How to butt weld stainless steel plates
By employing restraints to align stainless steel plates with specific distance settings, the method controls welding deformation, ensuring consistent angular deformation and reduced deformation amount, facilitating standardized straightening and improved productivity in stainless steel plate welding.
Patent Information
- Application Number
- JP2021059101
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-03-31
AI Technical Summary
Butt welding of stainless steel plates often results in unpredictable welding deformation, particularly angular and buckling deformations, which complicate the straightening process and require individual adjustments, especially in thin stainless steel plates like austenitic and ferritic-austenitic duplex steel sheets.
A method involving the use of first and second restraints to hold thin stainless steel plates with specific distance alignments to control welding deformation, ensuring consistent angular deformation with the weld line as the valley line and reducing the amount of deformation by setting the distance between restraints within a defined range.
This method ensures consistent welding deformation direction and reduced deformation amount, allowing for standardized straightening processes without individual adjustments, enhancing productivity in mass production.
Smart Images

Figure 0007591964000002 
Figure 0007591964000003 
Figure 0007591964000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for butt welding stainless steel plates. [Background technology]
[0002] When stainless steel base materials are butt-welded together without using a filler metal, the base materials may undergo welding deformation at the welded joint after welding, mainly due to thermal contraction in the direction of the weld line.
[0003] When viewed from the welding torch side, the welding deformation of the base material may be a combination of so-called angular distortion, which deforms into a V-shape with the weld line as the valley line, and buckling distortion, which curves the base material along the weld line so that it protrudes toward the welding torch side. This type of welding deformation is likely to occur when the base material is a thin stainless steel plate.
[0004] In order to suppress the welding deformation of the base metal, it is conceivable to set the restraint position of the base metal during welding as close as possible to the groove. However, when the restraint position of the base metal is brought closer to the groove, when viewed from the welding torch side, a welding deformation that combines reverse angular deformation, which is deformation in the opposite direction to the previous angular deformation, and buckling deformation, which is bending of the stainless steel plate along the weld line so that it protrudes to the opposite side from the welding torch side, may occur.
[0005] When welding deformation occurs that is a combination of reverse angular distortion and buckling distortion, the area around the welded part will have a complex shape. Even if the restraining position of the base material is kept constant, the direction of deformation may change as described above due to changes in the mechanical properties and plate thickness of the base material. It is possible to keep the direction of deformation constant by increasing the distance between the restraining devices that restrain each of the pair of base materials, but if the distance between the restraining devices is too wide, the amount of welding deformation itself will become large.
[0006] Such welding distortion problems are more likely to occur in austenitic stainless steel sheets, which have relatively lower yield strength and Young's modulus than ferritic stainless steel sheets. In addition, ferritic-austenitic dual-phase steel sheets, which have relatively higher strength than austenitic stainless steel sheets, are more likely to have welding distortion problems when the welding speed is low.
[0007] It is possible to obtain a welded joint with corrected welding distortion by performing correction on the welded joint after welding. However, as described above, if the welded joint has a complex shape around the weld, if the direction of deformation of the base material changes for each joint, or if the amount of deformation is too large, it becomes necessary to individually adjust the correction conditions according to the deformation state of the joint in the correction process after welding, which causes a problem of the correction process becoming complicated. In order to prevent the correction process from becoming complicated, it is required to make the deformation direction of the welding distortion constant in multiple welded joints manufactured, and further to reduce the amount of deformation itself.
[0008] Patent Document 1 describes a welding machine that uses a stage on which each plate material is placed, a first cooling body and a second cooling body that are respectively in contact with the upper surface of each plate material, a first pressing part and a second pressing part that press each cooling body, and a welding torch in order to butt weld different plate materials together. Patent Document 2 describes a method for preventing angular distortion caused by welding using a deformation suppressing member formed of a gate-shaped member provided to straddle the groove of the steel plate, a lifting plate inserted through the gate-shaped member and fixed to the steel plate, and a tapered pin inserted through approximately the center of the lifting plate in order to prevent deformation caused by welding heat when steel plates are butt welded on a backing metal.
[0009] However, even with the techniques described in Patent Documents 1 and 2, it is difficult to keep constant the welding deformation that occurs during butt welding of stainless steel plates. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2016-198822 A [Patent Document 2] JP 2012-139702 A Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for butt welding of stainless steel plates, which, when mass-producing welded joints, ensures that the welding deformation in each welded joint is in a consistent direction, making it possible to reduce the amount of deformation itself. [Means for solving the problem]
[0012] In order to solve the above problems, the present invention employs the following configuration. [1] A preparation step of arranging two stainless steel plates with a thickness of 3 mm or less so that their ends face each other, and clamping and restraining the two stainless steel plates from the thickness direction with a pair of first restraining devices and a pair of second restraining devices; and a welding process for butt-welding the ends of the opposed stainless steel plates without using a filler metal, In the preparation step, when a predicted width of a weld portion formed by welding is w (mm) and a plate thickness of the stainless steel plate is t (mm), the distance between an end of the first restraining tool and an end of the second restraining tool is set to be equal to or greater than {w+(40-10t)} mm. , 2×{w+(40-10t)}mm or less At the same time, A method for butt welding stainless steel plates, wherein the distance between the end of the stainless steel plate restrained by the first restraining tool and the end of the first restraining tool, and the distance between the end of the stainless steel plate restrained by the second restraining tool and the end of the second restraining tool are aligned within a range of ±5% based on half the distance between the end of the first restraining tool and the end of the second restraining tool. 。 [ 2 The stainless steel sheet is an austenitic stainless steel sheet or a ferritic-austenitic duplex stainless steel sheet, [1]2. The method for butt welding stainless steel plates according to claim 1 . Effect of the Invention
[0013] According to the method for butt welding stainless steel plates of the present invention, the distance between the end of the stainless steel plate and each of the first and second restraining devices is adjusted to within a range of ±5% based on half the distance between the end of the first restraining device and the end of the second restraining device, and the distance between the end of the first restraining device and the end of the second restraining device is set to be equal to or more than {w+(40-10t)} mm, so that during the welding process, there is room for the unrestrained portion to deform toward the opposite side of the welding torch, and it is possible to reliably generate a V-shaped angular deformation in the welded joint with the weld line as the valley line when viewed from the welding torch side. In addition, the occurrence of such angular deformation causes the cross-sectional neutral axis to move toward the welding torch side, and it is possible to generate a buckling deformation that protrudes toward the welding torch side. As a result, the direction of the welding deformation in the welded joint after welding can be made constant for each welded joint, and further, the amount of deformation itself can be reduced.
[0014] Therefore, according to the present invention, when welded joints are mass-produced, the welding deformation in each welded joint is oriented in a uniform direction, and the amount of deformation itself can be reduced. In addition, in the straightening process after welding, straightening can be performed without changing the straightening conditions for each welded joint. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view showing a preparation step of a method for butt welding stainless steel sheets according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a welding process of a method for butt welding stainless steel sheets according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a welded joint produced by the method for butt welding stainless steel plates according to an embodiment of the present invention. [Figure 4]FIG. 4 is a schematic diagram showing a preparation step of the method for butt welding stainless steel plates according to an embodiment of the present invention, and is a schematic plan view seen from the welding torch side. [Diagram 5] FIG. 5 is a schematic diagram illustrating angular deformation and reverse angular deformation. [Figure 6] FIG. 6 is a schematic diagram illustrating the amount of deformation of a welded joint. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] A method for butt welding stainless steel plates according to an embodiment of the present invention will be described with reference to the drawings.
[0017] The welding target of the welding method of this embodiment is a stainless steel plate. In particular, when austenitic stainless steel plates or ferritic-austenitic duplex stainless steel plates are used to mass-produce welded joints by the welding method of this embodiment, the welding deformation in each welded joint is in a constant direction, and the deformation amount itself can be reduced. Note that the welding method of stainless steel plates of this embodiment is not limited to austenitic stainless steel plates or ferritic-austenitic duplex stainless steel plates, and can also be suitably applied to other stainless steel plates such as ferritic stainless steel plates.
[0018] Moreover, the stainless steel plate to be welded is a thin steel plate with a plate thickness of 3 mm or less. Since a steel plate with a small plate thickness is prone to welding deformation, it is particularly suitable for use as a welding object in the welding method of this embodiment. The plate thickness is more preferably 1 to 3 mm, and may be 1 to 2 mm. By making the plate thickness 1 mm or more, the temperature gradient in the plate thickness direction at the welded portion during welding does not become too small, and buckling deformation does not become complicated. Furthermore, by making the plate thickness 3 mm or less, the penetration depth during welding becomes sufficient, and welding becomes possible without using a filler metal.
[0019] A groove may be provided on the end face of the stainless steel plate to be welded. The shape of the groove formed by butting the groove parts is preferably an I-groove. Also, the end face of the stainless steel plate may be left as it is without groove preparation. In the case of an I-groove, the root spacing is 0 mm.
[0020] The method for welding stainless steel sheets according to the present embodiment includes a preparation step and a welding step. Each step will be described below.
[0021] (preparation process) 1 and 4, in the preparation step, two stainless steel plates 1 and 2 are arranged so that their respective ends 1a and 2a face each other, and then the stainless steel plates 1 and 2 are restrained. As described above, a groove may be provided at each of the ends 1a and 2a.
[0022] In this embodiment, a first restraining device 3 and a second restraining device 4 are used to restrain the stainless steel plates 1, 2. The first restraining device 3 is composed of a pair of two block-shaped restraining bodies 3a, 3b, which sandwich and restrain one of the stainless steel plates 1 in the plate thickness direction. The second restraining device 4, like the first restraining device 3, is composed of a pair of two block-shaped restraining bodies 4a, 4b, which sandwich and restrain the other stainless steel plate 2 in the plate thickness direction.
[0023] 4, the first restraining device 3 and the second restraining device 4 extend along the longitudinal direction of the ends 1a, 2a of the stainless steel plates 1, 2. The first restraining device 3 and the second restraining device 4 are arranged with respect to the stainless steel plates 1, 2 so that the ends 3c, 4c of the first restraining device 3 and the second restraining device 4 on the steel plate end side are parallel to the ends 1a, 2a of the steel plates.
[0024] The lengths D1, D2 of the first restraining device 3 and the second restraining device 4 are made longer than the length of the ends 1a, 2a or the same as the length of the ends 1a, 2a, as shown in Fig. 4. If the lengths D1, D2 of the first restraining device 3 and the second restraining device 4 are shorter than the length of the ends 1a, 2a, regions of the stainless steel plates 1, 2 that are not restrained will be generated, which will result in unexpected welding deformation, and this is not preferable.
[0025] Furthermore, the widths h1, h2 of the first restraining device 3 and the second restraining device 4 are not particularly limited as long as they are wide enough to reliably restrain the stainless steel plates 1, 2, respectively.
[0026] Each of the stainless steel plates 1 and 2 is restrained by a first restraining device 3 and a second restraining device 4 at a position away from the ends 1a and 2a of the stainless steel plates 1 and 2. As shown in FIG. 4, the distance L1 between the tip of the end 1a of one of the stainless steel plates 1 restrained by the first restraining device 3 and the end 3c of the first restraining device 3, and the distance L2 between the tip of the end 2a of the other stainless steel plate 2 restrained by the second restraining device 4 and the end 4c of the second restraining device 4 are set to half the distance (L1+L2) between the end 3c of the first restraining device 3 and the end 4c of the second restraining device 4, and are aligned within a range of ±5% of this standard. If the distances L1 and L2 are out of this range, it becomes difficult to control the welding deformation after welding to a planned deformation state.
[0027] In the preparation step, the distance M between the end 3c of the first restraining device 3 on the steel plate end side and the end 4c of the second restraining device 4 on the steel plate end side is set to be {w+(40-10t)}mm or more, where w (mm) is the predicted width of the welded portion to be formed in the next welding step, and t (mm) is the thickness of the stainless steel plate. The upper limit of the distance M may be set to be 2×{w+(40-10t)}mm or less. More preferably, the distance M between the end 3c of the first restraining device 3 and the end 4c of the second restraining device 4 is set to be {w+(40-10t)}mm or more. The distance M may be set to be 1.1×{w+(40-10t)}mm or less. Most preferably, the distance M is set to be {w+(40-10t)}mm.
[0028] The smaller the plate thickness t of the stainless steel plates 1 and 2 serving as the base material, the smaller the gradient of the temperature distribution in the plate thickness direction of the welded portion receiving the welding heat input becomes, and the less likely angular distortion occurs. Therefore, by increasing the interval M between the end 3c of the first restraining device 3 and the end 4c of the second restraining device 4, it is possible to suppress unexpected welding deformation. On the other hand, if the interval M between the end 3c of the first restraining device 3 and the end 4c of the second restraining device 4 is too wide, the restraining force by the first and second restraining devices 3 and 4 at the ends 1a and 2a becomes weak, and the amount of deformation becomes large. In addition, the interval M between the end 3c of the first restraining device 3 and the end 4c of the second restraining device 4 needs to be at least equal to or larger than the width w of the welded portion. Based on the above knowledge, the present inventor conducted experiments and found the above range.
[0029] If the distance between the end 3c of the first restraint device 3 on the steel plate end side and the end 4c of the second restraint device 4 on the steel plate end side is less than {w+(40-10t)} mm, angular deformation (reverse angular deformation (see Figure 5(b))) may occur in which the weld line is bent when viewed from the welding torch side, and buckling deformation may occur in which the stainless steel plates 1 and 2 are curved along the weld line direction so as to protrude on the opposite side from the welding torch side. The combination of such unexpected deformations causes more complex deformations in the vicinity of the weld line, making post-welding correction difficult.
[0030] If the distance M between the end 3c of the first restraint device 3 on the steel plate end side and the end 4c of the second restraint device 4 on the steel plate end side exceeds 2×{w+(40-10t)} mm, the distance between the first restraint device 3 and the second restraint device 4 and the ends 1a, 2a of the steel plate will become wider, which will weaken the restraining force on the ends 1a, 2a and increase the amount of welding deformation.
[0031] The predicted width w (mm) of the weld is the predicted value of the width of the weld metal on the welding torch side of the weld formed by the welding process. This predicted width w is determined by conducting a preliminary test. In the preliminary test, welding is performed under the same welding conditions as those in the welding process, using stainless steel plates that are the same in material, plate thickness, and end shape as the stainless steel plates to be welded. The width of the weld formed in the preliminary test is taken as the predicted width w.
[0032] (Welding process) Next, as shown in Fig. 2, in the welding process, a welding torch 10 is placed against the opposed ends 1a, 2a, and butt welding is performed without using a filler metal. The welding method is laser welding or non-consumable electrode gas shielded arc welding, preferably TIG welding. The welding method is one-sided welding. Other welding conditions are not particularly limited.
[0033] In this embodiment, backing is not necessary. If backing is provided, the periphery of the ends 1a and 2a will be constrained more strongly than necessary, and buckling deformation may become large due to thermal contraction of the welded portion after welding.
[0034] Fig. 3 shows the state after welding is completed. A weld 20 is formed by welding. This results in a welded joint 30 in which the stainless steel plates 1 and 2 are joined by the weld. The predicted width w of the weld 20 used to determine the interval M is determined based on the width of the weld of the welded joint obtained by the preliminary test, as described above. For reference, Fig. 3 shows the measurement range of the width of the weld measured in the preliminary test by a dimension line together with the symbol w.
[0035] In the welded joint 30 obtained by the welding method of this embodiment, when viewed from the welding torch side during welding, by releasing the restraint by the first and second restraint parts 3 and 4, a welding deformation occurs that is a combination of so-called angular deformation, which deforms into a V-shape with the weld line as a valley line, and buckling deformation, which bends the base material along the weld line so as to protrude toward the welding torch side. This welding deformation is a planned deformation. Even if the welded joints 30 are mass-produced by the welding method of this embodiment, the directions of the angular distortion and buckling deformation do not change for each welded joint. Furthermore, the amount of deformation in each welded joint 30 is also small. As a result, when performing a correction process after welding, it is not necessary to adjust the correction conditions for each welded joint 30 according to the deformation state of the welded joint 30.
[0036] As described above, according to the method for butt welding stainless steel plates of this embodiment, the distance between the ends 1a, 2a of the stainless steel plates 1, 2 and the ends 3c, 4c of the first restraining device 3 and the second restraining device 4 is adjusted to within a range of ±5% based on half the distance between the end 3c of the first restraining device 3 and the end 4c of the second restraining device 4, and the distance M between the end 3c of the first restraining device 3 and the end 4c of the second restraining device 4 is set to {w+(40-10t)} mm or more, so that during the welding process, there is room for the unrestrained portion to deform toward the opposite side of the welding torch 10, and this ensures that a V-shaped angular deformation with the weld line as a valley line can be generated in the weld joint 30 when viewed from the welding torch 10 side. In addition, the occurrence of such angular deformation causes the cross-sectional neutral axis to move toward the welding torch 10 side, and buckling deformation that protrudes toward the welding torch 10 side along the weld line can be generated. As a result, in this embodiment, when mass-producing welded joints 30, the direction of welding deformation in the welded joints 30 after welding can be made constant for each welded joint 30, and further, the amount of deformation itself can be reduced. Then, in the straightening process after welding, straightening can be performed without adjusting the straightening conditions for each welded joint 30. EXAMPLES
[0037] Two stainless steel plates with a length of 200 mm, a width of 75 mm, and a thickness of 1.5 mm (steel type: SUS316L), two stainless steel plates with a length of 200 mm, a width of 75 mm, and a thickness of 2.0 mm (steel type: SUS316L), two stainless steel plates with a length of 200 mm, a width of 75 mm, and a thickness of 2.0 mm (steel type: NSSC2351, manufactured by Nippon Steel Stainless Steel Corporation), and two stainless steel plates with a length of 200 mm, a width of 75 mm, and a thickness of 2.0 mm (steel type: NSSC2120, manufactured by Nippon Steel Stainless Steel Corporation) were prepared. SUS316L is an austenitic stainless steel plate, and NSSC2351 and NSSC2120 are ferritic-austenitic duplex stainless steel plates.
[0038] Next, as a preparation step, the two stainless steel plates were arranged so that their end faces (200 mm long ends) parallel to the length direction faced each other, and then each stainless steel plate was restrained. In addition, when arranging the two stainless steel plates to be welded, they were arranged so that they were horizontal.
[0039] In order to restrain each stainless steel plate, a first restraining tool and a second restraining tool as shown in Fig. 1 and Fig. 4 were used. The first restraining tool and the second restraining tool extended along the longitudinal direction of the ends of the stainless steel plates parallel to the longitudinal direction, as shown in the schematic plan view of Fig. 4. The first restraining tool and the second restraining tool were also placed on each stainless steel plate so that the ends of the first restraining tool and the second restraining tool on the steel plate end side were parallel to the steel plate end.
[0040] The distance L1 between the end of one stainless steel plate restrained by the first restraining tool and the end of the first restraining tool, and the distance L2 between the end of the other stainless steel plate restrained by the second restraining tool and the end of the second restraining tool were the same length. The distance between the end of the first restraining tool on the side of the steel plate end and the end of the second restraining tool on the side of the steel plate end was as shown in Table 1.
[0041] Next, the opposed ends were butt-welded without using a filler metal. The welding method was TIG welding, and the welding speed and welding heat input were as shown in Table 1. One-sided welding was used as the welding procedure. In this manner, welded joints were produced. Three welded joints were produced for each condition number.
[0042] In addition, no backing was performed.
[0043] The direction of angular distortion was checked for the welded joints obtained. Three welded joints were produced for each condition, and all welded joints were marked as "○" if they were deformed into a V-shape with the weld line as a valley line when viewed from the welding torch side during welding. On the other hand, some or all of the welded joints were marked as "×" if they were deformed in the opposite direction so that the weld line became a crest line when viewed from the welding torch side during welding. The results are shown in Table 1. An example of deformation in the case of "○" is shown in Figure 5(a), and an example of deformation in the case of "×" is shown in Figure 5(b).
[0044] In addition, the amount of deformation after welding was evaluated for the welded joints that were evaluated as having an angular distortion direction of "○". The amount of deformation was evaluated by measuring the deformation angle θ centered on the welded part in a cross section in the plate thickness direction perpendicular to the longitudinal direction of the welded joint. Figure 6 shows the deformation angle θ. The deformation angle θ was defined as the inclination angle of one side of the stainless steel plate with respect to the horizontal plane M when the welded joint was placed on the horizontal plane M. When the deformation angle θ was 0 to 2° or less, the amount of deformation was small and was evaluated as "○", and when the deformation angle θ was more than 2°, the amount of deformation was large and was evaluated as "×". The results are shown in Table 1.
[0045] As shown in Table 1, all three welded joints manufactured under conditions where the spacing between the restraining devices satisfied the present invention were deformed into a V-shape with the weld line as the valley line when viewed from the welding torch side during welding, as shown in Figure 5(a). Thus, welded joints whose manufacturing conditions satisfied the present invention had a consistent direction of welding deformation in the welded joint after welding, and the deformation angle θ of the lateral bending could be kept in the range of 0 to 2°.
[0046] On the other hand, as shown in Table 1, some of the three welded joints manufactured under conditions where the spacing of the restraining devices did not satisfy the requirements of the present invention were deformed so that the weld line became a crest line when viewed from the welding torch side during welding, as shown in Figure 5(b). Therefore, the direction of the welding deformation was different for each welded joint.
[0047] For this reason, in the case of the invention examples, the deformation of the welded joint could be corrected using constant correction conditions regardless of the welded joint, but in the case of the comparative examples, it became necessary to adjust the correction conditions for each welded joint, which reduced the productivity of the welded joint.
[0048] [Table 1] [Explanation of symbols]
[0049] 1...one stainless steel plate (stainless steel plate), 2...other stainless steel plate (stainless steel plate), 1a, 2a...end, 3...first restraint, 4...second restraint, 3c...end of first restraint, 4c...end of second restraint, 10...welding torch, 30...welded joint, M...spacing.
Claims
1. A preparation step of arranging two stainless steel plates each having a thickness of 3 mm or less so that their ends face each other, and clamping and restraining the two stainless steel plates from the thickness direction using a pair of first restraining devices and a pair of second restraining devices; and a welding process for butt-welding the ends of the opposed stainless steel plates without using a filler metal, In the preparation step, when a predicted width of a weld portion formed by welding is w (mm) and a plate thickness of the stainless steel plate is t (mm), a distance between an end of the first restraint device and an end of the second restraint device is set in a range of {w+(40-10t)} mm or more and 2×{w+(40-10t)} mm or less; A method for butt welding stainless steel plates, wherein the distance between the end of the stainless steel plate restrained by the first restraint device and the end of the first restraint device, and the distance between the end of the stainless steel plate restrained by the second restraint device and the end of the second restraint device are aligned to within a range of ±5% based on half the distance between the end of the first restraint device and the end of the second restraint device.
2. 2. The method for butt welding stainless steel plates according to claim 1, wherein the stainless steel plates are austenitic stainless steel plates or ferritic-austenitic duplex stainless steel plates.
Citation Information
Patent Citations
The welding jig for preventing deformation
JP1986046084U
JP1987105786U
Device and method for butt welding of beltlike metallic sheet
JP1999347792A
Deformation suppression member for welded joint, and deformation suppression method using the deformation suppression member
JP2012139702A
Refrigerating machine and welding device
JP2016198822A