METHOD FOR PRODUCING SINTERED BODY AND APPARATUS FOR PRODUCING SINTERED BODY

By controlling current flow and using alternating current electric fields, the method addresses the limitations of conventional flash sintering to produce high-density sintered bodies efficiently and safely.

JP7593641B2Active Publication Date: 2024-12-03NAT UNIV CORP TOKAI NAT HIGHER EDUCATION & RES SYST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021535377
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-26
Filing Date
2020-07-29
Publication Date
2024-12-03
Estimated Expiration
2040-07-29

AI Technical Summary

Technical Problem

Conventional flash sintering methods are limited in controlling the flash temperature arbitrarily, which affects the density of the sintered body, and there is a risk of electrode melting due to high electric power input.

Method used

A method involving controlled current flow during flash sintering to maintain a constant sintering rate, using alternating current electric fields with specific frequency and power control to prevent electrode melting, and adjusting the electric field strength to achieve high-density sintered bodies.

Benefits of technology

The method enables the production of high-density sintered bodies in a shorter time and at lower temperatures, avoiding electrode melting and ensuring uniform density distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593641000001
    Figure 0007593641000001
  • Figure 0007593641000002
    Figure 0007593641000002
  • Figure 0007593641000003
    Figure 0007593641000003
Patent Text Reader

Abstract

This method is for manufacturing a sintered compact by heating a ceramic green compact while applying an electric field thereto. The method involves controlling an electric current flowing through the ceramic green compact so as to achieve a constant sintering rate.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application is based on and claims the benefit of priority from Japanese Patent Application No. 2019-138645 filed on July 29, 2019, Japanese Patent Application No. 2019-142722 filed on August 2, 2019, and Japanese Patent Application No. 2019-236358 filed on December 26, 2019, the entire contents of which are incorporated herein by reference. [Technical field]

[0002] The present disclosure relates to a sintered body. [Background technology]

[0003] Generally, ceramic sintered bodies are produced by compacting and molding raw material powders, and then heat-treating the molded body at high temperatures. The heat treatment temperature (called the sintering temperature) is 1200°C to 1500°C, depending on the type of ceramic, and the sintering time is about several hours. In addition to the general sintering methods mentioned above, various methods have been devised to improve the density of sintered bodies, such as methods that apply pressure from the outside (hot pressing method, HIP method, etc.).

[0004] Recently, a flash sintering method has been developed that can complete sintering at a lower temperature and in a shorter time than before by applying an electric field to a ceramic powder compact (see Non-Patent Document 1). This sintering method is characterized in that when the ceramic powder compact is heated while an electric field is applied, the sample current increases sharply at a certain temperature (hereinafter, this phenomenon may be referred to as the "flash phenomenon"), and the sintering process ends instantly. It has also been revealed that increasing the electric field strength lowers the temperature at which the sintered compact begins to shrink, and the shrinkage behavior changes more sharply. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Marco Cologna et al, “Flash Sintering of Nanograin Zirconia in <5 s at 850℃”, Rapid Communications of the American Ceramic Society, 2010, Vol. 93, No. 11, p. 3556-3559 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the flash temperature at which the flash phenomenon occurs is uniquely determined if the electric field is constant. On the other hand, in order to increase the final density of the sintered body, a higher flash temperature is considered to be advantageous, but with conventional flash sintering methods, the flash temperature cannot be controlled arbitrarily. In addition, if the amount of power input to the sample is large, the metal electrodes in contact with the sample may melt. For this reason, there is a limit to the amount of power that can be input to the ceramic powder compact during the sintering process. Therefore, there is room for further improvement in terms of the density (densification) of the sintered body.

[0007] The present disclosure has been made in light of these circumstances, and one of its exemplary objectives is to provide a new technique for improving the density of a sintered body. [Means for solving the problem]

[0008] In order to solve the above problems, a method for producing a sintered body according to one embodiment of the present invention is a method for producing a sintered body in which an electric field is applied to a ceramic compact while the temperature is increased, and the current flowing through the ceramic compact is controlled so as to keep the sintering rate constant. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a sintered body with a high density that is difficult to achieve using only conventional flash sintering methods. [Brief description of the drawings]

[0010] [Figure 1] FIG. 4 is a graph showing the change in linear shrinkage rate during the process of producing sintered bodies from each sample. [Diagram 2] FIG. 1 is a diagram showing changes in specimen current due to a conventional flash sintering method and a Rate Control Flash. [Diagram 3] FIG. 1 is a diagram showing the change in relative density when Ramping Flash is applied to high-speed sintering. [Figure 4] FIG. 1 shows the behavior of specimen current in ICEFAST and a general flash sintering method. [Diagram 5] FIG. 13 is a diagram showing the change in relative density in the process of producing a sintered body from each sample. [Figure 6] 1 is a diagram showing a schematic configuration of a manufacturing apparatus for a sintered body according to an embodiment; [Figure 7] FIG. 7(a) is a scanning electron microscope photograph of the center part of a sintered body produced by the flash sintering method, and FIG. 7(b) is a scanning electron microscope photograph of the outer periphery of a sintered body produced by the flash sintering method. [Figure 8] FIG. 8(a) is a scanning electron microscope photograph of the center part of a sintered body produced by Rate Control Flash, and FIG. 8(b) is a scanning electron microscope photograph of the outer periphery of a sintered body produced by Rate Control Flash. [Figure 9] FIG. 2 is a transmission electron microscope photograph of a sintered body produced by Rate Control Flash and a result of a composition analysis of yttrium in a specified region. [Figure 10] FIG. 10(a) is a transmission electron microscope photograph shown in FIG. 9, FIG. 10(b) is a diagram showing mapping of zirconium elements by EDS (Energy Dispersive X-ray spectroscopy) in the region shown in FIG. 10(a), and FIG. 10(c) is a diagram showing mapping of yttrium elements by EDS in the region shown in FIG. 10(a). [Figure 11]13 is a graph showing the relationship (line L12) between the linear shrinkage rate of a sample and the furnace temperature when the sample is produced by a flash sintering method after calcination in the production method according to the third embodiment. [Figure 12] FIG. 2 is a schematic diagram for explaining particle rearrangement and non-uniform neck formation during the calcination stage. [Figure 13] 13 is a graph showing a change in linear shrinkage rate in a production method according to a fourth embodiment. [Figure 14] 13 is a graph showing a change in sample current in a manufacturing method according to a fourth embodiment. [Figure 15] FIG. 13 is a diagram showing changes in linear shrinkage rate in the process of producing sintered bodies from the samples according to the fifth embodiment. [Figure 16] FIG. 1 is a diagram showing changes in specimen current due to a conventional flash sintering method and a Rate Control Flash. [Figure 17] FIG. 2 is a perspective view showing an outline of a rectangular parallelepiped ceramic powder compact provided between a pair of electrodes. [Figure 18] FIG. 1 is a diagram showing the change in relative density when a DC electric field and an AC electric field having the same electric field magnitude are applied in a flash sintering method. [Figure 19] FIG. 13 is a diagram showing the change in relative density when the frequency of an AC electric field is changed at the same electric field and the same limiting current value. [Figure 20] FIG. 13 is a diagram showing a change in relative density when AC electric fields having different frequencies and limiting current values ​​are applied. [Figure 21] FIG. 13 is a graph showing the change in relative density when a DC electric field is applied to ceramic powder samples having different cross-sectional areas. [Figure 22] FIG. 13 is a graph showing the change in relative density when an AC electric field is applied to ceramic powder compact samples having different cross-sectional areas. [Figure 23] FIG. 1 is a diagram for qualitatively explaining the relationship between the electric field and the specimen current in the flash phenomenon. [Figure 24] FIG. 13 is a diagram showing an example of voltage and current waveforms of AC control in the method for producing a sintered body according to the sixth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] A method for producing a sintered body according to an embodiment of the present disclosure is a method for producing a sintered body by heating a ceramic compact while applying an electric field to the ceramic compact, the method controlling the current flowing through the ceramic compact so as to keep the sintering rate constant.

[0012] According to this embodiment, it is possible to produce a sintered body with a high density in a relatively short time, which is difficult to achieve by the conventional flash sintering method alone. The sintering speed only needs to be constant for at least a predetermined time after the current flowing through the ceramic compact reaches a predetermined current value. In other words, the sintering speed does not need to be constant throughout the entire time that the ceramic compact is heated while an electric field is applied to it.

[0013] Another aspect of the present disclosure is also a method for producing a sintered body, which comprises increasing the temperature of a ceramic compact while applying an electric field to the ceramic compact, and controlling a current flowing through the ceramic compact according to a current profile determined to produce a ceramic sintered body having a density greater than a predetermined value.

[0014] According to this embodiment, it is possible to manufacture a sintered body with a high density, which is difficult to achieve by the conventional flash sintering method alone, in a comparatively short time.

[0015] Yet another embodiment of the present disclosure is also a method for producing a sintered body, which includes a first step of raising the temperature of the ceramic compact while applying a first electric field to the ceramic compact up to a flash sintering temperature at which a current flowing through the ceramic compact increases rapidly when the ceramic compact is heated while an electric field is applied to the ceramic compact, and a second step of raising the temperature while applying a second electric field smaller than the first electric field after the current flowing through the ceramic compact increases rapidly and reaches a predetermined current value.

[0016] According to this embodiment, it is possible to manufacture a sintered body with a high density, which is difficult to achieve by the conventional flash sintering method alone, in a comparatively short time.

[0017] The raw powder of the ceramic green compact may be composed mainly of zirconium oxide.

[0018] Yet another aspect of the present disclosure is an apparatus for producing a sintered body, the apparatus including: a heater for heating a ceramic compact, electrodes for applying a voltage to the ceramic compact, a voltage application unit for applying a voltage to the electrodes so that a predetermined current flows through the ceramic compact, a storage unit for storing a current profile determined to produce a ceramic sintered body having a density greater than a predetermined value, and a control unit for controlling the voltage application unit based on the current profile while raising the temperature of the ceramic compact with the heater.

[0019] According to this embodiment, by storing a current profile calculated in advance from experiments or calculations in the storage unit, it is possible to manufacture a ceramic sintered body having a density higher than a predetermined value without feedback control. Therefore, a detection device or a calculation device for grasping the sintering rate for feedback control is not required, and the device can be simplified.

[0020] A further embodiment of the present disclosure provides a method for producing a sintered body, which involves raising the temperature while applying an AC electric field to a ceramic compact of a predetermined shape placed between a pair of electrodes, and includes a first step of raising the temperature while applying a first AC electric field to the ceramic compact up to a flash sintering temperature at which the current flowing through the ceramic compact increases rapidly, and a second step of raising the temperature while applying a second AC electric field smaller than the first AC electric field after the current flowing through the ceramic compact increases rapidly and reaches a predetermined current value.

[0021] According to this embodiment, a sintered body with a high density, which is difficult to achieve by the conventional flash sintering method alone, can be manufactured with a relatively low power.

[0022] In the first step, the application of the first AC electric field may be performed in a voltage control mode, and in the second step, the application of the second AC electric field may be performed in a current control mode. This allows the current to be controlled so as not to exceed a predetermined current value after the flash phenomenon occurs, thereby reducing the possibility of the electrode melting due to the application of excessive power to the sample. Note that, in the second step, the application of the second AC electric field may be performed in a power control mode so as not to exceed a predetermined power value.

[0023] When it is detected that the current flowing through the ceramic powder compact has reached a predetermined current value, the control mode may be switched from the voltage control mode to the current control mode so that the current does not exceed the predetermined current value.

[0024] The first and second AC electric fields may have a frequency of 10 Hz or more, which can further increase the density of the sintered body.

[0025] In addition to being easily sintered, it is also important that the ceramic green compact has a practical shape after sintering. Therefore, the ceramic green compact of a predetermined shape may be a rectangular parallelepiped or a columnar shape.

[0026] The raw powder of the ceramic green compact may be composed mainly of zirconium oxide.

[0027] Yet another aspect of the present disclosure is an apparatus for manufacturing a sintered body. The apparatus includes a heater for heating a ceramic compact having a predetermined shape, a pair of electrodes for applying a voltage to the ceramic compact, a voltage application unit for applying a voltage to the pair of electrodes, and a control unit for controlling the voltage application unit while raising the temperature of the ceramic compact with the heater. The control unit voltage-controls the voltage application unit until a current flowing through the ceramic compact increases rapidly, and then current-controls the voltage application unit after the current flowing through the ceramic compact increases rapidly and reaches a predetermined current value.

[0028] According to this embodiment, even with a relatively low power that does not melt the electrodes, it is possible to produce a sintered body with a high density that is difficult to achieve by the conventional flash sintering method alone.

[0029] The control unit may have a detection unit that detects a current flowing through the ceramic powder compact. When the detection unit detects a predetermined current value, the control unit may transition from a voltage control mode controlled by the voltage application unit to a current control mode so that the current does not exceed the predetermined current value.

[0030] Any combination of the above components and conversion of the present disclosure into a method, device, system, etc. are also valid aspects of the present disclosure.

[0031] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the drawings. In the description of the drawings, the same elements are given the same reference numerals, and duplicated descriptions are omitted as appropriate. In addition, the configurations described below are examples, and do not limit the scope of the present disclosure in any way.

[0032] The method for producing a sintered body according to the present disclosure is a technique that allows production at a temperature range lower than the temperature range used in general sintering methods and that can significantly shorten the production time. The following points are particularly noted.

[0033] The densification achieved at lower temperatures and in a shorter time by flash sintering is largely due to the increase in the actual temperature of the ceramic powder compact caused by the Joule heat generated during the flash phenomenon.

[0034] As the applied electric field becomes stronger, the flash temperature becomes lower. The stronger the electric field, the more Joule heat can be input during the flash phenomenon, but on the other hand, the flash temperature decreases, so the heating effect from the electric furnace decreases.

[0035] The present inventors have focused on these facts and conducted extensive research to realize a high-density sintered body, which is difficult to achieve using conventional flash sintering methods alone, and have come up with several new methods for manufacturing a sintered body.

[0036] [First embodiment] The method for producing a sintered body according to the first embodiment is a technique for performing flash sintering while controlling the amount of limited current to keep the sintering rate constant. This technique adjusts the densification rate of the green compact to a constant rate while controlling the steep increase in the sample current that occurs during flash sintering, thereby improving the final density. By using the method for producing a sintered body according to the present embodiment, it is possible to suppress the non-uniformity of the densification state and structure caused by the too steep densification behavior that occurs during general flash sintering, and as a result, the final density can be improved. Hereinafter, the name of this method is referred to as Rate Control Flash.

[0037] (Method of manufacturing sintered body) In the manufacturing method of the sintered body according to the present embodiment, zirconia (ZrO2) powder (TZ-3Y: manufactured by Tosoh Corporation, hereinafter sometimes referred to as "3YSZ") in which 3 mol% of yttria (Y2O3) was uniformly dispersed and solid-solved was used as the ceramic raw material powder. This raw material powder was compressed, and a rectangular parallelepiped sample (ceramic powder compact) with a length of 15 mm and a cross-sectional shape of 3.5 mm x 3.5 mm was produced by uniaxial and isostatic pressing. After the sample was molded, platinum (Pt) foil was fixed as an electrode to both longitudinal end faces of the sample using Pt paste.

[0038] Next, the sample with the electrodes fixed was placed in a differential thermal dilatometer (Thermo plus EVO2 TMA8301: manufactured by Rigaku Corporation) that had been modified to allow connection to DC and AC power sources. The sample was then heated in a furnace while an electric field was applied to it.

[0039] Fig. 1 shows the change in linear shrinkage during the process of producing sintered bodies from each sample, and Fig. 2 shows the change in sample current due to the conventional flash sintering method and the Rate Control Flash.

[0040] Line L1 (Comparative Example 1) in Figure 1 shows the change in linear shrinkage over time in the conventional flash sintering method. As shown by line L1, in the conventional flash sintering method, when the temperature is raised while an electric field of a certain strength is applied to the sample, the current flowing through the sample increases rapidly as the temperature approaches the flash sintering temperature (see line L1 in Figure 2), and sintering is completed in a short time. However, the linear shrinkage of the obtained sintered body is about 18%, which leaves room for improvement.

[0041] On the other hand, lines L2, L2', L3, and L4 (Example 1, Example 1', Example 2, and Example 3) show the change in linear shrinkage over time in the Rate Control Flash. In the Rate Control Flash, for example, an electric field of 100 V / cm is applied to the sample, and when the temperature approaches the flash sintering temperature in that electric field, the sample current rises rapidly. At that time, when the sample current reaches the initial current limit value of 100 mA, the sample current is increased to 1200 mA while being controlled so that the sintering speed (linear shrinkage) thereafter becomes constant (see FIG. 2). Note that the initial current limit value does not necessarily have to be 100 mA, and a lower value is preferable.

[0042] The samples according to Example 1, Example 1', Example 2, and Example 3 shown by lines L2, L2', L3, and L4 have different speeds (sintering speeds) at which the current is increased after the initial limiting current value is reached. As shown by lines L2, L2', L3, and L4 in FIG. 1, it can be seen that the sintered bodies according to Example 1, Example 1', Example 2, and Example 3 produced by Rate Control Flash have a much higher density than the sintered body according to Comparative Example 1 produced by normal flash sintering. In particular, the sintered body according to Example 1' shown by line L2' has the highest density among the examples.

[0043] The fact that the sintering speed of Rate Control Flash is constant can be confirmed by the fact that the time-dependent change in linear shrinkage rate in Figure 1 is almost linear (constant). Here, the constant sintering speed does not require mathematical rigor, and a certain degree of error or deviation or amplitude due to control delay does not impair the essence of the invention. For example, if the slope of each line showing the time-dependent change in linear shrinkage rate (relative density) is within a range of about ±50% of the center value, the sintering speed can be considered constant.

[0044] In this way, the method for producing a sintered body according to the first embodiment does not control the increasing rate of the sample current to a constant value, but controls the sample current flowing through the ceramic powder compact so as to keep the sintering rate constant. With this type of control, it can be seen that the current increases gradually as shown by lines L2 to L4, rather than a steep increase as shown by line L1 in FIG. 2.

[0045] In other words, the method for producing a sintered body according to the first embodiment can be said to be a method for controlling the current flowing through the ceramic powder compact according to a current profile determined to produce a ceramic sintered body having a density greater than a predetermined value (e.g., a relative density of 90% or more and a linear shrinkage rate of 20% or more). Here, the current profile indicates, for example, a relationship between current application time and sample current calculated by experiments or theoretical verification, and may be stored in advance in a semiconductor memory or the like of the current control unit. In this case, it is not necessary to obtain information on the time change in the linear shrinkage rate and feedback control the sample current, and it is possible to omit a detection unit for detecting the linear shrinkage rate, simplifying the control system.

[0046] As described above, according to the method for producing a sintered body according to the present embodiment, a sintered body with a high density, which is difficult to achieve by the conventional flash sintering method alone, can be produced in a relatively short time.

[0047] Next, in the case where the sintering rate cannot be made constant as in the case of Rate Control Flash, the current increase rate during flash sintering may be made constant. This flash sintering method is called Ramping Flash. A modified example in which Ramping Flash is applied to high-speed sintering will be described. FIG. 3 is a diagram showing the change in relative density when Ramping Flash is applied to high-speed sintering. In the manufacturing method according to the modified example, the temperature is rapidly increased at a rate of 50°C / min, the electric field is AC 30V / cm, 100Hz, the sample current is 100mA to 1000mA, and the final furnace temperature is about 1200°C. Generally, sintering of zirconia ceramic (3YSZ) takes several hours at a temperature of about 1500°C, but in the manufacturing method according to the modified example, the relative density is almost 100% in only about 30 minutes from the start of temperature increase of the ceramic powder compact to the end of sintering.

[0048] [Second embodiment] The method for producing a sintered body according to the second embodiment is one of the flash sintering techniques that promotes the initial formation of necks and promotes further densification. In this production method, a high electric field is applied in the early stage of sintering, and the green compact is heated for a moment by Joule heating, forming necks (contact parts) between ceramic powder particles. If the electric field is continued to be applied in this state (this state is the same as in general flash sintering), the flash phenomenon progresses at a low temperature, and the final density achieved is low.

[0049] In order to prevent this, the main feature of the manufacturing method according to the present embodiment is that the electric field is lowered and sintering is performed immediately after the flash phenomenon occurs. Hereinafter, this method will be called ICEFAST.

[0050] Figure 4 shows the behavior of the specimen current in ICEFAST and in a general flash sintering method. The sintering conditions for ICEFAST (line L5) shown in Figure 4 are as follows. First, the temperature is raised with an AC of 100 V / cm and a limiting current value of 100 mA. A current spike is observed at the flash temperature (approximately 800°C) when the specimen temperature is at an electric field of 100 V / cm. This temperature coincides with the flash temperature during general flash sintering under conditions where 100 V / cm is applied. Therefore, the specimen current tries to increase significantly, but since the limiting current value is set to 100 mA in advance, the flash phenomenon is limited to this current value.

[0051] In other words, because ICEFAST limits the specimen current at the flash temperature to 100mA, the specimen current does not increase significantly as it does in general flash sintering. When this flash phenomenon occurs, the applied electric field is reduced to 30V / cm and the temperature is continued to rise. Lines L6 and L7 in Figure 4 show the behavior of the specimen current in the conventional flash sintering method when the electric fields are 30V / cm and 40V / cm.

[0052] FIG. 5 is a diagram showing the change in relative density in the process of producing sintered bodies from each sample. FIG. 5 shows sintering curves of general sintering (line L11: Comparative Example 7), general flash sintering (lines L6 to L10: Comparative Examples 2 to 6), and ICEFAST (line L5: Example 4).

[0053] First, in the normal sintering of Comparative Example 7, even when the temperature is raised to about 1300°C, the relative density is about 70%, whereas in the general flash sintering (Comparative Examples 2 to 6), the achieved density is improved at all electric fields. It can also be seen that the flash temperature shifts to the lower temperature side as the applied electric field increases. In the general flash sintering, the achieved density decreases despite the applied electric field being high, which is due to the difference in flash temperature. It can be seen from this comparison that even if the Joule heating amount is high, the achieved density obtained does not necessarily become high due to the influence of the furnace temperature.

[0054] In contrast, ICEFAST at 30 V / cm (Example 4) includes a first step of heating the ceramic compact while applying an electric field of 100 V / cm to the ceramic compact up to the flash sintering temperature (approximately 800°C) at which the current flowing through the ceramic compact increases rapidly when the ceramic compact is heated while an electric field is applied thereto, and a second step of heating the ceramic compact while applying an electric field of 30 V / cm, which is smaller than the electric field of 100 V / cm, after the current flowing through the ceramic compact increases rapidly and reaches a predetermined limiting current value of 100 mA.

[0055] As a result, the manufacturing method according to the present embodiment makes it possible to manufacture, in a comparatively short period of time, a sintered body with a high density that is difficult to achieve using only the conventional flash sintering method.

[0056] [Sintered body manufacturing equipment] A manufacturing apparatus suitable for the manufacturing method of the sintered body according to each of the above-mentioned embodiments will be described in more detail. Fig. 6 is a diagram showing a schematic configuration of the manufacturing apparatus of the sintered body according to the embodiment. The manufacturing apparatus 10 includes an apparatus main body 14 having an electric furnace 12 for raising the temperature when sintering the ceramic green compact, and a control system 16 for controlling each setting parameter in the manufacturing process in the apparatus main body 14.

[0057] The apparatus main body 14 includes a heater 12a used in the electric furnace 12, a sample 18 made of a ceramic compact, a sample stage 20 on which the sample 18 is placed, electrodes 22 arranged on both ends of the sample 18 for applying a voltage to the sample 18, a rod 24 that moves in response to a change in the volume of the ceramic compact, and a detector 26 that detects the length (density) of the sample 18 from the movement of the rod 24. For example, a thermal dilatometer is used as the detector 26.

[0058] The control system 16 includes a first arithmetic unit 28 that acquires information correlated with the length (density) of the sample 18 from the detector 26 via a signal line S1 and calculates a control signal for controlling the output of the heater 12a via a signal line S2 based on the information, a power source 30 that applies a voltage between the pair of electrodes 22 and controls the current flowing through the sample 18 via a signal line S3, and a second arithmetic unit 32 that calculates the rate of contraction of the sample 18 based on the information acquired from the detector 26 via a signal line S4. The first arithmetic unit 28 and the second arithmetic unit 32 are, for example, personal computers having a storage unit such as a semiconductor memory.

[0059] The second calculation device 32 controls the voltage and current value applied to the ceramic powder compact via signal line S5 using the power supply 30 based on the calculated shrinkage rate (sintering rate), and further controls the output of the electric furnace 12 in the apparatus main body 14 by the first calculation device 28 via signal line S6.

[0060] The manufacturing apparatus 10 according to the present embodiment can manufacture a ceramic sintered body having a higher density than the conventional one by using the above-mentioned feedback control. In addition, when manufacturing a ceramic sintered body, information on a current profile to be passed through the sample 18 and an appropriate temperature rise profile (temperature rise rate) by heating the sample 18 is created, and these profiles can be stored in the memory of each computing device.

[0061] Specifically, while raising the temperature of the ceramic powder compact with the heater of the electric furnace 12, a voltage is applied to the ceramic powder compact using the power supply 30, the length of the ceramic powder compact is detected with the detector 26, and the current flowing through the sample 18 is measured by the power supply 30. At this time, the change in the length of the sample 18 over time (shrinkage rate) is stored in the memory unit.

[0062] When the current value of the sample 18 starts to increase and the shrinkage speed of the sample 18 starts to increase, the second calculation device 32 controls the limit value of the current flowing through the sample 18 using the power source 30, or controls the voltage value, or controls the power value based on the data so that the shrinkage speed becomes constant. Furthermore, the output of the electric furnace 12 is controlled using the first calculation device 28.

[0063] As described above, the sintered body manufacturing apparatus 10 of this embodiment includes a heater 12a that heats the ceramic compact, an electrode 22 for applying a voltage to the ceramic compact, a power source 30 that applies a voltage to the electrode 22 so that a predetermined current flows through the ceramic compact, a memory unit that stores a current profile determined to produce a ceramic sintered body having a density greater than a predetermined value, and a first arithmetic unit 28 and a second arithmetic unit 32 that control the voltage application unit based on the current profile while raising the temperature of the ceramic compact with the heater 12a.

[0064] As a result, when a ceramic sintered body is manufactured by the manufacturing apparatus 10, the shrinkage rate of the sample 18 during manufacturing, the temperature of the sample 18, the voltage, current, power applied to the sample 18, the output of the electric furnace, the temperature, etc. are recorded in the memory of the first calculation device 28, the power source 30 and the second calculation device 32.

[0065] In this way, by storing a current profile calculated in advance from experiments or calculations in the memory unit, it is possible to manufacture a ceramic sintered body having a density higher than a predetermined value without feedback control. Therefore, a detection device or a calculation device for grasping the sintering rate for feedback control is not required, and the device can be simplified.

[0066] Therefore, by using each profile stored in the storage unit, the manufacturing apparatus 10 can manufacture a ceramic sintered body having a density higher than a predetermined value based on each profile without feedback control thereafter. Alternatively, by using each profile stored in the storage unit in another manufacturing apparatus, even a simple manufacturing apparatus that does not have a configuration for feedback control can manufacture a ceramic sintered body having a density higher than a predetermined value.

[0067] [Structure of sintered body produced by Rate Control Flash] Next, the influence of differences in manufacturing methods on the structure and composition of sintered bodies will be described. Fig. 7(a) is a scanning electron microscope photograph of the center of a sintered body manufactured by the flash sintering method, and Fig. 7(b) is a scanning electron microscope photograph of the outer periphery of a sintered body manufactured by the flash sintering method. Fig. 8(a) is a scanning electron microscope photograph of the center of a sintered body manufactured by Rate Control Flash, and Fig. 8(b) is a scanning electron microscope photograph of the outer periphery of a sintered body manufactured by Rate Control Flash.

[0068] The structure of the center of the sintered body produced by the flash sintering method has a relatively large average crystal grain size d of 2.25 μm, as shown in the photograph of Figure 7(a).On the other hand, the structure of the outer periphery of the sintered body produced by the flash sintering method has an average crystal grain size d of 1.25 μm, as shown in the photograph of Figure 7(b), which is about 55% smaller than the crystal grain size in the center.

[0069] In contrast, the structure of the center of the sintered body produced by Rate Control Flash has an extremely small average crystal grain size d of 0.60 μm, as shown in the photograph of Figure 8(a). The structure of the outer periphery of the sintered body produced by Rate Control Flash has an average crystal grain size d of 0.58 μm, as shown in the photograph of Figure 8(b), which is almost the same as the crystal grain size in the center. In other words, the crystal grain size of the sintered body produced by Rate Control Flash is extremely fine and uniform throughout the sintered body.

[0070] Next, the composition distribution of the sintered body will be described. Fig. 9 is a transmission electron microscope photograph of the sintered body produced by Rate Control Flash and a diagram showing the results of a composition analysis of yttrium in a predetermined region. Fig. 10(a) is a transmission electron microscope photograph shown in Fig. 9, Fig. 10(b) is a diagram showing zirconium element mapping by EDS (Energy Dispersive X-ray Spectroscopy) in the region shown in Fig. 10(a), and a diagram showing yttrium element mapping by EDS in the region shown in Fig. 10(a).

[0071] In the photograph in Figure 9, "4_Y 5.49", "5_Y 6.41", "6_Y 5.45", "7_Y 6.60", "8_Y 6.40", "9_Y 6.22", "10_Y 5.30", "11_Y 7.08", "12_Y 5.35", "13_Y 6.10", "14_Y 6.65", and "15_Y 6.37" are the EDS analysis results of the yttrium (Y) composition [at%] in the polycrystalline structure of the entire field of view shown in the photograph, and indicate that the analysis was performed 12 times. The average value is 6.12 [at%], which is equivalent to 3.06 [mol%] in Y2O3 conversion. Therefore, it can be seen that the composition of the sample shown in Figure 9 is almost identical to that of zirconia (ZrO2) with 3 mol% yttria (Y2O3) dissolved therein as raw material powder. Also, as shown in Figures 10(b) and 10(c), it can be seen that there is very little bias in the distribution of zirconium and yttrium in the region of the photograph shown in Figure 10(a).

[0072] As described above, the sintered body produced by Rate Control Flash has extremely high uniformity in crystal grain size and composition, and can achieve density and properties that are difficult to achieve with conventional manufacturing methods.

[0073] [Third embodiment] The manufacturing method according to the third embodiment is a method in which calcination is performed once in the initial sintering process (for example, in the case of 3YSZ, sintering starts at a temperature range of about 800 to 1200°C) which affects the final density of the sintered body, and then the temperature is lowered to a low temperature and a sintered body is manufactured by a flash sintering method. Fig. 11 is a graph showing the relationship between the linear shrinkage rate of a sample and the furnace temperature (line L12) when the sample is manufactured by the flash sintering method after the calcination by the manufacturing method according to the third embodiment.

[0074] Specifically, the 3YSZ powder compact is heated to a temperature at which sintering begins (1200°C in this embodiment), and the heated 3YSZ powder compact is cooled to a predetermined temperature or lower without being particularly maintained at that temperature. Here, the predetermined temperature or lower is, for example, a flash sintering temperature or lower, which is 780°C or lower in this embodiment. Next, the cooled 3YSZ powder compact is heated while a predetermined electric field (100 V / cm, 100 Hz) is applied thereto.

[0075] As a result, as shown by line L12 in Fig. 11, the linear shrinkage at the flash sintering temperature is significantly improved compared to the sintered body produced only by the flash sintering method (line L13). As a result, the sintered body produced by the production method according to the present embodiment exhibits a very high relative density of 99.6%.

[0076] The reason why such a high density sintered body was obtained is thought to be that the calcination stage provides time for the rearrangement of the raw material powder that occurs in the early sintering process and the unevenness of the neck formation between particles to be eliminated. Figure 12 is a schematic diagram to explain the rearrangement of particles and the uneven neck formation at the calcination stage.

[0077] As shown in the left diagram of Figure 12, when the raw powder is simply compressed, multiple particles P are caught together, forming large voids V1 inside. This state of multiple particles P being caught together is sometimes called bridging. When the powder is calcined at a temperature of around 1000°C in this state, the surface diffusion of the particles P becomes significant, and the particles P gradually change their positions as shown in the right diagram of Figure 12. As a result, the bridging is released, and the previously large voids V1 become small voids V2, which is thought to be one of the reasons for the high density of the sintered body. In addition, the neck formation that occurs in the early stage of sintering occurs uniformly, and as a result, the formation of voids larger than the particle diameter is suppressed.

[0078] [Fourth embodiment] One of the features of the manufacturing method according to the fourth embodiment is that the calcination step according to the third embodiment is implemented by the Rate Control Flash. For example, the manufacturing method of a sintered body according to the present embodiment includes a heating step of heating the ceramic compact to a predetermined temperature, an application step of applying a predetermined electric field to the ceramic compact until the predetermined temperature is reached, a first current control step of controlling the current flowing in the ceramic compact so that the sintering rate becomes constant after the current flowing in the ceramic compact reaches a first current value in the electric field application step, and a second current control step of increasing the current flowing in the ceramic compact to a second current value higher than the first current value after the first current control step is performed for a predetermined time.

[0079] Fig. 13 is a graph showing the change in linear shrinkage rate in the manufacturing method according to the fourth embodiment. Fig. 14 is a graph showing the change in sample current in the manufacturing method according to the fourth embodiment. The times (t1, t2, t3) on the horizontal axes in Fig. 13 and Fig. 14 correspond to the same time.

[0080] Next, a specific example of the manufacturing method according to the fourth embodiment will be described. First, the 3YSZ powder compact is heated at a heating rate of 300°C / h, and when the temperature reaches about 780°C (time t1), an AC electric field of 100V / cm, 100Hz is applied. At this point, the sample current momentarily rises to 100mA (this value is the preset limiting current value). Next, at time t2, a Rate Control Flash is performed for about 5 minutes (until time t3) so that the sintering speed becomes constant. After that, at time t3, the limiting current value is suddenly raised to 1200mA. As a result, the sintered body manufactured by the manufacturing method according to the present embodiment becomes a sintered body with a very high density.

[0081] [Fifth embodiment] In the manufacturing method of the sintered body according to the present embodiment, zirconia (ZrO2) powder (TZ-8Y: manufactured by Tosoh Corporation, hereinafter sometimes referred to as "8YSZ") in which 8 mol% of yttria (Y2O3) is uniformly dispersed and solid-solved is used as the ceramic raw material powder. Below, the conditions different from the first embodiment are mainly described.

[0082] Fig. 15 is a diagram showing the change in linear shrinkage rate during the process of producing a sintered body from each sample, and Fig. 16 is a diagram showing the change in sample current due to the conventional flash sintering method and the Rate Control Flash.

[0083] Line L14 (Comparative Example 8) in Fig. 15 shows the change in linear shrinkage over time in the conventional flash sintering method. As shown by line L14, in the conventional flash sintering method, when the temperature is raised while an electric field of a certain strength is applied to the sample, the current flowing through the sample increases rapidly as the temperature approaches the flash sintering temperature (see line L14 in Fig. 16), and sintering is completed in a short time. However, the relative density of the obtained sintered body is about 80%, leaving room for improvement.

[0084] On the other hand, lines L15, L16, and L17 (Examples 5, 6, and 7) show the change in linear shrinkage rate over time in Rate Control Flash. In Rate Control Flash, for example, an electric field of 50 V / cm is applied to the sample, and when the temperature approaches the flash sintering temperature in that electric field, the sample current rises rapidly. At that time, when the sample current reaches the initial current limit value of 100 mA, the sample current is increased to 1200 mA while being controlled so that the sintering speed thereafter becomes constant (see FIG. 16). Note that the initial current limit value does not necessarily have to be 100 mA, and a lower value is preferable.

[0085] The samples according to Example 5, Example 16, and Example 7 shown by lines L15, L16, and L17 have different speeds (sintering speeds) at which the current is increased after the initial limiting current value is reached. Specifically, the sintering speed (linear shrinkage rate) of Example 5 is 200 μm / min, that of Example 6 is 120 μm / min, and that of Example 7 is 60 μm / min. As shown by lines L15, L16, and L17 in FIG. 16, it can be seen that the sintered bodies according to Examples 15, 16, and 17 manufactured by Rate Control Flash have a much higher density than the sintered body according to Comparative Example 8 manufactured by normal flash sintering.

[0086] Furthermore, it can be confirmed that the sintering speed of Rate Control Flash is constant because the change in relative density over time in FIG. 16 is almost linear (constant).

[0087] [Sixth embodiment] The important factor for the shape of the sintered body produced in research and experiments is that it is easy to produce, and practical shapes are often not taken into consideration. However, when considering practicality of the produced sintered body, a rectangular parallelepiped or columnar shape is preferable. Figure 17 is a perspective view showing the outline of a rectangular parallelepiped ceramic powder compact placed between a pair of electrodes.

[0088] Sample 18 made of a ceramic compact shown in Fig. 17 is a rectangular parallelepiped with length D [mm] × width W [mm] × height H [mm], and a pair of electrodes 22 is provided at both ends in the height direction. In this case, since the electrode 22 for applying an electric field is in contact with the end face of sample 18 made of a ceramic compact, if the heat resistance of this part is low, the amount of power that can be input to sample 18 is limited. For this reason, a technology is required that can increase the final density of the sintered body with a low input power that does not melt the electrodes.

[0089] The method for producing a sintered body according to the present disclosure can produce a sintered body with a lower input power than that used in a general sintering method, and can also reduce melting of the electrodes. In particular, the use of an AC electric field in the flash sintering method makes it possible to produce a sintered body with a higher sintering density than when a DC electric field is used.

[0090] The present inventors have focused on these facts and conducted extensive research to realize a high-density sintered body, which is difficult to achieve using conventional flash sintering methods alone, and have come up with a new method for manufacturing a sintered body.

[0091] (Method of manufacturing sintered body) In the manufacturing method of the sintered body according to the sixth embodiment, zirconia (ZrO2) powder (TZ-3Y: manufactured by Tosoh Corporation, hereinafter sometimes referred to as "3YSZ") in which 3 mol% of yttria (Y2O3) was uniformly dispersed and solid-solved was used as the ceramic raw material powder. This raw material powder was compressed, and a rectangular parallelepiped sample (ceramic compact) with a length of 15 mm and a cross-sectional shape of 7 mm x 7 mm was produced by uniaxial and isostatic pressing. After the sample was molded, platinum (Pt) foil was fixed as an electrode to both longitudinal end faces of the sample using Pt paste.

[0092] Next, the sample with the electrodes fixed was placed in a differential thermal dilatometer (Thermo plus EVO2 TMA8301: manufactured by Rigaku Corporation) that had been modified to allow connection to DC and AC power sources. The sample was then heated in a furnace while an electric field was applied to it.

[0093] In sample 18 shown in FIG. 17, Pt foil is in direct contact with the ceramic compact as the electrode 22. Therefore, the amount of power that can be input when applying an electric field is limited to a range that does not exceed the temperature at which the metal (Pt) used for the electrode melts. Therefore, the inventors of the present application focused on AC electric fields. In the following, an example will be described in which the raw material powder of the ceramic compact is mainly composed of zirconium oxide, but it goes without saying that the manufacturing method of the sintered body disclosed herein can also be applied to sintered bodies made of raw material powders of other compounds.

[0094] (Differences in the effects of DC and AC electric fields) FIG. 18 is a diagram showing the change in relative density when a DC electric field and an AC electric field of the same electric field magnitude are applied in the flash sintering method. Line L1 in FIG. 18 shows the change in relative density over time in the flash sintering method when an AC electric field (50 V / cm, 1 Hz, limited current value 900 mA) is applied. Line L2 shows the change in relative density over time in the flash sintering method when a DC electric field (50 V / cm, limited current value 900 mA) is applied. The cross section of the sample has a length D of 7 mm and a width W of 7 mm. Unless otherwise specified below, the samples have the same cross section size.

[0095] As shown in Figure 18, the relative density is high when an AC electric field is applied (line L1). The reason for this is thought to be as follows. When a DC electric field is applied, ion flow occurs in one direction, so that the ceramic powder compact closest to the negative electrode of the pair of electrodes is strongly reduced, and nitriding may also occur in the atmosphere, severely impeding densification. Furthermore, the sample shape becomes non-uniform (deformed). On the other hand, when an AC electric field is applied, there is no bias in the ion flow as with a DC electric field, so densification proceeds more uniformly.

[0096] Here, in the case of a DC electric field, if a higher power is applied to the sample 18 in order to improve the ultimate density of the sintered body, the Pt foil used for the electrode 22 may melt. Therefore, a high ultimate density cannot be obtained with a DC electric field. The tendency for melting becomes more pronounced as the cross-sectional area of ​​the ceramic green compact increases.

[0097] (Effect of AC electric field frequency on attained density) Fig. 19 is a diagram showing the change in relative density when the frequency of the AC electric field is changed at the same electric field and the same limiting current value. Lines L3 to L6 shown in Fig. 19 are for frequencies of 1 Hz, 10 Hz, 100 Hz, and 1000 Hz, respectively. As can be seen from Fig. 19, the attained density increases as the frequency of the AC electric field increases.

[0098] (Frequency dependence of AC electric field on the amount of power that can be input to improve the transmission density) In order to improve the density of the sintered body, it is necessary to input a higher power. However, when using a rectangular ceramic powder compact as shown in Figure 17, the amount of power is limited so that the temperature range does not melt the electrodes.

[0099] Therefore, the inventors of the present application found that in the case of an AC electric field, a higher frequency allows for higher power input while suppressing melting of the electrodes. FIG. 20 is a diagram showing the change in relative density when AC electric fields with different frequencies and limiting current values ​​are applied. Line L7 shows the case where an AC electric field with a frequency of 10 Hz and a limiting current value of 900 mA is applied, and the relative density is less than 85%. When an AC electric field with a frequency of 10 Hz and a limiting current value of 1000 mA is applied, the electrodes melt and sufficient sintering cannot be performed. On the other hand, when an AC electric field with a frequency of 1000 Hz and a limiting current value of 900 mA is applied (line L8), the relative density of the sintered body exceeds 85%. When an AC electric field with a frequency of 1000 Hz and a limiting current value of 1100 mA is applied (line L9), the electrodes do not melt and the input power can be increased, resulting in a relative density of the sintered body exceeding 90%. In this way, in samples in which electrodes are in contact with a rectangular ceramic powder compact, by using an AC electric field with a higher frequency, it is possible to input higher power, thereby improving the achieved density of the sintered body.

[0100] (Effect of cross-sectional area of ​​ceramic powder compact) It was found that the behavior of the specimen current in the flash sintering method depends on the cross-sectional area of ​​the ceramic compact. Figure 21 shows the change in relative density when a DC electric field is applied to ceramic compact specimens with different cross-sectional areas. Line L10 shows the change in relative density when a DC electric field of 50 V / cm and a limited current value of 900 mA is applied to a specimen with a cross-sectional area of ​​7 x 7 mm, line L11 shows the change in relative density when a DC electric field of 50 V / cm and a limited current value of 816 mA is applied to a specimen with a cross-sectional area of ​​5 x 5 mm, and line L12 shows the change in relative density when a DC electric field of 50 V / cm and a limited current value of 400 mA is applied to a specimen with a cross-sectional area of ​​3.5 x 3.5 mm. From these results, it can be seen that the flash temperature decreases as the cross-sectional area increases.

[0101] 22 is a diagram showing the change in relative density when an AC electric field is applied to ceramic powder compact samples with different cross-sectional areas. Line L13 shows the change in relative density when an AC electric field of 50 V / cm, frequency 10 Hz, and limited current value 900 mA is applied to a sample with a cross-sectional area of ​​7×7 mm, line L14 shows the change in relative density when an AC electric field of 50 V / cm, frequency 10 Hz, and limited current value 816 mA is applied to a sample with a cross-sectional area of ​​5×5 mm, and line L15 shows the change in relative density when an AC electric field of 50 V / cm, frequency 10 Hz, and limited current value 400 mA is applied to a sample with a cross-sectional area of ​​3.5×3.5 mm.

[0102] It can be seen that the achieved density is higher for all samples when an AC electric field is applied compared to the same samples when a DC electric field is applied. On the other hand, the achieved density is lower for samples with larger cross-sectional area. Therefore, it is necessary to increase the input power for ceramic powder compact samples with larger cross-sectional area, and an effective way to achieve this is to increase the frequency of the AC electric field.

[0103] (Regarding control of AC electric field) Fig. 23 is a diagram for qualitatively explaining the relationship between the electric field and the specimen current in the flash phenomenon. Line L16 in Fig. 23 shows the change in relative density of the sintered body by the flash sintering method, and line L17 shows the change in relative density of the sintered body by the normal sintering method without applying an electric field. Line L18 shows the change in the electric field in the flash sintering method, and line L19 shows the change in the specimen current in the flash sintering method.

[0104] In the flash sintering method, the ceramic powder compact is heated while a constant electric field is applied. At this time, a limiting current value, which is the upper limit of the sample current value, is set in advance. When the temperature of the electric furnace rises and reaches the flash temperature, the flash phenomenon occurs, and the relative density also increases significantly.

[0105] As shown in Figure 23, the electric field and specimen current change significantly before and after this flash phenomenon. A stabilized power supply is generally used to apply the electric field to the specimen and control the specimen current. In the range where a constant voltage is applied at temperatures lower than the flash temperature, the control mode of this power supply is the voltage control mode (mode 1 in Figure 23). As shown in Figure 23, in the temperature range below the flash temperature, the resistance of the ceramic powder compact is high and almost no specimen current flows. After that, when the flash temperature is reached, the resistance of the specimen decreases significantly and, at the same time, the specimen current value increases sharply (line L19).

[0106] This specimen current increases up to a preset limiting current value. When the specimen current reaches the limiting current value, the stabilized power supply automatically switches from voltage control mode to current control mode (mode 2 in FIG. 23). From this point on, the power supply controls the current to be constant, so that the applied electric field is automatically controlled while decreasing significantly. The temperature of the electric furnace may be constant at the temperature at which this flash phenomenon occurs, or may continue to be increased further. The case where the furnace temperature is constant will be explained below.

[0107] In general, in the flash sintering method, attention has been focused on the phenomenon of rapid sintering (sintering in a short time), and so the idea of ​​continuing to pass a constant current through the sample at a constant temperature after the flash phenomenon described above occurs has not been considered. On the other hand, as mentioned above, when sintering is performed with an electrode such as Pt foil in direct contact with the ceramic powder compact, the amount of power that can be input to the sample is limited, so a sintered body with sufficient density cannot be obtained by densification during the flash phenomenon alone. Therefore, the process of maintaining the current through the sample after the flash phenomenon occurs is important.

[0108] When applying a DC voltage, the power supply can follow the steep increase in current value that occurs during the flash phenomenon, and the control mode can automatically switch from voltage control mode to current control mode. On the other hand, when applying an AC electric field, the electric field and current oscillate between positive and negative, so the increase in specimen current accompanying the flash phenomenon mixes with the original AC waveform, and a normal power supply cannot follow. Therefore, for example, by using the following method, it is possible to switch from voltage control mode to current control mode before and after the flash phenomenon occurs.

[0109] Fig. 24 is a diagram showing an example of voltage and current waveforms of AC control in the manufacturing method of a sintered body according to the sixth embodiment. The left side of the occurrence of the flash phenomenon in Fig. 24 shows the waveform below the flash temperature, and the right side shows the waveform above the flash temperature. Waveforms W1 and W2 show the change in voltage, and waveforms W3 and W4 show the change in current.

[0110] As shown in Figure 24, below the flash temperature, the voltage waveform W1 forms a sine wave, and since almost no current flows, the waveform W3 only oscillates slightly. On the other hand, above the flash temperature, the current value increases significantly. At this time, the current value is controlled so that any portion that exceeds the limited current value is cut off (waveform W4). At this time, the voltage waveform W2 also takes on the same waveform as the current value.

[0111] As a result, the resistance value of the sample that occurs during the transition from the voltage control mode to the current control mode and during the current control mode can be reduced, and the voltage control mode can be automatically transitioned to the current control mode, and the current can be automatically controlled at a preset limiting current value. Here, it is preferable that the maximum value of the positive part of the current waveform W4 is approximately the same as the maximum value of the negative part. If there is a difference between the positive and negative maximum values, the AC component is superimposed on the DC component, which may cause the influence of the bias of the ion flow that occurs when a DC electric field is applied, or the electrode may melt. Therefore, it is preferable that the absolute value of the voltage amplitude of the voltage waveform W2 after the flash phenomenon occurs is smaller in both positive and negative directions than that of the voltage waveform W1 before the flash phenomenon occurs.

[0112] As a method for controlling the AC electric field in this manner, for example, a detector for detecting an overload current is provided in the power supply 30, and when the detector detects a limit current value flowing through the ceramic powder compact, the voltage control mode of the power supply 30 is switched to a current control mode so that the limit current value is not exceeded.

[0113] As another method for controlling the AC electric field, the current flowing through the sample may be read by a high-speed ammeter. At this time, a peak current value (maximum current value) for several wavelengths is detected. When a flash phenomenon occurs, this value increases significantly. Therefore, this current value may be read by an arithmetic device such as a computer, and the stabilized power supply may be controlled using the signal line S5 so that the current value becomes a preset current value. In this case, it is also possible to control with a sine wave. Alternatively, a reference resistor may be inserted in the signal line S3 (see FIG. 6) described later, the voltages at both ends of the resistor may be read by a computer, the peak voltage value for several wavelengths may be read, the maximum voltage value may be calculated from this value, and the voltage of the stabilized power supply may be controlled by the signal line S5 using an arithmetic device.

[0114] As described above, the method for producing a sintered body according to the sixth embodiment is a method for producing a sintered body by applying an AC electric field to a ceramic compact having a predetermined shape while raising the temperature. The method includes a first step of raising the temperature while applying a first AC electric field (waveform W1) to the ceramic compact up to a flash sintering temperature at which the current flowing through the ceramic compact increases rapidly, as shown in Fig. 24, and a second step of raising the temperature while applying a second AC electric field (waveform W2) smaller than the first AC electric field after the current flowing through the ceramic compact increases rapidly and reaches the limiting current value shown in Fig. 23.

[0115] As a result, as shown in FIG. 21, it is possible to manufacture a high-density sintered body with relatively low power consumption, which is difficult to achieve using only the conventional flash sintering method in which a DC electric field is applied to a sample.

[0116] Also, as shown in Fig. 23, in mode 1, the application of the first AC electric field (waveform W1) is performed in a voltage control mode, and in mode 2, the application of the second AC electric field (waveform W2) is performed in a current control mode. As a result, after the flash phenomenon occurs, as shown in Fig. 24, the current can be controlled so that it does not exceed a predetermined current value, reducing the possibility of the electrodes melting due to the application of excessive power to the sample. In other words, as a result of being able to apply higher power to the ceramic powder compact sample, a more dense and high-density sintered body can be manufactured.

[0117] Moreover, from the results shown in Fig. 20, it is preferable that the first AC electric field (waveform W1 in Fig. 24) and the second AC electric field (waveform W2 in Fig. 24) have a frequency of 10 Hz or more. This can further improve the density of the sintered body.

[0118] In this way, the manufacturing method according to the sixth embodiment makes it possible to manufacture, in a comparatively short time, a sintered body with a high density that is difficult to achieve by the conventional flash sintering method alone.

[0119] [Manufacturing equipment] A manufacturing apparatus suitable for the manufacturing method of the sintered body according to the sixth embodiment is similar to the manufacturing apparatus 10 shown in FIG. 6, and therefore a description of the schematic configuration will be omitted.

[0120] The manufacturing apparatus 10 according to the sixth embodiment includes a heater 12a for heating a ceramic compact sample 18 having a predetermined shape, a pair of electrodes 22 for applying a voltage to the ceramic compact sample 18, a power supply 30 for applying a voltage to the pair of electrodes 22, and a first arithmetic unit 28 and a second arithmetic unit 32 for controlling the power supply 30 while raising the temperature of the ceramic compact with the heater 12a. The first arithmetic unit 28 and the second arithmetic unit 32 perform voltage control of the power supply 30 until the current flowing through the ceramic compact increases rapidly, and then perform current control of the power supply 30 after the current flowing through the ceramic compact increases rapidly and reaches a predetermined current value.

[0121] As a result, even with a relatively low power that does not melt the electrode 22, it is possible to produce a sintered body with a high density that is difficult to achieve using only the conventional flash sintering method.

[0122] The present disclosure has been described above based on the embodiments. These embodiments are merely examples, and it will be understood by those skilled in the art that various modifications are possible in the combination of each component and each treatment process, and that such modifications are also within the scope of the present disclosure. [Industrial Applicability]

[0123] The method for producing a sintered body disclosed herein can be used to produce various high-temperature ceramic components, structural ceramics at room temperature, furnace tubes for electric furnaces and the like, knives, tools, industrial abrasives and grinding materials, ceramic materials for dentistry, artificial bones, solid electrolyte membrane materials that utilize electrical conductivity, and ceramic materials for sensors. [Explanation of symbols]

[0124] 10 manufacturing apparatus, 12 electric furnace, 12a heater, 14 apparatus main body, 16 control system, 18 sample, 20 sample stage, 22 electrode, 24 rod, 26 detector, 28 first computing device, 30 power supply, 32 second computing device.

Claims

1. A method for producing a sintered body by heating a ceramic powder compact while applying an electric field thereto, comprising the steps of: a current flowing through the ceramic compact is controlled so as to maintain a constant sintering rate, and the current control is performed by increasing the current flowing through the ceramic compact so as to maintain a constant sintering rate for at least a predetermined time after the current flowing through the ceramic compact reaches a predetermined current value.

2. A method for producing a sintered body by heating a ceramic powder compact while applying an electric field thereto, comprising the steps of: a current profile determined so as to produce a ceramic sintered body having a density greater than a predetermined value, and the current control is performed by increasing the current flowing through the ceramic compact so as to maintain a constant sintering rate for at least a predetermined time after the current flowing through the ceramic compact reaches the predetermined current value.

3. raising the temperature of the ceramic powder compact to a temperature at which sintering begins; a step of lowering the temperature of the heated ceramic powder compact to a predetermined temperature or lower without maintaining the temperature at which sintering begins; raising the temperature of the ceramic powder compact while applying a predetermined electric field thereto; Including, The method for producing a sintered body, wherein the predetermined temperature is a flash sintering temperature at which a current flowing through the ceramic compact increases rapidly when the ceramic compact is heated while an electric field is applied thereto.

4. 4. The method for producing a sintered body according to claim 3, wherein the temperature at which the sintering starts is 800 to 1200° C.

5. a heating step of heating the ceramic powder compact to a predetermined temperature; applying a predetermined electric field to the ceramic powder compact until the predetermined temperature is reached; a first current control step of controlling a current flowing through the ceramic compact so that a sintering rate becomes constant after the current flowing through the ceramic compact reaches a first current value in the electric field application step; a second current control step of increasing the current flowing through the ceramic powder compact to a second current value higher than the first current value after the first current control step has been performed for a predetermined time; A method for producing a sintered body, comprising:

6. 6. The method for producing a sintered body according to claim 1, wherein the raw material powder for the ceramic green compact contains zirconium oxide as a main component.

7. a heater for heating the ceramic powder compact; an electrode for applying a voltage to the ceramic powder compact; a voltage application unit that applies a voltage to the electrodes so that a predetermined current flows in the ceramic powder compact; a memory unit that stores a current profile determined to produce a ceramic sintered body having a density greater than a predetermined value; a control unit that controls the voltage application unit based on the current profile while raising the temperature of the ceramic powder compact by the heater; Equipped with the current profile controls a current flowing through the ceramic compact so that a sintering rate of the ceramic compact becomes constant, and the current control is performed by increasing the current flowing through the ceramic compact so that the sintering rate becomes constant, at least for a predetermined time after the current flowing through the ceramic compact reaches a predetermined current value.