Silicon carbide semiconductor device
A transition region with controlled nitrogen concentration and thickness in the interface between silicon carbide and silicon dioxide layers addresses defects, improving the electrical performance of silicon carbide semiconductor devices by reducing defects and enhancing mobility.
Patent Information
- Application Number
- JP2020147099
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-09-01
AI Technical Summary
The interface between a silicon carbide layer and a silicon dioxide layer in silicon carbide semiconductor devices experiences defects, which degrade the electrical performance.
A transition region is introduced between the silicon carbide and silicon dioxide layers, containing carbon, oxygen, and nitrogen, with a maximum nitrogen concentration five times that of the silicon dioxide layer and a thickness of 3-5 nm, formed by heat-treating the interface with NO gas to reduce defects.
The transition region reduces defects, enhancing the field effect mobility and improving the electrical characteristics of the silicon carbide semiconductor device.
Smart Images

Figure 0007593011000001 
Figure 0007593011000002 
Figure 0007593011000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicon carbide semiconductor device. [Background technology]
[0002] A silicon carbide semiconductor device in which a silicon dioxide layer is formed on a silicon carbide layer is known (see, for example, Patent Document 1). [Patent Document 1] Patent No. 6648852 Summary of the Invention [Problem to be solved by the invention]
[0003] In a silicon carbide semiconductor device, it is preferable to reduce defects at the interface between a silicon carbide layer and a silicon dioxide layer. [Means for solving the problem]
[0004] In a first aspect of the present invention, there is provided a silicon carbide semiconductor device. The silicon carbide semiconductor device may have a silicon carbide layer. The silicon carbide semiconductor device may have a silicon dioxide layer. The silicon dioxide may be provided above the silicon carbide layer. The silicon dioxide may contain nitrogen. The silicon carbide semiconductor device may have a transition region. The transition region may be disposed between the silicon carbide layer and the silicon dioxide layer. The transition region may contain carbon, oxygen and nitrogen. A maximum nitrogen concentration in the transition region is 1.0×10 20 cm -3 It may be more than that.
[0005] The maximum nitrogen concentration of the transition region may be at least five times the maximum nitrogen concentration of the silicon dioxide layer.
[0006] The maximum nitrogen concentration of the silicon dioxide layer may be greater than the maximum nitrogen concentration of the silicon carbide layer.
[0007] The full width at half maximum of the nitrogen concentration of the transition region may be 1.0 nm or less.
[0008] The thickness of the transition region may be 3 nm or more. The thickness of the transition region may be 5 nm or less.
[0009] The silicon carbide layer may comprise a strained silicon carbide layer. The strained silicon carbide layer may be disposed below the transition region. The strained silicon carbide layer may be defined by LEED analysis. The silicon carbide layer may comprise a crystalline silicon carbide layer. The crystalline silicon carbide layer may be disposed below the strained silicon carbide layer.
[0010] The transition region may have a silicon dioxide altered layer. The silicon dioxide altered layer may be provided below the silicon dioxide layer. The transition region may have a mixed layer. The mixed layer may be provided below the silicon dioxide altered layer. The transition region may have a silicon carbide altered layer. The silicon carbide altered layer may be provided below the mixed layer. The maximum carbon concentration may be greatest in the order of the silicon carbide altered layer, the mixed layer, and the silicon dioxide altered layer. The maximum oxygen concentration may be greatest in the order of the silicon dioxide altered layer, the mixed layer, and the silicon carbide altered layer. The maximum nitrogen concentration may be greatest in the order of the mixed layer, the silicon dioxide altered layer, and the silicon carbide altered layer.
[0011] The silicon carbide altered layer may include a nitrided incomplete silicon carbide layer. The nitrided incomplete silicon carbide layer may be provided below the mixed layer. The silicon carbide altered layer may include an incomplete silicon carbide layer. The incomplete silicon carbide layer may be provided below the nitrided incomplete silicon carbide layer. The incomplete silicon carbide layer may not contain nitrogen. The silicon carbide altered layer may include an amorphous silicon carbide layer. The amorphous silicon carbide layer may be provided below the incomplete silicon carbide layer. The amorphous silicon carbide layer may not contain oxygen. The silicon dioxide altered layer may include a carbonized incomplete silicon dioxide layer. The carbonized incomplete silicon dioxide layer may be provided above the mixed layer. The silicon dioxide altered layer may include an incomplete silicon dioxide layer. The incomplete silicon dioxide layer may be disposed above the carbonized incomplete silicon dioxide layer. The incomplete silicon dioxide layer may be free of carbon.
[0012] The silicon carbide layer may be provided with a trench within which a silicon dioxide layer may be formed.
[0013] The above summary of the invention does not list all of the necessary features of the present invention. Also, subcombinations of these features may also be inventions. [Brief description of the drawings]
[0014] [Figure 1] 1 is a diagram showing an example of a configuration of a silicon carbide semiconductor device 100 according to an embodiment of the present invention. [Diagram 2] 1 shows the configuration of silicon carbide semiconductor device 100 in region A. [Diagram 3] 1A to 1C are diagrams illustrating an example of a method for forming a sample 200. [Figure 4] 1 is an example of a concentration profile resulting from SIMS analysis of the vicinity of the transition region 18 of the sample 200. [Diagram 5] 3 is a diagram showing an example of the results of a LEED analysis of a silicon carbide layer 20. FIG. [Figure 6] FIG. 2 shows an example of the results of a LEED analysis of a silicon carbide layer 20 that has been heat-treated with NO gas. [Figure 7] FIG. 4 is a diagram showing an example of the results of a LEED analysis of a silicon carbide layer 20 after a silicon dioxide layer 42 is formed. [Figure 8] 4 is a diagram showing an example of the results of an XPS analysis of a silicon carbide layer 20 for oxygen. FIG. [Figure 9] 4 is a diagram showing an example of the results of an XPS analysis of a silicon carbide layer 20 for nitrogen. FIG. [Figure 10] 4 is a diagram showing an example of the results of an XPS analysis of silicon carbide layer 20 for silicon. FIG. [Figure 11] FIG. 2 is a diagram showing the vicinity of the transition region 18 captured by a transmission electron microscope. [Figure 12] FIG. 13 is a diagram showing the results of EELS analysis of the transition region 18. [Figure 13] FIG. 2 is a diagram showing the layer structure of the transition region 18 in detail. [Figure 14] 11A to 11C are diagrams illustrating another example of a method for forming the sample 200. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described below through embodiments of the invention, but the following embodiments do not limit the scope of the invention according to the claims. Furthermore, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.
[0016] Fig. 1 is a diagram showing an example of a configuration of a silicon carbide semiconductor device 100 according to an embodiment of the present invention. The silicon carbide semiconductor device 100 in Fig. 1 is a vertical MOSFET (Metal Oxide Semiconductor Field Effect Transistor). The upper and lower surfaces of the silicon carbide semiconductor device 100 may be parallel to the XY plane. Fig. 1 is a cross section of a part of the silicon carbide semiconductor device 100 cut along the XZ plane. In this example, the X-axis direction and the Y-axis direction are perpendicular to each other, and the Z-axis direction is perpendicular to the XY plane.
[0017] In this example, the positive direction in the Z-axis direction may be referred to as "up" and the negative direction in the Z-axis direction may be referred to as "down". However, "up" and "down" do not necessarily mean the vertical direction with respect to the ground. In other words, the directions of "up" and "down" are not limited to the direction of gravity. "Up" and "down" are merely convenient expressions for specifying the relative positional relationship in a substrate, layer, region, film, etc.
[0018] The structure shown in FIG. 1 may be two vertical MOSFET unit structures arranged side by side. The unit structures may extend in the Y-axis direction and be repeatedly arranged in the X-axis direction. The unit structures may be arranged to form a substantially rectangular shape in the XY plan view. A region in which the unit structures are arranged may be referred to as an active region. An edge termination structure having a function of preventing electric field concentration in the active region may be provided around the active region. The edge termination structure may include one or more of a guard ring structure, a field plate structure, and a JTE (Junction Termination Extension) structure.
[0019] The silicon carbide semiconductor device 100 of this example has a silicon carbide substrate 10. The silicon carbide substrate 10 may be a so-called m-plane silicon carbide substrate. The m-axis direction of the silicon carbide substrate 10 may be parallel to the Z-axis direction. The silicon carbide substrate 10 may be a so-called Si-plane silicon carbide substrate. The Si-axis direction of the silicon carbide substrate 10 may be parallel to the Z-axis direction. The silicon carbide substrate 10 may be a so-called C-plane silicon carbide substrate. The C-axis direction of the silicon carbide substrate 10 may be parallel to the Z-axis direction. The silicon carbide substrate 10 may be a so-called a-plane silicon carbide substrate. The a-axis direction of the silicon carbide substrate 10 may be parallel to the Z-axis direction. The silicon carbide substrate 10 may be a so-called a-plane silicon carbide substrate. The a-axis direction of the silicon carbide substrate 10 may be parallel to the Z-axis direction. The silicon carbide substrate 10 has a threading dislocation density of 1×10 7 cm -2 The silicon carbide substrate 10 of this example is an n+ type substrate.
[0020] In this example, the substrate and each layer are described using either p-type or n-type conductivity, but in other examples, the substrate and each layer may have the opposite conductivity type. Note that n-type or p-type means that electrons or holes are the majority carriers, respectively. Regarding the + or - written after n or p, + means a higher carrier concentration than those without it, and - means a lower carrier concentration than those without it.
[0021] The silicon carbide layer 12 is an n-type silicon carbide layer having a lower impurity concentration than the silicon carbide substrate 10. The silicon carbide layer 12 is a low-concentration n-type drift layer. The silicon carbide layer 12 is provided on the upper surface of the silicon carbide substrate 10. The silicon carbide layer 12 may be formed by epitaxial growth. A high-concentration region 14 is formed on the opposite side of the silicon carbide layer 12 to the silicon carbide substrate 10. The high-concentration region 14 is an n-type silicon carbide layer having a lower impurity concentration than the silicon carbide substrate 10 and a higher impurity concentration than the silicon carbide layer 12. The high-concentration region 14 in this example is a high-concentration n-type drift layer. The high-concentration region 14 may be formed by epitaxial growth. A base layer 16 is formed on the opposite side of the high-concentration region 14 to the silicon carbide layer 12. The base layer 16 in this example is p-type. The base layer 16 may be formed by epitaxial growth.
[0022] 1, a drain electrode 54 is provided on the lower surface of the silicon carbide substrate 10. Below the drain electrode 54, a drain electrode pad 56 is provided.
[0023] A trench structure is formed on the upper surface side of the silicon carbide semiconductor device 100. Specifically, the trench 38 penetrates the base layer 16 from the upper surface (upper surface side of the silicon carbide semiconductor device 100) of the base layer 16 opposite to the silicon carbide substrate 10 side to reach the high concentration region 14. The trench 38 is formed in the base layer 16 and the high concentration region 14 (i.e., the silicon carbide layer). Along the inner wall of the trench 38, a transition region 18 is formed on the bottom and side wall of the trench 38, and a silicon dioxide layer 42 is formed inside the transition region 18 in the trench 38. That is, the transition region 18 is provided between the silicon carbide layer and the silicon dioxide layer 42. The silicon dioxide layer 42 may be formed by high temperature oxidation (HTO). The transition region 18 will be described in detail later. Furthermore, a gate electrode 44 is formed inside the silicon dioxide layer 42 in the trench 38. The gate electrode 44 is formed of, for example, polysilicon. The silicon dioxide layer 42 insulates the gate electrode 44 from the high concentration region 14 and the base layer 16. A part of the gate electrode 44 may protrude from above the trench 38 toward the source electrode pad 52. In addition, an interlayer insulating film 48 may be formed on the gate electrode 44. The interlayer insulating film 48 insulates the gate electrode 44 from the source electrode pad 52.
[0024] A source region 22 and a contact region 25 are selectively provided on the front surface side of the silicon carbide semiconductor device 100. The source region 22 and the contact region 25 may be in contact with a source electrode 50. The source region 22 may be in contact with a trench 38. In this example, the source region 22 is an n+ type, and the contact region 25 is a p+ type. The source region 22 and the contact region 25 may be formed by doping.
[0025] In the high concentration region 14 of this example, a first base region 26 and a second base region 28 are selectively provided. The lower end of the first base region 26 is located closer to the drain electrode 54 than the bottom of the trench 38. The lower end of the second base region 28 is located closer to the drain electrode 54 than the bottom of the trench 38. The second base region 28 is formed at a position facing the bottom of the trench 38 in the depth direction (Z-axis direction). The width of the second base region 28 in the X-axis direction may be wider than the width of the trench 38 in the X-axis direction. The bottom of the trench 38 may reach the second base region 28, or may be located in the high concentration region 14 sandwiched between the base layer 16 and the second base region 28 and not contact the second base region 28. In this example, the bottom of the trench 38 reaches the second base region 28. In this example, the first base region 26 and the second base region 28 are p+ type. The first base region 26 and the second base region 28 are doped with aluminum elements, for example.
[0026] A charge inversion region (i.e., a channel) is formed in the base layer 16 by supplying a predetermined positive potential to the gate electrode 44. When a predetermined potential difference is formed between the source electrode 50 (source electrode pad 52) and the drain electrode 54 (drain electrode pad 56), an electron current flows from the source electrode 50 to the drain electrode 54 through the channel.
[0027] 2 shows the configuration of silicon carbide semiconductor device 100 in region A. Region A shows silicon dioxide layer 42, base layer 16 and high concentration region 14 in the vicinity of trench 38.
[0028] A transition region 18 is provided between the silicon dioxide layer 42 and the silicon carbide layer (the base layer 16 and the high concentration region 14). The transition region 18 contains oxygen and carbon. The transition region 18 also contains nitrogen because it is heat-treated in an NO gas atmosphere described below. In this example, since the transition region 18 contains nitrogen, defects in the transition region 18 (the interface between the silicon carbide layer and the silicon dioxide layer 42) can be reduced. Therefore, the field effect mobility of the silicon carbide semiconductor device 100 can be increased, and the electrical characteristics can be improved. In this case, in order to analyze the transition region 18, a sample was created by the same formation method as that for the transition region 18 of the silicon carbide semiconductor device 100.
[0029] FIG. 3 is a diagram showing an example of a method for forming a sample 200. The sample 200 includes a silicon carbide substrate 10, a silicon carbide layer 20, a silicon dioxide layer 42, and a transition region 18. The silicon carbide layer 20 is the same as either the base layer 16 or the high concentration region 14. First, a silicon carbide layer forming step S101 is performed to form a silicon carbide layer 20 on the silicon carbide substrate 10 (S101). The silicon carbide layer 20 in this example has a thickness of 3 μm or more and 7 μm or less (for example, 5 μm). The silicon carbide layer forming step S101 may be performed by epitaxial growth. Note that it is preferable to clean the silicon carbide substrate 10 by RCA cleaning or the like before performing the silicon carbide layer forming step S101.
[0030] Next, a silicon dioxide layer forming step S102 is performed to form a silicon dioxide layer 42 on the silicon carbide layer 20 (S102). The thickness of the silicon dioxide layer 42 in this example is 30 nm or more (for example, 60 nm). The silicon dioxide layer forming step S102 may be performed by high temperature oxidation (HTO). The high temperature oxidation is performed by adding dichlorosilane and N 2 The high-temperature oxidation may be performed by introducing O. The processing temperature of the high-temperature oxidation is, for example, 800° C. The silicon dioxide layer forming step S102 may be performed by other known methods.
[0031] After the silicon dioxide layer 42 is formed, a heat treatment step S103 is carried out (S103). 2The heat treatment process may be performed in a gas atmosphere of 90% NO gas and 10% NO gas. The treatment temperature of the heat treatment process may be 1300°C or higher and 1500°C or lower. The treatment temperature of the heat treatment process S103 may be 1350°C or higher. The treatment temperature of the heat treatment process S103 in this example is 1300°C. The treatment time of the heat treatment process S103 in this example is 15 minutes or higher and 45 minutes or lower (e.g., 30 minutes). By increasing the treatment temperature and the treatment time, the transition region 18 can be efficiently formed. The heat treatment process S103 forms the transition region 18. Furthermore, the heat treatment process S103 causes nitrogen from the NO gas to accumulate in the transition region 18. The accumulation of nitrogen in the transition region 18 reduces defects in the transition region 18. Since nitrogen is introduced from the silicon dioxide layer 42, the silicon dioxide layer 42 contains nitrogen.
[0032] Fig. 4 is an example of a concentration profile resulting from a SIMS analysis of the vicinity of the transition region 18 of the sample 200. (a) of Fig. 4 shows the concentration profile in the vicinity of the transition region 18. The vicinity of the transition region 18 refers to a part of the silicon dioxide layer 42, the transition region 18, and a part of the silicon carbide layer 20. (a) of Fig. 4 shows the impurity concentrations of carbon, nitrogen, oxygen, and silicon. The horizontal axis of (a) of Fig. 4 is depth (depth in the Z-axis direction in Fig. 4).
[0033] Fig. 4(b) shows the layer structure in the vicinity of the transition region 18 of the sample 200. In Fig. 4(b), the lengths in the depth direction of regions not shown in Fig. 4(a) are partially omitted.
[0034] 4(a), the oxygen concentration is a substantially constant impurity concentration d1 in the silicon dioxide layer 42. The oxygen concentration starts to decrease monotonically when it reaches the transition region 18 from the silicon dioxide layer 42, and becomes a constant impurity concentration in the silicon carbide layer 20. The carbon concentration is a substantially constant impurity concentration d2 in the silicon carbide layer 20. The carbon concentration starts to decrease monotonically when it reaches the transition region 18 from the silicon carbide layer 20, and becomes a constant impurity concentration in the silicon dioxide layer 42.
[0035] The transition region 18 may be a region from a position where the oxygen concentration in the silicon dioxide layer 42 starts to decrease from the silicon dioxide layer 42 toward the silicon carbide layer 20 to a position where the carbon concentration of the silicon carbide layer 20 starts to decrease from the silicon carbide layer 20 toward the silicon dioxide layer 42. The position where the oxygen concentration in the silicon dioxide layer 42 starts to decrease may be a position where the oxygen concentration is 95% of the maximum oxygen concentration in the silicon dioxide layer 42, or may be a position where the oxygen concentration is 90% or less. In (a) of FIG. 4, the XY plane at that position is defined as the first plane 91. The maximum oxygen concentration in the silicon dioxide layer 42 may be an impurity concentration d1.
[0036] Similarly, the position where the carbon concentration of silicon carbide layer 20 starts to decrease may be a position where the carbon concentration becomes 95% or less of the maximum carbon concentration in silicon carbide layer 20, or may be a position where the carbon concentration becomes 90% or less. In (a) of FIG. 4, the XY plane at that position is defined as second plane 92. The maximum carbon concentration in silicon carbide layer 20 may be impurity concentration d2. Furthermore, the silicon concentration starts to decrease monotonically when it reaches transition region 18, and becomes a constant impurity concentration in silicon dioxide layer 42.
[0037] As described above, transition region 18 is disposed between silicon carbide layer 20 and silicon dioxide layer 42. Transition region 18 also contains carbon, oxygen, and nitrogen. Transition region 18 can be formed by depositing silicon dioxide layer 42 on silicon carbide layer 20 and performing heat treatment.
[0038] The nitrogen concentration in the transition region 18 has a peak. This is because nitrogen from the NO gas is accumulated in the transition region 18 by the heat treatment step S103. In this example, the maximum value of the nitrogen concentration in the transition region 18 is 1.0×10 20 cm -3 The maximum nitrogen concentration in the transition region 18 is 1.0×10 20 cm -3 As a result of the above, defects in the transition region 18 can be further reduced.
[0039] Furthermore, the maximum value of the nitrogen concentration in the transition region 18 may be greater than the maximum value of the nitrogen concentration in the silicon dioxide layer 42. In this example, the maximum value of the nitrogen concentration in the transition region 18 is five times or more greater than the maximum value of the nitrogen concentration in the silicon dioxide layer 42. The second surface 92 is where the nitrogen concentration in the silicon dioxide layer 42 shows its maximum value. There are more dangling bonds in the transition region 18 than in the silicon dioxide layer 42. Therefore, many dangling bonds in the transition region 18 are bonded to nitrogen, and as a result, the maximum value of the nitrogen concentration in the transition region 18 is greater than the maximum value of the nitrogen concentration in the silicon dioxide layer 42.
[0040] The maximum value of the nitrogen concentration in the silicon dioxide layer 42 may be greater than the maximum value of the nitrogen concentration in the silicon carbide layer 20. That is, the nitrogen concentration in the second surface 92 may be greater than the nitrogen concentration in the first surface 91. Nitrogen is supplied from the silicon dioxide layer 42 side, and as a result, the maximum value of the nitrogen concentration in the silicon dioxide layer 42 becomes greater than the maximum value of the nitrogen concentration in the silicon carbide layer 20.
[0041] Furthermore, the thickness of the transition region 18 may be 3 nm or more. By making the thickness of the transition region 18 3 nm or more, nitrogen can be sufficiently accumulated. The thickness of the transition region 18 may be 5 nm or less. By making the thickness of the transition region 18 5 nm or less, deterioration of electrical characteristics can be prevented. In this example, the thickness of the transition region 18 is 4 nm. The full width at half maximum of the maximum nitrogen concentration of the transition region 18 may be 1.0 nm or less. By narrowing the full width at half maximum of the maximum nitrogen concentration of the transition region 18, the thickness of the transition region 18 can be made 5 nm or less.
[0042] FIG. 5 is a diagram showing an example of the results of a LEED analysis of silicon carbide layer 20. In FIG. 5, the surface of silicon carbide layer 20 of sample 200 after silicon carbide layer forming step S101 is analyzed by LEED. Silicon carbide layer 20 of sample 200 after silicon carbide layer forming step S101 is referred to as silicon carbide layer 20-1. LEED analysis is low-energy electron diffraction. Also, in FIG. 5, the image is binarized into black and white at a certain threshold value. FIG. 5 shows a certain region of silicon carbide layer 20-1.
[0043] In FIG. 5, the spots (black dots in FIG. 5) are arranged at regular intervals. Therefore, it can be determined by the LEED analysis that the silicon carbide layer 20-1 has a crystalline structure. Whether the spots are arranged at regular intervals may be determined, for example, by whether each spot arranged in the arrangement direction in FIG. 5 can be identified. The arrangement direction is a direction in which at least three or more spots are arranged. In the example of FIG. 5, the arrangement direction may be D1 or D2. In the example of FIG. 5, whether the spot 82 can be identified may be determined as long as each spot arranged in the arrangement direction D1 is clearly a black dot. If the black dots can be identified, the silicon carbide layer 20-1 may be determined to have a crystalline structure.
[0044] Fig. 6 is a diagram showing an example of the results of a LEED analysis of silicon carbide layer 20 heat-treated with NO gas. In Fig. 6, after sample 200 has been subjected to heat treatment step S103, only silicon dioxide layer 42 is removed with HF (hydrofluoric acid), and the surface of silicon carbide layer 20 from which silicon dioxide layer 42 has been removed is subjected to LEED analysis. Silicon carbide layer 20 of sample 200 after heat treatment step S103 is referred to as silicon carbide layer 20-3. Also in Fig. 6, the image is binarized into black and white using a certain threshold value.
[0045] In FIG. 6, compared to FIG. 5, the spots are not arranged at regular intervals, and the arrangement of the black dots cannot be identified. The arrangement direction cannot be determined in FIG. 6. Therefore, in FIG. 6, it can be determined that the spots are not arranged at regular intervals. Therefore, in FIG. 6, it can be determined by the LEED analysis that the silicon carbide layer 20 has crystal disorder. In other words, distortion occurs in the silicon carbide layer 20-3 heat-treated with NO gas.
[0046] Fig. 7 is a diagram showing an example of the results of a LEED analysis of silicon carbide layer 20 after formation of silicon dioxide layer 42. In Fig. 7, after sample 200 has been subjected to silicon dioxide layer forming step S102, only silicon dioxide layer 42 is removed with HF (hydrofluoric acid), and then the surface of silicon carbide layer 20 from which silicon dioxide layer 42 has been removed is subjected to LEED analysis. Silicon carbide layer 20 of sample 200 after silicon oxide layer forming step S102 is referred to as silicon carbide layer 20-2. Also in Fig. 7, the image is binarized into black and white using a certain threshold value.
[0047] No spots are observed in Fig. 7. Therefore, it can be determined that the surface of the silicon carbide layer 20-2 is made amorphous after the formation of the silicon dioxide layer 42.
[0048] Fig. 8 is a diagram showing an example of the results of an XPS analysis of oxygen on silicon carbide layer 20. Fig. 8 shows the results for silicon carbide layer 20-1 (Fig. 5) and silicon carbide layer 20-2 (Fig. 7). XPS is an X-ray photoelectric spectroscopy method.
[0049] 8, silicon carbide layer 20-2 has an increased peak compared to silicon carbide layer 20-1. Therefore, by performing silicon dioxide layer forming step S102, oxygen can be left on the surface of silicon carbide layer 20-2.
[0050] Fig. 9 is a diagram showing an example of the results of an XPS analysis of nitrogen on silicon carbide layer 20. Fig. 9 shows the results for silicon carbide layer 20-3 (Fig. 6).
[0051] 9, a nitrogen peak is present in silicon carbide layer 20-3. Therefore, by performing heat treatment step S103, nitrogen can be made to exist in the surface of silicon carbide layer 20-3.
[0052] Fig. 10 is a diagram showing an example of the results of XPS analysis of silicon on silicon carbide layer 20. Fig. 10 shows the results for silicon carbide layer 20-1 (Fig. 5) and silicon carbide layer 20-3 (Fig. 6).
[0053] 10, silicon carbide layer 20-1 and silicon carbide layer 20-3 have silicon carbide peaks. Furthermore, silicon carbide layer 20-3 has a higher peak of incomplete silicon dioxide (SiOx) than silicon carbide layer 20-1. From the above, it can be determined that silicon carbide layer 20-3 has incomplete silicon dioxide compared to silicon carbide layer 20-1.
[0054] Fig. 11 is a diagram showing the vicinity of transition region 18 captured by a transmission electron microscope image. In Fig. 11, the vicinity of transition region 18 refers to part of silicon dioxide layer 42, transition region 18, and part of silicon carbide layer 20. In Fig. 11, the image has been binarized into black and white using a certain threshold value.
[0055] In Fig. 11, the transition region 18 may be a region where the crystals are disordered. The crystals may be defined as being disordered by contrast. In other words, a region where the contrast is unclear may be the transition region 18. In Fig. 11, the transition region 18 is a region where the difference between black and white is not clear.
[0056] FIG. 12 is a diagram showing the results of EELS analysis of the transition region 18. EELS stands for electron energy loss spectroscopy. The horizontal axis of FIG. 12 indicates loss energy, and the vertical axis indicates depth. In the example of FIG. 12, a peak of a π-C bond exists in the waveform at depth positions of -1.0 nm to -1.6 nm. Therefore, it can be determined that excess carbon is mixed into the transition region 18.
[0057] 13 is a diagram showing in detail the layer structure of the transition region 18. The transition region 18 has a silicon dioxide altered layer 66, a mixed layer 64, and a silicon carbide altered layer 62. The silicon dioxide altered layer 66 is provided below the silicon dioxide layer 42. The mixed layer 64 is provided below the silicon dioxide altered layer 66. The silicon carbide altered layer 62 is provided below the mixed layer 64.
[0058] The silicon dioxide altered layer 66, the mixed layer 64, and the silicon carbide altered layer 62 can be distinguished by SIMS analysis. The maximum carbon concentration is greatest in the silicon carbide altered layer 62, the mixed layer 64, and the silicon carbide altered layer 66, in that order. The maximum oxygen concentration is greatest in the silicon dioxide altered layer 66, the mixed layer 64, and the silicon carbide altered layer 62, in that order. The maximum nitrogen concentration is greatest in the mixed layer 64, the silicon dioxide altered layer 66, and the silicon carbide altered layer 62, in that order. In this way, the silicon dioxide altered layer 66, the mixed layer 64, and the silicon carbide altered layer 62 can be distinguished by SIMS analysis, XPS analysis, etc.
[0059] The silicon carbide alteration layer 62 may have a nitrided incomplete silicon carbide layer 72, an incomplete silicon carbide layer 70, and an amorphous silicon carbide layer 68. The nitrided incomplete silicon carbide layer 72 may be provided below the mixed layer 64. The incomplete silicon carbide layer 70 may be provided below the nitrided incomplete silicon carbide layer 72. The incomplete silicon carbide layer 70 may not contain nitrogen. The amorphous silicon carbide layer 68 may be provided below the incomplete silicon carbide layer 70. The amorphous silicon carbide layer 68 may not contain oxygen. The nitrided incomplete silicon carbide layer 72, the incomplete silicon carbide layer 70, and the amorphous silicon carbide layer 68 can be distinguished by SIMS analysis, XPS analysis, EELS analysis, or the like. Also, whether or not they are amorphous may be determined by LEED analysis or a transmission electron microscope.
[0060] The silicon dioxide alteration layer 66 may have a carbonized incomplete silicon dioxide layer 74 and an incomplete silicon dioxide layer 76. The carbonized incomplete silicon dioxide layer 74 may be provided above the mixed layer 64. The incomplete silicon dioxide layer 76 may be provided above the carbonized incomplete silicon dioxide layer 74. The incomplete silicon dioxide layer 76 may not contain carbon. The carbonized incomplete silicon dioxide layer 74 and the incomplete silicon dioxide layer 76 can be identified by SIMS analysis, XPS analysis, or the like.
[0061] The silicon carbide layer 20 may have a strained silicon carbide layer 80 and a crystalline silicon carbide layer 78. The strained silicon carbide layer 80 may be provided below the transition region 18. The strained silicon carbide layer 80 may be defined by a LEED analysis. That is, as shown in FIG. 6 , the strained silicon carbide layer 80 may be identified based on whether spots are arranged at regular intervals in the LEED analysis. The crystalline silicon carbide layer 78 may be provided below the strained silicon carbide layer 80.
[0062] 14 is a diagram showing another example of the method for forming the sample 200. First, a silicon carbide layer forming step S201 is performed to form a silicon carbide layer 20 on a silicon carbide substrate 10 (S201). The silicon carbide layer forming step S201 may be the same as the silicon carbide layer forming step S101 in FIG.
[0063] Next, a first heat treatment step S202 is carried out (S202). The treatment temperature of the first heat treatment step S202 may be 1200° C. or more and less than 1300° C. The first heat treatment step S202 is carried out by using N 2 The first heat treatment step S202 may be performed in a gas atmosphere of 90% NO gas and 10% NO gas. The treatment time of the first heat treatment step S202 in this example is 5 minutes or more and 10 minutes or less. By performing the first heat treatment step S202, a nitride layer 21 is formed above the silicon carbide layer 20. Also, a silicon dioxide layer 42-1 is formed above the nitride layer 21. The thickness of the silicon dioxide layer 42-1 is, for example, 1 nm or less. Since the silicon dioxide layer 42-1 is provided, it is possible to reduce oxidation in the silicon dioxide formation step S203 and the second heat treatment step S204.
[0064] After the nitride layer 21 and the silicon dioxide layer 42-1 are formed, the silicon dioxide layer formation step S203 is performed. The silicon dioxide layer formation step S203 may be performed by high temperature oxidation (HTO). The high temperature oxidation is performed by using dichlorosilane and N 2The high-temperature oxidation may be performed by introducing O. The processing temperature of the high-temperature oxidation is, for example, 800° C. Note that the high-temperature oxidation may be performed by introducing monosilane instead of dichlorosilane. By performing the silicon dioxide forming step S203, a silicon dioxide layer 42-2 is formed. The thickness of the silicon dioxide layer 42-2 is, for example, 2 nm. Also, by performing the silicon oxide forming step S203, nitrogen in the nitride layer 21 is removed.
[0065] After the silicon dioxide forming step S203 is performed, the second heat treatment step S204 is performed (S204). The treatment temperature of the second heat treatment step S204 may be 50° C. or more higher than the treatment temperature of the first heat treatment step S202. As an example, the treatment temperature of the second heat treatment step S204 may be 100° C. higher than the treatment temperature of the first heat treatment step S202. The treatment temperature of the second heat treatment step S204 may be 1300° C. or more and 1330° C. or less. The second heat treatment step S204 is performed by using N 2 The second heat treatment step S204 may be performed in a gas atmosphere of 90% H2O gas and 10% NO gas. The treatment time of the second heat treatment step S204 in this example is 5 minutes or more and 15 minutes or less. The total treatment time of the first heat treatment step S202 and the second heat treatment step S204 is preferably 30 minutes or less. By setting the treatment temperature of the second heat treatment step S204 higher than the treatment temperature of the first heat treatment step S202, nitrogen can be sufficiently introduced into the nitride layer 21, and defects at the silicon carbide layer 20 interface can be reduced. By performing the second heat treatment step S204, a transition region 18 is formed near the silicon carbide layer 20 interface. The transition region 18 may include the nitride layer 21.
[0066] The gas atmosphere in the first heat treatment step S202 and the gas atmosphere in the second heat treatment step S204 may be different. For example, the first heat treatment step S202 is N 2 The second heat treatment step S204 was carried out in a gas atmosphere of 92% N 2 The experiment is carried out in a gas atmosphere of 88% gas and 12% NO gas.
[0067] Although the present invention has been described above using the embodiments, the technical scope of the present invention is not limited to the scope described in the above embodiments. It is clear to those skilled in the art that various modifications and improvements can be made to the above embodiments. In addition, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.
[0068] It should be noted that the order of execution of each process, such as operations, procedures, steps, and stages, in the devices, systems, programs, and methods shown in the claims, specifications, and drawings is not specifically indicated as "before," "prior to," etc., and may be realized in any order unless the output of a previous process is used in a later process. Even if the operational flow in the claims, specifications, and drawings is described using "first," "next," etc. for convenience, it does not mean that it is essential to perform the process in this order. [Explanation of symbols]
[0069] 10··silicon carbide substrate, 12··silicon carbide layer, 14··high concentration region, 16··base layer, 18··transition region, 20··silicon carbide layer, 21··nitride layer, 22··source region, 25··contact region, 26··first base region, 28··second base region, 38··trench, 42··silicon dioxide layer, 44··gate electrode, 48··interlayer insulating film, 50··source electrode, 52··source electrode pad, 54··drain electrode, 5 6··Drain electrode pad, 62··Silicon carbide altered layer, 64··Mixed layer, 66··Silicon dioxide altered layer, 68··Amorphous silicon carbide layer, 70··Incomplete silicon carbide layer, 72··Nitride incomplete silicon carbide layer, 74··Carbide incomplete silicon dioxide layer, 76··Incomplete silicon dioxide layer, 78··Crystalline silicon carbide layer, 80··Distorted silicon carbide layer, 82··Spot, 91··First surface, 92··Second surface, 100··Silicon carbide semiconductor device, 200··Sample
Claims
1. a silicon carbide layer; a silicon dioxide layer containing nitrogen provided above the silicon carbide layer; a transition region disposed between the silicon carbide layer and the silicon dioxide layer, the transition region comprising carbon, oxygen and nitrogen; Equipped with the transition region is a region from a position, from the silicon dioxide layer toward the silicon carbide layer, where the oxygen concentration of the silicon dioxide layer is 95% of the maximum oxygen concentration in the silicon dioxide layer, to a position, from the silicon carbide layer toward the silicon dioxide layer, where the carbon concentration of the silicon carbide layer is 95% or less of the maximum carbon concentration in the silicon carbide layer, The maximum nitrogen concentration in the transition region is 1.0×10 20 cm -3 That's all. The nitrogen concentration in the transition region has a peak. Silicon carbide semiconductor devices.
2. A silicon carbide layer, a silicon dioxide layer containing nitrogen provided above the silicon carbide layer; a transition region disposed between the silicon carbide layer and the silicon dioxide layer, the transition region comprising carbon, oxygen and nitrogen; Equipped with the transition region is a region from a position, from the silicon dioxide layer toward the silicon carbide layer, where the oxygen concentration of the silicon dioxide layer is 95% of the maximum oxygen concentration in the silicon dioxide layer, to a position, from the silicon carbide layer toward the silicon dioxide layer, where the carbon concentration of the silicon carbide layer is 95% or less of the maximum carbon concentration in the silicon carbide layer, the maximum nitrogen concentration in the transition region is 1.0×10 20 cm −3 or more; The maximum nitrogen concentration of the transition region is at least five times the maximum nitrogen concentration of the silicon dioxide layer. Silicon carbide semiconductor device.
3. A silicon carbide layer, a silicon dioxide layer containing nitrogen provided above the silicon carbide layer; a transition region disposed between the silicon carbide layer and the silicon dioxide layer, the transition region comprising carbon, oxygen and nitrogen; Equipped with the maximum nitrogen concentration in the transition region is 1.0×10 20 cm −3 or more; The full width at half maximum of the nitrogen concentration in the transition region is 1.0 nm or less. Silicon carbide semiconductor device.
4. A silicon carbide layer; a silicon dioxide layer containing nitrogen provided above the silicon carbide layer; a transition region disposed between the silicon carbide layer and the silicon dioxide layer, the transition region comprising carbon, oxygen and nitrogen; Equipped with the maximum nitrogen concentration in the transition region is 1.0×10 20 cm −3 or more; The silicon carbide layer is a strained silicon carbide layer disposed below the transition region and defined by LEED analysis; a crystalline silicon carbide layer provided below the strained silicon carbide layer; have Silicon carbide semiconductor device.
5. A silicon carbide layer; a silicon dioxide layer containing nitrogen provided above the silicon carbide layer; a transition region disposed between the silicon carbide layer and the silicon dioxide layer, the transition region comprising carbon, oxygen, and nitrogen; Equipped with the maximum nitrogen concentration in the transition region is 1.0×10 20 cm −3 or more; The transition region is a silicon dioxide alteration layer provided below the silicon dioxide layer; A mixed layer provided below the silicon dioxide altered layer; a silicon carbide affected layer provided below the mixed layer; having The maximum carbon concentration is greatest in the silicon carbide altered layer, most in the mixed layer, and most in the silicon dioxide altered layer, in that order. The maximum oxygen concentration is greatest in the silicon dioxide altered layer, most in the mixed layer, and most in the silicon carbide altered layer, in that order. The maximum nitrogen concentration is greatest in the mixed layer, the silicon dioxide altered layer, and the silicon carbide altered layer in that order. Silicon carbide semiconductor device.
6. The silicon carbide affected layer is a nitrided incomplete silicon carbide layer provided below the mixed layer; an incomplete silicon carbide layer not containing nitrogen, the incomplete silicon carbide layer being provided below the nitrided incomplete silicon carbide layer; an amorphous silicon carbide layer not containing oxygen provided below the incomplete silicon carbide layer; having The silicon dioxide altered layer is a partially carbide silicon dioxide layer disposed above the mixed layer; a carbon-free incomplete silicon dioxide layer provided above the carbonized incomplete silicon dioxide layer; have The silicon carbide semiconductor device according to claim 5 .
7. The maximum nitrogen concentration of the transition region is 5 times or more the maximum nitrogen concentration of the silicon dioxide layer. The silicon carbide semiconductor device according to claim 1 or 3 to 6.
8. The maximum value of the nitrogen concentration in the silicon dioxide layer is greater than the maximum value of the nitrogen concentration in the silicon carbide layer. The silicon carbide semiconductor device according to claim 1 .
9. The thickness of the transition region is 3 nm or more. The silicon carbide semiconductor device according to claim 1 .
10. The thickness of the transition region is less than or equal to 5 nm. The silicon carbide semiconductor device according to claim 1 .
11. The silicon carbide layer is provided with a trench; Within the trench, the silicon dioxide layer is formed. The silicon carbide semiconductor device according to claim 1 .
12. The silicon dioxide layer, a lower region in which the carbon concentration is less than the nitrogen concentration; an upper region provided above the lower region, the upper region having a carbon concentration greater than a nitrogen concentration; The silicon carbide semiconductor device according to claim 1 , comprising:
Citation Information
Patent Citations
Insulating film structure, and semiconductor device using the same
JP2011082454A
Method for manufacturing silicon carbide semiconductor device
JP2014045053A
Nonvolatile semiconductor memory device, method for manufacturing same, and manufacturing apparatus
US20150069493A1
Silicon carbide semiconductor device and method for manufacturing same
WO2014103186A1