Test method and semiconductor device manufacturing method
A method for rapidly assessing thermal grease pump-out performance by varying plate distance and observing shape changes addresses the inefficiency of existing thermal shock tests, enabling quick determination of deformation characteristics.
Patent Information
- Application Number
- JP2022005047
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-17
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-01-17
AI Technical Summary
Existing methods for determining the pump-out performance of thermal grease are time-consuming due to the need for repeated thermal shock tests.
A test method involving arranging thermal grease between two plates, varying the distance between them, and observing the grease's shape to determine pump-out performance.
Enables rapid determination of thermal grease pump-out performance by analyzing shape changes and load variations, allowing for quick assessment of deformation characteristics.
Smart Images

Figure 0007592039000001 
Figure 0007592039000002 
Figure 0007592039000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a testing method and a manufacturing method for a semiconductor device. [Background technology]
[0002] Heat dissipation grease placed between a semiconductor package and a heat dissipation fin or the like can experience pumping out. Pumping out is a phenomenon in which the heat dissipation grease moves from the location where it should be placed due to changes in warping caused by temperature changes in the semiconductor package, causing the heat dissipation function of the heat dissipation grease to be lost.
[0003] Japanese Patent Laid-Open Publication No. 2004-039829 (Patent Document 1) describes a method for determining the pumping-out performance of thermal grease. In Patent Document 1, the pumping-out performance of the thermal grease is determined by performing a thermal shock test with the thermal grease sandwiched between two glass plates. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-039829 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the method of testing the pumping-out performance of thermal grease described in Patent Document 1 requires repeated thermal shock tests, making it difficult to determine the pumping-out performance of the thermal grease in a short period of time.
[0006] The present disclosure has been made in consideration of the above-mentioned problems of the conventional technology. More specifically, the present disclosure provides a test method capable of determining the pumping-out performance of a thermal grease in a short period of time. [Means for solving the problem]
[0007] The disclosed testing method includes the steps of placing the thermal grease on a retaining plate, placing a pressure plate opposite the retaining plate so as to sandwich the thermal grease, varying the distance between the retaining plate and the pressure plate, and observing the shape of the thermal grease after varying the distance between the retaining plate and the pressure plate. The pumping-out performance is determined based on the shape of the thermal grease. Effect of the Invention
[0008] The test method disclosed herein makes it possible to determine the pumping-out performance of the thermal grease in a short period of time. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a first cross-sectional view for explaining an outline of a test method according to the first embodiment. [Diagram 2] FIG. 2 is a second cross-sectional view for explaining an outline of the test method according to the first embodiment. [Diagram 3] 13 is a schematic plan view of the heat dissipating grease 20 when the pressure plate 30 is moved so that the gap between the holding plate 10 and the pressure plate 30 becomes larger. FIG. [Figure 4] 4 is a schematic plan view of the heat dissipating grease 20 when the pressure plate 30 is moved from the state shown in FIG. 3 so that the gap between the holding plate 10 and the pressure plate 30 becomes smaller. FIG. [Diagram 5] 1 is a schematic diagram of a test apparatus 100 used in a test method according to a first embodiment. [Figure 6] 4 is a schematic graph showing the relationship between the displacement of the pressure plate 30 and the load applied to the pressure plate 30. [Figure 7A] 2 is a cross-sectional view of the thermal grease 20 in a first state. FIG. [Figure 7B] 4 is a cross-sectional view of the thermal grease 20 in a second state. FIG. [Figure 7C] FIG. 4 is a cross-sectional view of the thermal grease 20 in a third state. [Figure 7D] 11 is a cross-sectional view of the thermal grease 20 in a fourth state. FIG. [Figure 7E] 13 is a cross-sectional view of the thermal grease 20 in a fifth state. FIG. [Figure 7F] 13 is a cross-sectional view of the thermal grease 20 in a sixth state. FIG. [Figure 8] FIG. 2 is a schematic cross-sectional view of a semiconductor device 200. [Figure 9] 2 is a manufacturing process diagram of the semiconductor device 200. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The details of the embodiments of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are designated by the same reference numerals, and redundant description will not be repeated.
[0011] Embodiment 1 A test method according to the first embodiment will be described.
[0012] (Determination of pumping-out characteristics based on thermal grease shape) Fig. 1 is a first cross-sectional view for explaining an outline of a test method according to the first embodiment. As shown in Fig. 1, the holding plate 10 is a plate-shaped member. The holding plate 10 has a first main surface 10a and a second main surface 10b. The first main surface 10a and the second main surface 10b are end surfaces in the thickness direction of the holding plate 10. The second main surface 10b is the opposite surface to the first main surface 10a.
[0013] The retaining plate 10 is made of, for example, a metal material. The retaining plate 10 may be made of glass. The retaining plate 10 may be selected according to the semiconductor package in which the thermal grease 20 is used. For example, when the thermal grease 20 is disposed on a copper base of a nickel-plated semiconductor package, the retaining plate 10 may be a nickel-plated copper plate.
[0014] The heat dissipating grease 20 is disposed on the retaining plate 10. More specifically, the heat dissipating grease 20 is disposed on the first main surface 10a. The shape of the heat dissipating grease 20 is, for example, circular in plan view. However, the planar shape of the heat dissipating grease 20 is not limited thereto. The heat dissipating grease 20 is, for example, a heat dissipating grease in which a filler is dispersed in silicone. The heat dissipating grease 20 is, for example, liquid at room temperature. The heat dissipating grease 20 may be formed of a phase change thermal interface material (PC-TIM). The phase change thermal interface material is a material that is solid at room temperature but becomes liquid at a predetermined temperature or higher.
[0015] The heat dissipating grease 20 is disposed on the holding plate 10 (first main surface 10a) by being printed on the holding plate 10 (first main surface 10a) by screen printing or the like. When the heat dissipating grease 20 is formed from a phase change thermal interface material, the heat dissipating grease 20 is disposed on the holding plate 10 by printing it on the holding plate 10 and then volatilizing the solvent.
[0016] The pressing plate 30 is a plate-shaped member. The pressing plate 30 has a third main surface 30a and a fourth main surface 30b. The third main surface 30a and the fourth main surface 30b are end surfaces in the thickness direction of the pressing plate 30. The fourth main surface 30b is the opposite surface to the third main surface 30a. The pressing plate 30 is disposed opposite the holding plate 10 so as to sandwich the heat dissipating grease 20. More specifically, the pressing plate 30 is disposed so that the third main surface 30a faces the first main surface 10a with the heat dissipating grease 20 interposed therebetween. The pressing plate 30 is formed, for example, from a material that transmits visible light.
[0017] The spacer 40 is disposed between the holding plate 10 and the pressing plate 30 (between the first main surface 10a and the third main surface 30a). The spacer 40 maintains the distance between the holding plate 10 and the pressing plate 30. That is, the spacer 40 makes it possible to control the thickness of the heat dissipating grease 20. The spacer 40 is, for example, a shim tape.
[0018] Fig. 2 is a second cross-sectional view for explaining an outline of the test method according to the first embodiment. Fig. 3 is a schematic plan view of the heat dissipating grease 20 when the pressing plate 30 is moved so that the distance between the holding plate 10 and the pressing plate 30 becomes larger. In Fig. 3, the shape of the heat dissipating grease 20 before deformation is indicated by a dotted line. As shown in Figs. 2 and 3, when the pressing plate 30 is moved so that the distance between the holding plate 10 and the pressing plate 30 (the distance between the first main surface 10a and the third main surface 30a) becomes larger, the heat dissipating grease 20 is stretched, and the shape of the heat dissipating grease 20 in plan view changes.
[0019] The planar shape of the thermal grease 20 is observed through the pressure plate 30 in a direction perpendicular to the first main surface 10a. This planar shape of the thermal grease 20 is affected by the ease (or difficulty) of deformation of the thermal grease 20. Therefore, the pumping-out performance of the thermal grease 20 is judged by observing the planar shape of the thermal grease 20 after the pressure plate 30 is moved.
[0020] FIG. 4 is a schematic plan view of the thermal grease 20 when the pressure plate 30 is moved so that the gap between the holding plate 10 and the pressure plate 30 is reduced from the state shown in FIG. 3. In FIG. 4, the shape of the thermal grease 20 before deformation is shown by a dotted line. As shown in FIG. 4, after the pressure plate 30 is moved so that the gap between the holding plate 10 and the pressure plate 30 is once increased and then reduced, voids 21 are formed in the thermal grease 20. The pumping-out performance of the thermal grease 20 is determined by measuring the size and / or number of the voids 21. In the state shown in FIG. 4, the pressure plate 30 is returned to the initial position.
[0021] In the example shown in Figure 3, the pumping-out performance of the heat-dissipating grease 20 was determined based on the shape of the heat-dissipating grease 20 after the pressure plate 30 is moved so that the gap between the retaining plate 10 and the pressure plate 30 becomes larger, but the pumping-out performance of the heat-dissipating grease 20 may also be determined based on the shape of the heat-dissipating grease 20 after the pressure plate 30 is moved so that the gap between the retaining plate 10 and the pressure plate 30 becomes smaller.
[0022] 4, the pumping-out performance was determined based on the shape of the heat-dissipating grease 20 after the pressure plate 30 was moved so that the gap between the retaining plate 10 and the pressure plate 30 was once increased and then decreased, but the combination of the movement directions of the pressure plate 30 is not limited to the example shown in Fig. 4. In other words, the combination of the movement directions of the pressure plate 30 and the movement distance of the pressure plate 30 may be appropriately selected depending on the characteristics of the heat-dissipating grease 20.
[0023] (Evaluation of pumping-out characteristics based on changes in the load applied to the retaining plate) Fig. 5 is a schematic diagram of a test apparatus 100 used in the test method according to the first embodiment. As shown in Fig. 5, the test apparatus 100 has a holding plate 10, a pressing plate 30, a temperature regulator 50, an attachment jig 60, and a driving unit 70. As described above, the heat dissipating grease 20 is sandwiched between the holding plate 10 and the pressing plate 30. In addition, a spacer 40 may be disposed between the holding plate 10 and the pressing plate 30.
[0024] The holding plate 10 is disposed on the temperature regulator 50. The second main surface 10b faces the temperature regulator 50. The temperature regulator 50 is configured to be able to adjust the temperature of the holding plate 10. This makes it possible to judge the pumping-out performance of the heat dissipation grease 20 in an environment that simulates a temperature rise of a semiconductor package. The temperature regulator 50 is, for example, a hot plate. However, the temperature regulator 50 is not limited to this. The temperature regulator 50 may be configured to be able to cool the holding plate 10 by water cooling or a Peltier element, etc.
[0025] The mounting jig 60 is connected to the pressing plate 30. More specifically, the mounting jig 60 is connected to the fourth main surface 30b side of the pressing plate 30 by a rod 61. An imaging device 62 may be attached to the mounting jig 60. The imaging device 62 makes it possible to observe the planar shape of the thermal grease 20 through the pressing plate 30. The imaging device 62 is, for example, a digital camera.
[0026] When the testing apparatus 100 has the imaging device 62, the change in shape of the thermal grease 20 and the size and number of the voids 21 may be measured by performing image processing on the image of the thermal grease 20 captured by the imaging device 62. This image processing is, for example, a binarization process on the image captured by the imaging device 62. Note that when the testing apparatus 100 does not have the imaging device 62, the change in shape of the thermal grease 20 and the size and number of the voids 21 may be observed visually.
[0027] The driving unit 70 is connected to the mounting jig 60. The driving unit 70 moves the pressure plate 30 via the mounting jig 60 so that the distance between the holding plate 10 and the pressure plate 30 changes. The load applied to the pressure plate 30 is measured by a load sensor 71 attached to the driving unit 70. Note that, when the testing apparatus 100 has the driving unit 70, the spacer 40 does not have to be disposed between the holding plate 10 and the pressure plate 30.
[0028] Fig. 6 is a schematic graph showing the relationship between the displacement of the pressure plate 30 and the load applied to the pressure plate 30. The horizontal axis of the graph in Fig. 6 represents the displacement of the pressure plate 30, and the vertical axis of the graph in Fig. 6 represents the load applied to the pressure plate 30.
[0029] The state in which the pressure plate 30 is located between the origin and position P1 in FIG. 6 is referred to as a first state. The state in which the pressure plate 30 is located between positions P1 and P2 in FIG. 6 is referred to as a second state. The state in which the pressure plate 30 is located between positions P2 and P3 in FIG. 6 is referred to as a third state. The state in which the pressure plate 30 is located between positions P3 and P4 in FIG. 6 is referred to as a fourth state. The state in which the pressure plate 30 is located between positions P4 and P5 in FIG. 6 is referred to as a fifth state. The state in which the pressure plate 30 is located between positions P5 and P6 in FIG. 6 is referred to as a sixth state.
[0030] Fig. 7A is a cross-sectional view of the thermal grease 20 in a first state. Fig. 7B is a cross-sectional view of the thermal grease 20 in a second state. Fig. 7C is a cross-sectional view of the thermal grease 20 in a third state. Fig. 7D is a cross-sectional view of the thermal grease 20 in a fourth state. Fig. 7E is a cross-sectional view of the thermal grease 20 in a fifth state. Fig. 7F is a cross-sectional view of the thermal grease 20 in a sixth state.
[0031] 6 and 7A, in the first state, the driving unit 70 moves the pressing plate 30 away from the spacer 40. At this time, the load sensor 71 detects the weight of the pressing plate 30 and the mounting jig 60.
[0032] As shown in FIG. 6 and FIG. 7B, in the second state, the driving unit 70 moves the pressing plate 30 so that the distance between the holding plate 10 and the pressing plate 30 becomes larger. At this time, as the displacement of the pressing plate 30 becomes larger, the load applied to the pressing plate 30 becomes larger. When the thermal grease 20 is a material that is easily deformed, the force with which the thermal grease 20 pulls the pressing plate 30 is small, so the slope of the graph in FIG. 6 between positions P1 and P2 becomes small. On the other hand, when the thermal grease 20 is a material that is not easily deformed, the force with which the thermal grease 20 pulls the pressing plate 30 is large, so the slope of the graph in FIG. 6 between positions P1 and P2 becomes large. Therefore, the pumping-out characteristic of the thermal grease 20 can be determined based on the slope of the graph in FIG. 6 between positions P1 and P2.
[0033] 6 and 7C, in the third state, the drive unit 70 holds the position of the pressure plate 30. If the deformation of the thermal grease 20 cannot keep up with the moving speed of the pressure plate 30, the shape of the thermal grease 20 will change if left alone, and the force with which the thermal grease 20 pulls the pressure plate 30 will gradually be released. This behavior also makes it possible to grasp how easily (or how difficult) the thermal grease 20 deforms, and therefore to determine the pumping-out characteristics of the thermal grease 20.
[0034] 6 and 7D, in the fourth state, the drive unit 70 moves the pressure plate 30 so that the distance between the retaining plate 10 and the pressure plate 30 becomes smaller. At this time, as the displacement of the pressure plate 30 becomes smaller, the load applied to the pressure plate 30 becomes smaller. Since the fourth state shows behavior that is generally opposite to that of the second state, the pumping-out characteristics of the thermal grease 20 can be determined based on the slope of the graph in FIG. 6 between positions P3 and P4.
[0035] As shown in Fig. 6 and Fig. 7E, in the fifth state, the driving unit 70 moves the pressing plate 30 so that the gap between the holding plate 10 and the pressing plate 30 becomes even smaller. At this time, the filler and the like inside the thermal grease 20 are compressed, so that the shear force inside the thermal grease 20 increases and a repulsive force is applied to the pressing plate 30. The slope of the graph in Fig. 6 between positions P4 and P5 changes depending on the size and ease of deformation of the filler inside the thermal grease 20. Therefore, the pumping-out characteristic of the thermal grease 20 can be determined based on the slope of the graph in Fig. 6 between positions P4 and P5.
[0036] As shown in Figures 6 and 7F, in the sixth state, the drive unit 70 holds the position of the retaining plate 30. The repulsive force described above is relieved over time due to the movement of the filler and resin inside the thermal grease 20. This behavior also makes it possible to determine the pumping-out characteristics of the thermal grease 20. As described above, the pumping-out characteristics of the thermal grease 20 can be determined based on the slope of the load change in the second state, the slope of the load change in the fourth state, the slope of the load change in the fifth state, the load change over time in the third state, and the load change over time in the sixth state.
[0037] The pumping-out characteristics of the thermal grease 20 may be determined by at least one of the slope of the load change in the second state, the slope of the load change in the fourth state, the slope of the load change in the fifth state, the load change over time in the third state, and the load change over time in the sixth state. The pumping-out characteristics of the thermal grease 20 may also be determined by a combination of two or more of these.
[0038] The results will vary depending on the moving speed of the pressure plate 30 in the second, fourth, and fifth states and the holding time in the third and sixth states, even when tests are performed on the same thermally conductive grease 20. Therefore, depending on the characteristics of the thermally conductive grease 20 to be measured, it is preferable that the moving speed and holding time of the pressure plate 30 be set to 1 μm / sec or more and 1 mm / sec or less and 0 minutes or more and 10 minutes or less, respectively.
[0039] When the pumping-out characteristics of the thermal grease 20 are determined based on the load applied to the pressure plate 30 when the pressure plate 30 is moved, the test device 100 does not need to have the imaging device 62, and the pressure plate 30 does not need to be made of a material that transmits visible light. However, even when the pumping-out characteristics of the thermal grease 20 are determined based on the load applied to the pressure plate 30 when the pressure plate 30 is moved, the test device 100 may have the imaging device 62 and the pressure plate 30 may be made of a material that transmits visible light in order to check for any abnormalities in the test.
[0040] (effect) As described above, in the test method according to embodiment 1, the pumping-out characteristics of the heat-dissipating grease 20 can be determined by applying one cycle of deformation to the heat-dissipating grease 20, and therefore the pumping-out performance of the heat-dissipating grease can be determined in a short period of time.
[0041] In the test method according to the first embodiment, when the pumping-out characteristics of the thermal grease 20 are determined by observing the planar shape of the thermal grease 20 after the gap between the retaining plate 10 and the pressure plate 30 is once increased and then decreased, the pumping-out characteristics can be determined quantitatively in a short time based on the size or number of voids 21. In the test method according to the first embodiment, when the planar shape of the thermal grease 20 is observed after the pressure plate 30 is moved using the imaging device 62, the pumping-out performance of the thermal grease can be determined quantitatively in a short time based on image processing of the acquired image.
[0042] As described above, in the test method of embodiment 1, the pumping-out characteristics of the heat-dissipating grease 20 can be determined based on the change in the load applied to the pressure plate 30 when the pressure plate 30 is moved or held, so that the pumping-out performance of the heat-dissipating grease can be determined quantitatively in a short period of time.
[0043] Embodiment 2 The following describes a method for manufacturing a semiconductor device according to the second embodiment. The semiconductor device according to the second embodiment is designated as a semiconductor device 200.
[0044] FIG. 8 is a schematic cross-sectional view of a semiconductor device 200. As shown in FIG. 8, the semiconductor device 200 has a semiconductor package 210 and heat dissipation grease 20. A base 211 is exposed from the back surface of the semiconductor package 210. The heat dissipation grease 20 is disposed on the base 211. Note that heat dissipation fins 220 are attached to the semiconductor device 200 after pre-assembly. The heat dissipation fins 220 are disposed on the heat dissipation grease 20. The semiconductor package 210 Heat generated inside is transferred to the heat dissipation fins 220 via the base 211 and the heat dissipation grease 20 , and is dissipated from the heat dissipation fins 220 .
[0045] Fig. 9 is a manufacturing process diagram of the semiconductor device 200. As shown in Fig. 9, the manufacturing method of the semiconductor device 200 includes a preparation step S1, a printing step S2, a drying step S3, and an inspection step S4. In the preparation step S1, a semiconductor package 210 is prepared.
[0046] In the printing step S2, the thermal grease 20 is printed on the back surface of the semiconductor package 210 by, for example, screen printing. The thermal grease 20 is, for example, a phase change thermal interface material. After the printing step S2 and before the drying step S3, the thermal grease 20 contains a solvent. In the drying step S3, the solvent contained in the thermal grease 20 is volatilized. In this manner, the semiconductor device 200 is pre-assembled.
[0047] In the inspection process S4, the thermal grease 20 arranged on the back surface of the semiconductor package 210 is inspected. More specifically, first, the thermal grease 20 belonging to the same lot as that used in the manufacture of the semiconductor device 200 is arranged on the holding plate 10 under the same conditions as the printing process S2 and the drying process S3. Second, the pressing plate 30 is arranged opposite the holding plate 10 so as to sandwich the thermal grease 20, and then the test method according to the first embodiment is performed. The pass / fail result in the inspection process S4 is determined by comparing with the test result when the thermal grease 20 is normally arranged on the holding plate 10. The inspection process S4 may be performed at least once while the thermal grease 20 of the same lot is being used.
[0048] According to the manufacturing method of the semiconductor device 200, semiconductor devices 200 using heat dissipating grease 20 belonging to the same lot can be collectively inspected for defects in the pumping-out performance of the heat dissipating grease 20 caused by insufficient evaporation of the solvent contained in the heat dissipating grease 20, insufficient amount of filler contained in the heat dissipating grease 20, abnormalities in the resin material contained in the heat dissipating grease 20, etc.
[0049] The embodiments disclosed herein are illustrative in all respects and should not be considered as limiting. The basic scope of the present disclosure is defined by the claims rather than the above embodiments, and it is intended to include all modifications within the scope and meaning equivalent to the claims. [Explanation of symbols]
[0050] 10 holding plate, 10a first main surface, 10b second main surface, 20 heat dissipation grease, 21 void, 30 holding plate, 30a third main surface, 30b fourth main surface, 40 spacer, 50 temperature regulator, 60 mounting jig, 61 rod, 62 imaging device, 70 drive unit, 71 load sensor, 100 test device, 200 semiconductor device, 210 semiconductor package, 211 base, 220 heat dissipation fin, P1, P2, P3, P4, P5, P6 positions, S1 preparation process, S2 printing process, S3 drying process, S4 inspection process.
Claims
1. A test method for pumping-out performance of thermal grease, comprising the steps of: placing the thermal grease on a retaining plate; a step of placing a pressing plate parallel to the holding plate and facing the holding plate so as to sandwich the heat dissipation grease therebetween; changing the distance between the holding plate and the pressure plate while the pressure plate is kept parallel to the holding plate; and observing a shape of the thermal grease after the distance is changed. The pumping out performance is determined based on the shape.
2. The method of claim 1 , wherein the pumping out performance is determined based on the shape after the spacing is changed to an increasing value.
3. 2. The method of claim 1, wherein the pumping-out performance is determined based on the shape after the spacing is changed from large to small.
4. The pressing plate is formed of a material that transmits visible light, The testing method according to any one of claims 1 to 3, wherein the shape is observed through the pressing plate.
5. A test method for pumping-out performance of thermal grease, comprising the steps of: placing the thermal grease on a retaining plate; a step of placing a pressing plate parallel to the holding plate and facing the holding plate so as to sandwich the heat dissipation grease therebetween; changing the distance between the holding plate and the pressure plate while the pressure plate is kept parallel to the holding plate; and measuring a load applied to the pressing plate. The pumping out performance is determined based on the load.
6. 6. The method of claim 5, wherein the pumping out performance is determined based on the change in the load as the spacing is changed.
7. 6. The test method of claim 5, wherein the pumping out performance is determined based on a change in the load while varying the spacing and then maintaining the spacing.
8. The test method according to any one of claims 5 to 7, wherein the pumping-out performance is determined based on a change in the load when the distance is changed and maintained in a first direction and when the distance is changed and maintained in a second direction opposite to the first direction.
9. A method for manufacturing a semiconductor device, comprising: providing a semiconductor package; placing a thermal grease on the semiconductor package; and testing the pumping-out performance of the thermal grease. The inspection is carried out by the test method according to any one of claims 1 to 8, the heat dissipation grease is placed on the holding plate under the same conditions as the heat dissipation grease is placed on the semiconductor package; The method for manufacturing a semiconductor device, wherein the heat dissipation grease placed on the semiconductor package and the heat dissipation grease placed on the holding plate belong to the same lot.
10. 10. The method for manufacturing a semiconductor device according to claim 9, wherein the heat dissipation grease is made of a phase change thermal interface material.
Citation Information
Patent Citations
Heat-conducting silicone grease and preparation method thereof
CN112194899A
Viscosity measuring device
JP1984188544A
Heat radiation member, its manufacturing method, and its lay-out method
JP2004039829A
Device and method for testing pumping out of heat transfer grease
JP2010203991A
Viscosity characteristic evaluation method and viscosity characteristic evaluation device