Protective coating and method of making same

Plasma-polymerized coatings with alicyclic epoxy structural units address the issues of poor binding and environmental toxicity in fluoropolymer coatings by forming dense, rigid structures with strong substrate adhesion and improved corrosion resistance.

JP7591587B2Active Publication Date: 2024-11-28JIANGSU FAVORED NANOTECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022575847
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-09
Filing Date
2021-05-20
Publication Date
2024-11-28
Estimated Expiration
2041-05-20

AI Technical Summary

Technical Problem

Existing plasma-polymerized coatings, particularly those using fluoropolymers, suffer from poor binding strength to substrates and can release toxic substances, posing environmental concerns and inadequate protection performance.

Method used

Development of plasma-polymerized coatings using monomers with alicyclic epoxy structural units, such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, to form dense and rigid molecular structures with high bonding strength to substrates, enhancing corrosion resistance and environmental safety.

Benefits of technology

The coatings exhibit superior bonding strength and corrosion protection, outperforming fluoropolymer-based coatings without releasing harmful substances, thus meeting environmental regulations and providing enhanced protective performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591587000001
    Figure 0007591587000001
  • Figure 0007591587000002
    Figure 0007591587000002
  • Figure 0007591587000003
    Figure 0007591587000003
Patent Text Reader

Abstract

A specific embodiment of the present invention provides a protective coating, which comprises forming a plasma polymerized coating of a monomer having an alicyclic epoxy structural unit to form a corrosion-protective layer with a tightly packed rigid molecular structure, and forming a hydrophobic coating by plasma polymerization on the plasma polymerized coating of the monomer having an alicyclic epoxy structural unit, thereby forming a coating with excellent protective performance for the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

cross reference

[0001] This application is This is a national phase application of International Application No. PCT / CN2021 / 094737 filed on May 20, 2021. Priority is claimed based on application number 202010526322.5, filed on June 9, 2020 with the China Patent Office, entitled "Protective Coating and Manufacturing Method Thereof," and on application number 202010526684.4, filed on June 9, 2020 with the China Patent Office, entitled "Protective Coating and Manufacturing Method Thereof," the entire contents of which are incorporated herein by reference. [Technical field]

[0002] The present invention is in the field of plasma chemistry, and more particularly, relates to plasma polymerized protective coatings and methods for their manufacture. [Background technology]

[0003] Organic polymer coatings can effectively protect the surfaces of various materials. Among the methods of organic polymer coating, the vapor deposition method for producing polymer protective coatings on the surface of a substrate is the mainstream method, which has the characteristics of being economical, applicable, easy to operate, etc. In particular, plasma chemical vapor deposition uses plasma to activate reactive monomer gases and deposit them on the surface of a substrate. This method is suitable for various substrates, the grown polymer protective coatings are uniform, the coating preparation temperature is low, the coating thickness is thin, the stress is small, there is little damage to the surface of the substrate, and there is little impact on the substrate performance.

[0004] Traditionally, the selection of plasma polymerization monomers has been one of the important research topics in plasma polymerization coating, for example, using organosiloxane as a monomer to prepare plasma polymerization coating, and using a mixture of monofunctional unsaturated fluorocarbon resin and polyfunctional unsaturated hydrocarbon derivative as a monomer to prepare plasma coating, so that the coating forms a dense mesh structure to protect the metal. Summary of the Invention

[0005] A specific embodiment of the present invention is to provide a protective coating formed by a novel plasma polymerized monomer and a method for producing the same, the specific scheme is as follows:

[0006] Protective Coating II, a plasma polymerized coating formed on a surface of a substrate by contacting the substrate with a plasma, the plasma comprising a plasma of monomer α, the monomer α comprising a cycloaliphatic epoxy structural unit as shown in Formula (1). TIFF0007591587000001.tif26161 (wherein A is a 3-20 membered alicyclic structure.)

[0007] Optionally, said A is a 5-membered alicyclic structure or a 6-membered alicyclic structure.

[0008] Optionally, the monomer α further comprises at least one of a carbon-carbon double bond structural unit, a carbon-carbon triple bond structural unit, or an epoxy structural unit.

[0009] Optionally, the monomer a has the structure shown in formula (2): TIFF0007591587000002.tif39161 (wherein R1, R2 and R3 each independently represent a hydrogen atom, C1 to C 10 or C1-C 10 A halogen atom-substituted alkyl group is selected from the group consisting of: R4 is a bond, C1~C 10 or an alkylene group of C1 to C 10 It is a halogen atom-substituted alkylene group.

[0010] Optionally, R1, R2, and R3 are each independently selected from a hydrogen atom or a methyl group; and R4 is a bond, a methylene group, or an ethylene group.

[0011] Optionally, the monomer α has a structure shown in Formula (3) or Formula (4). TIFF0007591587000003.tif26161

[0012] Optionally, the monomer a has the structure shown in formula (5): TIFF0007591587000004.tif23161 (where R5 is a bond, C1 to C 10 or an alkylene group of C1 to C 10 is a halogen atom-substituted alkylene group; R6 is TIFF0007591587000005.tif1243.)

[0013] Optionally, the monomer α has a structure shown in formula (6) or formula (7). TIFF0007591587000006.tif25161

[0014] Optionally, the monomer a has the structure shown in formula (8): TIFF0007591587000007.tif24160 (wherein R7 and R9 each independently represent a bond, C1 to C 10 or an alkylene group of C1 to C 10 halogen atom-substituted alkylene groups; R8 is C1~C 10 or an alkylene group of C1 to C 10 is a halogen atom-substituted alkylene group; X and Y are each independently selected from a bond, an oxygen atom, a carbonyl group, or an ester group.

[0015] Optionally, the monomer α has a structure shown in formula (9) or formula (10). TIFF0007591587000008.tif31160

[0016] Optionally, the plasma further comprises a plasma of monomer β, the monomer β comprising structural unit a; The structural unit a has a structure represented by formula (11). TIFF0007591587000009.tif36161 (where R 10 , R 11 and R 12 are each independently a hydrogen atom, C1 to C 10 or C1-C 10 The halogen atom-substituted alkyl group is selected from the group consisting of:

[0017] Optionally, the monomer β further comprises a structural unit b, the structural unit b comprising at least one of a double bond structural unit, a triple bond structural unit, or an epoxy structural unit.

[0018] Optionally, the structural unit b has a structure shown in formula (12): TIFF0007591587000010.tif32161 (where R 13 , R 14 and R 15 are each independently a hydrogen atom, C1 to C 10 or C1-C 10 The halogen atom-substituted alkyl group is selected from the group consisting of:

[0019] Optionally, the monomer β has the structure shown in formula (13): TIFF0007591587000011.tif32160 (where R 16 is C2~C 10 or an alkylene group of C2 to C 10 and n is an integer of 1 to 10.

[0020] Optionally, said R 10 , R 11 , R 12 , R 13 , R 14 and R 15 are each independently selected from a hydrogen atom or a methyl group.

[0021] Optionally, the substrate is a metal, plastic, textile, glass, electrical component, optical device, or electrical component.

[0022] A method for producing a protective coating II according to any one of the above, comprising the steps of: Providing a substrate; and forming a plasma polymerized coating on a surface of the substrate by contacting the substrate with the plasma.

[0023] Optionally, the plasma is a pulsed excited plasma.

[0024] Optionally, the pulse frequency of the pulse method is 20Hz to 80KHz, the duty ratio is 1‰ to 80%, and the average pulse power density is 0.001W / m 3 ~500W / m 3 It is.

[0025] A device, at least a portion of whose surface has a protective coating II according to any one of the preceding claims.

[0026] A protective coating comprising Coating I and Coating II grown on a substrate, said coating II being a protective coating II according to any one of the preceding claims; said coating I being a plasma polymerized coating formed on coating II by contacting said coating II with a plasma containing monomer γ; A protective coating, wherein the monomer γ is selected from one or more of an alkane, a halogenated alkane, an alkene, a halogenated alkene, an alkyne, a halogenated alkyne, an acrylate, or a halogenated acrylate.

[0027] Optionally, the monomer γ has the structure shown in formula (14): TIFF0007591587000012.tif38161 (where R 17 , R 18 and R 19 are each independently a hydrogen atom, C1 to C 10or C1-C 10 A halogen atom-substituted alkyl group is selected from the group consisting of: R 20 is C1~C 20 or a hydrocarbon group of C1 to C 20 is a halogen atom-substituted hydrocarbon group.

[0028] Optionally, said R 17 , R 18 and R 19 are each independently selected from a hydrogen atom or a methyl group; 20 is C4~C 20 or C4-C 20 is a halogen atom-substituted hydrocarbon group.

[0029] Optionally, the monomer γ has the structure shown in formula (15): TIFF0007591587000013.tif35161 (where R 21 is a bond, C1~C 10 or an alkylene group of C1 to C 10 is a halogen atom-substituted alkylene group; B is an aromatic ring structure or a 3- to 20-membered alicyclic structure.

[0030] Optionally, said R 21 is a bond, a methylene group or an ethylene group, and B is a cyclohexyl group or a cyclopentyl group.

[0031] Optionally, the coating further comprises a coating III that is a plasma polymerized coating formed by contacting the substrate with a plasma comprising monomer δ; said coating II being a plasma polymerized coating formed on coating III by contacting said coating III with a plasma comprising monomer α; The monomer δ includes a structural unit c and a structural unit d, and the structural unit c and the structural unit d each have a carbon-carbon double bond structure and an ester group structure.

[0032] Optionally, the structural unit c has a structure shown in formula (16): TIFF0007591587000014.tif43161 (where R 22 , R 23 and R 24 are each independently a hydrogen atom, C1 to C 10 or C1-C 10 The halogen atom-substituted alkyl group is selected from the group consisting of:

[0033] Optionally, the structural unit d has a structure shown in formula (17): TIFF0007591587000015.tif35160 (where R 25 , R 26 and R 27 are each independently a hydrogen atom, C1 to C 10 or C1-C 10 The halogen atom-substituted alkyl group is selected from the group consisting of:

[0034] Optionally, the monomer δ has the structure shown in formula (18): TIFF0007591587000016.tif38161 (where R 28 is C2~C 10 or an alkylene group of C2 to C 10 where n is an integer of 0 to 10, and R 22 , R 23 , R 24 , R 25 , R 26 and R 27 are each independently a hydrogen atom, C1 to C 10 or C1-C 10 The halogen atom-substituted alkyl group is selected from the group consisting of:

[0035] Optionally, said R 22 , R 23 , R 24 , R 25 , R 26 and R 27 are each independently selected from a hydrogen atom or a methyl group.

[0036] A method for producing a protective coating according to any one of the above, comprising the steps of: Providing a substrate; and forming said protective coating on a substrate as a plasma deposited coating.

[0037] Optionally, the plasma is a pulsed plasma.

[0038] Optionally, the pulsed plasma is generated by applying a pulsed voltage discharge, with a pulsed power of 20-500W, a pulse frequency of 20Hz-80KHz, a pulse duty ratio of 1‰-80%, and a plasma discharge time of 100s-20000s.

[0039] A device, at least a portion of whose surface has a protective coating according to any one of the preceding claims.

[0040] The protective coating II of a specific embodiment of the present invention is a plasma polymerization coating with a monomer having an alicyclic epoxy structural unit, which can form a dense rigid molecular structure and improve the protective performance of the coating. Furthermore, the monomer bond of the alicyclic epoxy structural unit has a multifunctional group site, especially a multifunctional monomer containing an acrylate structure, which forms multiple active sites under plasma discharge and crosslinks to form a dense network structure, which has a strong bond with the substrate, especially metal, and improves the corrosion resistance of the metal.

[0041] In a specific embodiment of the protective coating of the present invention, a monomer having an alicyclic epoxy structural unit is plasma polymerized to form a corrosion-resistant layer with a dense rigid molecular structure, and a hydrophobic coating is formed on the plasma polymerized coating of the monomer having an alicyclic epoxy structural unit by plasma polymerization, thereby forming a coating with excellent protective performance for the substrate; furthermore, when the plasma monomer of the hydrophobic coating adopts a monomer having an alicyclic epoxy structural unit, the hydrophobic layer adheres closely to the corrosion-resistant layer, and has better protective performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] In a specific embodiment of the present invention, protective coating II is a plasma polymerized coating formed on a surface of a substrate by contacting the substrate with a plasma, the plasma comprising a plasma of monomer α, the monomer α comprising a cycloaliphatic epoxy structural unit as shown in formula (1). TIFF0007591587000017.tif25161 (wherein A is a 3-20 membered alicyclic structure.)

[0043] In some specific embodiments of the protective coating II of the present invention, the alicyclic ring has one or more substituents, which may be, for example, an alkyl substituent such as a methyl group, an ethyl group, a propyl group, a butyl group, or a halogen atom substituent such as fluorine or chlorine, or a halogen atom substituted alkyl substituent such as a fluorine-substituted methyl group, a chlorine-substituted methyl group, a fluorine-substituted ethyl group, a chlorine-substituted ethyl group, a fluorine-substituted propyl group, a chlorine-substituted propyl group, a fluorine-substituted butyl group, or a chlorine-substituted butyl group.

[0044] In some specific embodiments of the protective coating II of the present invention, A is a 5-membered alicyclic structure or a 6-membered alicyclic structure, such alicyclic rings being more stable in their rigid structure.

[0045] In the protective coating II of a specific embodiment of the present invention, the monomer α further comprises at least one of a carbon-carbon double bond structural unit, a carbon-carbon triple bond structural unit, or an epoxy structural unit, which forms a plurality of active sites to facilitate crosslinking and forming a dense network structure. For example, the monomer α may be 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 3,4-epoxycyclohexylmethylmethacrylate, 3,4-epoxycyclohexylmethylacrylate, 1,2-epoxy-4-vinylcyclohexyl. and the like, and in some specific embodiments, the monomer α may be one or more of: cyclohexane, bis(2,3-epoxycyclopentyl)ether, 2,3-epoxycyclopentyl cyclopentyl ether, vinylcyclohexene diepoxide, diisoprene diepoxide, bis((3,4-epoxycyclohexyl)methyl)adipate, 3,4 epoxy-6-methylcyclohexylcarboxylic acid-3',4'-epoxy-6'-methylcyclohexylmethyl ester, or dicyclopentadiene diepoxide, and in some specific embodiments, the monomer α has the structure shown in formula (2): TIFF0007591587000018.tif40160

[0046] Here, R1, R2 and R3 each independently represent a hydrogen atom, C1 to C 10 or C1-C 10 R4 is a bond, C1 to C 10 or an alkylene group of C1 to C 10In particular, R1, R2 and R3 are each independently selected from a hydrogen atom, a C1-C4 alkylene group or a C1-C4 halogen atom-substituted alkyl group, and R4 is a bond, a C1-C4 alkylene group or a C1-C4 halogen atom-substituted alkylene group; in particular, R1, R2 and R3 are each independently selected from a hydrogen atom or a methyl group, and R4 is a bond, a methylene group or an ethylene group. As a specific example, the monomer α may be 3,4-epoxycyclohexylmethyl methacrylate having a structure represented by formula (3) or 3,4-epoxycyclohexylmethyl acrylate having a structure represented by formula (4). TIFF0007591587000019.tif29160

[0047] In some specific embodiments, the monomer α has the structure shown in formula (5). TIFF0007591587000020.tif25161

[0048] Here, R5 is a bond, C1 to C 10 or an alkylene group of C1 to C 10 R6 is a halogen atom-substituted alkylene group; TIFF0007591587000021.tif1145; in particular, R5 is a bond, a C1-C4 alkylene group, or a C1-C4 halogen atom-substituted alkylene group; as a specific example, the monomer α may be 1,2-epoxy-4-vinylcyclohexane having a structure represented by formula (6) or vinylcyclohexene diepoxide having a structure represented by formula (7). TIFF0007591587000022.tif23161

[0049] In some specific embodiments, the monomer α has the structure shown in formula (8). TIFF0007591587000023.tif23160

[0050] Here, R7 and R9 each independently represent a bond, C1 to C 10or an alkylene group of C1 to C 10 In particular, R7 and R9 are each independently selected from a bond, a C1-C4 alkylene group, or a C1-C4 halogen atom-substituted alkylene group; R8 is a C1-C 10 or an alkylene group of C1 to C 10 In particular, R8 is a C1-C4 alkylene group or a C1-C4 halogen atom-substituted alkylene group; X and Y are each independently selected from a bond, an oxygen atom, a carbonyl group, or an ester group; as a specific example, the monomer α may be 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate having a structure represented by formula (9) or bis((3,4-epoxycyclohexyl)methyl)adipate having a structure represented by formula (10). TIFF0007591587000024.tif32160

[0051] In some specific embodiments of the protective coating II of the present invention, the plasma comprises only a plasma of monomer α. In other specific embodiments, to further facilitate the formation of a dense protective layer with high bonding strength between the plasma coating and the substrate, the plasma comprises a plasma of monomer α and a plasma of monomer β, where monomer β comprises a structural unit a; and the structural unit a has the structure shown in formula (11). TIFF0007591587000025.tif37161

[0052] Here, R 10 , R 11 and R 12 are each independently a hydrogen atom, C1 to C 10 or C1-C 10As a specific example, the monomer β may be one or more of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, butyl acrylate, 1,4-butanediol methacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, or neopentyl glycol dimethacrylate. In particular, the R 10 , R 11 and R 12 are each independently selected from a hydrogen atom, a C1-C4 alkyl group, or a C1-C4 halogen atom-substituted alkyl group, and in particular, 10 , R 11 and R 12 are each independently selected from a hydrogen atom or a methyl group, and in particular, the monomer β includes a structural unit b, and the structural unit b is at least one of a carbon-carbon double bond structural unit, a carbon-carbon triple bond structural unit, or an epoxy structural unit, and in particular a double bond structural unit having a structure represented by formula (12). TIFF0007591587000026.tif34161

[0053] Here, R 13 , R 14 and R 15 are each independently a hydrogen atom, C1 to C 10 or C1-C 10 In particular, R 13 , R 14 and R 15 are each independently selected from a hydrogen atom, a C1-C4 alkyl group, or a C1-C4 halogen atom-substituted alkyl group; 13 , R 14 and R 15are each independently selected from a hydrogen atom or a methyl group. In particular, the monomer β has a structure shown in formula (13). TIFF0007591587000027.tif34161

[0054] Here, R 16 is C2~C 10 or an alkylene group of C2 to C 10 and n is an integer of 1 to 10; specifically, for example, n is 1, and R 11 is C2 to C such as ethylene, propylene, butylene, and pentylene. 10 or n is 1 and R 11 is a C2-C alkyl group such as a halogen atom-substituted ethylene group, a halogen atom-substituted propylene group, a halogen atom-substituted butylene group, and a halogen atom-substituted pentylene group. 10 or n is an integer of 2 to 10, and R 11 is an ethylene group or a propylene group, etc. In a specific embodiment of the present invention, when the monomer α having an epoxy alicyclic structure is combined with the monomer β having an acrylate structure, particularly when the monomer β adopts the diacrylate structure represented by formula (13), it is helpful to form a dense protective layer with high bonding strength with the substrate after plasma coating, and further improve the corrosion resistance of the substrate.

[0055] In the protective coating II of a specific embodiment of the present invention, the specific addition amounts of the monomer β and monomer α can be adjusted according to actual conditions, and the mass ratio of the monomer β to the monomer α is usually 1:10 to 10:1, specifically, for example, 1:1, 1:2, 1:3, 2:3, 1:4, 1:5, 2:1, 3:1, 3:2, 4:1 or 5:1.

[0056] In some specific embodiments, the protective coating II of the present invention is a metal, specifically, for example, iron, magnesium, aluminum, copper or their alloys, and in other specific embodiments, the substrate is various plastics, textiles, glass, electrical components or optical devices, etc. Specifically, the electrical components may be printed circuit boards (PCBs), electronic products or electronic subassemblies, etc. When the substrate is an electronic product, it includes, but is not limited to, mobile phones, tablets, keyboards, e-readers, wearable devices, displays, etc. The substrate may be any suitable electrical component of an electrical component, specifically, the electrical components may be resistors, capacitors, transistors, diodes, amplifiers, relays, transformers, batteries, fuses, integrated circuits, switches, LEDs, LED displays, piezoelectric elements, optoelectronic components, or antennas or oscillators, etc.

[0057] A specific embodiment of the present invention provides a method for producing the protective coating II above, comprising providing a substrate; and forming a plasma polymerized coating on a surface of the substrate by contacting the substrate with the plasma, the plasma and the substrate being as described above.

[0058] In the method for producing protective coating II according to a specific embodiment of the present invention, in order to further enhance the bonding strength between the plasma coating and the substrate, in some specific embodiments, the substrate is a substrate pretreated with continuous plasma, and specific conditions are, for example, under an inert gas atmosphere, the plasma discharge power is 20-500 W, the discharge method is continuous, and the continuous discharge time is 1-15 min. In other specific embodiments, the substrate is a substrate pretreated by methods such as heat, oxygen, or high-energy radiation.

[0059] In the method for producing the protective coating II of the specific embodiment of the present invention, in some specific embodiments, the plasma is a plasma excited by continuous wave, and in other specific embodiments, the plasma is a plasma excited by pulse mode. The specific conditions of the plasma coating can adopt the corresponding conditions in the prior art, for example, as follows: the substrate is placed in the reaction chamber of the plasma chamber, evacuated to 20-250 mTorr, inert gas such as He, Ar, O2 or some mixed gas is introduced, monomers participating in the reaction are introduced into the chamber in gas form, the monomer flow rate is 10-2000 μl / min, power is turned on, and plasma is generated, so that chemical vapor deposition occurs on the surface of the substrate. The temperature inside the chamber is controlled at 20°C to 80°C, the monomer vaporization temperature is 50°C to 120°C, and vaporization occurs under vacuum conditions. Plasma is excited in a continuous wave manner with a plasma discharge power of 10 to 180 W and a continuous discharge time of 10 to 600 min, or plasma is excited in a pulse manner with a pulse frequency of 20 Hz to 80 KHz, a duty ratio of 1‰ to 80%, and an average pulse power density of 0.001 W / m3 to 500 W / m3.

[0060] In the manufacturing method of the protective coating II of a specific embodiment of the present invention, the plasma discharge manner may be any of various conventional discharge manners, specifically, for example, electrodeless discharge (e.g., radio frequency inductively coupled discharge, microwave discharge), single electrode discharge (e.g., corona discharge, plasma jet by single electrode discharge), two electrode discharge (e.g., dielectric barrier discharge, exposed electrode radio frequency glow discharge) and multi-electrode discharge (e.g., discharge employing a floating electrode as the third electrode).

[0061] Specific embodiments of the present invention further provide a device, at least a portion of the surface of the device having a protective coating II as described above, and in some specific embodiments, some or all of the surface of the device is coated only with the protective coating II as described above, and in some specific embodiments, some or all of the surface of the device is coated with another coating in addition to the protective coating II as described above.

[0062] A specific embodiment of the present invention further provides a protective coating, the protective coating comprising Coating I and Coating II deposited on a substrate, said coating II being protective coating II described above; said coating I being a plasma polymerized coating formed on coating II by contacting said coating II with a plasma comprising monomer γ; Said monomer γ is selected from one or more of an alkane, a halogenated alkane, an alkene, a halogenated alkene, an alkyne, a halogenated alkyne, an acrylate or a halogenated acrylate.

[0063] The protective coating of specific embodiments of the present invention, in some specific embodiments, coating I is a plasma polymerized coating formed on coating II by contacting coating II with a plasma containing monomer γ as shown in formula (14) below: TIFF0007591587000028.tif36160

[0064] Here, R 17 , R 18 and R 19 are each independently a hydrogen atom, C1 to C 10 or C1-C 10 R is selected from halogen atom-substituted alkyl groups 20 is C1~C 20 or a hydrocarbon group of C1 to C 20In order to further improve the hydrophobicity, R 20 is C4~C 20 or C4-C 20 In consideration of the environmental impact of halogen elements, in some specific embodiments, R 17 , R 18 and R 19 are each independently a hydrogen atom or C1 to C 10 In particular, the alkyl group R 17 , R 18 and R 19 are each independently selected from a hydrogen atom or a methyl group, 20 is C1~C 20 In particular, the R 20 is C4~C 20 In some specific embodiments of the present invention, the hydrocarbon group is a saturated alkane group, such as, for example, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or an octadecyl group, and in other specific embodiments of the present invention, the hydrocarbon group is an unsaturated alkene group, an alkyne group, or an aromatic hydrocarbon group. As specific examples, the monomer γ may be one or more of cyclohexyl methacrylate, octadecyl acrylate, isodecyl methacrylate, allyl methacrylate, isobornyl methacrylate, t-butyl methacrylate, benzyl methacrylate, phenyl methacrylate, isopropyl methacrylate, and 9-anthracene methyl methacrylate. In some specific embodiments, the monomer γ has a structure shown in formula (15). TIFF0007591587000029.tif34160

[0065] Here, R 21 is a bond, C1~C 10 or an alkylene group of C1 to C 10In this case, B is an aromatic ring structure or a 3- to 20-membered alicyclic structure, particularly B is a 5- or 6-membered alicyclic structure, particularly B is a cyclohexyl group or a cyclopentyl group; in consideration of the environmental impact of halogen elements, in some specific embodiments, R 21 is a bond or C1 to C 10 In particular, R 21 is a bond, a methylene group, or an ethylene group. When the monomer γ has a structure represented by formula (15) and B is an alicyclic structure, both coating I and coating II have an alicyclic structure and have a better bonding effect, so that the combination of coating I and coating II has a better protective performance.

[0066] In some specific embodiments of the protective coating of the present invention, the coating further comprises a coating III, which is a plasma polymerized coating formed by contacting the substrate with a plasma of a monomer δ; the coating II is a plasma polymerized coating formed on the coating III by contacting the coating III with a plasma containing a monomer α; the monomer δ comprises a structural unit c and a structural unit d, the structural unit c and the structural unit d respectively having a carbon-carbon double bond structure and an ester group structure, and the coating III formed by chemical vapor deposition using a plasma of the monomer δ having such two unsaturated ester structures is beneficial for increasing the tight bonding between the substrate and the coating II, and further increasing the denseness and bonding strength of the protective coating. As specific examples, the monomer δ may be one or more of 1,4-butanediol methacrylate, 1,6-hexanediol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, neopentyl glycol dimethacrylate, methacrylic anhydride, 2-benzylidene malonate diprop-2-enyl, diallyl malonate diethyl, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, or 1,6-hexanediol diacrylate. In some specific embodiments, the structural unit c has a structure shown in formula (16). TIFF0007591587000030.tif37160

[0067] Here, in some specific embodiments, R 22 , R 23 and R 24 are C1 to C 10 In consideration of the environmental impact of halogen elements, in some specific embodiments, R 22 , R 23 and R24 are each independently a hydrogen atom or C1 to C 10 In some specific embodiments, the structural unit d has a carbon-carbon double bond structural unit having a structure represented by formula (17). TIFF0007591587000031.tif38161

[0068] Here, in some specific embodiments, R 25 , R 26 and R 27 are C1 to C 10 In consideration of the environmental impact of halogen elements, in some specific embodiments, R 25 , R 26 and R 27 are each independently a hydrogen atom or C1 to C 10 In particular, R is selected from the group consisting of a hydrogen atom and an alkyl group having 1 to 4 carbon atoms; 25 , R 26 and R 27 are each independently selected from a hydrogen atom or a methyl group, in particular a hydrogen atom or a methyl group. In some specific embodiments, the monomer δ has the structure shown in formula (18). TIFF0007591587000032.tif39161

[0069] wherein in some embodiments, R 28 is C2~C 10 In the halogen atom-substituted alkylene group, n is an integer of 0 to 10. Specifically, for example, n is 1, R 28 is a C2-C alkyl group such as a halogen atom-substituted ethylene group, a halogen atom-substituted propylene group, a halogen atom-substituted butylene group, and a halogen atom-substituted pentylene group. 10 In consideration of the environmental impact of halogen elements, in some embodiments, R 28 is C2~C 10where n is an integer of 1 to 10. Specifically, for example, n is 1, R 28 is C2 to C such as ethylene, propylene, butylene, and pentylene. 10 or n is an integer of 2 to 10; R 22 is an ethylene group or a propylene group, etc. Coating III, particularly Coating II, can be more closely bonded to the substrate by the monomer δ of Coating III being the diacrylate structure shown in formula (18), further enhancing the compactness and cohesive strength of such protective coating.

[0070] The more commonly used method of using plasma anticorrosive coating is to plasma coat the substrate with perfluoromonomer, but such coating has the problem that the monomer has poor bonding strength to the substrate due to the perfluoro group, and the fluoropolymer is prone to release toxic substances such as perfluorooctyl carboxylate and perfluorooctyl sulfonate into the environment, causing environmental pollution. In response to this, the United States Environmental Protection Agency (EPA) has issued stricter regulations prohibiting the use of fluoropolymers containing long carbon chains. On the other hand, the protective coating of a specific embodiment of the present invention has excellent bonding strength with the substrate and has better protective performance than plasma coatings formed by F-containing monomers, even if it does not contain halogen F.

[0071] Particular embodiments of the present invention further provide a method of making said protective coating, comprising providing a substrate; and forming said protective coating on the substrate as a plasma-deposited coating, the plasma and substrate being as described above.

[0072] In the manufacturing method of the protective coating of the specific embodiment of the present invention, in some specific embodiments, the specific conditions of the plasma coating can adopt the corresponding conditions in the prior art, for example, as follows: the substrate is placed in the reaction chamber of the plasma chamber, evacuated to 1-250 mTorr, inert gas such as He, Ar, O2 or some mixed gas is introduced, monomers participating in the reaction are introduced in gas form into the chamber, the monomer flow rate is 40-2000 μl / min, power is turned on, plasma is generated, chemical vapor deposition occurs on the surface of the substrate to form the coating III, coating II and coating I, respectively. The temperature inside the chamber is controlled at 20°C to 80°C, the monomer vaporization temperature is 70°C to 150°C, and vaporization occurs under vacuum conditions. Plasma is excited in a continuous wave manner with a plasma discharge power of 10 to 180 W and a continuous discharge time of 100 to 7200 s, or plasma is excited in a pulse manner with a pulse power of 20 to 500 W, a pulse frequency of 20 Hz to 80 KHz, a pulse duty ratio of 1‰ to 80%, and a plasma discharge time of 100 s to 20,000 s.

[0073] The present invention will now be further described with reference to specific examples. EXAMPLES

[0074] Test method description

[0075] 5V Salt Water Test: The test process is as follows: 1, the power supply supplied 5V voltage to the circuit board; 2, the circuit board was immersed in 3.6% salt water; 3, the current was detected by the computer; 4, the failure time (current > 0.6mA) was recorded.

[0076] Salt spray resistance test: Tested according to GB / T2423.18-2000 environmental test method for electrical and electronic products.

[0077] Damp heat test: Tested according to GB / T2423.34-2012 standard. Example 1-1

[0078] (1) The substrate Fe sheet (30*20*2mm) and Mg sheet (30*20*2mm) were placed in a 500L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 80 mTorr, and the chamber temperature was 35°C.

[0079] (2) Argon gas was flowed at a flow rate of 10 sccm, and the radio frequency plasma discharge was turned on to pretreat the substrate. In this pretreatment step, the discharge power was 100 W and the discharge lasted for 80 s.

[0080] (3) A mixed monomer of triethylene glycol dimethacrylate and 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate (mass ratio 1:1) was introduced, the mixed monomer flow rate was 600 μl / min, the reaction temperature inside the chamber was 60°C, the plasma in the chamber was generated by a radio frequency discharge method, the output method was changed to pulse, the pulse width was 100 μs, the pulse frequency was 100 Hz, the discharge power was 10 W, and the discharge time was 120 min.

[0081] (4) After the coating preparation was completed, air was introduced into the reaction chamber to return it to normal pressure, the chamber was opened, the Fe sheet and the Mg sheet were removed, and a salt spray resistance test and a high temperature and high humidity test were conducted. The test results are shown in Tables 1 and 2 below, respectively. Example 1-2

[0082] (1) The substrate Fe sheet (30*20*2mm) and Mg sheet (30*20*2mm) were placed in a 500L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 20 mTorr, and the chamber temperature was 45°C.

[0083] (2) Helium gas was introduced at a flow rate of 300 sccm, and the radio frequency plasma discharge was turned on to pretreat the substrate, and in this pretreatment step, the discharge power was 300 W and the discharge lasted for 60 s.

[0084] (3) A mixed monomer of tetraethylene glycol dimethacrylate and 3,4-epoxycyclohexylmethyl methacrylate (mass ratio 2:1) was introduced, the mixed monomer flow rate was 200 μl / min, the reaction temperature inside the chamber was 65°C, the plasma in the chamber was generated by a radio frequency discharge method, the output method was changed to pulse, the pulse width was 200 μs, the pulse frequency was 100 Hz, the discharge power was 35 W, and the discharge time was 40 min.

[0085] (4) After the coating preparation was completed, air was introduced into the reaction chamber to return it to normal pressure, the chamber was opened, the Fe sheet and the Mg sheet were removed, and a salt spray resistance test and a high temperature and high humidity test were conducted. The test results are shown in Tables 1 and 2 below, respectively. Examples 1-3

[0086] (1) The substrate Fe sheet (30*20*2mm) and Mg sheet (30*20*2mm) were placed in a 500L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 250 mTorr, and the chamber temperature was 45°C.

[0087] (2) Helium gas was introduced at a flow rate of 120 sccm, and the radio frequency plasma discharge was turned on to pretreat the substrate. In this pretreatment step, the discharge power was 300 W and the discharge lasted for 90 s.

[0088] (3) A mixed monomer of 1,6-hexanediol diacrylate and 1,2-epoxy-4-vinylcyclohexane (mass ratio 3:2) was introduced, the mixed monomer flow rate was 200 μl / min, the reaction temperature inside the chamber was 70 °C, the plasma in the chamber was generated by a radio frequency discharge method, the output method was changed to pulse, the pulse width was 200 μs, the pulse frequency was 50 Hz, the discharge power was 100 W, and the discharge time was 35 min.

[0089] (4) After the coating preparation was completed, air was introduced into the reaction chamber to return it to normal pressure, the chamber was opened, the Fe sheet and the Mg sheet were removed, and a salt spray resistance test and a high temperature and high humidity test were conducted. The test results are shown in Tables 1 and 2 below, respectively. Examples 1-4

[0090] (1) The substrate Fe sheet (30*20*2mm) and Mg sheet (30*20*2mm) were placed in a 500L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 100 mTorr, and the chamber temperature was 80°C.

[0091] (2) Oxygen gas was introduced at a flow rate of 300 sccm, and the microwave plasma discharge was turned on to pretreat the substrate. In this pretreatment step, the discharge power was 500 W, and the discharge lasted for 90 s.

[0092] (3) A mixed monomer of hydroxypropyl methacrylate and bis((3,4-epoxycyclohexyl)methyl)adipate (mass ratio 1:2) was introduced, the mixed monomer flow rate was 2000 μl / min, the reaction temperature inside the chamber was 45°C, the plasma in the chamber was generated by a radio frequency discharge method, the output method was changed to pulse, the pulse width was 300 μs, the pulse frequency was 50 Hz, the discharge power was 180 W, and the discharge time was 15 min.

[0093] (4) After the coating preparation was completed, air was introduced into the reaction chamber to return it to normal pressure, the chamber was opened, the Fe sheet and the Mg sheet were removed, and a salt spray resistance test and a high temperature and high humidity test were conducted. The test results are shown in Tables 1 and 2 below, respectively. Examples 1-5

[0094] (1) The substrate Fe sheet (30*20*2mm) and Mg sheet (30*20*2mm) were placed in a 500L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 100 mTorr, and the chamber temperature was 80°C.

[0095] (2) Helium gas was introduced at a flow rate of 180 sccm, and the microwave plasma discharge was turned on to pretreat the substrate. In this pretreatment step, the discharge power was 120 W, and the discharge lasted for 600 s.

[0096] (3) A mixed monomer of 1,3-butanediol dimethacrylate and vinylcyclohexene diepoxide (mass ratio 2:1) was introduced, the mixed monomer flow rate was 800 μl / min, the reaction temperature inside the chamber was 45°C, the plasma in the chamber was generated by a radio frequency discharge method, the output method was changed to pulse, the pulse width was 300 μs, the pulse frequency was 50 Hz, the discharge power was 300 W, and the discharge time was 20 min.

[0097] (4) After the coating preparation was completed, air was introduced into the reaction chamber to return it to normal pressure, the chamber was opened, the Fe sheet and the Mg sheet were removed, and a salt spray resistance test and a high temperature and high humidity test were conducted. The test results are shown in Tables 1 and 2 below, respectively. Examples 1-6

[0098] (1) The substrate Fe sheet (30*20*2mm) and Mg sheet (30*20*2mm) were placed in a 500L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 80 mTorr, and the chamber temperature was 50°C.

[0099] (2) Helium gas was introduced at a flow rate of 160 sccm, and the microwave plasma discharge was turned on to pretreat the substrate. In this pretreatment step, the discharge power was 180 W, and the discharge lasted for 300 s.

[0100] (3) 1,2-epoxy-4-vinylcyclohexane monomer was introduced, the mixed monomer flow rate was 500 μl / min, the reaction temperature inside the chamber was 85°C, the plasma in the chamber was generated by radio frequency discharge method, the output method was changed to pulse, the pulse width was 500 μs, the pulse frequency was 20 Hz, the discharge power was 100 W, and the discharge time was 20 min.

[0101] (4) After the coating preparation was completed, air was introduced into the reaction chamber to return it to normal pressure, the chamber was opened, the Fe sheet and the Mg sheet were removed, and a salt spray resistance test and a high temperature and high humidity test were conducted. The test results are shown in Tables 1 and 2 below, respectively. Comparative Example 1-1

[0102] (1) The substrate Fe sheet (30*20*2mm) and Mg sheet (30*20*2mm) were placed in a 500L plasma vacuum reaction chamber, and the reaction chamber was continuously evacuated to a vacuum degree of 80 mTorr, and the chamber temperature was 60°C.

[0103] (2) Helium gas was introduced at a flow rate of 140 sccm, and the microwave plasma discharge was turned on to pretreat the substrate. In this pretreatment step, the discharge power was 180 W, and the discharge lasted for 200 s.

[0104] (3) Ethylene glycol dimethacrylate monomer was introduced, the mixed monomer flow rate was 700 μl / min, the reaction temperature inside the chamber was 55°C, the plasma in the chamber was generated by radio frequency discharge method, the output method was changed to pulse, the pulse width was 300 μs, the pulse frequency was 50 Hz, the discharge power was 80 W, and the discharge time was 40 min.

[0105] (4) After the coating preparation was completed, air was introduced into the reaction chamber to return it to normal pressure, the chamber was opened, the Fe sheet and the Mg sheet were removed, and a salt spray resistance test and a high temperature and high humidity test were conducted. The test results are shown in Tables 1 and 2 below, respectively.

[0106] TIFF0007591587000033.tif86161

[0107] TIFF0007591587000034.tif85161 Example 2-1

[0108] The circuit board, Mg, and Fe sheets were placed in the plasma chamber, the chamber was evacuated to 20 mTorr, helium gas was introduced at a flow rate of 80 sccm, and the radio frequency plasma discharge was turned on to pretreat the substrates. In this pretreatment stage, the discharge power was 100 W and the discharge continued for 600 s.

[0109] Next, 1,4-butanediol dimethacrylate was introduced and vaporized at a vaporization temperature of 100°C, and then introduced into the chamber to carry out plasma chemical vapor deposition. The monomer flow rate was 150 μL / min, and the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 1000 Hz, the discharge power was 50 W, and the discharge time was 3600 s.

[0110] Next, the mixed monomer of 1,6-hexanediol diacrylate and 1,2-epoxy-4-vinylcyclohexane (mass ratio 2:1) was introduced, the mixed monomer flow rate was 40 μl / min, the monomer vaporization temperature was 120 °C, the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 1000 Hz, the discharge power was 10 W, and the discharge time was 7200 s.

[0111] Next, octadecyl acrylate vapor was introduced, the flow rate was 100 μl / min, the monomer vaporization temperature was 120 °C, and the plasma in the chamber was generated by radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 1000 Hz, the discharge power was 180 W, and the discharge time was 7200 s, and the coating was completed.

[0112] After the coating was completed, the chamber was returned to normal pressure by introducing compressed air. The circuit board, Mg, and Fe sheet samples were taken out and subjected to salt water and salt fog tests. The test results are shown in Table 3. Example 2-2

[0113] The circuit board, Mg, and Fe sheets were placed in the plasma chamber, the chamber was evacuated to 8 mTorr, helium gas was introduced at a flow rate of 80 sccm, and the radio frequency plasma discharge was turned on to pretreat the substrates. In this pretreatment stage, the discharge power was 100 W and the discharge continued for 600 s.

[0114] Next, 1,6-hexanediol dimethacrylate was introduced and vaporized at a vaporization temperature of 100°C, and then introduced into the chamber to carry out plasma chemical vapor deposition. The monomer flow rate was 150 μL / min, and the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 45%, the pulse frequency was 500 Hz, the discharge power was 50 W, and the discharge time was 3600 s.

[0115] Next, the mixed monomer of 1,6-hexanediol dimethacrylate and vinylcyclohexene diepoxide (mass ratio 1:2) was introduced, the mixed monomer flow rate was 40 μl / min, the monomer vaporization temperature was 120 °C, and the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 45%, the pulse frequency was 500 Hz, the discharge power was 10 W, and the discharge time was 7200 s.

[0116] Next, t-butyl methacrylate vapor was introduced, the flow rate was 100 μl / min, the monomer vaporization temperature was 120 °C, and the plasma in the chamber was generated by radio frequency discharge method, the output method was pulse, the pulse duty ratio was 45%, the pulse frequency was 500 Hz, the discharge power was 25 W, and the discharge time was 7200 s, and the coating was completed.

[0117] After the coating was completed, the chamber was returned to normal pressure by introducing compressed air. The circuit board, Mg, and Fe sheet samples were taken out and subjected to salt water and salt fog tests. The test results are shown in Table 3. Example 2-3

[0118] The circuit board, Mg, and Fe sheets were placed in the plasma chamber, the chamber was evacuated to 100 mTorr, helium gas was introduced at a flow rate of 120 sccm, and the radio frequency plasma discharge was turned on to pretreat the substrates. In this pretreatment stage, the discharge power was 180 W and the discharge continued for 300 s.

[0119] Next, 1,6-hexanediol dimethacrylate was introduced and vaporized at a vaporization temperature of 110 °C, and then introduced into the chamber to perform plasma chemical vapor deposition. The monomer flow rate was 220 μL / min, and the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 45%, the pulse frequency was 5000 Hz, the discharge power was 25 W, and the discharge time was 2200 s.

[0120] Next, a mixed monomer of triethylene glycol dimethacrylate and 3,4-epoxycyclohexylmethyl methacrylate (mass ratio 3:2) was introduced, the mixed monomer flow rate was 40 μl / min, the monomer vaporization temperature was 120 °C, and the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 45%, the pulse frequency was 5000 Hz, the discharge power was 10 W, and the discharge time was 7200 s.

[0121] Next, isobornyl methacrylate vapor was introduced, the flow rate was 100 μl / min, the monomer vaporization temperature was 120 °C, the plasma in the chamber was generated by radio frequency discharge method, the output method was pulse, the pulse duty ratio was 45%, the pulse frequency was 5000 Hz, the discharge power was 25 W, and the discharge time was 7200 s, and the coating was completed.

[0122] After the coating was completed, the chamber was returned to normal pressure by introducing compressed air. The circuit board, Mg, and Fe sheet samples were taken out and subjected to salt water and salt fog tests. The test results are shown in Table 3. Examples 2-4

[0123] The circuit board, Mg sheet was placed in the plasma chamber, the chamber was evacuated to 80 mTorr, helium gas was introduced at a flow rate of 120 sccm, and the radio frequency plasma discharge was turned on to pretreat the substrate, in this pretreatment stage, the discharge power was 180 W, and the discharge continued for 300 s.

[0124] Next, 1,4-butanediol dimethacrylate was introduced and vaporized at a vaporization temperature of 110°C, and then introduced into the chamber to perform plasma chemical vapor deposition. The monomer flow rate was 120 μL / min, and the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 20 kHz, the discharge power was 20 W, and the discharge time was 3600 s.

[0125] Next, a mixed monomer of 1,6-hexanediol diacrylate and bis((3,4-epoxycyclohexyl)methyl)adipate (mass ratio 2:1) was introduced, the mixed monomer flow rate was 150 μl / min, the monomer vaporization temperature was 120 °C, the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 20 kHz, the discharge power was 10 W, and the discharge time was 3600 s.

[0126] Next, benzyl methacrylate vapor was introduced, the flow rate was 150 μl / min, the monomer vaporization temperature was 150 °C, the plasma in the chamber was generated by radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 20 kHz, the discharge power was 150 W, and the discharge time was 7200 s, and the coating was completed.

[0127] After the coating was completed, the chamber was returned to normal pressure by introducing compressed air. The circuit board, Mg, and Fe sheet samples were taken out and subjected to salt water and salt fog tests. The test results are shown in Table 3. Comparative Example 2-1

[0128] The circuit board, Mg, and Fe sheets were placed in the plasma chamber, the chamber was evacuated to 80 mTorr, helium gas was introduced at a flow rate of 120 sccm, and the radio frequency plasma discharge was turned on to pretreat the substrate. In this pretreatment stage, the discharge power was 180 W and the discharge lasted for 300 s.

[0129] Next, 1,4-butanediol diacrylate was introduced and vaporized at a vaporization temperature of 110°C, and then introduced into the chamber to carry out plasma chemical vapor deposition. The monomer flow rate was 120 μL / min, and the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 20 kHz, the discharge power was 20 W, and the discharge time was 3600 s.

[0130] Next, 2-(perfluorohexyl)ethyl methacrylate was introduced, the monomer flow rate was 120 μl / min, the monomer vaporization temperature was 110 °C, the plasma in the chamber was generated by a radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 20 kHz, the discharge time was 3600 s, and the discharge power was 180 W.

[0131] Next, 2-(perfluorododecyl)ethyl acrylate vapor was introduced, the flow rate was 160 μl / min, the monomer vaporization temperature was 110 °C, the plasma in the chamber was generated by radio frequency discharge method, the output method was pulse, the pulse duty ratio was 25%, the pulse frequency was 20 kHz, the discharge time was 7200 s, and the discharge power was 180 W, and the coating was completed.

[0132] After the coating was completed, the chamber was returned to normal pressure by introducing compressed air. The circuit board, Mg, and Fe sheet samples were taken out and subjected to salt water and salt fog tests. The test results are shown in Table 3.

[0133] TIFF0007591587000035.tif107161

[0134] From the results in Table 3 above, it can be seen that the protective coating of the present invention, even without the halogen F, has better protective performance than the plasma protective coating formed from a perfluoromonomer.

[0135] Although the present invention has been disclosed as above, the present invention is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention should be based on the scope defined by the claims.

Claims

1. a protective coating comprising a protective coating II, the protective coating being a plasma polymerized coating formed on a surface of the substrate by contacting the substrate with a plasma; The plasma includes a plasma of monomer α, the monomer α including an alicyclic epoxy structural unit represented by formula (1), 11. A protective coating, comprising: the plasma further comprising a plasma of monomer β, the monomer β comprising structural unit a; the structural unit a having the structure shown in formula (11). (wherein A is a 3- to 20-membered alicyclic structure). (Here, R 10 , R 11 and R 12 are each independently a hydrogen atom, C 1 ~C 10 or C 1 ~C 10 is selected from the halogen atom-substituted alkyl groups.

2. 2. The protective coating of claim 1, wherein A is a 5-membered alicyclic structure or a 6-membered alicyclic structure.

3. 2. The protective coating of claim 1, wherein the monomer α further comprises at least one of a carbon-carbon double bond structural unit, a carbon-carbon triple bond structural unit, or an epoxy structural unit.

4. 4. The protective coating of claim 3, wherein the monomer α has the structure shown in formula (2). (Here, R 1 , R 2 and R 3 are each independently a hydrogen atom, C 1 ~C 10 or C 1 ~C 10 is selected from halogen atom-substituted alkyl groups; R 4 is a bond, C 1 ~C 10 or an alkylene group of C 1 ~C 10 is a halogen atom-substituted alkylene group.

5. The R 1 , R 2 and R 3 are each independently selected from a hydrogen atom or a methyl group; 4 5. The protective coating of claim 4, wherein is a bond, a methylene group, or an ethylene group.

6. 6. The protective coating of claim 5, wherein the monomer α has a structure shown in formula (3) or formula (4).

7. 4. The protective coating of claim 3, wherein the monomer α has the structure shown in formula (5). (Here, R 5 is a bond, C 1 ~C 10 or an alkylene group of C 1 ~C 10 is a halogen atom-substituted alkylene group; R 6 teeth It is.)

8. 8. The protective coating of claim 7, wherein the monomer α has a structure shown in formula (6) or formula (7).

9. 4. The protective coating of claim 3, wherein the monomer α has the structure shown in formula (8). (Here, R 7 and R 9 each independently represents a bond, C 1 ~C 10 or an alkylene group of C 1 ~C 10 halogen atom-substituted alkylene groups; R 8 is C 1 ~C 10 or an alkylene group of C 1 ~C 10 is a halogen atom-substituted alkylene group; X and Y are each independently selected from a bond, an oxygen atom, a carbonyl group, or an ester group.

10. 10. The protective coating of claim 9, wherein the monomer α has a structure shown in formula (9) or formula (10).

11. 2. The protective coating of claim 1, wherein the monomer β further comprises a structural unit b, the structural unit b being at least one of a double bond structural unit, a triple bond structural unit, or an epoxy structural unit.

12. 12. The protective coating of claim 11, wherein the structural unit b has a structure shown in formula (12). (Here, R 13 , R 14 and R 15 are each independently a hydrogen atom, C 1 ~C 10 or C 1 ~C 10 is selected from the halogen atom-substituted alkyl groups.

13. 13. The protective coating of claim 12, wherein the monomer β has the structure shown in formula (13). (Here, R 16 is C 2 ~C 10 or an alkylene group of C 2 ~C 10 and n is an integer of 1 to 10.

14. The R 10 , R 11 , R 12 , R 13 , R 14 and R 15 14. The protective coating of claim 13, wherein each is independently selected from a hydrogen atom or a methyl group.

15. A protective coating further comprising Coating I, said coating I being a plasma polymerized coating formed on said protective coating II by contacting said coating II with a plasma containing monomer γ; 15. The protective coating of any one of claims 1 to 14, wherein the monomer γ is selected from one or more of an alkane, a halogenated alkane, an alkene, a halogenated alkene, an alkyne, a halogenated alkyne, an acrylate, or a halogenated acrylate.

16. 16. The protective coating of claim 15, wherein the monomer γ has the structure shown in formula (14). (Here, R 17 , R 18 and R 19 are each independently a hydrogen atom, C 1 ~C 10 or C 1 ~C 10 is selected from halogen atom-substituted alkyl groups; R 20 is C 1 ~C 20 or a hydrocarbon group of C 1 ~C 20 is a halogen atom-substituted hydrocarbon group.

17. The R 17 , R 18 and R 19 are each independently selected from a hydrogen atom or a methyl group; 20 is C 4 ~C 20 or a hydrocarbon group of C 4 ~C 20 17. The protective coating of claim 16, wherein the halogen atom substituted hydrocarbon group is

18. 17. The protective coating of claim 16, wherein the monomer γ has the structure shown in formula (15). (wherein R21 is a bond, a C1-C10 alkylene group, or a C1-C10 halogen atom-substituted alkylene group; B is an aromatic ring structure or a 3- to 20-membered alicyclic structure.

19. The R 21 20. The protective coating of claim 18, wherein: is a bond, a methylene group, or an ethylene group; and B is a cyclohexyl group or a cyclopentyl group.

20. The coating further comprises a coating III, which is a plasma polymerized coating formed by contacting the substrate with a plasma comprising monomer δ; said protective coating II is a plasma polymerized coating formed on coating III by contacting said coating III with a plasma comprising monomer α; The protective coating of claim 15, wherein the monomer δ comprises a structural unit c and a structural unit d, and the structural unit c and the structural unit d each have a carbon-carbon double bond structure and an ester group structure.

21. 21. The protective coating of claim 20, wherein the monomer δ has the structure shown in formula (18). (Here, R 28 is C 2 ~C 10 or an alkylene group of C 2 ~C 10 n is an integer of 0 to 10; R 22 , R 23 , R 24 , R 25 , R 26 and R 27 are each independently a hydrogen atom, C 1 ~C 10 or C 1 ~C 10 is selected from the halogen atom-substituted alkyl groups.

22. Providing a substrate; and forming said protective coating on a substrate as a plasma deposited coating; A method for producing a protective coating according to any one of claims 1 to 21, comprising:

23. 23. The method for producing a protective coating according to claim 22, wherein the plasma is a pulsed plasma, the pulsed plasma being generated by applying a pulse voltage discharge, the pulse power being 20-500 W, the pulse frequency being 20 Hz-80 KHz, the pulse duty ratio being 1%-80%, and the plasma discharge time being 100 s-20,000 s.

24. A device, characterized in that at least a portion of the surface of the device has a protective coating according to any one of claims 1 to 21.

Citation Information

Patent Citations

  • Multi-layer structure and preparation method thereof

    CN110158060A

  • Waterproof nano-film, preparation method and application thereof, and product with waterproof nano-film

    CN110665768A

  • Apparatus and methods for plasma enhanced chemical vapor deposition of polymer coatings

    US20150291830A1

  • Transparent barrier sheet and method for producing same

    WO2007111098A1