Encapsulated antistatic composition and method for preparing same

Encapsulating antistatic agents in a silica-clay carrier addresses the short-term effectiveness of traditional agents by offering a controlled release mechanism for long-term antistatic performance, enhancing thermal stability and reducing costs.

JP7591567B2Active Publication Date: 2024-11-28AVIENT SWITZERLAND GMBH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022521132
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-11
Filing Date
2020-10-08
Publication Date
2024-11-28
Estimated Expiration
2040-10-08

AI Technical Summary

Technical Problem

Existing antistatic agents in plastics have short-term effectiveness due to migration to the surface and volatility, leading to temporary antistatic effects, and their long-lasting alternatives pose health and safety concerns and are expensive.

Method used

Encapsulating antistatic agents in a carrier mixture of silica and clay, which provides a controlled release mechanism for long-term antistatic performance, allowing higher loading percentages and maintaining effectiveness for up to seven years.

Benefits of technology

The encapsulated antistatic agent composition achieves a balance between temporary and permanent antistatic performance, providing effective static charge management with improved thermal stability and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591567000005
    Figure 0007591567000005
  • Figure 0007591567000001
    Figure 0007591567000001
  • Figure 0007591567000002
    Figure 0007591567000002
Patent Text Reader

Abstract

The present invention relates to an encapsulated antistatic agent composition and a method for preparing the same. The encapsulated antistatic agent composition of the present disclosure provides long-lasting antistatic effect in plastic products and is used in masterbatches. The encapsulated antistatic agent composition includes a carrier comprising a mixture of silica and clay, and an antistatic agent encapsulated in the carrier. Another object of the present invention is to provide an encapsulated antistatic agent composition having a higher loading of antistatic agent, up to 10-60%, preferably 25-55%, and most preferably 30-50%, due to the absorption capacity of the carrier.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THEINVENTION The present invention relates to an encapsulated antistatic agent composition. More specifically, the present invention relates to an encapsulated antistatic agent composition, wherein the antistatic agent is encapsulated in a carrier consisting of a mixture of silica and clay. Furthermore, the present invention relates to the production of a masterbatch (MB), the masterbatch comprising an encapsulated antistatic agent incorporated into the polymer matrix of the MB to overcome static electricity problems in plastic products. The present invention seeks to overcome the shortcomings of previously known antistatic agents. [Background technology]

[0002] 2. Background of the Invention Nowadays, plastics have replaced metals and become the material of choice because they are more flexible, lighter, better colorable and more cost effective (Harper C. A (1999), Amarasekera J (2005)). However, static electricity problems have a detrimental effect on the performance in use, mainly associated with plastic products, which poses challenges in the processing and transforming industries.

[0003] Antistatic agents are often incorporated into plastic products to overcome such problems. The function of an antistatic agent is to prevent the accumulation of static charge due to the transfer of electrons to the surface of a material. Antistatic agents reduce the tendency of a surface to accumulate a static charge (SR Hartshorn, SS Thind, in Comprehensive Heterocyclic Chemistry, 1984).

[0004] Non-ionic type antistatic agents have found the widest use due to their low cost and minimal effect on the mechanical properties of plastics. Ease of use is another favorable aspect of non-ionics. They can be mixed with the bulk of plastics before processing in masterbatch form, or applied as a coating to the surface of finished plastic articles as and when needed. However, the use of the non-ionics shows a short-lasting, temporary effect. Therefore, to overcome the above-mentioned drawbacks and extend the long-term antistatic effect, encapsulation technology would be a favorable solution.

[0005] Antistatic agents can be divided into ionic, amphoteric, and nonionic points. Ionic antistatic agents include cationic compounds (e.g., quaternary ammonium, phosphonium, or sulfonium salts) and anionic compounds (usually sodium salts of sulfonic, phosphoric, and carboxylic acids). Nonionic antistatic agents include esters (e.g., glycerol esters of fatty acids, ethoxylated tertiary amines, ethoxylated amides, and alkyl sulfonate esters). Many are FDA or EU approved. Nonionic antistatic agents are primarily used in polyolefins; glyceryl monostearate is used in many polypropylene injection molding applications at levels ranging from 0.05 to >1%. Loading levels depend on the resin processing temperature, the presence of other additives, and application requirements (e.g., transparency, printability, and FDA compliance) (Clive Maier, Teresa Calafut, in Polypropylene, 1998). They can be incorporated with other ingredients during the compounding stage or applied directly to a surface as an antistatic coating.

[0006] However, after incorporation, most of the antistatic agents have a tendency to rise to the surface and are washed off, and therefore are not available. Therefore, the duration for which the antistatic effect is maintained is very short.

[0007] CN 103709493 discloses a polymer composition, but the polymer is a combination of three different low density polyethylene (LDPE) polymers; MB contains additional inorganic materials. The above-mentioned components are fed into a high-speed blender, melted fully and uniformly after high-speed blending, then discharged, cooled, fully hardened, and then crushed and sieved to obtain the final product. The masterbatch and preparation method disclosed by this invention can be applied to the modification of plastic products in the plastic processing industry.

[0008] CN 104250403 discloses a composition, in which the MB contains, besides the polyethylene (PE) / polypropylene (PP) carrier and the antistatic agent, an anti-blocking agent (preferably 0.1-1 part, but silica as a mold release agent), an antioxidant, and one or more compound stabilizers. The masterbatch antistatic agent has good antistatic effect, lasting effect and good dust-proofing effect.

[0009] CN 106633392 discloses a composition, MB includes polypropylene (PP) carrier resin, polyamide (PA) resin particles, 10-15 parts of active aluminum oxide powder, 10-15% clay and further MgCl2, dispersant and coupling agent. The functional masterbatch has the advantage that PA resin particles, active aluminum oxide powder, clay and magnesium chloride are compounded, so that the wettability of the polypropylene product is improved by combining water through chemical or physical route, during which the excess charge generated in the polypropylene product is dispersed in a timely manner, so that the antistatic ability of the polypropylene material is improved.

[0010] CN 107556579 discloses a composition, MB includes 14-20% polyethylene (PE) polymer, 80-90% bentonite and further carbon black, PE wax, phosphate coupling agent and 3-5% stearic acid amide. According to the polyethylene antistatic agent filled masterbatch disclosed by this invention, tetradecylpyridinium bromide modified bentonite is adopted, and the compatibility between the modified bentonite and polyethylene is improved, so that the prepared filled masterbatch is easily dispersed in polyethylene, and the mechanical properties and antistatic agent properties of polyethylene are improved. JP 2000313875 discloses that the antistatic agent is (A) diethanolamide of C10-C14 fatty acid and (C) monoglyceride C10-C14 fatty acid; the carrier resin (B) is petaloid calcium silicate powder; and A / B and B / C are mixed together. As can be seen in the prior art, the encapsulation of antistatic agents in carriers consisting of a mixture of silica and clay is unknown. The prior art has therefore focused on the use of antistatic agents and on modifying the structure of the antistatic agent to improve its action. Long-lasting antistatic agents exist. However, the use of long-lasting antistatic agents has become a concern from a health and safety standpoint and is extremely expensive. Thus, there is a need to provide a cost-effective antistatic agent that can exhibit controlled release antistatic activity using a temporary antistatic agent. This can be achieved by encapsulating the temporary antistatic agent. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] PRC Patent Application Publication No. 103709493 [Patent Document 2] PRC Patent Application Publication No. 104250403 [Patent Document 3] PRC Patent Application Publication No. 106633392 [Patent Document 4] PRC Patent Application Publication No. 107556579 [Patent Document 5] Patent Application Publication No. 2000313875 [Non-patent literature]

[0012] [Non-Patent Document 1] Harper C. A (1999), Amarasekera J (2005) [Non-Patent Document 2] SR Hartshorn, SS Thind, in Comprehensive Heterocyclic Chemistry, 1984 Summary of the Invention [Means for solving the problem]

[0013] Object of the invention A primary object of the present invention is to provide an encapsulated antistatic composition.

[0014] Another object of the present invention is to provide an encapsulated antistatic agent composition having a higher loading of antistatic agent, due to the absorption capacity of the carrier, up to 10-60%, preferably 25-55% and most preferably 30-50%.

[0015] It is yet another object of the present invention to provide an encapsulated antistatic agent composition in which the silica and clay mixture carrier acts as a barrier to the antistatic agent resulting in slow release of the antistatic agent to the surface to achieve long term antistatic effect.

[0016] Yet another aspect of the present invention is to provide a masterbatch (MB) comprising an encapsulated antistatic agent that is fully incorporated into the polymer matrix of the MB.

[0017] Yet another aspect of the present invention is to provide an article, such as a film, sheet, extruded or injection molded article, which includes an encapsulated antistatic agent.

[0018] Summary of the Invention In one aspect, the present invention provides an encapsulated antistatic composition comprising: a) a carrier consisting of a mixture of silica and clay; and b) at least one antistatic agent encapsulated in said carrier; wherein the concentration of the carrier is in the range of 40-90%, preferably 45-75%, and most preferably 50-70%, and the antistatic agent is in the range of 10-60%, preferably 25-55%, and most preferably 30-50%, based on the total weight of the composition.

[0019] In another aspect of the invention, the antistatic agent is a glycerol ester or an ethoxylated amine ester or an ethoxylated amide or an alkyl sulfonate ester. The glycerol ester is glycerol monostearate. The glycerol stearate is a mixture of stearic acid, palmitic acid monoester and triglycerol (i.e., Atmer 129) or a blend of stearic acid, triglycerol monoester and 2,3-dihydroxypropyl laurate (i.e., Grinstead PGE 308). The ethoxylated amine is N,N-bis(2-hydroxyethyl)-C 12-18 -alkylamine.

[0020] In another aspect of the invention, the carrier has a concentration of clay as 50-90%, preferably 60-90% and most preferably 75-85%, based on the total weight of the composition.

[0021] In yet another aspect of the invention, the carrier has a silica to clay ratio of 1:10 to 10:1, preferably 1:5 to 5:1, and most preferably 1:3 to 3:1.

[0022] In one alternative aspect of the present invention, the clay is selected from the group consisting of natural clays including bentonite, montmorillonite, beidellite, saponite, hectorite, stevensite, kerolite-saponite, kerolite, talc, phyllosporin, attapulgite, sepiolite; mixtures of natural silica and bentonite; any modified clay; and any mixtures thereof.

[0023] In a further aspect of the invention, the clay comprises natural bentonite or sodium activated bentonite or a mixture comprising both.

[0024] In yet another aspect of the invention, the clay comprises natural bentonite or sodium activated bentonite having a cation exchange capacity in the range of 10 meq / 100g to 140 meq / 100g.

[0025] In another aspect of the invention, the clay comprises natural bentonite or sodium activated bentonite having a cation exchange capacity in the range of 20 to 130 meq / 100 g, preferably in the range of 30 to 120 meq / 100 g.

[0026] In one alternative aspect of the invention, the clay is 120m 2 / g, a total pore volume greater than 0.35 ml / g and a silicon content, calculated as SiO2, of at least 60 wt. %.

[0027] In yet another aspect of the invention, the clay has greater than 10% amorphous material as determined by quantitative X-ray diffraction analysis of the mineral phase of the clay material.

[0028] In yet another aspect of the invention, the silica is a precipitated silica.

[0029] In yet another aspect of the invention, the precipitated silica is a hydrophilic precipitated silica or a hydrophobic precipitated silica or a mixture of both.

[0030] In one aspect of the invention, the hydrophilic silica has a liquid carrying capacity, determined as the DOA absorption number, of at least 120 ml / 100 g, preferably at least 140 ml / 100 g, and most preferably at least 160 ml / 100 g of precipitated silica.

[0031] In another aspect of the invention, the hydrophilic silica has a particle size d50, determined by laser diffraction, of 4 to 300 μm, preferably 5 to 150 μm, most preferably 5 to 70 μm.

[0032] In yet another aspect of the invention, the hydrophobic silica has a particle size d50, determined by laser diffraction, of 2 to 50 μm, preferably 4 to 25 μm, most preferably 5 to 15 μm.

[0033] In one alternative aspect of the present invention, silica is used in an amount of 15% to 90%, preferably 25% to 85%, and most preferably 35% to 75%, based on the total weight of the composition.

[0034] In yet another aspect of the present invention, the encapsulated antistatic composition is used to form a masterbatch.

[0035] In another aspect of the invention, the invention provides a method for preparing a masterbatch of an encapsulated antistatic agent composition, wherein the encapsulated antistatic agent is expediently provided in the form of a masterbatch, and wherein the polymer is preferably a polyolefin into which the respective encapsulated antistatic agent is to be incorporated.

[0036] In one other aspect of the present invention, the produced masterbatch can be further converted into an article.

[0037] In yet other aspects of the invention, the article can be a film, sheet, extrusion or injection molded article. In yet another aspect of the invention, the encapsulated antistatic agent is subjected to a heat cycle at a temperature in the range of 100° C. to 250° C. during processing of the article. BRIEF DESCRIPTION OF THE ATTACHED DRAWINGS [Brief description of the drawings]

[0038] [Figure 1] FIG. 1 represents the TGA of the encapsulated antistatic sample and Grinsted PGE 308. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] Detailed Description of the Invention For purposes of the following detailed description, it should be understood that the present invention may assume various alternative variations and various sequences of steps, unless expressly specified to the contrary. Further, other than in any working examples or unless otherwise indicated, all numbers expressing amounts of ingredients used herein, for example, are to be understood as being modified in all instances by the term "about." Unless otherwise stated, all percentages set forth in this specification and the appended claims refer to weight percentages of the total composition.

[0040] Therefore, before describing the present invention in detail, it is to be understood that this invention is not limited to specifically exemplified process parameters, which may, of course, vary. It is also to be understood that the terminology used herein is for the purpose of describing particular embodiments of the invention only, and is not intended to limit the scope of the present invention in any way.

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0042] Weight percentages (wt% or %wt) herein are calculated based on the total weight of the composition, unless otherwise indicated.

[0043] It must be noted that as used in this specification and the appended claims, the singular forms "a," "an," and "the" include reference to the wind, unless the context clearly dictates otherwise.

[0044] The terms "preferred" and "preferably" refer to embodiments of the invention that may offer certain advantages, under certain circumstances, although other embodiments may be preferred, under the same or other circumstances.

[0045] Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.

[0046] As used herein, the terms "comprising," "including," "having," "containing," "involving," and the like, should be understood to be open-ended, i.e., including, but not limited to.

[0047] In one embodiment of the present invention, there is provided an antistatic composition, the composition comprising: a) a carrier consisting of a mixture of silica and clay; and b) at least one antistatic agent encapsulated in said carrier; wherein the concentration of the carrier is in the range of 40-90%, preferably 45-75%, most preferably 50-70%, and the concentration of the antistatic agent is in the range of 10-60%, preferably 25-55%, most preferably 30-50%, based on the total weight of the composition.

[0048] The masterbatch composition may comprise at least one encapsulated antistatic agent as an additive, where the additive present in the masterbatch has a higher concentration than it will have in the final article or final application. The concentration of the encapsulated antistatic agent in the masterbatch preferably ranges from 2 to 20% by weight, more preferably from 5 to 15% by weight (the % weight being in each case based on the total weight of the masterbatch).

[0049] In another embodiment, the antistatic agent is a glycerol ester or an ethoxylated amine or an ethoxylated amide or an alkyl sulfonate ester. The glycerol ester is glycerol monostearate. The antistatic agent is a mixture of stearic acid, palmitic acid monoester and triglycerol (i.e., Atmer 129) or a blend of stearic acid, triglycerol monoester and 2,3-dihydroxypropyl laurate (i.e., Grinsted PGE 308). The ethoxylated amine is N,N-bis(2-hydroxyethyl)-C 2H 2 O 4 O 5 O 6 O 7 O 8 O 9 O 10 O 11 O 12 O 13 O 14 O 15 O 16 O 17 O 18 O 19 O 20 O 21 O 22 O 23 O 24 O 25 O 30 O 35 O 46 O 47 O 58 O 59 O 60 O 61 O 62 O 63 O 64 O 65 O 76 O 65 O 87 O 66 O 67 O 68 O 69 O 78 O 79 O 80 O 81 O 82 O 84 O 85 O 85 O 86 O 87 O 88 O 88 O 89 O 90 O 91 O 92 O 93 O 94 O 95 O 96 O 97 O 98 O 9 ... 12-18 -alkylamine.

[0050] Atmer 129 is typically a mixture of stearic acid, palmitic acid monoester and triglycerol. Mostly, non-ionic surfactants are used to achieve the antistatic effect. The addition of actives plays a crucial role in bringing about the desired antistatic effect. However, the effect is still limited and not permanent.

[0051] Grinsted PGE 308 is a polyglycerol ester (a blend of stearic acid, monoester with triglycerol, and 2,3-dihydroxypropyl laurate) that acts as an antistatic agent and exhibits excellent thermal stability. It is completely free of amine and amide chemistry. This eliminates the risk of corrosive effects on polycarbonate stress cracking in the final application. It is compatible with polystyrene, polyamide, LDPE, LLDPE and HDPE and can be used in PE film, PE foam, electronic packaging and injection molding applications.

[0052] In another embodiment, the silica is selected from the group of precipitated silicas.

[0053] In one embodiment, the precipitated silica is hydrophilic precipitated silica, hydrophobic precipitated silica or a mixture of both. Precipitated silica is typically produced by precipitation of sodium silicate with mineral acids under neutral or slightly alkaline conditions. For final application, the precipitated silica filter cake is dried and ground.

[0054] In one embodiment, the silica is a hydrophilic precipitated silica.

[0055] The hydrophilic silica consists only of SiO2, does not exhibit any surface modification, and is wettable by water.

[0056] In a preferred embodiment of the invention, said hydrophilic silica has a particle size d50, determined by laser diffraction, of at least 4-300 μm, preferably at least 5-150 μm, most preferably at least 5-70 μm.

[0057] The precipitated silica is selected from the group consisting of: Sipernat® from Evonik Industries (登録商標) 22; Sipernat (登録商標) 22LS, Sipernat(登録商標) 22S、Sipernat (登録商標) 2200、Sipernat (登録商標) 25、Sipernat (登録商標) 33、Sipernat (登録商標) 50、Sipernat (登録商標) 50S、Sipernat (登録商標) 500LS、Sipernat (登録商標) 101M、Sipernat (登録商標) 120、Sipernat (登録商標) 160、Sipernat (登録商標) 186、Sipernat (登録商標) 218、Sipernat (登録商標) 266、Sipernat (登録商標) 268、Sipernat (登録商標) 288、Sipernat (登録商標) 298、Sipernat (登録商標) 303、Sipernat (登録商標) 306、Sipernat (登録商標) 310、Sipernat (登録商標) 320、Sipernat (登録商標) 320 DS、Sipernat (登録商標) 32s AP、Sipernat (登録商標) 32s C、Sipernat (登録商標) 340、Sipernat (登録商標) 350、Sipernat (登録商標) 360、Sipernat (登録商標) 622 S、Sipernat (登録商標) 622 LS、Sipernat (登録商標) 62s、Sipernat (登録商標) 680、Sipernat (登録商標) BG-2、Sipernat (登録商標) FPS-5、Sipernat (登録商標) FPS-1、Sipernat (登録商標) 11 PC、Sipernat (登録商標) 22 PC、Sipernat (登録商標) 2200 PC、Sipernat (登録商標) 44 MS、Sipernat (登録商標) 820A、Sipernat (登録商標)880, Sipernat (登録商標) D10, Sipernat (登録商標) D 13, Sipernat (登録商標) D 17, Ibersil by IGE Group (登録商標) D100, Ibersil (登録商標) D100P or Ibersil (登録商標) D 250, Flo-Gard by PPG (登録商標) SC-72, Flo-Gard (登録商標) LPC. The precipitated silica of the formulation of the present invention is suitably characterized by a high liquid absorption capacity, determined as DOA absorption number, of at least 120 ml / 100 g, preferably at least 140 ml / 100 g, most preferably at least 160 ml / 100 g precipitated silica. DOA is the abbreviation for di-(2-ethylhexyl) adipate (CAS number 103-23-1). The test method is based on ISO 19246 ("Rubber compounding ingredients- Silica - Oil absorption of precipitated silica").

[0058] Hydrophobic silica is not wetted by water and exhibits an organic surface modification caused by chemical reaction with reactive alkylsilanes. The presence of such surface modification can be demonstrated by various analytical methods (e.g. carbon content in elemental analyzer according to ISO 3262-19). In one embodiment, the precipitated silica or one of the precipitated silicas used in the formulation has a hydrophobic surface.

[0059] The hydrophobic precipitated silica for the formulations of the present invention is suitably characterized by a particle size d50, determined by laser diffraction (laser diffraction according to ISO 13320), of at least 42-50 μm, preferably at least 4-25 μm, most preferably at least 5-15 μm.

[0060] In one embodiment, the hydrophobic silica is Sipernat® D17 (d50 about 10 microns) or Sipernat (登録商標)D 13 (particle size -d50 approx. 10.5 microns) or Sipernat® D10 (particle size -d50 approx. 6.5 microns, free flowing) or Sipernat® (登録商標) 44 MS (particle size -d50 approx. 3 microns) or Sipernat (登録商標) 820 A (grain size -d50 approx. 7 microns) or Sipernat (登録商標) 880 (particle size -d50 approximately 8.5 microns) or a combination of these.

[0061] As used herein, the term "clay" refers to both natural clays and modified clays. Modified clays, in this context, refer to natural clays that have been alkali-activated or acid-activated. As used herein, the terms "clay mineral" or "special clay mineral" refer to natural clays.

[0062] In one embodiment, the clay used in the composition of the present invention is selected from the group consisting of natural clays including bentonite, montmorillonite, beidellite, saponite, hectorite, stevensite, kerolite-saponite, kerolite, talc, phyllosporin, attapulgite, sepiolite; mixtures of natural silica and bentonite; any modified clay; and any mixtures thereof.

[0063] In one embodiment, the clay is bentonite.

[0064] In another embodiment, the antistatic agent used is 10-60%, preferably 25-55% and most preferably 30-50% based on the total weight of the composition.

[0065] In yet another embodiment, the silica is used in an amount of 15% to 90%, preferably 25% to 85%, and most preferably 35% to 75%, based on the total weight of the encapsulated antistatic agent composition.

[0066] In another embodiment, the clay is used in an amount of 50% to 90%, preferably 60% to 90%, and most preferably 75% to 85%, based on the total weight of the encapsulated antistatic agent composition.

[0067] In one embodiment, the carrier has a silica to clay ratio concentration of 1:10 to 10:1, preferably 1:5 to 5:1 and most preferably 1:3 to 3:1.

[0068] Smectite clays such as bentonite, beidellite, saponite, hectorite, stevensite, kerolite-saponite are used in their natural Ca form or in soda activated form.

[0069] In another embodiment, natural sodium bentonite is used as the clay. A particularly preferred clay is montmorillonite in its natural form or in its sodium compound activated form or mixtures thereof.

[0070] In one embodiment, the clay used is bentonite having a cation exchange capacity in the range of 10 meq / 100g to 140 meq / 100g.

[0071] In one embodiment, the clay used is bentonite having a cation exchange capacity ranging between 20 meq / 100g and 130 meq / 100g, preferably between 30 meq / 100g and 120 meq / 100g.

[0072] In another embodiment, the present invention provides a method for preparing a masterbatch of an encapsulated antistatic agent and a resin composition, wherein the encapsulated antistatic agent is expediently provided in the form of a masterbatch, and wherein the polymer is preferably a polyolefin into which the respective encapsulated antistatic agent is to be incorporated.

[0073] In a preferred embodiment, the polymer includes polyolefins and polyolefin copolymers selected from the group consisting of polyethylene (PE), preferably high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), metallocene low density polyethylene (mLDPE) and metallocene linear low density polyethylene (mLLDPE), polypropylene (PP), preferably polypropylene homopolymer (PPH), polypropylene random copolymer (PP-R) and polypropylene block copolymer (PP-Block-COPO), PE copolymers, preferably ethylene-vinyl acetate copolymer (EVA), ethylene and methyl acrylate copolymer (EMA), ethylene and butyl acrylate copolymer (EBA), ethylene and ethyl acrylate copolymer (EEA), and cycloolefin copolymer (COC), general purpose polystyrene (GPPS) and high impact polystyrene (HIPS).

[0074] The masterbatches may be prepared by conventional physical mixing processes.

[0075] The mixing equipment for the use of solid master batch MB can be mixer, extruder, kneader, press, mill, calendar, blender, injection molding machine, injection and stretch blow molding machine (ISBM), extrusion blow molding machine (EBM), compression molding machine, compression and stretch blow molding machine; more preferably mixer, extruder, injection molding machine, injection and stretch blow molding machine, compression molding machine, compression and stretch blow molding machine; even more preferably mixer, extruder, injection and stretch blow molding machine and extrusion blow molding machine.

[0076] The extruder may be equipped with a metering system for introducing the additives and / or masterbatches into the main stream polymer. This metering may be done directly with one or more pure components or with one or more masterbatches.

[0077] The type of metering device used depends on the form in which the pure components or the masterbatch are metered.

[0078] For the solid components, a feed screw type metering device is usually used and the introduction point can be the main inlet of the extruder in conjunction with the main polymer granules feed or in a non-pressurized injection zone located along the extruder. For solid masterbatches, the metering device can be a system including a further extruder that pre-melts the masterbatch, pressurizes it and meters it by means of a metering pump, the amount of masterbatch to be metered being fed, advantageously without pressure, at a point along the main extruder.

[0079] In one embodiment, the encapsulated antistatic composition may be in powder or granule form.

[0080] The antistatic effect of glycerol ester is not permanent. It is well understood that antistatic agents migrate to the surface during processing and sometimes become volatile. As a result, the effect is temporary. Therefore, it is necessary and essential to form a protective shield, since this protects the active agent. The unique method of preparing an encapsulated antistatic agent formulation is to support a long-lasting effect. The release of the antistatic agent can be modified using a combination of inorganic absorbers, so that there is a controlled release of the active agent to the surface that is available for a long period of time.

[0081] Patent CN 104250403 discloses the use of release and antiblocking agents at 0.1-1 parts, with the highest loading of antistatic agent being only 35%. The present invention offers the advantage of using silica and clay mixtures as absorbents. If only silica is used, a higher loading percentage of antistatic agent is possible (40-60%). However, the antistatic agent is trapped in the matrix and its release to the surface is more rapid when silica is used as carrier. The antistatic agent is immobilized as a film or liquid or liquid droplets. Furthermore, silica is macroporous and the release from the carrier to the polymer depends on the mobility of the active ingredient in the polymer and the interaction of the active ingredient with the carrier. Surprisingly, it has been found that silica in combination with another inorganic material such as clay has the advantage of releasing the active ingredient in a controllable manner due to the intercalation and adsorption properties of the clay. The clay acts as a carrier for the liquids by absorbing them into the pores and between the sheets. Surprisingly, this provides a delayed release of the active agent.

[0082] The present invention provides an antistatic agent absorbed on a silica and clay composition, wherein the antistatic agent is fully incorporated on a porous hydrophilic mixture of silica and clay. The procedure of melting the antistatic agent at a desired temperature is carried out under the same temperature conditions of the silica and clay mixture mentioned, enhancing the penetration of the active substance into the porous walls of the silica and clay mixture. The concentration of the antistatic agent is preferably 10%-60%, preferably 25%-55%, most preferably 30%-50%.

[0083] The present invention also provides an encapsulation composition wherein the absorbent can be a combination of silica and clay with percentages ranging from 40-90%, preferably 45-75%, and most preferably 50-70%, or clay with percentages ranging from 50-90%, preferably 60-90% and most preferably 75-85%.

[0084] The present invention also provides the advantage of creating a non-existent product category that bridges the gap between temporary and permanent antistatic performance. Temporary antistatic performance exists for up to one year, while permanent antistatic lasts longer than seven years, which makes them expensive. Creating a new product range bridges the gap between temporary and permanent antistatic performance.

[0085] The use of examples anywhere in this specification, including examples of any term discussed herein, is illustrative only and in no way limits the scope and meaning of the invention or of any exemplified term. Similarly, the invention is not limited to the various embodiments shown in this specification. EXAMPLES

[0086] Working Example The following examples are offered by way of illustration only, and therefore should not be construed as limiting the scope of the present invention.

[0087] Preparation Example-1 The materials shown below are used to prepare an encapsulated antistatic agent surrounding Grinsted PGE 308 as the active agent. [Table 1]

[0088] To prepare the encapsulated antistatic agent, the silica is first introduced and its temperature is set above the melting point of Grinsted PGE 308. Grinsted PGE 308 is slowly added to the silica, allowing the antistatic agent to be absorbed onto the silica, resulting in the formation of an encapsulated antistatic agent.

[0089] Preparation Example-2 The materials shown below are used to prepare encapsulated antistatic agents surrounding Atmer 129 or Grinsted PGE 308 as the active material. [Table 2]

[0090] The clay powder used, Laundrosil DGA, exhibits a cation exchange capacity of 75 meq / 100 g, determined by the ammonium chloride method (method as described in EP2040562B1).

[0091] To prepare the encapsulated antistatic agent, the silica and clay are first introduced and the temperature is set higher than the melting point of the antistatic agent. The antistatic agent is slowly added to the silica and clay, allowing the antistatic agent to be absorbed onto the silica and clay mixture, resulting in the formation of the encapsulated antistatic agent.

[0092] The TGA results in Figure 1 show that Grinsted PGE 308 begins to decompose at 210°C, with a percentage loss of active substance of 36.24% at 350°C, whereas it was observed that there is an improvement in the thermal stability of Grinsted PGE 308 when encapsulated using Sipernat 22 (1d), with a percentage loss of active substance found to be 26.21%. Surprisingly, there is even an improvement in the thermal stability of Grinsted PGE 308 when encapsulated using silica and clay mixtures compared to Grinsted PGE 308 encapsulated with silica alone (2b, 2d and 2f). The percentage loss of active substance was found to be 22.76%, 20.175% and 23.92% for 2b, 2d and 2f, respectively.

[0093] Preparation Example 3 The materials shown below are used to prepare encapsulated antistatic agents surrounding Atmer 129 or Grinsted PGE 308 as the active material. [Table 3]

[0094] To prepare the encapsulated antistatic agents, the clay is first introduced, the temperature is set above the melting point of the antistatic agents, and the antistatic agents are slowly added, allowing them to be absorbed onto the clay, resulting in the formation of the encapsulated antistatic agents.

[0095] Preparation Example-4 The materials shown below are used to prepare encapsulated antistatic agents surrounding Atmer 129 or Grinsted PGE 308 as the active material. [Table 4]

[0096] To prepare the encapsulated antistatic agent, the Sipernat D 10 is first introduced and the temperature is set above the melting point of the antistatic agent. The antistatic agents are added slowly, allowing them to be absorbed onto the Sipernat D 10, resulting in the formation of the encapsulated antistatic agent. For example, the present invention provides the following: (Item 1) 1. An encapsulated antistatic composition, comprising: a) a carrier consisting of a mixture of silica and clay; and b) at least one antistatic agent encapsulated in said carrier; Including, wherein the concentration of the carrier is in the range of 40-90%, preferably 45-75%, and most preferably 50-70%, and the concentration of the antistatic agent is in the range of 10-60%, preferably 25-55%, and most preferably 30-50%, based on the total weight of the composition. (Item 2) 2. The composition of claim 1, wherein the antistatic agent is a glycerol ester. (Item 3) 3. The composition of claim 2, wherein the glycerol ester is glycerol monostearate. (Item 4) The composition according to any of the preceding items, wherein the antistatic agent is a mixture of stearic acid, palmitic acid monoester and triglycerol, or a blend of stearic acid, a monoester of triglycerol and 2,3-dihydroxypropyl laurate. (Item 5) The composition according to any of the preceding items, wherein the carrier has a concentration of clay of 50-90%, based on the total weight of the composition. (Item 6) The composition of any of the preceding items, wherein the carrier has a ratio of silica to clay of 1:10 to 10:1. (Item 7) The composition of any of the preceding items, wherein the clay is selected from the group consisting of natural clays including bentonite, montmorillonite, beidellite, saponite, hectorite, stevensite, kerolite-saponite, kerolite, talc, phyllosporin, attapulgite, sepiolite; mixtures of natural silica and bentonite; any modified clay; and any mixtures thereof. (Item 8) The composition of any of the preceding items, wherein the clay comprises natural bentonite or sodium activated bentonite or a mixture comprising both. (Item 9) The composition according to any of the preceding items, wherein the clay comprises natural bentonite or sodium activated bentonite having a cation exchange capacity in the range of 10 meq / 100 g to 140 meq / 100 g, preferably in the range of 20 to 130 meq / 100 g, particularly preferably in the range of 30 to 120 meq / 100 g. (Item 10) Item 2. The composition of any of the preceding items, wherein the silica is a precipitated silica. (Item 11) 11. The composition according to item 10, wherein the precipitated silica is a hydrophilic precipitated silica or a hydrophobic precipitated silica or a mixture of both. (Item 12) 12. The composition according to item 11, wherein said hydrophilic silica has a liquid carrying capacity, determined as the DOA absorption number of the precipitated silica, of at least 120 ml / 100 g, preferably at least 140 ml / 100 g, most preferably at least 160 ml / 100 g. (Item 13) 13. The composition according to item 11 or item 12, wherein the hydrophilic silica has a particle size d50 determined by laser diffraction of 4 to 300 μm, preferably of 5 to 150 μm, most preferably of 5 to 70 μm. (Item 14) 14. The composition according to any of items 11 to 13, wherein the hydrophobic silica has a particle size d50 determined by laser diffraction of 2 to 50 μm, preferably 4 to 25 μm and most preferably 5 to 15 μm. (Item 15) The composition according to any of the preceding items, wherein the silica is used in an amount of 15% to 90%, preferably 25% to 85%, and most preferably 35% to 75%, based on the total weight of the composition. (Item 16) A process for preparing a masterbatch of an encapsulated antistatic agent composition, preferably an encapsulated antistatic agent composition as described in any of the preceding paragraphs, wherein the encapsulated antistatic agent is expediently provided in the form of a masterbatch, and wherein the polymer is preferably a polyolefin into which the respective encapsulated antistatic agent is to be incorporated. (Item 17) The composition of any of the preceding items when used in a masterbatch. (Item 18) The composition according to any of the preceding items when used in a masterbatch for a polymer. (Item 19) 17. The masterbatch according to item 16, comprising an encapsulated antistatic agent composition, wherein said encapsulated antistatic agent is subjected to a heating cycle at a temperature in the range of 100° C. to 250° C. during processing of an article.

Claims

1. 1. An encapsulated antistatic composition, comprising: a) a carrier consisting of a mixture of silica and clay; and b) at least one antistatic agent encapsulated in said carrier; Including, wherein the concentration of the carrier is in the range of 40 to 90%, and the concentration of the at least one antistatic agent is in the range of 10 to 60%, based on the total weight of the composition; wherein the clay is selected from the group consisting of natural clays including bentonite, montmorillonite, beidellite, saponite, hectorite, stevensite, kerolite-saponite, kerolite, talc, phyllosporin, attapulgite, sepiolite; mixtures of natural silica and bentonite; modified clays; and mixtures of any of the foregoing; and wherein the modified clay is the natural clay which has been alkali-activated or acid-activated. composition.

2. The composition of claim 1 , wherein the antistatic agent is a glycerol ester.

3. The composition of claim 2 , wherein the glycerol ester is glycerol monostearate.

4. The composition according to any one of claims 1 to 3, wherein the antistatic agent is a mixture of stearic acid, palmitic acid monoester and triglycerol, or a blend of stearic acid, a monoester with triglycerol and 2,3-dihydroxypropyl laurate.

5. The composition of any one of claims 1 to 4, wherein the carrier has a concentration of clay as 50 to 90%, based on the total weight of the composition.

6. The composition of any one of claims 1 to 5, wherein the carrier has a silica to clay ratio of from 1:10 to 10:

1.

7. The composition of any one of claims 1 to 6, wherein the clay comprises natural bentonite or sodium activated bentonite or a mixture comprising both.

8. 8. The composition of claim 1, wherein the clay comprises natural bentonite or sodium activated bentonite having a cation exchange capacity in the range of 10 meq / 100g to 140 meq / 100g.

9. A composition according to any one of the preceding claims, wherein the silica is a precipitated silica.

10. 10. The composition of claim 9, wherein the precipitated silica is a hydrophilic precipitated silica or a hydrophobic precipitated silica or a mixture of both.

11. 11. The composition of claim 10, wherein the hydrophilic silica has a liquid carrying capacity determined as a DOA absorption number of at least 120 ml / 100 g of precipitated silica.

12. The composition according to claim 10 or claim 11, wherein the hydrophilic silica has a particle size d50, determined by laser diffraction, of 4 to 300 μm.

13. 13. The composition according to any of claims 10 to 12, wherein the hydrophobic silica has a particle size d50, determined by laser diffraction, of 2 to 50 μm.

14. The composition according to any one of claims 1 to 13, wherein the silica is used in an amount of from 15% to 90% based on the total weight of the composition.

15. 15. A method for preparing a masterbatch of an encapsulated antistatic agent composition according to any one of claims 1 to 14, wherein the encapsulated antistatic agent is expediently provided in the form of a masterbatch.

16. A masterbatch comprising the composition according to any one of claims 1 to 14.

17. A masterbatch for a polymer comprising the composition according to any one of claims 1 to 14.

18. 16. The method of claim 15, wherein the encapsulated antistatic agent is subjected to a heat cycle at a temperature in the range of 100° C. to 250° C. during processing of the article.

Citation Information

Patent Citations

  • High-concentration anti-static master batch for polyolefin and preparation method thereof

    CN103709493A

  • Antistatic masterbatch

    CN104250403A

  • Functional master batch capable of improving antistatic property of polypropylene

    CN106633392A

  • Polyethylene antistatic filling master batch and preparation method thereof

    CN107556579A

  • Powdered antistatic agent composition

    JP1992258649A