Method for producing proton-conducting electrolyte membrane, proton-conducting electrolyte membrane and fuel cell
The amorphous ruthenium hydrogen phosphate electrolyte membrane addresses the need for high proton conductivity in the 200 to 350°C range by enabling low-cost, thin-film production suitable for fuel cell stacks, enhancing efficiency and reducing manufacturing time.
Patent Information
- Application Number
- JP2021012801
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-01-29
AI Technical Summary
There is a lack of high-performance solid electrolyte materials with high proton conductivity in the medium temperature range of 200 to 350°C, and existing materials are difficult to manufacture at low cost and in a thin film form suitable for fuel cell stacks.
A proton-conducting electrolyte membrane composed of amorphous or mainly amorphous ruthenium hydrogen phosphate is produced by mixing alkali metal, ruthenium, and phosphoric acid, followed by heating and forming a thin film between organic thin films, allowing for easy handling and low-cost production.
The membrane exhibits high proton conductivity in the medium temperature range of 200 to 350°C and can be easily stacked, reducing manufacturing time and cost while maintaining mechanical strength and conductivity.
Smart Images

Figure 0007593624000004 
Figure 0007593624000005 
Figure 0007593624000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a proton-conductive electrolyte membrane that can be used as an electrolyte for fuel cells, and more particularly to a thin-film proton-conductive electrolyte membrane that exhibits high proton conductivity in the medium temperature range of 200 to 350°C. [Background technology]
[0002] In the development of fuel cells as a next-generation energy storage system, the development of stable, high-performance electrolyte materials is of great importance. Electrolyte materials that have high proton conductivity at high temperatures of 500°C or higher and at low temperatures of 100°C or lower have already been developed. Fluorine resin-based ion exchange membranes used in polymer electrolyte fuel cells are well known as electrolyte materials used at temperatures below 100°C. BaCe 0.8 Y 0.2 0 3-a Such perovskite-type metal oxides exhibit high ionic conductivity at temperatures above 500°C.
[0003] However, there are still very few solid electrolyte materials that are the most energy efficient and exhibit high proton conductivity in the mid-temperature range of 200 to 350°C, which is close to the expected usage environment, and currently, development of high-performance solid electrolyte materials is continuing vigorously.
[0004] For example, as proton-conductive materials that exhibit high proton conductivity even in a dry atmosphere at 100°C or higher, phosphate-based materials have been developed, such as a proton-conductive composition in which a metal phosphate is added to a phosphosilicate gel or silica gel (see, for example, Patent Document 1), and a proton-conductive material containing a metal phosphate in which a crystalline metal phosphate is treated by mechanical milling to disrupt part of the crystallinity and generate free phosphoric acid, thereby improving the proton conductivity (see, for example, Patent Document 2). [Patent Document 1] JP 2004-55181 A [Patent Document 2] Patent No. 3916139 [Patent Document 3] JP 2019-87463 A Summary of the Invention [Problem to be solved by the invention]
[0005] Here, the above-mentioned conventional solid electrolytes are mainly crystalline compounds designed with the idea of constructing nanospaces, such as tunnels or interlayer spaces, in the structure and using these spaces as conductive paths. However, such solid electrolytes have problems in that it is difficult to create large spaces and they need to be synthesized at high temperatures, which requires a lot of energy and increases the production costs.
[0006] In addition, in conventional phosphate-based solid electrolyte materials, phosphoric acid may dissolve and corrode the frame. Under these circumstances, there is a need for the development of a proton conductor that can be produced inexpensively using a simple production method and has high proton conductivity in the medium temperature range of, for example, 200 to 400°C.
[0007] Therefore, the inventors of the present application proposed a proton conductor containing an amorphous or mainly amorphous transition metal hydrogen phosphate in Patent Document 3. The precursor of the proton conductor obtained in Patent Document 3 was a material lacking in density. The proton conductor obtained in Patent Document 3 was a precursor formed into a block (bulk) shape by heating in a ceramic container for one week or more, and when measured in a state cut together with the ceramic container, it had high proton conductivity in the medium temperature range of 200 to 350°C.
[0008] Incidentally, in order to put fuel cells into practical use, it is necessary to form a structure called a stack in which unit cells are stacked in series, and in order to apply such a proton conductor to a fuel cell and put it into practical use, it is essential to make the proton conductor thin so that this stack can be made. However, the proton conductor obtained by the inventors of the present application in Patent Document 3 lacked denseness in the precursor, and it was only suggested that the precursor had high functionality as an electrolyte in a bulk sample obtained by sintering the precursor, and no knowledge on how to make a thin film was obtained.
[0009] The present invention has been made in view of the above-mentioned points, and has an object to provide a proton-conducting electrolyte membrane that has high proton conductivity in the medium temperature range of 200 to 350°C and can be stacked by a simple method, a method for producing the same, and a fuel cell including the proton-conducting electrolyte membrane. [Means for solving the problem]
[0010] In order to achieve the above object, the method for producing a proton-conductive electrolyte membrane of the present invention is a method for producing a proton-conductive electrolyte membrane containing amorphous or amorphous-based ruthenium hydrogen phosphate represented by the following general formula (1), and is characterized by comprising the steps of: mixing an alkali metal raw material, a ruthenium raw material, and phosphoric acid to prepare a mixture; heating the mixture to synthesize a precursor; spreading the powdered precursor on an organic thin film or applying the liquefied precursor on an organic thin film; overlaying an organic thin film on the precursor on the organic thin film; applying pressure to the precursor while heating it in a state where it is sandwiched between the organic thin films to form a proton-conductive electrolyte membrane; and peeling off the proton-conductive electrolyte membrane from the organic thin film.
[0011] [C1] H a A b RuP c O d (1) (Here, A is an alkali metal, a, b, and c are natural numbers, and d is a value defined to satisfy the charge neutrality condition of a+b+3+5c=2d.) Effect of the Invention
[0012] According to the present invention, it is possible to provide a method for producing a thin-film proton-conducting electrolyte membrane which has high proton conductivity in the medium temperature range of 200 to 350° C. and can be stacked, a proton-conducting electrolyte membrane, and a fuel cell including the proton-conducting electrolyte membrane. [Brief description of the drawings]
[0013] [Figure 1] 2 is a flowchart illustrating the flow of a method for producing a proton conducting electrolyte membrane according to the present embodiment. [Diagram 2] 1 is infrared absorption spectrum data showing the degree of condensation of phosphate. [Diagram 3] FIG. 1 is a schematic diagram of a fuel cell using a proton-conducting electrolyte membrane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The proton-conductive electrolyte membrane of the present invention is a thin film of a proton conductor containing an amorphous or mainly amorphous ruthenium hydrogen phosphate represented by the following general formula (1).
[0015] [C2] H a A b RuP c O d (1) (Here, A is an alkali metal, a, b, and c are natural numbers, and d is a value defined to satisfy the charge neutrality condition of a+b+3+5c=2d.) For example, if the alkali metal A is sodium, and a = 4, b = 4, and c = 13, then a + b + 3 + 5 c = 4 + 4 + 3 + 65 = 76 = 2d, so d = 38. H4Na4RuP 13 O 38 It becomes.
[0016] The proton-conducting electrolyte membrane of the present invention is an amorphous or mainly amorphous ruthenium hydrogen phosphate, and therefore may be not only a transition metal hydrogen phosphate that is entirely amorphous, but also a ruthenium hydrogen phosphate that is mostly amorphous, while ruthenium hydrogen phosphate that is only partially amorphous is not included.
[0017] The amorphous hydrogen phosphate is not limited to a specific hydrogen phosphate, and examples thereof include hydrogen tripolyphosphate, hydrogen pyrophosphate, and hydrogen orthophosphate. For example, hydrogen phosphates containing orthophosphate ions, pyrophosphate ions, tripolyphosphate ions, and phosphate ions with a higher degree of condensation can be suitably used as the proton-conducting electrolyte membrane of the present invention.
[0018] Further, while the proton-conductive electrolyte membrane of the present invention is a hydrogen phosphate, phosphates that do not contain any hydrogen are not included in the present invention.
[0019] The reason why amorphous hydrogen phosphate exhibits high proton conductivity is presumed to be as follows: "Amorphous" refers to a state in which short-range order between adjacent atoms is maintained but long-range order is absent.
[0020] Amorphous condensed hydrogen phosphate is a substance with a medium-range order of multiple PO4 tetrahedra, and protons can move freely within this medium-range order. Furthermore, by becoming amorphous, paths are formed between condensed phosphate ions, and it is thought that proton diffusion occurs easily. In the case of protons, unlike other ion conductors, the size is extremely small, so it is thought that a large tunnel or interlayer is not required for their movement, and it is sufficient that the paths for protons to move are connected. In crystalline substances with tunnel structures or layered structures, this path is connected only in a specific crystal axis direction, and it is difficult for protons to move in other directions. However, in amorphous solids, the loss of long-range order causes structural disorder at the atomic level, which creates many defects and slightly unstable local structures in the structure, so it is thought that there are countless paths for protons to pass through, and there is no restriction on the direction of movement. This is presumed to result in high proton conductivity.
[0021] It is believed that even when orthophosphate ions are combined with such a network of condensed phosphate ions, proton conduction is possible through a similar process.
[0022] In the ruthenium hydrogen phosphate of the present invention, ruthenium is a transition metal that takes a trivalent oxidation state (including those mainly composed of a transition metal that takes a trivalent oxidation state), and the hydrogen phosphate can exist stably in an amorphous or mostly amorphous state at a temperature of 200 to 350° C. Since the proton-conductive electrolyte membrane of the present invention is intended to be used in the medium temperature range of 200 to 350° C., stable performance can be obtained by using ruthenium that can exist stably in an amorphous or mostly amorphous state in this temperature range.
[0023] In addition, when a transition metal other than ruthenium is used, such as iron, aluminum, or chromium, which tends to assume a trivalent valence in phosphate, it is likely to crystallize, and therefore it is considered difficult to use it as the amorphous material of this embodiment. However, the transition metal does not necessarily have to consist of only ruthenium, and other transition metals may be added.
[0024] Furthermore, the proton-conductive electrolyte membrane of the present invention is not limited to one consisting only of ruthenium hydrogen phosphate, and may contain silicates, borates, sulfates, nitrates, and the like, as long as it contains ruthenium hydrogen phosphate, and does not adversely affect the ruthenium hydrogen phosphate.
[0025] In addition, the proton conductive electrolyte membrane of the present invention has a glass-like form without grain boundaries, which further increases the proton conductivity. A proton conductive electrolyte membrane in a glass-like form without grain boundaries can be easily manufactured by the method described below. In general, solid electrolytes such as those of the present invention are often in a powder form when synthesized. If a powdered proton conductor is simply pressure-molded, the resistance between particles is large and the proton conductivity decreases. In addition, handling is also inconvenient. For this reason, a method is generally adopted in which the proton conductor is molded using a binder or the like, or the proton conductor is fired at a high temperature to mold the proton conductor. However, in the method using a binder, a binder suitable for the temperature to be used is separately required, which increases the cost. Furthermore, if poor bonding occurs between the binder and the solid electrolyte, the proton conductivity cannot be sufficiently increased. In addition, in the method of molding by firing at a high temperature, measures against cracks and the like are necessary, and the high temperature requires a lot of time and energy.
[0026] In contrast, the proton-conductive electrolyte membrane of the present invention can be made into a glass-like form without grain boundaries at a relatively low temperature without using a binder, and can therefore be produced at low cost in a short time.
[0027] In the present invention, examples of the alkali metal that can be used include lithium, sodium, potassium, rubidium, and cerium, but from the viewpoint of production costs, it is preferable to use lithium and sodium.
[0028] In addition, the chemical environment around the alkali ions of potassium, rubidium, and cerium phosphates is similar to that of the sodium ions in sodium phosphates, and when each alkali metal alone forms a phosphate crystal, it often has the same structure, so they exhibit properties similar to those of sodium phosphate.
[0029] Furthermore, the proton-conductive electrolyte membrane of the present invention does not necessarily need to contain only one type of alkali metal, but may contain two or more types of alkali metals.
[0030] Next, an example of a method for producing the proton-conductive electrolyte membrane of the present invention will be described, however, the method for producing the proton-conductive electrolyte membrane of the present invention is not limited to the following method.
[0031] Water, an alkali metal source, a ruthenium source, and phosphoric acid are mixed and reacted at a predetermined temperature for a predetermined time, thereby obtaining a proton-conductive electrolyte membrane containing amorphous or mainly amorphous ruthenium hydrogen phosphate.
[0032] As the alkali metal raw material, carbonates, oxides, hydroxides, acetates, and halides of alkali metals can be used, but from the viewpoint of simplicity, it is preferable to use carbonates.
[0033] Ruthenium raw materials can be nitrates, carbonates, acetates, halides, and phosphates of ruthenium. Anhydrides are less reactive, so hydrates are preferred. When using powdered ruthenium raw materials, the smaller the particle size, the more preferred. The ruthenium raw material may be used in a state of being dissolved in water or alcohol in advance.
[0034] As the phosphoric acid, orthophosphoric acid and pyrophosphoric acid can be preferably used, and condensed phosphoric acid can also be used. These phosphoric acids may be used as an aqueous solution by dissolving them in water.
[0035] The water used may be ion-exchanged water or pure water. Note that water is not essential and may be mixed as needed.
[0036] [Method of manufacturing proton-conductive electrolyte membrane] FIG. 1 is a flow chart for explaining the process flow of the method for producing the proton-conductive electrolyte membrane of this embodiment. As shown in FIG. 1, the method for producing the proton-conductive electrolyte membrane of this embodiment includes a step S1 of mixing an alkali metal raw material, a ruthenium raw material, and phosphoric acid to prepare a mixture, a step S2 of heating the mixture to synthesize a precursor, a firing step S31 and a powdering step S32 when a powdered precursor is used, a liquefied precursor when a liquefied precursor is used, a step S5 of spreading the powdered precursor on an organic thin film or applying the liquefied precursor on an organic thin film, a step S6 of further stacking an organic thin film on the precursor on the organic thin film, a step S7 of heating the precursor while sandwiched between the organic thin films to form a proton-conductive electrolyte membrane, and a step S8 of peeling the proton-conductive electrolyte membrane from the organic thin film. Each step will be explained below.
[0037] [Raw material mixing process S1] It is preferable that the water, the alkali metal raw material, the ruthenium raw material, and the phosphoric acid are in a homogeneous state. By adding an aqueous phosphoric acid solution to the powdered ruthenium raw material, the water, the alkali metal raw material, the ruthenium raw material, and the phosphoric acid can be easily made homogeneous. Note that, when a large amount of phosphoric acid is added, it is not necessary to add water. Also, it is possible to promote homogenization in the same way by adding alcohol in this process.
[0038] The mixing ratio of the alkali metal raw material and phosphoric acid is preferably such that the content ratio of alkali metal to phosphorus in the proton conductive electrolyte membrane is 1:3 to 1:5 in terms of molar ratio.
[0039] The mixing ratio of the ruthenium raw material and phosphoric acid is preferably such that the molar ratio of ruthenium to phosphorus in the proton conductive electrolyte membrane is 1:6 to 1:19, more preferably 1:6 to 1:13. When water is added, the amount of water added is preferably 0.5 to 10 equivalents relative to phosphorus.
[0040] It was found that in the next synthesis step S2, when the molar ratio of ruthenium to phosphorus is within the range of 1:6 to 1:13, the time required for dehydration condensation increases as the phosphorus content increases. Figure 2 shows infrared absorption spectrum data for samples of raw materials with molar ratios of ruthenium:sodium:phosphorus of 1:3.5:8, 1:4:13, and 1:5:13, which were heated at 400°C for 1 hour and then at 360°C for 17 hours. According to this data, the sample with a molar ratio of ruthenium:sodium:phosphorus of 1:3.5:8 had a peak at 850 to 1100 cm. -1 Two split absorption lines were observed at the molar ratio of ruthenium:sodium:phosphorus, indicating that condensation had progressed to the tripolyphosphate ion. However, this absorption was not clearly observed when the molar ratio of ruthenium:sodium:phosphorus was 1:4:13 and 1:5:13, indicating that the condensation reaction had progressed less at 1:4:13 and 1:5:13 than at 1:3.5:8 in the synthesis step S2 under the same conditions. It was also found that after synthesis, the more phosphorus the compound, the higher the deliquescence and the more difficult it became to handle.
[0041] In a sample having a molar ratio of 14 or more of phosphorus to 1 ruthenium, the reaction takes a long time and handling becomes difficult. In addition, in a sample having a molar ratio of 5 or less of phosphorus to 1 ruthenium, it becomes difficult to synthesize a good glassy sample without grain boundaries in the following synthesis step S7. Therefore, the molar ratio of ruthenium to phosphorus in the proton conductive electrolyte membrane is preferably 1:6 to 1:13.
[0042] [Precursor synthesis step S2] The mixture of water, the alkali metal raw material, the ruthenium raw material, and phosphoric acid is heated at a predetermined temperature for a predetermined period of time using an electric furnace or the like.
[0043] When water, an alkali metal raw material, a ruthenium raw material, and phosphoric acid are mixed and heated, a dehydration and condensation reaction occurs, generating gas and water vapor. For example, when a metal chloride is used as the ruthenium raw material, hydrogen chloride gas is generated. This hydrogen chloride gas is produced in large amounts in the early stages of the reaction, and water vapor becomes the main component in the latter stages of the reaction.
[0044] The heating temperature is preferably 200 to 350° C. Ruthenium has a slow reaction rate and is difficult to crystallize even at high temperatures, so heating is preferably performed in the above-mentioned medium temperature range. The heating time is preferably about 1 hour.
[0045] Alternatively, it is also possible to first react ruthenium chloride hydrate with phosphoric acid to synthesize amorphous ruthenium phosphate, which is an amorphous phosphate of a transition metal, and then mix this with an alkali metal raw material and, if necessary, phosphoric acid, and heat the reaction.
[0046] The precursor synthesized by the above method is in a brittle lump immediately after synthesis, but the viscosity increases over time. According to the manufacturing method of the present invention, the precursor can be made into a thin film by sandwiching the powdered or liquefied precursor between organic thin films and heating it. Since the precursor can be changed into either a powdered or liquid state, it is easy to handle and can be applied to various existing thin film manufacturing devices, making it highly versatile.
[0047] [Firing process S31 and powdering process S32] When a powdered precursor is used, the highly viscous precursor synthesized in the synthesis step S2 is fired in an electric furnace. For example, when the phosphorus content is relatively small, such as when the molar ratio of ruthenium to phosphorus is 1:8, the precursor can be solidified by heating at 400°C for 1 hour and at 360°C for 2 hours. On the other hand, when the phosphorus content is relatively large, such as when the molar ratio of ruthenium to phosphorus is 1:11 to 1:13, the precursor is desirably solidified by heating at 400°C for 1 to 2 hours and at 360°C for 12 to 19 hours in order to reduce the deliquescence of the sample after synthesis. The precursor solidified in the firing step S31 is pulverized and powdered in the powderization step S32. When a powdered precursor is used, the precursor needs to be stored in a moisture-proof environment after synthesis to prevent deliquescence.
[0048] [Liquification process S4] When using a liquefied precursor, the highly viscous proton conductor synthesized in the synthesis step S2 may be deliquesced by placing it in the air. The liquefaction of the precursor is not limited to deliquescence, and water may be added.
[0049] [Spreading or coating process on organic thin film S5] When a powdered precursor is used, the powdered proton conductor obtained in the above-mentioned firing step S31 and powdering step S32 is spread into a mold formed of an organic thin film. When a powdered precursor is used, it is possible to form an electrolyte membrane of a specific shape by forming a mold from an organic thin film.
[0050] When a liquefied precursor is used, the liquid precursor obtained in the liquefaction step S4 is applied onto the organic thin film.
[0051] The organic thin film is a plate- or sheet-shaped material that does not deform itself even when heated to 300° C. or higher and does not react with the precursor, and is preferably a polyimide-based material or a polytetrafluoroethylene-based material. For example, Kapton (registered trademark) can be used as the polyimide-based material, and Teflon (registered trademark) can be used as the polytetrafluoroethylene-based material.
[0052] [Organic thin film overlay process S6] An organic thin film is further laminated on the precursor on the organic thin film obtained in the spreading or coating step S5 on the organic thin film. The upper and lower organic thin films are not limited to being made of the same material, and for example, a combination of polyimide and Teflon may be used.
[0053] [Heat forming process S7] In the organic thin film stacking step S6, the precursor sandwiched between the organic thin films is heated and pressurized in an electric furnace to form a proton-conductive electrolyte membrane. The heating temperature is 200 to 400° C., and the heating time is 1 to 2 hours.
[0054] Here, by applying pressure while heating the precursor, it is possible to adjust the thickness of the resulting proton-conductive electrolyte membrane. Table 1 shows the results of applying pressure to a precursor having a molar ratio of ruthenium:sodium:phosphorus of 1:4:13 in a heat molding process at 260°C for 95 minutes to adjust the thickness of the resulting proton-conductive electrolyte membrane. In this process, it is also possible to use a conventionally known hot press method for heating and pressurizing.
[0055] When a powdered precursor is used, the thickness of the resulting proton-conductive electrolyte membrane can be adjusted by changing the thickness of the mold formed from the organic thin film.
[0056] [Table 1]
[0057] The method of thinning and the thickness of the film are not particularly limited. For example, the liquefied precursor can be applied onto an organic thin film by a conventionally known coating method such as spin coating, casting, inkjet printing, printing, die coating, blade coating, roll coating, spray coating, curtain coating, etc., and can be formed to a desired thickness by a conventionally known thin film manufacturing device.
[0058] The thickness of the proton-conductive electrolyte membrane is preferably 10 to 500 μm, which can be produced by existing thin film production equipment. A thickness of 10 μm or more is preferable because a glassy proton-conductive electrolyte membrane without grain boundaries can obtain sufficient mechanical strength as an electrolyte membrane. If the thickness is within the above range, it is highly versatile as an electrolyte.
[0059] [Peeling process S8] In the heat molding step S7, after a predetermined time has elapsed at a predetermined temperature, the temperature is returned to room temperature and the proton conductive electrolyte membrane is peeled off from the organic thin film, thereby obtaining the proton conductive electrolyte membrane. EXAMPLES
[0060] The manufacturing method of the proton conductive electrolyte membrane will be described below based on the examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the gist of the present invention, and are not excluded from the scope of the present invention. The manufacturing method of Example 1 will be described in detail below. The other Examples 2 to 10 are almost the same, so their description will be omitted, and the composition, manufacturing conditions, and proton conductivity results of each Example are shown in Table 2.
[0061] [Table 2]
[0062] (Preparation of proton-conducting electrolyte membrane) (Example 1 Ru:Na:P=1:3.5:8) First, 10.062 g of powdered ruthenium chloride hydrate RuCl3·nH2O (Ru: 39.23 mass%, Tanaka Kikinzoku Kogyo Co., Ltd.), anhydrous sodium carbonate (Na2CO3, Nacalai Tesque, Inc., 7.055 g), and 36.006 g of 85 mass% aqueous orthophosphoric acid solution (Nacalai Tesque, Inc.) were mixed in a ceramic evaporating dish and reacted by heating in air with a gas burner for 30 minutes. After that, the mixture was cooled to room temperature to produce a highly viscous black-brown sample.
[0063] A Teflon sheet was placed inside a gold boat as an organic thin film, and the obtained precursor was applied onto the sheet. This was then baked in an electric furnace at 400°C for 1 hour and 360°C for 2 hours.
[0064] The solidified precursor after firing was ground in a mortar to a powder. Next, a Teflon (registered trademark) sheet was laid on a glass plate, and a mold carved out of a Kapton (registered trademark) sheet was placed on top of that. The powdered precursor was then spread into the mold, a Teflon sheet was placed on top of the spread precursor, and a Kapton sheet and a glass plate were placed on top of that.
[0065] The sample assembled as described above was heated in an electric furnace at 260°C for 1 hour. After heating, it was left in the electric furnace until it returned to room temperature. Then, it was peeled off from the Teflon sheet and Kapton to obtain a proton-conductive electrolyte membrane.
[0066] The products were identified by powder X-ray diffraction measurement (XRD). More specifically, a powder X-ray diffraction measurement device (manufactured by Bruker AXS, product name: D8-Advance, Cu Kα radiation) was used to perform X-ray diffraction measurement at measurement angles (2θ) ranging from 5° to 70° to confirm the amorphous nature of the samples. Since none of the samples showed any significant diffraction peaks, it was confirmed that the samples were amorphous or mainly amorphous ruthenium hydrogen phosphate.
[0067] In addition, infrared absorption spectroscopy (FT / IR) was performed to estimate the degree of condensation of the product. More specifically, the sample was sandwiched between KBr single crystal plates and molded under pressure, and the infrared absorption spectrum was measured by the transmission method using an infrared absorption spectrometer (manufactured by JASCO, product name: FT / IR-4100). Then, by examining the positions and shapes of the absorption bands of POP, PO...M, POH, and OH in the obtained spectrum, it was confirmed that all samples contained condensed phosphate ions.
[0068] (Measurement of proton conductivity) Next, the resistance value (impedance) in each example was measured using a Cole-Cole plot (Nyquist plot) by the complex impedance method, and the proton conductivity of the product was calculated. More specifically, the impedance was measured from 42 Hz to 5 MHz using an impedance analyzer (manufactured by HIOKI, product name: IM3536LCR meter), and a Cole-Cole plot (Nyquist plot) from room temperature to 350°C was obtained.
[0069] The measurement program used was the HIOKI LCR meter sample application, and measurements were performed at room temperature (25°C) to 350°C at measurement frequencies (AC) of 42 Hz to 5 MHz.
[0070] The measurement sample was a proton-conductive electrolyte membrane sandwiched between two electrode plates, placed in a glass tube with one end sealed, and then set in an electric furnace. After setting, the inside of the glass tube was evacuated with a rotary pump, and the proton conductivity was measured while the temperature was raised from room temperature. After reaching the maximum temperature (i.e., the proton conductivity measurement temperature shown in Table 2), the sample was cooled to room temperature, and after reaching room temperature, the proton conductivity was measured again during the temperature rise process to confirm the reproducibility of the measured value.
[0071] As shown in Table 2, the proton-conductive electrolyte membrane of the present invention represented by the above general formula (1) had high proton conductivity in the medium temperature range of 270 to 300°C.
[0072] (Fuel cell configuration) 3, the fuel cell 1 of the present invention is a single cell, which is the minimum unit having a proton-conductive electrolyte membrane 4 sandwiched between a fuel electrode 2 and an air electrode 3. Note that, although the fuel cell 1 having a single cell will be described here, the present invention is not limited to this, and the fuel cell may have a stack in which a plurality of cells are stacked in series.
[0073] The fuel cell 1 has a fuel electrode 2, an air electrode 3, and a proton-conductive electrolyte membrane 4 provided between the fuel electrode 2 and the air electrode 3. The fuel electrode 2 is supplied with, for example, hydrogen gas as a fuel, and the air electrode 3 is supplied with oxygen as an oxidant from the atmosphere. The fuel and the oxidant are not limited to hydrogen gas and air, and it is also possible to use methanol, ethanol, glucose, etc. as the fuel and oxygen as the oxidant. The fuel electrode 2 and the air electrode 3 are electrically connected to an external load 6 via wiring 5, and can supply power to the external load 6.
[0074] In the fuel cell 1, when fuel is supplied to the fuel electrode 2, hydrogen atoms contained in the fuel are converted into protons (H + ) and electrons (e - The protons move through the proton-conducting electrolyte membrane 4 to the air electrode 3. Meanwhile, the electrons move to the air electrode 3 through an external load 6. At the air electrode 3, oxygen contained in the supplied oxidant combines with the protons and electrons that have moved from the fuel electrode 2 to produce water. Expressed as an electrochemical equation, at the fuel electrode 2, H2 → 2H + +2e - , and 1 / 2O2+2H at cathode 3 + +2e - →The reaction of H2O occurs.
[0075] In the present invention, for the members constituting the fuel cell other than the electrolyte membrane, any conventionally known configuration in the field of fuel cells can be used.
[0076] (Evaluation as a fuel cell) The proton-conductive electrolyte membrane of Example 1, in which the molar ratio of ruthenium:sodium:phosphorus is 1:3.5:8, was evaluated when applied as an electrolyte for a fuel cell. A single cell prepared as shown in FIG. 3 was placed in an electric furnace as a measurement sample, and its performance was examined at 150°C, 250°C, and 300°C. Hydrogen gas (purity 99.99% or more) generated by a KOFLOC Hydrogen gas generator was passed through the single fuel cell at a flow rate of 0.1 L / min, and the generated current and voltage values were measured by a YOKOGAWA GS610 Source Measure Unit. Air (atmosphere) was used on the oxygen electrode side. As a result, as shown in Table 3, the maximum power density at 150°C was 0.39 mW / cm 2 , the maximum power density at 250℃ is 1.49mW / cm 2 , the maximum power density at 300℃ is 2.48mW / cm 2 It was confirmed that a fuel cell using a proton-conductive electrolyte membrane was obtained.
[0077] [Table 3]
[0078] As shown in Tables 2 and 3, according to the method for producing the proton-conductive electrolyte membrane of the present embodiment, a proton-conductive electrolyte membrane that is a laminated thin film and exhibits high proton conductivity in the medium temperature range of 200 to 350° C. can be easily obtained in a relatively short time, and can also be produced on an industrial scale.
[0079] Furthermore, the proton-conductive electrolyte membrane of the present embodiment can change the precursor into either a powder or liquid state, and is therefore easy to handle and can be applied to various existing thin film manufacturing devices, making it highly versatile.
Claims
1. A method for producing a proton-conducting electrolyte membrane containing an amorphous or mainly amorphous ruthenium hydrogen phosphate represented by the following general formula (1), mixing an alkali metal source, a ruthenium source, and phosphoric acid to prepare a mixture; heating the mixture to synthesize a precursor; A step of spreading the powdered precursor on an organic thin film or applying the liquefied precursor on an organic thin film; a step of overlaying an organic thin film on the precursor on the organic thin film; a step of applying pressure to the precursor while heating the precursor in a state where the precursor is sandwiched between the organic thin films to form a proton-conductive electrolyte membrane; peeling the proton-conductive electrolyte membrane from the organic thin film; Equipped with 2. A method for producing a proton-conductive electrolyte membrane, wherein the alkali metal source contains sodium as the alkali metal. [Chemical formula 1] H a Na b Ruur c O d (1) (Here, a, b, and c are natural numbers, and d is a value defined to satisfy the charge neutrality condition of a+b+3+5c=2d.)
2. 2. The method for producing a proton-conductive electrolyte membrane according to claim 1, wherein the organic thin film is at least one material selected from the group consisting of polyimide-based materials and polytetrafluoroethylene-based materials.
3. 2. The method for producing a proton conducting electrolyte membrane according to claim 1, wherein the ruthenium raw material and the phosphoric acid are mixed so that the content ratio of ruthenium to phosphorus is 1:6 to 1:13 in terms of molar ratio.
4. The present invention contains an amorphous or amorphous-based ruthenium hydrogen phosphate represented by the following general formula (1): A proton-conducting electrolyte membrane having a thickness of 10 to 500 μm. [Case 2] H a Na b Ruur c O d (1) (Here, a, b, and c are natural numbers, and d is a value defined to satisfy the charge neutrality condition of a+b+3+5c=2d.)
5. 5. The proton-conductive electrolyte membrane according to claim 4, wherein the molar ratio of ruthenium to phosphorus is 1:6 to 1:
13.
6. A fuel cell comprising the proton-conducting electrolyte membrane according to claim 4 or 5.
Citation Information
Patent Citations
Solid electrolyte sheet, electrode sheet, and all solid secondary battery
JP2014096311A
Proton conductor and production method thereof
JP2019087463A