Laminate and manufacturing method thereof

A laminate with a nickel-containing plating and gold plating layer, sealed with a fluoride passive film, addresses the insufficient corrosion resistance of semiconductor equipment components by effectively sealing pinholes and enhancing resistance to corrosive gases.

JP7593324B2Active Publication Date: 2024-12-03RESONAC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021550540
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-10
Filing Date
2020-09-11
Publication Date
2024-12-03
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

Conventional methods for improving corrosion resistance in semiconductor manufacturing equipment components, such as those using nickel-phosphorous alloy plating, are insufficient against corrosive gases like fluorine and hydrogen chloride, leading to corrosion from hydrolysis products and pinhole-induced corrosion.

Method used

A laminate structure comprising a metal base material coated with a nickel-containing plating layer and a gold plating layer, sealed with a fluoride passive film of at least 8 nm thickness, formed through specific electroless plating processes and fluorination treatment.

Benefits of technology

The laminate exhibits enhanced corrosion resistance, particularly against acids, by sealing pinholes and preventing direct contact of corrosive gases with the base material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593324000002
    Figure 0007593324000002
  • Figure 0007593324000001
    Figure 0007593324000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a metal material which is applicable to a constituent member of an apparatus for producing a semiconductor, while having excellent corrosion resistance. A multilayer body according to the present invention comprises a metal base material, a nickel-containing plating film layer that is formed on the metal base material, and a gold plating film layer that is formed on the nickel-containing plating film layer; and pinholes in the gold plating film layer are sealed with a fluoride passivation film that has a thickness of 8 nm or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate and a manufacturing method thereof, and more particularly to a laminate suitable as a component of a semiconductor manufacturing device or the like and a manufacturing method thereof. [Background technology]

[0002] Conventionally, in the semiconductor manufacturing process, highly reactive and corrosive special gases (hereinafter also referred to as "corrosive gases") containing halogens such as fluorine, hydrogen chloride, boron trichloride, nitrogen trifluoride, chlorine trifluoride, and hydrogen bromide have been used in the dry etching process and cleaning of manufacturing equipment.

[0003] However, when the corrosive gas reacts with moisture in the atmosphere and undergoes hydrolysis, products such as hydrogen fluoride, oxalic acid, and hydrogen chloride are generated, which are problematic because they easily corrode the metal surfaces of components such as valves, joints, piping, and reaction chambers when the corrosive gas is used.

[0004] On the other hand, pinholes on the plated surface can also cause corrosion. There are several possible causes for pinholes, such as hydrogen gas generated during the plating reaction turning into bubbles during the formation of the plating film, which inhibits film formation, or impurities (oxide film, dirt, oil, etc.) remaining on the base material that are not removed during the pretreatment process, inhibiting film formation.

[0005] In the past, in order to improve corrosion resistance, a method has been used in which a metal substrate is plated with a nickel-phosphorus alloy to form a nickel fluoride passivation film (see, for example, Patent Documents 1 to 3), but these methods were sometimes insufficient.

[0006] There is also a method in which a metal substrate is plated with a nickel-tungsten alloy and a thick nickel fluoride passivation film is formed at a low temperature by utilizing the standard enthalpy of formation of WF6 produced by a fluorination reaction. However, since this is an electrolytic plating method, there is a restriction that the materials to which this method can be applied are limited (see Patent Document 4). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 2954716 [Patent Document 2] Patent No. 3094000 [Patent Document 3] JP 2004-360066 A [Patent Document 4] JP 2008-056978 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention seeks to solve the problems associated with the conventional techniques as described above, and aims to provide a metal material which can be applied to components of semiconductor manufacturing equipment and which has excellent corrosion resistance, and to provide a method for manufacturing said metal material. [Means for solving the problem]

[0009] The present invention relates to, for example, the following [1] to

[12] . [1] A laminate comprising a metal substrate, a nickel-containing plating film layer formed on the metal substrate, and a gold plating film layer formed on the nickel-containing plating film layer, wherein pinholes in the gold plating film layer are sealed with a fluoride passivation film having a thickness of 8 nm or more.

[0010] [2] The laminate according to [1] above, wherein the metal substrate comprises at least one metal selected from the group consisting of stainless steel, iron, aluminum, an aluminum alloy, copper, and a copper alloy.

[0011] [3] The laminate according to [1] or [2] above, further comprising a nickel strike layer between the metal substrate and the nickel-containing plating layer. [4] The laminate according to any one of [1] to [3], wherein the nickel-containing plating film layer comprises, in this order from the metal substrate side, a nickel-phosphorus alloy plating layer (1) having a phosphorus concentration of 8 mass% or more and less than 10 mass%, and a nickel-phosphorus alloy plating layer (2) having a phosphorus concentration of 10 mass% or more and 12 mass% or less.

[0012] [5] The laminate according to any one of [1] to [4] above, wherein the gold plating film layer comprises a displacement type gold plating film layer and a reduction type gold plating film layer, in this order from the nickel-containing plating film layer side.

[0013] [6] A component of a semiconductor manufacturing device, comprising the laminate according to any one of [1] to [5] above. [7] A method for producing a laminate, comprising: a step (A) of forming a nickel-containing plating film layer on a metal substrate; a step (B) of forming a gold plating film layer on the nickel-containing plating film layer; and a sealing treatment step (C) of forming a fluoride passivation film having a thickness of 8 nm or more in pinholes in the gold plating film layer.

[0014] [8] The method for producing a laminate according to [7] above, wherein the sealing treatment step (C) is carried out in an atmosphere having a fluoride gas concentration of 8 vol % or more and a temperature of 100 to 150°C. [9] The method for producing a laminate according to [7] or [8] above, wherein the metal substrate comprises at least one metal selected from the group consisting of stainless steel, iron, aluminum, an aluminum alloy, copper, and a copper alloy.

[0015]

[10] Before the step (A), a current density of 5 to 20 A / dm is applied to the metal substrate. 2The method for producing the laminate according to any one of the above [7] to [9], comprising a step of carrying out nickel strike treatment under the conditions of:

[0016]

[11] The method for producing a laminate according to any one of [7] to

[10] above, wherein the step (A) comprises: a step (a1) of forming a nickel-phosphorus alloy plating layer (1) having a phosphorus concentration of 8 mass% or more and less than 10 mass%; and a step (a2) of forming, after the step (a1), a nickel-phosphorus alloy plating layer (2) having a phosphorus concentration of 10 mass% or more and 12 mass% or less.

[0017]

[12] The method for producing a laminate according to any one of the items [7] to

[11] , wherein the step (B) comprises a step (b1) of forming a displacement gold plating film layer and, following the step (b1), a step (b2) of forming a reduction gold plating film layer. Effect of the Invention

[0018] According to the present invention, it is possible to provide a laminate having excellent corrosion resistance, particularly corrosion resistance against acids. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a schematic diagram showing a laminate before and after a pore-sealing treatment ((a): before pore-sealing treatment, (b): after pore-sealing treatment). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, one embodiment of the present invention will be specifically described. A laminate according to one embodiment of the present invention comprises a metal substrate, a nickel-containing plating film layer formed on the metal substrate, and a gold plating film layer formed on the nickel-containing plating film layer, and pinholes in the gold plating film layer are sealed with a fluoride passivation film having a thickness of 8 nm or more.

[0021] A method for producing a laminate according to one embodiment of the present invention includes a step (A) of forming a nickel-containing plating layer on a metal substrate, a step (B) of forming a gold plating layer on the nickel-containing plating layer, and a sealing treatment step (C) of forming a fluoride passivation coating having a thickness of 8 nm or more in pinholes in the gold plating layer.

[0022] [Metal base material] The metal substrate used in one embodiment of the present invention is a substrate having at least a surface made of metal. The metal substrate is not particularly limited, and examples thereof include metals commonly used in components of semiconductor manufacturing equipment, and are preferably stainless steel, iron, aluminum, aluminum alloys, copper, and copper alloys.

[0023] In order to strengthen the adhesion of the metal substrate to the nickel-containing plating layer, the metal substrate may be subjected to a treatment appropriate to the substrate, such as degreasing, acid washing, or nickel strike treatment, as a pretreatment for step (A). The nickel strike treatment is a preliminary plating treatment using a nickel-containing plating bath, and the current density in the nickel strike treatment is preferably 5 to 20 A / dm 2 , more preferably 5 to 10 A / dm 2 The time for the nickel strike treatment is preferably 5 seconds or more and 5 minutes or less.

[0024] [Nickel-containing plating layer] The nickel-containing plating layer is formed on the metal substrate by the step (A). When the metal substrate is subjected to a nickel strike treatment, a nickel strike layer is formed between the metal substrate and the nickel plating layer.

[0025] From the viewpoint of improving corrosion resistance, the nickel-containing plating coating layer preferably contains phosphorus, and preferably includes, from the metal substrate side, a nickel-phosphorus alloy plating layer (1) having a phosphorus concentration of 8 mass% or more and less than 10 mass%, and a nickel-phosphorus alloy plating layer (2) having a phosphorus concentration of 10 mass% or more and 12 mass% or less.

[0026] The nickel content in the nickel-containing plating film layer is preferably 80% by mass or more, more preferably 85 to 95% by mass, and particularly preferably 88 to 92% by mass, when the nickel-containing plating film layer as a whole is taken as 100% by mass. By having the nickel content in the above range, the ratio of phosphorus in the film layer increases, and excellent corrosion resistance can be exhibited. In addition, when electroless nickel-phosphorus alloy plating films with different phosphorus concentrations are laminated, pinhole defects are formed at different positions during film formation, so that disturbances are less likely to reach the substrate directly, and improvement in corrosion resistance can be expected.

[0027] <Process (A)> The nickel-containing plating layer can be formed on the metal substrate using an electroless plating bath containing a nickel salt and a phosphorus compound as a reducing agent. Examples of the nickel salt include nickel sulfate, nickel chloride, nickel acetate, and nickel carbonate. Examples of the phosphorus compound include sodium hypophosphite and potassium hypophosphite.

[0028] The step (A) preferably includes a step (a1) of forming a nickel-phosphorus alloy plating layer (1) and, after the step (a1), a step (a2) of forming a nickel-phosphorus alloy plating layer (2).

[0029] The deposition rate of the nickel-phosphorus alloy plating layer (1) is preferably 20 to 30 μm / h (hour), more preferably 22 to 25 μm / h (hour), and the deposition rate of the nickel-phosphorus alloy plating layer (2) is preferably 10 to 15 μm / h (hour), more preferably 11 to 13 μm / h (hour). By forming the nickel-phosphorus alloy plating layers (1) and (2) in this manner, corrosion resistance can be improved. The thickness of the nickel-phosphorus alloy plating layers (1) and (2) is preferably 5 μm or more, more preferably 7 to 25 μm, and even more preferably 10 to 20 μm from the viewpoint of film performance that is less likely to cause pinholes and cost.

[0030] [Gold plating layer] A gold plating layer is formed on the nickel-containing plating layer by step (B).

[0031] The gold content in the gold plating film is preferably 90% by mass or more, more preferably 99% by mass or more, and particularly preferably 99.9% by mass or more, when the entire gold plating film layer is taken as 100% by mass. The gold content in the above range stabilizes the corrosion resistance of the laminate according to one embodiment of the present invention. The gold content is determined by an impurity determination method, that is, the gold plating is dissolved in aqua regia and measured by atomic absorption spectrometry and inductively coupled plasma (ICP) atomic emission spectrometry.

[0032] The thickness of the gold plating film is preferably 0.1 μm to 1 μm, more preferably 0.2 to 0.9 μm, and particularly preferably 0.3 to 0.8 μm, from the viewpoints of film performance such that pinholes are unlikely to occur and cost. It is known from the prior art that the thicker the precious metal plating film, the fewer the pinholes will be, and high corrosion resistance is expected, but the cost is high, so it is preferable to set the thickness to an appropriate level.

[0033] <Process (B)> The method for forming the gold plating film layer is not particularly limited, but electroless gold plating is preferred. In the electroless gold plating method, it is preferable to perform displacement gold plating followed by reduction gold plating. That is, the step (B) preferably includes a step (b1) of forming a displacement gold plating film layer and a step (b2) of forming a reduction gold plating film layer after the step (b1).

[0034] In substitution gold plating, nickel dissolves from the nickel coating, and the gold ions in the solution are reduced by the electrons released during the process, depositing a gold plating film.In reduction gold plating, gold ions in the solution are reduced by electrons released during the oxidation reaction of a reducing agent, depositing a gold plating film.

[0035] Examples of electroless gold plating solutions include plating baths containing potassium gold cyanide, gold chloride, gold sulfite, gold thiosulfate, etc., and examples of reducing agents include sodium hydroxide, dimethylamine borane, hexamethylenetetramine, and chain polyamines having an alkyl group with three or more carbon atoms and multiple amino groups.

[0036] A gold plating film layer can be formed by carrying out substitution gold plating preferably at 50 to 90°C for 3 to 7 minutes, more preferably at 65 to 75°C for 3 to 7 minutes, and reduction gold plating preferably at 55 to 65°C for 7 to 15 minutes, more preferably at 58 to 62°C for 7 to 15 minutes.

[0037] [Fluoride passivation film] By subjecting the surface of the gold plating film layer to a fluoride treatment in step (C), pinholes in the gold plating film layer are sealed with a fluoride passivation film.

[0038] 1(b), the fluoride passivation film is formed only on the exposed surface of the nickel-phosphorus alloy plating layer (2b). In other words, it grows only in the vertical direction of the fluoride passivation film 5, and does not form on the side surfaces inside pinholes in the gold plating film layer 3 or on the outermost surface of the gold plating film layer 3, and does not extend beyond the upper end of the gold plating film layer 3.

[0039] The thickness of the fluoride passivation film is usually 8 nm or more, preferably 10 to 20 nm, and more preferably 12 to 18 nm. When the thickness of the fluoride passivation film is within the above range, the durability of the fluoride passivation film becomes suitable for practical use. The thickness of the fluoride passivation film here refers to the length in the lamination direction of the obtained laminate, for example, the length in the vertical direction of the fluoride passivation film 5 in FIG. 1(b).

[0040] <Process (C)> In step (C), the surface of the nickel-containing plating film layer exposed through the pinholes in the gold plating film layer that has been subjected to steps (A) and (B) is forcibly fluorinated using a fluoride gas to form a fluoride passivation film and seal the pinholes.

[0041] Step (C) is carried out in an atmosphere having a fluorination gas concentration of preferably 8% by volume or more, more preferably 10 to 25% by volume, and the fluorination temperature is preferably 100 to 150°C, more preferably 105 to 145°C, more preferably 110 to 140°C.

[0042] Fluoride gas is a general term for at least one gas selected from the group consisting of fluorine (F2), chlorine trifluoride (ClF3) and nitrogen fluoride (NF3) used in fluorination treatment, or any of these gases diluted with an inert gas.

[0043] For example, when chlorine trifluoride is used, it is thermally decomposed at 60 to 100°C to generate fluorine radicals, which can be used in the fluorination reaction. When nitrogen trifluoride is used, it is decomposed by plasma energy to generate fluorine radicals, which can be used in the fluorination reaction.

[0044] Examples of the diluent gas to be entrained in the fluorinated gas include inert gases such as nitrogen gas and argon gas, with nitrogen gas being preferred. When the fluoride gas is used after dilution, its concentration can be appropriately set depending on the reaction conditions. For example, in the case of fluorine, it is preferable to use it at a concentration of about 10% in consideration of costs, etc.

[0045] When the metal substrate is stainless steel, the fluorination is preferably performed at 150 to 190° C., more preferably 155 to 175° C., and when the metal substrate is an aluminum alloy, the fluorination is preferably performed at 140 to 160° C., more preferably 145 to 155° C. By using a film formation temperature within the above range, a good balance of thermal diffusion between the electroless nickel-alloy plating and the gold plating is achieved.

[0046] The fluorination treatment time varies depending on the thickness of the fluoride passivation film to be formed, but in order to exert excellent corrosion resistance, it is preferably 20 to 100 hours, more preferably 30 to 80 hours. EXAMPLES

[0047] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.

[0048] [Example 1] <Process (A)> The surface of stainless steel (SUS316L) processed into a test piece size of 15 mm long x 15 mm wide x 1 mm thick was subjected to degreasing, acid cleaning, and nickel strike treatment as pretreatment. The acid cleaning was performed at room temperature for 25 seconds using hydrochloric acid as a cleaning agent. On the surface of the stainless steel subjected to the nickel strike treatment, an electroless nickel-phosphorus alloy plating film layer (1) having a phosphorus content of 8% by mass or more and less than 10% by mass was formed at a plating temperature of 90°C, pH 4.5 to 4.8, and a film formation rate of 10 μm / 25 minutes. Next, an electroless nickel-phosphorus alloy plating film layer (2) having a phosphorus content of 10% by mass or more and 12% by mass or less was formed at a film formation rate of 10 μm / 50 minutes using an electroless nickel-phosphorus plating film layer (2). This resulted in the formation of a nickel-containing plating layer having a total thickness of 20 μm on the nickel-strike treated stainless steel.

[0049] <Process (B)> Two types of electroless gold plating solutions, "Flash Gold NC (substitution type)" and "Self Gold OTK-IT (reduction type)" (both manufactured by Okuno Chemical Industries Co., Ltd.), were used in that order to treat the nickel-containing plating film layer formed in step (A) at a substitution plating temperature of 70°C for 5 minutes and then at a reduction plating temperature of 60°C for 10 minutes, in that order, to form a gold plating film layer with a total thickness of 0.6 μm.

[0050] <Process (C)> The stainless steel having the nickel-containing plating layer and the gold plating layer formed in steps (A) and (B) was placed in a normal pressure gas-phase flow reactor, and the temperature inside the reactor was raised to 115°C. After that, the atmosphere was replaced with nitrogen gas, and then 10% by volume fluorine gas diluted with nitrogen gas was introduced to replace the nitrogen gas in the reactor with 10% by volume fluorine gas. After complete replacement, the state was maintained for 36 hours, and the exposed parts of the electroless nickel-phosphorus coating of the base due to pinholes generated when gold plating was applied were forcibly fluorinated to form a fluoride passivation film. The obtained fluoride passivation film was analyzed with a W-SEM "JSM-IT200" (manufactured by JEOL Ltd.), and it was confirmed that the film thickness of the fluoride passivation film was 10 nm. The film thickness of the fluoride passivation film here is the length in the stacking direction of the obtained laminate, for example, the length in the vertical direction of the fluoride passivation film 5 in FIG. 1(b).

[0051] [Example 2] A fluoride passivation film was formed in the same manner as in Example 1, except that the forced fluorination time using 10 volume % fluorine gas diluted with nitrogen gas was changed to 72 hours in step (C) of Example 1. The film thickness of the obtained fluoride passivation film was measured in the same manner as in Example 1, and it was confirmed to be 13 nm.

[0052] [Example 3] In Example 1, an aluminum alloy (A5052) was used instead of the stainless steel (SUS316L), and the aluminum alloy was subjected to degreasing, activation treatment, acid cleaning, and zinc substitution treatment as pretreatments. Then, steps (A) and (B) were carried out in the same manner as in Example 1.

[0053] The activation treatment was performed at room temperature for 30 seconds using a mixed acid of acidic ammonium fluoride and nitric acid as a treatment agent. The acid cleaning was performed at room temperature for 25 seconds using nitric acid as a cleaning agent. The zinc replacement treatment was performed at room temperature for 25 seconds using a zincate bath as a treatment agent. The acid cleaning and zinc replacement treatment were each performed twice under the above conditions.

[0054] In step (C), a fluoride passivation film was formed on the gold plating film in the same manner as in Example 2, except that the forced fluorination temperature was 105° C. The thickness of the resulting fluoride passivation film was determined in the same manner as in Example 1, and was confirmed to be 10 nm.

[0055] [Comparative Example 1] Only step (A) of Example 1 was carried out, and a nickel-containing plating film layer of 20 μm in total was formed on the surface of the stainless steel.

[0056] [Comparative Example 2] After carrying out steps (A) and (B) of Example 1, the stainless steel having the nickel-containing plating layer and the gold plating layer was exposed to the atmosphere to form a natural oxide film. The thickness of the obtained natural oxide film was measured in the same manner as in Example 1, and it was confirmed to be 7 nm.

[0057] [Comparative Example 3] After carrying out step (A) of Example 1, the following treatment was carried out. The stainless steel having the nickel-containing plating layer was placed inside a normal pressure gas-phase flow type reactor, and the temperature inside the reactor was raised to 300°C. After that, the air was replaced with nitrogen gas, and then 100% by volume oxygen gas was introduced to replace the nitrogen gas with oxygen gas. After complete replacement, this state was maintained for 12 hours. Next, 10% by volume fluorine gas diluted with nitrogen gas was introduced, and this state was maintained for 12 hours to form a nickel fluoride (NiF2) film on the nickel-containing plating layer. After that, nitrogen gas was injected for 12 hours to stabilize the film formation.

[0058] [evaluation] The coatings on the surfaces of the metal substrates obtained in the above Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated by the following methods. The evaluation results are shown in Table 1.

[0059] <Hydrochloric acid corrosion resistance test> A test piece measuring 15 mm in length, 15 mm in width, and 1 mm in thickness was immersed in a 35% by weight hydrochloric acid solution at 25°C for 5 hours. The mass loss [mg / dm 2 ] and the hydrochloric acid corrosion resistance was evaluated according to the following criteria. (Evaluation Criteria) A: 0.1 mg / dm 2 less than B: 0.1 mg / dm 2 More than 3mg / dm 2 less than C: 3 mg / dm 2 End

[0060] [Table 1]

[0061] In the table, SUS stands for stainless steel (SUS316L) and Al stands for aluminum alloy (A5052). [Explanation of symbols]

[0062] 1...Metal base material 2. Nickel-containing plating layer 2a Nickel-phosphorus alloy plating layer (1) 2b Nickel-phosphorus alloy plating layer (2) 3. Gold plating layer 4. Pinhole 5. Fluoride passivation film

Claims

1. A metal substrate, a nickel-containing plating film layer formed on the metal substrate, and a gold plating film layer formed on the nickel-containing plating film layer, A laminate having a fluoride passivation film having a thickness of 8 nm or more formed only on the exposed surface of the nickel-containing plating film layer.

2. 2. The laminate of claim 1, wherein the metal substrate comprises at least one metal selected from the group consisting of stainless steel, iron, aluminum, an aluminum alloy, copper, and a copper alloy.

3. 3. The laminate according to claim 1, further comprising a nickel strike layer between the metal substrate and the nickel-containing plating layer.

4. The nickel-containing plating film layer includes, in this order from the metal substrate side, a nickel-phosphorus alloy plating layer (1) having a phosphorus concentration of 8% by mass or more and less than 10% by mass, and a nickel-phosphorus alloy plating layer (2) having a phosphorus concentration of 10% by mass or more and 12% by mass or less. The laminate according to any one of claims 1 to 3.

5. The laminate according to any one of claims 1 to 4, wherein the gold plating film layer comprises a substitution type gold plating film layer and a reduction type gold plating film layer in this order from the nickel-containing plating film layer side.

6. A component of a semiconductor manufacturing device, comprising the laminate according to any one of claims 1 to 5.

7. Step (A) of forming a nickel-containing plating film layer on a metal substrate; A step (B) of forming a gold plating film layer on the nickel-containing plating film layer; and The method for producing a laminate includes a sealing treatment step (C) of forming a fluoride passivation film having a thickness of 8 nm or more only on the exposed surface of the nickel-containing plating film layer.

8. The method for producing a laminate according to claim 7, wherein the sealing treatment step (C) is carried out in an atmosphere having a fluoride gas concentration of 8 volume % or more and a temperature of 100 to 150°C.

9. The method for producing a laminate according to claim 7 or 8, wherein the metal substrate comprises at least one metal selected from the group consisting of stainless steel, iron, aluminum, an aluminum alloy, copper, and a copper alloy.

10. Before the step (A), a current density of 5 to 20 A / dm is applied to the metal substrate. 2 The method for producing the laminate according to any one of claims 7 to 9, further comprising a step of performing nickel strike treatment under the conditions of

11. The method for producing a laminate according to any one of claims 7 to 10, wherein the step (A) includes a step (a1) of forming a nickel-phosphorus alloy plating layer (1) having a phosphorus concentration of 8% by mass or more and less than 10% by mass, and a step (a2) of forming a nickel-phosphorus alloy plating layer (2) having a phosphorus concentration of 10% by mass or more and 12% by mass or less after the step (a1).

12. The method for producing a laminate according to any one of claims 7 to 11, wherein the step (B) comprises a step (b1) of forming a substitution gold plating film layer, and a step (b2) of forming a reduction gold plating film layer after the step (b1).

Citation Information

Patent Citations

  • Excimer laser system

    JP1994132582A

  • Material having fluoroplastic formed on surface fluorinated passivated film and various devices and parts using the same

    JP1999165375A

  • Corrosion resistant material, and its production method

    JP2004360066A

  • Metallic material with outermost surface layer of nickel fluoride film and method for producing the same

    JP2008056978A

  • INDUSTRIAL MATERIAL HAVING FLUORINE PASSIVE FILM, AND METHOD FOR MANUFACTURING THE SAME

    JP2954716B2