Polyimide film and its manufacturing method
A polyimide film with enhanced heat and mechanical properties is achieved by combining specific dianhydride and diamine components, addressing the limitations of conventional films in advanced circuit boards, with improved tensile strength, chemical resistance, and thermal stability.
Patent Information
- Application Number
- JP2023106870
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-06-29
- Filing Date
- 2023-06-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-06-29
AI Technical Summary
Conventional polyimide films exhibit relatively low heat resistance, which compromises mechanical strength and thermal properties, making them unsuitable for advanced circuit boards requiring high heat resistance and chemical stability.
A polyimide film is produced using a specific combination of dianhydride and diamine components, including biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, benzophenone tetracarboxylic dianhydride, oxydianiline, paraphenylenediamine, 4,4'-diaminobenzanilide, and 2,2-bis[4-(4-aminophenoxy)phenyl]propane, with precise molar ratios, followed by polymerization and imidization processes to enhance mechanical strength, chemical resistance, and thermal stability.
The resulting polyimide film demonstrates excellent mechanical properties, high heat resistance, and chemical resistance, with tensile strength of 350 MPa or more, chemical resistance of 80% or more, and a glass transition temperature of 350°C or higher, suitable for flexible metal foil laminates and electronic components.
Smart Images

Figure 0007592123000001 
Figure 0007592123000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide film having excellent mechanical properties, heat resistance and chemical resistance, and a method for producing the same. [Background technology]
[0002] Polyimide (PI) is a polymeric material based on imide rings, which have excellent chemical stability along with a rigid aromatic main chain, and has the highest levels of chemical resistance, electrical insulation, chemical resistance, and weather resistance among organic materials.
[0003] In particular, due to its excellent electrical properties such as excellent insulating properties, i.e., low dielectric constant, it has been attracting attention as a highly functional polymer material in the electrical, electronic and optical fields.
[0004] 2. Description of the Related Art Recently, with the trend towards lighter and smaller electronic products, flexible thin circuit boards with high integration density have been actively developed.
[0005] Such thin circuit boards tend to have a structure in which a circuit containing metal foil is formed on a polyimide film that has excellent heat resistance, low temperature resistance and insulating properties, but is also easily flexible.
[0006] Flexible metal clad laminates are mainly used for such thin circuit boards, and an example is Flexible Copper Clad Laminate (FCCL), which uses a thin copper plate as a metal foil. Polyimide is also used as a protective film and insulating film for thin circuit boards.
[0007] In particular, as electronic devices have recently been equipped with a variety of functions, there has been a demand for high calculation and communication speeds in the electronic devices. To meet this demand, thin circuit boards capable of high-speed communication at high frequencies have been developed.
[0008] However, conventional polyimide films have the disadvantage of being relatively low in heat resistance, making them unsuitable for use in the latest circuit boards. Although various prior research efforts have been conducted to improve heat resistance, improvements in heat resistance have been accompanied by a decrease in thermal properties such as mechanical strength and glass transition temperature.
[0009] Therefore, there is still a need to develop polyimide films that have improved heat resistance while maintaining the inherent thermal properties of polyimide, such as mechanical strength and glass transition temperature.
[0010] In particular, the heat resistance of the polyimide film is an important factor to be considered in the lamination process during the production of FCCL.
[0011] In addition, during the FPCB manufacturing process, a chemical is used to remove smears that occur on the inner walls of the holes due to heat during laser and bit processing. Since strong oxides (such as K2MnO4) are used, the chemical resistance of the polyimide film is becoming increasingly important. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Korean Patent No. 10-1004429 Summary of the Invention [Problem to be solved by the invention]
[0013] An object of the present invention is to provide a polyimide film having both excellent heat resistance and mechanical properties, and a method for producing the same.
[0014] In particular, the present invention aims to provide a polyimide film having high high-temperature stability, excellent tensile strength and chemical resistance, and a method for producing the same.
[0015] Therefore, a substantial object of the present invention is to provide specific examples thereof. [Means for solving the problem]
[0016] In order to achieve the above object, one embodiment of the present invention relates to a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA) and benzophenonetetracarboxylic dianhydride (BTDA); and a diamine component including oxydianiline (ODA), paraphenylenediamine (PPD), 4,4'-diaminobenzanilide (DABA), and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), and is produced by imidizing a polyamic acid solution including the diamine component. A polyimide film is provided.
[0017] Another embodiment of the present invention is a process for producing a polyamic acid by polymerizing a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA) and benzophenonetetracarboxylic dianhydride (BTDA) and a diamine component including oxydianiline (ODA), paraphenylenediamine (PPD), 4,4'-diaminobenzanilide (DABA) and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) in an organic solvent; (b) imidizing the polyamic acid; A method for producing a polyimide film is provided.
[0018] Yet another embodiment of the present invention provides a multilayer film comprising the polyimide film.
[0019] Yet another embodiment of the present invention provides an electronic component comprising the multilayer film. Effect of the Invention
[0020] The polyimide film according to the embodiment of the present invention can simultaneously have excellent mechanical properties, high heat resistance, and chemical resistance by using a specific dianhydride acid component and a specific diamine component in combination in a specific molar ratio.
[0021] Meanwhile, the present invention can be effectively applied to electronic parts such as flexible metal foil laminates by including the polyimide film as described above. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, the embodiments of the present invention will be described in more detail, in the order of "polyimide film" and "method for producing polyimide film" according to the present invention.
[0023] Prior to this, the terms and words used in this specification and claims should not be interpreted limited to their ordinary or dictionary meanings, but should be interpreted with a meaning and concept that corresponds to the technical idea of the present invention, in accordance with the principle that an inventor can appropriately define the concept of a term in order to explain his / her invention in the best possible way.
[0024] Therefore, it should be understood that the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention and does not fully represent the technical ideas of the present invention, and that there may be various equivalents and modifications that can replace them at the time of this application.
[0025] In this specification, the singular expression includes the plural expression unless the context clearly indicates otherwise. It should be understood that in this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0026] Whenever an amount, concentration, or other value or parameter is given herein as a range, a preferred range or a list of an upper preferred value and a lower preferred value, it should be understood to specifically disclose all ranges formed by any pair of any upper range limit or preferred value, and any lower range limit or preferred value, regardless of whether a range is otherwise disclosed.
[0027] Where a range of numerical values is recited herein, unless otherwise stated, the range is intended to include the endpoints thereof, and all integers and fractions within the range. It is not intended that the scope of the invention be limited to the specific values recited when defining a range.
[0028] As used herein, "dianhydride acid" is intended to include precursors or derivatives thereof which may not technically be dianhydrides but which nevertheless must react with a diamine to form a polyamic acid which is then converted back to a polyimide.
[0029] As used herein, "diamine" is intended to include precursors or derivatives thereof, which may not technically be diamines, but which nevertheless must react with a dianhydride to form a polyamic acid, which is then converted back to a polyimide.
[0030] The polyimide film according to the present invention is produced by imidizing a polyamic acid solution containing a dianhydride component including 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), and 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), and a diamine component including 4,4'-oxydianiline (ODA), p-phenylenediamine (PPD), 4,4'-diaminobenzanilide (DABA), and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP).
[0031] The dianhydride acid component of the polyimide film consists only of biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, and benzophenonetetracarboxylic dianhydride, and the diamine component consists only of oxydianiline, paraphenylenediamine, 4,4'-diaminobenzanilide, and 2,2-bis[4-(4-aminophenoxy)phenyl]propane.
[0032] In one embodiment, based on a total content of the dianhydride acid components of 100 mol%, the content of the biphenyltetracarboxylic dianhydride may be 5 mol% or more and 25 mol% or less, the content of the pyromellitic dianhydride may be 45 mol% or more and 65 mol% or less, and the content of the benzophenonetetracarboxylic dianhydride may be 20 mol% or more and 40 mol% or less.
[0033] For example, based on 100 mol% of the total content of the dianhydride acid components, the content of the biphenyltetracarboxylic dianhydride may be 10 mol% or more and 20 mol% or less, the content of the pyromellitic dianhydride may be 50 mol% or more and 60 mol% or less, and the content of the benzophenonetetracarboxylic dianhydride may be 25 mol% or more and 35 mol% or less.
[0034] The polyimide chains derived from biphenyltetracarboxylic dianhydride have a structure called a charge transfer complex (CTC), i.e., a regular linear structure in which the electron donor and electron acceptor are located close to each other, enhancing intermolecular interactions.
[0035] In addition, benzophenone tetracarboxylic dianhydride, which has a carbonyl group, also contributes to the expression of CTCs, just like biphenyl tetracarboxylic dianhydride.
[0036] In particular, the dianhydride component may further include pyromellitic dianhydride, which is a dianhydride component having a relatively rigid structure and is preferred in that it can impart appropriate elasticity to the polyimide film.
[0037] In addition, biphenyltetracarboxylic dianhydride and benzophenonetetracarboxylic dianhydride contain two benzene rings corresponding to the aromatic moiety, whereas pyromelitic dianhydride contains one benzene ring corresponding to the aromatic moiety.
[0038] An increase in the content of pyromellitic dianhydride in the dianhydride acid component can be understood as an increase in the imide groups in the molecule when the same molecular weight is used as a standard, and this can be understood as a relative increase in the ratio of imide groups derived from the pyromellitic dianhydride in the polyimide polymer chain compared to the imide groups derived from biphenyltetracarboxylic dianhydride and benzophenonetetracarboxylic dianhydride.
[0039] If the content ratio of the pyromellitic dianhydride is reduced too much, the components having a relatively rigid structure are reduced, and the mechanical properties of the polyimide film may be reduced below a desired level.
[0040] For this reason, when the content of the biphenyltetracarboxylic dianhydride and the benzophenonetetracarboxylic dianhydride exceeds the above range, the mechanical properties of the polyimide film are deteriorated.
[0041] In one embodiment, based on 100 mol% of the total content of the diamine components, the content of the oxydianiline may be 1 mol% or more and 30 mol% or less, the content of the paraphenylenediamine may be 56 mol% or more and 75 mol% or less, the content of the 4,4'-diaminobenzanilide may be 1 mol% or more and 15 mol% or less, and the content of the 2,2-bis[4-(4-aminophenoxy)phenyl]propane may be 2 mol% or more and 39 mol% or less.
[0042] For example, based on 100 mol% of the total content of the diamine components, the content of the oxydianiline may be 2 mol% or more and 27 mol% or less, the content of the paraphenylenediamine may be 60 mol% or more and 70 mol% or less, the content of the 4,4'-diaminobenzanilide may be 1 mol% or more and 10 mol% or less, and the content of the 2,2-bis[4-(4-aminophenoxy)phenyl]propane may be 2 mol% or more and 35 mol% or less.
[0043] In particular, the content of the 2,2-bis[4-(4-aminophenoxy)phenyl]propane may be 5 mol % or more and 30 mol % or less, based on 100 mol % of the total content of the diamine components.
[0044] If the content of 2,2-bis[4-(4-aminophenoxy)phenyl]propane in the diamine component exceeds the range of the present application, the mechanical strength of the polyimide film may decrease, and the glass transition temperature may decrease, resulting in reduced thermal stability.
[0045] In addition, the 4,4'-diaminobenzanilide contains an amide group and can contribute to improving the excellent heat resistance and mechanical properties of the polyimide film of the present invention within the content range of the present invention.
[0046] In addition, if the content of oxydianiline and paraphenylenediamine is outside the range of the present invention, the mechanical strength and chemical resistance of the polyimide film may be reduced, or the glass transition temperature may be lowered, resulting in reduced thermal stability.
[0047] In one embodiment, the polyimide film may include a block copolymer consisting of two or more blocks.
[0048] By adjusting the blocks of the block copolymer, the glass transition temperature of the polyimide film can be increased, ensuring the high temperature stability of the polyimide film, and improving the mechanical strength and chemical resistance of the polyimide film.
[0049] In one embodiment, the polyimide film of the present application may have a tensile strength of 350 MPa or more, a chemical resistance of 80% or more, and a glass transition temperature of 350° C. or more.
[0050] In the present invention, the polyamic acid can be produced, for example, by (1) A method in which the entire amount of the diamine component is placed in a solvent, and then the dianhydride component is added in an amount substantially equimolar to the diamine component to polymerize it; (2) A method in which the entire amount of the dianhydride component is placed in a solvent, and then a diamine component is added in an amount substantially equimolar to the dianhydride component to polymerize the mixture; (3) A method in which a part of the diamine component is placed in a solvent, a part of the dianhydride component is mixed with the reaction components in a ratio of about 95 to 105 mol %, the remaining diamine component is added, and the remaining dianhydride component is added continuously thereto, so that the diamine component and the dianhydride component are substantially equimolar, thereby polymerizing the mixture; (4) A method in which a dianhydride component is placed in a solvent, a part of the components in the diamine compound is mixed in a ratio of 95 to 105 mol % relative to the reactive components, and then another dianhydride component is added, followed by the remaining diamine component, so that the diamine component and the dianhydride component are substantially equimolar, thereby polymerizing the mixture; (5) A method of forming a first composition by reacting some diamine components and some dianhydride acid components in a solvent so that one of them is in excess, and forming a second composition by reacting some diamine components and some dianhydride acid components in another solvent so that one of them is in excess, and then mixing the first and second compositions to complete polymerization, in which if the diamine component is in excess when the first composition is formed, the dianhydride acid component is in excess in the second composition, and if the dianhydride acid component is in excess in the first composition, the diamine component is in excess in the second composition, and the first and second compositions are mixed to polymerize so that the total diamine components and dianhydride acid components used in these reactions are substantially equimolar.
[0051] However, the polymerization method is not limited to the above example, and any known method can be used to produce polyamic acid.
[0052] In one embodiment, a method for producing a polyimide film according to the present invention includes the steps of: The method may include the steps of: (a) polymerizing a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), and benzophenonetetracarboxylic dianhydride (BTDA) and a diamine component including oxydianiline (ODA), paraphenylenediamine (PPD), 4,4'-diaminobenzanilide (DABA), and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) in an organic solvent to produce a polyamic acid; and (b) imidizing the polyamic acid.
[0053] In one embodiment, based on a total content of the dianhydride acid components of 100 mol%, the content of the biphenyl tetracarboxylic dianhydride may be 5 mol% or more and 25 mol% or less, the content of the pyromellitic dianhydride may be 45 mol% or more and 65 mol% or less, the content of the benzophenone tetracarboxylic dianhydride may be 20 mol% or more and 40 mol% or less, based on a total content of the diamine components of 100 mol%, the content of the oxydianiline may be 1 mol% or more and 30 mol% or less, the content of the paraphenylenediamine may be 56 mol% or more and 75 mol% or less, the content of the 4,4'-diaminobenzanilide may be 1 mol% or more and 15 mol% or less, and the content of the 2,2-bis[4-(4-aminophenoxy)phenyl]propane may be 2 mol% or more and 39 mol% or less.
[0054] The polyimide film may have a tensile strength of 350 MPa or more, a chemical resistance of 80% or more, and a glass transition temperature of 350° C. or more.
[0055] In the present invention, the polymerization method of the polyamic acid may be defined as a random polymerization method, and the polyimide film prepared from the polyamic acid of the present invention prepared by the above process can be preferably applied to the effects of the present invention, which are to improve mechanical properties, heat resistance, and chemical resistance.
[0056] On the other hand, the solvent for synthesizing the polyamic acid is not particularly limited, and any solvent that dissolves the polyamic acid can be used, but an amide-based solvent is preferable.
[0057] Specifically, the solvent may be an organic polar solvent, more specifically, an aprotic polar solvent, or may be, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methyl-pyrrolidone (NMP), p-chlorophenol, o-chlorophenol, N-methyl-pyrrolidone (NMP), gamma-butyrolactone (GBL), and diglyme, but is not limited thereto, and may be used alone or in combination of two or more kinds as necessary.
[0058] In one example, the solvent is preferably N,N-dimethylformamide or N,N-dimethylacetamide.
[0059] In addition, in the manufacturing process of the polyamic acid, fillers other than nanosilica can be added for the purpose of improving various properties of the film such as sliding properties, thermal conductivity, corona resistance, loop hardness, etc. The fillers to be added are not particularly limited, but preferred examples include titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.
[0060] The particle size of the filler is not particularly limited and may be determined depending on the film properties to be modified and the type of filler to be added. In general, the average particle size is 0.05 to 100 μm, preferably 0.1 to 75 μm, more preferably 0.1 to 50 μm, and particularly preferably 0.1 to 25 μm.
[0061] If the particle size is below this range, the modifying effect is unlikely to be achieved, whereas if it exceeds this range, the surface properties may be significantly damaged or the mechanical properties may be significantly reduced.
[0062] The amount of the filler to be added is not particularly limited, and may be determined depending on the film properties to be modified, the particle size of the filler, etc. In general, the amount of the filler to be added is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.02 to 80 parts by weight, relative to 100 parts by weight of polyimide.
[0063] If the amount of the filler added is less than this range, the modifying effect of the filler is unlikely to be exhibited, and if the amount exceeds this range, the mechanical properties of the film may be significantly damaged. The method of adding the filler is not particularly limited, and any known method may be used.
[0064] In the production method of the present invention, the polyimide film is produced by a thermal imidization method and a chemical imidization method.
[0065] Alternatively, the imidation layer may be produced by a hybrid imidation method in which a thermal imidization method and a chemical imidization method are performed in parallel.
[0066] The thermal imidization method is a method in which a chemical catalyst is excluded and the imidization reaction is induced by a heat source such as hot air or an infrared dryer.
[0067] The thermal imidization method can imidize the amic acid groups present in the gel film by heat-treating the gel film at a variable temperature in the range of 100 to 600°C, specifically, by heat-treating the gel film at 200 to 500°C, more specifically, by heat-treating the gel film at 300 to 500°C, to imidize the amic acid groups present in the gel film.
[0068] However, even during the process of forming the gel film, a portion of the amic acid (approximately 0.1 mol % to 10 mol %) is imidized, and therefore the polyamic acid composition can be dried at a variable temperature in the range of 50°C to 200°C, which also falls within the category of the thermal imidization method.
[0069] In the case of chemical imidization, a polyimide film can be produced using a dehydrating agent and an imidization agent according to a method known in the art. Here, the term "dehydrating agent" refers to a substance that promotes a ring-closing reaction by dehydrating polyamic acid, and non-limiting examples thereof include aliphatic acid anhydrides, aromatic acid anhydrides, N,N'-dialkylcarbodiimides, halogenated lower aliphatic acids, halogenated lower fatty acid anhydrides, arylphosphonic dihalides, and thionyl halides. Among these, aliphatic acid anhydrides are preferred from the viewpoint of availability and cost, and non-limiting examples thereof include acetic anhydride (or acetic anhydride, AA), propionic anhydride, and lactic anhydride, which can be used alone or in combination of two or more.
[0070] The term "imidizing agent" refers to a substance having an effect of promoting a ring-closing reaction with polyamic acid, and may be, for example, an imine-based component such as an aliphatic tertiary amine, an aromatic tertiary amine, or a heterocyclic tertiary amine. Among them, heterocyclic tertiary amines are preferred from the viewpoint of reactivity as a catalyst. Non-limiting examples of heterocyclic tertiary amines include quinoline, isoquinoline, β-picoline (BP), pyridine, etc., which can be used alone or in combination of two or more kinds.
[0071] The amount of the dehydrating agent added is preferably within a range of 0.5 to 5 mol, and more preferably within a range of 1.0 to 4 mol, per mol of amic acid groups in the polyamic acid, and the amount of the imidizing agent added is preferably within a range of 0.05 to 2 mol, and more preferably within a range of 0.2 to 1 mol, per mol of amic acid groups in the polyamic acid.
[0072] If the amount of the dehydrating agent and the imidizing agent is less than the above range, the chemical imidization is insufficient, cracks are formed in the polyimide film produced, and the mechanical strength of the film may be reduced.If the amount of the dehydrating agent and the imidizing agent is more than the above range, the imidization proceeds too quickly, which makes it difficult to cast the polyimide film into a film or the polyimide film produced may show brittle properties, which is undesirable.
[0073] As an example of the composite imidization method, a dehydrating agent and an imidization agent are added to a polyamic acid solution, which is then heated at 80 to 200°C, preferably 100 to 180°C, partially cured and dried, and then heated at 200 to 400°C for 5 to 400 seconds to produce a polyimide film.
[0074] The present invention provides a multilayer film comprising the above-mentioned polyimide film and a thermoplastic resin layer, and a multilayer film comprising the above-mentioned polyimide film and an electrically conductive metal foil (for example, a flexible metal foil laminate).
[0075] As the thermoplastic resin layer, for example, a thermoplastic polyimide resin layer can be used.
[0076] The metal foil to be used is not particularly limited, but for example, when the multilayer film of the present invention is used for electronic or electrical equipment applications, the metal foil may be one containing copper or a copper alloy, stainless steel or an alloy thereof, nickel or a nickel alloy (including alloy 42), or aluminum or an aluminum alloy.
[0077] In general flexible metal foil laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, and are also preferably usable in the present invention. In addition, the surface of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer.
[0078] In the present invention, there is no particular limitation on the thickness of the metal foil, so long as it can exhibit sufficient function depending on the application.
[0079] The multilayer film usable as the flexible metal foil laminate according to the present invention may have a structure in which a metal foil is laminated on one side of the polyimide film, or in which an adhesive layer containing a thermoplastic polyimide is added to one side of the polyimide film, and the metal foil is laminated in a state of adhering to the adhesive layer.
[0080] The present invention further provides an electronic device comprising the multilayer film (eg, a flexible metal foil laminate) as an electrical signal transmission circuit.
[0081] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these examples are merely presented as examples of the present invention and do not define the scope of the invention.
[0082] <Production Example> DMF was added to a 500 ml reactor equipped with a stirrer and nitrogen inlet / outlet tubes while injecting nitrogen, and the temperature of the reactor was set to 30°C. Then, oxydianiline (ODA), paraphenylenediamine (PPD), 4,4'-diaminobenzanilide (DABA), and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) as diamine components, and biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), and benzophenonetetracarboxylic dianhydride (BTDA) as dianhydride components were added, and it was confirmed that they were completely dissolved.
[0083] Thereafter, the temperature of the reactor was raised to 40° C. under a nitrogen atmosphere, and stirring was continued for 120 minutes to produce polyamic acid.
[0084] A catalyst and a dehydrating agent were added to the polyamic acid produced in this manner, and the mixture was rotated at a high speed of 1,500 rpm or more to remove air bubbles, and then coated onto a glass substrate using a spin coater.
[0085] Thereafter, the gel film was prepared by drying at 120°C for 30 minutes under a nitrogen atmosphere, and the temperature was increased to 450°C at a rate of 2°C / min, and heat-treated at 450°C for 60 minutes. The gel film was then cooled again at a rate of 2°C / min to 30°C to obtain a final polyimide film, which was peeled off from the glass substrate by dipping in distilled water.
[0086] The thickness of the polyimide film was 15 μm. The thickness of the polyimide film was measured using an Anritsu Electric Film Thickness Tester.
[0087] <Examples 1 to 4 and Comparative Examples 1 to 3> The contents of the diamine monomer and the dianhydride monomer were adjusted as shown in Table 1 by the same method as described above.
[0088] [Table 1]
[0089] <Experimental Example> Evaluation of tensile strength, glass transition temperature and chemical resistance As shown in Table 1, the polyimide films produced in Examples 1 to 4 and Comparative Examples 1 to 3 were measured for tensile strength, elastic modulus, glass transition temperature, and chemical resistance, and the results are shown in Table 2.
[0090] (1) Tensile strength and elastic modulus Tensile strength and elastic modulus were measured using an Instron 3365SER instrument according to ASTM D882 measurement method.
[0091] (2) Measurement of glass transition temperature Glass transition temperature (T g ) measured the loss modulus and storage modulus of each film using DMA, and measured the inflection point on the tangent graph as the glass transition temperature.
[0092] (3) Chemical resistance measurement The manufactured polyimide film is corona-treated on both sides, and then the polyimide film + bonding sheet (adhesive) + copper foil structure is bonded using a hot press at a pressure of 50 kgf and a temperature of 160°C for 30 minutes to create an FCCL sample.
[0093] FCCL cut into a size of 4 x 10 cm was exposed to a 10% NaOH solution at 55°C for 3 minutes, and then exposed to a desmear solution (10% NaMnO4 + 4% NaOH) at 55°C for 5 minutes, followed by washing. This process was repeated twice, and the thickness of the film was measured and compared with the thickness before exposure to the NaOH solution and the desmear solution, and the degree of change in thickness after exposure relative to the thickness before exposure was expressed as a percentage.
[0094] For example, in the case of the polyimide film of Example 1, the thickness of the polyimide film after exposure to the desmear solution was equivalent to 86% of the thickness of the polyimide film before the exposure.
[0095] [Table 2]
[0096] As can be seen from Table 2, the polyimide films prepared according to the examples of the present invention had a tensile strength of 350 MPa or more, a chemical resistance of 80% or more, and a glass transition temperature (Tg) of 350° C. or more, and thus had excellent mechanical properties, chemical resistance, and thermal stability.
[0097] Such results are achieved by the components and composition ratios specified in this application, and it is understood that the content of each component plays a decisive role.
[0098] In contrast, the polyimide films of Comparative Examples 1 to 3 were inferior to the polyimide films of Examples 1 to 4 in at least one of the tensile strength, chemical resistance, and heat resistance.
[0099] This suggests that the polyimide films of the comparative examples would be difficult to apply to actual electronic components.
[0100] The present invention has been described above with reference to an embodiment thereof. However, a person having ordinary knowledge in the field to which the present invention pertains will be able to make various applications and modifications within the scope of the present invention based on the above content.
Claims
1. dianhydride acid components including biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA) and benzophenonetetracarboxylic dianhydride (BTDA); and a diamine component including oxydianiline (ODA), paraphenylenediamine (PPD), 4,4'-diaminobenzanilide (DABA), and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), and the polyamic acid solution including the diamine component is imidized. Based on 100 mol% of the total content of the dianhydride acid components, the content of the biphenyl tetracarboxylic dianhydride is 5 mol% or more and 25 mol% or less, the content of the pyromellitic dianhydride is 45 mol% or more and 65 mol% or less, and the content of the benzophenone tetracarboxylic dianhydride is 20 mol% or more and 40 mol% or less, and based on 100 mol% of the total content of the diamine components, the content of the oxydianiline is 1 mol% or more and 30 mol% or less, the content of the paraphenylenediamine is 56 mol% or more and 75 mol% or less, the content of the 4,4'-diaminobenzanilide is 1 mol% or more and 15 mol% or less, and the content of the 2,2-bis[4-(4-aminophenoxy)phenyl]propane is 2 mol% or more and 39 mol% or less; Polyimide film.
2. Including block copolymers consisting of two or more blocks, The polyimide film according to claim 1 .
3. The tensile strength is 350 MPa or more, Chemical resistance is 80% or more, The glass transition temperature is 350° C. or higher, The chemical resistance was evaluated by subjecting both sides of a polyimide film to a corona treatment, and then bonding a laminated structure of the polyimide film, a bonding sheet, and a copper foil by applying a pressure of 50 kgf at a temperature of 160° C. for 30 minutes using thermocompression bonding to prepare a sample, and then exposing the sample to a 10% NaOH solution at 55° C. for 3 minutes, exposing the sample to a desmear solution, which is a mixed solution of 10% NaMnO 4 and 4% NaOH, at 55° C. for 5 minutes, and then washing the sample. The thickness of the polyimide film was measured, and the thickness before exposure to the NaOH solution and the desmear solution was compared to the thickness before exposure, and the degree of change in thickness after exposure was expressed as a percentage. The polyimide film according to claim 1 .
4. (a) preparing a polyamic acid by polymerizing a dianhydride component including biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA) and benzophenonetetracarboxylic dianhydride (BTDA) and a diamine component including oxydianiline (ODA), paraphenylenediamine (PPD), 4,4′-diaminobenzanilide (DABA) and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) in an organic solvent; (b) imidizing the polyamic acid; Based on 100 mol% of the total content of the dianhydride acid components, the content of the biphenyl tetracarboxylic dianhydride is 5 mol% or more and 25 mol% or less, the content of the pyromellitic dianhydride is 45 mol% or more and 65 mol% or less, and the content of the benzophenone tetracarboxylic dianhydride is 20 mol% or more and 40 mol% or less, and based on 100 mol% of the total content of the diamine components, the content of the oxydianiline is 1 mol% or more and 30 mol% or less, the content of the paraphenylenediamine is 56 mol% or more and 75 mol% or less, the content of the 4,4'-diaminobenzanilide is 1 mol% or more and 15 mol% or less, and the content of the 2,2-bis[4-(4-aminophenoxy)phenyl]propane is 2 mol% or more and 39 mol% or less; A method for producing a polyimide film.
5. The polyimide film has a tensile strength of 350 MPa or more; Chemical resistance is 80% or more, The glass transition temperature is 350° C. or higher, The chemical resistance was evaluated by subjecting both sides of a polyimide film to a corona treatment, and then bonding a laminated structure of the polyimide film, a bonding sheet, and a copper foil by applying a pressure of 50 kgf at a temperature of 160° C. for 30 minutes using thermocompression bonding to prepare a sample, and then exposing the sample to a 10% NaOH solution at 55° C. for 3 minutes, exposing the sample to a desmear solution, which is a mixed solution of 10% NaMnO 4 and 4% NaOH, at 55° C. for 5 minutes, and then washing the sample. The thickness of the polyimide film was measured, and the thickness before exposure to the NaOH solution and the desmear solution was compared to the thickness before exposure, and the degree of change in thickness after exposure was expressed as a percentage. The method for producing a polyimide film according to claim 4 .
6. The polyimide film according to any one of claims 1 to 3, Multilayer film.
7. A thermoplastic resin layer is included. The multilayer film of claim 6.
8. [0023] Including an electrically conductive metal foil; The multilayer film of claim 6.
9. The multilayer film according to claim 8, Electronic components.
Citation Information
Patent Citations
Metal laminate and its manufacturing method
JP2007512988A
Polyimide film, multilayered polyimide film, coverlay and flexible printed wiring board
JP2017145325A
Polyamic acid composition for manufacturing display substrates and method for manufacturing display substrates using the same
JP2022515452A
Method of preparing wholly aromatic polyimide resin having enhanced thermal stability and tensile properties in high temperature
KR101004429B1
Polyimide film
WO2006109832A1