Recycled aggregate

By producing recycled aggregate from sludge cake and sewage sludge incineration ash, the sludge disposal problem is solved, creating a carbon dioxide-fixing concrete component with improved strength and particle size.

JP7593658B2Active Publication Date: 2024-12-03KAIKOU ONODA REMIKON
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022095342
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-06-13
Publication Date
2024-12-03
Estimated Expiration
2042-06-13

AI Technical Summary

Technical Problem

The disposal of sludge from mixer trucks used in ready-mixed concrete production is a costly environmental issue, and existing methods to utilize this sludge as a resource do not effectively address its carbon dioxide fixation potential.

Method used

Recycled aggregate is produced by kneading sludge cake from mixer truck washings with cement and sewage sludge incineration ash, which is made by mixing sewage sludge with silica sand and firing, to create a porous material that can fix carbon dioxide.

Benefits of technology

This process transforms sludge into a valuable resource for concrete production while addressing disposal costs and enhancing carbon dioxide fixation capabilities, maintaining adequate strength and particle size.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593658000002
    Figure 0007593658000002
  • Figure 0007593658000003
    Figure 0007593658000003
  • Figure 0007593658000004
    Figure 0007593658000004
Patent Text Reader

Abstract

To provide a recycled aggregate having carbon dioxide fixing function while solving a problem of sludge disposal cost, and a method for producing the same.SOLUTION: A recycled aggregate is made of sludge cake derived from washing water of a mixer truck transporting ready-mixed concrete as a raw material, and further contains cement and sewage sludge incineration ash. A method for producing the recycled aggregate includes a crushing step in which the sludge cake is kneaded and mixed by a kneading machine, a kneading step in which cement is poured into the kneading machine and the sludge cake is kneaded and mixed, and a granulation step in which sewage sludge incineration ash is added to the mixture of the sludge cake and cement and the sludge cake is kneaded and mixed.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is a method for producing regenerated bone using sludge as a raw material. Material Regarding. [Background technology]

[0002] Ready-mixed concrete is produced by mixing cement, water, aggregates, etc. This ready-mixed concrete has the characteristic that it hardens after production, so as soon as it is produced in the factory, it is transported by mixer truck to the site where it is to be poured. The transport time is generally within one hour. In general, the mixer truck makes several trips a day between the ready-mixed concrete production plant and the pouring site, and at the end of the trip, it returns to the production plant and is washed with water. The sludge that is generated from the washing water at this time is called sludge, and in most cases it is disposed of as industrial waste. However, there are also known attempts to make effective use of this sludge as a resource, and for example, Patent Document 1 discloses a method for producing recycled aggregate using sludge. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-149611 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, the progression of global warming due to carbon dioxide has come to be seen as a problem, and concrete production activities have been cited as one of the main causes of climate change. However, on the other hand, calcium hydroxide remains on the surface of concrete, which reacts with carbon dioxide to produce calcium carbonate and water. In other words, recent research has revealed that concrete has the ability to absorb and fix carbon dioxide (the so-called "carbon sponge effect").

[0005] Calcium hydroxide, which contributes to the fixation of carbon dioxide, is produced by the hydration reaction of cement that constitutes concrete. On the other hand, aggregate, which constitutes concrete together with cement, does not usually contribute to the fixation of carbon dioxide. The present inventors have repeatedly studied ways to impart the ability to fix carbon dioxide to this aggregate. In addition, they thought that if sludge is effectively used to produce the aggregate as in Patent Document 1, the problem of disposal costs could be solved at the same time, and thus they have completed the present invention.

[0006] The present invention provides a regenerated bone having the ability to fix carbon dioxide while solving the problem of sludge disposal costs. Materials The purpose is to provide. [Means for solving the problem]

[0007] The raw aggregate according to the present invention is sludge cake derived from the washing water of a mixer truck transporting ready-mix concrete. and, Cement and 、 Sewage sludge incineration ash The sewage sludge incineration ash is made by burning a mixture of sewage sludge and silica sand. The cement is normal high-early-strength Portland cement or blast furnace fly ash cement. The amount of sewage sludge incineration ash is in the range of 4% by weight or more and 30% by weight or less for a sludge cake with a moisture content of 45%, and the amount of cement is in the range of 2% by weight or more and 20% by weight or less for a sludge cake with a moisture content of 45%. Characterized by 。 Effect of the Invention

[0012] The recycled aggregate according to the present invention is made from sludge cake, which is often disposed of as industrial waste. According to the present invention, the sludge cake is recycled into aggregate for concrete, and the problem of the disposal cost of the sludge cake is solved while the recycled aggregate, which is a valuable material, can be obtained. Furthermore, in the present invention, the recycled aggregate contains sewage sludge incineration ash. This makes it possible to make the recycled aggregate porous and increase its surface area. In other words, it is possible to impart the ability to fix carbon dioxide to the recycled aggregate. Like sludge cake, sewage sludge incineration ash is also originally a waste. By using this sewage sludge incineration ash, it is possible to reduce the cost of imparting the ability to fix carbon dioxide to the recycled aggregate.

[0013] In the present invention, it is useful to use sewage sludge incineration ash obtained by mixing sewage sludge with silica sand and then calcining it. Since the main component of silica sand is silicon dioxide, which is a porous material, mixing it can make the sewage sludge incineration ash even more porous, thereby further increasing the carbon dioxide fixation capacity of the recycled aggregate.

[0014] When the amount of sewage sludge incineration ash mixed is 4-30% by weight of the sludge cake, recycled aggregate with an appropriate particle size and sufficient strength can be obtained. If the amount of sewage sludge incineration ash mixed is less than 4% by weight, the recycled aggregate may not be granulated properly, and if the amount is more than 30% by weight, the strength of the recycled aggregate may decrease.

[0015] When the amount of cement mixed is 2 to 20% by weight of the sludge cake, recycled aggregate with sufficient strength can be obtained inexpensively. If the amount of high-early-strength Portland cement mixed is less than 2% by weight, the strength of the recycled aggregate obtained may be insufficient, and if the amount is more than 20% by weight, the manufacturing cost of the recycled aggregate becomes high, which is a disadvantage.

[0016] This method of producing recycled aggregate sequentially involves a deflocculation process in which sludge cake is mixed in a mixer, a mixing process in which cement is added to the mixer and mixed with the sludge cake, and a granulation process in which sewage sludge incineration ash is added to the sludge cake and cement mixture and mixed, making it possible to obtain recycled aggregate with good shape, particle size, strength, etc. [Brief description of the drawings]

[0017] [Figure 1] 1 is a pie chart showing the main components of sewage sludge incineration ash. [Diagram 2] These are photographs of sludge cake before and after thawing. [Diagram 3] This is a photograph of recycled aggregate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] In the present invention, recycled aggregate is produced by adding cement and sewage sludge incineration ash to sludge cake, which is derived from the washing water of a mixer truck that transports ready-mixed concrete. The manufacturing process for obtaining recycled aggregate from sludge cake consists of three stages: desludging the sludge cake, kneading with cement, and granulation with sewage sludge incineration ash. For example, normal high-early-strength Portland cement or blast furnace fly ash cement can be used as the cement. If the moisture content of the sludge cake is 45%, the amount of cement mixed is preferably 2 to 20% by weight (2% by weight or more and 20% by weight or less) of the sludge cake. If the amount of cement mixed is less than 2% by weight, the strength of the resulting recycled aggregate may be insufficient, and if the amount of cement mixed is more than 20% by weight, the manufacturing cost of the recycled aggregate becomes high, which is a disadvantage.

[0019] Sewage sludge incineration ash is ash produced by drying and incinerating sewage sludge generated during the sewage treatment process. Organic matter, which accounts for about 80% of sewage sludge, disappears under high temperature and high pressure conditions during incineration, and harmless solid matter remains in the incinerator as sewage sludge incineration ash. The sewage sludge incineration ash obtained in this way contains silicon dioxide (SiO2), a porous material, as its main component, and is therefore useful for making recycled aggregate porous. If the moisture content of the sludge cake is 45%, the amount of sewage sludge incineration ash is preferably 4 to 30% by weight (4% by weight or more and 30% by weight or less) of the sludge cake. If the amount of sewage sludge incineration ash is less than 4% by weight, the recycled aggregate may not be properly granulated, and if the amount exceeds 30% by weight, the strength of the recycled aggregate may decrease. EXAMPLES

[0020] (Sewage sludge incineration ash) First, the sewage sludge incineration ash will be described. The sewage sludge incineration ash used in this embodiment is obtained by mixing dried sewage sludge with silica sand, and then firing the mixture at a temperature in the range of 700 to 1000° C. Since the main component of silica sand is silicon dioxide, which is a porous material, mixing the silica sand can make the sewage sludge incineration ash even more porous.

[0021] In order to identify the constituent elements of this sewage sludge incineration ash, fluorescent X-ray analysis was performed. Fluorescent X-rays are X-rays that are emitted in response to the energy difference between the inner and outer shells when the inner shell electrons of atoms in a substance are excited when the substance is irradiated with X-rays with a certain level of energy, resulting in a vacancy (hole) that is created and an outer shell electron moves to it. Since the energy difference between the inner and outer shells is unique to each element, the energy of fluorescent X-rays is also unique to each element. For this reason, it is possible to analyze the constituent elements by looking at the fluorescent spectrum of the target sample, and the concentration of a specific element in the target sample can be determined by measuring the intensity of the spectrum.

[0022] The results of X-ray fluorescence analysis of sewage sludge incineration ash are shown in Table 1 and Figure 1. The components present in descending order are diphosphorus pentoxide (P205) at 28.80%, aluminum oxide (Al2O3) at 23.23%, and silicon dioxide (SiO2) at 17.06%, with these three accounting for more than two-thirds of the sewage sludge incineration ash. As this sewage sludge incineration ash was incinerated together with silica sand, it contains a large amount of silicon dioxide, the main component of silica sand. Note that since Table 1 and Figure 1 show the contents of the main components of sewage sludge incineration ash, the sum of their composition ratios does not equal 100%.

[0023] [Table 1]

[0024] (Mixer truck cleaning process) The ready-mix concrete produced at the factory is transported to the casting site in a mixer truck equipped with a mixer drum that can carry the ready-mix concrete. The mixer truck makes several trips a day between the ready-mix concrete manufacturing plant and the casting site, and finally returns to the manufacturing plant where it is washed with water. During this washing process, washing water containing ready-mix concrete is discharged.

[0025] (Sieving process of washing water) The washing water discharged from the washing process contains aggregates (fine aggregates and coarse aggregates) that can be used as resources. Therefore, a sieving process is carried out to sift the washing water and recover the aggregates. The liquid that passes through this sieve is called sludge water in this invention.

[0026] (Sludge water dewatering process) The sludge water is dewatered using various types of filtering equipment, in this embodiment a filter press (pressure filtering equipment). The solid matter remaining after dewatering is called sludge cake in this invention. The water content of this sludge cake is about 45%. The supernatant water separated from the sludge cake in this dewatering process is reused in the production of ready-mix concrete.

[0027] (Sludge cake deflocculation process) The dewatered sludge cake is crushed to an appropriate size of about 70 mm, and then fed into a kneader to be mixed, i.e., deflocculated. In this example, a PM-60 made by Nikko Co., Ltd. was used as the kneader. 20 kg of sludge cake was fed into the kneader, and the kneading time was 6 minutes. The state of the sludge cake before deflocculation (kneading) is shown in Figure 2(a), and the state after deflocculation is shown in Figure 2(b). Another kneader that can be used is the PUPPET50 made by Koyo Machinery Industry Co., Ltd.

[0028] (Mixing process with cement) Next, cement is put into the kneader and mixed with the thawed sludge cake. In this example, normal high-early-strength Portland cement is used, and the amount of cement put in is 10% by weight of the sludge cake, i.e., 2 kg. The kneading time is 2 minutes.

[0029] (Granulation process using sewage sludge incineration ash) Finally, the sewage sludge incineration ash is fed into the kneader. The mixture of sludge cake and high-early-strength Portland cement is granulated by mixing with the sewage sludge incineration ash, and becomes recycled aggregate that can be used in the production of concrete. In this embodiment, the amount of sewage sludge incineration ash fed was 14% by weight of the sludge cake, i.e., 2.8 kg. The kneading time was 2 minutes and 30 seconds. In this granulation process and the previous kneading and sludge thawing processes, the rotation speed of the kneader was set to 36 rpm, and the revolution speed was set to 21.5 rpm (frequency 30 Hz).

[0030] A photograph of the obtained recycled aggregate is shown in Figure 3(a), and a photograph of the cross section of the same aggregate is shown in Figure 3(b). This recycled aggregate has a particle size of about 5 to 40 mm, and therefore can be used as coarse aggregate for concrete.

[0031] After the granulation process, water may seep out from the surface of the recycled aggregate. In that case, adding cement again will absorb the water and stabilize the state of the recycled aggregate. Adding this cement is thought to be effective not only for absorbing water, but also for expanding the particle size of the recycled aggregate and for dealing with solutes in the sewage sludge incineration ash.

[0032] As described above, the recycled aggregate according to this embodiment is made from sludge cake, which is often disposed of as industrial waste. According to this embodiment, in which the sludge cake is recycled into aggregate for concrete, it is possible to obtain a valuable recycled aggregate while solving the problem of the disposal cost of the sludge cake. Furthermore, in this embodiment, the recycled aggregate contains sewage sludge incineration ash. This makes it possible to make the recycled aggregate porous and increase its surface area. In other words, it is possible to impart the ability to fix carbon dioxide to the recycled aggregate. Like sludge cake, sewage sludge incineration ash is also originally a waste. By using this sewage sludge incineration ash, it is possible to keep the cost of imparting the ability to fix carbon dioxide to the recycled aggregate low.

[0033] This method of producing recycled aggregate sequentially involves a deflocculation process in which sludge cake is mixed in a mixer, a mixing process in which cement is added to the mixer and mixed with the sludge cake, and a granulation process in which sewage sludge incineration ash is added to the sludge cake and cement mixture and mixed, making it possible to obtain recycled aggregate with good shape, particle size, strength, etc.

Claims

[Claim 1] A recycled aggregate made by mixing sludge cake derived from washing water of a mixer truck transporting ready-mix concrete, cement, and sewage sludge incineration ash into granular form, Sewage sludge incineration ash is obtained by firing a mixture of sewage sludge and silica sand, The cement is ordinary Portland cement or blast furnace or fly ash cement. This recycled aggregate is characterized in that the amount of sewage sludge incineration ash is in the range of 4% by weight or more and 30% by weight or less with respect to a sludge cake having a moisture content of 45%, and the amount of cement is in the range of 2% by weight or more and 20% by weight or less with respect to a sludge cake having a moisture content of 45%.

Citation Information

Patent Citations

  • Cement solidified material comprising burned ash of sewage sludge as raw material, graded grain treating material using the cement solidified material and stabilization treatment

    JP2000128613A

  • Filler for construction work