Flame-retardant polyolefin resin composition and wiring material using same

A flame-retardant polyolefin resin composition with specific components addresses the challenges of wear resistance, flame retardancy, and flexibility in thin wiring materials, ensuring dimensional stability and reducing manufacturing costs.

JP7593857B2Active Publication Date: 2024-12-03FURUKAWA ELECTRIC CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021055919
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-12-03
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Existing wiring materials face challenges in achieving high wear resistance, flame retardancy, and low-temperature flexibility while maintaining dimensional stability, particularly with reduced thickness, and conventional solutions lead to issues like conductor exposure and increased manufacturing costs.

Method used

A flame-retardant polyolefin resin composition comprising specific ratios of high-density polyethylene, polypropylene, ethylene vinyl acetate copolymer, and halogenated flame retardants, along with a flame retardant aid, which forms a coating layer that balances wear resistance, flame retardancy, and low-temperature flexibility.

Benefits of technology

The composition enables the formation of a coating layer with high abrasion resistance, excellent flame retardancy, and dimensional stability, suitable for thin wiring materials without excessive shrinkage, reducing the need for protective members and improving installation workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593857000001
    Figure 0007593857000001
  • Figure 0007593857000002
    Figure 0007593857000002
Patent Text Reader

Abstract

To provide a flame-retardant polyolefin resin composition capable of molding a molded body which expresses excellent fire retardancy, low temperature flexibility, and high abrasion resistance while suppressing excessive shrinkage, and a wiring material provided with a coated layer formed with the composition.SOLUTION: A flame-retardant polyolefin resin composition includes: a resin; a halogen-based flame-retardant agent; and an auxiliary flame-retardant agent of the halogen-based flame-retardant agent, where the halogen-based flame-retardant agent and the auxiliary flame-retardant agent are contained by a rate of total 15-60 pts. mass to 100 pts.mass of the resin, and the resin satisfies specific compositions of composition [A] and [B]. Also provided is a wiring material having a coated layer formed with the composition on an outer peripheral surface of a conductor.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flame-retardant polyolefin resin composition and a wiring material using the same. [Background technology]

[0002] Electrical and electronic devices, vehicles, etc. are usually equipped with wiring materials (insulated wires or cables, (electrical) cords, optical fiber cores, optical fiber cords, optical cables, etc.) that transport power or transmit information. Depending on the application, such wiring materials are required to satisfy required properties such as sufficient flame retardancy and excellent low-temperature flexibility that is flexible even at low temperatures and less likely to cause insulation breakdown, while also being abrasion resistant to prevent exposure of the conductor due to damage (cracks, tears, etc.) to the coating layer even when repeatedly contacted or rubbed against other components or other wiring materials. The abrasion resistance of the wiring material can be improved by providing (attaching) a protective member to the wiring material. However, in this case, the space required for providing the protective member is gradually narrowing, and this is not necessarily applicable to recent electric and electronic devices and the like. Therefore, it is desired that the covering layer of the wiring material itself (the material forming the covering layer) exhibits sufficient abrasion resistance while satisfying the above-mentioned required characteristics. For example, Patent Document 1 proposes a heat-resistant crosslinked electric wire as a wiring material having a covering layer that exhibits abrasion resistance, which is a heat-resistant crosslinked electric wire formed by forming a covering layer covering the periphery of a conductor with a resin composition containing high-density polyethylene, low-density polyethylene, an ethylene copolymer, and an ethylene copolymer modified with an unsaturated carboxylic acid anhydride, a bromine-based flame retardant, and magnesium hydroxide, and in which the total amount of the bromine-based flame retardant and the magnesium hydroxide is 30 to 55 parts by mass relative to 100 parts by mass of the resin, and crosslinking the covering layer, and the hardness and specific gravity of the resin composition are within a specific range. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-132530 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, as electrical and electronic devices and vehicles become more complex and sophisticated, the number of wiring materials installed is increasing, and the installation space is becoming narrower. In addition, there is a demand for the wiring material itself to be further thinned (lightened). For this reason, the installed wiring material frequently comes into contact with and rubs against other members, and the abrasion resistance of the coating layer decreases as the coating layer becomes thinner, particularly for wiring materials with a thinner diameter. Therefore, there is a demand for the development of a material for forming a coating layer that exhibits sufficient abrasion resistance even when the coating layer is thinned (the material itself exhibits high abrasion resistance). However, Patent Document 1 does not consider the realization of such high abrasion resistance that exceeds the conventional abrasion resistance, nor the compatibility with the above-mentioned required properties (flame retardancy and low-temperature flexibility).

[0005] However, when a resin such as high-density polyethylene is used for the coating layer to improve abrasion resistance, problems occur such as the coating layer shrinking after formation, exposing the conductor. Therefore, an electric wire with such a coating layer has poor dimensional stability, and the conductor is easily exposed after installation, which reduces the reliability of the electric wire and the installation state. This problem can be solved by cutting the electric wire once cut (sliced) to a predetermined length again before installation. However, this leads to a deterioration in installation workability and an increase in manufacturing costs.

[0006] The present invention aims to provide a flame-retardant polyolefin resin composition capable of forming a molded article (coating layer) that exhibits high abrasion resistance while suppressing excessive shrinkage and maintaining excellent flame retardancy and low-temperature flexibility. Another object of the present invention is to provide a wiring material that exhibits high abrasion resistance while being excellent in flame retardancy, low-temperature flexibility and dimensional stability. [Means for solving the problem]

[0007] The present inventors have intensively studied materials for forming the coating layer of wiring materials, and have found that by forming the base resin of the material with a resin that satisfies specific compositions [A] and [B] that specify the type and content of copolymers, etc., and then using a halogen-based flame retardant and its flame retardant assistant in a specific ratio with this resin, a molded body (coating layer) that exhibits high abrasion resistance while maintaining excellent flame retardancy and low-temperature flexibility can be formed while suppressing excessive shrinkage. And, it was found that a composition containing the above resin, a halogen-based flame retardant, and its flame retardant assistant can form a molded body (coating layer) that exhibits high abrasion resistance while being excellent in flame retardancy, low-temperature flexibility, and dimensional stability, and is suitable as a material for forming the coating layer (molded body) of wiring materials. Based on this knowledge, the present inventors have further studied and have come up with the present invention.

[0008] That is, the object of the present invention has been achieved by the following means. <1> A flame-retardant polyolefin resin composition comprising a resin, a halogen-based flame retardant, and a flame retardant assistant for the halogen-based flame retardant. The halogen-based flame retardant and the flame retardant auxiliary are contained in a total amount of 15 to 60 parts by mass per 100 parts by mass of the resin, The resin satisfies the following compositions [A] and [B]. [A] The resin contains high-density polyethylene and polypropylene in a total amount of 50 to 80% by mass, the content of the high-density polyethylene in the resin is 10 to 70% by mass, and the total content of homopolypropylene and block polypropylene in the resin is 30% by mass or less. [B] The total content of ethylene-vinyl acetate copolymer, polyethylene copolymer having an acid copolymerization component, acid-modified copolymer thereof, ethylene rubber, and styrene-based elastomer in the resin is 10 mass% or less, and the density is 0.90 g / cm 3 Polymers less than 100% are not required.

[0009] <2> The resin contains a component having a melting point exceeding 200°C in a total amount of 120 parts by mass or less per 100 parts by mass of the resin. <1> The flame-retardant polyolefin resin composition according to claim 1. <3> In the composition [A], the total content of the high-density polyethylene, homopolypropylene and block polypropylene in the resin is 30 mass% or more. <1> or <2> The flame-retardant polyolefin resin composition according to claim 1. <4> The total content of the composition [B] is 5% by mass or less. <1> ~ <3> 13. The flame-retardant polyolefin resin composition according to claim 12. <5> It is a cross-linked product. <1> ~ <4> 13. The flame-retardant polyolefin resin composition according to claim 12. <6> A wiring material having a coating layer on an outer peripheral surface of a conductor, The coating layer is <1> ~ <5> 13. A wiring material formed from the flame-retardant polyolefin resin composition according to any one of claims 1 to 12. <7> Insulated wire for automotive use. <6> The wiring material according to claim 1.

[0010] In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. Effect of the Invention

[0011] The flame-retardant polyolefin resin composition of the present invention can form a molded article (coating layer) that exhibits high abrasion resistance while suppressing excessive shrinkage and maintaining excellent flame retardancy and low-temperature flexibility. Also, the wiring material of the present invention has a tubular molded article of the flame-retardant polyolefin resin composition of the present invention as a coating layer, and exhibits high abrasion resistance while being excellent in flame retardancy, low-temperature flexibility and dimensional stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] [Flame-retardant polyolefin resin composition] The flame-retardant polyolefin resin composition of the present invention contains a resin, a halogen-based flame retardant, and a flame retardant assistant for the halogen-based flame retardant. In addition, the halogen-based flame retardant and the flame retardant assistant are contained in a total amount of 15 to 60 parts by mass per 100 parts by mass of the resin, and the resin satisfies the following compositions [A] and [B]. By combining a resin that satisfies such specific compositions [A] and [B] with a specific ratio of the halogen-based flame retardant and the flame retardant assistant, it is possible to form a molded body that exhibits higher abrasion resistance than conventional molded bodies while suppressing excessive shrinkage and maintaining excellent flame retardancy and low-temperature flexibility, and particularly preferably a coating layer for a wiring material. Therefore, for example, by using the flame-retardant polyolefin resin composition of the present invention as a material for forming a coating layer, it is possible to realize (manufacture) a wiring material that exhibits high abrasion resistance while being excellent in flame retardancy, low-temperature flexibility, and dimensional stability. Composition [A]: High density polyethylene and polypropylene in resin, total amount 50 to 80 mass% The content of high density polyethylene in the resin is 10 to 70% by mass. The percentage of homopolypropylene and block polypropylene in the resin is Total content is 30% by mass or less Composition [B]: Ethylene vinyl acetate copolymer, polyethylene copolymer with acid copolymerization component , acid-modified copolymers thereof, ethylene rubber, and styrene-based elastomers The total content of these in the resin is 10% by mass or less, and the density is 0.90 g / cm m 3 Copolymers less than 100% are not required. Thus, the flame-retardant polyolefin resin composition of the present invention is suitable as a material for forming a covering layer for wiring materials, for example, as a material for forming a thin covering layer for insulated electric wires for automobiles, particularly for thin-walled electric wires.

[0013] The flame-retardant polyolefin resin composition of the present invention may be a non-crosslinked flame-retardant polyolefin resin composition (also referred to as a flame-retardant non-crosslinked polyolefin resin composition) or a crosslinked flame-retardant polyolefin resin composition (also referred to as a flame-retardant crosslinked polyolefin resin composition), and the necessity of crosslinking is appropriately selected depending on the application and required characteristics. When used as a material for forming a covering layer of a wiring material, it is preferably a flame-retardant crosslinked polyolefin resin composition. Among the flame-retardant polyolefin resin compositions of the present invention, compositions intended to be crosslinked are referred to as crosslinkable flame-retardant polyolefin resin compositions, and are distinguished from the above-mentioned flame-retardant non-crosslinked polyolefin resin compositions that are not intended to be crosslinked. In the present invention, the term "flame-retardant polyolefin resin composition" is used as a general term including flame-retardant non-crosslinked polyolefin resin compositions, flame-retardant crosslinked polyolefin resin compositions, and crosslinkable flame-retardant polyolefin resin compositions, unless otherwise specified.

[0014] The flame-retardant crosslinked polyolefin resin composition (crosslinked product) of the present invention is prepared by subjecting a crosslinkable flame-retardant polyolefin resin composition to a crosslinking reaction. The flame-retardant crosslinked polyolefin resin composition has a crosslinked structure in which at least the resin (constituting (co)polymer, etc.) is crosslinked directly or via a crosslinking agent, etc., and exhibits a high level of suppression of excessive shrinkage, flame retardancy, low-temperature flexibility, and abrasion resistance in a well-balanced manner. The crosslinked structure differs depending on the type of crosslinking reaction (crosslinking method), and cannot be clearly and generally defined. The crosslinking reaction (crosslinking method) is not particularly limited, and a known resin crosslinking method, for example, a crosslinking reaction of polyolefin, etc., can be applied. For example, an electron beam crosslinking method, an organic peroxide crosslinking method, and a silane crosslinking method can be mentioned, and the silane crosslinking method is preferred in that it does not require special equipment and can perform a crosslinking reaction treatment with high productivity. In the present invention, the organic peroxide crosslinking method is one of the chemical crosslinking methods, and refers to a method in which a crosslinkable flame-retardant polyolefin resin composition containing an organic peroxide as a crosslinking catalyst is heated to a temperature equal to or higher than the decomposition temperature of the organic peroxide, and the resins are directly crosslinked by the radicals generated from the organic peroxide. In addition, the silane crosslinking method, which is a chemical crosslinking method different from the organic peroxide crosslinking method, refers to a method in which a crosslinkable flame-retardant polyolefin resin composition containing a silane graft resin, which is a silane coupling agent as a crosslinking agent, and a silanol condensation catalyst are brought into contact with moisture, and the silane coupling agent is subjected to a silanol condensation reaction, thereby crosslinking the resin via the silane coupling agent.

[0015] Each component used in the present invention and its content will be described below. <Resin> The resin includes the polymers (including resins, elastomers and rubbers) defined in the above compositions [A] and [B], as well as other polymers. In the present invention, the density of the polymer is a value measured in accordance with "Method A (water displacement method)" specified in Japanese Industrial Standards (JIS) K 7112 (1999). In the present invention, the polymer includes homopolymers and copolymers, and generally means a resin thereof, but also includes an elastomer and a rubber thereof.

[0016] (High density polyethylene: HDPE) High density polyethylene has a density of 0.940 g / cm 3 This polyethylene is also called crystalline hard polyethylene. This HDPE includes homopolymers of ethylene (homopolyethylene) and copolymers of ethylene and α-olefins other than ethylene. The α-olefin is not particularly limited, but may be an α-olefin having 3 to 12 carbon atoms. The density and molecular weight of the high density polyethylene are not particularly limited and may be set appropriately. The flame-retardant polyolefin resin composition may contain one or more types of high-density polyethylene.

[0017] (Polypropylene: PP) The polypropylene may be any polypropylene containing a polymer (composition) containing a propylene component as a main component, and includes a propylene homopolymer (homopolypropylene: h-PP), random propylene (also called ethylene-propylene random copolymer, r-PP), block propylene (also called ethylene-propylene block copolymer, b-PP), and the like. The ethylene-propylene random copolymer refers to a copolymer containing an ethylene component of about 1 to 10% by mass, in which the ethylene component is randomly incorporated into the propylene chain. Here, the ethylene component content is a value measured according to the method described in ASTM D3900. The ethylene-propylene block copolymer refers to a copolymer containing an ethylene or ethylene-propylene rubber (EPR) component of about 5 to 20% by mass, in which the ethylene or EPR component is independently present in the propylene component, forming an island-sea structure. When the flame-retardant polyolefin resin composition of the present invention contains polypropylene, it is preferably a homopolypropylene or a block polypropylene in terms of abrasion resistance. The flame-retardant polyolefin resin composition may contain one or more types of polypropylene.

[0018] (Ethylene vinyl acetate copolymer: EVA) The ethylene-vinyl acetate copolymer may be a copolymer of ethylene and vinyl acetate, and may be an alternating copolymer formed by alternating polymerization of an ethylene component and a vinyl acetate component, a block copolymer formed by combining a polymerization block of an ethylene component and a polymerization block of a vinyl acetate component, or a random copolymer formed by randomly polymerizing an ethylene component and a vinyl acetate component. When the flame-retardant polyolefin resin composition of the present invention contains an ethylene-vinyl acetate copolymer, the flame retardancy and low-temperature flexibility of the composition are improved. The vinyl acetate content (also referred to as VA content) of the ethylene-vinyl acetate copolymer is not particularly limited and is appropriately determined in consideration of the flame retardancy and the like. The density and molecular weight of the ethylene-vinyl acetate copolymer are also not particularly limited and are appropriately set. The ethylene-vinyl acetate copolymer contained in the flame-retardant polyolefin resin composition may be one type or two or more types.

[0019] (Polyethylene copolymer having an acid copolymerization component) The acid copolymerization component constituting the polyethylene copolymer having an acid copolymerization component is not particularly limited, and examples thereof include carboxylic acid compounds such as (meth)acrylic acid, and (meth)acrylic acid alkyl ester compounds. Here, the alkyl group of the (meth)acrylate is preferably one having 1 to 12 carbon atoms. Examples of polyolefin copolymers having an acid copolymerization component include ethylene-(meth)acrylic acid copolymers and ethylene-(meth)alkyl acrylate copolymers. More specifically, examples of the copolymers described in paragraph

[0017] of Patent Document 1 include the copolymers described in Patent Document 1. For the polyethylene copolymer having an acid copolymerization component, the contents described in Patent Document 1 can be appropriately referred to, and the contents are incorporated as they are into the present specification as a part of the description. In the present invention, the polyethylene copolymer having an acid copolymerization component does not include the above-mentioned ethylene-vinyl acetate copolymer. The flame-retardant polyolefin resin composition may contain one or more types of polyethylene copolymer having an acid copolymerization component.

[0020] (Acid-modified copolymer) The acid-modified copolymer includes the acid-modified copolymer of the ethylene-vinyl acetate copolymer and the acid-modified copolymer of the polyethylene copolymer having the acid copolymerization component. Specifically, the ethylene-vinyl acetate copolymer or the polyethylene copolymer having the acid copolymerization component is modified with an unsaturated carboxylic acid compound (also simply called unsaturated carboxylic acid) or its anhydride. Such an acid-modified copolymer has an unsaturated carboxylic acid-derived group, usually as a side chain (pendant chain, graft chain, etc.), as a result of the reaction of an unsaturated group of an unsaturated carboxylic acid with the copolymer. The amount of modification by the unsaturated carboxylic acid in the acid-modified polyolefin polymer is not particularly limited, but is preferably 0.1 to 2.0 mass %, more preferably 0.2 to 1.0 mass %, based on the copolymer (before modification). The acid-modified copolymer may be synthesized as appropriate, or a commercially available product may be used. When synthesizing the acid-modified copolymer, the copolymer and the unsaturated carboxylic acid are usually heated and mixed in the presence of an organic peroxide at a temperature equal to or higher than the decomposition temperature of the organic peroxide to modify the copolymer (react with the unsaturated carboxylic acid) to obtain the copolymer. The unsaturated carboxylic acid (including anhydride) is not particularly limited, and a suitable example is a carboxylic acid having an unsaturated bond capable of reacting with the copolymer (for example, radical addition reaction). The unsaturated carboxylic acid may have one or more carboxyl groups. Specific examples of preferred unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, itaconic acid, and fumaric acid, as well as metal salts or organic salts thereof, and unsaturated carboxylic acid anhydrides such as maleic anhydride, itaconic anhydride, and fumaric anhydride. The unsaturated carboxylic acid modified to the copolymer may be one or more. As the unsaturated carboxylic acid, maleic anhydride or acrylic acid is preferred. The flame-retardant polyolefin resin composition may contain one or more types of acid-modified copolymer.

[0021] (Ethylene rubber) The ethylene rubber is not particularly limited as long as it is a rubber (including elastomer) made of a copolymer obtained by copolymerizing a compound having an ethylenically unsaturated bond, and known rubbers can be used.Preferably, the ethylene rubber includes a binary copolymer rubber of ethylene and an α-olefin, a ternary copolymer rubber of ethylene, an α-olefin, and a diene, and the like.The diene compound constituting the ternary copolymer may be a conjugated diene compound or a non-conjugated diene compound, but a non-conjugated diene compound is preferred. The α-olefin is preferably an α-olefin having 3 to 12 carbon atoms. Examples of the conjugated diene compound include butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc., and butadiene compounds are preferred. Specific examples of the non-conjugated diene compound include dicyclopentadiene (DCPD), ethylidenenorbornene (ENB), 1,4-hexadiene, etc. As the binary copolymer rubber, ethylene-propylene rubber (EPM) is preferred, and as the ternary copolymer rubber, ethylene-propylene-diene rubber (EPDM) is preferred. The flame-retardant polyolefin resin composition may contain one or more types of ethylene rubber.

[0022] (styrene elastomer) The styrene-based elastomer refers to a polymer having a component derived from an aromatic vinyl compound in the molecule. Examples of such styrene-based elastomers include block copolymers and random copolymers of conjugated diene compounds and aromatic vinyl compounds, or hydrogenated products thereof. Examples of such styrene-based elastomers include styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-isoprene-styrene block copolymers (SIS), hydrogenated SIS, styrene-butadiene-styrene block copolymers (SBS), hydrogenated SBS, styrene-ethylene-ethylene-propylene-styrene block copolymers (SEEPS), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-butadiene rubber (SBR), hydrogenated styrene-butadiene rubber (HSBR), etc. The flame-retardant polyolefin resin composition may contain one or more types of styrene-based elastomer.

[0023] (Density is 0.90g / cm 3 (polymers less than The flame-retardant polyolefin resin composition of the present invention has a density of 0.90 g / cm 3 Polymers less than 100% are not required. stomach. In the present invention, the phrase "polymer is not essential" includes both an embodiment in which no polymer is contained and an embodiment in which a polymer may be contained within a range that does not impair the effects of the present invention. The range in which the effects of the present invention are not impaired is not unique depending on the composition of the flame-retardant polyolefin resin composition, but is, for example, 1 mass % or less in 100 mass % of the resin. Density 0.90g / cm 3 The polymer having a density of less than 1000 nm is not particularly limited, but examples thereof include ultra-low density polyethylene (VLDPE, ULDPE) that satisfies the above density, and polyolefin elastomers that satisfy the above density (for example, CAS No. 25087-34-7). The flame-retardant polyolefin resin composition has a density of 0.90 g / cm 3 When the polymer contains less than 100 parts by weight, the polymer may be one type or two or more types.

[0024] (Other polymers) The flame-retardant polyolefin resin composition of the present invention may contain a polymer other than the above-mentioned polymers. Examples of such a polymer include a polymer other than high-density polyethylene having a density of 0.90 g / cm3. 3 Examples of the polyethylene include the above-mentioned polyethylenes (for example, low-density polyethylene (LDPE), ultra-high molecular weight polyethylene (UHMW-PE), linear low-density polyethylene (LLDPE)), halogen resins, and acid-modified polymers thereof. As the other polymer, low-density polyethylene or linear low-density polyethylene is preferred, and linear low-density polyethylene is more preferred, in that it can achieve a high level of both shrinkability and low-temperature flexibility and abrasion resistance, which are in a trade-off relationship. Other polymers with a density of 0.90 g / cm 3 Although the above-mentioned ultra-low density polyethylene may be contained, it is preferable from the viewpoint of abrasion resistance not to contain it (it is not essential).

[0025] (Organic mineral oil) In order to maintain low-temperature flexibility while exhibiting high abrasion resistance, it is preferable that the flame-retardant polyolefin resin composition of the present invention does not necessarily contain (does not contain) organic mineral oil. The meaning of "not essential" is as described above. Examples of organic mineral oils include those that are commonly used in resin compositions, such as paraffinic oils and naphthenic oils. The organic mineral oils have a density of 0.90 g / cm 3 In the present invention, the density of the polymer is less than 0.90 g / cm. 3 All of the above are classified as organic mineral oils.

[0026] (Resin Composition) The resins contained in the flame-retardant polyolefin resin composition of the present invention are set to a ratio that totals 100% by mass and satisfy the following compositions [A] and [B]. The resin satisfies both compositions [A] and [B], so that a molded article that exhibits high abrasion resistance while suppressing excessive shrinkage and maintaining excellent flame retardancy and low-temperature flexibility can be formed. Therefore, by using it as a material for forming a coating layer for wiring material, the coating layer can be made thin, and it is not necessary to attach a protective member after arranging the wiring material. Composition [A]: High density polyethylene and polypropylene in resin, total amount 50 to 80 mass% The content of high density polyethylene in the resin is 10 to 70% by mass. The percentage of homopolypropylene and block polypropylene in the resin is Total content is 30% by mass or less Composition [B]: Ethylene vinyl acetate copolymer, polyethylene copolymer with acid copolymerization component , acid-modified copolymers thereof, ethylene rubber, and styrene-based elastomers The total content of these in the resin is 10% by mass or less, and the density is 0.90 g / cm m 3 Copolymers less than 100% are not required.

[0027] (Composition [A]) The resin contains high density polyethylene and polypropylene in a total ratio of 50 to 80 mass% in 100 mass% of the resin. This, combined with the action and effect of the composition [B], allows the low temperature flexibility and abrasion resistance, which are in a trade-off relationship, to be compatible at a high level while maintaining excellent flame retardancy while suppressing excessive shrinkage. The total content of high density polyethylene and polypropylene is preferably 55 to 80 mass%, more preferably 60 to 80 mass%, in that excessive shrinkage suppression, flame retardancy, low temperature flexibility and abrasion resistance can be realized at a well-balanced high level. Here, the content of polypropylene is the total amount (total amount) of the content of homopolypropylene, the content of random propylene and the content of block propylene. The content of high-density polyethylene in 100% by mass of the resin is set to 10 to 70% by mass, taking into consideration the above total content. This allows the effects of using it in combination with polypropylene to be complementarily expressed, and allows both excessive shrinkage suppression and low-temperature flexibility to be achieved while maintaining excellent abrasion resistance and flame retardancy. The content of high-density polyethylene is preferably 30 to 70% by mass, more preferably 30 to 60% by mass, in that excessive shrinkage suppression, flame retardancy, low-temperature flexibility and abrasion resistance can be achieved at a well-balanced high level. Among polypropylenes, the total content of homopolypropylene and block polypropylene in 100% by mass of the resin is set to 30% by mass or less. This allows the effect of using it in combination with high-density polyethylene to be complementarily expressed, and allows both excessive shrinkage suppression and low-temperature flexibility to be achieved while maintaining excellent abrasion resistance and flame retardancy. The above total content is preferably 0 to 25% by mass, more preferably 10 to 25% by mass, in that excessive shrinkage suppression, flame retardancy, low-temperature flexibility, and abrasion resistance can be achieved at a well-balanced high level.

[0028] The composition [A] may satisfy the above-mentioned composition, but it is also preferable that the composition [A] satisfies the following composition. The total content of polypropylene in 100% by mass of resin is not particularly limited, and is appropriately determined in consideration of the total content of high-density polyethylene and polypropylene. For example, in terms of low-temperature flexibility and excessive shrinkage suppression, it is preferably 60% by mass or less, more preferably 0 to 50% by mass, and even more preferably 20 to 50% by mass. The total content of polypropylene is the total (total) of the content of homopolypropylene, the content of random propylene, and the content of block propylene. The mass ratio of the content of high-density polyethylene to the content (total) of polypropylene [content of high-density polyethylene / content (total)] is not particularly limited. The total content of the high density polyethylene, homopolypropylene and block polypropylene in 100% by mass of the resin is not particularly limited, and is appropriately determined in consideration of the content of the high density polyethylene and the total content of the homopolypropylene and block polypropylene. For example, in order to further improve the abrasion resistance, it is preferably 30% by mass or more, more preferably 30 to 70% by mass, and even more preferably 40 to 70% by mass. The mass ratio of the content of the high density polyethylene to the total content of the homopolypropylene and block polypropylene [the content of the high density polyethylene / the total content of the homopolypropylene and block polypropylene] is not particularly limited. Furthermore, the mass ratio of the total content of polypropylene to the total content of homopolypropylene and block polypropylene [total content of polypropylene / total content of homopolypropylene and block polypropylene] is not particularly limited.

[0029] (Composition [B]) The resin contains ethylene-vinyl acetate copolymer, polyethylene copolymer having an acid copolymerization component, acid-modified copolymers thereof, ethylene rubber, and styrene-based elastomer in a total content of 10% by mass or less based on 100% by mass of the resin. This, combined with the effect of composition [A], makes it possible to suppress excessive shrinkage while maintaining excellent flame retardancy, and simultaneously achieve a high level of low-temperature flexibility and abrasion resistance, which are in a trade-off relationship. The above total content is preferably 0 to 5% by mass, in that it is possible to achieve a high level of a well-balanced suppression of excessive shrinkage, flame retardancy, low-temperature flexibility, and abrasion resistance. The resin has a density of 0.90 g / cm 3 This makes it possible to obtain an excellent effect of improving abrasion resistance.

[0030] The composition [B] may satisfy the above-mentioned composition, but it is also preferable that the composition [B] satisfies the following composition. The content of the ethylene-vinyl acetate copolymer in 100% by mass of the resin is appropriately determined taking into consideration the above composition [B]. For example, from the standpoint of flame retardancy, abrasion resistance, etc., it is preferably 10% by mass or less, and more preferably 0 to 5% by mass. The content of the polyethylene copolymer having an acid copolymerization component in 100% by mass of the resin is appropriately determined taking into consideration the above composition [B]. For example, from the viewpoint of abrasion resistance, etc., it is preferably 10% by mass or less, and more preferably 0 to 5% by mass. The content of the acid-modified copolymer in 100% by mass of the resin is appropriately determined taking into consideration the above-mentioned composition [B]. For example, in terms of abrasion resistance and flame retardancy, it is preferably 10% by mass or less, and more preferably 0 to 5% by mass. The content of the ethylene rubber in 100% by mass of the resin is appropriately determined taking into consideration the above composition [B]. For example, from the standpoint of abrasion resistance, etc., it is preferably 10% by mass or less, and more preferably 0 to 5% by mass. The content of the styrene-based elastomer in 100% by mass of the resin is appropriately determined taking into consideration the above composition [B]. For example, from the standpoint of abrasion resistance, etc., it is preferably 10% by mass or less, and more preferably 0 to 5% by mass.

[0031] (Other polymer compositions) The resin contained in the flame-retardant polyolefin resin composition of the present invention may satisfy the above-mentioned compositions [A] and [B]. However, when the resin contains the above-mentioned other polymers, the content of the other polymers in 100 mass% of the resin is appropriately determined taking into consideration the above-mentioned compositions [A] and [B]. The content of the other polymer is, for example, preferably 50% by mass or less, and more preferably 10 to 40% by mass. When the other polymer is polyethylene (particularly LLDPE), the content can be set within the above range, or can be set to an appropriate content regardless of the above range.

[0032] <Halogen-based flame retardants> The flame-retardant polyolefin resin composition of the present invention contains a halogen-based flame retardant in the presence of a flame retardant assistant described later. This allows a high flame retardant effect to be effectively exhibited by using the flame retardant assistant in combination, and the content can be reduced. Therefore, the deterioration of abrasion resistance due to the inclusion of a halogen-based flame retardant can be effectively suppressed. The halogen-based flame retardant is not particularly limited as long as it is a flame retardant having a halogen atom, but preferred examples include a chlorine-based flame retardant containing a chlorine atom and a bromine-based flame retardant containing a bromine atom, and a bromine-based flame retardant having a high flame retardancy enhancing effect by the flame retardant assistant described later is preferred. The brominated flame retardant is not particularly limited, and those that are usually used in flame retardant compositions can be used without any particular limitation. Examples of the brominated flame retardant include brominated ethylene bisphthalimide compounds, bisbrominated phenyl terephthalamide compounds, brominated bisphenols (e.g., tetrabromobisphenol A) compounds, 1,2-bis(bromophenyl)ethane compounds, polybrominated diphenyl ethers (e.g., decabromodiphenyl ether) compounds, polybromobiphenyls (e.g., tribromophenyl) compounds, hexabromocyclododecane, brominated polystyrene, and hexabromobenzene. In addition to these, examples of the brominated flame retardants include those described in paragraph

[0020] of Patent Document 1. For the brominated flame retardant, the contents described in Patent Document 1 can be appropriately referred to, and the contents are incorporated as they are into the present specification as a part of the description. The chlorine-based flame retardant is not particularly limited, and can be any of those commonly used in flame retardant compositions. For example, decachlorododecahydrodimethanocyclooctene compounds, 1,6,7,8,9,14,15,16,17,17,18,18-dodecachloropentacyclo[12.2.1.16,9.02,13.05,10]octadeca-7,15-diene (Dechlorane Plus), etc. can be mentioned.

[0033] <Flame retardant synergist> The flame-retardant polyolefin resin composition of the present invention contains a flame retardant assistant for a halogen-based flame retardant. The flame retardant assistant is one that exerts a high flame retardant effect exceeding the flame retardant effect exhibited by the halogen-based flame retardant alone due to a synergistic effect when used in combination with the halogen-based flame retardant. Such a flame retardant assistant can be one that is normally used in flame-retardant compositions and is not particularly limited, and is appropriately selected according to the halogen-based flame retardant. For example, antimony oxide such as antimony trioxide is preferably used. Antimony trioxide can react stepwise with the halogen-based flame retardant to exert a high flame retardant effect.

[0034] <Composition of flame retardants, etc.> The flame-retardant polyolefin resin composition of the present invention contains a halogen-based flame retardant and a flame retardant auxiliary in a total amount of 15 to 60 parts by mass per 100 parts by mass of the resin, which allows the composition to exhibit high flame retardancy and, in combination with the composition of the resin, to exhibit remarkable abrasion resistance. The total content of the halogen-based flame retardant and the flame retardant assistant is preferably 30 to 60 parts by mass, and more preferably 30 to 50 parts by mass, in order to achieve a well-balanced high level of excessive shrinkage suppression, flame retardancy, low-temperature flexibility, and abrasion resistance.

[0035] As long as the above total content of the halogen-based flame retardant and the flame retardant auxiliary is satisfied, the respective contents thereof may be appropriately determined. For example, the content of the halogen-based flame retardant is preferably 10 to 55 parts by mass or less, more preferably 15 to 50 parts by mass, and even more preferably 15 to 40 parts by mass, per 100 parts by mass of the resin, in order to achieve a good balance between flame retardancy and abrasion resistance. The content of the flame retardant auxiliary is preferably 5 to 30 parts by mass, more preferably 5 to 25 parts by mass, and even more preferably 5 to 20 parts by mass, relative to 100 parts by mass of the resin, in order to enhance the flame retardant effect of the halogen-based flame retardant and achieve a good balance between flame retardancy and abrasion resistance. The mass ratio of the content of the halogen-based flame retardant to the content (total amount) of the flame retardant assistant [content of the halogen-based flame retardant / content (total amount) of the flame retardant assistant] is usually appropriately determined in consideration of the flame retardancy enhancing action of the halogen-based flame retardant and the flame retardant assistant (for example, the above reaction). The mass ratio [content of the halogen-based flame retardant / content (total amount) of the flame retardant assistant] is, for example, preferably 1 to 3, more preferably 1.5 to 2.5.

[0036] <Other ingredients> In addition to the above-mentioned resin, halogen-based flame retardant, and flame retardant assistant, the flame-retardant polyolefin resin composition of the present invention may contain various components such as additives generally used in resin compositions (referred to as other components) within the scope of the present invention. Examples of other components include inorganic fillers (including flame retardants), antioxidants (antioxidants), lubricants, crosslinking agents, crosslinking assistants, etc. The crosslinkable flame-retardant polyolefin resin composition preferably further contains a crosslinking agent, a crosslinking assistant, a crosslinking catalyst, a crosslinking accelerator, etc., depending on the type of crosslinking reaction to be applied. The flame-retardant polyolefin resin composition may contain one or more types of each of the other components.

[0037] (Inorganic filler) As the inorganic filler, any filler that is usually used as a filler in a resin composition can be used without any particular limitation. Examples of inorganic fillers include metal hydrates such as compounds having hydroxyl groups or crystal water, such as aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, hydrated aluminum silicate, hydrated magnesium silicate, basic magnesium carbonate, hydrotalcite, and talc. Other examples include boron nitride, silica (crystalline silica, amorphous silica, etc.), carbon, clay (calcined clay), zinc oxide, tin oxide, titanium oxide, silicone compounds, quartz, zinc borate, white carbon, zinc borate, zinc hydroxystannate, and zinc stannate. Some of the above compounds have a flame retardant effect in addition to a filling effect, but are classified as inorganic fillers in the present invention. Of the inorganic fillers mentioned above, metal hydroxides such as aluminum hydroxide and magnesium hydroxide are preferred, with magnesium hydroxide being preferred because it has a high ability to form a shell upon combustion and exhibits high flame retardancy.

[0038] The inorganic filler may be surface-treated with a silane coupling agent or the like. Examples include Kisuma 5L and Kisuma 5P (both trade names, magnesium hydroxide, manufactured by Kyowa Chemical Industry Co., Ltd.). The amount of the silane coupling agent used to surface-treat the inorganic filler is not particularly limited, but is preferably, for example, 3 mass% or less. The inorganic filler is usually contained as a powder or particles. The average particle size in this case is not particularly limited, but is preferably 0.2 to 10 μm. If the average particle size is within the above range, secondary aggregation can be suppressed. The average particle size is determined by dispersing the inorganic filler in alcohol or water and using an optical particle size measuring device such as a laser diffraction / scattering type particle size distribution measuring device.

[0039] The content of the inorganic filler in the flame-retardant polyolefin resin composition is not particularly limited and may be appropriately determined, but is preferably determined in consideration of the content (total amount) of components having a melting point exceeding 200° C., which will be described later. The content of the inorganic filler is, for example, preferably 100 parts by mass or less, more preferably 75 parts by mass or less, and even more preferably 70 parts by mass or less.

[0040] (Anti-aging agent) The age inhibitor (antioxidant) is not particularly limited, but examples thereof include amine antioxidants, phenol antioxidants, and sulfur antioxidants, with phenol antioxidants being preferred. The content of the antioxidant in the flame-retardant polyolefin resin composition is set within a range that does not impair the effects of the present invention, and can be, for example, 0.5 to 15 parts by mass per 100 parts by mass of the resin.

[0041] (lubricant) The lubricant is not particularly limited, but examples thereof include silicone compounds, fatty acid metal salts, and fatty acid amides, with silicone compounds being preferred. The content of the lubricant in the flame-retardant polyolefin resin composition is set within a range that does not impair the effects of the present invention, and can be, for example, 0 to 5 parts by mass per 100 parts by mass of the resin.

[0042] (Components with melting points exceeding 200°C) The flame-retardant polyolefin resin composition of the present invention may contain a total of 120 parts by mass or less of the above-mentioned other components having a melting point of more than 200°C. Examples of components having a melting point of more than 200°C include components (compounds) other than the above-mentioned resins that have a melting point of more than 200°C, and specifically refer to components that can exist in a solid state (particles, powder) during melt mixing when preparing the flame-retardant polyolefin resin composition (the components themselves do not change, specifically, do not melt, decompose (thermal decomposition), or change in quality (removal of hydration water, etc.)). The melting point may be more than 200°C, but is preferably higher than the melt mixing temperature described below, and can be, for example, 250°C or higher or 270°C or higher. Such components are not particularly limited, but include, for example, inorganic compounds, more specifically, the above-mentioned inorganic fillers, and further include halogen-based flame retardants, flame retardant assistants, and the like. When the total content of components having a melting point exceeding 200°C is 120 parts by mass or less relative to 100 parts by mass of the resin, the effect of containing each component can be obtained without excessively impairing shrinkage suppression, flame retardancy, low-temperature flexibility, and abrasion resistance. The total content of the above components is, for example, preferably 120 parts by mass or less, more preferably 30 to 100 parts by mass, and even more preferably 45 to 100 parts by mass relative to 100 parts by mass of the resin. In the present invention, the melting point is a value measured in an ordinary pressure (1 atm) environment according to the method specified in JIS K 0064.

[0043] (Silane coupling agent) In the present invention, when the crosslinkable flame-retardant polyolefin resin composition is crosslinked by the electron beam crosslinking method or the silane crosslinking method, the crosslinkable flame-retardant polyolefin resin composition contains one or more silane coupling agents as a crosslinking agent. The silane coupling agent has a grafting reaction site (group or atom) that can undergo a grafting reaction with a resin in the presence of a radical generated by irradiation with an electron beam or decomposition of an organic peroxide. The silane coupling agent used in the silane crosslinking method further has a hydrolyzable group capable of silanol condensation, and it is preferable that this hydrolyzable group can react with the site of the inorganic filler that can be chemically bonded. The grafting reaction site of the silane coupling agent is preferably an ethylenically unsaturated group, and the hydrolyzable group is preferably, for example, an alkoxysilyl group.

[0044] The silane coupling agent having the above-mentioned site is not particularly limited, and may be the silane coupling agent that has been used in the electron beam crosslinking method or the silane crosslinking method.Specifically, may be vinyl alkoxysilane such as vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tributoxysilane, vinyl dimethoxyethoxysilane, vinyl dimethoxybutoxysilane, vinyl diethoxybutoxysilane, allyl trimethoxysilane, allyl triethoxysilane, vinyl triacetoxysilane, methacryloxypropyl trimethoxysilane, methacryloxypropyl triethoxysilane, methacryloxypropyl methyl dimethoxysilane, etc. (meth) acryloxy alkoxysilane. The content of the silane coupling agent in the flame-retardant polyolefin resin composition is preferably from 2 to 15 parts by mass, more preferably from 2.5 to 12 parts by mass, and even more preferably from 3 to 10 parts by mass, based on 100 parts by mass of the resin.

[0045] (organic peroxide) When the crosslinkable flame-retardant polyolefin resin composition is crosslinked by an organic peroxide crosslinking method or a silane crosslinking method, the crosslinkable flame-retardant polyolefin resin composition preferably contains one or more organic peroxides. The organic peroxide generates radicals at least by thermal decomposition and acts as a catalyst to cause a crosslinking reaction between resins or a grafting reaction by radical reaction of a silane coupling agent to a resin. The organic peroxide is not particularly limited, and those used in radical polymerization reaction or conventional silane crosslinking method can be used without any particular limitation.As such organic peroxide, for example, benzoyl peroxide, dicumyl peroxide (DCP), 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane or 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3 are preferable. The content of the organic peroxide in the flame-retardant polyolefin resin composition is not particularly limited and can be appropriately determined depending on the crosslinking method. For example, the content is preferably 0.003 to 0.5 parts by mass, more preferably 0.005 to 0.5 parts by mass, and even more preferably 0.005 to 0.2 parts by mass, relative to 100 parts by mass of the resin.

[0046] (Silanol condensation catalyst) When the crosslinkable flame-retardant polyolefin resin composition is crosslinked by the silane crosslinking method, the crosslinkable flame-retardant polyolefin resin composition preferably contains one or more silanol condensation catalysts. The silanol condensation catalysts have the function of promoting the condensation reaction of the silane coupling agent grafted to the resin in the presence of moisture. This condensation reaction crosslinks the resin via the silane coupling agent and, if appropriate, the inorganic filler. Examples of the silanol condensation catalyst include organic tin compounds, metal soaps, platinum compounds, etc. Organic tin compounds are preferred, such as dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin dioctiate, and dibutyltin diacetate. The content of the silanol condensation catalyst in the crosslinkable flame-retardant polyolefin resin composition is not particularly limited, but is preferably 0.0001 to 0.5 parts by mass, and more preferably 0.001 to 0.2 parts by mass, per 100 parts by mass of the resin.

[0047] (Crosslinking aid) When the crosslinkable flame-retardant polyolefin resin composition is crosslinked by the electron beam crosslinking method, the crosslinkable flame-retardant polyolefin resin composition may contain one or more crosslinking aids. As the crosslinking aid, those usually used in the electron beam crosslinking method can be used without any particular limitation. Usually, polyfunctional compounds are mentioned, for example, (meth)acrylate-based compounds such as polypropylene glycol diacrylate and trimethylolpropane triacrylate, allyl-based compounds such as triallyl cyanurate, maleimide-based compounds, and divinyl-based compounds. The content of the crosslinking auxiliary in the crosslinkable flame-retardant polyolefin resin composition is appropriately set, and can be set, for example, from 1 to 8 mass %.

[0048] (Preparation of flame-retardant non-crosslinked polyolefin resin composition and crosslinkable flame-retardant polyolefin resin composition) Both of the above compositions can be prepared by melt mixing the above ingredients. The kneading method is not particularly limited as long as it is a method that is usually adopted for preparing a rubber or resin composition. For example, various mixing devices such as a single screw extruder, a twin screw extruder, a roll, a Banbury mixer, and various kneaders can be used for mixing. The kneading conditions such as the kneading temperature and the kneading time are not particularly limited, and can be appropriately set within a temperature range equal to or higher than the melting temperature of the resin. The kneading temperature is preferably set to the melt mixing conditions of the step (1) described below. The mixing order of each component is not particularly limited, and the above components can be mixed at once (melt) or mixed sequentially in an appropriate order. In this way, a non-crosslinked or crosslinked (uncrosslinked) flame-retardant polyolefin resin composition in which each component is dispersed (mixed) can be obtained. The crosslinkable flame-retardant polyolefin resin composition to be applied to the silane crosslinking method is preferably prepared by the step (1) described below, regardless of the above preparation method.

[0049] Both of the above compositions can also be molded into an appropriate shape. When preparing the crosslinkable flame-retardant polyolefin resin composition, it is preferable to mold it before (during or after) the crosslinking treatment. The molding method and molding conditions are appropriately selected depending on the shape and form after molding. For example, molding methods include extrusion molding using an extrusion molding machine, extrusion molding using an injection molding machine, and molding using other molding machines. Extrusion molding is preferable when forming a coating layer for a wiring material, in terms of productivity and the ability to be co-extruded with a conductor.

[0050] (Preparation of Flame-Retardant Crosslinked Polyolefin Resin Composition) The flame-retardant crosslinked polyolefin resin composition (crosslinked product) of the present invention can be prepared by subjecting the above-mentioned crosslinkable flame-retardant polyolefin resin composition to the above-mentioned crosslinking reaction treatment. The flame-retardant crosslinked polyolefin resin composition may be crosslinked in an unmolded state, but it is preferable to mold the composition by the above-mentioned molding method and then crosslink the composition to form a crosslinked molded product.

[0051] When the crosslinkable flame-retardant polyolefin resin composition is subjected to a crosslinking reaction treatment by an electron beam crosslinking method, the crosslinkable flame-retardant polyolefin resin composition prepared as described above is preferably molded into an appropriate shape and then irradiated with an electron beam. The irradiation conditions of the electron beam are not particularly limited as long as the crosslinkable flame-retardant polyolefin resin composition (resin) can be crosslinked. For example, the irradiation dose of the electron beam can be 1 to 30 Mrad, and the accelerating voltage during irradiation can be 500 to 750 keV.

[0052] When the crosslinkable flame-retardant polyolefin resin composition is subjected to a crosslinking reaction treatment by an organic peroxide crosslinking method, the crosslinkable flame-retardant polyolefin resin composition prepared as described above is preferably molded into an appropriate shape and then heated to a temperature equal to or higher than the decomposition temperature of the organic peroxide. The heating conditions are sufficient as long as they are equal to or higher than the decomposition temperature of the organic peroxide contained in the crosslinkable flame-retardant polyolefin resin composition, and the heating time is also not particularly limited.

[0053] When the crosslinkable flame-retardant polyolefin resin composition is subjected to a crosslinking reaction treatment by the silane crosslinking method, it is preferable to mold the crosslinkable flame-retardant polyolefin resin composition containing a resin grafted with a silane coupling agent into a suitable shape and then contact the composition with moisture. The method for producing a crosslinked molded article by the silane crosslinking method is preferably a production method including the following steps (1), (2) and (3).

[0054] Step (1): A step of melt-mixing a resin, a halogen-based flame retardant, a flame retardant assistant, a silane coupling agent, an organic peroxide, a silanol condensation catalyst, and preferably an inorganic filler to obtain a molten mixture (a crosslinkable flame-retardant polyolefin resin composition). Step (2): A step of forming the molten mixture obtained in step (1) to obtain a formed body. Step (3): A step of contacting the molded article obtained in step (2) with water to obtain a molded article of the flame-retardant crosslinked polyolefin resin composition.

[0055] When carrying out the above step (1), if the entire resin is melt-mixed in the following step (a), the process comprises steps (a) and (c); and when only a portion of the resin is melt-mixed in the following step (a), the process comprises steps (a), (b), and (c). Step (a): A step of melt-mixing all or a part of a resin, a halogen-based flame retardant, a flame retardant assistant, a silane coupling agent, an organic peroxide, and preferably an inorganic filler at a temperature equal to or higher than the decomposition temperature of the organic peroxide to prepare a silane master batch (Silane MB). Step (b): Melt-mixing the remainder of the resin with a silanol condensation catalyst to prepare a catalyst master batch (catalyst MB). Step (c): Melt-mixing the silane master batch with the silanol condensation catalyst or the catalyst master batch. When the remainder of the resin is melt-mixed as a carrier resin in step (b), preferably 80 to 99 parts by mass, more preferably 94 to 98 parts by mass of the resin is melt-mixed in step (a), and preferably 1 to 20 parts by mass, more preferably 2 to 6 parts by mass of the resin is melt-mixed in step (b).

[0056] The content of each component to be melt-mixed in step (1) is the same as the content in the above-mentioned flame-retardant polyolefin resin composition.

[0057] The melt mixing in step (1) and step (a) can be carried out by appropriately selecting a method that is usually used for rubber, plastics, etc., and examples thereof include a method of mixing using various mixing devices such as a Banbury mixer or various kneaders. The melt mixing temperature is equal to or higher than the decomposition temperature of the organic peroxide, and is preferably a temperature of the decomposition temperature of the organic peroxide + (1 to 80) ° C. Although it is difficult to uniquely determine the melt mixing temperature, for example, 80 to 250 ° C. is preferable, and 100 to 240 ° C. is more preferable. Other conditions can be appropriately set. In step (a), it is preferable to melt mix the above-mentioned components in the absence of a silanol condensation catalyst (for example, a ratio of 0.01 parts by mass or less relative to 100 parts by mass of the resin) to suppress the condensation reaction of the silane coupling agent. In step (1) and step (a), the order of mixing the components when melt-mixing is not particularly limited, and the above-mentioned components can be melt-mixed at once. However, when an inorganic filler is used, it is preferable that the silane coupling agent is mixed with the inorganic filler and further with an appropriate organic peroxide before being melt-mixed with the resin. This premixing (premixing) can be performed, for example, at 20 to 35°C, preferably by dry blending. By premixing, a silane coupling agent that strongly bonds with the inorganic filler and a silane coupling agent that weakly bonds with the inorganic filler can be formed in a well-balanced manner. In the premixing method, the obtained mixture, all or a part of the resin, and the remaining components are then melt-kneaded, for example, under the above-mentioned melt mixing conditions.

[0058] The melt mixing in steps (b) and (c) can be carried out in the same manner as the melt mixing in step (a). However, in step (c), it is preferable that the silane MB and the silanol condensation catalyst are not kept in a high temperature state for a long time in a mixed state in order to avoid a silanol condensation reaction. In step (c), the resins can be mixed (e.g., dry blended) before melt mixing under non-melted conditions, for example, under the above premixing conditions.

[0059] In step (1), steps (a) to (c) can be carried out simultaneously or consecutively. In step (1), a crosslinkable flame-retardant polyolefin resin composition is prepared as a molten mixture.

[0060] Next, the step (2) is carried out in which the obtained molten mixture is molded to obtain a molded body. The molding in the step (2) may be carried out by any molding method and conditions appropriate to the shape of the molded body, as long as the molten mixture can be molded. The molding method is as described above. This step (2) can be carried out, for example, by using an extrusion molding machine, simultaneously with or consecutively to the above step (c). The thus obtained molded article of the crosslinkable flame-retardant polyolefin resin composition is brought into contact with water in step (3), and the silane coupling agent is subjected to a silanol condensation reaction (crosslinking reaction). This step (3) can be carried out by a conventional method, and the crosslinking reaction proceeds simply by leaving the molded article at room temperature, but the molded article can also be brought into contact with water in an intentional manner in order to promote the crosslinking reaction. In this manner, a flame-retardant crosslinked polyolefin resin composition (molded article) containing a resin crosslinked via a silane coupling agent can be prepared.

[0061] Regarding the above-mentioned silane crosslinking method, the components other than the resin, flame retardant, etc. used (silane coupling agent, organic peroxide, silanol condensation catalyst, etc.), the steps (1) to (3) in the above-mentioned production method, and further the reaction in the silane crosslinking method and the form of the obtained condensation cured product can be appropriately applied by, for example, the descriptions in International Publication No. 2016 / 140253 or JP 2017-145370 A, and the contents of these publications are incorporated as they are into this specification as part of their description.

[0062] <Applications of flame-retardant polyolefin resin composition> The flame-retardant polyolefin resin composition of the present invention exhibits the above-mentioned excellent properties, and therefore can be suitably used as a material for forming a covering layer of wiring materials, particularly wiring materials. It can also be applied to general molded products (sealing materials, packings, etc.). In particular, by taking advantage of the above-mentioned excellent properties, it is suitable for applications requiring extremely high abrasion resistance, for example, among wiring materials, it is suitable as a material for forming a covering layer of automotive insulated wires, particularly (very) thin-walled wires described later.

[0063] [Wiring material] A wiring material using a tubular molding formed from the flame-retardant polyolefin resin composition of the present invention as a covering layer will be described below. The wiring material of the present invention has a coating layer (including an insulating layer, a sheath, etc.) formed of the flame-retardant polyolefin resin composition of the present invention on the outer peripheral surface of the conductor. This wiring material is prevented from excessive shrinkage of the coating layer, can suppress exposure of the conductor, and has excellent dimensional accuracy. In addition, it exhibits flame retardancy, low-temperature flexibility, and remarkable abrasion resistance. The wiring material of the present invention may have at least one coating layer made of the flame-retardant polyolefin resin composition of the present invention on the outer peripheral surface of the conductor, and the other configurations may be the same as those of ordinary wiring materials. For example, an insulated electric wire having at least one coating layer on the outer peripheral surface of the conductor, a cable in which a sheath is formed as a coating layer on the outer peripheral surface of such an insulated electric wire or a bundle of electric wires in which a plurality of such insulated electric wires are bundled, and the like can be mentioned. In addition, the coating layer made of the flame-retardant polyolefin resin composition of the present invention may be provided directly on the outer peripheral surface of the conductor, or may be provided indirectly via another layer such as an adhesive layer. The coating layer may be a single layer or multiple layers, and in the case of multiple layers, at least one layer may be formed of the flame-retardant polyolefin resin composition of the present invention. In addition, the sheath of the cable may be formed of the flame-retardant polyolefin resin composition of the present invention.

[0064] Examples of wiring materials include insulated electric wires or cables, (electric) cords, optical fiber cores, optical fiber cords, optical cables, etc. These include wiring materials used for internal wiring or external wiring of electric / electronic devices, wiring materials arranged indoors, and wiring materials arranged outdoors. The wiring material of the present invention can be preferably used as an insulated electric wire or cable for vehicles (on-board vehicles such as automobiles or railway cars), an electric wire or cable for communication, an optical fiber or optical cable for communication, or an electric wire or cable for power. Among these, it is suitable as an insulated electric wire for on-board use, particularly a (very) thin-walled electric wire (e.g., AESSX class).

[0065] As the conductor, a suitable conductor according to the wiring material can be used. For example, a single-wire conductor or a stranded conductor (including a stranded wire in which tensile strength fibers are vertically attached or twisted together) can be used as appropriate. For example, the conductor used in the insulated electric wire or the like may be a bare wire, a tin-plated wire, or an enamel-coated wire. Examples of the metal material forming the conductor include soft copper, copper alloy, and aluminum. The outer diameter of the conductor is appropriately determined depending on the application, and can be set in the same manner as that of a normal wiring material used for each application. For example, it can be 0.5 to 4.0 mm. On the other hand, examples of the conductor used in the optical fiber core wire and the optical fiber cable include conductors made of quartz glass, various plastics, and the like. The thickness (wall thickness) of the coating layer is appropriately determined depending on the application, etc., but can be set to a thickness similar to that of ordinary wiring materials used for each application. For example, for insulated electric wires, etc., it is usually set to about 0.15 to 10 mm (0.4 mm or less for extremely thin-walled electric wires), and for optical fiber cables, etc., it is usually set to about 0.1 to 10 mm.

[0066] <Manufacturing method of wiring material> The wiring material of the present invention can be produced by any suitable method, but is preferably produced by disposing the flame-retardant polyolefin resin composition of the present invention on the outer peripheral surface of a conductor and appropriately carrying out a crosslinking reaction treatment. The method of disposing the flame-retardant polyolefin resin composition of the present invention on the outer peripheral surface of the flame-retardant polyolefin resin composition conductor may be any method capable of covering the conductor with the flame-retardant polyolefin resin composition, and may be any suitable molding method, such as the above-mentioned molding method. The method of disposing the flame-retardant polyolefin resin composition of the present invention on the outer peripheral surface of the conductor (disposing the flame-retardant polyolefin resin composition) may also be carried out as a series of steps (all at once) using an extrusion molding machine, in succession to the method of preparing the flame-retardant polyolefin resin composition of the present invention (preparation of the flame-retardant polyolefin resin composition in the extrusion molding machine). When the flame-retardant polyolefin resin composition of the present invention is a crosslinkable flame-retardant polyolefin resin composition, the crosslinkable flame-retardant polyolefin resin composition disposed on the outer peripheral surface of the conductor is then subjected to a crosslinking reaction treatment. This crosslinking reaction treatment can be applied without any particular restrictions to the method and conditions normally applied to each crosslinking method suitable for the crosslinkable flame-retardant polyolefin resin composition, and specifically, is as described above. When the flame-retardant polyolefin resin composition of the present invention is crosslinked by the silane crosslinking method, the manufacturing method is the same as the above-mentioned manufacturing method, except that the molten mixture obtained in step (1) is molded onto the outer peripheral surface of the conductor, for example, using an extrusion molding machine.

[0067] In this manner, the flame-retardant polyolefin resin composition of the present invention can be used to produce wiring materials having a coating layer that is excellent in dimensional accuracy, flame retardancy, low-temperature flexibility and abrasion resistance. EXAMPLES

[0068] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. In the following Tables 1-1 and 1-2 (collectively referred to as Table 1), the numerical values ​​relating to the blending amounts of each example are based on mass unless otherwise specified.

[0069] Details of each compound used in the examples and comparative examples are given below. <Resin> HDPE: Hi-Zex 5305E (product name, high density polyethylene, density 0.95 g / cm3 (manufactured by SunAllomer Co., Ltd.) h-PP: SunAllomer PM600A (product name, homopolypropylene, manufactured by SunAllomer Co., Ltd.) r-PP: SanAllomer PB222A (product name, random polypropylene, manufactured by SanAllomer Co., Ltd.) EEA: NUC6510 (product name, ethylene-methyl acrylate copolymer, manufactured by NUC) Styrene-based elastomer: Kraton FG1901X (product name, SEBS, manufactured by Kraton) Other polymers: Evolu 1540 (trade name, linear low-density polyethylene (LLDPE), density 0.91 g / cm 3 (Prime Polymer Co., Ltd.) Density 0.90g / cm 3 Polymers below: Kernel KS240T (trade name, very low density polyethylene (VLDPE), density 0.88 g / cm 3 (Japan Polyethylene Corporation) <Halogen-based flame retardants> Brominated flame retardant: Cytex 8010 (product name, ethylene bis(pentabromophenyl), melting point over 200°C, manufactured by Albemarle) Chlorine-based flame retardant: Dechlorane Plus (trade name, 1,6,7,8,9,14,15,16,17,17,18,18-dodecachloropentacyclo[12.2.1.16,9.02,13.05,10]octadeca-7,15-diene, melting point over 200°C, manufactured by HighChem) <Flame retardant synergist> Chlorine-based flame retardant: Antimony trioxide (melting point over 200°C, manufactured by Nihon Seiko Co., Ltd.) <Other ingredients> Inorganic filler: Magseeds FK-621 (product name, magnesium hydroxide, melting point over 200°C, manufactured by Konoshima Chemical Co., Ltd.) Silane coupling agent: KBM-1003 (trade name, trimethoxyvinylsilane, melting point 200°C or less, manufactured by Shin-Etsu Silicones) Organic peroxide: Perhexa 25B (trade name, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, manufactured by NOF Corporation) Silanol condensation catalyst: Adeka STAB OT-1 (trade name, dioctyltin dilaurate, melting point 200°C or less, manufactured by ADEKA Corporation) Crosslinking aid: Ogmont T200 (trade name), trimethylolpropane trimethacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd. Antioxidant: Irganox 1010 (trade name: Pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), melting point below 200°C, manufactured by BASF) Lubricant: X-22-2125H (product name, silicone mixture, melting point 200°C or less, manufactured by Shin-Etsu Silicone Co., Ltd.)

[0070] [Examples 1 to 21 , Reference example 11 and Comparative Examples 1 to 11] Flame-retardant polyolefin resin compositions having the compositions shown in Table 1 were prepared by the following manufacturing method, and these were extrusion-molded (extrusion coating) onto the outer peripheral surface of a conductor to produce an insulated wire (AESSX-0.3SQf, compliant with Japan Automotive Engineering Society (JASO) D 625) having a coating layer formed thereon. Working Example , reference example In the comparative examples, the following other components were used in addition to the inorganic filler depending on the crosslinking method. <Silane crosslinking method> Silane coupling agent 2.8 parts by weight, organic peroxide 0.1 parts by weight, silanol condensation catalyst 0.1 parts by weight, antioxidant 1 part by weight, and lubricant 1 part by weight <Electron beam crosslinking method> 3 parts by weight of a methacrylate-based multifunctional compound as a crosslinking aid, 1 part by weight of an antioxidant, and 1 part by weight of a lubricant <Non-crosslinked (Example 3)> Antioxidant 1 part by weight and lubricant 1 part by weight In Table 1, the components other than the inorganic filler and their mixed amounts are omitted, and the total content is recorded together in the "Other Components" column.

[0071] <Examples 1, 5, 7 to 21 , Reference example 11 and Comparative Examples 1 to 9 and 11> An insulated wire was produced by the following silane crosslinking method. Working Example , reference example and in the comparative example, a portion of the resin was used in step (a) and the remainder of the resin (5 parts by weight of HDPE) was used as a carrier resin for catalyst MB in step (b).

[0072] Specifically, 100 parts by mass of resin were mixed at room temperature (25°C) with the inorganic filler shown in Table 1, 2.8 parts by mass of silane coupling agent, and 0.1 parts by mass of organic peroxide. The mixture obtained, a part of the resin, a halogen-based flame retardant, a flame retardant assistant, 1 part by mass of antioxidant, and 1 part by mass of lubricant were melt-mixed for 5 minutes at a temperature (200°C) higher than the decomposition temperature of the organic peroxide in the contents shown in Table 1 using a 2L Banbury mixer (manufactured by Nippon Roll Co., Ltd.), and then discharged at a material discharge temperature of 130°C and pelletized to obtain Silane MB (step (a)). The remainder of the resin and 0.1 parts by mass of a silanol condensation catalyst were melt-mixed at 150° C. in a Banbury mixer (manufactured by Nippon Roll Co., Ltd.) and discharged at a material discharge temperature of 130° C. to obtain catalyst MB (step (b)). Next, the silane MB obtained in step (a) and the catalyst MB obtained in step (b) were dry-blended immediately above an extrusion molding machine (screw diameter: 25 mm, L / D (ratio of effective screw length L to diameter D): 25) at 25°C for about 1 minute to obtain a dry blend. The obtained dry blend was put into the extrusion molding machine and extrusion-coated (step (2)) at a wire speed of 100 m / min (screw rotation speed of 40 rpm) on the outer periphery of a stranded conductor (outer diameter 0.80 mm) in which 19 soft copper wires with a diameter of 0.16 mm were concentrically twisted, to a finished outer diameter of 1.40 mm (thickness 0.30 mm) under the following extrusion temperature conditions to produce an electric wire precursor. In this case, the dry blend is melt-mixed in the extruder before extrusion (step (c)), to prepare a crosslinkable flame-retardant polyolefin resin composition. The extrusion temperature conditions are as follows: the temperature control in the cylinder part of the extruder is divided into three zones C1, C2, and C3 from the feeder side to the die side; the C1 zone is set to 150°C, the C2 zone to 170°C, and the C3 zone to 190°C; and the die temperature (molding temperature) is set to 200°C. The wire precursor thus obtained was left in an environment of 25°C and 50% RH for 24 hours (step (3)), whereby the tubular molding of the crosslinkable flame-retardant polyolefin resin composition was brought into contact with water to carry out a silanol condensation reaction, thereby producing an insulated wire having a tubular molding of the flame-retardant crosslinked polyolefin resin composition as a coating layer.

[0073] <Examples 2, 4, 6 and Comparative Example 10> An insulated wire was produced by the following electron beam crosslinking method. The components shown in Table 1 in the amounts shown in Table 1, 3 parts by mass of crosslinking auxiliary, 1 part by mass of antioxidant, and 1 part by mass of lubricant were charged into a Banbury mixer and melt-mixed at 120 to 200°C for 10 minutes, and then discharged at a material discharge temperature of 200°C and passed through a feeder rudder to obtain pellets of a crosslinkable flame-retardant polyolefin resin composition. The obtained pellets were used to form an insulating coating as follows to produce an electric wire precursor. That is, the obtained pellets were introduced into an extrusion molding machine equipped with a screw having a diameter of 25 mm (ratio of effective screw length L to diameter D: L / D=25, compression section screw temperature 190° C., head temperature 200° C.). While melting the pellets in this extrusion molding machine, the pellets were extrusion-coated at a wire speed of 100 m / min (screw rotation speed 40 rpm) on the outer periphery of a stranded conductor (outer diameter 0.80 mm) in which 19 soft copper wires having a diameter of 0.16 mm were concentrically twisted, so that the finished outer diameter was 1.40 mm (thickness 0.30 mm), thereby producing an electric wire precursor. Next, the crosslinkable flame-retardant polyolefin resin composition placed on the outer peripheral surface of the conductor was irradiated with an electron beam at an acceleration voltage of 500 kV to a dose of 10 Mrad. In this manner, an insulated wire having a tubular molding of the flame-retardant crosslinked polyolefin resin composition as a covering layer was produced.

[0074] <Example 3> In Example 2, an insulated wire having a tubular molding of a flame-retardant non-crosslinked polyolefin resin composition as a coating layer was produced in the same manner as in Example 2, except that the flame-retardant crosslinked polyolefin resin composition (not containing 3 parts by mass of crosslinking aid) placed on the outer peripheral surface of the conductor was not irradiated with electron beams.

[0075] The following tests were carried out on each of the produced insulated wires, and the results are shown in Table 1. An overall evaluation as an insulated wire was also made.

[0076] <Overall Judgment> The overall judgment was made as follows: if any one of the following abrasion resistance test, low-temperature winding test, flame retardancy test, and shrinkage test was failed, it was marked as "X" (fail); if all tests were passed, it was marked as "O" (passed as an insulated wire that realizes the effects of the present invention).

[0077] <Wear resistance test> In accordance with the Japan Automotive Engineering Society standard (JASO) D 625, a scrape abrasion test was conducted in which a 0.45 mm diameter stainless steel (SUS) wire was moved back and forth on the surface of the insulated wire with a load of 7 N applied. The test was conducted on four test points on the surface of the insulated wire, forming a central angle of 90°, and the number of reciprocating abrasions was recorded at the point when the coating layer peeled off and electrical continuity with the conductor was established. The minimum number of reciprocating abrasions out of the four was regarded as the abrasion number of the insulated wire. The abrasion resistance of the insulated wire was evaluated according to which of the following evaluation criteria the abrasion count fell under. In the above standard, a test is considered to pass if it was abraded 100 times or more, but in this test, a grade of "△" or higher is considered to pass. The insulated wire produced in Comparative Example 10 was abraded about 300 times. - Evaluation Criteria - ◎: 1000 times or more ○: 700 or more times, but less than 1000 times △: 500 times or more, but less than 700 times ×: 500 times or less

[0078] <Low temperature flexibility (winding at low temperature) test> In accordance with JASO D 625, a low-temperature winding test was conducted by winding an insulated wire around a rod with a diameter five times the outer diameter of the insulated wire and keeping it at -40°C for four hours. After 4 hours had passed, the insulated wires were subjected to a voltage withstand test at 1 kV for 1 minute. If no dielectric breakdown occurred (passed the voltage withstand test), the wire was marked as "O" (passed the low-temperature winding test), and if dielectric breakdown occurred, the wire was marked as "X" (failed the low-temperature winding test).

[0079] <Flame retardancy test> Flame retardancy tests were conducted in accordance with JASO D 625, with the following 45-degree inclined burning test and horizontal burning test. As a result, those that passed both the 45-degree inclined burning test and the horizontal burning test were rated as "Good", those that passed only the horizontal burning test were rated as "Good", and those that did not pass either the horizontal burning test were rated as "Poor" (failed this test). (Horizontal burning test) The prepared insulated wire was fixed horizontally and exposed to a flame from a burner with an outer flame length adjusted to 20 mm for 5 seconds. The test piece was then burned, and the time from the start of exposure to the flame until it went out (extinguishing time) was measured. If the flame went out within 30 seconds, the horizontal combustion test was passed. (45 degree inclination combustion test) The prepared insulated electric wire was fixed at a 45° inclination from the vertical direction and exposed to a flame from a burner with an outer flame length adjusted to 20 mm for 15 seconds. The test piece was burned in this manner, and the time from the start of flame exposure to extinction (extinction time) was measured. If the extinction time was within 70 seconds and the burning part was more than 50 mm below the top end of the insulated electric wire, it was deemed to have passed the 45° inclination combustion test.

[0080] <Contractility test> The insulated wire cut to a length of 3,000 mm was left horizontally in an environment of normal temperature and humidity (25°C, 50 RH%) for 24 hours. The length of the conductor protruding from the end of the coating layer at both ends of the insulated wire was measured, and the protruding length at each end and the shrinkage of the insulated wire were evaluated. When each protrusion length was 0.5 mm or less, it was evaluated as "◯" (pass), and when it exceeded 0.5 mm, it was evaluated as "×" (fail).

[0081] [Table 1-1]

[0082] [Table 1-2]

[0083] In Table 1, in the column "Crosslinking method", "Silane" indicates silane crosslinking method, "Electron beam" indicates electron beam crosslinking method, and "None" indicates no crosslinking (non-crosslinking). In the present invention, the inorganic filler is included in the other components, but in order to clearly indicate its content, it is described separately from "other components" other than the inorganic filler in Table 1. The "other components" in Table 1 are selected depending on the crosslinking method, and are specifically as described above. In the "Composition [A]" column of Table 1, "HDPE+PP" indicates the total content of high-density polyethylene and polypropylene, "HDPE+h-PP" indicates the total content of high-density polyethylene and homopolypropylene, "HDPE" indicates the content of high-density polyethylene, and "h-PP" indicates the content of homopolypropylene. In the "Composition [B]" column of Table 1, "EEA+SEBS" indicates the total content of polyethylene copolymer having an acid copolymerization component and styrene-based elastomer, and "Density 0.90 g / cm 3 "Less than" has a density of 0.90g / cm 3 The polymer content is less than 100%.

[0084] As is clear from the results shown in Table 1, the comparative compositions in which the resin does not satisfy the compositions [A] and [B], the comparative compositions containing only one of flame retardancy and a flame retardant auxiliary, and the comparative compositions in which the flame retardant auxiliary is contained but the total content with the flame retardant is not satisfied are all unable to form a coating layer (molded body) that combines flame retardancy, low-temperature flexibility, dimensional stability, and high abrasion resistance. In contrast, the flame-retardant polyolefin resin composition of the present invention, which contains a resin satisfying the compositions [A] and [B] and a flame retardant and flame retardant auxiliary in a specific total content, can form a coating layer that is excellent in flame retardancy, low-temperature flexibility, and dimensional stability and exhibits extremely high abrasion resistance, regardless of whether it is crosslinked or not, and regardless of the crosslinking method.

Claims

1. A flame-retardant polyolefin resin composition comprising a resin, a halogen-based flame retardant, and a flame retardant assistant for the halogen-based flame retardant. The halogen-based flame retardant and the flame retardant auxiliary are contained in a total amount of 15 to 60 parts by mass per 100 parts by mass of the resin, The resin satisfies the following compositions [A] and [B]. [A] A resin composition comprising both high-density polyethylene and polypropylene, the total content of the two in the resin being 50 to 80% by mass, the content of the high-density polyethylene in the resin being 10 to 70% by mass, and the total content of homopolypropylene and block polypropylene in the resin being 0 to 30% by mass. [B] The total content of ethylene-vinyl acetate copolymer, polyethylene copolymer having an acid copolymerization component, acid-modified copolymer thereof, ethylene rubber, and styrene-based elastomer in the resin is 0 to 10 mass % and the density is 0.90 g / cm 3 Polymers less than 100% are not required.

2. 2. The flame-retardant polyolefin resin composition according to claim 1, comprising a total of 120 parts by mass or less of components having a melting point exceeding 200° C. per 100 parts by mass of the resin.

3. 3. The flame-retardant polyolefin resin composition according to claim 1, wherein in the composition [A], the total content of the high-density polyethylene, homopolypropylene and block polypropylene in the resin is 30 mass% or more.

4. The flame-retardant polyolefin resin composition according to any one of claims 1 to 3, wherein the total content of the composition [B] is 5 mass% or less.

5. The flame-retardant polyolefin resin composition according to any one of claims 1 to 4, which is a crosslinked product.

6. A wiring material having a coating layer on an outer peripheral surface of a conductor, A wiring material, wherein the coating layer is formed from the flame-retardant polyolefin resin composition according to any one of claims 1 to 5.

7. The wiring material according to claim 6, which is an insulated wire for use in a vehicle.

Citation Information

Patent Citations

  • Thin-walled nonflammable insulated wire

    JP1994215644A

  • Flame-retardant resin composition

    JP1996311259A

  • Flame-retardant resin composition and molding comprising the same

    JP2010265350A

  • Thermostable crosslinked electric wire

    JP2014132530A

  • Flame-retardant resin composition, and cable and optical fiber cable using the same

    JP2017025203A