incorporated herein by reference.

[0044] In another embodiment, the polyolefin elastomer may include a propylene-based plastomer. In one embodiment, the propylene-based plastomer has from 3% to less than 10% by weight ethylene comonomer and has the following properties: (i) a density of less than 0.860 g / cc, or 0.870 g / cc, or 0.880 g / cc to 0.885 g / cc, or 0.890, or 0.895, or 0.90 g / cc as measured according to ASTM D792; (ii) a Vicat softening temperature of 60° C., or 61° C., or 62° C. to 63° C., or 64° C., or 65° C.; (iii) a melting temperature of 70° C., or 73° C., or 75° C., or 77° C. to 80° C., or 82° C., or 83° C. to 85° C., or 87° C., or 89° C., or 90° C. m and (iv) a propylene / ethylene copolymer having one, some, or all of the following melt flow rates (MFR), as determined in accordance with ASTM D1238 (230°C, 2.16 kg): 0.5 g / 10 min, or 1.0 g / 10 min, or 1.5 g / 10 min, or 2.0 g / 10 min, or 2.5 g / 10 min to 3.0 g / 10 min, or 3.5 g / 10 min, or 4.0 g / 10 min, or 4.5 g / 10 min, or 5.0 g / 10 min. Vicat softening temperature is a determination of the softening point for materials that do not have a distinct melting point. Vicat softening temperature is measured in accordance with ASTM D1525.

[0045] Non-limiting examples of suitable propylene-based plastomers include VERSIFY™ 2400 and VERSIFY™ 2300 available from The Dow Chemical Company (Midland, MI).

[0046] In embodiments, in addition to the polyolefin elastomer, the core layer may further include one or more additives. Examples of additives include, by way of example and not limitation, viscosity reducing polymers, plasticizers, tackifiers, dyes, pigments, antioxidants, antistatic agents, adhesion aids, heat stabilizers, light stabilizers, blowing agents, glass bubbles, starch, metal salts, microfibers, and the like. In some embodiments, one or more elastomeric materials, such as styrene-ethylene-butene-styrene (SEBS) block copolymers, are added to the core layer to further improve elastic performance. When present, any additive is included in the core layer in an amount of 25% by weight or less. For example, the core layer may include 0% to 25% by weight, 1% to 25% by weight, 5% to 20% by weight, 10% to 15% by weight, and the like. All individual values ​​and subranges from 0% to 25% by weight are included and disclosed herein.

[0047] outer layer In various embodiments, the multilayer film further comprises a first outer layer and a second outer layer. Each outer layer comprises at least 75 wt% of an ethylene-based copolymer. For example, the outer layer may comprise 75 wt% to 100 wt% of an ethylene-based copolymer, based on the total weight of the outer layer. All individual values ​​and subranges between 75 wt% and 100 wt% are included. For example, the outer layer may comprise a lower limit of 75 wt%, 76 wt%, 77.5 wt%, or 80 wt% of an ethylene-based copolymer, based on the total weight of the outer layer, to an upper limit of 100 wt%, 99.5 wt%, 99 wt%, 97 wt%, or 95 wt% of an ethylene-based copolymer.

[0048] In some embodiments, the ethylene-based copolymer is an ethylene acid copolymer. The ethylene acid copolymer is a polymerization reaction product of ethylene and one or more carboxylic acids, and may optionally include an alkyl acrylate. The ethylene may be present in an amount of more than 50% by weight, based on the total weight of the ethylene acid copolymer. For example, the ethylene acid copolymer may include 50% to 95% by weight ethylene, 55% to 90% by weight ethylene, 60% to 85% by weight ethylene, 65% to 80% by weight ethylene, or 70% to 75% by weight ethylene. The ethylene acid copolymer may include more than 60% by weight ethylene, more than 70% by weight ethylene, or more than 80% by weight ethylene, based on the total weight of the ethylene acid copolymer. All individual values ​​and subranges from 75% to 95% by weight are included.

[0049] In various embodiments, the carboxylic acid is an α,β-ethylenically unsaturated 3-C8 carboxylic acid. The carboxylic acid can be, for example, acrylic acid, methacrylic acid, fumaric acid, itaconic acid, maleic acid, aconitic acid, various α-substituted acrylic acids, or combinations thereof. In various embodiments, the α,β-ethylenically unsaturated C3-C8 carboxylic acid is present in an amount of 5% to 16%, 6% to 15%, or 7% to 11% by weight based on the total weight of monomers present in the ethylene acid copolymer. All individual values ​​and subranges from 5% to 16% by weight are included.

[0050] In some embodiments, the ethylene acid copolymer optionally includes an alkyl acrylate. In embodiments in which an alkyl acrylate is included, the alkyl acrylate can be present in an amount of 0.5% to 10% by weight. For example, the alkyl acrylate can be included in an amount of 0.5% to 10% by weight, 1% to 9% by weight, 2% to 8% by weight, or 3% to 7% by weight. All individual values ​​and subranges between 0.5% and 10% by weight are included.

[0051] Suitable ethylene acid copolymers may include those commercially available under the trade names NUCREL™, such as NUCREL™ 3990 (available from The Dow Chemical Company, Midland, MI), PRIMACOR™ (available from SK Global Chemical), and ESCOR™ (available from ExxonMobil Chemical).

[0052] In yet other embodiments, the ethylene-based copolymer is a copolymer of ethylene and an alkyl acrylate. The ethylene can be present in an amount of 86% to 95% by weight, based on the total weight of the ethylene-based copolymer. For example, the ethylene-based copolymer can include 86% to 95% by weight ethylene, 87% to 94% by weight ethylene, or 88% to 94% by weight ethylene. All individual values ​​and subranges between 86% and 95% by weight are included.

[0053] Suitable acrylate copolymers may include ethyl methyl acrylate (EMA), ethylene ethyl acrylate (EEA), and ethylene butyl acrylate (EBA). The ethylene acrylate copolymers may have a weight percent of maleic anhydride (MA), ethyl acrylate (EA), or butyl acrylate (BA) at comonomer levels of 5.0% to 50%, 10% to 45%, 15% to 40%, or 20% to 35% by weight. The ethylene acrylate copolymers may have a melt index (I2) of 4 to 20 g / 10 min, 4 to 15 g / 10 min, 4 to 12 g / 10 min, or 5 to 10 g / 10 min, as determined according to ASTM D1238 (190° C., 2.16 kg). An example of a commercially available copolymer resin that may be used in some embodiments includes ELVALOY™ 1609AC, all available from The Dow Chemical Company, Midland, MI.

[0054] In such embodiments, the alkyl acrylate can be present in an amount of 5% to 14% by weight based on the total weight of the ethylene-based copolymer. For example, the alkyl acrylate can be present in an amount of 5% to 14% by weight, 6% to 13% by weight, or 6% to 12% by weight based on the total weight of the ethylene-based copolymer. All individual values ​​and subranges between 5% and 14% by weight are included. Without being bound by theory, it is believed that this range of alkyl acrylate provides suitable adhesion properties for the ethylene-based copolymer, whereas ethylene-based copolymers having more than 14% alkyl acrylate are too tacky, leading to poor roll blocking properties.

[0055] In some embodiments, the ethylene-based copolymer is an ethylene acid copolymer or an ethylene-alkyl acrylate copolymer, although it is contemplated that in other embodiments the ethylene-based polymer can include a combination of copolymers. For example, the outer layer can include an ethylene acid copolymer and an ethylene-alkyl acrylate copolymer.

[0056] In various embodiments, the ethylene-based copolymer of the outer layer has a density of, in some embodiments, 0.920 to 0.950 g / cc, 0.920 to 0.945 g / cc, or 0.925 to 0.940 g / cc.

[0057] Additional compositions and additives are also contemplated to be included in the outer layer. Examples of additives include, by way of example and not limitation, viscosity reducing polymers, plasticizers, tackifiers, dyes, pigments, antioxidants, antistatic agents, adhesion aids, heat stabilizers, light stabilizers, foaming agents, glass bubbles, starches, metal salts, microfibers, and the like. In some embodiments, the outer layer may include mineral fillers such as CaCO3, which may be beneficial in the extrusion process.

[0058] Multilayer Film As mentioned above, various embodiments include a multilayer configuration including a core layer adjacent to a first outer layer and a second outer layer. The multilayer film can be formed by a variety of processes. For example, the multilayer film can be formed by a blown film process or a cast film process.

[0059] The blown film process may utilize an extruder to heat, melt, and convey the components of the multilayer film to a die. Each layer of the multilayer film may have a corresponding stream introduced into the die. Generally, the extrusion temperature is between 150°C and 275°C, but the specific temperature may vary depending on the specific film composition. The components of the multilayer film may be drawn from the die, formed into a tubular shape, and passed through a pair of draw-in or nip rollers. Internal compressed air may then be introduced from a mandrel to increase the diameter of the tube, thereby forming a "bubble" of the desired size. Thus, the blown film may be stretched in two directions, i.e., axially, by using forced air to "blow" the diameter of the bubble, and longitudinally, by the action of a take-up element that pulls the bubble through the machine. External air may also be introduced around the bubble to cool the melt as it exits the die. The film width may be varied by introducing more or less internal air into the bubble, thus increasing or decreasing the bubble size. The film thickness can be controlled by increasing or decreasing the speed of the draw rolls or nip rolls to control the drawdown rate. After passing through the draw rolls or nip rolls, the bubble can collapse. The cooled film can then be further processed by cutting or sealing to produce various consumer products.

[0060] In the cast film process, the components of the multilayer film can be extruded onto a rotating roll where the multilayer film is quenched on one side by the roll. The speed of the roller can be used to control the draw ratio and final film thickness. The multilayer film can then be sent to a second roller to cool the other side.

[0061] The core layer can be 70% to 90% by weight of the multilayer film, based on the total weight of the multilayer film layers, including all individual values ​​and subranges between 70% and 90% by weight. For example, the core layer can be from a lower limit of 70, 71, 72, 73, 74, or 75% by weight, to an upper limit of 90, 89, 88, 87, 86, or 85% by weight, based on the total weight of the multilayer film.

[0062] The core layer can have a thickness of 15 microns (μm) to 60 μm, including all individual values ​​and subranges between 15 and 60 μm. For example, the core layer can have a lower limit of 15, 17.5, 20, 22.5, or 25 μm to an upper limit of 60, 57.5, 52.5, or 50 μm.

[0063] Each outer layer may individually be from 5% to 15% by weight of the multilayer film, based on the total weight of the multilayer film layers, including all individual values ​​and subranges between 5% and 15% by weight. For example, the outer layers may be from a lower limit of 5, 5.5, 6, 6.5, 7, or 7.5% by weight, to an upper limit of 15, 14.5, 14, 13.5, 13, or 12.5% ​​by weight, based on the total weight of the multilayer film.

[0064] Each outer layer may have a thickness of 1 μm to 10 μm, including all individual values ​​and subranges between 1 μm and 10 μm. For example, the outer layers may have a thickness from a lower limit of 1, 1.5, 1.75, 2, or 2.5 μm to an upper limit of 10, 9.5, 9, 8.5, or 8 μm.

[0065] The multilayer film may have a thickness of 17 μm to 80 μm, including all individual values ​​and subranges between 17 μm and 80 μm. For example, the multilayer film may have a thickness of 17, 20.5, 24, 26.5, or 30 μm at lower limits to 80, 76.5, 73, 69.5, or 66 μm at upper limits.

[0066] In various embodiments described herein, the multilayer film is a laminate having less than 1 wt.% of an anti-blocking or slip additive. For example, the multilayer film may have 0 wt.% to 1 wt.%, 0 wt.% to 0.75 wt.%, 0 wt.% to 0.5 wt.%, 0 wt.% to 0.25 wt.%, or no anti-blocking or slip additive.

[0067] As noted, the multilayer films described herein may advantageously have improved blocking compared to other films, despite limitations or lack of anti-blocking or slip additives. Additionally, the multilayer films may advantageously have comparable or even improved elasticity compared to other films. In some specific embodiments, the multilayer films may have an unwind force of less than 1 N / 50 mm after 12 weeks at lengths ranging from 10 m to 50 m.

[0068] Goods In various embodiments, the multilayer films disclosed herein can be used to form articles such as disposable personal care articles. Such articles can be formed from any of the multilayer films described herein. Examples of disposable personal care articles that can be formed from the multilayer films of various embodiments can include diapers, training pants, adult incontinence products, and feminine hygiene products. Such personal care articles can be formed using techniques known to those skilled in the art based on the teachings herein and based on the specific use of the article.

[0069] Test Method Test methods include: Melt Index (I2) Melt index (I2) was measured according to ASTM D-1238 at 190° C. and 2.16 kg. Values ​​are reported in g / 10 min, which corresponds to grams dissolved per 10 minutes.

[0070] Melt Flow Rate (MFR) MFR was measured according to ASTM D-1238 at 230° C. and 2.16 kg. Values ​​are reported in g / 10 min, which corresponds to grams dissolved per 10 minutes.

[0071] density Samples for density measurements were prepared according to ASTM D4703 and measured in grams per cubic centimeter (g / cc or g / cm 3 The measurements were made within 1 hour of specimen compression using ASTM D792, Method B.

[0072] Melting point Differential scanning calorimetry (DSC) is used to measure the melting and crystallization behavior of polymers over a wide range of temperatures. For example, a TA Instruments Q1000 DSC equipped with an RCS (refrigerated cooling system) and an autosampler is used to perform this analysis. The instrument is first calibrated using the software calibration wizard. A baseline is obtained by heating the cell from -80°C to 280°C without any sample in an aluminum DSC pan. A sapphire standard is then used as instructed by the calibration wizard. Next, 1-2 milligrams (mg) of fresh indium sample is analyzed by heating the standard sample to 180°C, cooling to 120°C at a cooling rate of 10°C / min, and then holding the standard sample isothermal at 120°C for 1 minute. The standard sample is then heated from 120°C to 180°C at a heating rate of 10°C / min. The indium standard is then determined to have a heat of fusion (Hf) = 28.71 ± 0.50 Joules per gram (J / g), and an onset of melting = 156.6 ° C. ± 0.5 ° C. The test sample is then analyzed on a DSC instrument.

[0073] A nitrogen purge gas flow rate of 50 ml / min is used during testing. Each sample is melt pressed into a thin film at approximately 175°C, and then the molten sample is air cooled to room temperature (approximately 25°C). Film samples are formed by pressing 0.1-0.2 gram samples at 175°C, 1,500 psi, and 30 seconds to form a 0.1-0.2 mil thick film. A 3-10 mg, 6 mm diameter specimen is extracted from the cooled polymer, weighed, placed in a light (approximately 50 mg) aluminum pan, and crimped shut. Analysis is then performed to determine its thermal properties.

[0074] The thermal behavior of the sample is determined by ramping the sample temperature to generate a heat flow vs. temperature profile. First, the sample is rapidly heated to 180°C and held isothermal for 5 minutes to remove thermal history. Next, the sample is cooled to -40°C at a cooling rate of 10°C / min and held isothermal at -40°C for 5 minutes. The sample is then heated to 150°C at a heating rate of 10°C / min (this is the "second heat" ramp). The cooling curve and the second heating curve are recorded. The cooling curve is analyzed by setting a baseline end point from the onset of crystallization to -20°C. The heating curve is analyzed by setting a baseline end point from -20°C to the end of melting. The determined value is the peak melting temperature (T m ), peak crystallization temperature (T c ), onset crystallization temperature (Tc onset), heat of fusion (H f ) (grams per joule), and the % crystallinity calculated for the polyethylene samples using % crystallinity PE = ((Hf) / (292 J / g)) x 100, and the % crystallinity calculated for the polypropylene samples using % crystallinity PP = ((Hf) / 165 J / g)) x 100. f ) and peak melt temperature are reported from the second heat curve. The peak crystallization temperature and onset crystallization temperature are determined from the cooling curve.

[0075] Elasticity Performance The elastic properties of the film samples were evaluated by performing a two-cycle hysteresis test according to ASTM D5459. Specifically, a 25 mm wide specimen was stretched to 100% elongation at a rate of 250 mm / min and immediately retracted to 0% elongation at the same rate. After 60 seconds, a second cycle was performed. The grip distance was set at 50 mm. The permanent set values ​​were reported. Lower permanent set values ​​indicate improved elastic performance.

[0076] Roll Blocking Roll blocking was evaluated by unwinding 50m rolls on a Dr. Collin cast rewinder with a load cell capacity of 25kg and measuring the force. The rolls were unwound at a speed of 10m / min and the film had a width of 180mm. The force per 50mm of length was reported in N / 50mm after unwinding the film samples at 10, 20, 30, 40 and 50m. Blocking behavior was evaluated at 1 week and 12 weeks after extrusion. EXAMPLES

[0077] The following examples illustrate features of the present disclosure and are not intended to limit the scope of the disclosure.

[0078] In the examples, the following materials were used:

[0079] Granic 421 is a calcium carbonate masterbatch (73% CaCO3 in LLDPE) and is commercially available from Granic Group (Tarragona, Spain).

[0080] POLYBATCH™ FSU-105-E is a slip and antiblock masterbatch containing 5% erucamide as a slip agent, and 10% silica as an antiblock agent, and is commercially available from Schulmann.

[0081] STYRON A-TECH™ 1200 is an impact resistant polystyrene containing approximately 8% by weight polybutadiene rubber, having a density of 1.05 g / cc (measured according to ISO 1388), and having a mass melt flow of 5 g / 10 min (measured at 200° C. and 5 kg according to ISO 1388) and is commercially available from TRINSEO.

[0082] INFUSE™ 9107 is an ethylene-alpha olefin block copolymer having an I2 of 1 g / 10 min, and a density of 0.866 g / cc, and is commercially available from The Dow Chemical Company, Midland, MI.

[0083] VERSIFY™ 3300 is a propylene-based plastomer (propylene block copolymer) with an MFR of 8 g / 10 min, and a density of 0.868 g / cc, and is commercially available from The Dow Chemical Company, Midland, MI.

[0084] ELVALOY AC2615 is used as a comonomer 15 It is an ethylene acrylate copolymer containing % by weight methyl acrylate, having an I2 of 6.0 g / 10 min and a density of 0.930 g / cc, and is commercially available from The Dow Chemical Company, Midland, MI.

[0085] ELVALOY AC1609 is used as a comonomer 9 It is an ethylene acrylate copolymer containing % by weight ethyl acrylate, having an I2 of 6.0 g / 10 min and a density of 0.930 g / cc, and is commercially available from The Dow Chemical Company, Midland, MI.

[0086] NUCREL™ 3990 is an ethylene acid copolymer containing 9 wt. % acrylic acid and having an I2 of 10.0 g / 10 min and is commercially available from The Dow Chemical Company, Midland, MI.

[0087] The following multilayer films in Table 1 had a coextrusion of ABC 3-layer structure. The coextrusion was carried out on a Collin coextrusion cast film line equipped with a 25mm extruder under the following conditions: layer ratio (A / B / C): 10 / 80 / 10, throughput: 10kg / hr, take speed: 12m / min, die gap: 0.8mm. [Table 1]

[0088] Blocking was measured for Comparative Samples 1-3 and Samples 1-2 at lengths of 10 m, 20 m, 30 m, 40 m, and 50 m at 1 week and 12 weeks after extrusion and the results are reported in Table 2 as N / 50 mm. [Table 2]

[0089] As can be seen from Table 2, films formed from Samples 1 and 2 show improved aging compared to the film formed from Comparative Sample 1. Without being bound by theory, it is believed that the anti-blocking additives (CaCO3 and silica) in Comparative Sample 1 migrate from the surface over time, leading to reduced blocking over time. Comparative Sample 3 is believed to have exhibited poor blocking performance due to the inclusion of ELVALOY™ AC2615, which contains 15 wt. % ethyl acrylate. This amount of acrylate comonomer made the film too tacky, which adversely affected blocking performance.

[0090] Elastic performance was measured for Comparative Samples 1-3, and Samples 1 and 2. Results are reported in Table 3 as force (N) at permanent set for the cross direction (CD) and machine direction (MD). [Table 3]

[0091] As shown in Table 3, each of Samples 1 and 2 had comparable elasticity to Comparative Samples 1 and 3, but also showed improved blocking over time compared to these samples. Samples 1 and 2 also showed improved elasticity performance over Comparative Example 2, which contained polystyrene and polypropylene to keep blocking under control.

[0092] It will be apparent that modifications and variations are possible without departing from the scope of the present disclosure, as defined in the appended claims. More specifically, although certain aspects of the present disclosure have been identified herein as preferred or particularly advantageous, it is contemplated that the present disclosure is not necessarily limited to those aspects. The present invention may include the following aspects. [1] 1. A multilayer elastic film comprising a core layer, a first outer layer, and a second outer layer, The core layer has a density of 0.850 g / cc to 0.890 g / cc and a melt index (I 2 % by weight of an ethylene / alpha-olefin block copolymer having the first outer layer and the second outer layer each comprise at least 75 weight percent of an ethylene-based copolymer, the ethylene-based copolymer comprising: (I) More than 50% by weight of ethylene, 5 to 16% by weight of α,β-ethylenically unsaturated C 3 -C 8 a carboxylic acid, and optionally 0.5 to 10 wt. % of an alkyl acrylate; (II) 86 to 95% by weight of ethylene and 5 to 14% by weight of an alkyl acrylate; (III) combinations thereof. [2] The multilayer elastic film according to [1], wherein the ethylene / alpha-olefin block copolymer has a melting temperature of 115°C to 125°C. [3] The ethylene / alpha-olefin block copolymer has a molecular weight distribution (MWD=M w / M n 13. The multilayer elastic film of any one of the preceding claims, having a [4] The ethylene / alpha-olefin block copolymer I 2 The multilayer elastic film of any one of the preceding claims, wherein the viscosity is 0.5 to 2.0 g / 10 min. [5] 10. The multilayer elastic film of any one of the preceding claims, wherein the core layer comprises 75-100% by weight of the ethylene / alpha-olefin block copolymer. [6] 1. A multilayer elastic film comprising a core layer, a first outer layer, and a second outer layer, the core layer comprises at least 75% by weight of a propylene-based plastomer having a density of 0.860 g / cc to 0.900 g / cc and a melt flow rate (MFR) of 0.5 g / 10 min to 5.0 g / 10 min; the first outer layer and the second outer layer each comprise at least 75 weight percent ethylene-based copolymer, the ethylene-based copolymer comprising: (I) More than 50% by weight of ethylene, 5 to 16% by weight of α,β-ethylenically unsaturated C 3 -C 8 a carboxylic acid, and optionally 0.5 to 10 wt. % of an alkyl acrylate; (II) 86 to 95% by weight of ethylene and 5 to 14% by weight of an alkyl acrylate; (III) combinations thereof. [7] 2. The multilayer elastic film of any one of the preceding claims, wherein the first outer layer and the second outer layer each comprise at least 75 weight percent of the ethylene-based copolymer. [8] 4. The multilayer elastic film of any one of the preceding claims, wherein the first outer layer and the second outer layer each comprise 75-100 weight percent ethylene-based copolymer. [9] The ethylene-based copolymer of the first outer layer, the second outer layer, or both has a melt index (I 2 13. The multilayer elastic film of any one of the preceding claims, having a

[10] The ethylene-based copolymer of the first outer layer, the second outer layer, or both, is greater than 80 weight percent ethylene and from 7 to 11 weight percent α,β-ethylenically unsaturated C 3 -C 8 20. The multilayer elastic film of any one of the preceding claims, comprising a carboxylic acid.

[11] 2. The multilayer elastic film of any one of the preceding claims, wherein the ethylene-based copolymer of the first outer layer, the second outer layer, or both has 88 to 94 weight percent ethylene and 6 to 12 weight percent alkyl acrylate.

[12] 2. The multilayer elastic film of any one of the preceding claims, wherein the ethylene-based copolymer of the first outer layer, the second outer layer, or both, has a density from 0.920 g / cc to 0.950 g / cc.

[13] 13. The multilayer elastic film of any one of the preceding claims, wherein the multilayer elastic film comprises less than 1 wt. % of an anti-blocking or slip additive.

[14] 2. The multilayer elastic film of any one of the preceding claims, wherein the multilayer elastic film is a blown film or a cast film.

[15] 10. The multilayer elastic film of any one of the preceding claims, wherein the multilayer elastic film is a cast film, and the cast film has an unwind force of less than 1 N / 50 mm after 12 weeks at a length in the range of 10 m to 50 m.

Claims

1. 1. A multilayer elastic film comprising a core layer, a first outer layer, and a second outer layer, The core layer has a density of 0.850 g / cc to 0.890 g / cc and a melt index (I 2 % of an ethylene / alpha-olefin block copolymer having the first outer layer and the second outer layer each comprise at least 75 weight percent of an ethylene-based copolymer, the ethylene-based copolymer comprising: (I) More than 50% by weight of ethylene, 5 to 16% by weight of α,β-ethylenically unsaturated C 3 -C 8 a carboxylic acid, and optionally 0.5 to 10 wt. % of an alkyl acrylate; (II) 86 to 95% by weight of ethylene and 5 to 14% by weight of an alkyl acrylate; (III) combinations thereof.

2. The multilayer elastic film of claim 1 , wherein the ethylene / alpha-olefin block copolymer has a melting temperature of from 115°C to 125°C.

3. The ethylene / alpha-olefin block copolymer has a molecular weight distribution (MWD=M w / M n The multilayer elastic film of claim 1 or 2, wherein

4. The ethylene / alpha-olefin block copolymer I 2 The multilayer elastic film according to any one of claims 1 to 3, wherein the elastic modulus is 0.5 to 2.0 g / 10 min.

5. The multilayer elastic film of any one of claims 1 to 4, wherein the core layer comprises up to 100% by weight of the ethylene / alpha-olefin block copolymer.

6. 1. A multilayer elastic film comprising a core layer, a first outer layer, and a second outer layer, the core layer comprises at least 75% by weight of a propylene-based plastomer having a density of 0.860 g / cc to 0.900 g / cc and a melt flow rate (MFR) of 0.5 g / 10 min to 5.0 g / 10 min; the first outer layer and the second outer layer each comprise at least 75 weight percent of an ethylene-based copolymer, the ethylene-based copolymer comprising: (I) More than 50% by weight of ethylene, 5 to 16% by weight of α,β-ethylenically unsaturated C 3 -C 8 a carboxylic acid, and optionally 0.5 to 10 wt. % of an alkyl acrylate; (II) 86 to 95% by weight of ethylene and 5 to 14% by weight of an alkyl acrylate; (III) combinations thereof.

7. The multilayer elastic film of any one of claims 1 to 6, wherein the first outer layer and the second outer layer each comprise up to 100 weight percent ethylene-based copolymer.

8. The ethylene-based copolymer of the first outer layer, the second outer layer, or both has a melt index (I 2 The multilayer elastic film of any one of claims 1 to 7, wherein

9. The ethylene-based copolymer of the first outer layer, the second outer layer, or both, is greater than 80 weight percent ethylene and from 7 to 11 weight percent α,β-ethylenically unsaturated C 3 -C 8 The multilayer elastic film of any one of claims 1 to 8, comprising a carboxylic acid.

10. 10. The multilayer elastic film of any one of the preceding claims, wherein the ethylene-based copolymer of the first outer layer, the second outer layer, or both has 88 to 94 weight percent ethylene and 6 to 12 weight percent alkyl acrylate.

11. 11. The multilayer elastic film of any one of the preceding claims, wherein the ethylene-based copolymer of the first outer layer, the second outer layer, or both, has a density from 0.920 g / cc to 0.950 g / cc.

12. The multilayer elastic film of any one of claims 1 to 11, wherein the multilayer elastic film comprises less than 1 weight percent of an anti-blocking or slip additive.

13. The multilayer elastic film according to any one of claims 1 to 12, wherein the multilayer elastic film is a blown film or a cast film.

14. 14. The multilayer elastic film of any one of claims 1 to 13, wherein the multilayer elastic film is a cast film, and the cast film has an unwind force of less than 1 N / 50 mm after 12 weeks at a length ranging from 10 m to 50 m.

Citation Information

Patent Citations

  • Elastic laminate, method for producing same, and article using same

    JP2018523596A

  • Elastic structure

    JP2019126938A

  • Packaging Film

    JP2019501038A

  • Elastic laminate and article containing same

    US20170313034A1

  • Elastic laminate and article containing same

    US20170320300A1