Resin sheets, metal foil laminates, and printed wiring boards

A resin sheet with a tailored resin composition addresses warpage and rigidity issues in printed wiring boards by optimizing storage modulus and glass transition temperature, improving handling and heat resistance.

JP7593314B2Active Publication Date: 2024-12-03MITSUBISHI GAS CHEM CO INC
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2021526986
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-26
Filing Date
2020-06-22
Publication Date
2024-12-03
Estimated Expiration
2040-06-22

AI Technical Summary

Technical Problem

Existing printed wiring boards face challenges in reducing warpage while maintaining rigidity and heat resistance, as previous solutions like reducing thermal expansion coefficients are insufficient.

Method used

A resin sheet with a specific resin composition that satisfies certain storage modulus and glass transition temperature ranges, combined with a support, to enhance viscous behavior and improve handling properties.

Benefits of technology

The resin sheet effectively reduces warpage and enhances rigidity and heat resistance in printed wiring boards, ensuring better handling and performance in manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593314000001
    Figure 0007593314000001
  • Figure 0007593314000002
    Figure 0007593314000002
  • Figure 0007593314000003
    Figure 0007593314000003
Patent Text Reader

Abstract

This resin sheet is provided with a support body, and a layer which is arranged on the surface of the support body and which contains a resin composition that satisfies the relations expressed in (i), (ii) and (iii). (i) ... 0.15 ≤ b / a ≤ 0.60, (ii) ... 0.015 ≤ c / a ≤ 0.07, and (iii) 3 ≤ a ≤ 10 (a, b and c in formulas (i), (ii) and (iii) represent the storage modulus (unit: GPa) at 40°C, 170°C and 230°C in a cured product of the aforementioned resin composition).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin sheet, a metal foil-clad laminate, and a printed wiring board. [Background technology]

[0002] In recent years, semiconductor packages, which are widely used in electronic devices, communication devices, personal computers, etc., have become more highly functional and smaller, and the integration and high density mounting of each component has been accelerating. Accordingly, the properties required for printed wiring boards for semiconductor packages are becoming more and more stringent. Examples of properties required for such printed wiring boards include low water absorption, moisture absorption heat resistance, flame retardancy, low dielectric constant, low dielectric dissipation factor, low thermal expansion coefficient, heat resistance, chemical resistance, and high plating peel strength. In addition to these, suppressing the warping of printed wiring boards (achieving low warping) has become an important issue, and various studies have been conducted.

[0003] For example, Patent Document 1 describes a resin sheet that has a support and an adhesive layer, and that reduces warping in a high-temperature environment when applied to a printed wiring board. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-179564 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in Patent Document 1, the warpage of the printed wiring board is reduced by decreasing the thermal expansion coefficient, so the warpage cannot be reduced sufficiently. Therefore, further improvements in the reduction of warpage are desired.

[0006] In response to this, the present inventors conducted extensive research and found that in order to reduce the warpage of a printed wiring board, it is effective to reduce the elastic modulus of a cured product of a resin composition (hereinafter also referred to as a "resin material") used in a printed wiring board and to cause the resin composition to exhibit viscous behavior in a resin sheet having a layer containing the resin composition. Therefore, the present inventors considered using a resin material that has a low elastic modulus and is prone to plastic deformation (exhibits viscous behavior). However, when such a resin material is used, another problem occurs in that the handling properties (handling ability) in the manufacturing process of the printed wiring board are insufficient due to the low rigidity. In addition, such a resin material tends to have a high water absorption rate and insufficient heat resistance and chemical resistance, which may cause further problems from the viewpoint of quality.

[0007] Therefore, an object of the present invention is to provide a resin sheet, a metal foil-clad laminate, and a printed wiring board that can sufficiently reduce the warping of a printed wiring board (achieve low warping) while also exhibiting excellent rigidity and heat resistance. [Means for solving the problem]

[0008] As a result of extensive research to solve the above problems, the inventors have discovered that by using a resin sheet having a layer containing a resin composition in the form of a cured product obtained by curing the resin composition, the physical property parameters defined by the storage modulus at a predetermined temperature fall within a predetermined range, it is possible to sufficiently reduce warping of a printed wiring board and to exhibit excellent rigidity and heat resistance, thereby completing the present invention.

[0009] That is, the present invention is as follows. [1] A resin sheet comprising a support and a layer disposed on a surface of the support, the layer containing a resin composition that satisfies the relationships represented by the following formulas (i), (ii), and (iii): 0.15≦b / a≦0.60 (i) 0.015≦c / a≦0.07 (ii) 3≦a≦10 (iii) (In formulas (i), (ii), and (iii), a, b, and c respectively represent the storage modulus (unit: GPa) of the cured product of the resin composition at 40° C., 170° C., and 230° C.). [2] The resin sheet described in [1], wherein the resin composition further satisfies the relationship represented by the following formula (iv). 175≦Tg≦215…(iv) (In formula (iv), Tg represents the glass transition temperature (unit: ° C.) of the cured product of the resin composition.) [3] The resin sheet according to [1] or [2], wherein the resin composition further satisfies the relationship represented by the following formula (v). 0.015≦d / a≦0.08…(v) (In formula (v), d represents the storage modulus (unit: GPa) at 260° C. of the cured product of the resin composition, and a has the same meaning as defined above.) [4] The resin sheet according to any one of [1] to [3], wherein the resin composition contains an elastomer component. [5] A resin sheet according to any one of [1] to [4], wherein the resin composition contains at least one compound selected from the group consisting of cyanate ester compounds, phenol compounds, epoxy compounds, and maleimide compounds.

[0010] [6] The resin sheet according to [5], wherein the resin composition contains the cyanate ester compound and / or the phenol compound, and the epoxy compound and / or the maleimide compound. [7] The resin sheet according to [5] or [6], wherein the resin composition contains the phenol compound and the epoxy compound and / or the maleimide compound. [8] The resin sheet according to any one of [5] to [7], wherein the resin composition contains two or more types of the epoxy compounds, and the two or more types of the epoxy compounds contain a naphthalene-type epoxy resin and / or an aralkyl-type epoxy resin having a naphthalene skeleton. [9] A resin sheet according to any one of [1] to [8], wherein the resin composition contains a filler and the content of the filler is 100 parts by mass to 700 parts by mass per 100 parts by mass of resin solids in the resin composition.

[10] The resin sheet described in [9], wherein the filler includes an inorganic filler and / or an organic filler.

[0011]

[11] The resin sheet according to

[10] , wherein the inorganic filler comprises at least one selected from the group consisting of silica, boehmite, and alumina.

[12] The resin sheet according to any one of [1] to

[11] , wherein the support is a resin sheet or a metal foil.

[13] A metal foil-clad laminate comprising a layer containing a cured product of the resin composition according to any one of [1] to

[11] , and a metal foil disposed on one or both sides of the layer containing the cured product.

[14] A printed wiring board comprising an insulating layer containing a cured product of the resin composition according to any one of [1] to

[11] , and a conductor layer disposed on a surface of the insulating layer. Effect of the Invention

[0012] According to the present invention, it is possible to provide a resin sheet, a metal foil-clad laminate, and a printed wiring board that can sufficiently reduce warping of a printed wiring board (achieve low warping) and exhibit excellent rigidity and heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Below, we will explain in detail the form for implementing the present invention (hereinafter referred to as the "present embodiment"). However, the present invention is not limited to this, and various modifications are possible without departing from the gist of the present invention.

[0014] As used herein, unless otherwise specified, the term "resin solids" refers to the components in the resin composition of this embodiment excluding additives (silane coupling agents, wetting dispersants, curing accelerators, etc.), solvents, and fillers (organic fillers and inorganic fillers), and 100 parts by mass of resin solids refers to 100 parts by mass of the total components in the resin composition excluding additives (silane coupling agents, wetting dispersants, curing accelerators, etc.), solvents, and fillers (organic fillers and inorganic fillers).

[0015] [Resin sheet] The resin sheet of the present embodiment comprises a support and a layer, disposed on the surface of the support, containing a resin composition that satisfies the relationships represented by the following formulas (i), (ii), and (iii). That is, the resin sheet of the present embodiment is, for example, a support having the above-mentioned resin composition applied to one or both sides thereof. 0.15≦b / a≦0.60 (i) 0.015≦c / a≦0.07 (ii) 3≦a≦10 (iii)

[0016] In formulas (i), (ii), and (iii), a, b, and c respectively represent the storage modulus (unit: GPa) of the cured product obtained by curing the resin composition at 40° C., 170° C., and 230° C. In this embodiment, the storage modulus of the cured product at 40° C., 170° C., and 230° C. is 30 kgf / cm 2 The resin composition is cured at 230° C. for 100 minutes, and the cured product is subjected to dynamic viscoelasticity measurement (DMA) in accordance with JIS C6481. The specific measurement method is as described in the Examples.

[0017] In this embodiment, by using a resin sheet having a layer containing a resin composition having the above-mentioned configuration, it is possible to sufficiently reduce warping of a metal foil laminate, a printed wiring board, and a multilayer printed wiring board (e.g., a multilayer coreless substrate), and to exhibit excellent rigidity and heat resistance. The reason for this is considered to be as follows. Note that the following description includes considerations, but the present embodiment is not limited by these considerations.

[0018] That is, in order to reduce the warpage of a printed wiring board, it is important to reduce the elastic modulus of the cured product of the resin composition (resin material) used in the printed wiring board and to cause the resin composition to exhibit viscous behavior in a resin sheet having a layer containing the resin composition (resin material). Therefore, it is considered to use a resin material that has a low elastic modulus and is easily plastically deformed (exhibits viscous behavior). However, when such a resin material is used, the handling (handling) in the manufacturing process of a printed wiring board (for example, a thin substrate such as a multilayer coreless substrate) is insufficient due to low rigidity. In addition, such a resin material tends to have a high water absorption rate and insufficient heat resistance and chemical resistance, which causes problems from the viewpoint of quality.

[0019] In contrast, in the resin sheet having a layer containing the resin composition of this embodiment, in the form of the cured product obtained by curing the resin composition (also referred to as the "cured form of the resin composition"), the storage modulus at 40 ° C. is within a predetermined range (satisfying the above formula (iii)), and therefore the rigidity can be sufficiently ensured and the warping of metal foil-clad laminates, printed wiring boards, and multilayer printed wiring boards (for example, multilayer coreless substrates) can be reduced. In addition, in the cured form of the resin composition, the ratio of the storage modulus at 170 ° C. to the storage modulus at 40 ° C. is within a predetermined range (satisfying the above formula (i)), and therefore the rigidity is sufficiently maintained even when heated to 170 ° C. As a result, by using the resin sheet of this embodiment, for example, in the manufacturing process of a printed wiring board (for example, a thin substrate such as a multilayer coreless substrate), it is possible to impart handleability. In addition, by setting the ratio of the storage modulus at 230°C to the storage modulus at 40°C within a predetermined range (satisfying the above formula (ii)), viscous behavior can be exhibited during a process including a heat treatment (for example, a press molding process, an annealing process, etc.). As a result, the warping of a metal foil-clad laminate, a printed wiring board, and a multilayer printed wiring board (for example, a multilayer coreless substrate) can be reduced. In addition, by setting the storage modulus at 40°C within a predetermined range (satisfying the above formula (iii)) and setting the ratio of the storage modulus at 170°C to the storage modulus at 40°C within a predetermined range (satisfying the above formula (i)), excellent heat resistance can be imparted to a metal foil-clad laminate, a printed wiring board, and a multilayer printed wiring body. In addition, as described later, by setting the glass transition temperature of the cured product of the resin composition within a predetermined range (satisfying the following formula (iv)), excellent heat resistance can be imparted to a metal foil-clad laminate, a printed wiring board, and a multilayer printed wiring body. Furthermore, as described below, by making the storage modulus of the cured resin composition at 260°C fall within a predetermined range (satisfying the following formula (v)), it is possible to impart even better heat resistance to the metal foil-clad laminate, the printed wiring board, and the multilayer printed wiring body.

[0020] The resin sheet of this embodiment is preferably a resin sheet that is semi-cured (B-staged) after the resin composition in the layer containing the resin composition according to this embodiment is applied to a support. In this embodiment, the semi-cured state (B-stage) refers to a state in which each component contained in the layer containing the resin composition has not actively started to react (cure), but the layer containing the resin composition is in a dry state, that is, the layer is heated to a degree where it is no longer sticky, and the state in which the solvent has only volatilized without curing even without heating is also included. In this embodiment, the minimum melt viscosity of the semi-cured state (B-stage) is usually 20,000 Pa·s or less. In this embodiment, the minimum melt viscosity is measured by the following method. That is, 1 g of resin powder collected from the layer containing the resin composition is used as a sample, and the minimum melt viscosity is measured by a rheometer (TA Instruments ARES-G2 (trade name)). Here, a disposable plate with a diameter of 25 mm is used to measure the minimum melt viscosity of the resin powder under the conditions of a temperature rise rate of 2°C / min, a frequency of 10.0 rad / sec, and a strain of 0.1% in the range of 40°C to 180°C. The lower limit of the minimum melt viscosity is, for example, 10 Pa s or more.

[0021] The support and the layer containing the resin composition in the resin sheet of this embodiment will be described. (Support) The support according to the present embodiment is not particularly limited, but may be a known one used in various printed wiring board materials, and is preferably a resin sheet or metal foil. The resin sheet is different from the layer containing the resin composition layer according to the present embodiment. Examples of the resin sheet and metal foil include resin sheets such as polyimide film, polyamide film, polyester film, polyethylene terephthalate (PET) film, polybutylene terephthalate (PBT) film, polypropylene (PP) film, and polyethylene (PE) film, and metal foils such as aluminum foil, copper foil, and gold foil. Among them, copper foil and PET film are preferred. As the copper foil, a commercially available product may be used, and examples thereof include 3EC-VLP (trade name) manufactured by Mitsui Mining & Smelting Co., Ltd., 3EC-M2S-VLP (trade name) manufactured by Mitsui Mining & Smelting Co., Ltd., MT18Ex (trade name) manufactured by Mitsui Mining & Smelting Co., Ltd., and JXUT-I (trade name) manufactured by JX Nippon Mining & Metals Co., Ltd.

[0022] [Characteristics of Resin Composition] In a resin sheet having a layer containing the resin composition of this embodiment, the resin composition, in the cured product (hereinafter simply referred to as the "cured product") obtained by curing the resin composition, has physical property parameters defined by the storage modulus at a specified temperature that fall within a specified range, as described above.

[0023] 0.15≦b / a≦0.60 (i) 0.015≦c / a≦0.07 (ii) 3≦a≦10 (iii)

[0024] In formulas (i), (ii), and (iii), a, b, and c represent the storage modulus (unit: GPa) of the cured product of the resin composition at 40° C., 170° C., and 230° C., respectively.

[0025] In this embodiment, the cured product is obtained by thermally curing the above resin composition under conditions of a heating temperature of 180°C to 270°C and a heating time of 30 to 210 minutes, and refers to a cured product that satisfies at least the above formulas (i), (ii), and (iii). The heating temperature is preferably 200°C to 240°C, more preferably 225°C to 235°C, and even more preferably 230°C. The heating time is preferably 60 to 180 minutes, and more preferably 100 minutes. The pressure conditions for curing are not particularly limited as long as they do not impair the effects of this embodiment, and conditions suitable for curing a normal resin composition can be used. The pressure conditions are preferably 10 kgf / cm 2 ~50kgf / cm 2 and more preferably 20 kgf / cm 2 ~40kgf / cm 2 and more preferably 30 kgf / cm 2 The heating means for curing the resin composition is not particularly limited as long as it does not impair the effects of the present embodiment, and a typical heating means (for example, a dryer, etc.) may be used.

[0026] The storage modulus of the cured product can be measured by DMA (Dynamic Mechanical Analysis) in accordance with JIS C6481. The specific measurement method is as described in the Examples.

[0027] In the above formula (iii), when a (storage modulus at 40°C) is 3 GPa or more, it is believed that sufficient rigidity can be ensured. From the same viewpoint, a is preferably 4 GPa or more, and more preferably 4.5 GPa or more. On the other hand, when a is 10 GPa or less, it is believed that warping of metal foil-clad laminates, printed wiring boards, and multilayer printed wiring boards (for example, multilayer coreless substrates) can be reduced. From the same viewpoint, a is preferably 8 GPa or less, and more preferably 7 GPa or less.

[0028] In the above formula (i), when b / a (the ratio of the storage modulus at 170°C to the storage modulus at 40°C) is 0.15 or more, it is believed that the rigidity is sufficiently maintained even when heated to 170°C. As a result, by using a resin sheet having a layer containing the resin composition of this embodiment, it is believed that the handling property (handling ability) is excellent in the manufacturing process of, for example, a printed wiring board (for example, a thin board such as a multilayer coreless board). From the same viewpoint, it is preferable that b / a is 0.17 or more. On the other hand, it is preferable that b / a is 0.60 or less.

[0029] In the above formula (ii), when c / a (the ratio of the storage modulus at 230°C to the storage modulus at 40°C) is within the above range, it is considered that viscous behavior can be exhibited during a process including a heat treatment (e.g., a press molding process, an annealing process, etc.). As a result, it is considered that the warpage of a metal foil-clad laminate, a printed wiring board, and a multilayer printed wiring board (e.g., a multilayer coreless substrate) can be reduced. The lower limit of c / a is preferably 0.02 or more from the viewpoint of further improving the handleability (handling ability) in the manufacturing process of a printed wiring board (e.g., a thin substrate such as a multilayer coreless substrate). The upper limit of c / a is more preferably 0.06 or less from the viewpoint of further reducing the warpage of a metal foil-clad laminate, a printed wiring board, and a multilayer printed wiring board (e.g., a multilayer coreless substrate).

[0030] In a resin sheet having a layer containing the resin composition of this embodiment, it is preferable that the glass transition temperature of the cured product obtained by curing the resin composition satisfies the following formula (iv), since this can improve heat resistance and also allows the above formula (ii) to be controlled within the desired range. 175≦Tg≦215…(iv) The glass transition temperature is more preferably from 180°C to 213°C.

[0031] The glass transition temperature of the cured product can be measured by the DMA method in accordance with JIS C6481. The specific measurement method is as described in the Examples.

[0032] In the resin sheet having a layer containing the resin composition of this embodiment, it is preferable that a cured product obtained by curing the resin composition further satisfies the relationship represented by the following formula (v). 0.015≦d / a≦0.08…(v)

[0033] In the above formula (v), d represents the storage modulus (unit: GPa) of the cured product of the resin composition at 260°C, and a has the same meaning as above. In this embodiment, the storage modulus of the cured product at 260°C can be obtained by the same method as the storage modulus of the cured product described above, and can be measured by the DMA method in accordance with JIS C6481. The specific measurement method is as described in the Examples.

[0034] When the cured product satisfies the relationship represented by the above formula (v), the heat resistance of the cured product is more excellent. For example, the cured product tends to exhibit sufficient heat resistance even when exposed to a high temperature of 300°C, and further tends to have better handleability in the mounting process for mounting a semiconductor chip on a printed wiring board (e.g., a multilayer coreless substrate). From the same viewpoint, the lower limit of d / a is more preferably 0.018 or more.

[0035] [Constituents of Resin Composition] (Elastomer component) The resin composition in the layer containing the resin composition according to the present embodiment may contain, but is not limited to, an elastomer component. When the resin composition contains an elastomer component, the storage modulus of the cured product at a predetermined temperature tends to decrease. The elastomer component is not limited to, but examples thereof include acrylic rubber, silicone rubber, acrylonitrile butadiene rubber, styrene butadiene rubber, butadiene rubber, polyisoprene rubber, urethane rubber, butyl rubber, and core-shell rubber, which are different from the organic filler and other additives described below. These elastomer components may be used alone or in combination of two or more.

[0036] The acrylic rubber is not particularly limited, but examples thereof include alkyl acrylates such as ethyl acrylate and butyl acrylate. The silicone rubber is not particularly limited, but examples thereof include copolymers containing dimethylsiloxane groups, methylvinyl groups, methylphenyl groups, and diphenylsiloxane groups, and polydimethylsiloxanes composed only of dimethylsiloxane groups. Examples of the core-shell rubber include, but are not limited to, methacrylate ester-styrene / butadiene rubber graft copolymer, acrylonitrile-styrene / butadiene rubber graft copolymer, acrylonitrile-styrene / ethylene-propylene rubber graft copolymer, acrylonitrile-styrene / acrylic acid ester graft copolymer, methacrylate / acrylic acid ester rubber graft copolymer, and methacrylate ester-acrylonitrile / acrylic acid ester rubber graft copolymer.

[0037] The content of the elastomer is not particularly limited, but is, for example, less than 30 parts by mass, preferably 25 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the resin solid content in the resin composition. By making the content less than the above value, the heat resistance and water absorbency of the obtained cured product tend to be further improved.

[0038] (Short glass fibers with an average fiber length of 10 μm to 300 μm) The resin composition in the layer containing the resin composition according to the present embodiment may contain glass short fibers having an average fiber length of 10 μm to 300 μm, but is not particularly limited thereto. When the resin composition contains glass short fibers, excellent adhesion to the copper foil, toughness is imparted to the layer containing the resin composition, and a low thermal expansion coefficient tends to be obtained. In this embodiment, the glass short fibers having an average fiber length of 10 μm to 300 μm are different from the inorganic filler described below. Such glass short fibers are not particularly limited as long as they are mainly composed of SiO2, Al2O3, CaO, MgO, B2O3, Na2O, and K2O and have an average fiber length of 10 μm to 300 μm.

[0039] The average fiber length of the short glass fibers is preferably 20 μm or more, more preferably 30 μm or more, in order to reduce the thermal expansion coefficient, and is preferably 250 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less, in order to improve the dispersibility of the short glass fibers.

[0040] The average fiber diameter of the short glass fibers is not particularly limited, but is preferably 3 μm to 15 μm, more preferably 3 μm to 13 μm, and even more preferably 3.5 μm to 11 μm, in order to reduce the thermal expansion coefficient.

[0041] The average fiber length and fiber diameter of the short glass fibers can be measured using an optical microscope, an electron microscope, or the like.

[0042] Specific examples of the short glass fibers include milled fibers (also called milled fibers), glass wool, and microrods. As the short glass fibers, milled fibers are preferred because they can provide excellent adhesion to copper foil and are inexpensive. These short glass fibers can be used alone or in a suitable mixture of two or more kinds. The glass short fibers may be commercially available products. Examples of commercially available glass short fibers include, but are not limited to, "EFH30-01 (trade name)", "EFH50-01 (trade name)", "EFH30-31 (trade name)", "EFH75-01 (trade name)", "EFH100-31 (trade name)", "EFH150-01 (trade name)", "EFH150-31 (trade name)", "EFK80-31 (trade name)", "EFDE50-01 (trade name)", "EFDE50-31 (trade name)", and "EFDE90-01 (trade name)" manufactured by Central Glass Fiber Co., Ltd.

[0043] The content of the short glass fibers is not particularly limited, but from the viewpoints of thermal expansion coefficient, toughness, and moldability, it is preferably 5 parts by mass to 450 parts by mass, and more preferably 10 parts by mass to 400 parts by mass, per 100 parts by mass of the resin solid content.

[0044] (Cyanate ester compounds, phenol compounds, epoxy compounds, and maleimide compounds) The resin composition in the layer containing the resin composition according to the present embodiment is not particularly limited, but preferably contains at least one compound selected from the group consisting of cyanate ester compounds, phenol compounds, epoxy compounds, and maleimide compounds. When these compounds are contained in the resin composition, the glass transition temperature, chemical resistance, and peel strength of the obtained cured product tend to be improved. These compounds are used alone or in combination of two or more. Among these, the compound preferably contains a cyanate ester compound and / or a phenol compound and an epoxy compound and / or a maleimide compound from the viewpoint of further improving the glass transition temperature, chemical resistance, and peel strength of the obtained cured product. From the same viewpoint, it is more preferable that the compound contains a phenol compound and an epoxy compound and / or a maleimide compound.

[0045] (Cyanate ester compounds) In this embodiment, the term "cyanate ester compound" refers to a compound having two or more cyanate groups (cyanate ester groups) in one molecule, and the term "compound" refers to a concept that includes resin. The cyanate ester compound is not particularly limited as long as it has two or more cyanate groups (cyanate ester groups) in one molecule, but examples thereof include aromatic hydrocarbon compounds containing two or more cyanate groups in one molecule, compounds in which two aromatic rings containing two or more cyanate groups are bonded by a linking group, novolac-type cyanate ester compounds, bisphenol-type cyanate ester compounds, diallyl bisphenol-type cyanate ester compounds (e.g., diallyl bisphenol A-type cyanate ester compounds, diallyl bisphenol E-type cyanate ester compounds, diallyl bisphenol F-type cyanate ester compounds, diallyl bisphenol S-type cyanate ester compounds, etc.), aralkyl-type cyanate ester compounds, and prepolymers of these cyanate esters. These cyanate ester compounds may be used alone or in combination of two or more. Among these, from the viewpoint of further improving the glass transition temperature, chemical resistance, and peel strength of the obtained cured product, aralkyl-type cyanate ester compounds are preferred, and the α-naphthol aralkyl-type cyanate ester compounds and biphenyl aralkyl-type cyanate ester compounds described below are more preferred.

[0046] Examples of aromatic hydrocarbon compounds containing two or more cyanato groups in one molecule include those represented by the formula (I): Ar-(OCN) p (wherein Ar represents any one of a benzene ring, a naphthalene ring, and a biphenyl ring, and p represents an integer of 2 or more). The compound represented by the above formula (I) is not particularly limited, and examples thereof include 1,3-dicyanatobenzene, 1,4-dicyanatobenzene, 1,3,5-tricyanatobenzene, 1,3-dicyanatonaphthalene, 1,4-dicyanatonaphthalene, 1,6-dicyanatonaphthalene, 1,8-dicyanatonaphthalene, 2,6-dicyanatonaphthalene, 2,7-dicyanatonaphthalene, 1,3,6-tricinatonaphthalene, and 4,4'-dicyanatobiphenyl.

[0047] The compound in which two aromatic rings containing two or more cyanato groups are linked by a linking group is not particularly limited, and examples thereof include bis(4-cyanatophenyl) ether, bis(4-cyanatophenyl) thioether, and bis(4-cyanatophenyl) sulfone.

[0048] An example of the novolac-type cyanate ester compound is a compound represented by the following formula (1).

[0049] [ka]

[0050] In the above formula (1), R 1a R each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. 1b each independently represents a hydrogen atom or a methyl group, and preferably represents a hydrogen atom. n represents an integer of 1 to 10, and preferably an integer of 1 to 7.

[0051] The compound represented by the above formula (1) is not particularly limited, but examples thereof include bis(3,5-dimethyl-4-cyanatophenyl)methane, bis(4-cyanatophenyl)methane, and 2,2'-bis(4-cyanatophenyl)propane.

[0052] These cyanate ester compounds may be used alone or in combination of two or more. Among these, the cyanate ester compound is preferably a bisphenol-type cyanate ester compound and / or an aralkyl-type cyanate ester compound, from the viewpoint of obtaining a cured product having better heat resistance and low water absorption.

[0053] (Bisphenol-type cyanate ester compounds) The bisphenol type cyanate ester compound is not particularly limited, but examples thereof include bisphenol A type cyanate ester compounds, bisphenol E type cyanate ester compounds, bisphenol F type cyanate ester compounds, and bisphenol S type cyanate ester compounds.

[0054] The bisphenol-type cyanate ester compound may be a commercially available product, or a preparation prepared by a known method. An example of a commercially available bisphenol-type cyanate ester compound is "CA210 (product name)" manufactured by Mitsubishi Gas Chemical Company, Inc.

[0055] (Aralkyl-type cyanate ester compounds) The aralkyl cyanate ester compound is not particularly limited, but examples thereof include α-naphthol aralkyl cyanate ester compounds and biphenyl aralkyl cyanate ester compounds.

[0056] An example of the α-naphthol aralkyl cyanate ester compound is a compound represented by the following formula (1a).

[0057] [ka]

[0058] In the above formula (1a), R 1c each independently represents a hydrogen atom or a methyl group, and preferably represents a hydrogen atom. n1 represents an integer of 1 to 10, and preferably an integer of 1 to 6.

[0059] An example of the biphenylaralkyl cyanate ester compound is a compound represented by the following formula (1b).

[0060] [ka]

[0061] In the above formula (1b), R1d R each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. 1e each independently represents a hydrogen atom or a methyl group, and preferably represents a hydrogen atom. n2 represents an integer of 1 to 10, and preferably an integer of 1 to 6.

[0062] The aralkyl cyanate ester compound may be a commercially available product or a product synthesized by a known method. Examples of the synthesis method of the aralkyl cyanate ester compound include a method of reacting a phenolic resin (hereinafter also referred to as "corresponding phenolic resin") corresponding to the target aralkyl cyanate ester compound with a cyanogen halide and a basic compound in an inert organic solvent, and a method of reacting a corresponding phenolic resin with a basic compound in an aqueous solution to form a salt and a cyanogen halide at a two-phase interface. In either method, the hydrogen atom of the phenolic hydroxyl group of the corresponding phenolic resin is cyanated to obtain an aralkyl cyanate ester compound. More specifically, for example, the method described in the examples is used.

[0063] The content of the cyanate ester compound is not particularly limited, but is preferably 10 to 45 parts by mass relative to 100 parts by mass of the resin solid content. By having the content within the above range, the storage modulus during heating tends to be a value suitable for suppressing warpage, and warpage of metal foil-clad laminates, printed wiring boards, and multilayer printed wiring boards (e.g., multilayer coreless substrates) tends to be further reduced. From the same viewpoint, the lower limit of the content is more preferably 15 parts by mass, even more preferably 20 parts by mass, and even more preferably 30 parts by mass, and the upper limit of the content is more preferably 40 parts by mass, and even more preferably 35 parts by mass.

[0064] The cyanate equivalent of the cyanate ester compound is preferably 100 g / eq to 500 g / eq, more preferably 400 g / eq or less, and even more preferably 300 g / eq or less. When the cyanate equivalent is within the above range, the rigidity of the obtained cured product is more excellent, and the glass transition temperature and storage modulus during heating tend to be values ​​suitable for suppressing warpage.

[0065] (Phenol compounds) In the present embodiment, the term "phenol compound" refers to a compound having two or more phenolic hydroxyl groups in one molecule, and the term "compound" refers to a concept that includes resins. The phenol compound is not particularly limited as long as it is a compound having two or more phenolic hydroxyl groups in one molecule, and examples thereof include phenols having two or more phenolic hydroxyl groups in one molecule, bisphenols (e.g., bisphenol A, bisphenol E, bisphenol F, and bisphenol S), diallyl bisphenols (e.g., diallyl bisphenol A, diallyl bisphenol E, diallyl bisphenol F, and diallyl bisphenol S), bisphenol-type phenolic resins (e.g., bisphenol A-type resin, bisphenol E-type resin, bisphenol F-type resin, and bisphenol S-type resin), phenol novolac resins (e.g., phenol novolac resin, naphthol novolac resin, and cresol novolac resin), glycidyl ester-type phenolic resins, naphthalene-type phenolic resins, anthracene-type phenolic resins, dicyclopentadiene-type phenolic resins, biphenyl-type phenolic resins, alicyclic phenolic resins, polyol-type phenolic resins, aralkyl-type phenolic resins, and phenol-modified aromatic hydrocarbon formaldehyde resins. These phenolic compounds may be used alone or in combination of two or more. Among these, the phenolic compound is preferably an aralkyl type phenolic resin and / or a phenol-modified aromatic hydrocarbon formaldehyde resin, more preferably a biphenylaralkyl type phenolic resin and / or a phenol-modified xylene resin, from the viewpoint of obtaining a cured product with better heat resistance and low water absorption.

[0066] (Aralkyl-type phenolic resin) An example of the aralkyl phenol resin is a compound represented by the following formula (2a).

[0067] [ka]

[0068] In the above formula (2a), Ar 1 each independently represents a benzene ring or a naphthalene ring. 2 R represents a benzene ring, a naphthalene ring, or a biphenyl ring. 2a each independently represents a hydrogen atom or a methyl group, and m represents an integer of 1 to 50. Each ring may have a substituent other than a hydroxyl group (for example, an alkyl group having 1 to 5 carbon atoms or a phenyl group).

[0069] The compound represented by the above formula (2a) is preferably selected from the group consisting of Ar 1 is a naphthalene ring, and Ar 2 is a benzene ring (also referred to as "naphthol aralkyl type phenol resin"); and in the above (2a), Ar 1 is a benzene ring, and Ar 2 is a biphenyl ring (also referred to as a "biphenyl aralkyl type phenol resin").

[0070] The naphthol aralkyl phenol resin is preferably a compound represented by the following formula (2b).

[0071] [ka]

[0072] In the above formula (2b), R 2a is R in the above formula (2a) 2aand is preferably a hydrogen atom. m is the same as m in the above formula (2a), and is preferably an integer of 1 to 10, and more preferably an integer of 1 to 6.

[0073] The biphenylaralkyl phenol resin is preferably a compound represented by the following formula (2c).

[0074] [ka]

[0075] In the above formula (2c), R 2b each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, and preferably represents a hydrogen atom. m1 represents an integer of 1 to 20, and preferably an integer of 1 to 6.

[0076] The aralkyl type phenol resin may be a commercially available product, or a product synthesized by a known method. Commercially available aralkyl type phenol resins include "SN-495 (trade name)" manufactured by Nippon Steel Chemical Co., Ltd. (naphthol aralkyl type phenol resin represented by formula (2b)), and "KAYAHARD (registered trademark) GPH-65 (trade name)", "KAYAHARD (registered trademark) GPH-78 (trade name)", and "KAYAHARD (registered trademark) GPH-103 (trade name)" manufactured by Nippon Kayaku Co., Ltd. (all biphenyl aralkyl type phenol resins represented by formula (2c)).

[0077] (Phenol modified aromatic hydrocarbon formaldehyde resin) In this specification, the term "phenol-modified aromatic hydrocarbon formaldehyde resin" refers to a resin obtained by heating an aromatic hydrocarbon formaldehyde resin and a phenol in the presence of an acid catalyst (e.g., paratoluenesulfonic acid, oxalic acid, etc.) to cause a condensation reaction (modification condensation reaction).

[0078] The aromatic hydrocarbon formaldehyde resin is not particularly limited, and examples thereof include compounds obtained by condensation reaction of an aromatic hydrocarbon compound (e.g., toluene, ethylbenzene, xylene, mesitylene, pseudocumene, monocyclic aromatic hydrocarbon compounds having 10 or more carbon atoms, and polycyclic aromatic hydrocarbon compounds such as methylnaphthalene) with formaldehyde. Among these, xylene formaldehyde resin obtained by condensation reaction of xylene with formaldehyde is preferable.

[0079] The phenols are not particularly limited, and examples thereof include phenol, cresols, bisphenolpropane, bisphenolmethane, resorcin, pyrocatechol, hydroquinone, para-tertiary butylphenol, bisphenol sulfone, bisphenol ether, and para-phenylphenol, etc. These phenols may be used alone or in combination of two or more.

[0080] The phenol-modified aromatic hydrocarbon formaldehyde resin is preferably a phenol-modified xylene formaldehyde resin obtained by heating a xylene formaldehyde resin and the above-mentioned phenols in the presence of the above-mentioned acid catalyst to cause a condensation reaction, and is more preferably a phenol-modified xylene resin.

[0081] The phenol-modified aromatic hydrocarbon formaldehyde resin may be a commercially available product, or a preparation prepared by a known method may be used. Examples of commercially available phenol-modified aromatic hydrocarbon formaldehyde resins include the Zystar (registered trademark) series manufactured by Fudow Co., Ltd., such as "HP-120 (trade name)", "HP-100 (trade name)", "HP-210 (trade name)", "HP-70 (trade name)", "NP-100 (trade name)", "GP-212 (trade name)", "P-100 (trade name)", "GP-100 (trade name)", "GP-200 (trade name)", and "HP-30 (trade name)". Examples of known methods include the method described in JP 2015-174874 A.

[0082] The content of the phenol compound is not particularly limited, but is preferably 10 to 60 parts by mass relative to 100 parts by mass of the resin solid content. By having the content within the above range, the storage modulus during heating tends to be a value suitable for suppressing warpage, and warpage of metal foil-clad laminates, printed wiring boards, and multilayer printed wiring boards (e.g., multilayer coreless substrates) tends to be further reduced. From the same viewpoint, the lower limit of the content is more preferably 20 parts by mass, more preferably 30 parts by mass, and the upper limit of the content is more preferably 55 parts by mass, more preferably 50 parts by mass, and even more preferably 40 parts by mass.

[0083] The phenol equivalent of the phenol compound (hydroxyl equivalent of phenolic hydroxyl group) is preferably 500g / eq or less, more preferably 400g / eq or less, even more preferably 350g / eq or less, and particularly preferably 300g / eq or less. By having the phenol equivalent within the above range, the rigidity of the obtained cured product is more excellent, and the glass transition temperature and storage modulus during heating tend to be suitable values ​​for suppressing warpage. The lower limit is not particularly limited, but is 100g / eq or more.

[0084] (Epoxy compounds) In the present embodiment, the term "epoxy compound" refers to a compound having two or more epoxy groups in one molecule, and the term "compound" refers to a concept that includes resins. The epoxy compound is not particularly limited as long as it is a compound having two or more epoxy groups in one molecule, and examples thereof include bisphenol type epoxy resins (e.g., bisphenol A type epoxy resins, bisphenol E type epoxy resins, bisphenol F type epoxy resins, and bisphenol S type epoxy resins), diallyl bisphenol type epoxy resins (e.g., diallyl bisphenol A type epoxy resins, diallyl bisphenol E type epoxy resins, diallyl bisphenol F type epoxy resins, and diallyl bisphenol S type epoxy resins), phenol novolac type epoxy resins (e.g., phenol novolac type epoxy resins, bisphenol A novolac type epoxy resins, and cresol novolac type epoxy resins), aralkyl type epoxy resins, biphenyl type epoxy resins containing a biphenyl skeleton, naphthalene type epoxy resins containing a naphthalene skeleton, anthracene type epoxy resins containing an anthracene skeleton, glycidyl ester type epoxy resins, polyol type epoxy resins, isocyanurate ring-containing epoxy resins, dicyclopentadiene type epoxy resins, epoxy resins consisting of bisphenol A type structural units and hydrocarbon-based structural units, and halogen compounds thereof. These epoxy compounds are used alone or in combination of two or more. Among these, from the viewpoint of obtaining a cured product with better heat resistance and low water absorption, it is preferable to use one or more selected from the group consisting of aralkyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, and epoxy resins consisting of bisphenol A type structural units and hydrocarbon-based structural units. In this embodiment, from the viewpoint of obtaining a more suitable value for suppressing warpage during heating, it is preferable to contain two or more types of epoxy compounds, and the two or more types of epoxy compounds contain a naphthalene type epoxy resin and / or an aralkyl type epoxy resin containing a naphthalene skeleton, and more preferably contain a naphthalene type epoxy resin and an aralkyl type epoxy resin. As the aralkyl type epoxy resin, a biphenyl aralkyl type epoxy resin is more preferable.

[0085] (Aralkyl type epoxy resin) An example of the aralkyl type epoxy resin is a compound represented by the following formula (3a).

[0086] [ka]

[0087] In the above formula (3a), Ar 3 each independently represents a benzene ring or a naphthalene ring. 4 R represents a benzene ring, a naphthalene ring, or a biphenyl ring. 3a each independently represents a hydrogen atom or a methyl group. k represents an integer of 1 to 50. Each ring may have a substituent other than a glycidyloxy group (for example, an alkyl group having 1 to 5 carbon atoms or a phenyl group).

[0088] The compound represented by the above formula (3a) is, from the viewpoint of providing a cured product having even better heat resistance and low water absorption, preferably contains Ar 3 is a naphthalene ring, and Ar 4 is a compound having a benzene ring (also called "naphthalene aralkyl type epoxy resin"), and Ar 3 is a benzene ring, and Ar 4 is preferably a compound having a biphenyl ring (also referred to as a "biphenyl aralkyl type epoxy resin"), and more preferably a biphenyl aralkyl type epoxy resin.

[0089] The aralkyl epoxy resin may be a commercially available product, or a product prepared by a known method. Examples of commercially available naphthalene aralkyl epoxy resins include "Epotohto (registered trademark) ESN-155 (trade name)", "Epotohto (registered trademark) ESN-355 (trade name)", "Epotohto (registered trademark) ESN-375 (trade name)", "Epotohto (registered trademark) ESN-475V (trade name)", "Epotohto (registered trademark) ESN-485 (trade name)", and "Epotohto (registered trademark) ESN-175 (trade name)" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; "NC-7000 (trade name)", "NC-7300 (trade name)", and "NC-7300L (trade name)" manufactured by Nippon Kayaku Co., Ltd.; and "HP-5000 (trade name)", "HP-9900 (trade name)", "HP-9540 (trade name)", and "HP-9500 (trade name)" manufactured by DIC Corporation. Commercially available biphenylaralkyl epoxy resins include, for example, "NC-3000 (trade name)", "NC-3000L (trade name)", and "NC-3000FH (trade name)" manufactured by Nippon Kayaku Co., Ltd.

[0090] From the viewpoint of obtaining a cured product having even better heat resistance and low water absorption, the biphenylaralkyl epoxy resin is preferably a compound represented by the following formula (3b).

[0091] [ka]

[0092] In the above formula (3b), ka represents an integer of 1 or more, preferably an integer of 1 to 20, and more preferably an integer of 1 to 6.

[0093] The aralkyl epoxy resin is also preferably a compound represented by the following formula (3c).

[0094] [ka]

[0095] In the above formula (3c), ky represents an integer of 1 to 10. Furthermore, Me represents a methyl group.

[0096] (Naphthalene type epoxy resin) The naphthalene type epoxy resin is not particularly limited, and examples thereof include naphthalene skeleton-containing polyfunctional epoxy resins having a naphthalene skeleton represented by the following formula (3d) and epoxy resins having a naphthalene skeleton (for example, epoxy resins represented by the following formula (3e)) that are epoxy resins other than the above-mentioned naphthalene aralkyl type epoxy resins. Specific examples of the naphthalene type epoxy resins include naphthylene ether type epoxy resins, and naphthylene ether type epoxy resins are preferred from the viewpoint of obtaining a cured product with even better heat resistance and low water absorption.

[0097] [ka]

[0098] In the above formula (3d), Ar 31 each independently represents a benzene ring or a naphthalene ring. 41 R represents a benzene ring, a naphthalene ring, or a biphenyl ring. 31a each independently represents a hydrogen atom or a methyl group; p represents an integer of 0 to 2, and preferably an integer of 0 or 1; kz represents an integer of 1 to 50; each ring may have a substituent other than a glycidyloxy group (for example, an alkyl group, an alkoxy group, or a phenyl group having 1 to 5 carbon atoms); 31 and Ar 41 At least one of these represents a naphthalene ring.

[0099] An example of the compound represented by the above formula (3d) is a compound represented by the following formula (3f).

[0100] [ka]

[0101] In the above formula (3f), kz has the same meaning as kz in the above formula (3d).

[0102] The naphthalene skeleton-containing polyfunctional epoxy resin may be a commercially available product, or a product prepared by a known method. Commercially available naphthalene skeleton-containing polyfunctional epoxy resins include, for example, "HP-9540 (trade name)" and "HP-9500 (trade name)" manufactured by DIC Corporation.

[0103] [ka]

[0104] The epoxy resin represented by the formula (3e) may be a commercially available product or a product prepared by a known method. An example of a commercially available product is "HP-4710 (product name)" manufactured by DIC Corporation.

[0105] (Naphthylene ether type epoxy resin) An example of the naphthylene ether type epoxy resin is a compound represented by the following formula (3g).

[0106] [ka]

[0107] In the above formula (3g), R 3b each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an aralkyl group, a naphthyl group, or a naphthyl group containing a glycidyloxy group. k1 represents an integer of 1 to 10.

[0108] In the compound represented by the above formula (3g), the number of glycidyloxy groups containing an epoxy group in the molecule is preferably 2-6, and more preferably 2-4.

[0109] In the above formula (3g), k1 represents an integer of 0 to 10, and from the viewpoint of more effectively and reliably achieving the effects of this embodiment, k1 preferably represents an integer of 0 to 6, more preferably an integer of 0 to 4, and even more preferably an integer of 2 to 3.

[0110] In the above formula (3g), R 3b From the viewpoint of more effectively and reliably achieving the effects of the present embodiment, it is preferable that each independently represent a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an aralkyl group, or a naphthyl group.

[0111] In addition, when the naphthylene ether type epoxy resin contains a compound represented by the above formula (3g), it may contain multiple types of compounds with the same k1, or multiple types of compounds with different k1. When the naphthylene ether type epoxy resin contains multiple types of compounds with different k1, it is preferable that the naphthylene ether type epoxy resin contains a compound in which k1 in the above formula (3g) is an integer of 0 to 4, and more preferably contains a compound in which k1 is an integer of 2 to 3.

[0112] An example of the compound represented by the above formula (3g) is a compound represented by the following formula (3h).

[0113] [ka]

[0114] The epoxy resin represented by the formula (3h) may be a commercially available product or a product prepared by a known method. Examples of commercially available products include "HP-4032 (trade name)" manufactured by DIC Corporation.

[0115] The naphthylene ether type epoxy resin may be a commercially available product, or a product prepared by a known method. Commercially available naphthylene ether type epoxy resins include, for example, "HP-4032 (trade name)", "HP-6000 (trade name)", "EXA-7300 (trade name)", "EXA-7310 (trade name)", "EXA-7311 (trade name)", "EXA-7311L (trade name)", and "EXA7311-G3 (trade name)" manufactured by DIC Corporation.

[0116] (Dicyclopentadiene type epoxy resin) An example of a dicyclopentadiene type epoxy resin is a compound represented by the following formula (3i).

[0117] [ka]

[0118] In the above formula (3i), R 3c each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. k2 represents an integer of 0 to 10.

[0119] In the above formula (3i), k2 represents an integer of 0 to 10. From the viewpoint of more effectively and reliably achieving the effects of this embodiment, k2 preferably represents an integer of 0 to 6, more preferably an integer of 0 to 2, and even more preferably 0 to 1.

[0120] When the dicyclopentadiene type epoxy resin contains a compound represented by the above formula (3i), it may contain multiple types of compounds with the same k2, or multiple types of compounds with different k2. When the dicyclopentadiene type epoxy resin contains multiple types of compounds with different k2, it is preferable that the dicyclopentadiene type epoxy resin contains a compound represented by the above formula (3i), where k2 is an integer of 0 to 2.

[0121] The dicyclopentadiene type epoxy resin may be a commercially available product, or a preparation prepared by a known method. Commercially available dicyclopentadiene type epoxy resins include "EPICRON (registered trademark) HP-7200L (product name)", "EPICRON (registered trademark) HP-7200 (product name)", "EPICRON (registered trademark) HP-7200H (product name)", and "EPICRON (registered trademark) HP-7000HH (product name)" manufactured by Dainippon Ink and Chemicals, Inc.

[0122] (Epoxy resin consisting of bisphenol A structural units and hydrocarbon-based structural units) An epoxy resin consisting of a bisphenol A structural unit and a hydrocarbon-based structural unit (also referred to as a "specific epoxy resin") has one or more bisphenol A structural units and one or more hydrocarbon-based structural units in the molecule. An example of the specific epoxy resin is a compound represented by the following formula (3j).

[0123] [ka]

[0124] In the above formula (3j), R 1x and R 2x R each independently represents a hydrogen atom or a methyl group. 3x ~R 6x each independently represents a hydrogen atom, a methyl group, a chlorine atom, or a bromine atom. X represents an ethyleneoxyethyl group, a di(ethyleneoxy)ethyl group, a tri(ethyleneoxy)ethyl group, a propyleneoxypropyl group, a di(propyleneoxy)propyl group, a tri(propyleneoxy)propyl group, or an alkylene group having 2 to 15 carbon atoms. k3 represents an integer.

[0125] In the above formula (3j), k3 represents an integer, and from the viewpoint of more effectively and reliably achieving the effects of this embodiment, k3 is preferably an integer from 1 to 10, more preferably an integer from 1 to 6, even more preferably an integer from 1 to 2, and particularly preferably 1.

[0126] In the above formula (3j), X is preferably an ethylene group, from the viewpoint of more effectively and reliably achieving the effects of the present embodiment.

[0127] The specific epoxy resin may be a commercially available product, or a preparation prepared by a known method. Commercially available products of the specific epoxy resin include "EPICLON (registered trademark) EXA-4850-150 (trade name)" and "EPICLON (registered trademark) EXA-4816 (trade name)" manufactured by DIC Corporation.

[0128] The content of the epoxy compound is not particularly limited, but is preferably 10 to 80 parts by mass relative to 100 parts by mass of the resin solid content. By the content being within the above range, the storage modulus during heating tends to be a value suitable for suppressing warping, and the warping of metal foil-clad laminates, printed wiring boards, and multilayer printed wiring boards (for example, multilayer coreless substrates) tends to be further reduced. In addition, by the content being within the above range, the rigidity, heat resistance, and low water absorption of the obtained cured product tend to be further improved. From the same viewpoint, the lower limit of the content is more preferably 20 parts by mass, more preferably 25 parts by mass, even more preferably 30 parts by mass, and particularly preferably 45 parts by mass, and the upper limit of the content is more preferably 75 parts by mass, even more preferably 64 parts by mass, even more preferably 70 parts by mass, and particularly preferably 55 parts by mass.

[0129] The epoxy equivalent of the epoxy compound is preferably 500g / eq or less, more preferably 400g / eq or less, and even more preferably 350g / eq or less. By having the epoxy equivalent within the above range, the rigidity of the obtained cured product is more excellent, and the glass transition temperature and the storage modulus during heating tend to be suitable values ​​for suppressing warpage. The lower limit is not particularly limited, but is preferably 100g / eq or more.

[0130] When the resin composition contains a phenolic compound and / or a cyanic acid ester compound and an epoxy compound, the ratio of the amount of phenolic groups (parts by mass / phenol equivalent) and / or the amount of cyanic acid ester groups (parts by mass / cyanic acid ester equivalent) in the resin composition to the amount of epoxy groups (parts by mass / epoxy equivalent) in the resin composition is preferably 0.5 to 1.5. When the resin composition contains both a phenolic compound and a cyanic acid ester compound, the above ratio is the ratio of the total amount of the amount of phenolic groups and the amount of cyanate groups to the amount of epoxy groups. By having the ratio within the above range, the storage modulus during heating tends to be a value suitable for suppressing warpage. From the same viewpoint, the lower limit of the ratio is preferably 0.5, more preferably 0.6, even more preferably 0.7, and even more preferably 0.9. The upper limit of the ratio is preferably 1.5, more preferably 1.4, even more preferably 1.3, and even more preferably 1.2. When there are multiple types of phenol compounds, the above-mentioned phenol group amount refers to the total value of the phenol group amounts of the respective phenol compounds, when there are multiple types of cyanate ester compounds, the above-mentioned cyanate group amount refers to the total value of the cyanate group amounts of the respective cyanate ester compounds, and when there are multiple types of epoxy compounds, the above-mentioned epoxy group amount refers to the total value of the epoxy group amounts of the respective epoxy compounds.

[0131] (Maleimide compounds) In this embodiment, the term "maleimide compound" refers to a compound having one or more maleimide groups in one molecule, and the term "compound" refers to a concept that includes resin. The maleimide compound is not particularly limited as long as it is a compound having one or more maleimide groups in one molecule, and examples thereof include monomaleimide compounds having one maleimide group in one molecule (e.g., N-phenylmaleimide, N-hydroxyphenylmaleimide, etc.), polymaleimide compounds having two or more maleimide groups in one molecule (e.g., bis(4-maleimidophenyl)methane, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, and polyphenylmethane maleimide compounds), and prepolymers of these maleimide compounds and amine compounds. These maleimide compounds may be used alone or in combination of two or more. Among these, the maleimide compound is preferably a polymaleimide compound from the viewpoint of further improving the heat resistance and glass transition temperature of the resulting cured product.

[0132] Examples of polymaleimide compounds include compounds having multiple maleimide groups bonded to a benzene ring (e.g., phenylene bismaleimides such as m-phenylene bismaleimide, and 4-methyl-1,3-phenylene bismaleimide), compounds having maleimide groups bonded to both ends of a linear or branched alkyl chain (e.g., 1,6-bismaleimide-(2,2,4-trimethyl)hexane), bisphenol A diphenyl ether bismaleimide, and compounds represented by the following formula (4a):

[0133] [ka]

[0134] In the above formula (4a), R 4a and R 5a R each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and preferably represents a hydrogen atom. 4beach independently represents a hydrogen atom or a methyl group, and preferably represents a hydrogen atom. s represents an integer of 1 or more. There is no particular upper limit for s, but it is preferably an integer of 10 or less, and more preferably an integer of 7 or less.

[0135] Examples of the compound represented by the formula (4a) include bis(4-maleimidophenyl)methane, 2,2-bis{4-(4-maleimidophenoxy)-phenyl}propane, and bis(3-ethyl-5-methyl-4-maleimidophenyl)methane. By including the maleimide compound represented by the formula (4a), the thermal expansion coefficient of the obtained cured product tends to be lowered, and the heat resistance and glass transition temperature (Tg) tend to be improved. The maleimide compound may be used alone or in combination of two or more.

[0136] The maleimide compound may be a commercially available product or a preparation prepared by a known method. Commercially available maleimide compounds include "BMI-70 (trade name)" and "BMI-80 (trade name)" manufactured by K.I. Chemical Industry Co., Ltd., and "BMI-2300 (trade name)", "BMI-1000P (trade name)", "BMI-3000 (trade name)", "BMI-4000 (trade name)", "BMI-5100 (trade name)", and "BMI-7000 (trade name)" manufactured by Daiwa Chemical Industry Co., Ltd.

[0137] The content of the maleimide compound is not particularly limited, but is preferably 1 to 45 parts by mass relative to 100 parts by mass of the resin solid content. By having the content within the above range, the obtained cured product tends to have better low water absorption and more reduced warping of a printed wiring board (for example, a thin board such as a multilayer coreless board). From the same viewpoint, the lower limit of the content is more preferably 4 parts by mass, even more preferably 10 parts by mass, and even more preferably 15 parts by mass, and the upper limit of the content is more preferably 40 parts by mass, even more preferably 30 parts by mass, even more preferably 25 parts by mass, and particularly preferably 20 parts by mass.

[0138] (Other resins) The resin composition in the layer containing the resin composition according to the present embodiment is not particularly limited, but may contain other resins. Examples of other resins include alkenyl-substituted nadiimide compounds, oxetane resins, benzoxazine compounds, and compounds having a polymerizable unsaturated group. These resins may be used alone or in combination of two or more.

[0139] (Alkenyl-substituted nadiimide compounds) In the present specification, the term "alkenyl-substituted nadimide compound" refers to a compound having one or more alkenyl-substituted nadimide groups in the molecule. Examples of the alkenyl-substituted nadimide compound include the compound represented by the following formula (5a).

[0140] [ka]

[0141] In the above formula (5a), R 6a R each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. 6b represents an alkylene group having 1 to 6 carbon atoms, a phenylene group, a biphenylene group, a naphthylene group, or a group represented by the following formula (5b) or (5c).

[0142] [ka]

[0143] In the above formula (5b), R 6c represents a methylene group, an isopropylidene group, or a divalent substituent represented by CO, O, S, or SO2.

[0144] [ka]

[0145] In the above formula (5c), R 6deach independently represents an alkylene group having 1 to 4 carbon atoms or a cycloalkylene group having 5 to 8 carbon atoms.

[0146] Further, the alkenyl-substituted nadimide compound also includes compounds represented by the following formula (6) and / or (7).

[0147] [ka]

[0148] [ka]

[0149] The alkenyl-substituted nadiimide compound may be a commercially available product, or a product prepared by a known method may be used. The commercially available alkenyl-substituted nadiimide compound is not particularly limited, but examples thereof include "BANI-M (trade name)" and "BANI-X (trade name)" manufactured by Maruzen Petrochemical Co., Ltd. These alkenyl-substituted nadimide compounds may be used alone or in combination of two or more.

[0150] (Oxetane resin) Examples of oxetane resins include alkyl oxetanes such as oxetane, 2-methyloxetane, 2,2-dimethyloxetane, 3-methyloxetane, and 3,3-dimethyloxetane, 3-methyl-3-methoxymethyloxetane, 3,3'-di(trifluoromethyl)perfluorooxetane, 2-chloromethyloxetane, 3,3-bis(chloromethyl)oxetane, biphenyl-type oxetane, and "OXT-101 (trade name)" and "OXT-121 (trade name)" manufactured by Toagosei Co., Ltd. These oxetane resins may be used alone or in combination of two or more.

[0151] (Benzoxazine compounds) The term "benzoxazine compound" as used herein refers to a compound having two or more dihydrobenzoxazine rings in one molecule. Examples of the benzoxazine compound include "bisphenol F-type benzoxazine BF-BXZ (trade name)" and "bisphenol S-type benzoxazine BS-BXZ (trade name)" manufactured by Konishi Chemical Co., Ltd. These benzoxazine compounds may be used alone or in combination of two or more.

[0152] (Compound having a polymerizable unsaturated group) Examples of compounds having a polymerizable unsaturated group include vinyl compounds such as ethylene, propylene, styrene, divinylbenzene, and divinylbiphenyl; (meth)acrylates of monohydric or polyhydric alcohols such as methyl(meth)acrylate, 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; epoxy (meth)acrylates such as bisphenol A type epoxy (meth)acrylate and bisphenol F type epoxy (meth)acrylate; and benzocyclobutene resins. These compounds having a polymerizable unsaturated group may be used alone or in combination of two or more.

[0153] These other resins are not particularly limited, but are each preferably contained in an amount of 1 part by mass to 30 parts by mass relative to 100 parts by mass of the resin solid content.

[0154] (filling material) The resin composition in the layer containing the resin composition according to the present embodiment is not particularly limited, but preferably contains a filler. Examples of the filler include an inorganic filler and / or an organic filler.

[0155] The inorganic filler is not particularly limited, and examples thereof include silica and silicon compounds (e.g., white carbon, etc.), metal oxides (e.g., alumina, titanium white, zinc oxide, magnesium oxide, zirconium oxide, etc.), metal nitrides (e.g., boron nitride, aggregated boron nitride, silicon nitride, aluminum nitride, etc.), metal sulfates (e.g., barium sulfate, etc.), metal hydroxides (e.g., aluminum hydroxide and heat-treated aluminum hydroxide (e.g., aluminum hydroxide that has been heat-treated to remove some of the water of crystallization), boehmite, etc.), and the like. Examples of inorganic fillers include inorganic fillers such as carbide, ... Among these, from the viewpoint of achieving even greater rigidity in the obtained cured product and further reducing warpage of a printed wiring board (e.g., a thin substrate such as a multilayer coreless substrate), the filler is preferably at least one selected from the group consisting of silica, metal hydroxides, and metal oxides, more preferably contains at least one selected from the group consisting of silica, boehmite, and alumina, and even more preferably is silica.

[0156] Examples of silica include natural silica, fused silica, synthetic silica, amorphous silica, aerosil, and hollow silica. Among these, spherical fused silica is preferable from the viewpoint of obtaining a cured product with better rigidity and further reducing warpage of a printed wiring board (for example, a thin substrate such as a multilayer coreless substrate). Commercially available spherical fused silica includes SC2050-MB (trade name), SC5050-MOB (trade name), SC2500-SQ (trade name), SC4500-SQ (trade name), SC5050-MOB (trade name), SO-C2 (trade name), and SO-C1 (trade name) manufactured by Admatechs Co., Ltd., and SFP-130MC (trade name) manufactured by Denki Kagaku Kogyo Co., Ltd.

[0157] The organic filler is not particularly limited, and examples thereof include rubber powders such as styrene type powder, butadiene type powder, and acrylic type powder; core-shell type rubber powder; silicone type powder, etc. These organic fillers are used alone or in combination of two or more. Among these, silicone type powder is preferable from the viewpoint of further reducing warpage of printed wiring boards (for example, thin boards such as multilayer coreless boards) with better rigidity of the obtained cured product.

[0158] Examples of silicone type powders include silicone resin powder, silicone rubber powder, and silicone composite powder. These silicone type powders may be used alone or in combination of two or more. Among these, silicone composite powders are preferred from the viewpoint of providing a cured product with better rigidity and further reducing warpage of printed wiring boards (e.g., thin boards such as multilayer coreless boards). Examples of silicone composite powders include KMP-600 (trade name), KMP-601 (trade name), KMP-602 (trade name), KMP-605 (trade name), and X-52-7030 (trade name) manufactured by Nissin Chemical Industry Co., Ltd.

[0159] The content of the silicone type powder is not particularly limited, but is preferably 0 to 100 parts by mass relative to 100 parts by mass of the resin solid content. By having the content within the above range, the rigidity of the obtained cured product tends to be further improved, and the warpage of the printed wiring board (for example, a thin board such as a multilayer coreless board) tends to be further reduced. From the same viewpoint, the lower limit of the content is more preferably 10 parts by mass, more preferably 15 parts by mass, and the upper limit of the content is more preferably 50 parts by mass, even more preferably 40 parts by mass, and even more preferably 30 parts by mass.

[0160] The filler of the present embodiment preferably contains an inorganic filler and an organic filler, which tends to further improve the rigidity of the obtained cured product and further reduce the warpage of a printed wiring board (for example, a thin board such as a multilayer coreless board).

[0161] The content of the inorganic filler is not particularly limited, but is preferably 90 to 700 parts by mass relative to 100 parts by mass of the resin solid content. By having the content within the above range, the rigidity of the obtained cured product tends to be further improved, and the warpage of the printed wiring board (for example, a thin board such as a multilayer coreless board) tends to be further reduced, and further, the above formulas (i), (ii), and (iii) can be controlled within the desired range. From the same viewpoint, the lower limit of the content is more preferably 120 parts by mass, more preferably 140 parts by mass, and the upper limit of the content is more preferably 600 parts by mass, more preferably 500 parts by mass, and even more preferably 250 parts by mass.

[0162] When the resin composition contains an organic filler, the content of the organic filler is not particularly limited, but is preferably 1 to 50 parts by mass relative to 100 parts by mass of the resin solid content. By having the content within the above range, the rigidity of the obtained cured product tends to be further improved, and the warpage of a printed wiring board (for example, a thin board such as a multilayer coreless board) tends to be further reduced. From the same viewpoint, the lower limit of the content is more preferably 5 parts by mass, and even more preferably 10 parts by mass, and the upper limit of the content is more preferably 40 parts by mass, and even more preferably 30 parts by mass, and even more preferably 25 parts by mass.

[0163] The total content of the filler is not particularly limited, but is preferably 100 to 700 parts by mass relative to 100 parts by mass of the resin solid content. By having the content within the above range, the rigidity of the obtained cured product tends to be further improved, and the warpage of the printed wiring board (for example, a thin board such as a multilayer coreless board) tends to be further reduced. From the same viewpoint, the lower limit of the content is more preferably 130 parts by mass, and even more preferably 150 parts by mass, and the upper limit of the content is more preferably 600 parts by mass, and even more preferably 500 parts by mass, and even more preferably 250 parts by mass.

[0164] (Silane coupling agent) The resin composition in the layer containing the resin composition according to the present embodiment is not particularly limited, but preferably contains a silane coupling agent.In the present embodiment, by containing a silane coupling agent, the dispersibility of the filler is further improved, and the adhesive strength between the resin composition component in the layer containing the resin composition according to the present embodiment and the substrate described later tends to be further improved.

[0165] The silane coupling agent is not particularly limited, and includes silane coupling agents generally used for surface treatment of inorganic substances, such as aminosilane compounds (e.g., γ-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, etc.), epoxysilane compounds (e.g., γ-glycidoxypropyltrimethoxysilane, etc.), acrylsilane compounds (e.g., γ-acryloxypropyltrimethoxysilane, etc.), cationic silane compounds (e.g., N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride, etc.), and phenylsilane compounds. These silane coupling agents are used alone or in combination of two or more. Among these, the silane coupling agent is preferably an epoxysilane compound. Examples of epoxysilane-based compounds include "KBM-403 (product name)", "KBM-303 (product name)", "KBM-402 (product name)", and "KBE-403 (product name)" manufactured by Shin-Etsu Chemical Co., Ltd.

[0166] The content of the silane coupling agent is not particularly limited, but is preferably 0.1 to 5 parts by mass with respect to 100 parts by mass of the resin solid content.

[0167] (Wetting and dispersing agent) The resin composition in the layer containing the resin composition according to the present embodiment is not particularly limited, but preferably contains a wetting dispersant. In the present embodiment, by containing a wetting dispersant, the dispersibility of the filler is further improved, the rigidity of the obtained cured product is further improved, and the warpage of the metal foil laminate, the printed wiring board, and the multilayer printed wiring board (for example, the multilayer coreless substrate) tends to be further reduced.

[0168] The wetting dispersant may be any known dispersant (dispersion stabilizer) used to disperse a filler, such as DISPERBYK (registered trademark)-110 (trade name), 111 (trade name), 118 (trade name), 180 (trade name), 161 (trade name), W996 (trade name), W9010 (trade name), and W903 (trade name) manufactured by Big Chemie Japan Co., Ltd. These wetting dispersants may be used alone or in combination of two or more kinds.

[0169] The content of the wetting dispersant is not particularly limited, but is preferably 1 to 5 parts by mass relative to 100 parts by mass of the resin solid content. By having the content within the above range, the dispersibility of the filler is further improved, the rigidity of the obtained cured product is further improved, and the warpage of the metal foil-clad laminate, printed wiring board, and multilayer printed wiring board (for example, multilayer coreless substrate) tends to be further reduced. From the same viewpoint, the lower limit of the content is more preferably 1.5 parts by mass, and even more preferably 2 parts by mass.

[0170] (Cure accelerator) The resin composition in the layer containing the resin composition according to the present embodiment is not particularly limited, but preferably contains a curing accelerator. The curing accelerator is not particularly limited, and examples thereof include imidazoles (e.g., triphenylimidazole, etc.), organic peroxides (e.g., benzoyl peroxide, lauroyl peroxide, acetyl peroxide, parachlorobenzoyl peroxide, and di-tert-butyl-di-perphthalate, etc.), azo compounds (e.g., azobisnitrile, etc.), tertiary amines (e.g., N,N-dimethylbenzylamine, N,N-dimethylaniline, N,N-dimethyltoluidine, N,N-dimethylpyridine, 2-N-ethylanilinoethanol, tri-n-butylamine, pyridine, quinoline, N-methylmorpholine, triethanolamine, triethylenediamine, etc.), and the like. Examples of the curing accelerator include tin, tetramethylbutanediamine, and N-methylpiperidine, phenols (e.g., phenol, xylenol, cresol, resorcin, and catechol), organic metal salts (e.g., lead naphthenate, lead stearate, zinc naphthenate, zinc octylate, tin oleate, dibutyltin maleate, manganese naphthenate, cobalt naphthenate, and iron acetylacetonate), and organic metal salts obtained by dissolving these organic metal salts in hydroxyl-containing compounds such as phenol and bisphenol, inorganic metal salts (e.g., tin chloride, zinc chloride, and aluminum chloride), and organic tin compounds (e.g., dioctyltin oxide, other alkyl tins, and alkyl tin oxides). These curing accelerators may be used alone or in combination of two or more. Among these, the curing accelerator is preferably 2,4,5-triphenylimidazole, from the viewpoint of promoting the curing reaction and further improving the glass transition temperature (Tg) of the obtained cured product. The content of the curing accelerator is not particularly limited, but is preferably 0.1 to 5 parts by mass with respect to 100 parts by mass of the resin solid content.

[0171] (Other additives) The resin composition in the layer containing the resin composition according to this embodiment may contain, but is not limited to, various polymer compounds such as thermosetting resins, thermoplastic resins, and their oligomers and elastomers not mentioned so far, as long as the characteristics of this embodiment are not impaired. These are not particularly limited as long as they are commonly used. Examples of additives include, but are not limited to, ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent brighteners, photosensitizers, dyes, pigments, thickeners, flow regulators, lubricants, defoamers, dispersants, leveling agents, gloss agents, and polymerization inhibitors. These other additives may be used alone or in a suitable mixture of two or more. The content of the other additives is not particularly limited, but is usually 0.1 to 10 parts by mass each relative to 100 parts by mass of the resin solid content.

[0172] (solvent) The resin composition in the layer containing the resin composition according to the present embodiment is not particularly limited, but may contain a solvent. By containing a solvent, the resin composition according to the present embodiment tends to have a lower viscosity during preparation of the resin composition, and to have further improved handleability and impregnation into the substrate.

[0173] The solvent is not particularly limited as long as it can dissolve a part or all of the resin content in the resin composition, and examples thereof include ketones (acetone, methyl ethyl ketone, methyl cellosolve, etc.), aromatic hydrocarbons (for example, toluene, xylene, etc.), amides (for example, dimethylformaldehyde, etc.), propylene glycol monomethyl ether and its acetate, etc. These solvents may be used alone or in combination of two or more.

[0174] (Method of producing resin composition) As a method for producing the resin composition in the layer containing the resin composition according to the present embodiment, for example, each component is mixed in a solvent all at once or successively, stirred, and obtained in the form of a varnish dissolved or dispersed in the solvent. At this time, in order to dissolve or disperse each component uniformly, known processes such as stirring, mixing, and kneading are used. The solvent is as described above. For a specific production method, the examples can be referred to.

[0175] (Manufacturing method of resin sheet) The resin sheet of the present embodiment is preferably produced by a method of producing a composite of a layer containing a resin composition in a B stage and a support. Specifically, for example, the resin composition of the present embodiment is in the form of a varnish, and the varnish is applied to a support such as copper foil using a known method such as a bar coater, and then semi-cured by heating for 1 minute to 60 minutes in a dryer at 100°C to 200°C to produce a resin sheet. For specific production methods, the examples can be referred to. The thickness of the layer containing the resin composition is not particularly limited, but is preferably in the range of 1.0 μm to 300 μm.

[0176] [Application] As described above, the resin sheet of this embodiment can sufficiently reduce the warpage of metal foil-clad laminates, printed wiring boards, and multilayer printed wiring boards (e.g., multilayer coreless substrates), and can exhibit excellent rigidity and heat resistance. Therefore, the resin sheet of this embodiment is used, for example, in metal foil-clad laminates, printed wiring boards, and multilayer printed wiring boards. The resin composition of this embodiment is also suitable for use as an insulating layer for printed wiring boards and the like, or as a laminate.

[0177] [Laminate] In this embodiment, the resin sheet of this embodiment may be used for a laminate. The laminate includes one or more layers containing the cured product of the resin composition in the resin sheet of this embodiment, and when multiple layers are included, the layers containing the cured product have a laminated form or a form in which they are laminated via a conductive layer such as a metal foil. By using the resin sheet of this embodiment, the laminate has sufficient reduction in warpage and has excellent rigidity and heat resistance.

[0178] [Metal foil laminate] The metal foil-clad laminate of this embodiment is a resin sheet of this embodiment, which includes a layer containing a cured product of the resin composition and a metal foil arranged on one or both sides of the layer containing the cured product. The metal foil-clad laminate of this embodiment is a resin sheet of this embodiment, which includes one or more layers containing a cured product of the resin composition. When the number of layers containing a cured product is one, the metal foil-clad laminate has a form in which a metal foil is arranged on one or both sides of the layer containing the cured product. When the number of layers containing a cured product is multiple, the metal foil-clad laminate has a form in which a metal foil is arranged on one or both sides of the layer containing the laminated cured product. The metal foil-clad laminate of this embodiment has sufficient warping and excellent rigidity and heat resistance by using the resin sheet of this embodiment.

[0179] The metal foil (conductor layer) may be any metal foil used in various printed wiring board materials, such as copper and aluminum foil, and examples of copper foil include rolled copper foil, electrolytic copper foil, etc. The thickness of the conductor layer is, for example, 1 μm to 70 μm, and preferably 1.5 μm to 35 μm.

[0180] The molding method and molding conditions for the laminate and metal foil-clad laminate are not particularly limited, and general methods and conditions for laminates and multilayer boards for printed wiring boards can be applied. For example, a multi-stage press machine, a multi-stage vacuum press machine, a continuous molding machine, an autoclave molding machine, etc. can be used when molding the laminate or metal foil-clad laminate (lamination molding). In addition, the temperature is 100°C to 300°C, and the pressure is a surface pressure of 2 kgf / cm.2 ~100kgf / cm 2 The heating time is generally in the range of 0.05 to 5 hours. If necessary, post-curing can be performed at a temperature of 150°C to 300°C. For example, when a multi-stage press is used, the temperature is 200°C to 250°C and the pressure is 10 kgf / cm from the viewpoint of sufficiently promoting the curing of the resin composition in the resin sheet. 2 ~40kgf / cm 2 and the heating time is preferably 80 to 130 minutes, the temperature is 215°C to 235°C, and the pressure is 25 kgf / cm 2 ~35kgf / cm 2 and the heating time is more preferably 90 to 120 minutes. In addition, in the resin sheet of the present embodiment, a layer containing the cured product of the resin composition and a separately prepared wiring board for an inner layer are combined and laminated to form a multilayer board.

[0181] [Printed wiring board] The printed wiring board of the present embodiment includes an insulating layer formed of a cured product of the resin composition of the resin sheet of the present embodiment, and a conductor layer formed on the surface of the insulating layer. The printed wiring board of the present embodiment can be formed, for example, by etching the metal foil of the metal foil-clad laminate of the present embodiment into a predetermined wiring pattern to form a conductor layer. The printed wiring board of the present embodiment has sufficient reduction in warping by using the resin sheet of the present embodiment, and has excellent rigidity and heat resistance.

[0182] The printed wiring board of this embodiment can be manufactured, for example, by the following method. First, the metal foil-clad laminate of this embodiment is prepared. The metal foil of the metal foil-clad laminate is etched into a predetermined wiring pattern to create an inner layer substrate having a conductor layer (inner layer circuit). Next, a predetermined number of prepregs or layers containing a resin composition in a resin sheet and a metal foil for an outer layer circuit are laminated in this order on the surface of the conductor layer (interior circuit) of the inner layer substrate, and the laminate is integrally molded (lamination molding) by heating and pressing to obtain a laminate. The method and molding conditions for the laminate molding are the same as those for the laminate and metal foil-clad laminate described above. Next, the laminate is subjected to a hole punching process for through holes and via holes, and a plated metal film for conducting the conductor layer (interior circuit) and the metal foil for the outer layer circuit is formed on the wall surface of the hole thus formed. Next, the metal foil for the outer layer circuit is etched into a predetermined wiring pattern to create an outer layer substrate having a conductor layer (outer layer circuit). In this manner, a printed wiring board is manufactured.

[0183] Here, the prepreg includes a base material and a resin composition impregnated or applied to the base material. The prepreg may be a prepreg obtained by a known method, specifically, the resin composition is impregnated or applied to the base material, and then the base material is semi-cured (B-staged) by heating and drying at 100°C to 200°C. The resin composition is not particularly limited, and examples thereof include known resin compositions used as materials for various printed wiring boards. The base material is not particularly limited, and examples thereof include known base materials used as materials for various printed wiring boards.

[0184] In addition, when a metal foil-clad laminate is not used, a conductor layer that becomes a circuit may be formed on the layer containing the resin composition in the resin sheet to produce a printed wiring board. In this case, a method of electroless plating may be used to form the conductor layer.

[0185] [Multilayer printed wiring board (multilayer coreless board)] In this embodiment, the resin sheet of this embodiment may be used for a multilayer printed wiring board. The multilayer printed wiring board is not particularly limited, and may have, for example, a plurality of insulating layers consisting of a first insulating layer and one or more second insulating layers laminated on one side of the first insulating layer, a first conductor layer arranged between each of the plurality of insulating layers, and a plurality of conductor layers consisting of a second conductor layer arranged on the surface of the outermost layer of the plurality of insulating layers, and the first insulating layer and the second insulating layer are each an insulating layer formed of a cured product of the resin composition in the resin sheet of this embodiment.

[0186] The multilayer printed wiring board may be, for example, a so-called coreless type multilayer printed wiring board (multilayer coreless substrate) in which a second insulating layer is laminated only on one side of a first insulating layer. In this embodiment, an insulating layer formed of a cured product of the resin composition in the resin sheet of this embodiment is used, so that the multilayer printed wiring board has sufficiently reduced warpage and has excellent rigidity and heat resistance. Therefore, in this embodiment, the multilayer coreless substrate can be effectively used as a multilayer coreless substrate for semiconductor packages because it can sufficiently reduce warpage (achieve low warpage). EXAMPLES

[0187] The present invention will be further described below using examples and comparative examples, but the present invention is not limited to these examples in any way.

[0188] [Synthesis Example 1] The α-naphthol aralkyl cyanate ester compound (SN495VCN) was synthesized according to the following procedure. 0.47 moles (OH equivalent) of α-naphthol aralkyl resin (SN495V, OH equivalent: 236g / eq., manufactured by Nippon Steel Chemical Co., Ltd.: the number of repeating units n of naphthol aralkyl includes 1 to 5) was dissolved in 500 ml of chloroform, and 0.7 moles of triethylamine was added to this solution (solution 1). While keeping the temperature at -10°C, the above solution 1 was dropped over 1.5 hours into 300 g of chloroform solution in which 0.93 moles of cyanogen chloride was dissolved, and after the dropwise addition, the mixture was stirred for 30 minutes. Thereafter, a mixed solution of 0.1 moles of triethylamine and 30 g of chloroform was dropped into the reactor, and the reaction was completed by stirring for 30 minutes. The by-product triethylamine hydrochloride was filtered out from the reaction solution, and the obtained filtrate was washed with 500 mL of 0.1 N hydrochloric acid, and then washed with 500 mL of water four times. This was dried over sodium sulfate, then evaporated to dryness at 75° C., and further degassed under reduced pressure at 90° C. to obtain a brown solid α-naphthol aralkyl cyanate compound represented by the above formula (1a) (R 1c are all hydrogen atoms, and the number of repeating units n1 is 1 to 5.) was obtained. The obtained α-naphthol aralkyl cyanate ester compound was analyzed by infrared absorption spectroscopy, and found to have a peak at 2264 cm -1 Absorption of cyanate ester groups was confirmed in the vicinity.

[0189] [Example 1] Biphenylaralkyl-type phenolic resin (KAYAHARD (registered trademark) GPH-103 (trade name), manufactured by Nippon Kayaku Co., Ltd., hydroxyl group equivalent: 231 g / eq., represented by the above formula (2c), in which R 2bare all hydrogen atoms), 36 parts by mass of biphenyl aralkyl type epoxy resin (NC-3000FH (trade name), epoxy equivalent: 320 g / eq., manufactured by Nippon Kayaku Co., Ltd., represented by the above formula (3b)), 39 parts by mass of aralkyl type epoxy resin (HP-9900 (trade name), epoxy equivalent: 274 g / eq., manufactured by DIC Corporation, represented by the above formula (3c)), 7 parts by mass of bis(3-ethyl-5-methyl-4-maleimidophenyl)methane (BMI-70 (trade name), manufactured by K.I. Kasei Co., Ltd.), 18 parts by mass of slurry silica 1 (SC2050-MB (trade name), average particle size 0.7 μm, manufactured by Admatechs Co., Ltd.), 100 parts by mass of slurry silica 2 (SC5050-MB (trade name), average particle size 0.7 μm, manufactured by Admatechs Co., Ltd.), OB (trade name), average particle size 1.5 μm, manufactured by Admatechs Co., Ltd.) 100 parts by mass, silicone composite powder (KMP-600 (trade name), manufactured by Nissin Chemical Co., Ltd.) 20 parts by mass, wetting dispersant 1 (DISPERBYK (registered trademark) -161 (trade name), manufactured by BYK Japan Co., Ltd.) 1 part by mass, wetting dispersant 2 (DISPERBYK (registered trademark) -111 (trade name), manufactured by BYK Japan Co., Ltd.) 2 parts by mass, silane coupling agent (KBM-403 (trade name), manufactured by Shin-Etsu Chemical Co., Ltd.) 1 part by mass, 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.) 0.5 parts by mass were blended (mixed), and then diluted with methyl ethyl ketone to obtain a varnish (resin composition). This varnish (resin composition) was diluted with methyl ethyl ketone and applied to the matte side of a copper foil (3EC-M2S-VLP (product name), manufactured by Mitsui Mining & Smelting Co., Ltd.) measuring 350 mm × 250 mm × 12 μm in thickness using a bar coater, and then heated and dried at 130°C for 5 minutes to obtain a copper foil with a B-stage layer containing the resin composition (minimum melt viscosity: approximately 1500 Pa s) having a layer containing the resin composition of 20 μm in thickness.

[0190] [Example 2] The amount of biphenyl aralkyl type epoxy resin (NC-3000-FH (trade name)) was changed from 39 parts by mass to 19 parts by mass, and naphthylene ether type epoxy resin (HP-6000 (trade name), epoxy equivalent: 250 g / eq., manufactured by DIC Corporation, represented by the above formula (3g), R in the formula was 3bA copper foil with a B-staged layer containing a resin composition (minimum melt viscosity: approximately 1000 Pa s) having a thickness of 20 μm and containing the resin composition was obtained in the same manner as in Example 1, except that 20 parts by mass of a compound having a B-staged layer containing a resin composition (minimum melt viscosity: approximately 1000 Pa s) was added (wherein all of the compound represented by formula (I) are hydrogen atoms, and the number of repeating units k1 is 2).

[0191] [Example 3] Biphenylaralkyl type phenolic resin (KAYAHARD (registered trademark) GPH-103 (trade name)) 20 parts by mass, phenol-modified xylene resin (ZYSTAR (registered trademark) GP-100 (trade name), Fudow Co., Ltd., phenol equivalent: 194 g / eq.) 15 parts by mass, biphenylaralkyl type epoxy resin (NC-3000-FH (trade name)) 34 parts by mass, naphthalenearalkyl type epoxy resin (HP-9900 (trade name)) 5 parts by mass, dicyclopentadiene type epoxy resin (EPICRON (registered trademark) HP-7200L (trade name), epoxy equivalent: 249 g / eq., DIC Corporation, represented by the above formula (3i), R in the formula 3c are all hydrogen atoms), 7 parts by mass of a polyphenylmethane maleimide compound (BMI-2300 (trade name), manufactured by Daiwa Kasei Kogyo Co., Ltd.), 19 parts by mass of slurry silica 1 (SC2050-MB (trade name), average particle size 0.7 μm), 100 parts by mass of slurry silica 2 (SC5050-MOB (trade name), average particle size 1.5 μm), 20 parts by mass of silicone composite powder (KMP-600 (trade name)), 1 part by mass of wetting dispersant 1 (DISPERBYK (registered trademark)-161 (trade name)), 2 parts by mass of wetting dispersant 2 (DISPERBYK (registered trademark)-111 (trade name)), 1 part by mass of a silane coupling agent (KBM-403 (trade name)), and 0.5 parts by mass of 2,4,5-triphenylimidazole were mixed and then diluted with methyl ethyl ketone to obtain a varnish (resin composition). This varnish (resin composition) was diluted with methyl ethyl ketone and applied to the matte side of a copper foil (3EC-M2S-VLP (product name), manufactured by Mitsui Mining & Smelting Co., Ltd.) measuring 350 mm × 250 mm × 12 μm in thickness using a bar coater, and then heated and dried at 130°C for 5 minutes to obtain a copper foil with a layer containing the resin composition in a B-stage (minimum melt viscosity: approximately 1000 Pa s) and with a thickness of 20 μm.

[0192] [Example 4] The mixture was mixed with 34 parts by mass of an α-naphthol aralkyl type cyanate ester compound (cyanate equivalent: 261 g / eq) synthesized by the method described in Synthesis Example 1, 15 parts by mass of a biphenyl aralkyl type epoxy resin (NC-3000-FH (trade name)), 5 parts by mass of a naphthylene ether type epoxy resin (HP-6000 (trade name)), 26 parts by mass of a dicyclopentadiene type epoxy resin (EPICRON (registered trademark) HP-7200L (trade name)), and an epoxy resin consisting of a bisphenol A type structural unit and a hydrocarbon-based structural unit (EPICLON (registered trademark)). EXA-4816 (trade name), manufactured by DIC Corporation, epoxy equivalent: 403 g / eq., represented by the above formula (3j)) 15 parts by mass, bis(3-ethyl-5-methyl-maleimidophenyl)methane (BMI-70 (trade name)) 5 parts by mass, slurry silica 1 (SC2050-MB (trade name), average particle size 0.7 μm) 100 parts by mass, slurry silica 2 (SC5050-MOB (trade name), average particle size 1.5 μm) 100 parts by mass, silicone 20 parts by mass of composite powder (KMP-600 (trade name)), 1 part by mass of wetting dispersant 1 (DISPERBYK (registered trademark)-161 (trade name)), 2 parts by mass of wetting dispersant 2 (DISPERBYK (registered trademark)-111 (trade name)), 1 part by mass of silane coupling agent (KBM-403 (trade name)), and 0.5 parts by mass of 2,4,5-triphenylimidazole were mixed and then diluted with methyl ethyl ketone to obtain a varnish (resin composition). This varnish (resin composition) was diluted with methyl ethyl ketone and applied to the matte side of a copper foil (3EC-M2S-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd.) measuring 350 mm x 250 mm x 12 μm in thickness using a bar coater, and dried by heating at 130 ° C. for 5 minutes to obtain a copper foil with a layer containing the resin composition and a B-stage (minimum melt viscosity: about 1500 Pa s) containing the resin composition, with a thickness of 20 μm.

[0193] [Comparative Example 1] 40 parts by mass of an α-naphthol aralkyl type cyanate ester compound (cyanate equivalent: 261 g / eq) synthesized by the method described in Synthesis Example 1, 20 parts by mass of a polyphenylmethane maleimide compound (BMI-2300 (trade name)), 40 parts by mass of a naphthylene ether type epoxy resin (HP-6000 (trade name)), 100 parts by mass of slurry silica 1 (SC2050-MB (trade name), average particle size 0.7 μm), 100 parts by mass of slurry silica 2 (SC5050-MOB (trade name), average particle size 100 parts by mass of 1.5 μm silicone composite powder (KMP-600 (trade name)), 20 parts by mass of wetting dispersant 1 (DISPERBYK (registered trademark)-161 (trade name)), 2 parts by mass of wetting dispersant 2 (DISPERBYK (registered trademark)-111 (trade name)), 1 part by mass of silane coupling agent (KBM-403 (trade name)), and 0.5 parts by mass of 2,4,5-triphenylimidazole were mixed and then diluted with methyl ethyl ketone to obtain a varnish (resin composition). This varnish (resin composition) was diluted with methyl ethyl ketone and applied to the matte side of a 350 mm × 250 mm × 12 μm thick copper foil (3EC-M2S-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd.) using a bar coater, and heated and dried at 130 ° C. for 5 minutes to obtain a copper foil with a B-stage layer containing the resin composition having a thickness of 20 μm.

[0194] [Comparative Example 2] Biphenylaralkyl type phenol compound (KAYAHARD (registered trademark) GPH-103 (trade name)) 20 parts by mass, phenol-modified xylene compound (ZYSTAR (registered trademark) GP-100 (trade name)) 15 parts by mass, biphenylaralkyl type epoxy resin (NC-3000-FH (trade name)) 30 parts by mass, dicyclopentadiene type epoxy resin (EPICRON (registered trademark) HP-7200L (trade name)) 20 parts by mass, bis(3-ethyl-5-methyl-maleimidophenyl)methane (BMI-70 (trade name)) 15 parts by mass, slurry silica 1 (SC2050-MB (trade name), average particle size 0.7 μm) 100 parts by mass, slurry silica 2 (SC5050-MOB (trade name), average particle size 1.5 μm) 100 parts by mass, silicone composite powder (KMP-600 (trade name)) 20 parts by mass, wetting dispersant 1 (DISPERBYK (registered trademark) -161 (trade name)) 1 part by mass, wetting dispersant 2 (DISPERBYK (registered trademark) -111 (trade name)) 2 parts by mass, silane coupling agent (KBM-403 (trade name)) 1 part by mass, 2,4,5-triphenylimidazole 0.5 parts by mass were mixed and then diluted with methyl ethyl ketone to obtain a varnish (resin composition). This varnish (resin composition) was diluted with methyl ethyl ketone and applied to the matte side of a 350 mm x 250 mm x 12 μm thick copper foil (3EC-M2S-VLP (product name), manufactured by Mitsui Mining & Smelting Co., Ltd.) using a bar coater, and then heated and dried at 130°C for 5 minutes to obtain a copper foil with a B-stage layer containing the resin composition, the layer containing the resin composition being 20 μm thick.

[0195] [Comparative Example 3] 5 parts by mass of the α-naphthol aralkyl type cyanate ester compound synthesized by the method described in Synthesis Example 1, 50 parts by mass of a polyphenylmethane maleimide compound (BMI-2300 (trade name)), 10 parts by mass of a biphenyl aralkyl type epoxy resin (NC-3000-FH (trade name)), 35 parts by mass of an alkenyl-substituted nadiimide compound (BANI-M (trade name), manufactured by Maruzen Petrochemical Co., Ltd.), 100 parts by mass of slurry silica 1 (SC2050-MB (trade name), average particle size 0.7 μm), 100 parts by mass of slurry silica 2 (SC505 A varnish (resin composition) was obtained by mixing 100 parts by mass of 0-MOB (trade name), average particle size 1.5 μm, 20 parts by mass of silicone composite powder (KMP-600 (trade name)), 1 part by mass of wetting dispersant 1 (DISPERBYK (registered trademark)-161 (trade name)), 2 parts by mass of wetting dispersant 2 (DISPERBYK (registered trademark)-111 (trade name)), 1 part by mass of silane coupling agent (KBM-403 (trade name)), and 0.5 parts by mass of 2,4,5-triphenylimidazole, and then diluting with methyl ethyl ketone. This varnish (resin composition) was diluted with methyl ethyl ketone and applied to the matte side of a 350 mm x 250 mm x 12 μm thick copper foil (3EC-M2S-VLP (product name), manufactured by Mitsui Mining & Smelting Co., Ltd.) using a bar coater, and then heated and dried at 130°C for 5 minutes to obtain a copper foil with a B-stage layer containing the resin composition, the layer containing the resin composition being 20 μm thick.

[0196] [Comparative Example 4] 30 parts by mass of the α-naphthol aralkyl type cyanate ester compound synthesized by the method described in Synthesis Example 1, 35 parts by mass of a polyphenylmethane maleimide compound (BMI-2300 (trade name)), 5 parts by mass of a naphthylene ether type epoxy resin (HP-6000 (trade name)), 30 parts by mass of an acrylic acid ester rubber compound (Teisan Resin (registered trademark) SG-P3 (trade name, manufactured by Nagase ChemteX Corporation), 30 parts by mass of slurry silica 1 (SC2050-MB (trade name), average particle size 0 100 parts by weight of silica gel 2 (SC5050-MOB (trade name)), 100 parts by weight of wetting agent 1 (DISPERBYK (registered trademark)-161 (trade name)), 2 parts by weight of wetting agent 2 (DISPERBYK (registered trademark)-111 (trade name)), 1 part by weight of silane coupling agent (KBM-403 (trade name)), and 0.5 parts by weight of 2,4,5-triphenylimidazole were mixed and then diluted with methyl ethyl ketone to obtain a varnish (resin composition). This varnish (resin composition) was diluted with methyl ethyl ketone and applied to the matte side of a 350 mm x 250 mm x 12 μm thick copper foil (3EC-M2S-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd.) using a bar coater, and heated and dried at 130 ° C. for 5 minutes to obtain a copper foil with a B-stage layer containing the resin composition, the layer containing the resin composition being 20 μm thick.

[0197] [Comparative Example 5] A copper foil with a B-stage layer containing a resin composition having a thickness of 20 μm was obtained in the same manner as in Comparative Example 4, except that slurry silica 2 (SC-5050MOB (trade name)) and wetting dispersant 2 (DISPERBYK (registered trademark)-111 (trade name)) were not used and the amount of slurry silica 1 (SC-2050MB (trade name)) was changed from 100 parts by mass to 75 parts by mass.

[0198] [Physical property measurement and evaluation] Using the B-staged layered copper foils containing the resin compositions obtained in Examples 1 to 4 and Comparative Examples 1 to 5, samples for measuring and evaluating physical properties were prepared according to the procedures shown in the following items, and mechanical properties (storage modulus at 40°C, 170°C, and 230°C), glass transition temperature (Tg), warpage, and heat resistance were measured and evaluated. The results of the Examples and Comparative Examples are summarized in Table 1.

[0199] (Mechanical properties) First, the central portion of a copper foil-clad laminate (HL832NS (trade name) T / T 0.8mmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was cut out to a size of 100mm x 150mm, and the copper foil-clad laminate was placed on top of a copper foil (3EC-M2S-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 12μm). Next, 25g of the resin content in the layer containing the resin composition in the layered copper foil obtained in Example 1 was placed in the cut-out portion, and copper foil (3EC-M2S-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 12μm) was placed on the copper foil-clad laminate so as to cover the resin content, and the resin content was sandwiched between the front and back copper foils. Thereafter, a pressure of 30kgf / cm was applied. 2 Lamination molding (thermal curing) was performed at a temperature of 230°C for 100 minutes to obtain a laminate having copper foil, an insulating layer with a cured resin, and copper foil. The thickness of the insulating layer was about 800 μm. After cutting the obtained laminate into a size of 13 mm x 35 mm with a dicing saw (after downsizing) so as to include the insulating layer, the copper foil on both sides of the laminate was removed by etching to obtain a measurement sample. By performing this series of operations in the same manner, three measurement samples were produced. Dynamic viscoelasticity measurements (DMA) were performed on each of these three measurement samples using a dynamic viscoelasticity analyzer (manufactured by TA Instruments) in accordance with JIS C6481 to measure mechanical properties (storage modulus E' at 40°C, 170°C, 230°C, and 260°C). Using the storage modulus E' obtained from each measurement sample, the arithmetic mean value of the storage modulus E' at each temperature was calculated, and these values ​​were defined as the storage modulus E'. For the copper foils with the B-staged layers containing the resin compositions obtained in Examples 2 to 4 and Comparative Examples 1 to 5, the mechanical properties were measured in the same manner, and the storage modulus E' of each was calculated.

[0200] (Glass transition temperature (Tg)) First, the central portion of a copper foil-clad laminate (HL832NS (trade name) T / T 0.8mmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was cut out to a size of 100mm x 150mm, and the copper foil-clad laminate was placed on top of a copper foil (3EC-M2S-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 12μm). Next, 25g of the resin content in the layer containing the resin composition in the layered copper foil obtained in Example 1 was placed in the cut-out portion, and copper foil (3EC-M2S-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 12μm) was placed on the copper foil-clad laminate so as to cover the resin content, and the resin content was sandwiched between the front and back copper foils. Thereafter, a pressure of 30kgf / cm was applied. 2 Lamination molding (thermal curing) was performed at a temperature of 230°C for 100 minutes to obtain a laminate having copper foil, an insulating layer with a cured resin, and copper foil. The thickness of the insulating layer was about 800 μm. After cutting the obtained laminate into a size of 13 mm x 35 mm with a dicing saw (after downsizing) so as to include the insulating layer, the copper foil on both sides of the laminate was removed by etching to obtain a measurement sample. By performing this series of operations in the same manner, three measurement samples were produced. The glass transition temperature (Tg) of each of these three measurement samples was measured by the DMA method using a dynamic viscoelasticity analyzer (manufactured by TA Instruments) in accordance with JIS C 6481. The arithmetic mean value was calculated using the glass transition temperatures obtained from each measurement sample, and this value was taken as the glass transition temperature. For the copper foils with the B-staged layers containing the resin compositions obtained in Examples 2 to 4 and Comparative Examples 1 to 5, the glass transition temperatures were similarly measured and calculated.

[0201] (Warpage: Bimetal method) First, two copper foils with a B-stage layer containing a resin composition were prepared. Using one of these layered copper foils, a copper foil (3EC-M2S-VLP (product name), manufactured by Mitsui Mining & Smelting Co., Ltd., thickness 12 μm) was placed on the surface of the layer containing the resin composition in the layered copper foil, and a pressure of 30 kgf / cm was applied. 2 and laminate molding (thermosetting) at a temperature of 220°C for 120 minutes to obtain a copper foil-clad laminate 1 having copper foil on both sides of a cured insulating layer. The insulating layer had a thickness of about 20 µm. Next, only one side of the copper foil on both sides of the copper foil-clad laminate 1 was removed by etching to obtain a copper foil-clad laminate 2. Next, the surface of the layer containing the resin composition of another layered copper foil was placed on the surface of the insulating layer of the copper foil-clad laminate 2, and a pressure of 30 kgf / cm was applied. 2 , and laminated molding (thermosetting) at a temperature of 220°C for 120 minutes to obtain a copper foil-clad laminate 3. The total thickness of the two insulating layers was about 40 μm. In the copper foil-clad laminate 3, the copper foil was removed from both sides by etching to obtain a laminate. Then, a rectangular plate of 20 mm x 200 mm was cut out from the obtained laminate. Then, one end of the short side of the rectangular plate was attached to a surface perpendicular to the plane with a magnet, and a straightedge was placed parallel to the plane to measure the maximum distance between the perpendicular surface and the rectangular plate, and this value was taken as the "warpage amount." When the warpage amount was less than 4 mm, it was evaluated as "AA", and otherwise as "CC". The copper foils with the B-staged layers containing the resin compositions obtained in Examples 2 to 4 and Comparative Examples 1 to 5 were also similarly measured and evaluated for the amount of warpage.

[0202] (heat resistance) First, a copper foil-clad laminate 1 (HL832NS (product name) T / T 0.8 mmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was prepared. The copper foil surfaces on both sides of this copper foil-clad laminate 1 were etched to about 1 μm to 3 μm (inner layer roughening treatment, CZ-8100 (product name), manufactured by MEC Co., Ltd.), and the surface of the layer containing the resin composition in the layered copper foil obtained in Example 1 was placed on each of the copper foil surfaces on both sides, and a pressure of 30 kgf / cm was applied. 2, and laminated molding (thermal curing) was performed at a temperature of 230 ° C for 100 minutes to obtain a copper foil-clad laminate 2. Next, the copper foil-clad laminate 2 was cut (downsized) to a size of 50 mm × 50 mm with a dicing saw to obtain a measurement sample. The obtained sample was left in a thermostatic bath at 120 ° C for 1 hour, and then immersed in a solder bath at 260 ° C for 30 seconds to evaluate heat resistance. After 30 seconds, the presence or absence of delamination between the copper foil on the surface of the copper foil-clad laminate 1 and the cured layer obtained by curing the layer containing the resin composition was confirmed for each of both sides of the copper foil-clad laminate 1. When delamination did not occur on both sides, it was designated as "AA", and when delamination occurred on either side, it was designated as "CC". The heat resistance of each of the copper foils with the B-staged layers containing the resin compositions obtained in Examples 2 to 4 and Comparative Examples 1 to 5 was measured and evaluated in the same manner.

[0203] [Table 1]

[0204] This application is based on a Japanese patent application (Patent Application No. 2019-118888) filed on June 26, 2019, the contents of which are incorporated herein by reference. [Industrial Applicability]

[0205] The resin sheet of the present invention can be used, for example, in metal foil-clad laminates, printed wiring boards, and multilayer printed wiring boards.

Claims

1. A support; A layer made of a resin composition that satisfies the relationships represented by the following formulas (i), (ii), and (iii) and is disposed on a surface of the support; Equipped with the resin composition comprises a phenol compound, an epoxy compound, a maleimide compound, an inorganic filler, and an organic filler; the phenol compound includes at least one selected from the group consisting of a biphenyl aralkyl phenol resin and a phenol-modified xylene resin, and the content of the phenol compound is 30 to 40 parts by mass relative to 100 parts by mass of a resin solid content; the epoxy compound includes a naphthalene aralkyl type epoxy resin and a biphenyl aralkyl type epoxy resin, and the content of the epoxy compound is 45 to 55 parts by mass relative to 100 parts by mass of a resin solid content; the maleimide compound includes a compound represented by the following formula (4a), and the content of the maleimide compound is 15 to 25 parts by mass relative to 100 parts by mass of a resin solid content, The inorganic filler contains silica, and the content of the inorganic filler is 140 to 250 parts by mass relative to 100 parts by mass of a resin solid content; The resin sheet, wherein the organic filler includes a silicone type powder, and the content of the organic filler is 10 to 30 parts by mass per 100 parts by mass of resin solids. 0.15≦b / a≦0.60...(i) 0.015≦c / a≦0.07...(ii) 3≦a≦10...(iii) (In formulas (i), (ii), and (iii), a, b, and c respectively represent the storage moduli (unit: GPa) of the cured product of the resin composition at 40° C., 170° C., and 230° C.) 【Chemistry 1】 (In formula (4a), R 4a and R 5a each independently represent a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 4b each independently represent a hydrogen atom or a methyl group, and s represents an integer of 1 or more and 10 or less).

2. A resin sheet as described in claim 1, wherein the resin composition further contains a naphthylene ether type epoxy resin.

3. A resin sheet as described in claim 1, wherein the resin composition further contains a dicyclopentadiene type epoxy resin.

4. A support, A layer made of a resin composition that satisfies the relationships represented by the following formulas (i), (ii), and (iii) and is disposed on a surface of the support; Equipped with the resin composition comprises a cyanate ester compound, an epoxy compound, a maleimide compound, an inorganic filler, and an organic filler; the cyanate ester compound includes an α-naphthol aralkyl cyanate ester compound, and the content of the cyanate ester compound is 30 to 40 parts by mass relative to 100 parts by mass of a resin solid content; the epoxy compound includes a compound represented by the following formula (3j), a biphenyl aralkyl type epoxy resin, a naphthylene ether type epoxy resin, and a dicyclopentadiene type epoxy resin, and the content of the epoxy compound is 45 to 64 parts by mass relative to 100 parts by mass of a resin solid content, the maleimide compound includes a compound represented by the following formula (4a), and the content of the maleimide compound is 4 to 20 parts by mass relative to 100 parts by mass of a resin solid content, The inorganic filler contains silica, and the content of the inorganic filler is 140 to 250 parts by mass relative to 100 parts by mass of a resin solid content; The resin sheet, wherein the organic filler includes a silicone type powder, and the content of the organic filler is 10 to 30 parts by mass per 100 parts by mass of resin solids. 0.15≦b / a≦0.60...(i) 0.015≦c / a≦0.07...(ii) 3≦a≦10...(iii) (In formulas (i), (ii), and (iii), a, b, and c respectively represent the storage moduli (unit: GPa) of the cured product of the resin composition at 40° C., 170° C., and 230° C.) 【Chemistry 2】 (In formula (3j), R 1x and R 2x each independently represent a hydrogen atom or a methyl group, R 3x to R 6x each independently represent a hydrogen atom, a methyl group, a chlorine atom, or a bromine atom, X represents an ethyleneoxyethyl group, a di(ethyleneoxy)ethyl group, a tri(ethyleneoxy)ethyl group, a propyleneoxypropyl group, a di(propyleneoxy)propyl group, a tri(propyleneoxy)propyl group, or an alkylene group having 2 to 15 carbon atoms, and k3 represents an integer of 1 to 10.) 【Chemistry 3】 (In formula (4a), R 4a and R 5a each independently represent a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 4b each independently represent a hydrogen atom or a methyl group, and s represents an integer of 1 or more and 10 or less).

5. The resin composition further comprises a silane coupling agent, a wetting and dispersing agent, and a curing accelerator, The content of the silane coupling agent is 0.1 to 5 parts by mass relative to 100 parts by mass of the resin solid content, The content of the wetting and dispersing agent is 1 to 5 parts by mass relative to 100 parts by mass of the resin solid content, The resin sheet according to any one of claims 1 to 4, wherein the content of the curing accelerator is 0.1 to 5 parts by mass per 100 parts by mass of resin solids.

6. The resin sheet according to any one of claims 1 to 5, wherein the resin composition further satisfies the relationship represented by the following formula (iv): 175≦Tg≦215…(iv) (In formula (iv), Tg represents the glass transition temperature (unit: ° C.) of the cured product of the resin composition.)

7. The resin sheet according to any one of claims 1 to 6, wherein the resin composition further satisfies the relationship represented by the following formula (v): 0.015≦d / a≦0.08…(v) (In formula (v), d represents the storage modulus (unit: GPa) at 260° C. of the cured product of the resin composition, and a has the same meaning as defined above.)

8. The resin sheet according to any one of claims 1 to 7, wherein the resin composition contains an elastomer component.

9. The resin sheet according to any one of claims 1 to 8, wherein the support is a resin sheet or a metal foil.

10. A layer comprising a cured product of the resin composition according to claim 1; A metal foil disposed on one or both sides of the layer containing the cured product; A metal foil-clad laminate comprising:

11. An insulating layer comprising a cured product of the resin composition according to claim 1; A conductor layer disposed on a surface of the insulating layer; A printed wiring board comprising:

12. A layer comprising a cured product of the resin composition according to claim 4; A metal foil disposed on one or both sides of the layer containing the cured product; A metal foil-clad laminate comprising:

13. An insulating layer comprising a cured product of the resin composition according to claim 4; A conductor layer disposed on a surface of the insulating layer; A printed wiring board comprising:

Citation Information

Patent Citations

  • Nonwoven fabric base material for printed circuit board and prepreg using the same

    JP1998072752A

  • Resin composition, adhesive-attached film for semiconductor device, metal foil-attached laminate film and semiconductor device using the same

    JP2003113320A

  • Multilayer wiring board

    JP2004303887A

  • Resin composition

    JP2015017247A

  • Metal-clad laminate, printed wiring board, and semiconductor device

    JP2015089622A