Copolymer-based proton-conducting electrolyte membranes and fuel cells
The described proton-conducting electrolyte membrane, featuring a copolymer with a pKa 2.5 or less plasticizer, addresses the humidity limitation and wrinkle issues of conventional membranes, enabling high conductivity and improved handling for large-area applications.
Patent Information
- Application Number
- JP2020196798
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-11-27
AI Technical Summary
Conventional proton-conducting electrolyte membranes, such as Nafion, require high humidity for optimal performance, limiting their operating temperature to below the boiling point of water, and may develop wrinkles during manufacturing, making large-area membranes difficult to produce.
A proton-conducting electrolyte membrane composed of a copolymer with a first portion and a second portion covalently linked, where the first portion aggregates to form domains and the second portion bridges these domains, incorporating a plasticizer with a pKa of 2.5 or less that penetrates the second portion, reducing the glass transition temperature and forming a pseudo-crosslinked structure with one- or two-dimensionally extending domains.
The membrane exhibits high proton conductivity in low-humidity or anhydrous environments, is resistant to wrinkles during manufacture, and has good handling properties, allowing for the production of large-area membranes.
Smart Images

Figure 0007593795000008 
Figure 0007593795000009 
Figure 0007593795000010
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a proton-conducting electrolyte membrane and a fuel cell. [Background technology]
[0002] Conventionally, perfluorosulfonic acid resin membranes such as Nafion (registered trademark, the same applies below) have been known as proton-conductive electrolyte membranes used as electrolyte materials for fuel cells. However, the presence of water is essential to achieve high proton conductivity in such perfluorosulfonic acid resin membranes. Therefore, it has been necessary to limit the operating temperature of fuel cells equipped with such perfluorosulfonic acid resin membranes to below the boiling point of water.
[0003] Therefore, proton-conductive electrolyte membranes that can be used in low-humidity or anhydrous environments have been developed.
[0004] For example, Patent Document 1 discloses a proton-conducting electrolyte membrane that exhibits high proton conductivity even in a low-humidity or anhydrous environment. More specifically, the proton-conducting electrolyte membrane of Patent Document 1 is a proton-conducting membrane that includes "a polymer having a first portion and a second portion that are connected by a covalent bond, and a plasticizer, the first portions are mutually aggregated to form domains at the operating temperature of the proton-conducting membrane, and the second portion bridges the domains, the second portion has a proton-accepting group, and the plasticizer includes a proton-donating compound having a pKa of 2.5 or less, whereby the plasticizer permeates the second portion, and the glass transition temperature of the polymer is lowered compared to a case where the plasticizer is not included." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-068130 A Summary of the Invention [Problem to be solved by the invention]
[0006] The proton-conductive electrolyte membrane of Patent Document 1 exhibits high proton conductivity, but wrinkles may occur in the membrane surface direction during production. This may result in poor handling of the produced proton-conductive electrolyte membrane, and in some cases, may make it difficult to produce a proton-conductive electrolyte membrane with a desired large area.
[0007] The present disclosure seeks to improve the above-mentioned circumstances, and has an object to provide a proton-conductive electrolyte membrane that is less prone to wrinkles during production and has good handleability. [Means for solving the problem]
[0008] The present disclosure which achieves the above objectives is as follows.
[0009] <Aspect 1> A proton-conducting electrolyte membrane, a copolymer having a first portion and a second portion covalently linked together; and Plasticizer Including, the first portions are aggregated together to form domains at a temperature at which the proton conductive membrane is used, and the second portions bridge the domains; the second portion having a proton accepting group; At least a portion of the domains extend in one or two dimensions; and The plasticizer comprises a proton donating compound having a pKa of 2.5 or less, whereby the plasticizer permeates the second portion and the glass transition temperature of the copolymer is lowered compared to when the plasticizer is not present. Proton-conducting electrolyte membrane. <Aspect 2> 2. The proton conducting electrolyte membrane according to claim 1, wherein the domains are in a glassy or crystalline state. <Aspect 3> 3. The proton conducting electrolyte membrane according to claim 1 or 2, wherein at least a portion of the domains has a cylindrical or lamellar structure. <Aspect 4> The proton conducting electrolyte membrane according to any one of aspects 1 to 3, wherein the copolymer is a block copolymer, and the first portion and the second portion are an A block and a B block of the block copolymer, respectively. <Aspect 5> 5. The proton conducting electrolyte membrane according to any one of aspects 1 to 4, wherein the block copolymer is an ABA type triblock copolymer constituted by the A block and the B block. Aspect 6 6. The proton conducting electrolyte membrane according to claim 4 or 5, further comprising a homopolymer consisting of the A block. Aspect 7 7. The proton-conducting electrolyte membrane according to any one of aspects 1 to 6, which is isotropic in the planar direction. <Aspect 8> 8. The proton conducting electrolyte membrane according to any one of aspects 1 to 7, wherein a volume fraction of the first portion in all polymers present in the proton conducting electrolyte membrane is 10% or more and 70% or less. <Aspect 9> 9. The proton-conducting electrolyte membrane according to any one of aspects 1 to 8, further comprising a non-fluorine-based porous sheet, the non-fluorine-based porous sheet being impregnated with the copolymer and the plasticizer. Aspect 10 10. The proton conducting electrolyte membrane according to any one of aspects 1 to 9, wherein a molar ratio of the proton donating compound to the proton accepting group is 1.0 or more and 10.0 or less. <Aspect 11> 11. The proton conducting electrolyte membrane according to any one of aspects 1 to 10, wherein the combination of the copolymer and the plasticizer is a viscoelastic solid at least in the temperature range of 50° C. or more and 100° C. or less. Aspect 12 12. The proton conducting electrolyte membrane according to any one of aspects 1 to 11, wherein the content of the plasticizer is 50 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the total of the copolymer and the plasticizer. Aspect 13 13. The proton conducting electrolyte membrane according to any one of aspects 1 to 12, wherein the proton donating compound is at least one selected from sulfuric acid and phosphoric acid. Aspect 14 14. The proton conducting electrolyte membrane according to any one of aspects 1 to 13, wherein the proton accepting group is a nitrogen-containing heterocyclic group. Aspect 15 15. The proton conducting electrolyte membrane according to any one of aspects 1 to 14, wherein the first portion is a polystyrene-based polymer. Effect of the Invention
[0010] The proton-conductive electrolyte membrane of the present disclosure is less prone to wrinkles during production and has good handling properties.
[0011] Therefore, the proton-conducting electrolyte membrane of the present disclosure is particularly suitable for use as a proton-conducting electrolyte membrane in a fuel cell. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram for explaining the mechanism by which the proton-conductive electrolyte membrane of the present disclosure exhibits its function. [Diagram 2] FIG. 2 is a diagram showing an example of an image of a cylindrical structure. [Diagram 3] FIG. 3 is a diagram showing an example of an image of a lamellar structure. [Figure 4] FIG. 4 is a photograph of the nanostructure of the copolymer of Example 1 (SPS-1 membrane) observed with a transmission electron microscope. [Diagram 5] FIG. 5 is a photograph of the proton-conductive electrolyte membrane of Example 1. [Figure 6]FIG. 6 is a graph showing the proton conductivities of the proton-conducting electrolyte membranes of Examples 1 to 3 and Comparative Example 1. As shown in FIG. [Figure 7] FIG. 7 is a diagram showing stress-strain curves of the proton conducting electrolyte membranes of Examples 1 to 4 and Comparative Example 1. [Figure 8] FIG. 8 is a photograph of the nanostructure of the copolymer of Comparative Example 1 (SPS-2 membrane) observed with a transmission electron microscope. [Figure 9] FIG. 9 is a photograph of the proton-conductive electrolyte membrane of Comparative Example 1. [Figure 10] FIG. 10 is a photograph of the nanostructure of the copolymer of Example 2 (SPS-3 membrane) observed with a transmission electron microscope. [Figure 11] FIG. 11 is a photograph of the nanostructure of the copolymer of Example 3 (SPS-4 membrane) observed with a transmission electron microscope. [Figure 12] FIG. 12 is a graph showing the proton conductivity of the proton-conducting electrolyte membranes of Examples 5 and 6. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Proton-conducting electrolyte membrane> The proton-conducting electrolyte membrane of the present disclosure is a copolymer having a first portion and a second portion covalently linked together; and Plasticizer Including, the first portions are mutually aggregated to form domains at a temperature at which the proton-conductive electrolyte membrane is used, and the second portions bridge the domains; the second portion has a proton accepting group; At least a portion of the domain extends in one or two dimensions; and the plasticizer comprises a proton donating compound having a pKa of 2.5 or less, whereby the plasticizer permeates the second portion and reduces the glass transition temperature of the copolymer compared to the absence of the plasticizer; A proton-conducting electrolyte membrane.
[0014] In the present disclosure, the "usage temperature of the proton-conductive electrolyte membrane" refers to the temperature at which the proton-conductive electrolyte membrane is used, and can be a desired temperature within a range of, for example, room temperature or higher, or 50°C or higher, and 200°C or lower, 150°C or lower, or 120°C or lower.
[0015] The term "domain" refers to a portion in which the first portion of the copolymer is aggregated by intermolecular forces other than covalent bonds, and is an aggregate portion that reversibly occurs in response to changes in the environment, such as temperature. Examples of intermolecular forces other than covalent bonds include, but are not limited to, van der Waals forces, charge transfer forces, Coulomb forces, hydrophobic bond forces, hydrogen bond forces, ionic bond forces, or coordinate bond forces, or combinations thereof.
[0016] "Bridged" refers to a structure in which a second portion of the copolymer bridges between the domains described above.
[0017] Therefore, in the proton-conductive electrolyte membrane of the present disclosure, at its operating temperature, the first portion forming the above-mentioned "domain" and the second portion forming the "bridge" form a pseudo-crosslinked structure as a whole.
[0018] As long as the effects of the present disclosure are not impaired, the copolymer of the present disclosure may contain chemical crosslinks (covalent crosslinks), or chemical crosslinks may be generated after the production of a proton-conductive electrolyte membrane consisting only of physical crosslinks.
[0019] It is preferable that the plasticizer containing the proton donor compound involved in proton transport dissolves well in the second part, which is a copolymer, and penetrates well. Here, "dissolves well" means that the respective molecules (plasticizer, second part, which is a copolymer) spontaneously "mix" with each other at the molecular level, and the Gibbs energy of mixing Δ mix This means that G will be a large negative value. Δ mix G=Δ mix H-TΔ mix S(Δ mix H is the enthalpy of mixing, Δmix S is the entropy of mixing, and T is the absolute temperature at the time of mixing, so Δ mix H is negative and has a large absolute value, TΔ mix If S is a large positive value, Δ mix Since G has a large negative absolute value, the plasticizer is well mixed at the molecular level, and if the plasticizer is liquid, it achieves a well-dissolved state.
[0020] In addition, "permeation" refers to the Δ mix This is promoted by G taking a large negative value, and the penetrating medium spontaneously permeates into the penetrating medium simply by contacting the two, achieving uniform mixing at the molecular level. When the penetrating medium is a plasticizer and the penetrating medium is a second part that is a polymer, Δ mix The value of G is mainly positive Δ mix Depending on the magnitude of S, this Δ mix Even though G can be negative, it will not have a large absolute value, and therefore no significant penetration will occur.
[0021] However, in the case of the present disclosure, the second part is a flexible polymer that easily undergoes conformational changes and has a proton-accepting group, and the plasticizer contains a proton-donating compound with a pKa of 2.5 or less, so that the proton-accepting group of the second part and the proton-donating compound form a pair that generates an attractive ionic interaction. When considering mixing the second part, which is a flexible polymer that easily undergoes conformational changes, with the plasticizer, TΔ mix Since S is a positive value of medium magnitude, Δ mix G takes a negative value, and since the second part and the plasticizer are a pair that generates heat when mixed, Δ mix H has a large negative absolute value, and the contribution of this ionic attractive interaction is Δ mix G also becomes a large negative value, making it easier for the plasticizer to "penetrate" into the second part. Even after penetrating, Δmix Since G remains negative, the plasticizer will not leach out naturally.
[0022] A "plasticizer" is one that is capable of lowering the glass transition temperature of the copolymer, which in this disclosure corresponds to the glass transition temperature of the second portion of the copolymer.
[0023] In the proton-conductive electrolyte membrane of the present disclosure, at least a part of the domain formed by the mutual aggregation of the first portions of the copolymer extends one-dimensionally or two-dimensionally. Such one-dimensionally or two-dimensionally extending domains are not dissolved in plasticizers containing a proton-donating compound having a pKa of 2.5 or less, and can be in a glassy or crystalline state at the use temperature of the proton-conductive electrolyte membrane, so that the proton-conductive electrolyte membrane of the present disclosure produced is unlikely to deform even under the weight of the proton-conductive electrolyte membrane or the load applied to the proton-conductive electrolyte membrane, and therefore it is considered that the handleability can be improved. Such one-dimensional or two-dimensional domains can be obtained by the copolymer having an appropriate proportion of the first portion (i.e., by setting the volume fraction of the first portion in the copolymer to a certain range). In addition, "setting the volume fraction of the first portion in the copolymer to a certain range" can also be achieved by adjusting the ratio of raw materials when synthesizing the copolymer, or by appropriately mixing a homopolymer described later.
[0024] In contrast to the first part of the copolymer of the proton-conductive electrolyte membrane of the present disclosure, at least a part of which extends one-dimensionally or two-dimensionally, the proton-conductive electrolyte membrane described in, for example, Patent Document 1 has scattered domains of the first part of the polymer (corresponding to the "copolymer" of the present disclosure) (i.e., the domains of the first part have a spherical structure). Due to this difference, the proton-conductive electrolyte membrane of the present disclosure can more significantly exhibit the effect of improving the handling property and the effect of improving the breaking elongation and / or tensile strength compared to the proton-conductive electrolyte membrane described in Patent Document 1.
[0025] Thus, the proton-conductive electrolyte membrane of the present disclosure exhibits high proton conductivity even in a low-humidity or anhydrous environment, while being less prone to wrinkles during production and having good handling properties. Below, the mechanism by which the proton-conductive electrolyte membrane of the present disclosure exerts its function will be described with reference to FIG. 1. However, the mechanism described below does not limit the present disclosure.
[0026] FIG. 1 is a schematic diagram for explaining the mechanism by which the proton-conductive electrolyte membrane of the present disclosure exhibits its function.
[0027] The proton-conductive electrolyte membrane of FIG. 1 includes a copolymer having a first portion and a second portion linked by a covalent bond, and a plasticizer (indicated as "proton-donating compound" in FIG. 1). The first portions are aggregated together to form domains at the operating temperature of the proton-conductive electrolyte membrane. In the proton-conductive electrolyte membrane, the second portion bridges the domains formed by the first portions. The second portion has a proton-accepting group. At least a portion of the domain in which the first portion is formed extends one-dimensionally. In the proton-conductive electrolyte membrane of FIG. 1, at least a portion of the domain in the first portion has a cylindrical structure.
[0028] As shown in FIG. 1, in the proton-conducting electrolyte membrane of the present disclosure, the second part of the copolymer has a proton-accepting group, and therefore can have an ionic interaction with a plasticizer containing a proton-donating compound having a pKa of 2.5 or less, and can also liberate protons from an excess of the plasticizer. The liberation of protons from the plasticizer will be described later. As shown in FIG. 1, the second part of the copolymer, the plasticizer, and the protons liberated from the plasticizer form a continuous uniform mixed molten phase. On the other hand, the first part of the copolymer does not dissolve in the plasticizer, and at the operating temperature of the proton-conducting electrolyte membrane, they aggregate with each other to form domains, in this case forming a continuous solid phase (glass phase) consisting of hard domains such as cylindrical ones. In this way, the first part and the uniform mixed molten phase including the second part are phase-separated at the nanometer level. For this reason, the proton-conductive electrolyte membrane shown in FIG. 1 maintains its membrane shape without flowing as a whole, and in the uniform mixed molten phase including the second portion, free protons can easily move even in an anhydrous environment, and high proton conductivity can be exhibited even in an anhydrous environment, so that the proton-conductive electrolyte membrane can be used as an anhydrous proton-conductive electrolyte membrane.
[0029] Furthermore, unlike polymers that are chemically cross-linked by covalent bonds, copolymers consisting of a first part and a second part forming such a pseudo-cross-linked structure can be processed by solution casting and can also be made into a hot melt having fluidity as a whole. Therefore, they can be produced by a solvent casting method, a spin coating method, or a hot melt method.
[0030] Therefore, the proton conducting electrolyte membrane of the present disclosure is less likely to wrinkle during production and has good handling properties.
[0031] The handleability can be judged, for example, by visually checking the presence or absence of deformation due to its own weight or the load applied when contacted. The Young's modulus of the proton-conductive electrolyte membrane of the present disclosure can also be used as an index of the handleability. This is because, according to intensive research by the inventors of the present disclosure, it has been found that the larger the Young's modulus of the proton-conductive electrolyte membrane, the lower the adhesion of the proton-conductive electrolyte membrane, making it easier to handle, i.e., improving the handleability.
[0032] The plasticizer according to the present disclosure includes a proton donating compound having a pKa of 2.5 or less. A proton can be released from such a proton donating compound. When the proton is released, the proton donating compound becomes an anion. In addition, since a proton accepting group is present in the second part of the copolymer, some of the free protons can be bonded to the proton accepting group. This causes the proton accepting group in the second part to become a cation. As shown in FIG. 1, in the proton conducting electrolyte membrane of the present disclosure, an ionic interaction can occur between the anionized proton donating compound, the free proton, and the cationized proton accepting group. Since such an ionic interaction exists throughout the entire membrane of the proton conducting electrolyte membrane, the free proton can easily move between ions even in an anhydrous environment. In other words, it is believed that the proton conducting electrolyte membrane of the present disclosure can be provided with high proton conductivity.
[0033] Since ionic interactions occur between the anions and cations thus formed, the proton donating compound having a pKa of 2.5 or less can remain in the membrane. In other words, it is believed that the proton donating compound having a pKa of 2.5 or less as a plasticizer is unlikely to leak or does not leak at all from the proton conducting electrolyte membrane of the present disclosure.
[0034] In addition, as described above, the ionic interaction makes it easier for the plasticizer to "permeate" into the second portion. According to the intensive research of the present inventors, it has been found that simply by contacting the copolymer according to the present disclosure with the plasticizer, the plasticizer spontaneously permeates into the copolymer, forming a uniform mixed phase. It is considered that in the proton-conducting electrolyte membrane of the present disclosure, even if the copolymer and the plasticizer coexist, the plasticizer mainly permeates into the second portion of the copolymer, and the state of the domain of the first portion of the copolymer is maintained.
[0035] As this "permeation" progresses, that is, as a large amount of plasticizer permeates into the second portion, the glass transition temperature of the copolymer decreases compared to when the plasticizer is not included. It is believed that the decrease in the glass transition temperature of the copolymer also activates the segment motion of the polymer chain, thereby imparting high proton conductivity to the proton-conducting electrolyte membrane of the present disclosure.
[0036] In FIG. 1, the proton-donating compound is depicted as a proton-donating dibasic acid, but the proton-donating compound is not limited to this.
[0037] <Copolymer> The copolymer contained in the proton conducting electrolyte membrane of the present disclosure has a first portion and a second portion that are linked by a covalent bond.
[0038] (First part) In the proton conducting electrolyte membrane of the present disclosure, the first portions of the copolymer are aggregated with each other to form domains at the operating temperature of the proton conducting electrolyte membrane, and the second portions of the copolymer bridge the domains.
[0039] In the present disclosure, at the use temperature of the proton-conductive electrolyte membrane, the domains formed by the mutual aggregation of the first portions of the copolymer may be in a glassy state or a crystalline state. Here, the "glassy state" refers to a solid amorphous state. Whether the domain is in a glassy state or a crystalline state can be determined by differential scanning calorimetry (DSC) measurement. More specifically, when an endothermic step is observed (or a peak is sometimes observed), it is in a "glassy state," and when no endothermic step is observed and only a sharp endothermic peak is observed, it is in a "crystalline state."
[0040] In the proton conducting electrolyte membrane of the present disclosure, at least a part of the domain of the first portion extends one-dimensionally or two-dimensionally. Here, "extending one-dimensionally" means that the domain formed by the first portion of the copolymer forms a one-dimensional continuous phase (e.g., a columnar or linear continuous phase), and "extending two-dimensionally" means that the domain forms a two-dimensional continuous phase (e.g., a planar continuous phase).
[0041] From the viewpoint of further exerting the effects of the present disclosure, it is preferable that the first portion has as many domains extending one-dimensionally or two-dimensionally as possible. That is, it is sufficient that at least a part of the domains of the first portion extends one-dimensionally or two-dimensionally, and preferably, the domains of the first portion extend one-dimensionally or two-dimensionally at 10 mol% or more, 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, or 100 mol% (i.e., the entire first portion) of the entire first portion. Note that, in the first portion, domains partly extending one-dimensionally and domains partly extending two-dimensionally may be mixed.
[0042] In the proton conducting electrolyte membrane of the present disclosure, one of the preferred aspects of the first portion domain "extending one-dimensionally" is that at least a part of the first portion domain has a cylindrical structure. Note that FIG. 2 is a diagram showing an example of the cylindrical structure.
[0043] In the proton conducting electrolyte membrane of the present disclosure, one of the preferred aspects of the first portion having a domain that "extends two-dimensionally" is that at least a part of the first portion has a lamellar structure. Note that FIG. 3 is a diagram showing an example of an image of the lamellar structure.
[0044] The proton-conductive electrolyte membrane of the present disclosure is preferably isotropic in the plane direction. Since the first portions of the proton-conductive electrolyte membrane of the present disclosure having such a structure can be regularly and periodically arranged on the nanometer order, the proton-conductive electrolyte membrane of the present disclosure can have a larger breaking elongation and / or tensile strength than a proton-conductive electrolyte membrane including covalent crosslinking points arranged irregularly and non-periodically.
[0045] The copolymer contained in the proton conducting electrolyte membrane of the present disclosure may have a volume fraction of the first portion of 10% or more, and may be 70% or less. More specifically, for example, the volume fraction of the first portion may be 10% or more, 11% or more, 12% or more, 13% or more, 14% or more, 15% or more, 16% or more, 17% or more, 18% or more, 19% or more, 20% or more, 21% or more, 22% or more, 23% or more, 24% or more, 25% or more, 26% or more, 27% or more, 28% or more, 29% or more, 30% or more, 31% or more, 32% or more, 33% or more, 34% or more, 35% or more, 36% or more, 37% or more, 38% or more, 39% or more, 40% or more, 42% or more, or 44% or more. Additionally, the volume fraction of the first portion may be 70% or less, 65% or less, 60% or less, 55% or less, or 50% or less.
[0046] Furthermore, when the proton conducting electrolyte membrane of the present disclosure contains other polymers besides the copolymer, for example, when it further contains a homopolymer composed of an A block described later, the volume fraction of the first portion in all the polymers (copolymers and homopolymers) present in the proton conducting electrolyte membrane of the present disclosure may be 10% or more and 70% or less. More specifically, it may be a value that the volume fraction of the first portion in the above-mentioned copolymer can take.
[0047] The volume fraction φ1 of the first portion can be calculated from the following formula:
number
[0048] In the present disclosure, a copolymer having a first portion and a second portion that are covalently linked can be, for example, a block copolymer.
[0049] From the viewpoint of the variety of variations, ease of handling, and the viewpoint of further exerting the effects of the present disclosure, the copolymer having the first and second portions linked by a covalent bond is preferably a block copolymer. In particular, when a block copolymer having the first portion at an appropriate ratio is self-assembled, the first and second portions can form a continuous phase in the membrane. By contacting such a block copolymer membrane with an anhydrous liquid strongly acidic electrolyte, the phase consisting of the second portion is swollen by the liquid strongly acidic electrolyte to become an anhydrous electrolyte membrane, and a continuous solid phase (e.g., glassy or crystalline state) consisting of the first portion that is not dissolved in the strongly acidic electrolyte exists throughout the anhydrous electrolyte membrane. Therefore, such a proton-conducting electrolyte membrane of the present disclosure is less likely to wrinkle, and can exhibit a high Young's modulus, high strength, low adhesion, and good handling properties even without containing a nonwoven fabric or filler.
[0050] In the following, the proton-conductive electrolyte membrane of the present disclosure will be described using as an example a case where the copolymer having the first and second portions linked by a covalent bond is a block copolymer. In this case, the first and second portions may be the A and B blocks of the block copolymer, respectively. Therefore, in the following description, the term "block copolymer" corresponds to "copolymer having the first and second portions", the term "A block" corresponds to "first portion", and the term "B block" corresponds to "second portion".
[0051] Block Copolymer The block copolymer may have an A block and a B block.
[0052] (A Block) In the present disclosure, the A blocks aggregate with each other to form domains at the operating temperature of the proton-conductive electrolyte membrane.
[0053] In other words, the A blocks are not particularly limited as long as they can be aggregated together to form domains at the temperature at which the proton-conductive electrolyte membrane is used. Therefore, examples of the A blocks include, but are not limited to, polystyrene-based polymers, polyacrylic acid ester-based polymers, polymethacrylic acid ester-based polymers, and polyolefin-based polymers.
[0054] The polystyrene-based polymer means a polymer having 50 mol% or more of a styrene moiety as a repeating unit, and examples thereof include, but are not limited to, polystyrene, polyacetylstyrene, polyanisoylstyrene, polybenzoylstyrene, polybiphenylstyrene, polybromoethoxystyrene, polybromomethoxystyrene, polybromostyrene, polybutoxymethylstyrene, polytert-butylstyrene, polybutyrylstyrene, polychlorofluorostyrene, polychloromethylstyrene, polychlorostyrene, polycyanostyrene, polydichlorostyrene, polydifluorostyrene, polydimethylstyrene, polyethoxymethylstyrene, polyethoxystyrene, polyfluoromethylstyrene, polyfluorostyrene, polyiodostyrene, polymethoxycarbonylstyrene, polymethoxymethylstyrene, polymethylstyrene, polymethoxystyrene, polyperfluorostyrene, polyphenoxystyrene, polyphenylacetylstyrene, polyphenylstyrene, polypropoxystyrene, polytoluoylstyrene, or polytrimethylstyrene.
[0055] The polyacrylate polymer refers to a polymer having 50 mol % or more of an acrylate moiety as a repeating unit, and examples thereof include, but are not limited to, polyadamantyl acrylate, polytert-butyl acrylate, polytert-butylphenyl acrylate, cyanoheptyl polyacrylate, cyanohexyl polyacrylate, cyanomethyl polyacrylate, cyanophenyl polyacrylate, fluoromethyl polyacrylate, methoxycarbonylphenyl polyacrylate, methoxyphenyl polyacrylate, naphthyl polyacrylate, pentachlorophenyl polyacrylate, and phenyl polyacrylate.
[0056] The polymethacrylate polymer means a polymer having 50 mol % or more of a methacrylate portion as a repeating unit, and examples thereof include polymethyl methacrylate, polyethyl methacrylate, polymethacrylonitrile, polyadamantyl methacrylate, polybenzyl methacrylate, polytert-butyl methacrylate, polytert-butylphenyl methacrylate, polycycloethyl methacrylate, polycyanoethyl methacrylate, polycyanomethylphenyl methacrylate, poly ... Examples of the polymethacrylate include, but are not limited to, cyanophenyl methacrylate, polycyclobutyl methacrylate, polycyclodecyl methacrylate, polycyclododecyl methacrylate, polycyclobutyl methacrylate, polycyclohexyl methacrylate, polycyclooctyl methacrylate, polyfluoroalkyl methacrylate, polyglycidyl methacrylate, polyisobornyl methacrylate, polyisobutyl methacrylate, polyphenyl methacrylate, polytrimethylsilyl methacrylate, and polyxylenyl methacrylate.
[0057] The polyolefin polymer means a polymer having 50 mol % or more of an olefin moiety as a repeating unit, and examples thereof include, but are not limited to, polyethylene, polypropylene, polyα-olefin, and the like.
[0058] It is noted that, in this disclosure, the prefix "poly" refers to a polymer containing two or more monomers.
[0059] Among the above, depending on the use temperature of the proton-conductive electrolyte membrane, one having a glass transition temperature or melting temperature higher than the use temperature of the proton-conductive electrolyte membrane can be selected as the block A. Moreover, from the viewpoints of, for example, low miscibility with plasticizers containing proton-donating compounds, ease of handling, low cost, etc., it is preferable that the block A is a polystyrene-based polymer.
[0060] (Block B) In the present disclosure, the B block has a proton-accepting group. Therefore, the B block is not particularly limited as long as it has a proton-accepting group.
[0061] The proton-accepting group may be a nitrogen-containing heterocyclic group. The nitrogen-containing heterocyclic group may be, for example, a pyridine ring group, an imidazole ring group, a pyrazole ring group, an imidazoline ring group, an oxazole ring group, a pyrimidine ring group, a pyrazine ring group, a triazole ring group, or a tetrazole ring group. These nitrogen-containing heterocyclic groups are preferably nitrogen-containing heteroaromatic ring groups, and are particularly preferably pyridine ring groups or imidazole ring groups.
[0062] The amount (molar number) of proton accepting groups per 1 g of B block is not particularly limited and may be, for example, 0.1 mmol / g or more, 0.5 mmol / g or more, 1.0 mmol / g or more, 2.5 mmol / g or more, or 5.0 mmol / g or more. From the viewpoint of facilitating the synthesis of the B block and ensuring the handleability of the resulting polymer, the amount (molar number) of proton accepting groups per 1 g of B block may be, for example, 50 mmol / g or less, 40 mmol / g or less, 30 mmol / g or less, or 25 mmol / g or less.
[0063] The repeating units constituting the B block are not particularly limited, and may be derived from, for example, vinyl monomers, ether monomers, ester monomers, amide monomers, silicone monomers, etc. Among these, those derived from vinyl monomers are preferred because the monomers are easily available and the molecules can be easily modified.
[0064] Examples of polymers that can serve as the B block are shown below, but are not limited to these.
[0065] Vinyl polymers having a pyridine ring: poly(2-vinylpyridine), poly(4-vinylpyridine), and the like.
[0066] Vinyl polymers having an imidazole ring: poly(1-vinylimidazole), poly(2-methyl-1-vinylimidazole), poly(2-vinylimidazole), poly(4-vinylimidazole), poly(2-phenyl-1-vinylimidazole), poly(1-vinylcarbazole), poly(2-(1H-imidazol-1-yl)ethyl (meth)acrylate), and the like.
[0067] Vinyl polymers having a pyrazole ring: poly(1-vinylpyrazole), poly(3-vinylpyrazole), and the like.
[0068] Vinyl polymers having an imidazoline ring: poly(1-vinyl-2-imidazoline), poly(1-vinyl-2-methylimidazoline), poly(2-vinyl-2-imidazoline), poly(2-(1H-imidazolin-1-yl)ethyl (meth)acrylate), and the like.
[0069] Vinyl polymers having an oxazole ring: poly(2-phenyl-5-vinyloxazole), etc.
[0070] Vinyl polymers having a pyrimidine ring: poly(5-vinylpyrimidine), poly(2,4-dichloro-6-vinylpyrimidine), etc.
[0071] Vinyl polymers having a pyrazine ring: poly(2-vinylpyrazine), poly(2,5-dimethyl-3-vinylpyrazine), poly(2-methyl-5-vinylpyrazine), and the like.
[0072] Vinyl polymers having a triazole ring: poly(2,4-diamino-6-vinyltriazine), etc.
[0073] Vinyl polymers having a tetrazole ring: poly(1-vinyl-1H-tetrazole), poly(2-vinyl-2H-tetrazole), poly(5-vinyl-1H-tetrazole), poly(1-methyl-5-vinyl-1H-tetrazole), and the like.
[0074] Of these, poly(2-vinylpyridine), poly(4-vinylpyridine) or poly(1-vinylimidazole) is more preferred.
[0075] In this specification, the term "(meth)acrylic acid" is a concept that includes both acrylic acid and methacrylic acid. "(meth)acrylate", "(meth)acrylamide", etc. should be understood in the same manner.
[0076] In the B block, from the viewpoint of ensuring higher proton conductivity and further suppressing leakage of plasticizer through ionic interactions, it is preferable that the proton-accepting groups are present in a proportion of 10 mol % or more of the repeating units constituting the B block.
[0077] The abundance ratio of the proton-accepting group may be 15 mol% or more, 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, 96 mol% or more, or 97 mol% or more. The abundance ratio may be 99.5 mol% or less, 99 mol% or less, 98 mol% or less, 95 mol% or less, 90 mol% or less, 80 mol% or less, 70 mol% or less, 60 mol% or less, 50 mol% or less, 40 mol% or less, or 35 mol% or less.
[0078] The B block combines with a plasticizer described later to form a proton-conductive electrolyte membrane, thereby providing high molecular mobility. Therefore, the glass transition temperature Tg of the B block alone may be relatively high. However, if the glass transition temperature of the B block is too high, the molecular mobility may not be sufficiently improved even after mixing with the plasticizer.
[0079] Thus, the glass transition temperature of the B block may be 400° C. or less, 350° C. or less, 300° C. or less, or 250° C. or less. The B block may have two or more glass transition temperatures. By mixing the B block with the plasticizer, the mixture has a low glass transition temperature, which allows the B block to maintain high molecular mobility during use of the resulting proton-conducting electrolyte membrane. Furthermore, the presence of free protons allows high proton conductivity to be achieved.
[0080] (Block copolymer arrangement) The arrangement of the block copolymer composed of A blocks and B blocks is not particularly limited, and may be, for example, a diblock copolymer such as "AA...AABB...BB" (also called "AB type"), a triblock copolymer such as "AA...AABB...BBAA...AA" (also called "ABA type"), or a triblock copolymer such as "BB...BBAA...AABB...BB" (also called "BAB type").
[0081] In order to more effectively exert the effects of the present disclosure, the block copolymer is preferably an ABA type triblock copolymer constituted by an A block and a B block.
[0082] An example of an ABA type triblock copolymer is shown in Formula 1 below. [ka] In the formula, p is an integer of 2 or more, and may be, for example, 2 or more, 10 or more, 30 or more, 50 or more, 100 or more, 200 or more, 500 or more, 800 or more, 1000 or more, 1500 or more, or 2000 or more, and may be 20000 or less, 15000 or less, 10000 or less, 8000 or less, 5000 or less, or 4000. Furthermore, q is an integer of 1 or more, and may be, for example, 1 or more, 5 or more, 15 or more, 25 or more, 50 or more, or 75 or more, and may be 1000 or less, 500 or less, 400 or less, 250 or less, or 150 or less.
[0083] In addition, as long as the effects of the present disclosure are not impaired, the block copolymer may further contain other monomers or polymers different from the A block and the B block, and may further contain residues of an initiator, a coupling agent, a chain transfer agent, or the like used in producing the block copolymer.
[0084] An example of the block copolymer further having a residue of a chain transfer agent is shown in the following formula 2. [ka] In the formula, m is an integer of 1 or more, and may be, for example, 1 or more, 5 or more, 15 or more, 25 or more, 50 or more, 100 or more, 250 or more, 400 or more, 500 or more, 750 or more, or 1000 or more, and may be 10000 or less, 7500 or less, 5000 or less, 4000 or less, 2500 or less, or 2000. Also, n is an integer of 1 or more, and may be, for example, 1 or more, 5 or more, 15 or more, 25 or more, 50 or more, or 75 or more, and may be 1000 or less, 500 or less, 400 or less, 250 or less, or 150 or less. Also, -R and -SC(S)-S- are residues of chain transfer agents.
[0085] (Synthesis of block copolymers) The method for synthesizing a block copolymer having an A block and a B block is not particularly limited, and for example, the following method can be used, but is not limited thereto.
[0086] That is, in the presence of a small amount of polymerization initiator, a RAFT agent (reversible non-cleavable chain transfer agent) and a monomer constituting an A block (or a B block) are polymerized, and then isolated and purified to synthesize a macro RAFT agent containing an A block (or a B block). Then, by polymerizing this macro RAFT agent and a monomer constituting a B block (or an A block) in the presence of a small amount of polymerization initiator, a block copolymer having an A block and a B block can be synthesized.
[0087] Examples of the polymerization initiator include azo-based radical polymerization initiators such as azobisisobutyronitrile (AIBN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2-cyclopropylpropionitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), and dimethyl 2,2'-azobisisobutyrate; and peroxide-based radical polymerization initiators such as benzoyl peroxide, t-butyl hydroperoxide, and cumene hydroperoxide, but are not limited to these.
[0088] Examples of RAFT agents include thiocarbonylthio compounds such as dithioesters, dithiocarbamates, trithiocarbonates, and xanthates. Specific examples of RAFT agents include, but are not limited to, bis(n-octylmercapto-thiocarbonyl)disulfide, 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid, 2-(dodecylthiocarbonothioylthio)-2-methylpropionic acid, S,S'-bis(α,α'-dimethyl-α''-acetic acid)trithiocarbonate, 2-cyano-2-propyldodecyltrithiocarbonate, 4-cyano-4-(phenylcarbonothioylthio)pentanoic acid, cyanomethyldodecyltrithiocarbonate, and 2-cyano-2-propylbenzodithioate.
[0089] By appropriately selecting the RAFT agent, the desired block copolymer sequence can be synthesized. For example, when a RAFT agent such as a dithioester or dithiocarbamate is used, an AB-type diblock copolymer can be synthesized. When a RAFT agent such as a trithiocarbonate is used, an ABA-type or BAB-type triblock copolymer can be synthesized.
[0090] The average degree of polymerization of the A block is not particularly limited, and may be, for example, 2 or more, 10 or more, 30 or more, 50 or more, 100 or more, or 150 or more, and may be 2000 or less, 1000 or less, 800 or less, 500 or less, or 300 or less. If the average degree of polymerization of the A block is 2 or more, the A blocks are likely to aggregate with each other to form domains at the operating temperature of the proton-conductive electrolyte membrane. If the average degree of polymerization of the A block is 10000 or less, the sample is easily handled. For example, in the case of an ABA-type triblock copolymer, the "average degree of polymerization of the A block" refers to the total average degree of polymerization of the components of the A block contained therein.
[0091] The average degree of polymerization of the B block is not particularly limited, and may be, for example, 2 or more, 10 or more, 30 or more, 50 or more, 100 or more, 200 or more, 500 or more, 800 or more, 1000 or more, 1500 or more, or 2000 or more, and may be 20000 or less, 15000 or less, 10000 or less, 8000 or less, 5000 or less, or 4000. If the average degree of polymerization of the B block is 2 or more, it is easy to mix with a plasticizer to form a more uniform mixed phase. Also, if the average degree of polymerization of the B block is 20000 or less, it is easy to adjust the acidity or basicity of the proton-conductive electrolyte membrane.
[0092] In the present disclosure, the average degree of polymerization is 1 It can be determined by H-NMR.
[0093] <Homopolymer> In the present disclosure, the proton-conductive electrolyte membrane may further contain a homopolymer composed of the above-mentioned A block, in addition to the block copolymer.
[0094] For example, when the copolymer is an ABA type block copolymer, by further containing a homopolymer consisting of an A block, the homopolymer can enter the phase consisting of the block A relative to the phase-separated ABA type block copolymer. This allows the volume fraction of the A block to be adjusted to a desired range in all polymers (copolymers and homopolymers) present in the proton-conductive electrolyte membrane. In addition, by adjusting the volume fraction of this A block, the dimension (one-dimensional or two-dimensional) of the continuous phase of the domain formed by the A block can be adjusted.
[0095] When a homopolymer is contained, its content is not particularly limited as long as it does not impair the effects of the present disclosure, and may be, for example, 1 mol % to 80 mol % relative to 100 mol % of the copolymer.
[0096] <Plasticizer> The plasticizer contained in the proton-conducting electrolyte membrane of the present disclosure includes a proton-donating compound having a pKa of 2.5 or less, pKa of 2.3 or less, pKa of 2.1 or less, pKa of 2.0 or less, pKa of 1.0 or less, pKa of 0.0 or less, pKa of -1.0 or less, or pKa of -2.0 or less. Thus, the plasticizer includes a proton-donating compound having a high degree of acidity, i.e., a compound having a high tendency to release protons.
[0097] In this disclosure, pKa refers to the acid dissociation constant in water at 25°C, and for compounds that dissociate in multiple stages, such as sulfuric acid or phosphoric acid, it refers to the value pKa1 in the first stage of dissociation. For example, the pKa of sulfuric acid is -3.0, and the pKa of phosphoric acid is 1.83 (Reference: "Chemical Handbook," 5th Revised Edition, Chemical Society of Japan, pp. II-332-333, "Evans group pKa table, Harvard University").
[0098] The proton donating compound may be sulfuric acid, phosphoric acid, or an organic acid such as ethanedisulfonic acid or 4-hydroxybenzene-1,3-bis(sulfonic acid). Of these, the proton donating compound is preferably one or more selected from sulfuric acid and phosphoric acid.
[0099] The proton donor compound preferably has a high boiling point or decomposition temperature so that it does not volatilize or decompose at the operating temperature of the proton conductive electrolyte membrane. From this viewpoint, the boiling point or decomposition temperature of the proton donor compound may be, for example, higher than 120° C., 150° C. or higher, or 200° C. or higher.
[0100] The proton donating compound may be one or more selected from sulfuric acid and phosphoric acid, and may be sulfuric acid or phosphoric acid. Note that the boiling point of sulfuric acid is about 290°C (decomposition), and the boiling point of phosphoric acid is about 213°C (decomposition).
[0101] The plasticizer may be composed of only a proton-donating compound, or may be composed of a proton-donating compound and other plasticizers. The other plasticizer may be a plasticizer that does not have proton-donating properties, specifically, for example, polyalkylene glycol, polyvinyl ether, polyol ester, etc. The proportion of the other plasticizer used may be, for example, 50 parts by mass or less, 30 parts by mass or less, 10 parts by mass or less, 5 parts by mass or less, or 1 part by mass or less, when the total mass of the plasticizer is 100 parts by mass, or no other plasticizer may be used at all.
[0102] In this specification, the term "alkylene group" is a concept that encompasses a methylene group, an alkylmethylene group, and a dialkylmethylene group.
[0103] (Molar ratio of proton donor to proton acceptor) The molar ratio of the proton-donating compound to the proton-accepting group (proton-donating compound / proton-accepting group) is not particularly limited, and from the viewpoint of ensuring the function of the proton-donating compound as a plasticizer, it may be, for example, 1.0 or more, 1.1 or more, 1.3 or more, 1.4 or more, 1.5 or more, 1.6 or more, 1.7 or more, 1.8 or more, 1.9 or more, 2.0 or more, 2.1 or more, 2.2 or more, 2.3 or more, 2.4 or more, 2.5 or more, 2.6 or more, 2.7 or more, 2.8 or more, 2.9 or more, 3.0 or more, 3.1 or more, 3.4 or more, 3.5 or more, 3.6 or more, 3.7 or more, 3.8 or more, 3.9 or more, 4.0 or more, 4.1 or more, 4.2 or more, or 4.3 or more. Furthermore, the upper limit of this molar ratio is not particularly limited, and from the viewpoint of maintaining the membrane strength and ensuring the stability as a membrane, it may be, for example, 10.0 or less, 9.0 or less, 8.5 or less, 8.0 or less, 7.5 or less, 7.0 or less, 6.5 or less, 6.0 or less, 5.5 or less, 5.0 or less, 4.5 or less, 4.4 or less, or 4.3 or less.
[0104] Ratio of the copolymer of the present disclosure to the plasticizer The ratio of the copolymer of the present disclosure (i.e., a copolymer having a first portion and a second portion linked by a covalent bond) to the plasticizer may be 50 parts by mass or more, 60 parts by mass or more, 65 parts by mass or more, 70 parts by mass or more, 75 parts by mass or more, or 80 parts by mass or more, based on 100 parts by mass of the copolymer and the plasticizer in total, from the viewpoint of increasing the molecular mobility of the resulting proton-conductive electrolyte membrane and obtaining sufficiently high proton conductivity. On the other hand, from the viewpoint of maintaining the membrane strength and ensuring the stability of the membrane, the ratio of the plasticizer to 100 parts by mass of the copolymer and the plasticizer in total may be 90 parts by mass or less, 85 parts by mass or less, 82 parts by mass or less, 80 parts by mass or less, 75 parts by mass or less, 70 parts by mass or less, or 65 parts by mass or less.
[0105] In the present disclosure, the total number of moles of protons that can be donated by the proton-donating compound having a pKa of 2.5 or less contained in the plasticizer is preferably greater than the total number of moles of protons that can be accepted by the proton-accepting group.
[0106] <Non-fluorinated porous sheet> The proton-conductive electrolyte membrane of the present disclosure may further include a non-fluorine-based porous sheet. In this case, it is preferable that the copolymer and the plasticizer are impregnated into the non-fluorine-based porous sheet. In addition, one of the preferable aspects of "the copolymer and the plasticizer are impregnated into the non-fluorine-based porous sheet" is a state in which the copolymer and the plasticizer permeate the non-fluorine-based porous sheet and cover the surface of the non-fluorine-based porous sheet. By including a non-fluorine-based porous sheet, the proton-conductive electrolyte membrane of the present disclosure is less likely to wrinkle during production, and the handling properties are further improved, that is, the effect of the present disclosure can be more effectively exhibited.
[0107] The non-fluorinated porous sheet according to the present disclosure is preferably made of hydrocarbon fibers.
[0108] More specifically, the non-fluorine-based porous sheet according to the present disclosure is preferably made of fibers of at least one resin selected from the group consisting of polypropylene resin, polyethylene resin, polyester resin, nylon resin, polyamide resin, acrylic resin, cellulose resin, vinylon resin, polyolefin resin, rayon resin, vinyl resin, and synthetic rubber, and more preferably made of fibers of at least one resin selected from polypropylene resin and polyethylene resin.
[0109] Moreover, the non-fluorine-based porous sheet according to the present disclosure may be a non-fluorine-based nonwoven fabric or a non-fluorine-based mesh.
[0110] In the present disclosure, examples of non-fluorinated nonwoven fabrics that may be used include, but are not limited to, general-purpose nonwoven fabrics used in commercially available disposable masks, household gardening nonwoven fabrics manufactured by Nihon Matai Co., Ltd., and Tyvek (registered trademark) 1442R manufactured by Asahi DuPont Flashspun Products Co., Ltd.
[0111] As the non-fluorine-based mesh, for example, PP70 manufactured by NBC Meshtec Co., Ltd. may be used, but the present invention is not limited to this.
[0112] The thickness of the fibers of the non-fluorine-based porous sheet according to the present disclosure is not particularly limited, and may be, for example, about 0.0005 mm or more and about 0.50 mm or less. More specifically, from the viewpoint of smooth proton transfer and suppressing the overall thickness of the proton-conductive electrolyte membrane, the thickness of the fibers may be, for example, 0.50 mm or less, 0.40 mm or less, 0.30 mm or less, 0.20 mm or less, 0.15 mm or less, 0.10 mm or less, 0.08 mm or less, 0.05 mm or less, 0.04 mm or less, 0.03 mm or less, 0.02 mm or less, 0.01 mm or less, 0.025 mm or less, or 0.02 mm or less. Furthermore, from the viewpoint of increasing the tensile strength per fiber, the thickness of such fibers may be, for example, 0.0005 mm or more, 0.001 mm or more to 0.005 mm or more, 0.01 mm or more, 0.015 mm or more, 0.02 mm or more, 0.03 mm or more, 0.04 mm or more, 0.05 mm or more, 0.08 mm or more, 0.10 mm or more, 0.15 mm or more, or 0.20 mm or more.
[0113] It is preferable to appropriately set the above-mentioned fiber thickness in accordance with the properties of the type of non-fluorine-based porous sheet used (for example, in the case of a nonwoven fabric or mesh).
[0114] The thickness of the non-fluorine-based porous sheet is not particularly limited, and from the viewpoint of reducing the overall thickness of the proton-conductive electrolyte membrane, it may be, for example, 0.50 mm or less, 0.45 mm or less, 0.40 mm or less, 0.35 mm or less, 0.30 mm or less, 0.25 mm or less, 0.20 mm or less, 0.18 mm or less, 0.15 mm or less, 0.10 mm or less, 0.09 mm or less, or 0.08 mm or less, and from the viewpoint of increasing the overall tensile strength of the proton-conductive electrolyte membrane, it may be, for example, 0.05 mm or more, 0.08 mm or more, 0.09 mm or more, 0.10 mm or more, 0.15 mm or more, 0.16 mm or more, 0.17 mm or more, 0.18 mm or more, 0.19 mm or more, 0.20 mm or more, or 0.30 mm or more.
[0115] In the proton conducting electrolyte membrane of the present disclosure, when the total amount of the above-mentioned copolymer, plasticizer, and non-fluorine-based porous sheet is taken as 100 parts by mass, the content of the non-fluorine-based porous sheet is not particularly limited, but from the viewpoint of suppressing the occurrence of wrinkles during production and improving the handleability of the proton conducting electrolyte membrane, it is preferable that the content of the non-fluorine-based porous sheet is, for example, 1.0 part by mass or more, 1.5 parts by mass or more, 2.0 parts by mass or more, 2.1 parts by mass or more, 2.2 parts by mass or more, 2.5 parts by mass or more, 3.0 parts by mass or more, 3.5 parts by mass or more, 4.0 parts by mass or more, 4.5 parts by mass or more, 5.0 parts by mass or more, 6.0 parts by mass or more, 7.0 parts by mass or more, 8.0 parts by mass or more, 9.0 parts by mass or more, 10.0 parts by mass or more, 11.0 parts by mass or more, 12.0 parts by mass or more, 13.0 parts by mass or more, 14.0 parts by mass or more, 15.0 parts by mass or more, 16.0 parts by mass or more, 17.0 parts by mass or more, 18.0 parts by mass or more, 19.0 parts by mass or more, 20.0 parts by mass or more, 21.0 parts by mass or more, 22.0 parts by mass or more, 23.0 parts by mass or more, 24.0 parts by mass or more, 25.0 parts by mass or more, 26.0 parts by mass or more, 27.0 parts by mass or more, 28.0 parts by mass or more, 29.0 parts by mass or more, 30.0 parts by mass or more, 31.0 parts by mass or more, 32.0 parts by mass and from the viewpoint of smooth proton transfer and improving proton conductivity, it may be, for example, 50.0 parts by mass or less, 40.0 parts by mass or less, 30.0 parts by mass or less, or 20.0 parts by mass or less, and from the viewpoint of smooth proton transfer and improving proton conductivity, it may be, for example, 50.0 parts by mass or less, 40.0 parts by mass or less, 30.0 parts by mass or less, or 20.0 parts by mass or less.
[0116] Properties of proton-conducting electrolyte membrane (Young's Modulus) The Young's modulus of the proton conductive electrolyte membrane of the present disclosure is preferably greater than 0.10 MPa, and more specifically, is 0.15 MPa or more, 0.25 MPa or more, 0.50 MPa or more, 0.70 MPa or more, 0.90 MPa or more, 1.0 MPa or more, 1.5 MPa or more, 1.8 MPa or more, 2.0 MPa or more, 2.2 MPa or more, 2.5 MPa or more, 2.8 MPa or more, 3.0 MPa or more, 3.5 MPa or more, 4.0 MPa or more, 4.5 MPa or more, 5.0 MPa or more, 5.3 MPa or more, 5.5 MPa or more, 6. 0 MPa or more, 6.5 MPa or more, 7.0 MPa or more, 7.5 MPa or more, 7.9 MPa or more, 8.0 MPa or more, 8.5 MPa or more, 9.0 MPa or more, 9.5 MPa or more, 10.0 MPa or more, 11.0 MPa or more, 12.0 MPa or more, 13.0 MPa or more, 14.0 MPa or more, 15.0 MPa or more, 16.0 MPa or more, 17.0 MPa or more, 18.0 MPa or more, 19.0 MPa or more, 20.0 MPa or more, 25.0 MPa or more, 30.0 MPa or more, or 35.0 MPa or more. The upper limit of the Young's modulus is not particularly limited, and may be, for example, 50.0 MPa or less, or 40.0 MPa or less.
[0117] The Young's modulus of the proton-conductive electrolyte membrane can be determined, for example, from the "tensile test" carried out in the examples.
[0118] (form) The combination of the copolymer and plasticizer that forms the proton-conductive electrolyte membrane of the present disclosure is preferably a viscoelastic solid at least in the temperature range of 50°C or higher and 100°C or lower.
[0119] Here, "viscoelastic solid" means a solid that has viscosity and elasticity, does not show fluidity, and maintains its shape. More specifically, when a material that is a "viscoelastic solid" is subjected to stress to cause a small deformation, the stress against the deformation reaches a maximum immediately after the deformation, and although it decreases over time, it eventually reaches a constant value that is not 0. Furthermore, when the stress that caused the deformation is removed in this state, the deformation becomes small, and in some cases the material returns to its original shape.
[0120] In the proton-conductive electrolyte membrane of the present disclosure, the proton-donating compound as a plasticizer donates a proton to become anionized, and the proton-accepting group of the B block accepts a proton to become cationized, so that the proton-donating compound as a plasticizer remains in the proton-conductive electrolyte membrane due to the electrostatic interaction between them, thereby maintaining the proton-conductive electrolyte membrane as a whole in a viscoelastic solid state. Such a viscoelastic solid is believed to promote molecular motion in the proton-conductive electrolyte membrane due to its characteristic mechanical properties (flexibility), thereby promoting proton conductivity.
[0121] (Film thickness) The proton-conductive electrolyte membrane of the present disclosure has excellent moldability and can be formed into a thin film by a hot melt method or a solvent casting method.
[0122] Therefore, the membrane thickness of the proton conducting electrolyte membrane of the present disclosure can be, for example, 1.50 mm or less, 1.40 mm or less, 1.30 mm or less, 1.20 mm or less, 1.00 mm or less, 0.90 mm or less, 0.80 mm or less, 0.75 mm or less, 0.74 mm or less, 0.73 mm or less, 0.72 mm or less, 0.71 mm or less, 0.70 mm or less, 0.69 mm or less, 0.68 mm or less, 0.65 mm or less, 0.60 mm or less, 0.58 mm or less, 0.56 mm or less, 0.55 mm or less, 0.53 mm or less, 0.50 mm or less, 0.45 mm or less, 0.40 mm or less, 0.35 mm or less, 0.30 mm or less, 0.28 mm or less, 0.25 mm or less, 0.23 mm or less, 0.21 mm or less, or 0.20 mm or less. Moreover, the thickness of the film may be, for example, 0.05 mm or more, or 0.10 mm or more.
[0123] (glass transition temperature) The proton-conductive electrolyte membrane of the present disclosure contains a block copolymer and a plasticizer, and thus exhibits high molecular mobility throughout the membrane. The high molecular mobility of the proton-conductive electrolyte membrane can be evaluated by its low glass transition temperature Tg.
[0124] The proton conductive electrolyte membrane of the present disclosure has high molecular mobility of the plasticizer itself and low glass transition temperature Tg of the mixture of the second part and the plasticizer, so that the molecular mobility can be maintained even at low temperatures, and therefore high proton conductivity can be obtained. The glass transition temperature Tg of the proton conductive electrolyte membrane is preferably equal to or lower than the lower limit of the use temperature of the proton conductive electrolyte membrane, and may be, for example, below room temperature, below 5°C, 2°C or lower, 0°C or lower, -20°C or lower, -40°C or lower, -60°C or lower, -65°C or lower, -70°C or lower, -75°C or lower, -80°C or lower, -84°C or lower, -85°C or lower, or lower than -85°C.
[0125] In this specification, the glass transition temperature Tg is a value obtained in accordance with JIS K 7121:2012 based on a DSC curve obtained by measurement at a temperature increase rate of 10° C. / min.
[0126] (Proton Conductivity) The proton conductive electrolyte membrane of the present disclosure exhibits high proton conductivity in a low humidity or anhydrous environment. The proton conductivity of the proton conductive electrolyte membrane of the present disclosure may be 0.003 S / cm or more in a low humidity or anhydrous environment at 50° C. This value may be, for example, 0.0032 S / cm or more, 0.005 S / cm or more, 0.010 S / cm or more, 0.014 S / cm or more, 0.015 S / cm or more, 0.016 S / cm or more, 0.017 S / cm or more, 0.020 S / cm or more, 0.024 S / cm or more, 0.030 S / cm or more, 0.033 S / cm or more, 0.040 S / cm or more, 0.045 S / cm or more, 0.047 S / cm or more, 0.050 S / cm or more, 0.052 S / cm or more, or 0.060 S / cm or more.
[0127] The proton conductivity of the proton-conducting electrolyte membrane of the present disclosure is, in a low humidity or anhydrous environment at 80° C., for example, 0.010 S / cm or more, 0.015 S / cm or more, 0.019 S / cm or more, 0.020 S / cm or more, 0.024 S / cm or more, 0.027 S / cm or more, 0.029 S / cm or more, 0.030 S / cm or more, 0.035 S / cm or more, 0.040 S / cm or more, 0.0 It may be 43 S / cm or more, 0.046 S / cm or more, 0.048 S / cm or more, 0.050 S / cm or more, 0.059 S / cm or more, 0.060 S / cm or more, 0.063 S / cm or more, 0.070 S / cm or more, 0.076 S / cm or more, 0.080 S / cm or more, 0.082 S / cm or more, 0.090 S / cm or more, 0.093 S / cm or more, or 0.100 S / cm or more.
[0128] Furthermore, the proton conductivity of the proton-conducting electrolyte membrane of the present disclosure may be, for example, 0.050 S / cm or more, 0.060 S / cm or more, 0.062 S / cm or more, 0.070 S / cm or more, 0.075 S / cm or more, 0.080 S / cm or more, 0.085 S / cm or more, 0.088 S / cm or more, 0.097 S / cm or more, 0.100 S / cm or more, 0.120 S / cm or more, 0.130 S / cm or more, 0.140 S / cm or more, 0.150 S / cm or more, 0.160 S / cm or more, 0.170 S / cm or more, or 0.200 S / cm or more in a low humidity or anhydrous environment at 120°C.
[0129] (water content) The proton-conductive electrolyte membrane of the present disclosure exhibits high proton conductivity even when the membrane does not contain water. Therefore, the water content of the proton-conductive electrolyte membrane may be, for example, 10 parts by mass or less, 5 parts by mass or less, 1 part by mass or less, 0.1 parts by mass or less, 0.01 parts by mass or less, or 0.001 parts by mass or less, when the total mass of the membrane is 100 parts by mass.
[0130] (Preparation of proton-conductive electrolyte membrane) Proton conducting electrolyte membranes of the present disclosure can be prepared, for example, by incorporating a plasticizer into a copolymer having a first portion and a second portion that are covalently linked.
[0131] Hereinafter, a method for producing the proton-conductive electrolyte membrane of the present disclosure using an ABA type block copolymer as the copolymer will be described as an example.
[0132] First, a unit monomer for constituting the A block is polymerized to synthesize a polymer that is a precursor of the A block. Next, a unit monomer for constituting the B block is polymerized into a polymer that is a precursor of the A block to prepare an ABA type block copolymer. Then, the solvent used in preparing the ABA type block copolymer is removed to obtain a film of the block copolymer. Here, the means for removing the solvent is not particularly limited, and may be, for example, evaporation at room temperature or by heating. In addition, an operation such as drying may be added as appropriate.
[0133] Next, a plasticizer is introduced into the film of the block copolymer. The method for introducing the plasticizer is not particularly limited, and can be carried out, for example, by the following methods (i) to (ii).
[0134] (i) Dissolving or dispersing the plasticizer in a solvent to prepare a solution or dispersion of the plasticizer. The solvent used here may be selected from polar solvents that have high affinity with the block copolymer and the plasticizer and are stable to strong acids, and is preferably one that evaporates relatively easily. For example, the solvent may be, but is not limited to, an alcohol solvent such as methanol or ethanol, an ether solvent such as dimethyl ether, diethyl ether, or tetrahydrofuran, etc. In addition, the amount of the solvent used here may be, for example, 500 parts by mass or more, 750 parts by mass or more, 1,000 parts by mass or more, 1,250 parts by mass or more, or 1,500 parts by mass or more, relative to 100 parts by mass of the total of the plasticizer and the film of the block copolymer, and may be, for example, 5,000 parts by mass or less, 4,500 parts by mass or less, 4,000 parts by mass or less, 3,500 parts by mass or less, or 3,000 parts by mass or less.
[0135] (ii) The proton-conducting electrolyte membrane of the present disclosure can be obtained by immersing the block copolymer membrane in the solution or dispersion of the plasticizer prepared in (i) above and then removing the solvent. The means for removing the solvent is not particularly limited, and may be, for example, evaporation at room temperature or by heating. In addition, an operation such as drying may be added as appropriate.
[0136] <Fuel cell> The fuel cell of the present disclosure has the proton conductive electrolyte membrane of the present disclosure. In particular, the fuel cell of the present disclosure has a laminate in which a fuel electrode side separator having a fuel flow channel, a fuel electrode side catalyst layer, the proton conductive electrolyte membrane of the present disclosure, an air electrode side catalyst layer, and an air electrode side separator having an air flow channel are laminated in this order. In particular, the fuel cell of the present disclosure has a laminate in which a fuel electrode side separator having a fuel flow channel, a fuel electrode side gas diffusion layer, a fuel electrode side catalyst layer, the proton conductive electrolyte membrane of the present disclosure, an air electrode side catalyst layer, an air electrode side gas diffusion layer, and an air electrode side separator having an air flow channel are laminated in this order. EXAMPLES
[0137] The present disclosure will be described in detail below in the form of examples. The following examples are not intended to limit the application of the present disclosure in any way.
[0138] Example 1 Preparation of the proton-conductive electrolyte membrane of Example 1 In Example 1, a polystyrene triblock copolymer having a relatively large volume fraction of about 30% (hereinafter, φ S A polystyrene-b-poly(4-vinylpyridine)-b-polystyrene (hereinafter also referred to as "SPS triblock copolymer") having the structure (first step) was synthesized, and the proton-conductive electrolyte membrane of Example 1 was produced by swelling this SPS triblock copolymer membrane (also simply referred to as "SPS membrane") with sulfuric acid (H2SO4) (second step).
[0139] In the term "SPS," the "S" at both ends is an abbreviation for polystyrene, which does not have a proton-accepting group and aggregates with each other to form a glassy domain at the operating temperature of the proton-conducting electrolyte membrane, i.e., the "A block" in this disclosure. The "P" in the center is an abbreviation for poly(4-vinylpyridine), which is a polymer having a proton-accepting group, i.e., the "B block" in this disclosure.
[0140] [ka]
[0141] (1) First step (Process 1-1) Styrene monomer was purified by passing it through a column packed with basic alumina. The purified styrene monomer, RAFT agent, and azobisisobutyronitrile (AIBN) were weighed out in amounts of 90.6 g (0.869 mol), 502 mg (0.906 mmol), and 17.1 mg (0.104 mmol), respectively, and mixed in a round-bottom flask with a stopcock to prepare a solution. Nitrogen gas was then bubbled in for 30 minutes, and polymerization was carried out at normal pressure in an oil bath at 130°C while stirring at 500 rpm. After 8 hours, the polymerization reaction was completely stopped by immersing the flask in liquid nitrogen.
[0142] The RAFT agent used was bis(4-[ethyl-(2-hydroxyethyl)carbamoyl]benzyl)trithiocarbonate, and the molar ratio of styrene monomer to RAFT agent was approximately 959:1.
[0143] Tetrahydrofuran (THF) was added to the above reaction solution to prepare a polymer solution of about 8% by mass. This polymer solution was dropped into about 2000 mL of methanol to precipitate a powdered polymer (crude polystyrene). The obtained polymer was separated by suction filtration, thoroughly dried by vacuum drying, and then dissolved again in THF and dropped into methanol to precipitate the polymer. The polymer precipitation process was performed three times in total to remove unreacted monomers and low molecular weight oligomers, and purified polystyrene was obtained.
[0144] The purified polystyrene was dissolved in deuterated chloroform to prepare a solution of about 2% by mass, and the solution was analyzed by proton nuclear magnetic resonance spectroscopy ( 1 The average degree of polymerization was determined by H-NMR, and was found to be 240 and the average molecular weight was approximately 25,000.
[0145] This purified polystyrene was dissolved in N,N-dimethylformamide (DMF) to prepare a solution of about 0.3% by mass, and the molecular weight distribution (Mw / Mn) was determined by gel permeation chromatography (GPC). Standard polystyrene was used for molecular weight calibration. The result was Mw / Mn = 1.15. The eluent was DMF, the flow rate was 1 mL / min, and the elution was performed using a TSK-GEL column 4000H manufactured by Tosoh Corporation. HR The measurements were carried out with three of these connected together.
[0146] (Step 1-2) The purified polystyrene obtained in step 1-1 above had a RAFT agent residue introduced into the center, and was used as a macro RAFT agent (a RAFT agent with a large molecular weight, hence referred to as a "macro RAFT agent") to polymerize with 4-vinylpyridine monomer.
[0147] More specifically, 4-vinylpyridine monomer was purified by passing it through basic alumina. 19.8 g (0.188 mol), 1.37 g (0.0548 mmol), and 19.5 mg (0.119 mmol) of the purified 4-vinylpyridine monomer, macro RAFT agent, and AIBN were weighed out, respectively, and mixed in a round-bottom flask with a stopcock to prepare a solution. Nitrogen gas was then bubbled for 60 minutes, and polymerization was carried out at 70 °C and 500 rpm while stirring in an oil bath at normal pressure. After 1 hour and 5 minutes, the polymerization reaction was completely stopped by immersing the flask in liquid nitrogen.
[0148] The molar ratio of 4-vinylpyridine monomer to macro RAFT agent was approximately 3430:1.
[0149] Chloroform was added to the reaction solution to prepare a polymer solution of about 8% by mass. This polymer solution was dropped into about 800 mL of hexane to precipitate a powdery crude SPS triblock copolymer. The obtained polymer was separated by suction filtration and thoroughly dried by vacuum drying, and then dissolved again in chloroform and dropped into hexane to precipitate the polymer. The polymer precipitation process was performed three times in total to remove unreacted monomers and low molecular weight oligomers, and a purified SPS triblock copolymer was obtained. The purified SPS triblock copolymer of Example 1 is also referred to as "SPS-1".
[0150] SPS-1 was dissolved in deuterated chloroform to prepare a solution of about 2% by mass. 1 The average degree of polymerization was determined by H-NMR. The average degree of polymerization of the A block components combined was 240, and the average degree of polymerization of the B block component chain was 640, giving an overall number average molecular weight of approximately 92,000.
[0151] The density of polystyrene is 1.05 g / cm 3 , the density of poly(4-vinylpyridine) is 1.17 g / cm 3 Therefore, the volume fraction of polystyrene in SPS-1 was 29%.
[0152] In addition, SPS-1 was dissolved in DMF to prepare a solution of about 0.5% by mass, and the Mw / Mn was determined by GPC to be 1.56. The eluent was DMF, the flow rate was 1 mL / min, and the measurement was performed using three TSK-GEL columns G4000HHR (Tosoh Corporation) connected together.
[0153] (3)Second process About 0.6 g of the SPS-1 obtained above was dissolved in about 6 g of pyridine solvent. This solution was poured into a polytetrafluoroethylene (hereinafter referred to as PTFE) beaker (inner diameter 4.3 cm) and left to stand at 50°C for about 2 days to evaporate the volatile solvent (pyridine). After that, the volatile solvent was completely removed by drying at 50°C for about 1 day using a vacuum dryer to obtain an SPS-1 membrane.
[0154] Transmission electron microscope (TEM) observations were performed to observe the nanostructure of the SPS-1 membrane. Ultrathin sections (approximately 80 nm thick) were prepared from the SPS-1 membrane using a microtome method. The P components of the ultrathin sections were stained using iodine (I2) vapor, and TEM observations were performed at an accelerating voltage of 120 kV (equipment: JEOL JEM-1400). The obtained TEM image is shown in Figure 4. Due to the vapor staining with I2, the S phase has a bright contrast and the P phase has a dark contrast, indicating that the SPS-1 membrane has a lamellar structure.
[0155] The detailed molecular characteristics of the SPS-1 membrane are shown in Table 1 below.
[0156] A solution of 0.140 g of concentrated sulfuric acid (98%) dissolved in 1.24 g of methanol was poured into a PTFE container (inner diameter 4.3 cm), 49.2 mg of SPS-1 membrane was immersed in the solution, and the volatile solvent (methanol) was evaporated by leaving it at 50 ° C for about 2 days. The volatile solvent was then completely removed by drying at 50 ° C for about 1 day using a vacuum dryer, and 0.189 g (thickness 0.56 mm) of SPS-1 / H2SO4 membrane in which the SPS-1 membrane was swollen with H2SO4 was obtained as the proton conductive electrolyte membrane of Example 1. During swelling, H2SO4 penetrates only the P component of SPS-1, so that the phase separation interface form, i.e., morphology, of the swollen SPS-1 / H2SO4 membrane is considered to be unchanged from the lamellar structure of the SPS-1 membrane before swelling.
[0157] In the proton conductive electrolyte membrane of Example 1, the weight ratio of SPS-1 to H2SO4 was 26:74, and the molar ratio of sulfuric acid to pyridyl groups (ie, pyridine ring groups) was 4.3.
[0158] <evaluation> (Visual evaluation) As shown in the photograph of Figure 5, the proton-conductive electrolyte membrane obtained in Example 1 is not easily deformed by its own weight or the load applied during contact, and it is self-supporting and not highly adhesive. Therefore, it is easy to handle and a large-area membrane can be produced relatively easily.
[0159] (AC impedance measurement) Using a platinum mesh having a thickness of 0.1 mm as an electrode, the sample of the proton-conductive electrolyte membrane of Example 1 was subjected to AC impedance measurement.
[0160] A sample of the proton-conductive electrolyte membrane of Example 1 cut into a strip (thickness 0.56 mm, width 1.25 mm, length 10 mm) was sandwiched between a pair of electrodes arranged facing each other with an inter-electrode distance of 0.70 cm. The sample sandwiched between the electrodes was placed in a natural convection constant temperature dryer and dried for 1 hour or more under conditions of a temperature of 120°C and a relative humidity of substantially 0% RH. The temperature and relative humidity were measured using a professional thermo-hygrometer testo635-2 (manufactured by Testo).
[0161] A potentiostat / galvanostat with FRA (frequency response analysis) option, VERSASTAT 4-400 (Prinston Applied Research), was used to set the voltage to 80 mV and the frequency to 10 5 Hz to 10 0 The AC impedance was measured under non-humidified conditions, changing the frequency in the range of Hz. The resistance value was read in the frequency range where the absolute value of the resistance was almost constant, and was 8.3 × 10 2 It was Omega.
[0162] The proton conductivity of the sample of the proton-conductive electrolyte membrane was calculated by the following formula (1) and was found to be 0.12 S / cm, which is a very high proton conductivity comparable to that of a humidified Nafion (registered trademark) membrane. Proton conductivity = electrode distance / (membrane thickness x membrane width x resistance) (1)
[0163] Next, AC impedance measurements were performed under the conditions of a temperature of 110°C and a relative humidity of essentially 0%RH. The resistance in the frequency range where the absolute value of the resistance is almost constant was 9.1×10 2 The proton conductivity was 0.11 S / cm, indicating high proton conductivity.
[0164] In addition, when AC impedance measurements were performed under the conditions of a temperature of 95°C and a relative humidity of 2.3%, the resistance value in the frequency range where the absolute value of the resistance value is almost constant was 1.2 × 10 3 Ω and the proton conductivity was 0.085 S / cm.
[0165] In addition, when AC impedance measurements were performed under the conditions of a temperature of 80°C and a relative humidity of 2.4%, the resistance in the frequency range where the absolute value of the resistance is almost constant was 1.6×10 3 Ω and the proton conductivity was 0.063 S / cm.
[0166] In addition, when AC impedance measurements were performed under the conditions of a temperature of 50°C and a relative humidity of 3.0%, the resistance in the frequency range where the absolute value of the resistance is almost constant was 3.0×10 3 Ω and the proton conductivity was 0.033 S / cm.
[0167] The measurement results of the proton conductivity of Example 1 are shown in Table 2 below and in FIG. 6, and are represented by black circles and a solid line in FIG.
[0168] 6, the proton conductivity of the proton-conducting electrolyte membrane of Example 1 tended to increase with increasing temperature. This is believed to be because the molecular mobility of the proton-conducting mixed phase in the pseudo-fluid state increased with increasing temperature, resulting in improved proton conductivity.
[0169] (Tensile test) The sample of the proton conductive electrolyte membrane of Example 1 was punched out with a punching blade to prepare a dog-bone type test piece with a width of 4 mm. The thickness of the test piece was about 0.56 mm. The measurement was performed using Shimadzu Corporation's AGS-X, a 50N load cell, and a 50N clip-type gripper with a gripper distance of about 4.0 mm and an initial strain rate of 0.33 / s (tensile rate of 1.3 mm / s).
[0170] The results of the tensile test of the sample of the proton-conductive electrolyte membrane of Example 1 showed that the Young's modulus, breaking strain, tensile strength, and inner area value of the stress-strain curve (an index of the toughness of the material) were 7.9 MPa, 130%, 2.2 MPa, and 2.0 MJ / m, respectively. 3 This result is also shown in Table 3 below and in FIG. 7, where it is represented by a solid line.
[0171] In addition, the "x" marks in FIG. 7 indicate the breaking points.
[0172] In addition, Young's modulus was determined from the initial gradient of the stress-strain curve (within 10% strain), the maximum stress was determined from the maximum value of stress, and the breaking elongation was determined from the elongation at which breaking occurred.
[0173] Comparative Example 1 <Preparation of proton-conductive electrolyte membrane of Comparative Example 1> In Comparative Example 1, the same procedure as in Example 1 was carried out except that the amount of the styrene monomer and the amount of the 4-vinylpyridine monomer were appropriately changed, and the φ S SPS triblock copolymer with relatively small number average molecular weight (175,000, Mw / Mn=1.95, φ S = 7%, hereinafter referred to as "SPS-2") was synthesized to prepare an SPS-2 membrane.
[0174] When the nanostructure of the SPS-2 film was observed by TEM in the same manner as in Example 1, the image shown in FIG. 8 was obtained, and it was found that the SPS-2 film had a spherical structure.
[0175] Except for appropriately changing the amounts of H2SO4 and methanol, the SPS-2 membrane was swollen with H2SO4 in the same manner as in Example 1 to prepare a proton-conductive electrolyte membrane (also referred to as "SPS-2 / H2SO4 membrane", thickness 0.50 mm). The weight ratio of SPS-2 to H2SO4 was 21:79, and the molar ratio of sulfuric acid to pyridyl groups was 4.2, which was almost the same as in Example 1. During swelling, H2SO4 penetrates only the P component of SPS-2, so it is considered that the morphology of the swollen SPS-2 / H2SO4 membrane does not change from the sphere structure of the SPS-2 membrane before swelling.
[0176] <evaluation> (Visual evaluation) The proton-conductive electrolyte membrane obtained in Comparative Example 1 was soft, so that the sample deformed under its own weight, had low self-supporting ability, and was highly sticky, as shown in the photograph in Figure 9. Therefore, the handling properties were relatively poor, and it was difficult to take out a large-area membrane, making it difficult to handle.
[0177] (AC impedance measurement) AC impedance measurement was performed in the same manner as in Example 1 to measure proton conductivity under non-humidified conditions. The measurement results are shown in Table 2 and Fig. 6. In Fig. 6, they are represented by x and dotted lines. Under non-humidified conditions and in the temperature range of 50 to 120°C, the membrane of Comparative Example 1 showed a conductivity of 0.052 to 0.17 S / cm.
[0178] From this result, it was found that the proton conductive electrolyte membrane of Example 1 exhibited high proton conductivity comparable to that of the proton conductive electrolyte membrane of Comparative Example 1.
[0179] (Tensile test) A tensile test was carried out on the sample of the proton conductive electrolyte membrane of Comparative Example 1 in the same manner as in Example 1. The Young's modulus, breaking strain, tensile strength, and inner area value of the stress-strain curve of the sample of the proton conductive electrolyte membrane of Comparative Example 1 were 0.002 MPa, 77%, 0.01 MPa, and 0.004 MJ / m, respectively. 3 and the proton conductive electrolyte membrane of Comparative Example 1 has a thickness of φ SIt was found that the Young's modulus and tensile strength were about 1 / 3950 and 1 / 220, respectively, lower than those of the proton-conductive electrolyte membrane of Example 1 using SPS-1, which has a large tensile strength. The results of Comparative Example 1 are shown in Table 3 and Fig. 7, and are represented by the dotted line in Fig. 7.
[0180] The reason why the proton-conductive electrolyte membrane of Example 1 exhibited a higher Young's modulus and tensile strength than the proton-conductive electrolyte membrane of Comparative Example 1 is believed to be because the plate-like hard domains of the S component in the lamellar structure formed by SPS-1 exhibit higher continuity than the spherical hard domains of the S component in the spherical structure formed by SPS-2.
[0181] The proton-conductive electrolyte membrane of Comparative Example 1, due to its low Young's modulus, was highly adhesive and easily deformed significantly under the load generated upon contact, and had poor handling properties.
[0182] On the other hand, the proton-conductive electrolyte membrane of Example 1 has a Young's modulus of more than 0.1 MPa, which is higher than that of the proton-conductive electrolyte membrane of Comparative Example 1, and therefore has a relatively low adhesiveness and does not easily deform under the load generated upon contact, and therefore is considered to have had relatively good handleability.
[0183] Example 2 In Example 2, an SPS triblock copolymer (number average molecular weight 73,000, Mw / Mn=1.42, φ) was prepared in the same manner as in Example 1, except that the amount of styrene monomer and the amount of 4-vinylpyridine monomer were appropriately changed. S = 16%, hereinafter referred to as "SPS-3") was synthesized to prepare an SPS-3 membrane.
[0184] When the nanostructure of the SPS-3 film was observed by TEM in the same manner as in Example 1, the image shown in FIG. 10 was obtained, which revealed that the SPS-3 film had a cylindrical structure.
[0185] A proton-conductive electrolyte membrane (also called "SPS-3 / H2SO4 membrane", thickness 0.53 mm) was prepared by swelling the SPS-3 membrane with H2SO4 in the same manner as in Example 1, except that the amounts of H2SO4 and methanol were appropriately changed. The weight ratio of SPS-3 to H2SO4 was 20:80, the molar ratio of sulfuric acid to pyridyl groups was 5.0, and the weight ratio of SPS to H2SO4 was almost equal to that of Comparative Example 1. During swelling, H2SO4 penetrates only the P component of SPS-3, so it is considered that the morphology of the swollen SPS-3 / H2SO4 membrane does not change from the cylindrical structure of the SPS-3 membrane before swelling.
[0186] <evaluation> (Visual evaluation) It was found that the proton-conductive electrolyte membrane obtained in Example 2 was not easily deformed by its own weight or the load applied during contact, and was not highly adhesive. Therefore, the handling properties were relatively good. Due to the characteristics of the proton-conductive electrolyte membrane, it is possible to relatively easily prepare a large-area membrane.
[0187] (AC impedance measurement) The AC impedance measurement was performed in the same manner as in Example 1 to measure the proton conductivity under non-humidified conditions. The measurement results are shown in Table 2 and FIG. 6. In FIG. 6, they are represented by black squares and dashed lines. Under non-humidified conditions and in the temperature range of 50 to 120° C., it was found that the proton conductive membrane of Example 2 exhibited a conductivity of 0.047 to 0.14 S / cm, which is comparable to the proton conductive electrolyte membrane of Comparative Example 1 in high proton conductivity.
[0188] (Tensile test) A tensile test was carried out on the sample of the proton conductive electrolyte membrane of Example 2 in the same manner as in Example 1. The Young's modulus, breaking strain, tensile strength, and inner area value of the stress-strain curve of the sample of the proton conductive electrolyte membrane of Example 2 were 0.18 MPa, 114%, 0.22 MPa, and 0.14 MJ / m, respectively. 3 and the proton-conductive electrolyte membrane of Example 2 has a thickness of φ SIt was found that the Young's modulus and tensile strength were about 90 and 22 times higher, respectively, than the proton-conductive electrolyte membrane of Comparative Example 1 using SPS-2, which has a smaller molecular weight. This result is also shown in Table 3 and Figure 7, and is represented by the dashed line in Figure 7.
[0189] The proton-conductive electrolyte membrane of Example 2 exhibited higher mechanical properties than the proton-conductive electrolyte membrane of Comparative Example 1, presumably because the columnar hard domains of the S component in the cylindrical structure formed by SPS-3 exhibited higher continuity than the spherical hard domains of the S component in the spherical structure formed by SPS-2.
[0190] The proton-conductive electrolyte membrane of Example 2 has a Young's modulus that is about two orders of magnitude higher than that of the proton-conductive electrolyte membrane of Comparative Example 1. It is therefore considered that the proton-conductive electrolyte membrane of Example 2 has lower adhesion than the membrane of Comparative Example 1 and is less susceptible to deformation due to the load generated upon contact, and therefore has relatively good handleability.
[0191] Example 3 In Example 3, an SPS triblock copolymer (number average molecular weight 79,000, Mw / Mn=1.51, φ) was prepared in the same manner as in Example 1, except that the amount of styrene monomer and the amount of 4-vinylpyridine monomer were appropriately changed. S = 44%, hereinafter referred to as "SPS-4") was synthesized to prepare an SPS-4 membrane.
[0192] When the nanostructure of the SPS-4 film was observed by TEM in the same manner as in Example 1, the image shown in FIG. 11 was obtained, which revealed that the SPS-4 film had a lamellar structure.
[0193] Except for appropriately changing the amounts of H2SO4 and methanol, the SPS-4 membrane was swollen with H2SO4 in the same manner as in Example 1 to prepare a proton-conductive electrolyte membrane (also referred to as "SPS-4 / H2SO4 membrane", thickness 0.53 mm). The weight ratio of SPS-4 to H2SO4 was 28:72, and the molar ratio of sulfuric acid to pyridyl groups was 4.7. During swelling, H2SO4 penetrates only the P component of SPS-4, so it is considered that the morphology of the swollen SPS-4 / H2SO4 membrane does not change from the lamellar structure of the SPS-4 membrane before swelling.
[0194] <evaluation> (Visual evaluation) It was found that the proton-conductive electrolyte membrane obtained in Example 3 is unlikely to deform due to its own weight or the load applied during contact, has self-supporting properties, and is not highly adhesive. Therefore, it is easy to handle. Due to the characteristics of the proton-conductive electrolyte membrane, it is possible to relatively easily prepare a large-area membrane.
[0195] (AC impedance measurement) The AC impedance measurement was performed in the same manner as in Example 1 to measure the proton conductivity under non-humidified conditions. The measurement results are shown in Table 2 and FIG. 3. In FIG. 3, they are represented by black triangles and dashed lines. Under non-humidified conditions and in the temperature range of 50 to 120° C., it was found that the proton conductive electrolyte membrane of Example 3 exhibited a conductivity of 0.031 to 0.097 S / cm, which is comparable to the proton conductive electrolyte membrane of Comparative Example 1 in high proton conductivity.
[0196] (Tensile test) A tensile test was carried out on the sample of the proton conductive electrolyte membrane of Example 3 in the same manner as in Example 1. The Young's modulus, breaking strain, tensile strength, and inner area value of the stress-strain curve of the sample of the proton conductive electrolyte membrane of Example 3 were 35 MPa, 19%, 4.5 MPa, and 0.69 MJ / m, respectively. 3 and the proton conductive electrolyte membrane of Example 3 has a thickness of φ SIt was found that, compared to the proton-conductive electrolyte membrane of Comparative Example 1 using SPS-2 with a smaller strain, the breaking strain was smaller, but the Young's modulus and tensile strength were about 17,500 and 450 times higher, respectively. This result is also shown in Table 3 and Fig. 7, and is represented by the dashed line in Fig. 7.
[0197] The reason why the proton-conductive electrolyte membrane of Example 3 exhibited a higher Young's modulus and tensile strength than the proton-conductive electrolyte membrane of Comparative Example 1 is believed to be because the plate-like hard domains of the S component in the lamellar structure formed by SPS-4 exhibit higher continuity than the spherical hard domains of the S component in the spherical structure formed by SPS-2.
[0198] The proton-conductive electrolyte membrane of Example 3 has a Young's modulus (1 MPa or more) four orders of magnitude higher than that of the proton-conductive electrolyte membrane of Comparative Example 1, and therefore has lower adhesion and is less susceptible to deformation due to the load generated upon contact, and therefore has good handleability, compared to the membrane of Comparative Example 1.
[0199] Example 4 In Example 4, an SPS triblock copolymer (number average molecular weight 171,000, Mw / Mn=1.54, φ S = 21%, hereafter referred to as "SPS-5") was synthesized to prepare an SPS-5 film. Based on its composition, SPS-5 is expected to form a cylindrical morphology.
[0200] Except for appropriately changing the amounts of H2SO4 and methanol, the SPS-5 membrane was swollen with H2SO4 in the same manner as in Example 1 to prepare a proton-conductive electrolyte membrane (also referred to as "SPS-5 / H2SO4 membrane", thickness 0.74 mm). The weight ratio of SPS-5 to H2SO4 was 23:77, and the molar ratio of sulfuric acid to pyridyl groups was 4.5. During swelling, H2SO4 penetrates only the P component of SPS-5, so it is believed that the morphology of the swollen SPS-5 / H2SO4 membrane does not change from before swelling.
[0201] <evaluation> (Visual evaluation) It was found that the proton-conductive electrolyte membrane obtained in Example 4 is not easily deformed by its own weight or the load applied during contact, and is not highly adhesive. Therefore, it is easy to handle. Due to the characteristics of the proton-conductive electrolyte membrane, it is relatively easy to prepare a large-area membrane.
[0202] (AC impedance measurement) The AC impedance measurement was performed in the same manner as in Example 1 to measure the proton conductivity under non-humidified conditions. The measurement results are shown in Table 2 and FIG. 12. In FIG. 12, they are represented by black circles and solid lines. Under non-humidified conditions and in the temperature range of 80 to 120° C., it was found that the proton conductive electrolyte membrane of Example 4 exhibited a conductivity of 0.050 to 0.10 S / cm, which is comparable to the proton conductive electrolyte membrane of Comparative Example 1 in high proton conductivity.
[0203] <evaluation> (Visual evaluation) The proton-conductive electrolyte membrane of Example 4 was relatively easy to handle because it was not easily deformed by the load generated upon contact.
[0204] (Tensile test) A tensile test was carried out on the sample of the proton conductive electrolyte membrane of Example 4 in the same manner as in Example 1. The Young's modulus, breaking strain, tensile strength, and inner area value of the stress-strain curve of the sample of the proton conductive electrolyte membrane of Example 4 were 0.90 MPa, 264%, 0.61 MPa, and 1.2 MJ / m, respectively. 3 and the proton-conductive electrolyte membrane of Example 4 has a thickness of φ S It was found that the Young's modulus and tensile strength were about 450 and 61 times higher, respectively, than the proton-conductive electrolyte membrane of Comparative Example 1 using SPS-2, which has a smaller molecular weight. This result is also shown in Table 3 and Figure 7, and is represented by the two-dot chain line in Figure 7.
[0205] The proton conductive electrolyte membrane of Example 4 exhibited higher Young's modulus and tensile strength than the proton conductive electrolyte membrane of Comparative Example 1 because of the φS This is thought to be because the cylindrical hard domains of the S component show higher continuity than the spherical hard domains of the S component in the spherical structure formed by SPS-2.
[0206] The proton-conductive electrolyte membrane of Example 4 has a Young's modulus two orders of magnitude higher than that of the proton-conductive electrolyte membrane of Comparative Example 1, and therefore has lower adhesion than the membrane of Comparative Example 1 and is less susceptible to deformation due to the load generated upon contact, and therefore has relatively good handleability.
[0207] Example 5 In Example 5, a hybrid membrane (hereinafter also simply referred to as "SPS-5 / PP nonwoven membrane") was prepared from SPS-5 synthesized in Example 4 and nonwoven fabric of polypropylene resin, a non-fluorinated hydrocarbon polymer (a nonwoven fabric with a fiber diameter of about 0.02 mm and a thickness of 0.18 mm, used in disposable masks, etc., hereinafter also referred to as "PP nonwoven membrane"). The proton-conductive electrolyte membrane of Example 5 was then produced by swelling the SPS-5 / PP nonwoven membrane with H2SO4.
[0208] 1.21 g of SPS-5 obtained in Example 4 was taken and dissolved in about 12 g of pyridine solvent. This solution was poured into a 4 cm square silicone cup. 24.6 mg of PP nonwoven fabric (thickness 0.18 mm) was submerged in the solution and left to stand at 50 ° C for about 2 days to evaporate the volatile solvent (pyridine). Then, the volatile solvent was completely removed by drying at 50 ° C for about 1 day using a vacuum dryer, and then a part of the membrane consisting of only SPS-5 without nonwoven fabric was cut off to obtain an SPS-5 / PP nonwoven fabric membrane (weight ratio 94.4 / 5.6).
[0209] The SPS-5 / PP nonwoven fabric membrane was swollen with H2SO4 in the same manner as in Example 1, except that the amounts of H2SO4 and methanol were appropriately changed, to prepare a proton-conductive electrolyte membrane (also referred to as "SPS-5 / PP nonwoven fabric / H2SO4 membrane", thickness 1.5 mm).
[0210] In the proton-conductive electrolyte membrane of Example 5, the weight ratio of SPS-5 to H2SO4 was 22:78, the molar ratio of sulfuric acid to pyridyl groups (i.e., pyridine ring groups) was 4.6, and the weight ratio of SPS-5 to PP nonwoven fabric to H2SO4 was 22:1.3:77.
[0211] <evaluation> (Visual evaluation) It was found that the proton-conductive electrolyte membrane obtained in Example 5 was neither poor in homogeneity nor highly adhesive, even though it contained a nonwoven fabric. In addition, the sample was not easily deformed by its own weight or the load applied during contact, and was easy to handle.
[0212] (AC impedance measurement) The AC impedance measurement was performed in the same manner as in Example 1 to measure the proton conductivity under non-humidified conditions. The measurement results are shown in Table 2 and Fig. 12. In Fig. 12, they are represented by black diamonds and two-dot chain lines. Under non-humidified conditions and in the temperature range of 80 to 120°C, it was found that the proton-conductive electrolyte membrane of Example 5 exhibited a conductivity of 0.029 to 0.062 S / cm, and thus exhibited a relatively high proton conductivity of 0.01 S / cm or more.
[0213] Example 6 In Example 6, a mixed membrane (hereinafter, simply referred to as "SPS-5 / S homopolymer membrane") of SPS-5 used in Example 4 and polystyrene homopolymer (hereinafter, simply referred to as "S homopolymer") was prepared. The S homopolymer was synthesized by RAFT polymerization in the same manner as in step 1-1 of Example 1, and its number average molecular weight was 14,000, and Mw / Mn=1.12. Thereafter, the proton-conductive electrolyte membrane of Example 6 was produced by swelling the SPS-5 / S homopolymer membrane with H2SO4.
[0214] More specifically, 0.253 g of SPS-5 obtained in Example 4 was dissolved in about 2.5 g of pyridine solvent. In addition, 0.0130 g of S homopolymer was dissolved in about 0.13 g of pyridine solvent. After mixing these solutions, the mixed solution was poured into a 4 cm x 2 cm PTFE cup and left to stand at 50°C for about 2 days to evaporate the volatile solvent (pyridine). Thereafter, the volatile solvent was completely removed by drying at 50°C for about 1 day using a vacuum dryer, and an SPS-5 / S homopolymer membrane (weight ratio 95.1 / 4.9) was obtained. The φ of this SPS-5 / S homopolymer membrane was S was 24%.
[0215] The SPS-5 / S homopolymer membrane was swollen with H2SO4 in the same manner as in Example 1, except that the amounts of H2SO4 and methanol were appropriately changed, to prepare a proton-conductive electrolyte membrane (also referred to as "SPS-5 / S homopolymer / H2SO4 membrane", thickness 0.25 mm).
[0216] In the proton-conductive electrolyte membrane of Example 6, the weight ratio of SPS-5 to H2SO4 was 22:78, the weight ratio of SPS-5 to S homopolymer to H2SO4 was 22:1.3:73, and the molar ratio of sulfuric acid to pyridyl groups (i.e., pyridine ring groups) was 3.8.
[0217] <evaluation> (Visual evaluation) It was found that the proton-conductive electrolyte membrane obtained in Example 6 was neither poor in homogeneity nor highly adhesive even though it contained the S homopolymer. In addition, the sample was not easily deformed by its own weight or the load applied during contact, and was easy to handle.
[0218] (AC impedance measurement) The AC impedance measurement was performed in the same manner as in Example 1 to measure the proton conductivity under non-humidified conditions. The measurement results are shown in Table 2 and Fig. 12. In Fig. 12, they are represented by black squares and dashed lines. Under non-humidified conditions and in the temperature range of 50 to 120°C, it was found that the proton-conductive electrolyte membrane of Example 6 exhibited a conductivity of 0.017 to 0.088 S / cm, and thus exhibited a relatively high proton conductivity of 0.01 S / cm or more.
[0219] Example 7 In Example 7, the weight ratio was SPS-5 / S homopolymer / H2SO4 = 28 / 2.8 / 69 (SPS-5 / S homopolymer = 91 / 9, SPS-5 / H2SO4 = 29 / 71), and the molar ratio of sulfuric acid to pyridyl groups was 4.5. In the same manner as in Example 6, an SPS-5 / S homopolymer / H2SO4 membrane (thickness 0.49 mm) was prepared as the proton-conductive electrolyte membrane of Example 7. The φ S was 27%.
[0220] <evaluation> (Visual evaluation) It was found that the proton-conductive electrolyte membrane obtained in Example 7 was neither poor in homogeneity nor highly adhesive even though it contained the S homopolymer. In addition, the sample was not easily deformed by its own weight or the load applied during contact, and the handling properties were also good.
[0221] (AC impedance measurement) The AC impedance measurement was performed in the same manner as in Example 1 to measure the proton conductivity under non-humidified conditions. The measurement results are shown in Table 2 and Fig. 12. In Fig. 12, they are represented by black triangles and a chain line. Under non-humidified conditions and in the temperature range of 50 to 120°C, it was found that the proton-conductive electrolyte membrane of Example 7 exhibited a conductivity of 0.016 to 0.085 S / cm, and thus exhibited a relatively high proton conductivity of 0.01 S / cm or more.
[0222] The basic configuration of the proton-conductive electrolyte membranes prepared in the above examples and comparative examples is shown in Table 1 below.
[0223]
Table 1
[0224]
Table 2
[0225]
Table 3
Claims
1. A proton-conducting electrolyte membrane, a copolymer having a first portion and a second portion covalently linked together; and Plasticizer Including, the first portions are aggregated together to form domains at a temperature at which the proton-conductive electrolyte membrane is used, and the second portions bridge the domains; the second portion having a proton accepting group; At least a portion of the domains extend in one or two dimensions; the plasticizer comprises a proton donating compound having a pKa of 2.5 or less, whereby the plasticizer permeates the second portion and reduces the glass transition temperature of the copolymer compared to a case in which the plasticizer is not present; At least a portion of the domains have a cylindrical or lamellar structure; Proton-conducting electrolyte membrane.
2. 2. The proton conducting electrolyte membrane according to claim 1, wherein the copolymer is a block copolymer, and the first portion and the second portion are an A block and a B block of the block copolymer, respectively.
3. The proton conducting electrolyte membrane according to claim 2 , further comprising a homopolymer consisting of the A block.
4. A proton-conducting electrolyte membrane, a copolymer having a first portion and a second portion covalently linked together; and Plasticizer Including, the first portions are aggregated together to form domains at a temperature at which the proton-conductive electrolyte membrane is used, and the second portions bridge the domains; the second portion having a proton accepting group; At least a portion of the domains extend in one or two dimensions; the plasticizer comprises a proton donating compound having a pKa of 2.5 or less, whereby the plasticizer permeates the second portion and reduces the glass transition temperature of the copolymer compared to a case in which the plasticizer is not present; the copolymer is a block copolymer and the first portion and the second portion are, respectively, an A block and a B block of the block copolymer; and Further comprising a homopolymer consisting of the A block, Proton-conducting electrolyte membrane.
5. The proton conducting electrolyte membrane according to claim 4 , wherein at least a portion of the domains has a cylindrical or lamellar structure.
6. The proton-conducting electrolyte membrane according to any one of claims 2 to 5, wherein the block copolymer is an A-B-A type triblock copolymer constituted by the A block and the B block.
7. The proton-conducting electrolyte membrane according to any one of claims 1 to 6, wherein the domains are in a glassy or crystalline state.
8. The proton-conducting electrolyte membrane according to any one of claims 1 to 7, which is isotropic in a planar direction.
9. The proton conducting electrolyte membrane according to any one of claims 1 to 8, wherein the volume fraction of the first portion in all polymers present in the proton conducting electrolyte membrane is 10% or more and 70% or less.
10. The proton-conducting electrolyte membrane according to any one of claims 1 to 9, further comprising a non-fluorine-based porous sheet, and the copolymer and the plasticizer are impregnated into the non-fluorine-based porous sheet.
11. 11. The proton conducting electrolyte membrane according to claim 1, wherein a molar ratio of the proton donating compound to the proton accepting group is 1.0 or more and 10.0 or less.
12. 12. The proton conducting electrolyte membrane according to claim 1, wherein the combination of the copolymer and the plasticizer is a viscoelastic solid at least in the temperature range of 50° C. to 100° C.
13. The proton conducting electrolyte membrane according to any one of claims 1 to 12, wherein the content of the plasticizer is 50 parts by mass or more and 90 parts by mass or less when the total content of the copolymer and the plasticizer is 100 parts by mass.
14. The proton-conducting electrolyte membrane according to any one of claims 1 to 13, wherein the proton-donating compound is at least one selected from sulfuric acid and phosphoric acid.
15. The proton-conducting electrolyte membrane according to any one of claims 1 to 14, wherein the proton-accepting group is a nitrogen-containing heterocyclic group.
16. The proton conducting electrolyte membrane according to any one of claims 1 to 15, wherein the first portion is a polystyrene-based polymer.
Citation Information
Patent Citations
Method for manufacturing membrane electrode assembly used for polymer electrolyte fuel cell, membrane electrode assembly, and fuel cell
JP2010257598A
Proton conductive film with crosslinking structure, and fuel cell
JP2020068130A
Ion conducting polymer comprising partially branched block copolymer and use thereof
US20150307659A1