Laminated Structure
A mist CVD process using a lithium tantalate substrate and specific metal layers addresses thermal instability and cost issues in β-Ga2O3 semiconductor devices, resulting in low-cost semiconductor devices with enhanced electrical properties.
Patent Information
- Application Number
- JP2023126947
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-08-03
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2039-09-03
AI Technical Summary
Existing methods for manufacturing β-Ga2O3 semiconductor devices face challenges such as thermal instability, high production costs, and insufficient electrical characteristics like withstand voltage, with unclear processes for forming high-quality β-Ga2O3 semiconductor layers at lower temperatures.
A method involving a mist CVD process using a lithium tantalate substrate to grow crystalline β-Ga2O3 semiconductor layers, followed by forming conductive layers with specific metals from Groups 4, 10, and 11 of the periodic table, enabling a laminated structure that is thermally stable and cost-effective.
The method allows for the production of low-cost semiconductor devices with superior electrical properties, including high breakdown voltage and stable characteristics even under high-temperature processes.
Smart Images

Figure 0007592131000001 
Figure 0007592131000002 
Figure 0007592131000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a laminated structure, a method for manufacturing a semiconductor device, and a laminated structure. [Background technology]
[0002] Oxide semiconductors, such as gallium oxide (Ga2O3), are semiconductors with a large band gap and are expected to be used in next-generation switching elements that can achieve high voltage resistance, low loss, and high heat resistance. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-072463 A [Patent Document 2] JP 2014-015366 A [Patent Document 3] JP 2015-091740 A [Patent Document 4] JP 2005-260101 A [Patent Document 5] JP 2009-081468 A Summary of the Invention [Problem to be solved by the invention]
[0004] Patent Document 1 describes a method for producing gallium oxide (α-Ga2O3) having a corundum structure at a relatively low temperature. However, since α-Ga2O3 is in a metastable phase, there is a problem that it is thermally unstable.
[0005] In contrast, β-Ga2O3 having a beta-gallium structure is the most stable phase, and the above-mentioned phase transition does not occur. However, as described in Patent Documents 2 and 3, it is necessary to heat the material to an extremely high temperature in order to form the film, and it is preferable to form the film at a lower temperature. In addition, Patent Documents 4 and 5 disclose semiconductor devices having electrodes with β-Ga2O3 as a semiconductor layer, but it is unclear how to fabricate the semiconductor layer β-Ga2O3. There was no technical knowledge known for fabricating a semiconductor device containing high-quality β-Ga2O3 at low cost. In addition, the electrical characteristics such as the breakdown voltage characteristics of the semiconductor devices described in Patent Documents 4 and 5 were not sufficient.
[0006] The present invention has been made to solve the above problems, and an object of the present invention is to fabricate a semiconductor device containing high quality β-Ga2O3 at low cost, and to provide a low-cost semiconductor device having good electrical characteristics such as breakdown voltage characteristics. [Means for solving the problem]
[0007] The present invention has been made to achieve the above-mentioned object, and provides a method for manufacturing a laminated structure including a semiconductor layer having a first main surface and a second main surface, a first conductive layer on the first main surface side, and a second conductive layer on the second main surface side, the method comprising the steps of: growing a semiconductor layer on a substrate by a mist CVD method to obtain a laminated body including the substrate and the semiconductor layer; removing the substrate from the laminated body; forming a first conductive layer on the first main surface side of the semiconductor layer; and forming a second conductive layer on the second main surface side of the semiconductor layer, wherein a substrate containing lithium tantalate as a main component is used as the substrate, and a layer containing crystalline β-Ga2O3 as a main component is grown as the semiconductor layer.
[0008] According to such a method for manufacturing a laminated structure, a semiconductor device containing high quality β-Ga2O3 can be fabricated at low cost.
[0009] In this case, the method for manufacturing a laminated structure can be such that the first conductive layer is a first metal layer containing a metal of Group 4 or Group 11 of the periodic table, and the second conductive layer is a second metal layer containing a metal of Group 4 or Group 11 of the periodic table.
[0010] This makes it possible to provide a low-cost semiconductor device having good electrical characteristics such as voltage resistance.
[0011] In this case, the method for producing the laminated structure may be such that the first metal layer contains Ti and / or Au.
[0012] This makes it possible to provide a low-cost semiconductor device having better electrical characteristics such as breakdown voltage characteristics.
[0013] In this case, the method for manufacturing the laminate structure can be such that the first metal layer further contains a metal of Group 10 of the periodic table, and the method for manufacturing the laminate structure can be such that the metal of Group 10 of the periodic table is Pt.
[0014] This makes it possible to provide a low-cost semiconductor device having better electrical characteristics such as voltage resistance.
[0015] In this case, the method for producing the laminated structure may be such that the second metal layer contains Ti and / or Au.
[0016] This makes it possible to provide a low-cost semiconductor device having better electrical characteristics such as breakdown voltage characteristics.
[0017] In this case, the method for producing the laminated structure may be such that the second conductive layer is an ohmic electrode containing a conductive metal oxide or a metal of Group 4 or Group 11 of the periodic table.
[0018] This makes it possible to provide a low-cost semiconductor device having better electrical characteristics such as breakdown voltage characteristics.
[0019] In this case, the method for producing the laminated structure may be such that the first conductive layer is an electrode containing a metal of Group 4 or Group 11 of the periodic table.
[0020] This makes it possible to provide a low-cost semiconductor device having better electrical characteristics such as breakdown voltage characteristics.
[0021] In this case, the method for manufacturing the laminated structure may be such that the first conductive layer is an electrode containing a metal or a conductive metal oxide, and the second conductive layer is an ohmic electrode containing a conductive metal oxide.
[0022] This makes it possible to provide a low-cost semiconductor device having better electrical characteristics such as breakdown voltage characteristics.
[0023] In this case, the method for manufacturing a semiconductor device may include the method for manufacturing the stacked structure described above, and in particular, the method for manufacturing a semiconductor device in which the semiconductor device is a diode, a Schottky barrier diode, or a power device.
[0024] The present invention also provides a laminated structure including a semiconductor layer having a first principal surface and a second principal surface, a first conductive layer on the first principal surface side, and a second conductive layer on the second principal surface side, in which the semiconductor layer is a crystal layer containing crystalline β-Ga2O3 as a main component, the first conductive layer is a first metal layer containing a metal of Group 4 or Group 11 of the periodic table, and the second conductive layer is a second metal layer containing a metal of Group 4 or Group 11 of the periodic table.
[0025] The present invention also provides a laminated structure including a semiconductor layer having a first principal surface and a second principal surface, a first conductive layer on the first principal surface side, and a second conductive layer on the second principal surface side, in which the semiconductor layer is a crystal layer containing crystalline β-Ga2O3 as a main component, and the second conductive layer is an ohmic electrode containing a conductive metal oxide or a metal of Group 4 or 11 of the periodic table.
[0026] The present invention also provides a laminated structure including a semiconductor layer having a first main surface and a second main surface, a first conductive layer on the first main surface side, and a second conductive layer on the second main surface side, in which the semiconductor layer is a crystal layer containing crystalline β-Ga2O3 as a main component, the first conductive layer is an electrode containing a conductive metal oxide or a metal, and the second conductive layer is an ohmic electrode containing a conductive metal oxide.
[0027] These laminated structures provide low-cost semiconductor devices with good electrical characteristics such as voltage resistance. Effect of the Invention
[0028] As described above, according to the method for manufacturing a laminated structure of the present invention, it is possible to provide a low-cost semiconductor device having good electrical characteristics such as voltage resistance. In particular, since both β-Ga2O3 and lithium tantalate substrates are thermally stable, it is possible to manufacture a stable semiconductor device with small fluctuations in characteristics even when subjected to high-temperature processes.
[0029] Moreover, the laminated structure of the present invention provides a low-cost semiconductor device with good electrical characteristics such as voltage resistance. In particular, β-Ga2O3 is thermally stable, so that even if it is subjected to a high-temperature process, the characteristics are stable with little fluctuation. Such a laminated structure has excellent electrical conductivity and is therefore useful for semiconductor devices and the like. [Brief description of the drawings]
[0030] [Figure 1] 1 is a schematic diagram showing an example of a laminated structure according to the present invention. [Diagram 2] 1 is a schematic diagram showing an example of a film forming apparatus used in a film forming method according to the present invention; [Diagram 3] FIG. 2 is a diagram illustrating an example of a mist generating unit in a film forming apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The present invention will be described in detail below, but the present invention is not limited thereto.
[0032] As described above, there has been a demand for fabricating a high-quality semiconductor device containing β-Ga2O3 at low cost, and for providing a low-cost semiconductor device having good electrical characteristics such as breakdown voltage characteristics.
[0033] As a result of intensive investigations into the above-mentioned problems, the inventors have found that a method for manufacturing a laminated structure including a semiconductor layer having a first main surface and a second main surface, a first conductive layer on the first main surface side, and a second conductive layer on the second main surface side, the method comprising the steps of growing a semiconductor layer on a substrate by a mist CVD method to obtain a laminated body including the substrate and the semiconductor layer, removing the substrate from the laminated body, forming a first conductive layer on the first main surface side of the semiconductor layer, and forming a second conductive layer on the second main surface side of the semiconductor layer, wherein a substrate containing lithium tantalate as a main component is used, and a layer containing crystalline β-Ga2O3 as a main component is grown as the semiconductor layer, makes it possible to manufacture at low cost a thermally stable, high-voltage laminated structure applicable to semiconductor devices, and have completed the present invention.
[0034] The present inventors also provide a laminated structure including a semiconductor layer having a first main surface and a second main surface, a first conductive layer on the first main surface side, and a second conductive layer on the second main surface side, wherein the semiconductor layer is a crystal layer containing crystalline β-Ga2O3 as a main component, the first conductive layer is a first metal layer containing a metal of Group 4 or Group 11 of the periodic table, and the second conductive layer is a second metal layer containing a metal of Group 4 or Group 11 of the periodic table. The inventors have found that this results in a thermally stable, high-voltage-resistant, low-cost laminated structure applicable to semiconductor devices, and have completed the present invention.
[0035] The present inventors have also discovered that a laminate structure including a semiconductor layer having a first principal surface and a second principal surface, a first conductive layer on the first principal surface side, and a second conductive layer on the second principal surface side, wherein the semiconductor layer is a crystal layer containing crystalline β-Ga2O3 as a main component, and the second conductive layer is an ohmic electrode containing a conductive metal oxide, and a metal of Group 4 or 11 of the periodic table, can provide a thermally stable, high-voltage-resistant laminate structure at low cost that can be applied to semiconductor devices, and have completed the present invention.
[0036] The present inventors have also discovered that a laminated structure including a semiconductor layer having a first main surface and a second main surface, a first conductive layer on the first main surface side, and a second conductive layer on the second main surface side, wherein the semiconductor layer is a crystal layer containing crystalline β-Ga2O3 as a main component, the first conductive layer is an electrode containing a conductive metal oxide or metal, and the second conductive layer is an ohmic electrode containing a conductive metal oxide, can provide a thermally stable, high-voltage resistant laminated structure at low cost that can be applied to semiconductor devices, and have completed the present invention.
[0037] The following description will be given with reference to the drawings.
[0038] (Laminated structure) 1, one embodiment of a laminated structure 10 according to the present invention is a laminated structure 10 including a first conductive layer 3 on a first principal surface 2 side and a second conductive layer 5 on a second principal surface 4 side on a semiconductor layer 1 which is a crystal layer containing crystalline β-Ga2O3 as a main component. Note that the semiconductor layer 1 is not limited to a single layer, and may be a semiconductor layer consisting of multiple layers.
[0039] The term "crystalline" as used herein means that the crystalline state includes polycrystalline and single crystalline. Amorphous matter may be mixed in with the polycrystalline or single crystalline state.
[0040] (Crystalline substrate mainly composed of lithium tantalate) First, a substrate containing lithium tantalate as a main component, which is used in the method for producing a laminated structure according to the present invention, will be described.
[0041] In the method for producing a laminated structure according to the present invention, first, a substrate containing lithium tantalate as a main component is prepared. Here, the "substrate containing lithium tantalate as a main component" refers to a substrate containing 50 to 100% lithium tantalate, and includes not only single crystal lithium tantalate but also polycrystalline lithium tantalate.
[0042] Lithium tantalate has an ilmenite structure, and its lattice constant is relatively close to that of α-Ga2O3. The relationship of the distance between oxygen atoms on the α-Ga2O3(001) and β-Ga2O3(-201) planes, as well as on the lithium tantalate(001) plane, is generally α-Ga2O3<lithium tantalate<β-Ga2O3. Since β-Ga2O3 is energetically more stable than α-Ga2O3, it is presumed that α-Ga2O3 does not form on the lithium tantalate substrate even at low temperatures, and β-Ga2O3 forms preferentially.
[0043] It is most preferable to use a lithium tantalate single crystal substrate as a substrate mainly composed of lithium tantalate. This is because the film quality of the semiconductor layer formed on the substrate will be of the highest quality. Furthermore, the lithium tantalate single crystal substrate is of the same cost as a sapphire substrate, and is a material that enables the formation of a high-quality semiconductor layer at low cost.
[0044] The following description will be given taking a lithium tantalate single crystal substrate as an example. The lithium tantalate single crystal substrate can be obtained, for example, by growing a lithium tantalate single crystal by the Czochralski method to form a lithium tantalate single crystal ingot, and then slicing the ingot to form a substrate shape.
[0045] The lithium tantalate single crystal substrate that can be used in the present invention is preferably cut so that the lattice constant of its surface approaches the lattice constant of the crystalline oxide film to be deposited later. For example, when a semiconductor layer containing β-Ga2O3 as a main component (hereinafter sometimes referred to as a "crystalline oxide film") is deposited, it is preferable that the substrate is cut so that the crystal orientation is within Z±10°, and more preferably, the crystal orientation is within Z±5°.
[0046] Furthermore, it is preferable that the lithium tantalate single crystal substrate is subjected to a uniform polarization state, since this promotes uniform growth of the oxide single crystal film. That is, it is preferable that the lithium tantalate substrate is subjected to a single polarization treatment or a multi-polarization treatment.
[0047] To obtain a single-poled substrate, for example, a lithium tantalate single crystal ingot produced by the Czochralski method may be heated to 700°C, and subjected to a poling treatment for 10 hours by applying a voltage of 200V in the crystal orientation Z direction, and then the ingot may be sliced and processed into a substrate shape. Alternatively, the substrate processed into the substrate shape may itself be heated to 700°C, and subjected to a poling treatment for 10 hours by applying a voltage of 200V in the crystal orientation Z direction.
[0048] When using a substrate that has been subjected to a single polarization treatment, it is preferable to further subject the substrate surface to a pyroelectric suppression treatment, since this can suppress the substrate from being charged when a crystalline oxide film is deposited on the heated substrate. The pyroelectric suppression treatment is, for example, performed by embedding a lithium tantalate single crystal substrate that has been subjected to a single polarization treatment in lithium carbonate powder and performing a heat treatment at a temperature of 350°C or higher and the Curie temperature (approximately 610°C) or lower in a reducing gas atmosphere. At this time, the volume resistivity in the thickness direction of the substrate is 1.0×10 11 Ω cm or more, 2.0×10 13 By processing the substrate so that the resistivity is Ω·cm or less and the ratio of the maximum to minimum volume resistivity within the substrate is 4.0 or less, the electrical resistance of the substrate can be effectively suppressed when a crystalline oxide film is deposited on the substrate.
[0049] On the other hand, to obtain a multi-polarized substrate, for example, a single crystal (ingot or substrate) that has been once polarized to a single polarization, or a single crystal (ingot or substrate) that has not been subjected to a single polarization treatment, is heated to 700°C or higher and annealed for several hours (preferably 1000°C or higher, preferably 5 hours or more, more preferably 10 hours or more) to relieve distortion, and in the case of an ingot, it is sliced and processed into a substrate shape. The use of a multi-polarized substrate is preferable because it can suppress the substrate from being charged when a crystalline oxide film is deposited on the heated substrate. In particular, charging can be effectively suppressed by setting the average domain size of the polarization on the substrate surface to 5 μm or less. It is more preferable that the charging effect of the lithium tantalate substrate is suppressed, so that a crystalline oxide film can be stably deposited. It is preferable that the composition of the lithium tantalate single crystal (at least on the substrate surface) is a congruent composition, because it is easy to reduce the average domain size of the polarization on the substrate surface. Here, in the case of lithium tantalate, the congruent composition means that the ratio of Li to Ta is Li:Ta=48.5-α:51.5+α, where α is in the range of -0.5≦α≦0.5.
[0050] If the surface of the substrate mainly made of lithium tantalate is polished smoothly to reduce unevenness, a flat laminated film of the crystalline oxide film can be obtained. It is preferable to make Ra 10 nm or less. It is more preferable to make Ra 5 nm or less.
[0051] In addition, ions selected from hydrogen, helium, argon, and other rare gases can be implanted in advance into the surface of a substrate mainly composed of lithium tantalate on which a crystalline oxide film is to be deposited, forming a brittle layer 50 nm to 3 μm directly below the deposition surface. In this way, after the crystalline oxide film is deposited, the deposited crystalline oxide film can be easily peeled off from the lithium tantalate single crystal substrate by impacting the brittle layer.
[0052] The thickness of the substrate is not particularly limited, but is preferably 10 to 2000 μm, and more preferably 50 to 800 μm. 2The aperture (diameter) is preferably 2 inches (50 mm) or more, and more preferably 2 inches (50 mm) or more.
[0053] (Semiconductor layer) The semiconductor layer 1 in the laminated structure 10 according to the present invention is a semiconductor layer containing crystalline β-Ga2O3 as a main component, and is a crystalline oxide film having a beta gallium structure. A crystalline oxide film is usually composed of metal and oxygen, but in the semiconductor layer 1 of the laminated structure according to the present invention, it is sufficient that it contains β-Ga2O3 as a main component. β-Ga2O3 is a crystalline oxide film that is more thermally stable. Here, in the present invention, when it is said that "containing β-Ga2O3 as a main component", it means that β-Ga2O3 occupies 50 to 100% of the film. As a metal component other than gallium, for example, one or more metals selected from iron, indium, aluminum, vanadium, titanium, chromium, rhodium, iridium, nickel and cobalt may be included. Note that the semiconductor layer 1 may be either single crystal or polycrystalline as long as it contains β-Ga2O3 as a main component, but is most preferably single crystal.
[0054] As described above, the semiconductor layer 1 may be a single layer or multiple layers. In the case of multiple layers, the multiple layers may be formed on a substrate and then the substrate may be removed, as described below, or the substrate may be removed and then another semiconductor layer may be formed, resulting in the semiconductor layer 1 being made of multiple semiconductor layers with different properties.
[0055] The semiconductor layer 1 may contain a dopant. For example, n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium, or niobium, or p-type dopants such as copper, silver, tin, iridium, or rhodium, may be included. The dopant is not particularly limited, but is preferably tin. The concentration of the dopant is, for example, about 1×10 16 / cm 3 ~1×10 22 / cm 3 may be about 1 x 10 17 / cm 3 Even at low concentrations below 1×10 20 / cm 3A concentration higher than this may be used.
[0056] In the laminated structure according to the present invention, the thickness of the semiconductor layer 1 is not particularly limited, but can be 1.0 μm or more. For example, it may be 1.0 to 50 μm, preferably 5.0 to 30 μm, and more preferably 10 to 20 μm.
[0057] When growing the semiconductor layer 1, another layer may be interposed between the substrate and the semiconductor layer 1. The other layer is a layer having a different composition from the substrate and the outermost semiconductor layer, and may be, for example, any of a crystalline oxide film, an insulating film, a metal film, etc.
[0058] The laminated structure 10 according to the present invention can be used in semiconductor devices by appropriately designing the structure. For example, it can form the semiconductor layers of Schottky barrier diodes (SBDs), metal semiconductor field effect transistors (MESFETs), high electron mobility transistors (HEMTs), metal oxide semiconductor field effect transistors (MOSFETs), static induction transistors (SITs), junction field effect transistors (JFETs), insulated gate bipolar transistors (IGBTs), light emitting diodes (LEDs), and the like. In particular, the laminated structure 10 according to the present invention can be suitably used in diodes, Schottky barrier diodes, or power devices.
[0059] (Film forming equipment) In one embodiment of the laminated structure and the method for manufacturing the laminated structure according to the present invention, an aqueous solution containing at least gallium is atomized or turned into droplets, the mist is transported to a substrate using a carrier gas, and the mist is then thermally reacted on the substrate to form a semiconductor layer (crystalline oxide film), the substrate being a substrate mainly composed of lithium tantalate, the semiconductor layer (crystalline oxide film) being a layer mainly composed of crystalline β-Ga2O3, and a conductive layer is formed on the semiconductor layer (crystalline oxide film) obtained by removing the substrate to obtain the laminated structure. A film forming apparatus capable of forming such a semiconductor layer (crystalline oxide film) will be described.
[0060] 2 shows an example of a film forming apparatus 101 that can be used in the method for forming a semiconductor layer (crystalline oxide film) according to the present invention. The film forming apparatus 101 has a mist generating section 120 that generates mist by turning a raw material solution into mist, a carrier gas supplying section 130 that supplies a carrier gas for transporting the mist, a film forming section 140 that heat-treats the mist to form a film on a substrate, and a transporting section 109 that connects the mist generating section 120 and the film forming section 140 and transports the mist by the carrier gas. The film forming apparatus 101 may also be provided with a control section (not shown) that controls the whole or part of the film forming apparatus 101, thereby controlling its operation.
[0061] In addition, the term "mist" as used herein refers to a general term for fine particles of liquid dispersed in a gas, and includes what is called fog, droplets, and the like.
[0062] (Raw material solution) The raw material solution (aqueous solution) 104a is not particularly limited as long as it contains at least gallium. That is, in addition to gallium, it may contain, for example, one or more metals selected from iron, indium, aluminum, vanadium, titanium, chromium, rhodium, iridium, nickel, and cobalt. The metals in the form of a complex or salt can be preferably dissolved or dispersed in water. Examples of the complex include acetylacetonate complexes, carbonyl complexes, ammine complexes, and hydride complexes. Examples of the salt include metal chlorides, metal bromides, and metal iodides. In addition, the above metals can be dissolved in hydrobromic acid, hydrochloric acid, hydroiodic acid, or the like to be used as an aqueous solution of salt. The solute concentration is preferably 0.01 to 1 mol / L.
[0063] The raw material solution 104a may contain a dopant element for controlling the conductivity of the semiconductor layer (crystalline oxide film). Examples of the dopant include n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium, or niobium, or p-type dopants such as copper, silver, tin, iridium, or rhodium. The dopant is not particularly limited, but is preferably tin. The dopant element is preferably ionized. Therefore, an acid may be mixed into the raw material solution 104a to promote dissolution of the dopant element. Examples of the acid include hydrogen halides such as hydrobromic acid, hydrochloric acid, and hydroiodic acid, halogen oxo acids such as hypochlorous acid, chlorous acid, hypobromous acid, bromous acid, hypoiodous acid, and iodic acid, carboxylic acids such as formic acid, and nitric acid. Heating or applying ultrasonic waves is also effective for promoting dissolution.
[0064] (Mist generating section) In the mist generating section 120, the raw solution 104a is adjusted and the raw solution 104a is turned into mist to generate mist. The mist generating means is not particularly limited as long as it can turn the raw solution 104a into mist, and any known mist generating means may be used, but it is preferable to use a mist generating means using ultrasonic vibrations, as this allows for more stable mist generation.
[0065] An example of such a mist generating unit 120 is shown in FIG. 3. For example, the mist generating unit 120 may include a mist generating source 104 in which the raw solution 104a is stored, a medium capable of transmitting ultrasonic vibration, for example, a container 105 in which water 105a is stored, and an ultrasonic vibrator 106 attached to the bottom surface of the container 105. In detail, the mist generating source 104, which is a container in which the raw solution 104a is stored, is stored in the container 105 in which the water 105a is stored, using a support (not shown). The bottom of the container 105 is provided with an ultrasonic vibrator 106, which is connected to an oscillator 116. When the oscillator 116 is operated, the ultrasonic vibrator 106 vibrates, and ultrasonic waves are propagated into the mist generating source 104 through the water 105a, turning the raw solution 104a into mist.
[0066] (Transportation section) The transport unit 109 connects the mist generating unit 120 and the film forming unit 140. The mist is transported by a carrier gas from the mist generating source 104 of the mist generating unit 120 to the film forming chamber 107 of the film forming unit 140 via the transport unit 109. The transport unit 109 can be, for example, a supply pipe 109a. For example, a quartz pipe or a resin tube can be used as the supply pipe 109a.
[0067] (Film forming part) In the film formation section 140, the mist is heated to cause a thermal reaction, and a film is formed on a part or the entire surface of the substrate 110. The film formation section 140 may include, for example, a film formation chamber 107 in which the substrate 110 is placed and a hot plate 108 for heating the substrate 110. The hot plate 108 may be provided outside the film formation chamber 107 as shown in FIG. 2, or may be provided inside the film formation chamber 107. In addition, the film formation chamber 107 may be provided with an exhaust gas exhaust port 112 at a position that does not affect the supply of the mist to the substrate 110.
[0068] In addition, the substrate 110 may be placed on the upper surface of the film formation chamber 107 in a face-down position, or may be placed on the bottom surface of the film formation chamber 107 in a face-up position.
[0069] The thermal reaction is not particularly limited as long as the mist reacts by heating. The reaction conditions can be appropriately set according to the raw material and the film to be formed. For example, the heating temperature can be in the range of 250 to 900°C, preferably in the range of 300°C to 800°C, and more preferably in the range of 350°C to 700°C.
[0070] The thermal reaction may be carried out under any of the following atmospheres: vacuum, non-oxygen atmosphere, reducing gas atmosphere, air atmosphere, and oxygen atmosphere, and may be appropriately set depending on the film to be formed. The reaction pressure may be under any of atmospheric pressure, pressurized pressure, and reduced pressure, but film formation under atmospheric pressure is preferred because the apparatus configuration can be simplified.
[0071] (Carrier gas supply unit) The carrier gas supply unit 130 has a carrier gas source 102a for supplying a carrier gas, and may be provided with a flow rate control valve 103a for adjusting the flow rate of the carrier gas (hereinafter referred to as "main carrier gas") sent out from the carrier gas source 102a. In addition, the carrier gas supply unit 130 may be provided with a dilution carrier gas source 102b for supplying a dilution carrier gas as required, and a flow rate control valve 103b for adjusting the flow rate of the dilution carrier gas sent out from the dilution carrier gas source 102b.
[0072] The type of carrier gas is not particularly limited and can be appropriately selected depending on the film to be formed. For example, oxygen, ozone, inert gas such as nitrogen or argon, or reducing gas such as hydrogen gas or forming gas can be used. The type of carrier gas may be one type or two or more types. For example, a dilution gas obtained by diluting the same gas as the first carrier gas with another gas (e.g., diluted 10 times) may be used as the second carrier gas, or air may be used.
[0073] In this specification, the flow rate Q of the carrier gas refers to the total flow rate of the carrier gas. In the above example, the total flow rate of the main carrier gas sent from the carrier gas source 102a and the dilution carrier gas sent from the dilution carrier gas source 102b is the flow rate Q of the carrier gas.
[0074] The flow rate Q of the carrier gas is appropriately determined depending on the size of the film formation chamber and the substrate, but is usually 1 to 60 L / min, and preferably 2 to 40 L / min.
[0075] (Film forming method) Next, an example of a method for forming a semiconductor layer (crystalline oxide film) according to the present invention will be described with reference to Fig. 2. First, raw material solution 104a is contained in mist source 104 of mist generating section 120, and substrate 110, a crystalline substrate mainly composed of lithium tantalate, is placed on hot plate 108 directly or through the wall of film forming chamber 107, and hot plate 108 is operated. Lithium tantalate used as the crystalline substrate has a large thermal expansion coefficient, so it is preferable to gradually increase the temperature from a low temperature.
[0076] Next, the flow rate control valves 103a and 103b are opened to supply carrier gas from the carrier gas sources 102a and 102b into the film formation chamber 107, and the atmosphere in the film formation chamber 107 is thoroughly replaced with the carrier gas. At the same time, the flow rates of the main carrier gas and the dilution carrier gas are respectively adjusted to control the carrier gas flow rate Q.
[0077] In the step of generating mist, ultrasonic vibrator 106 is vibrated, and the vibration is propagated to raw material solution 104a through water 105a, thereby turning raw material solution 104a into mist and generating mist. Next, in the step of transporting the mist by carrier gas, the mist is transported by carrier gas from mist generating section 120 through transport section 109 to film forming section 140, and introduced into film forming chamber 107. In the step of forming a film, the mist introduced into film forming chamber 107 is heat-treated by heat from hot plate 108 in film forming chamber 107, causing a thermal reaction, and forming a film on substrate 110.
[0078] In this case, multiple layers can be formed on the substrate, for example by varying the concentration and / or type of dopant to provide multiple layers with different electrical properties.
[0079] (Annealing treatment) After the semiconductor layer (crystalline oxide film) is formed, annealing can be performed. For example, the temperature can be set to 500° C. or higher as a condition for the annealing treatment. The upper limit is not particularly limited, and may be within a range in which the semiconductor layer (crystalline oxide film) and the substrate can withstand the heat treatment, and can be set to, for example, 1000° C. The time for the annealing treatment is not particularly limited, but can be set to, for example, 1 minute or more. In addition, in consideration of productivity, it is preferable to set it to 1 hour or less, and more preferably 30 minutes or less. The atmosphere for the annealing treatment is not particularly limited, but it is preferable to set it to an inert gas atmosphere such as nitrogen or rare gas. Such an annealing treatment can be expected to have the effect of lowering the resistivity of the film and stabilizing the electrical characteristics. In addition, the surface roughness (arithmetic mean roughness: Ra) of the crystalline oxide film can be set to 0.1 μm or less. The surface roughness represents the arithmetic mean roughness (Ra) calculated based on JIS B0601 using the surface shape measurement results for a 10 μm square area by an atomic force microscope (AFM).
[0080] (Removal of the substrate) In the method for producing a laminated structure according to the present invention, the substrate is removed from a laminate including a substrate and a semiconductor layer 1. The method for removing the substrate at this time is not particularly limited. For example, the substrate can be peeled off. The peeling means is not particularly limited and may be a known means. For example, a means for peeling by applying mechanical impact, a means for peeling by applying heat and using thermal stress, a means for peeling by applying vibration such as ultrasonic waves, a means for peeling by etching, and a laser lift-off are included. The substrate itself may be dissolved and removed, but peeling removal is preferable from the viewpoint of cost because the substrate can be reused. By removing the substrate, the semiconductor layer can be obtained as a free-standing film.
[0081] In addition, after removing the substrate, another semiconductor layer can be formed on the semiconductor layer 1. For example, the concentration and / or type of the dopant can be changed to form a plurality of layers with different electrical characteristics. This can be appropriately set according to the intended semiconductor device.
[0082] (conductive layer / electrode) As a result of intensive research, the inventors have found that a combination of specific materials results in a thermally stable, excellent electrical property, and inexpensive laminated structure. In the laminated structure 10 according to the present invention, one of the features is the combination of the semiconductor layer 1 containing β-Ga2O3 as a main component and the conductive layers 3, 5 formed on the semiconductor layer 1. Specifically, when the following combination is used, the laminated structure has excellent electrical properties such as high breakdown voltage and low on-resistance. The explanation will be given with reference to FIG. 1 again. In the following explanation, for example, when it says "the first conductive layer 3 formed on the first main surface 2 side of the semiconductor layer 1", it includes not only the case where the semiconductor layer 1 and the first conductive layer 3 are formed (laminated) in direct contact with each other, but also the case where they are formed (laminated) via another layer. When it says "the first metal layer containing a metal of Group 4 or Group 11 of the periodic table", it includes not only a single layer but also a laminate of multiple layers. It goes without saying that it may contain both metals of Group 4 and Group 11.
[0083] (Conductive layer / electrode morphology 1) The first conductive layer 3 formed on the first main surface 2 side of the semiconductor layer 1 is a first metal layer containing a metal of group 4 or group 11 of the periodic table, and the second conductive layer 5 formed on the second main surface 4 side of the semiconductor layer 1 is a second metal layer containing a metal of group 4 or group 11 of the periodic table. In this case, it is preferable that the first metal layer contains Ti and / or Au. It is also preferable that the first metal layer further contains a metal of group 10 of the periodic table. As the metal of group 10 of the periodic table, Ni, Pd, and Pt are preferable, and Pt is more preferable. It is also preferable that the second metal layer contains Ti and / or Au.
[0084] (Conductive layer / electrode morphology 2) The second conductive layer formed on the second main surface 4 side of the semiconductor layer 1 is an ohmic electrode containing a conductive metal oxide and a metal of Group 4 or Group 11 of the periodic table. In this case, it is preferable that the first conductive layer is an electrode containing a metal of Group 4 or Group 11 of the periodic table.
[0085] (Conductive layer / electrode morphology 3) The first conductive layer formed on the first main surface 2 side of the semiconductor layer 1 is an electrode containing a conductive metal oxide or a metal, and the second conductive layer formed on the second main surface 4 side of the semiconductor layer 1 is an ohmic electrode containing a conductive metal oxide.
[0086] (Examples of conductive layer / electrode materials) Regarding the above-mentioned electrode materials, the metals of Group 4 of the periodic table are preferably Ti, Zr, and Hf. The metals of Group 11 of the periodic table are preferably Cu, Ag, and Au. The conductive metal oxides are preferably conductive metal oxides such as tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), and indium zinc oxide (IZO).
[0087] The method of forming the conductive layer / electrode is not particularly limited, and a general method can be used. That is, any of deposition, sputtering, CVD, plating, and printing methods for bonding together with resin, etc. can be used. In addition, when the material of the conductive layer / electrode is not particularly limited, a material having known conductivity can be used. For example, metals such as Al, Ag, Ti, Pd, Au, Cu, Cr, Fe, W, Ta, Nb, Mn, Mo, Hf, Co, Zr, Sn, Pt, V, Ni, Ir, Zn, In, and Nd can be used, as well as metal oxide conductive films such as tin oxide, zinc oxide, indium oxide, indium tin oxide (ITO), and indium zinc oxide (IZO), and organic conductive compounds such as polyaniline, polythiophene, and polypyrrole, and alloys and mixtures of two or more of these can also be used. EXAMPLES
[0088] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.
[0089] Example 1 On a lithium tantalate single crystal substrate, - After forming a β-Ga2O3 film as a type semiconductor layer, the substrate was peeled off and - On the n-type semiconductor layer + A layer of n-type semiconductor is formed. -A Schottky electrode is placed on the surface of the n-type semiconductor layer. + An ohmic electrode was formed on the surface of the type semiconductor layer to manufacture a laminated structure. An IV measurement was performed to evaluate the electrical characteristics.
[0090] (n - (Deposition conditions of the semiconductor layer) Substrate: Shin-Etsu Chemical Co., Ltd. lithium tantalate single crystal substrate Diameter 4 inches (100 mm), thickness 600 μm, c-face Mirror finish Film formation method: Mist CVD method Raw material aqueous solution: Gallium bromide, 0.05 mol / L Hydrobromic acid, 10% Carrier gas: N2, 4L / min Dilution gas: N2, 20L / min Film forming temperature: 408℃ Film formation time: 120 minutes
[0091] (Removal of the substrate) Using the laser lift method.
[0092] (n + (Deposition conditions of the semiconductor layer) Film formation method: Mist CVD method Raw material aqueous solution: Gallium bromide, 0.05 mol / L Tin bromide, 4 x 10 -3 mol / L Ga:Sn=1:0.02 Hydrobromic acid 10% Carrier gas: N2, 4L / min Dilution gas: N2, 20L / min Film forming temperature: 408℃ Film formation time: 180 minutes
[0093] (Conditions for forming the first conductive layer / Schottky electrode) Formation method: Electron beam deposition method Electrode configuration: - The following order is applied to the surface of the semiconductor layer: Pt layer 10nm, Ti layer 4nm, Au layer 200nm
[0094] (Conditions for forming the second conductive layer / ohmic electrode) Formation method: Electron beam deposition method Electrode configuration: + The following order is applied to the surface of the semiconductor layer: Ti layer 40nm, Au layer 200nm
[0095] Specifically, first, a lithium tantalate single crystal substrate with a congruent composition (Li / (Li+Ta) value of 0.485) was prepared as the substrate. The lithium tantalate single crystal produced by the Czochralski method was cut on the Z axis and processed into a C-face substrate, which was then subjected to a multi-polarization treatment by heat treatment at 700°C for 10 hours, and the surface was polished to a surface roughness of Ra = 0.5 nm.
[0096] Next, a raw material aqueous solution was prepared. Gallium bromide was used as the gallium source, and the concentration of gallium bromide was 0.05×10 -1 The aqueous solution was prepared so that the atomic ratio of gallium bromide and tin chloride was 1:0.02 mol / L. A 10% volumetric ratio of 48% hydrobromic acid solution was added to the prepared aqueous solution to prepare the raw aqueous solution.
[0097] The raw material solution 104a obtained as described above was contained in the mist generating source 104. Next, a lithium tantalate single crystal substrate having a size of 4 inches (diameter 100 mm) and a thickness of 600 μm as the substrate 110 was placed on the hot plate 108 in the film formation chamber 107, and the hot plate 108 was operated to raise the temperature to 408° C.
[0098] Next, the flow rate control valves 103a and 103b were opened to supply nitrogen gas as a carrier gas from the carrier gas sources 102a and 102b into the deposition chamber 107, and the atmosphere in the deposition chamber 107 was sufficiently replaced with the carrier gas, while the flow rate of the main carrier gas was adjusted to 4.0 L / min and the flow rate of the dilution carrier gas was adjusted to 20.0 L / min, respectively. In other words, the carrier gas flow rate Q was set to 24.0 L / min.
[0099] Next, the ultrasonic vibrator 106 was vibrated at 2.4 MHz, and the vibration was propagated to the raw material solution 104a through the water 105a, thereby turning the raw material solution 104a into mist and generating mist. This mist was introduced into the film formation chamber 107 through the supply pipe 109a by the carrier gas. Then, the mist was thermally reacted in the film formation chamber 107 under atmospheric pressure and at 408°C, forming a Ga2O3 film on the lithium tantalate single crystal substrate.
[0100] Next, the substrate is removed by the laser lift method, - A free-standing film of the n-type semiconductor layer was obtained. - On top of the free-standing film of the n-type semiconductor layer, + A type semiconductor layer was formed. + In the formation of the semiconductor layer, gallium bromide was used as the gallium source in the raw solution, and the concentration of gallium bromide was 0.05×10 -1 The aqueous solution was adjusted so that the atomic ratio of gallium bromide and tin chloride was 1:0.02 mol / L. The raw aqueous solution was prepared by adding 10% by volume of 48% hydrobromic acid solution to the prepared aqueous solution. - The deposition of the semiconductor layer is similar to that of the semiconductor layer.
[0101] The phase of the formed Ga2O3 film was identified by performing 2θ / ω scanning from 10 degrees to 120 degrees using an XRD diffractometer. The measurement was performed using CuKα radiation. As a result, the formed gallium oxide film was - n-type semiconductor layer + Both the GaN-type and GaN-type semiconductor layers were made of gallium oxide (β-Ga2O3) with a beta-gallium oxide structure.
[0102] Thereafter, as described above, a Schottky electrode and an ohmic electrode were formed to obtain a laminated structure.
[0103] The electrical characteristics of the laminated structure were evaluated by measuring the I-V characteristics. The breakdown voltage was 874 V and the on-resistance (differential resistance) was 0.09 mΩ cm. 2 It was.
[0104] (Reference example) n - A laminate structure similar to that of Example 1 was fabricated, except that a Pt layer of only 200 nm was formed on the surface of the type semiconductor layer by electron beam deposition, and the I-V characteristics were measured. As a result, the breakdown voltage was 92 V, and the on-resistance (differential resistance) was 57 Ω cm 2 It was.
[0105] Example 2 n - A laminate structure similar to that of Example 1 was fabricated, except that a 15 nm Ti layer and a 200 nm Au layer were laminated in this order on the surface of the type semiconductor layer, and the I-V characteristics were measured. As a result, the breakdown voltage was 856 V and the on-resistance (differential resistance) was 0.13 mΩcm. 2 It was.
[0106] Example 3 n + A laminate structure similar to that in Example 1 was produced, except that an ITO film was formed on the surface of the type semiconductor layer, and the IV characteristics were measured. The conditions for forming the ITO film were as follows.
[0107] (ITO film formation conditions) Film formation method: Mist CVD method Raw material aqueous solution: Indium bromide, 0.025 mol / L Tin bromide, 2.5 x 10 -4 mol / L Hydrobromic acid, 10% Carrier gas: N2, 4L / min Dilution gas: N2, 20L / min Film forming temperature: 500℃ Film formation time: 30 minutes
[0108] As a result, the breakdown voltage was 864V and the on-resistance (differential resistance) was 0.16mΩcm 2 It was.
[0109] As described above, by using β-Ga2O3 as a semiconductor layer, it was possible to manufacture an inexpensive semiconductor device that has high pressure resistance and high heat resistance.
[0110] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0111] 1...semiconductor layer; 2...first main surface; 3...first conductive layer; 4...second main surface; 5... second conductive layer, 10... laminated structure, 101...film forming apparatus, 102a...carrier gas source, 102b...dilution carrier gas source; 103a...flow rate control valve; 103b...flow rate control valve, 104...mist source, 104a...raw material solution (aqueous solution), 105...container, 105a...water, 106...ultrasonic transducer, 107...film formation chamber, 108...hot plate; 109...transport unit; 109a...supply pipe; 110...substrate; 112...exhaust port; 116...oscillator; 120: mist generating section, 130: carrier gas supply section, 140: film forming section.
Claims
1. A laminated structure including a semiconductor layer having a first main surface and a second main surface, a first conductive layer on the first main surface side, and a second conductive layer on the second main surface side, The semiconductor layer is a crystalline β-Ga 2 O 3 A crystal layer containing as a main component the first conductive layer is a first metal layer containing a metal of Group 4 or Group 11 of the periodic table; the second conductive layer is a second metal layer containing a metal of Group 4 or Group 11 of the periodic table; The surface roughness (arithmetic mean roughness: Ra) of the semiconductor layer is 0.1 μm or less, The semiconductor layer has a thickness of 1.0 to 50 μm.
2. A laminated structure including a semiconductor layer having a first main surface and a second main surface, a first conductive layer on the first main surface side, and a second conductive layer on the second main surface side, The semiconductor layer is a crystalline β-Ga 2 O 3 A crystal layer containing as a main component the second conductive layer is an ohmic electrode containing a conductive metal oxide or a metal of Group 4 or Group 11 of the periodic table; The surface roughness (arithmetic mean roughness: Ra) of the semiconductor layer is 0.1 μm or less, The semiconductor layer has a thickness of 1.0 to 50 μm.
3. A laminated structure including a semiconductor layer having a first main surface and a second main surface, a first conductive layer on the first main surface side, and a second conductive layer on the second main surface side, The semiconductor layer is a crystalline β-Ga 2 O 3 A crystal layer containing as a main component the first conductive layer is an electrode comprising a conductive metal oxide or a metal; the second conductive layer is an ohmic electrode including a conductive metal oxide; The surface roughness (arithmetic mean roughness: Ra) of the semiconductor layer is 0.1 μm or less, The semiconductor layer has a thickness of 1.0 to 50 μm.
4. The semiconductor layer is a crystalline β-Ga 2 O 3 or crystalline β-Ga 2 O 3 The laminate structure according to any one of claims 1 to 3, characterized in that the laminate structure is a crystal layer containing as a main component one or more metals selected from iron, indium, vanadium, titanium, chromium, rhodium, iridium, nickel and cobalt as a metal component other than gallium.
Citation Information
Patent Citations
Ga2O3-BASED SEMICONDUCTOR ELEMENT
JP2005260101A
HIGHLY FUNCTIONAL Ga2O3 SINGLE CRYSTAL FILM AND METHOD FOR PRODUCING THE SAME
JP2008303119A
Ga2O3-BASED SEMICONDUCTOR ELEMENT AND MANUFACTURING METHOD OF Ga2O3-BASED SEMICONDUCTOR ELEMENT
JP2009081468A
SUBSTRATE WITH ??-Ga2O3 SINGLE CRYSTAL FILM AND ITS MANUFACTURING METHOD
JP2014015366A
Gallium oxide substrate and manufacturing method of the same
JP2014031300A