Tray for insulating film forming apparatus, insulating film forming apparatus, and insulating film forming method

The tray design with an annular groove and low thermal conductivity member addresses the issue of insulating film formation on the outer periphery of semiconductor wafers, improving productivity by minimizing defects and enabling continuous film formation.

JP7593310B2Active Publication Date: 2024-12-03SUMCO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021212944
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-27
Publication Date
2024-12-03
Estimated Expiration
2041-12-27

AI Technical Summary

Technical Problem

Conventional methods for forming an insulating film on the back surface of semiconductor wafers result in the formation of insulating film on the outer periphery, leading to defects and reduced productivity due to the need for rework to remove the excess film, which is known as 'bleeding'.

Method used

A tray design for insulating film formation apparatus featuring a cylindrical recess with an annular groove and a low thermal conductivity member, which reduces heat transfer to the wafer periphery, minimizing the formation of the insulating film on the outer periphery by reducing contact area and radiant heat.

Benefits of technology

The tray design effectively suppresses the formation of insulating film on the outer periphery of semiconductor wafers, enhancing productivity by preventing defects and allowing continuous film formation on multiple wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593310000001
    Figure 0007593310000001
  • Figure 0007593310000002
    Figure 0007593310000002
  • Figure 0007593310000003
    Figure 0007593310000003
Patent Text Reader

Abstract

To provide a tray for an insulating film forming apparatus, which can form an insulating film on the backside of a semiconductor wafer while suppressing the formation of an insulating film on the outer periphery of the semiconductor wafer.SOLUTION: A tray 1 for placing a semiconductor wafer in an insulating film forming apparatus for forming an insulating film on the backside of a semiconductor wafer, has a tray body 11 on which the semiconductor wafer is placed, the tray body 11 has a cylindrical recess 11c on the top surface 11a of the tray body 11 that accommodates the semiconductor wafer, and an annular groove 11d in the recess 11c whose inner diameter is smaller than the diameter of the semiconductor wafer and whose outer diameter is larger than the diameter of the semiconductor wafer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tray for an insulating film forming apparatus, an insulating film forming apparatus, and an insulating film forming method. [Background technology]

[0002] In recent years, epitaxial wafers, which have an epitaxial layer of silicon or the like formed on a semiconductor wafer such as a silicon wafer, are generally used as substrates in various semiconductor devices such as MOSFETs (Metal-Oxide-Semiconductor Field-Effect Transistors), DRAMs (Dynamic Random Access Memories), power transistors, and back-illuminated solid-state imaging devices.

[0003] For example, an epitaxial silicon wafer can be obtained by placing a silicon wafer in a single-wafer epitaxial growth furnace, supplying a source gas such as dichlorosilane gas or trichlorosilane gas into the epitaxial growth furnace together with a carrier gas such as hydrogen gas, and growing a silicon epitaxial layer on the silicon wafer.

[0004] Incidentally, when forming an epitaxial layer with high resistivity on a semiconductor wafer with low resistivity, a phenomenon called autodoping is likely to occur, in which dopants in the semiconductor wafer jump out from the back surface of the semiconductor wafer into the gas phase and are incorporated into the epitaxial layer. Therefore, prior to the growth of the epitaxial layer, an insulating film such as an oxide film is formed on the back surface of the semiconductor wafer as a protective film to suppress autodoping (see, for example, Patent Document 1).

[0005] The insulating film is formed by, for example, chemical vapor deposition. long(For example, in the atmospheric pressure CVD method in which CVD is performed at atmospheric pressure, a semiconductor wafer is placed on a tray with the surface on which the insulating film is to be formed (i.e., the back surface) facing up, and then, while the semiconductor wafer is heated, a source gas for the insulating film is supplied onto the semiconductor wafer, thereby forming the insulating film on the back surface of the semiconductor wafer.

[0006] In the conventional method, the insulating film is formed from the back surface of the semiconductor wafer to the edge of the wafer and the front surface of the semiconductor wafer because the insulating film is formed around the edge of the back surface of the semiconductor wafer. On the other hand, when an epitaxial layer is formed on a semiconductor wafer having an insulating film formed on the outer periphery of the wafer from the outer periphery of the back surface to the edge of the wafer and the outer periphery of the front surface, cracks may occur on the outer periphery of the wafer and the epitaxial layer may grow abnormally, that is, nodules may occur. Therefore, when an insulating film is formed on the back surface of the wafer by the conventional method, the insulating film formed on the outer periphery of the wafer is removed after that. The insulating film on the outer periphery of the wafer can be removed by wiping using a nozzle soaked in a removing liquid such as hydrofluoric acid (HF) liquid. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2011 / 070741 Summary of the Invention [Problem to be solved by the invention]

[0008] When removing the insulating film on the outer periphery of the wafer by the above-mentioned wiping method, the removing solution may seep not only into the insulating film on the outer periphery of the wafer but also into part of the insulating film on the back surface of the wafer, which is called "smearing". If such smearing occurs, the semiconductor wafer becomes a defective product and cannot be used as a substrate for an epitaxial wafer. Therefore, it is necessary to once remove the insulating film that has been formed, and then form an insulating film again, which causes a problem of reduced productivity.

[0009] In order to prevent the occurrence of the bleeding described above, it is preferable to prevent the formation of an insulating film on the outer periphery of the wafer.

[0010] The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide a tray for an insulating film forming apparatus that can form an insulating film on the back surface of a semiconductor wafer while suppressing the formation of an insulating film on the outer periphery of the semiconductor wafer. [Means for solving the problem]

[0011] The present invention which solves the above problems is as follows. [1] A tray for placing a semiconductor wafer in an insulating film forming apparatus for forming an insulating film on a back surface of a semiconductor wafer, comprising: A tray body for placing a semiconductor wafer thereon is provided, The tray body includes: The tray body On a cylindrical recess provided on a surface thereof for accommodating the semiconductor wafer; an annular groove provided in the recess, the inner diameter of which is smaller than the diameter of the semiconductor wafer and the outer diameter of which is larger than the diameter of the semiconductor wafer; A tray for an insulating film forming apparatus, comprising:

[0012] [2] The tray for an insulating film forming apparatus described in [1] above, wherein the tray body has a low thermal conductivity member disposed in the annular groove, the low thermal conductivity member being made of a material having a lower thermal conductivity than the material constituting the tray body.

[0013] [3] The tray for an insulating film forming apparatus according to [1] or [2] above, wherein the low thermal conductive member is made of an annular member or a plurality of block-shaped members.

[0014] [4] The tray for an insulating film forming apparatus according to any one of [1] to [3] above, wherein the tray body is made of silicon carbide, and the low thermal conductive member is made of quartz.

[0015] [5] A tray for an insulating film forming apparatus according to any one of [1] to [4], wherein the difference between the inner diameter of the annular groove and the diameter of the semiconductor wafer is 10 mm or more and 20 mm or less, and the difference between the outer diameter of the annular groove and the diameter of the semiconductor wafer is 1 mm or more and 16 mm or less.

[0016] [6] A tray for an insulating film forming apparatus described in any one of [3] to [5], wherein the width of the annular member is smaller than the width of the annular groove, and the difference between the width of the annular member and the width of the annular groove is 1 mm or more and 2 mm or less.

[0017] [7] An apparatus for forming an insulating film on a back surface of a semiconductor wafer, comprising: A tray according to any one of the above [1] to [6], a source gas supply unit disposed above the tray and configured to supply a source gas for the insulating film toward a rear surface of the semiconductor wafer placed on the tray; a heater disposed below the tray for heating the semiconductor wafer; An insulating film forming apparatus comprising:

[0018] [8] A plurality of the trays are provided, and a conveying roller is provided at the bottom of the tray body; The insulating film forming apparatus according to [7] above, wherein the plurality of trays are transported between the raw material gas supply unit and the heater so that the insulating film can be continuously formed on a plurality of semiconductor wafers.

[0019] [9] A method for forming an insulating film, comprising the steps of: placing a semiconductor wafer with its back side facing up on the tray of the insulating film forming apparatus described in [7] or [8] above; then arranging the semiconductor wafer between the raw material gas supply unit and the heater; and, while the semiconductor wafer is heated to a predetermined temperature by the heater, supplying a raw material gas for the insulating film from the raw material gas supply unit to form an insulating film on the back surface of the semiconductor wafer.

[0020]

[10] The method for forming an insulating film according to [9] above, wherein the semiconductor wafer is a silicon wafer.

[0021]

[11] The method for forming an insulating film according to [9] or

[10] above, wherein the insulating film is an oxide film. Effect of the Invention

[0022] According to the present invention, it is possible to form an insulating film on the rear surface of a semiconductor wafer while suppressing the formation of the insulating film on the outer periphery of the semiconductor wafer. [Brief description of the drawings]

[0023] [Figure 1] 1A and 1B are diagrams showing a preferred example of a tray for an insulating film forming apparatus according to the present invention, in which (a) is a top view, (b) is a cross-sectional view taken along line AA of (a), and (c) is an enlarged view of area C surrounded by a dashed line in (b). [Diagram 2] FIG. 1 is a diagram showing an example of an insulating film forming apparatus according to the present invention. [Diagram 3] FIG. 1 is a diagram showing details of a tray used in an example of the invention. [Figure 4] 5A to 5C are diagrams for explaining the positional relationship between the inner diameter of the annular groove and the outer periphery of the wafer in the examples, where (a) is a comparative example, (b) is an example 2 of the invention, and (c) is an example 4 of the invention. [Diagram 5] FIG. 13 is a diagram showing the relationship between the inner diameter of the annular groove and the thickness of the oxide film at the measurement points. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] (Tray for insulating film forming equipment) Hereinafter, an embodiment of the present invention will be described with reference to the drawings. A semiconductor wafer has a front surface which is a flat surface on which devices are formed, a back surface which is a flat surface opposite to the front surface, and a wafer end surface located on the outer side of the front surface and the back surface in the wafer radial direction and connecting the outer edge of the front surface and the outer edge of the back surface. A tray for an insulating film forming apparatus according to the present invention is a tray on which a semiconductor wafer is placed in an insulating film forming apparatus which forms an insulating film on the back surface of a semiconductor wafer, and includes a tray main body on which the semiconductor wafer is placed. Here, the tray main body is characterized by having a cylindrical recess provided on the upper surface of the tray main body for accommodating the semiconductor wafer, and an annular groove provided in the recess, the inner diameter of which is smaller than the diameter of the semiconductor wafer and the outer diameter of which is larger than the diameter of the semiconductor wafer.

[0025] As described above, in conventional insulating film forming apparatuses, the semiconductor wafer is placed on a tray with the surface on which the insulating film is to be formed, i.e., the back side, facing up, and a source gas is supplied from above the semiconductor wafer to form an insulating film on the back side of the semiconductor wafer. In this case, the insulating film is formed not only on the back side of the semiconductor wafer but also from the edge of the wafer to the front side. The insulating film formed on the outer periphery of the wafer, from the outer edge of the back side to the edge of the wafer and then to the outer edge of the front side, can cause nodules and must be removed.

[0026] The present inventors have intensively studied ways to suppress the formation of an insulating film on the outer periphery of a semiconductor wafer as described above. In the process, they focused on a tray on which a semiconductor wafer is placed, and came up with the idea of ​​providing a cylindrical recess for accommodating a semiconductor wafer on the upper surface of a tray body, which is the base of the tray, and providing an annular groove in this recess, the inner diameter of which is smaller than the diameter of the semiconductor wafer and the outer diameter of which is larger than the diameter of the semiconductor wafer. They then found that the formation of an insulating film on the outer periphery of a semiconductor wafer can be suppressed by placing a semiconductor wafer on a tray thus configured with the back side on which the insulating film is to be formed facing upward, and supplying a source gas from above the semiconductor wafer to form the insulating film, thereby completing the present invention. The tray for an insulating film forming apparatus according to the present invention will be described in detail below.

[0027] 1 shows a preferred example of a tray for an insulating film forming apparatus according to the present invention, where (a) is a top view, (b) is an AA cross-sectional view of (a), and (c) is an enlarged view of an area C surrounded by a dashed line in (b). The tray 1 for an insulating film forming apparatus shown in FIG. 1 includes a tray body 11 that constitutes the base of the tray 1. Both an upper surface 11a and a lower surface 11b of the tray body 11 are flat. The tray body 11 also includes a cylindrical recess 11c that is provided on the upper surface 11a of the tray body 11 and that accommodates a semiconductor wafer, and an annular groove 11d that is provided in the recess 11c and has an inner diameter smaller than the diameter of the semiconductor wafer and an outer diameter larger than the diameter of the semiconductor wafer.

[0028] It is preferable that the tray body 11 is made of a material that has heat resistance and deformation resistance against the temperature at which the insulating film is formed and does not contaminate the semiconductor wafers. For example, the tray body 11 can be made of sintered silicon carbide or sintered silicon carbide whose surface is covered with a silicon carbide film.

[0029] The size of the tray body 11 can be appropriately set depending on the diameter and number of semiconductor wafers to be placed, the material constituting the tray body 11, and the like.

[0030] The diameter of the recess 11c is equal to or larger than the outer diameter of the annular groove 11d. The depth of the recess 11c is preferably equal to or larger than the thickness of the semiconductor wafer. This allows the tray 1 (tray body 11) to hold the semiconductor wafer well.

[0031] The annular groove 11d is provided in the recess 11c, and has an inner diameter smaller than the diameter of the semiconductor wafer and an outer diameter larger than the diameter of the semiconductor wafer. By making the inner diameter of the annular groove 11d smaller than the diameter of the semiconductor wafer, the contact area between the semiconductor wafer and the bottom surface of the recess 11c is reduced, and the heat transferred from the tray body 11 to the outer periphery of the semiconductor wafer is reduced, suppressing the temperature rise of the wafer outer periphery and suppressing the formation of an insulating film on the outer periphery of the semiconductor wafer. In addition, by making the outer diameter of the annular groove 11d larger than the diameter of the semiconductor wafer, a space is formed below the outer periphery of the wafer, suppressing the radiant heat from the tray body 11 to the outer periphery of the wafer, suppressing the temperature rise of the wafer outer periphery, and suppressing the formation of an insulating film on the outer periphery of the wafer.

[0032] Specifically, the difference between the inner diameter of the annular groove 11d and the diameter of the semiconductor wafer is preferably 10 mm or more and 20 mm or less. By making the difference between the inner diameter of the annular groove 11d and the diameter of the semiconductor wafer 10 mm or more, the heat transferred to the outer periphery of the wafer can be reduced, improving the effect of suppressing the formation of an insulating film on the outer periphery of the wafer. In addition, by making the difference between the inner diameter of the annular groove 11d and the diameter of the semiconductor wafer 20 mm or less, the width of the region on the outer periphery of the semiconductor wafer where the formation of an insulating film is suppressed can be set to a desired value.

[0033] In addition, the difference between the outer diameter of the annular groove 11d and the diameter of the semiconductor wafer is preferably 1 mm or more and 16 mm or less. By making the difference between the outer diameter of the annular groove 11d and the diameter of the semiconductor wafer 12 1 mm or more, the radiation heat from the tray body 11 to the outer periphery of the wafer is suppressed, the temperature rise of the outer periphery of the wafer is suppressed, and the effect of suppressing the formation of an insulating film on the outer periphery of the wafer is improved. The greater the difference between the outer diameter of the annular groove 11d and the diameter of the semiconductor wafer, the greater the effect of suppressing the radiation heat from the tray body 11 to the outer periphery of the wafer. Therefore, in terms of the effect of suppressing the radiation heat, there is no upper limit to the difference between the outer diameter of the annular groove 11d and the diameter of the semiconductor wafer, but it is preferable to make it 16 mm or less due to restrictions due to the size of the tray body 11.

[0034] The depth of the annular groove 11d is preferably shallower than the thickness of the tray body 11, 4 mm or less. This allows the strength of the tray body 11 to be maintained. Also, the depth of the annular groove 11d is preferably 2 mm or more. This suppresses the radiant heat from the tray body 11 to the outer periphery of the wafer, suppressing the temperature rise of the outer periphery of the wafer, and improves the effect of suppressing the formation of an insulating film on the outer periphery of the wafer.

[0035] On the tray 1 having such a configuration, a semiconductor wafer is placed in the recess 11c with the back side on which the insulating film is formed facing up, and a raw material gas is supplied from above the semiconductor wafer while the tray 1 and the semiconductor wafer are heated to a predetermined temperature by a heater. Then, since the inner diameter of the annular groove 11d provided in the recess 11c is smaller than the diameter of the semiconductor wafer, the contact area between the semiconductor wafer and the tray body 11 is reduced, and the heat transferred from the tray body 11 to the outer periphery of the wafer is reduced. In addition, the space of the annular groove 11d prevents heat from being directly transferred from the tray body 11 to the outer periphery of the wafer, so that the temperature rise of the outer periphery of the wafer is suppressed. In this way, the formation of an insulating film on the outer periphery of the wafer can be suppressed.

[0036] 1, it is preferable that a low thermal conductive member 12 made of a material having a lower thermal conductivity than the material constituting the tray body 11 is disposed in the annular groove 11d. This reduces the radiant heat from the tray body 11 at the bottom of the annular groove 11d, and further reduces the heat transmitted to the outer periphery of the wafer, thereby improving the effect of suppressing the formation of an insulating film on the outer periphery of the wafer.

[0037] As shown in FIG. 1, the low thermal conductive member 12 can be made of an annular member having a size and shape to fit into the annular groove 11d, or can be made of multiple block-shaped members that can be accommodated in the annular groove 11d. The block-shaped member can have any shape, such as a sphere or a rectangular parallelepiped. The annular member may be arranged in the annular groove 11d as a single annular member, or multiple annular members may be stacked and arranged in the annular groove 11d. The block-shaped members can be arranged in a spread manner in the annular groove 11d. Among them, it is more preferable that the low thermal conductive member 12 is made of an annular member, since the effect of suppressing radiant heat to the outer periphery of the wafer can be uniformly obtained in the circumferential direction of the wafer.

[0038] The material constituting the low thermal conductive member 12 is not particularly limited as long as it has a lower thermal conductivity than the material constituting the tray body 11. For example, when the tray body 11 is made of silicon carbide, the low thermal conductive member 12 can be made of quartz, alumina, yttria, etc. Among them, it is preferable that the low thermal conductive member 12 is made of quartz because it is a material that does not contaminate semiconductor wafers.

[0039] When the low thermal conductive member 12 is an annular member, its width (i.e., 1 / 2 the difference between the outer diameter and the inner diameter of the low thermal conductive member 12) is smaller than the width of the annular groove 11d (i.e., 1 / 2 the difference between the outer diameter and the inner diameter of the annular groove 11d), and the difference between them is preferably 1 mm or more and 2 mm or less. By making the difference between the width of the low thermal conductive member 12 and the width of the annular groove 11d 1 mm or more, a sufficient gap is formed between the low thermal conductive member 12 and the annular groove 11d, and the low thermal conductive member 12 can be easily placed in the annular groove 11d. In addition, by making the difference between the width of the low thermal conductive member 12 and the width of the annular groove 11d 2 mm or less, the effect of suppressing radiant heat transferred from the tray body 11 to the semiconductor wafer can be improved.

[0040] Also, the thickness of the low thermal conductive member 12 is preferably 1 mm or more and equal to or less than the depth of the annular groove 11d. By making the thickness of the low thermal conductive member 12 1 mm or more, it is possible to suppress the radiant heat transmitted from the tray body 11 to the outer periphery of the semiconductor wafer. By making the thickness of the low thermal conductive member 12 equal to or less than the depth of the annular groove 11d, the low thermal conductive member 12 does not come into contact with the semiconductor wafer, thereby improving the effect of suppressing the temperature rise of the outer periphery of the semiconductor wafer. Note that, when the low thermal conductive member 12 is formed by stacking a plurality of annular members, the above thickness means the total thickness of the plurality of annular members.

[0041] (Insulating film forming equipment) The insulating film forming apparatus according to the present invention is an apparatus for forming an insulating film on the back surface of a semiconductor wafer, and is characterized by comprising: a tray for the insulating film forming apparatus according to the present invention described above; a raw material gas supply unit arranged above the tray for supplying a raw material gas for the insulating film toward the back surface of the semiconductor wafer placed on the tray; and a heater arranged below the tray for heating the semiconductor wafer.

[0042] An example of an insulating film forming apparatus according to the present invention is shown in Fig. 2. The insulating film forming apparatus 100 shown in Fig. 2 includes a tray 1, a source gas supply unit 2, a heater 3, and a quartz plate 4.

[0043] The tray 1 is the tray 1 according to the present invention shown in Fig. 1, and details thereof have already been described, so they will be omitted. A conveying roller 1a is provided below the tray 1 so that the tray 1 can be conveyed.

[0044] The source gas supply unit 2 is disposed above the tray 1, and supplies the source gas for the insulating film toward the rear surface of the semiconductor wafer W placed on the tray 1 through the recess 11c of the tray 1. In the example shown in Fig. 2, it is configured to supply silane (SiH4) and oxygen gas (O2) which are source gases for supplying a silicon oxide film, but it can also be configured to supply other source gases to form other insulating films such as a nitride film.

[0045] Moreover, as shown in FIG. 2, the raw material gas supply unit 2 is preferably configured to supply an inert gas such as nitrogen or a rare gas so as to surround the raw material gas in order to reduce the inclusion of impurities in the raw material gas.

[0046] The heater 3 is disposed below the tray 1 and heats the semiconductor wafer W to a temperature at which the source gas supplied to the rear surface of the semiconductor wafer W is decomposed and an insulating film is formed on the rear surface of the semiconductor wafer W.

[0047] The quartz plate 4 is a member provided to ensure the movement of the transport rollers 1a that transport the tray 1. For example, when the transport rollers 1a are provided at the four corners of the rear surface of the tray 1, two elongated quartz plates 4 can be arranged parallel to the transport direction of the tray 1, so that the tray 1 can move on the quartz plate 4 via the transport rollers 1a.

[0048] Here, the operation of the insulating film forming apparatus 100 will be described. First, the semiconductor wafer W is placed on the tray 1 so that the back side on which the insulating film is to be formed faces upward and is accommodated in the recess 11c. Next, the tray 1 is placed below the raw material gas supply unit 2 and above the heater 3.

[0049] Next, the semiconductor wafer W is heated to a predetermined temperature by the heater 3, and then a raw material gas for the insulating film is supplied from the raw material gas supply unit 2. In this manner, the formation of the insulating film on the outer periphery of the semiconductor wafer W is suppressed, and the insulating film can be formed on the back surface of the semiconductor wafer W.

[0050] In addition, the insulating film forming apparatus 100 is preferably configured to include a plurality of trays 1 and to transport the plurality of trays 1 between the raw material gas supply unit 2 and the heater 3. This allows the insulating film to be formed on a plurality of semiconductor wafers W continuously.

[0051] (Insulating film formation method) The insulating film forming method according to the present invention is characterized in that a semiconductor wafer is placed with its back side facing up on a tray of the insulating film forming apparatus according to the present invention described above, and then the semiconductor wafer is disposed between a raw material gas supply unit and a heater. After that, while the semiconductor wafer is heated to a predetermined temperature by the heater, a raw material gas for the insulating film is supplied from the raw material gas supply unit to form an insulating film on the back surface of the semiconductor wafer.

[0052] An example of the insulating film forming method according to the present invention will be described below using the insulating film forming apparatus 100 according to the present invention shown in Fig. 2. First, the semiconductor wafer W is placed on the tray 1 so that the back side on which the insulating film is to be formed faces upward and is accommodated in the recess 11c.

[0053] The semiconductor wafer W is not particularly limited, and may be a silicon wafer, a germanium wafer, a silicon carbide wafer, a gallium arsenide wafer, etc. In particular, a silicon wafer can be suitably used as the semiconductor wafer.

[0054] The diameter of the semiconductor wafer W is not particularly limited and can be set according to the material and design constituting the semiconductor wafer W. When the semiconductor wafer W is a silicon wafer, the diameter can be 150 mm or more, for example, 150 mm, 200 mm, 300 mm, or 450 mm.

[0055] The insulating film is not particularly limited, but may be an oxide film, a nitride film, etc. For example, in the case of an epitaxial silicon wafer in which a silicon epitaxial layer is formed on a silicon wafer, the oxide film may be a silicon oxide film or a silicon nitride film.

[0056] Next, the tray 1 is placed below the raw material gas supply unit 2 and above the heater 3 .

[0057] Subsequently, the semiconductor wafer W is heated to a predetermined temperature by the heater 3, and then a source gas for the insulating film is supplied from the source gas supply unit 2 to form an insulating film on the rear surface of the semiconductor wafer W.

[0058] The temperature of the semiconductor wafer during the formation of the insulating film depends on the type of insulating film to be formed, but for example, when a silicon oxide film is formed on the back surface of a silicon wafer, it is preferably set to 380° C. or higher and 460° C. or lower.

[0059] The source gas supplied from the source gas supply unit 2 can be an appropriate gas depending on the source material of the insulating film. For example, when the insulating film is a silicon oxide film, the source gas can be SiH4 gas and O2 gas. When the insulating film is a silicon nitride film, the source gas can be SiH4 gas and N2 gas or ammonia (NH3) gas.

[0060] Moreover, the region where the insulating film is not formed can be adjusted by the inner diameter and depth of the annular groove 11d, or by the thickness of the low thermal conductive member 12.

[0061] In this way, the formation of the insulating film on the outer periphery of the semiconductor wafer W can be suppressed, and the insulating film can be formed on the back surface of the semiconductor wafer W. EXAMPLES

[0062] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0063] (Example 1) A silicon oxide film was formed on the back surface of a silicon wafer using an insulating film forming apparatus 100 shown in FIG. 2 equipped with a tray 1 shown in FIG. 1. Detailed dimensions of the tray 1 are shown in FIGS. 3(a) to 3(c). The annular groove 11d provided on the upper surface 11a of the tray body 11 had an inner diameter of 195 mm, an outer diameter of 216 mm, and a width of 10.5 mm. The low thermal conductive member 12 was composed of a quartz ring (width: 9.5 mm, thickness: 2 mm).

[0064] Specifically, first, a silicon wafer having a diameter of 200 mm was prepared, and placed on the tray 1 so that the back side on which the insulating film was to be formed was faced upward and accommodated in the recess 11c.

[0065] Next, the tray 1 was placed below the source gas supply unit 2 and above the heater 3 of the insulating film forming apparatus 100 .

[0066] Next, the silicon wafer was heated to 450° C. by the heater 3 and maintained at that temperature, and SiH4 gas and O2 gas were supplied from the raw material gas supply unit 2. In this manner, a silicon oxide film was formed on the back surface of the silicon wafer.

[0067] (Example 2) As in Example 1, a silicon oxide film was formed on the back surface of a silicon wafer with a diameter of 200 mm. However, in the tray 1, the inner diameter of the annular groove 11d provided on the upper surface 11a of the tray body 11 was set to 190 mm, and the width of the quartz ring was set to 12 mm. All other conditions were the same as in Example 1.

[0068] (Example 3) As in Example 1, a silicon oxide film was formed on the back surface of a silicon wafer with a diameter of 200 mm. However, in the tray 1, the inner diameter of the annular groove 11d provided on the upper surface 11a of the tray body 11 was set to 180 mm, and the width of the quartz ring was set to 17 mm. All other conditions were the same as in Example 1.

[0069] (Example 4) As in Example 1, a silicon oxide film was formed on the back surface of a silicon wafer with a diameter of 200 mm. However, in the tray 1, the inner diameter of the annular groove 11d provided on the upper surface 11a of the tray body 11 was 185 mm, and the width of the quartz ring was 14.5 mm. All other conditions were the same as in Example 1.

[0070] (Comparative Example) As in Example 1, a silicon oxide film was formed on the back surface of a silicon wafer with a diameter of 200 mm. However, in the tray 1, the inner diameter of the annular groove 11d provided on the upper surface 11a of the tray body 11 was set to 200 mm, and the width of the quartz ring was set to 7 mm. All other conditions were the same as in Example 1.

[0071] (Conventional example) A silicon oxide film was formed on the back surface of a silicon wafer in the same manner as in Example 1. However, the silicon oxide film was formed using the apparatus described in Patent Document 1. All other conditions were the same as in Example 1.

[0072] <Evaluation of oxide film thickness> The thickness of the oxide film formed on the silicon wafers of Examples 1 to 4, the comparative example, and the conventional example was measured. The thickness of the silicon wafers of Examples 1 to 4 and the comparative example was measured at a position 99.5 mm from the center of the recess using a film thickness measuring device (Nanospec 8000XSE, manufactured by NANOMETRICS). FIG. 4 is a diagram for explaining the positional relationship between the inner diameter of the annular groove and the outer periphery of the wafer, where (a) is for the comparative example, (b) is for Example 2, and (c) is for Example 4. Meanwhile, for the silicon wafers of the conventional examples, the thickness of the oxide film was measured every 90°, and the average value was obtained. The measurement results obtained are shown in FIG. 5.

[0073] As is clear from FIG. 5, the average thickness of the oxide film in the conventional example was about 3500 Å. In addition, in the comparative example in which the inner diameter of the annular groove provided on the upper surface of the tray body was equal to the diameter of the silicon wafer, the thickness of the oxide film was about the same as that of the conventional example. On the other hand, in the invention examples 1 to 4, the thickness of the oxide film was reduced compared to the conventional example, and the thickness of the oxide film decreased as the inner diameter of the annular groove became smaller. In particular, in the invention examples 3 and 4 in which the inner diameter of the annular groove was 185 mm or less, the thickness of the oxide film was significantly reduced, and in the invention example 4, the thickness of the oxide film was zero. [Industrial Applicability]

[0074] INDUSTRIAL APPLICABILITY According to the present invention, an insulating film can be formed on the rear surface of a wafer while suppressing the formation of the insulating film on the outer periphery of the wafer, and therefore the present invention is useful in the semiconductor wafer manufacturing industry. [Explanation of symbols]

[0075] 1 tray 1a Transport roller 2. Raw gas supply section 3. Heater 4 Quartz plate 11 Tray body 11a Top side 11b Bottom side 11c Recess 11d Annular groove 12 Annular member 12a opening 100 Insulating film forming device W Semiconductor wafer

Claims

1. A tray for placing a semiconductor wafer in an insulating film forming apparatus for forming an insulating film on a back surface of a semiconductor wafer, comprising: A tray body for placing a semiconductor wafer thereon is provided, The tray body includes: a cylindrical recess provided on an upper surface of the tray body for accommodating the semiconductor wafer; an annular groove provided in the recess, the inner diameter of which is smaller than the diameter of the semiconductor wafer and the outer diameter of which is larger than the diameter of the semiconductor wafer; A tray for an insulating film forming apparatus, comprising:

2. 2. The tray for an insulating film forming apparatus according to claim 1, wherein the tray body has a low thermal conductivity member disposed in the annular groove, the low thermal conductivity member being made of a material having a lower thermal conductivity than a material constituting the tray body.

3. 3. The tray for an insulating film forming apparatus according to claim 2, wherein said low thermal conductive member is made of an annular member or a plurality of block-shaped members.

4. 4. The tray for an insulating film forming apparatus according to claim 3, wherein the width of said annular member is smaller than the width of said annular groove, and the difference between the width of said annular member and the width of said annular groove is 1 mm or more and 2 mm or less.

5. 5. The tray for an insulating film forming apparatus according to claim 2, wherein the tray body is made of silicon carbide, and the low thermal conductive member is made of quartz.

6. 6. A tray for an insulating film forming apparatus according to any one of claims 1 to 5, wherein the difference between the inner diameter of the annular groove and the diameter of the semiconductor wafer is 10 mm or more and 20 mm or less, and the difference between the outer diameter of the annular groove and the diameter of the semiconductor wafer is 1 mm or more and 16 mm or less.

7. An apparatus for forming an insulating film on a back surface of a semiconductor wafer, comprising: A tray according to any one of claims 1 to 6; a source gas supply unit disposed above the tray and configured to supply a source gas for the insulating film toward a rear surface of the semiconductor wafer placed on the tray; a heater disposed below the tray for heating the semiconductor wafer; An insulating film forming apparatus comprising:

8. A plurality of the trays are provided, and a conveying roller is provided at the bottom of the tray body, 8. The insulating film forming apparatus according to claim 7, wherein the plurality of trays are transported between the raw material gas supply unit and the heater so that the insulating film can be continuously formed on a plurality of semiconductor wafers.

9. 9. An insulating film forming method comprising the steps of: placing a semiconductor wafer with its back side facing up on the tray of the insulating film forming apparatus according to claim 7 or 8; arranging the semiconductor wafer between the raw material gas supply unit and the heater; and, while the semiconductor wafer is heated to a predetermined temperature by the heater, supplying a raw material gas for the insulating film from the raw material gas supply unit to form an insulating film on the back surface of the semiconductor wafer.

10. 10. The method for forming an insulating film according to claim 9, wherein the semiconductor wafer is a silicon wafer.

11. 11. The method for forming an insulating film according to claim 9, wherein the insulating film is an oxide film.

Citation Information

Patent Citations

  • Semiconductor wafer and manufacture thereof

    JP1989246822A

  • Wafer tray for CVD system

    JP1997115840A

  • A holder that supports wafers during semiconductor manufacturing

    JP2007518249A

  • Conveyance tray and vacuum treatment apparatus using the same

    JP2008171996A

  • Susceptor and semiconductor manufacturing apparatus

    JP2012033574A