Fuel electrodes for electrochemical cells
The fuel electrode with Ni catalyst and controlled pore ratios addresses mass production stability and overvoltage issues by expanding the three-phase interface, improving electrochemical cell efficiency.
Patent Information
- Application Number
- JP2020138358
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-08-19
AI Technical Summary
Existing technologies face challenges in achieving stable mass production of fuel electrodes for solid oxide electrochemical cells while maintaining low reaction overvoltage.
The fuel electrode incorporates Ni as a metal catalyst with a specific ratio of first pores to total pores (10% to 40%) and a ratio of first interface to total interfaces (5% to 20%) to expand the three-phase interface, facilitating easier oxidation reactions and quality control.
This configuration reduces reaction overvoltage and enables easier quality control in mass production by expanding the three-phase interface, enhancing the electrochemical cell's performance.
Smart Images

Figure 0007591887000002 
Figure 0007591887000003 
Figure 0007591887000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an anode for a solid oxide electrochemical cell. [Background technology]
[0002] In an electrochemical cell, oxide ions generated at the air electrode reach the three-phase interface of the fuel electrode through the electrolyte layer, where the fuel reacts with the oxide ions. When the three-phase interface is enlarged, the oxidation reaction of the fuel occurs more easily, and the reaction overvoltage is reduced. In order to enlarge the three-phase interface that serves as the reaction field of the fuel electrode of a solid oxide electrochemical cell, Patent Document 1 discloses a fuel electrode in which Mg oxide sintered particles are covered with a mixed conductive coating and metal fine particles are supported by the mixed conductive coating. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-44966 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, it is difficult to achieve stable mass production using the above technology.
[0005] The present invention has been made to solve these problems, and has an object to provide a fuel electrode for an electrochemical cell which can easily control the quality of mass production and can reduce reaction overvoltage. [Means for solving the problem]
[0006] To achieve this objective, the electrochemical cell fuel electrode of the present invention comprises an oxide and Ni as a metal catalyst, and the pores appearing in the cross section of the electrochemical cell fuel electrode include first pores contained in the Ni, and the ratio of the number of the first pores to the total number of pores is 10% or more and 40% or less. Effect of the Invention
[0007] According to the first aspect, the fuel electrode contains an oxide and Ni, which is a metal catalyst. The pores appearing in the cross section of the electrochemical cell fuel electrode include first pores contained in Ni. By setting the ratio of the number of first pores to the number of pores to be 10% or more and 40% or less, the three-phase interface that serves as the reaction field is expanded, making it easier for the oxidation reaction of the fuel to occur. This makes it possible to reduce the reaction overvoltage. Furthermore, since the ratio of the number of first pores to the number of pores is used as an index, quality control of mass production can be facilitated.
[0008] According to the second aspect, in the cross section, the ratio of the length of the first interface between the first pores and Ni to the length of the interface between the pores and Ni is 5% or more and 20% or less, thereby making it possible to further reduce the reaction overvoltage in addition to the effect of the first aspect. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of an electrochemical cell according to one embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of the fuel electrode showing a portion indicated by II in FIG. [Diagram 3] FIG. 2 is a schematic diagram of the structure of the fuel electrode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Preferred embodiments of the present invention will now be described with reference to the accompanying drawings. Fig. 1 is a schematic cross-sectional view of an electrochemical cell 30 in one embodiment. The electrochemical cell 30 includes, in order, an electrochemical cell fuel electrode 10 (hereinafter referred to as "fuel electrode"), an electrolyte layer 11, and an air electrode 13. The electrochemical cell 30 is used, for example, as a solid oxide fuel cell (SOFC), a steam reforming cell, a steam electrolysis cell (SOEC), or a hydrogen generation cell (SOHG).
[0011] In this embodiment, the electrochemical cell 30 has an intermediate layer 12 provided between the electrolyte layer 11 and the air electrode 13. The electrochemical cell 30 in this embodiment is an anode-supported electrochemical cell in which the anode 10 is thicker than the electrolyte layer 11 and the air electrode 13.
[0012] The electrolyte layer 11 is made of a solid electrolyte that exhibits oxide ion conductivity under the operating conditions of the electrochemical cell 30. Examples of the solid electrolyte include stabilized zirconia and ceria-based solid solutions. Examples of the solid electrolyte include a solid solution of one or more selected from stabilized zirconia and ceria-based solid solutions and alumina. Examples of stabilizers for stabilized zirconia include CaO, MgO, Y2O3, Sc2O3, and Yb2O3. Examples of elements that are solid-dissolved in ceria in the ceria-based solid solution include Gd, Sm, and Y. When the electrolyte layer 11 contains a ceria-based solid solution, the electrolyte layer 11 exhibits non-negligible electronic conductivity in the reducing atmosphere of the fuel electrode atmosphere, so that stabilized zirconia or BaCe, which has low electronic conductivity in that atmosphere, is used. 1-X Sm X It is preferable to provide a layer such as O3 on the electrolyte layer 11.
[0013] In a fuel cell, the air electrode 13 is the site where gas-phase oxygen reacts with electrons to become oxide ions. The air electrode 13 must be able to easily adsorb oxidant gas (oxygen, air) and must have high oxide ion conductivity, as well as electronic conductivity. The material for the air electrode 13 is a perovskite oxide called La 1-X Sr X MnO 3-δ ,La 1-X Sr X Chief of Staff 3-δ ,La 1-X Sr X Co 1-Y Fe Y O 3-δ ,Pr 1-X Sr X MnO 3-δ Examples of the material for the air electrode 13 include a composite material of one or more oxides selected from these perovskite oxides and a solid electrolyte capable of forming the electrolyte layer 11.
[0014] The intermediate layer 12 reduces the reaction between the electrolyte layer 11 and the air electrode 13 at high temperatures during the manufacture (firing) and operation of the electrochemical cell 30. A ceria-based solid solution is exemplified as the material for the intermediate layer 12. Examples of elements that dissolve in ceria in the ceria-based solid solution include Gd, Sm, La, and Y.
[0015] Fig. 2 is an enlarged cross-sectional view of the fuel electrode 10 of a portion indicated by II in Fig. 1. The fuel electrode 10 is a porous body having gas permeability. The fuel electrode 10 includes a support layer 14 and an active layer 15 disposed between the support layer 14 and the electrolyte layer 11. In this embodiment, the support layer 14 is in contact with the active layer 15, and the active layer 15 is in contact with the electrolyte layer 11.
[0016] The support layer 14 mainly functions to support the active layer 15. The thickness of the support layer 14 is, for example, 200 μm to 1000 μm. In the fuel cell, the active layer 15 functions to generate electrons by reacting oxide ions supplied from the electrolyte layer 11 with fuel (hydrogen, carbon monoxide, hydrocarbon, etc.). The thickness of the active layer 15 is, for example, 10 μm to 40 μm. The material constituting the support layer 14 may be the same as the material constituting the active layer 15, or may be a material different from the material constituting the active layer 15.
[0017] The fuel electrode 10 is formed into a shape such as a cylinder or a plate depending on the desired shape of the electrochemical cell 30. When the electrochemical cell 30 is shaped like a cylinder, the fuel electrode 10 serving as a support is formed into a hollow cylinder, the electrolyte layer 11 is provided on the outer peripheral surface of the fuel electrode 10, and the intermediate layer 12 and the air electrode 13 are provided on the outer peripheral surface of the electrolyte layer 11. When the electrochemical cell 30 is shaped like a plate, the fuel electrode 10 serving as a support is formed into a plate shape, and the electrolyte layer 11, the intermediate layer 12, and the air electrode 13 are provided on the fuel electrode 10.
[0018] The electrochemical cell 30 is manufactured through the steps of preparing and mixing, molding, and firing the raw materials constituting the fuel electrode 10, electrolyte layer 11, intermediate layer 12, and air electrode 13. In the mixing step, a binder, a pore former, a plasticizer, and the like are also mixed as necessary. Examples of the means for molding the fuel electrode 10 include extrusion molding, press molding, tape casting, and injection molding. Examples of the means for molding the electrolyte layer 11, intermediate layer 12, and air electrode 13 include thick film printing by applying a slurry in which the raw materials are dispersed in a liquid, and tape casting. The electrochemical cell 30 is obtained by firing the molded body.
[0019] The forming and firing can be carried out, for example, by stacking a green body of the fuel electrode 10 and a green body of the electrolyte layer 11 and firing the stack to obtain the fuel electrode 10 and the electrolyte layer 11, then providing a green body of the intermediate layer 12 on the electrolyte layer 11 and firing the green body of the air electrode 13 on the intermediate layer 12 and firing the green body to obtain the electrochemical cell 30. Alternatively, the electrochemical cell 30 can be obtained by stacking the green bodies of the fuel electrode 10, the electrolyte layer 11, the intermediate layer 12, and the air electrode 13 and firing the stack.
[0020] Figure 3 is a schematic diagram of the structure of the fuel electrode 10, particularly the structure of the active layer 15. The structure of the active layer 15 (fuel electrode 10) is identified by observing, with a scanning electron microscope (SEM), a surface (hereinafter referred to as the "observation surface") obtained by irradiating a cross section of the active layer 15 including the normal to the interface 15a (see Figure 2) between the electrolyte layer 11 and the active layer 15 from an oblique direction with a focused ion beam (FIB). The observation surface is a smooth cross section with very little deformation of the metal.
[0021] The active layer 15 includes Ni16, which is a metal catalyst having electronic conductivity, and an oxide 17 having oxide ion conductivity. Ni16 is included in pure Ni, Ni-based alloys, cermets, which are composites (sintered bodies) of NiO and solid electrolytes, and the like. NiO included in the cermet changes to Ni16 by hydrogen reduction. NiO remaining after hydrogen reduction is not included in Ni16. Examples of the solid electrolyte included in the cermet include a solid solution of one or more selected from stabilized zirconia and ceria-based solid solutions and alumina, stabilized zirconia, and ceria-based solid solutions. Examples of stabilizers for stabilized zirconia include CaO, MgO, Y2O3, Sc2O3, and Yb2O3. Examples of elements that are solid-solved in ceria in ceria-based solid solutions include Gd, Sm, and Y.
[0022] The oxide 17 is a solid electrolyte, and examples thereof include stabilized zirconia and ceria-based solid solutions. Examples of stabilizers for stabilized zirconia include CaO, MgO, Y2O3, Sc2O3, and Yb2O3. Examples of elements dissolved in ceria in the ceria-based solid solutions include Gd, Sm, and Y. The ceria-based solid solutions have electronic conductivity and oxide ion conductivity.
[0023] The volume ratio of Ni16 in the active layer 15 is preferably 40 vol%-60 vol%. This is to ensure the electronic conductivity of Ni16 and the ionic conductivity of oxide 17. The volume ratio of Ni16 is the volume ratio of Ni16 in the active layer 15 after reduction. The volume ratio of Ni16 is calculated from an SEM image, and is the value (%) obtained by dividing the area of Ni16 by the combined area of Ni16 and oxide 17.
[0024] The gas-permeable active layer 15 includes numerous pores that are three-dimensionally connected. The pores that appear in a cross section (observation surface) of the active layer 15 are one cross section of the numerous pores that are three-dimensionally connected, and include first pores 18 contained in Ni 16, second pores 20 contained in oxide 17, and third pores 22 in contact with Ni 16 and oxide 17. The first interface 19 is the interface between Ni 16 and the first pores 18. The second interface 21 is the interface between the oxide 17 and the second pores 20.
[0025] The third pores 22 form a third interface 23 between the Ni 16 and the third pores 22, and a fourth interface 24 between the oxide 17 and the third pores 22. A fifth interface 25 is an interface between the Ni 16 and the oxide 17. The Ni 16, the oxide 17, and the third pores 22 form a three-phase interface 26 where the third interface 23, the fourth interface 24, and the fifth interface 25 intersect. The three-phase interface 26 is a reaction field where the fuel supplied through the third pores 22, the Ni 16, and the oxide 17 come into contact with each other.
[0026] The oxide 17 is preferably a ceria-based solid solution. + moves to the surface of the ceria and O 2- It is presumed that the reaction field expands not only to the three-phase interface 26 but also to the ceria surface in the vicinity of the three-phase interface 26. This is expected to reduce the reaction overvoltage.
[0027] The structure of the active layer 15 is specified as follows. First, an SEM image is obtained in a rectangular field of view measuring 10 μm in length and 20 μm in width on the observation surface of the active layer 15. The image is processed to obtain three values, for example, so that the pores 18, 20, and 22 are black, the oxide 17 is white, and Ni 16 is gray. Next, the ratio (%) of the number of the first pores 18 to the number of all the pores 18, 20, and 22 is obtained by image analysis. Similarly, the ratio (%) of the length of the first interface 19 to the length of all the third interfaces 23 is obtained by image analysis. These ratios are the average values obtained in three randomly set fields of view. In calculating the ratio of the number of the first pores 18 and the ratio of the length of the first interface 19, those at the edge of the field of view where the entire pores 18 and interfaces 19 and 23 are not visible are excluded.
[0028] The field of view can be set at any position on the active layer 15. When the fuel electrode 10 (see FIG. 2) is a flat plate, the field of view can be set so that the long side of the rectangular field of view is aligned with the interface 15a. If the distance between the interface 15b and the interface 15a between the active layer 15 and the support layer 14 (the thickness of the active layer 15) is 10 μm or more, the long side (20 μm) of the field of view is set along the interface 15a, and the short side (10 μm) of the field of view is set in the thickness direction of the active layer 15. The area of the field of view should be at least 200 μm to ensure the accuracy of quality control. 2 When the thickness of the active layer 15 is less than 10 μm, the short side of the field of view is set to the maximum in the thickness direction of the active layer 15, and the area of the field of view is set to 200 μm. 2 The longer side of the field of view is set along the interface 15a so that the above is achieved.
[0029] The decrease in the ratio of the number of the first pores 18 to the number of all pores 18, 20, 22 appearing in the actual field of the active layer 15 means that Ni16 is in a relatively large particle size because Ni16 approaches a solid state from a porous state. When the Ni16 particles become larger, the three-phase interface 26 shrinks, and the reaction overvoltage tends to increase.
[0030] An increase in the ratio of the number of the first pores 18 to the number of all the pores 18, 20, 22 appearing in the actual field of the active layer 15 means a relative decrease in the number of the pores 20, 22. If the number of the third pores 22 decreases, the three-phase interface 26 shrinks and the fuel supplied to the three-phase interface 26 decreases, making it difficult for the oxidation reaction of combustion to occur. As a result, there is a tendency for the reaction overvoltage to increase.
[0031] The ratio of the number of the first pores 18 to the number of all pores 18, 20, 22 appearing in the actual field of view of the active layer 15 is 10% or more and 40% or less. This expands the three-phase interface 26, making it easier for the oxidation reaction of the fuel to occur. This reduces the reaction overvoltage. Furthermore, since the ratio of the number of the first pores 18 to the number of the pores 18, 20, 22 is used as an index, quality control of mass production can be facilitated.
[0032] The decrease in the ratio of the length of the first interface 19 to the length of all the third interfaces 23 appearing in the actual field of view of the active layer 15 means that Ni16 is relatively large particles because Ni16 approaches a solid state from a porous state. When the Ni16 particles become larger, the three-phase interface 26 shrinks, and the reaction overvoltage tends to increase.
[0033] The increase in the ratio of the length of the first interface 19 to the length of all the third interfaces 23 appearing in the actual field of view of the active layer 15 means that the length of the third interfaces 23 becomes relatively shorter and the cross-sectional area of the third pores 22 becomes smaller. When the cross-sectional area of the third pores 22 becomes smaller, the fuel supplied to the three-phase interface 26 decreases, making it difficult for the oxidation reaction of combustion to occur. As a result, there is a tendency for the reaction overvoltage to increase.
[0034] The ratio of the length of the first interface 19 to the length of all the third interfaces 23 appearing in the actual field of the active layer 15 is preferably 5% or more and 20% or less, which can further reduce the reaction overvoltage. EXAMPLES
[0035] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0036] (Preparation of electrochemical cells) Yttria-stabilized zirconia (YSZ) powder and NiO powder were mixed, and butyral resin, polymethylmethacrylate beads as a pore former, plasticizer, dispersant, and solvent were added and mixed to obtain a slurry. The slurry was made into a green sheet with a thickness of 200 μm by a doctor blade method to obtain a molded body for the support layer. The average particle size of the NiO powder was 0.5 μm, and the mixing ratio (mass ratio) of the YSZ powder and the NiO powder was 50:50.
[0037] Gd-doped ceria (Gd 0.2 Ce 0.8 O 2-δThe powder (GDC powder) and NiO powder were mixed, and butyral resin, polymethylmethacrylate beads as a pore former, plasticizer, dispersant, and solvent were added and mixed to obtain a slurry. The slurry was made into a green sheet with a thickness of 20 μm by the doctor blade method to obtain a green body for the active layer.
[0038] Butyral resin, plasticizer, dispersant, and solvent were added to the YSZ powder and mixed to obtain a slurry. The slurry was made into a green sheet of 10 μm thickness by doctor blade method to obtain a green body of the electrolyte layer. The green bodies of the support layer, active layer, and electrolyte layer were stacked and pressed together, degreased, and then fired at 1350° C. in air to obtain a laminate of the fuel electrode 10 and the electrolyte layer 11.
[0039] Polyvinyl alcohol and a solvent were added to the GDC powder, mixed, and the viscosity was adjusted to obtain a paste. The paste was applied to the electrolyte layer 11 of the laminate by screen printing to form a film. After drying, the laminate was fired at 1200°C in air to obtain a laminate provided with an intermediate layer 12.
[0040] La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ The powder was mixed with polyvinyl alcohol and a solvent, and the viscosity was adjusted to obtain a paste. The paste was applied to the intermediate layer 14 of the laminate by screen printing to form a film. After drying, the film was fired at 1100°C in air to obtain an electrochemical cell 30 provided with an air electrode 13.
[0041] Various electrochemical cells 30 having different structures of the fuel electrode 10 were fabricated by varying the particle size distribution of the NiO powder, which is the raw material of the fuel electrode 10, and the sintering temperature when the fuel electrode 10 was obtained.
[0042] The electrochemical cell 30 was heated in a hydrogen atmosphere so that the fuel electrode 10 was heated to 700° C., thereby reducing the fuel electrode 10. The hydrogen concentration was set to 100%, and the reduction time was set to 1 hour.
[0043] (Performance evaluation test) The electrochemical cell 30 was evaluated as a water vapor electrolysis cell (SOEC). The electrochemical cell 30, which had been subjected to a reduction treatment, was heated to 700° C., hydrogen containing water vapor (H2O: 90 ml / min, H2: 10 ml / min) was supplied to the fuel electrode 10, and air (100 ml / min) was supplied to the air electrode 13. At this time, a current of 1.5 A / cm was applied between the fuel electrode 10 and the air electrode 13. 2 The voltage between the fuel electrode 10 and the air electrode 13 was measured when a current of 1.40 V or less was applied. Voltages of 1.40 V or less were rated as "A," voltages of more than 1.40 V and less than 1.45 V were rated as "B," and voltages of more than 1.45 V were rated as "C."
[0044] (Identification of fuel electrode structure) A sample of the electrochemical cell 30 was embedded in a room temperature curing resin, and the cross section of the active layer 15 perpendicular to the interface between the fuel electrode 10 and the electrolyte layer 11 was polished. The cross section of the active layer 15 was irradiated with FIB from an oblique direction to prepare a smooth observation surface of the active layer 15. An image of the observation surface in a rectangular real field of view measuring 10 μm in length and 20 μm in width was obtained by SEM. After ternary processing was performed to make the pores 18, 20, and 22 black, the oxide 17 white, and Ni16 gray, the ratio (%) of the number of the first pores 18 to the number of all the pores 18, 20, and 22 was obtained by image analysis. Similarly, the ratio (%) of the length of the first interface 19 to the length of all the third interfaces 23 was obtained by image analysis. Table 1 shows the average value of the ratios obtained in three randomly set real fields of view.
[0045] The ratio (%) of the number of first pores 18 to the number of all pores 18, 20, 22, the ratio (%) of the length of first interface 19 to the length of all third interfaces 23, the voltage between the fuel electrode 10 and the air electrode 13 in the performance evaluation test, and the judgment are shown in Table 1.
[0046] [Table 1] As shown in Table 1, No. 1-6 was judged to be A. In No. 1-6, the number of first pores 18 relative to the number of pores 18, 20, and 22 was 10% or more and 40% or less, and the length of first interface 19 relative to the length of third interface 23 was 5% or more and 20% or less. No. 1-6 had a lower electrical resistance between anode 10 and cathode 13 than No. 7-14, and therefore it is presumed that the three-phase interface 26 of anode 10 has expanded.
[0047] No. 7-10 was rated B. In No. 7-10, the number of first pores 18 relative to the number of pores 18, 20, and 22 was 10% or more and 40% or less, but the length of first interface 19 relative to the length of third interface 23 was 3% or 25%. It is presumed that the three-phase interface 26 of the fuel electrode 10 in No. 7-10 was reduced compared to No. 1-6.
[0048] No. 11-14 was rated as C. In No. 11-14, the length of the first interface 19 relative to the length of the third interface 23 was 5% or more and 20% or less, but the number of the first pores 18 relative to the number of the pores 18, 20, and 22 was 5% or 45%. It is presumed that the three-phase interface 26 of the fuel electrode 10 in No. 11-14 was further reduced compared to No. 1-10.
[0049] According to the examples, it was revealed that the reaction overvoltage can be reduced when the number of first pores 18 is 10% or more and 40% or less relative to the number of pores 18, 20, and 22. It was revealed that the reaction overvoltage can be further reduced when the number of first pores 18 is 10% or more and 40% or less relative to the number of pores 18, 20, and 22 and the length of first interface 19 is 5% or more and 20% or less relative to the length of third interface 23.
[0050] The present invention has been described above based on an embodiment, but the present invention is in no way limited to the above embodiment, and it can be easily inferred that various improvements and modifications are possible within the scope of the present invention without departing from the spirit of the present invention.
[0051] In the embodiment, the electrochemical cell 30 in which the intermediate layer 12 is disposed between the electrolyte layer 11 and the air electrode 13 has been described, but the present invention is not necessarily limited to this. It is of course possible to omit the intermediate layer 12 depending on the materials of the electrolyte layer 11 and the air electrode 13.
[0052] In the embodiment, the electrolyte contained in the fuel electrode 10 is Gd 0.2 Ce 0.8 O 2-δ However, the present invention is not limited to this. The electrolyte contained in the fuel electrode 10 can be appropriately selected. [Explanation of symbols]
[0053] 10 Fuel electrodes for electrochemical cells 16 Ni 17 Oxides 18 First pore 19 First Interface 20 Second pore 22 The third pore 23 The Third Interface
Claims
1. A fuel electrode for an electrochemical cell comprising an oxide and Ni as a metal catalyst, A fuel electrode for an electrochemical cell, wherein pores appearing in a cross section of the fuel electrode for an electrochemical cell include first pores contained in the Ni, and the ratio of the number of the first pores to the number of the pores is 10% or more and 40% or less.
2. In the cross section, the interface between the pore and the Ni includes a first interface between the first pore and the Ni; 2. The fuel electrode for an electrochemical cell in accordance with claim 1, wherein the ratio of the length of said first interface to the length of said interface is 5% or more and 20% or less.
Citation Information
Patent Citations
Solid oxide electrochemical cell and method for manufacturing the same
JP2010044966A
Fuel battery cell
JP2014026720A
Solid oxide type fuel battery
JP2015092459A
Electrochemical reaction single cell and electrochemical reaction cell stack
JP2019091584A
Fuel cell
US20130236811A1