ELECTRODE FOR ELECTRICITY STORAGE DEVICE AND ELECTRICITY STORAGE DEVICE

By integrating an oxide-based lithium ion conductive solid electrolyte with an ionic liquid in a garnet-type crystal structure, the electrodes in all-solid-state batteries achieve improved lithium ion conductivity and safety, addressing the limitations of existing technologies.

JP7593928B2Active Publication Date: 2024-12-03NITERRA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021540649
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-22
Filing Date
2020-06-24
Publication Date
2024-12-03
Estimated Expiration
2040-06-24

AI Technical Summary

Technical Problem

Existing all-solid-state batteries face challenges with low lithium ion conductivity due to low adhesion between particles in oxide-based electrolytes and safety concerns with sulfide-based electrolytes, which can generate toxic gas.

Method used

Incorporating an oxide-based lithium ion conductive solid electrolyte with an ionic liquid to form electrodes that enhance lithium ion conductivity without generating toxic gases, using a specific garnet-type crystal structure for improved adhesion and conductivity.

Benefits of technology

The electrodes exhibit high lithium ion conductivity and safety, reducing internal resistance and corrosion, thereby enhancing the performance of power storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593928000001
    Figure 0007593928000001
  • Figure 0007593928000002
    Figure 0007593928000002
  • Figure 0007593928000003
    Figure 0007593928000003
Patent Text Reader

Abstract

The present invention provides an electrode for a power storage device wherein the lithium ion conductivity in the electrode and at the interface between the electrode and another member is improved. The electrode for a power storage device comprises an oxide-based lithium ion-conductive solid electrolyte, an active material, and an ionic liquid.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technology disclosed in this specification relates to an electrode for an electricity storage device. [Background technology]

[0002] In recent years, the demand for high-performance batteries has been increasing with the spread of electronic devices such as personal computers and mobile phones, the spread of electric vehicles, and the expanded use of natural energy such as solar and wind power. In particular, the use of all-solid-state lithium-ion secondary batteries (hereinafter referred to as "all-solid-state batteries"), in which all battery elements are made of solids, is expected to become more widespread. Compared to conventional lithium-ion secondary batteries that use an organic electrolyte solution in which lithium salt is dissolved in an organic solvent, all-solid-state batteries are safer because there is no risk of the organic electrolyte leaking or catching fire, and the exterior can be simplified, which allows the energy density per unit mass or unit volume to be improved.

[0003] As the solid electrolyte constituting the solid electrolyte layer of the all-solid-state battery, for example, an oxide-based lithium ion conductive solid electrolyte or a sulfide-based lithium ion conductive solid electrolyte is used. Since the oxide-based lithium ion conductive solid electrolyte is relatively hard in a powder state, the adhesion between particles is low and the lithium ion conductivity is low in a compact (green compact) formed by pressing the powder or a compact formed into a sheet shape using a binder. By sintering or vapor deposition using the powder of the oxide-based lithium ion conductive solid electrolyte, the lithium ion conductivity can be increased, but warping and deformation caused by heat treatment make it difficult to increase the size of the battery.

[0004] On the other hand, sulfide-based lithium ion conductive solid electrolytes are relatively soft in powder form, and therefore have high adhesion between particles and high lithium ion conductivity when pressed into a compact or formed into a sheet using a binder. However, sulfide-based lithium ion conductive solid electrolytes react with moisture in the air to generate hydrogen sulfide gas, which may be undesirable from a safety standpoint.

[0005] In addition, a technology is known in which a lithium ion conductor is produced by mixing an oxide-based lithium ion conductive solid electrolyte and a sulfide-based lithium ion conductive solid electrolyte, thereby achieving both improved safety and improved lithium ion conductivity (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] US Patent Application Publication No. 2015 / 0171463 Summary of the Invention [Problem to be solved by the invention]

[0007] In an all-solid-state battery, for example, in order to improve the lithium ion conductivity of an electrode (positive electrode and / or negative electrode, the same applies below), it is possible to add a lithium ion conductive solid electrolyte to the electrode in addition to an active material. When an oxide-based lithium ion conductive solid electrolyte is used as the solid electrolyte to be added to the electrode, the adhesion between particles is low in the state of a compact formed by pressure molding or in the state of a compact formed into a sheet shape using a binder, as in the case of the above-mentioned solid electrolyte layer, and the lithium ion conductivity is low. On the other hand, when a sulfide-based lithium ion conductive solid electrolyte is used as the solid electrolyte to be added to the electrode, it may be undesirable in terms of safety. In addition, when a mixture of the oxide-based lithium ion conductive solid electrolyte and the sulfide-based lithium ion conductive solid electrolyte as described above is used as the solid electrolyte to be added to the electrode, the content ratio of the sulfide-based lithium ion conductive solid electrolyte is reduced, but since the sulfide-based lithium ion conductive solid electrolyte is still included, there is room for improvement in terms of safety.

[0008] It should be noted that such a problem is not limited to electrodes for all-solid-state lithium-ion secondary batteries, but is a common problem for electrodes for electricity storage devices.

[0009] This specification discloses a technique that can solve the above-mentioned problems. [Means for solving the problem]

[0010] The technology disclosed in this specification can be realized, for example, in the following forms.

[0011] (1) The electrode for a power storage device disclosed in this specification contains an oxide-based lithium ion conductive solid electrolyte, an active material, and an ionic liquid. The electrode for a power storage device contains an oxide-based lithium ion conductive solid electrolyte that is not likely to generate toxic gas, rather than a sulfide-based lithium ion conductive solid electrolyte that may generate toxic gas, and therefore can avoid the generation of toxic gas. In addition, since the oxide-based lithium ion conductive solid electrolyte is a material that is not easily plastically deformed, unless sintering is performed, the contact between the particles becomes insufficient and high lithium ion conductivity cannot be exhibited. However, since the electrode is nonvolatile and flame-retardant and contains an ionic liquid that functions as a fluid lithium ion conductive component, the presence of the ionic liquid can improve the lithium ion conductivity in the electrode and at the interface between the electrode and other members. Therefore, if a power storage device is constructed using this electrode, the performance of the power storage device can be improved.

[0012] (2) In the above-mentioned electrode for a power storage device, the volume content of the active material may be 40 vol% or more and 85 vol% or less, the volume content of the oxide-based lithium ion conductive solid electrolyte may be 5 vol% or more and 40 vol% or less, and the volume content of the ionic liquid may be 3 vol% or more and 35 vol% or less. By adopting such a configuration, it is possible to effectively improve the lithium ion conductivity in the electrode and at the interface between the electrode and other members. Therefore, by constructing a power storage device using an electrode having such a configuration, it is possible to effectively improve the performance of the power storage device.

[0013] (3) In the above-mentioned power storage device electrode, the oxide-based lithium ion conductive solid electrolyte may have a garnet-type crystal structure containing at least Li, La, Zr, and O. Such an oxide-based lithium ion conductive solid electrolyte has a wider potential window than other oxide-based lithium ion conductive solid electrolytes, and thus by employing this configuration, the range of materials that can be selected for the active material of the electrode can be widened, and an electrode containing an optimal active material can be constructed.

[0014] (4) The electricity storage device disclosed in the present specification may include a solid electrolyte layer, a positive electrode, a negative electrode, and a current collector, and at least one of the positive electrode and the negative electrode may be the above-mentioned electricity storage device electrode. According to this electricity storage device, the performance of the electricity storage device can be improved by improving the lithium ion conductivity in the electrode and at the interface between the electrode and another member.

[0015] The technology disclosed in this specification can be realized in various forms, for example, in the form of an electrode for an electricity storage device, an electricity storage device including an electrode for an electricity storage device, a manufacturing method thereof, etc. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is an explanatory diagram illustrating a schematic cross-sectional configuration of an all-solid-state lithium-ion secondary battery 102 according to an embodiment of the present invention. [Diagram 2] FIG. 1 is an explanatory diagram showing a schematic configuration of a portion of a positive electrode 114. [Diagram 3] FIG. 1 is an explanatory diagram showing a schematic configuration of a portion of a negative electrode 116. [Figure 4] Schematic diagram of the garnet-type crystal structure [Diagram 5] FIG. 1 is an explanatory diagram showing the results of performance evaluation of the positive electrode 114. [Figure 6] FIG. 1 is an explanatory diagram showing the results of performance evaluation of the positive electrode 114. [Figure 7] FIG. 1 is an explanatory diagram showing the results of performance evaluation of the negative electrode 116. [Figure 8]FIG. 1 is an explanatory diagram showing the results of performance evaluation of the negative electrode 116. [Figure 9] FIG. 1 is an explanatory diagram showing a schematic configuration of a pressing tool 300 and a sample S used in evaluating the performance of a positive electrode 114. [Figure 10] FIG. 1 is an explanatory diagram showing a schematic configuration of a pressing tool 300 and a sample S used in evaluating the performance of a negative electrode 116. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] A. Embodiment: A-1. Configuration of the all-solid-state battery 102: (Overall composition) Fig. 1 is an explanatory diagram that shows a schematic cross-sectional configuration of an all-solid-state lithium ion secondary battery (hereinafter referred to as "all-solid-state battery") 102 in this embodiment. Fig. 1 shows mutually orthogonal XYZ axes for specifying directions. In this specification, for convenience, the positive direction of the Z axis is referred to as the upward direction, and the negative direction of the Z axis is referred to as the downward direction.

[0018] The all-solid-state battery 102 includes a battery body 110, a positive electrode side current collector 154 disposed on one side (upper side) of the battery body 110, and a negative electrode side current collector 156 disposed on the other side (lower side) of the battery body 110. The positive electrode side current collector 154 and the negative electrode side current collector 156 are conductive, approximately flat plate-shaped members, and are formed of, for example, stainless steel, Ni (nickel), Ti (titanium), Fe (iron), Cu (copper), Al (aluminum), conductive metal materials selected from alloys thereof, carbon materials, and the like. In the following description, the positive electrode side current collector 154 and the negative electrode side current collector 156 are also collectively referred to as current collectors.

[0019] (Configuration of Battery Body 110) The battery body 110 is a lithium ion secondary battery body in which all battery elements are solid. In this specification, the battery elements being all solid means that the skeleton of all battery elements is solid, and does not exclude, for example, a form in which the skeleton is impregnated with a liquid. The battery body 110 includes a positive electrode 114, a negative electrode 116, and a solid electrolyte layer 112 disposed between the positive electrode 114 and the negative electrode 116. In the following description, the positive electrode 114 and the negative electrode 116 are also collectively referred to as electrodes. The all-solid-state battery 102 or the battery body 110 corresponds to the power storage device in the claims.

[0020] (Configuration of Solid Electrolyte Layer 112) The solid electrolyte layer 112 is a member having a substantially flat plate shape, and contains a lithium ion conductive solid electrolyte (for example, an LLZ-based lithium ion conductive solid electrolyte described later). The solid electrolyte layer 112 may further contain an ionic liquid having lithium ion conductivity. The solid electrolyte layer 112 may be a compact (compressed powder compact) obtained by compressing and molding a powder of the lithium ion conductive solid electrolyte, or may be a compact obtained by adding a binder to the powder of the lithium ion conductive solid electrolyte and molding it into a sheet shape.

[0021] (Configuration of Positive Electrode 114) The positive electrode 114 is a member having a substantially flat plate shape. FIG. 2 is an explanatory diagram that shows a schematic configuration of a portion of the positive electrode 114 (portion X1 in FIG. 1). As shown in FIG. 2, the positive electrode 114 includes a positive electrode active material 214. The positive electrode active material 214 is added, for example, to increase the amount of lithium ions that can be inserted and removed from the positive electrode 114 and improve the energy density. Examples of the positive electrode active material 214 include S (sulfur), TiS2, LiCoO2 (hereinafter referred to as "LCO"), LiMn2O4, LiFePO4, Li(Co 1 / 3 Ni 1 / 3 Mn 1 / 3 )O2 (hereinafter referred to as "NCM"), LiNi 0.8 Co 0.15 Al 0.05O2 (hereinafter referred to as "NCA"), etc. may be used. The positive electrode 114 may further contain a conductive assistant (for example, conductive carbon, Ni (nickel), Pt (platinum), Ag (silver)).

[0022] The positive electrode 114 also contains an ionic liquid 224 having lithium ion conductivity. The ionic liquid 224 is added, for example, to reduce the internal resistance of the positive electrode 114. The ionic liquid 224 having lithium ion conductivity is, for example, an ionic liquid in which a lithium salt is dissolved. The ionic liquid is composed of only cations and anions, is liquid at room temperature, and is a non-volatile, flame-retardant substance. Specific materials and the like of the ionic liquid 224 contained in the positive electrode 114 will be described later.

[0023] The positive electrode 114 also contains an oxide-based lithium ion conductive solid electrolyte 204. The oxide-based lithium ion conductive solid electrolyte 204 is added, for example, to suppress a decrease in the lithium ion conductivity of the positive electrode 114 and to suppress corrosion of the positive electrode side current collector 154 provided adjacent to the positive electrode 114 by reducing the area where the ionic liquid 224 comes into contact with the positive electrode side current collector 154. Specific materials and the like of the oxide-based lithium ion conductive solid electrolyte 204 contained in the positive electrode 114 will be described later.

[0024] (Configuration of negative electrode 116) The negative electrode 116 is a member having a substantially flat plate shape. FIG. 3 is an explanatory diagram that shows a schematic configuration of a portion (part X2 in FIG. 1) of the negative electrode 116. As shown in FIG. 3, the negative electrode 116 includes a negative electrode active material 216. The negative electrode active material 216 is added, for example, to increase the amount of lithium ions that can be inserted and extracted in the negative electrode 116 and improve the energy density. Examples of the negative electrode active material 216 include Li metal, Li-Al alloy, Li4Ti5O 12 (hereinafter referred to as "LTO"), carbon (graphite, natural graphite, artificial graphite, core-shell graphite with a surface coated with low crystalline carbon), Si (silicon), SiO, etc. may be used. The negative electrode 116 may further contain a conductive assistant (e.g., conductive carbon, Ni, Pt, Ag).

[0025] The negative electrode 116 also contains an ionic liquid 226 having lithium ion conductivity. The ionic liquid 226 is added, for example, to reduce the internal resistance of the negative electrode 116. The ionic liquid 226 having lithium ion conductivity is, for example, an ionic liquid in which a lithium salt is dissolved. Specific materials and the like of the ionic liquid 226 contained in the negative electrode 116 will be described later.

[0026] The negative electrode 116 also contains an oxide-based lithium ion conductive solid electrolyte 206. The oxide-based lithium ion conductive solid electrolyte 206 is added, for example, to suppress a decrease in the lithium ion conductivity of the negative electrode 116 and to suppress corrosion of the negative electrode side current collector 156 provided adjacent to the negative electrode 116 by reducing the area where the ionic liquid 226 comes into contact with the negative electrode side current collector 156. Specific materials and the like of the oxide-based lithium ion conductive solid electrolyte 204 contained in the negative electrode 116 will be described later.

[0027] A-2. Detailed configuration of the positive electrode 114 and the negative electrode 116: Next, the configuration of the electrodes (positive electrode 114 and negative electrode 116) constituting the battery body 110 will be described in more detail. As described above, the positive electrode 114 contains an oxide-based lithium ion conductive solid electrolyte 204 in addition to the positive electrode active material 214, and the negative electrode 116 contains an oxide-based lithium ion conductive solid electrolyte 206 in addition to the negative electrode active material 216. As the oxide-based lithium ion conductive solid electrolytes 204, 206, for example, a solid electrolyte having a garnet-type crystal structure containing at least Li (lithium), La (lanthanum), Zr (zirconium), and O (oxygen) is used. More specifically, for example, Li7La3Zr2O 12(hereinafter referred to as "LLZ"), or LLZ with at least one element substitution of Mg (magnesium) with A (A is at least one element selected from the group consisting of Ca (calcium), Sr (strontium) and Ba (barium)) (for example, LLZ with element substitution of Mg and Sr (hereinafter referred to as "LLZ-MgSr")) is used. Hereinafter, these lithium ion conductive solid electrolytes are referred to as "LLZ-based lithium ion conductive solid electrolytes (or LLZ-based lithium ion conductive powder)".

[0028] The "garnet-type crystal structure" is defined as a structure having the general formula C3A2B3O 12 FIG. 4 is an explanatory diagram showing a garnet-type crystal structure. As shown in FIG. 4, in the garnet-type crystal structure, the C site Sc is dodecahedrally coordinated with the oxygen atom Oa, the A site Sa is octahedrally coordinated with the oxygen atom Oa, and the B site Sb is tetrahedrally coordinated with the oxygen atom Oa. In a lithium ion conductive powder (lithium ion conductive solid electrolyte) having a garnet-type crystal structure, lithium may exist in a void V, which is a position where the oxygen atom Oa is octahedrally coordinated in a normal garnet-type crystal structure. The void V is, for example, a position sandwiched between the B site Sb1 and the B site Sb2 in FIG. 4. The lithium existing in the void V is octahedrally coordinated with the oxygen atom Oa constituting an octahedron including the face Fb1 of the tetrahedron forming the B site Sb1 and the face Fb2 of the tetrahedron forming the B site Sb2. For example, Li7La3Zr2O 12 In a lithium ion conductive powder (lithium ion conductive solid electrolyte) having a garnet-type crystal structure with the above composition, lanthanum can occupy the C site Sc, zirconium can occupy the A site Sa, and lithium can occupy the B site Sb and the voids V.

[0029] In addition, it can be confirmed by analyzing the lithium ion conductive solid electrolyte (lithium ion conductive powder) with an X-ray diffractometer (XRD) that the lithium ion conductive solid electrolyte has a garnet-type crystal structure containing at least Li, La, Zr, and O. Specifically, an X-ray diffraction pattern is obtained by analyzing the lithium ion conductive solid electrolyte with an X-ray diffractometer. The obtained X-ray diffraction pattern and the ICDD (International Center for Diffraction Data) card (01-080-4947) corresponding to the LLZ (Li7La3Zr2O 12 ) and if the diffraction angles and diffraction intensity ratios of the diffraction peaks in both are roughly the same, it can be determined that the lithium ion conductive solid electrolyte has a garnet-type crystal structure containing at least Li, La, Zr, and O. For example, each lithium ion conductive powder described in "A-7. Preferred embodiments of LLZ-based lithium ion conductive powder" below has diffraction angles and diffraction intensity ratios of the diffraction peaks in both the X-ray diffraction pattern obtained from the lithium ion conductive powder and the ICDD card corresponding to LLZ that are roughly the same, and therefore is determined to have a garnet-type crystal structure containing at least Li, La, Zr, and O.

[0030] Furthermore, as the oxide-based lithium ion conductive solid electrolytes 204, 206, a solid electrolyte other than the LLZ-based lithium ion conductive solid electrolyte (for example, the following ones) may be used. (1) A solid electrolyte having a NASICON-type crystal structure containing at least Li, M (M is at least one of Ti, Zr, and Ge (germanium)), P (phosphorus), and O (e.g., (Li,Ti,Al)(PO4)3, LiZr2(PO4)3, (Li,Ge,Al)(PO4)3). (2) A solid electrolyte having a perovskite-type crystal structure containing at least Li, Ti, La, and O (e.g., (La,Li)TiO3) (3) A solid electrolyte having an antiperovskite crystal structure containing at least Li, Cl, and O (e.g., Li2(OH)Cl) (4) Complex hydrides

[0031] The average particle size of the oxide-based lithium ion conductive solid electrolytes 204, 206 contained in the electrodes (positive electrode 114 and negative electrode 116) is preferably 0.1 μm or more and 10 μm or less.

[0032] As described above, the positive electrode 114 contains an ionic liquid 224 in which a lithium salt is dissolved, and the negative electrode 116 contains an ionic liquid 226 in which a lithium salt is dissolved. Examples of the lithium salt include lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium trifluoromethanesulfonate (CF3SO3Li), lithium bis(trifluoromethanesulfonyl)imide (LiN(SO2CF3)2) (hereinafter referred to as "Li-TFSI"), lithium bis(fluorosulfonyl)imide (LiN(SO2F)2) (hereinafter referred to as "Li-FSI"), and lithium bis(pentafluoroethanesulfonyl)imide (LiN(SO2C2F5)2).

[0033] The ionic liquid may contain, as a cation, Ammonium compounds such as butyltrimethylammonium and trimethylpropylammonium, Imidazolium compounds such as 1-ethyl-3-methylimidazolium and 1-butyl-3-methylimidazolium; piperidinium compounds such as 1-butyl-1-methylpiperidinium and 1-methyl-1-propylpiperidinium; Pyridinium compounds such as 1-butyl-4-methylpyridinium and 1-ethylpyridinium; Pyrrolidinium compounds such as 1-butyl-1-methylpyrrolidinium and 1-methyl-1-propylpyrrolidinium; Sulfonium compounds such as trimethylsulfonium and triethylsulfonium, Phosphonium series, Morpholinium, etc. are used.

[0034] The ionic liquid may contain, as an anion, Cl - , Br - Halide-based compounds such as BF4 - Boron compounds such as (NC)2N - , (CF3SO2)2N - , (FSO2)2N - Amine-based compounds such as CH3SO4 - , CF3SO3 - Sulfates, sulfonates, etc. PF6 - Phosphate-based compounds such as etc. are used.

[0035] More specifically, examples of the ionic liquid that can be used include butyltrimethylammonium bis(trifluoromethanesulfonyl)imide, trimethylpropylammonium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide (hereinafter referred to as "EMI-FSI"), 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-methyl-1-propylpyrrolidinium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-methyl-1-propylpyrrolidinium bis(fluorosulfonyl)imide (hereinafter referred to as "P13-FSI"), and 1-methyl-1-propylpiperidinium bis(fluorosulfonyl)imide (hereinafter referred to as "PP13-FSI").

[0036] The electrodes (positive electrode 114 and negative electrode 116) of this embodiment are not sintered bodies formed by high-temperature firing. Therefore, the electrodes of this embodiment contain hydrocarbons. More specifically, the ionic liquid constituting the electrodes of this embodiment contains hydrocarbons. The inclusion of hydrocarbons in the electrodes (ionic liquid) can be identified by one or a combination of methods such as NMR (nuclear magnetic resonance), Raman spectroscopy, LC-MS (liquid chromatography mass spectrometry), GC-MS (gas chromatography mass spectrometry), and FT-IR (Fourier transform infrared spectroscopy).

[0037] Thus, the electrodes (positive electrode 114 and negative electrode 116) of this embodiment contain ionic liquids 224, 226 having lithium ion conductivity in addition to the oxide-based lithium ion conductive solid electrolytes 204, 206 and active materials (positive electrode active material 214, negative electrode active material 216), and have high lithium ion conductivity in the state of a compact (compressed powder) that has been pressure-molded. Therefore, the use of the electrodes of this embodiment can improve the performance of the battery body 110. The reason why the electrodes of this embodiment have such high lithium ion conductivity is not necessarily clear, but is presumed to be as follows.

[0038] In general, since an oxide-based lithium ion conductive solid electrolyte is harder than a non-oxide-based lithium ion conductive solid electrolyte (for example, a sulfide-based lithium ion conductive solid electrolyte), in the state of a compact (compressed powder) obtained by pressurizing a powder of an oxide-based lithium ion conductive solid electrolyte, the contact between particles becomes a point contact, the resistance between the particles becomes high, and the lithium ion conductivity becomes relatively low. In addition, although the lithium ion conductivity can be increased by firing the powder of the oxide-based lithium ion conductive solid electrolyte at a high temperature, it is difficult to increase the size of the battery because warping and deformation occur due to high-temperature firing, and there is a risk that a high-resistance layer is generated by reaction with the electrode active material, etc., due to high-temperature firing, and the lithium ion conductivity is reduced. However, the electrodes (positive electrode 114 and negative electrode 116) of this embodiment contain ionic liquids 224, 226 having lithium ion conductivity in addition to the oxide-based lithium ion conductive solid electrolytes 204, 206. 2 and 3, the ionic liquids 224, 226 are distributed around the particles of the oxide-based lithium ion conductive solid electrolytes 204, 206. Therefore, in the state of the pressure-molded compact, the ionic liquids 224, 226 functioning as lithium ion conductive paths are present in the grain boundaries of the oxide-based lithium ion conductive solid electrolytes 204, 206 throughout the compact, improving the lithium ion conductivity at the grain boundaries, which is thought to result in improved lithium ion conductivity within the electrode and at the interface between the electrode and other members (for example, the solid electrolyte layer 112).

[0039] In addition, the electrodes (positive electrode 114 and negative electrode 116) of this embodiment may be configured to further include a binder in addition to the oxide-based lithium ion conductive solid electrolyte 204, 206, the active material (positive electrode active material 214, negative electrode active material 216), and the ionic liquid 224, 226, and be formed into a sheet shape. Examples of the binder include polyvinylidene fluoride (PVDF), a copolymer of polyvinylidene fluoride (PVDF) and hexafluoropropylene (HFP) (hereinafter referred to as "PVDF-HFP"), polytetrafluoroethylene (PTFE), polyimide, polyamide, silicone (polysiloxane), styrene-butadiene rubber (SBR), acrylic resin (PMMA), polyethylene oxide (PEO), and the like. With such a configuration, the lithium ion conductivity of the electrodes can be improved while the formability and handling of the electrodes can be improved.

[0040] In addition, in the electrodes (positive electrode 114 and negative electrode 116) of this embodiment, the volume content of the active material (positive electrode active material 214, negative electrode active material 216) is preferably 40 vol% or more and 85 vol% or less. If the volume content of the active material in the electrodes is too low, the battery capacity is not sufficiently ensured, while if the volume content of the active material in the electrodes is too high, the internal resistance of the electrodes cannot be effectively reduced. It is more preferable that the volume content of the active material in the electrodes is 40 vol% or more and 70 vol% or less.

[0041] In addition, the volume content of the oxide-based lithium ion conductive solid electrolytes 204, 206 in the electrodes (positive electrode 114 and negative electrode 116) is preferably 5 vol% or more and 40 vol% or less. If the volume content of the oxide-based lithium ion conductive solid electrolytes 204, 206 in the electrodes is too low, the decrease in the lithium ion conductivity of the electrodes cannot be suppressed and the corrosion of the current collector cannot be effectively suppressed. On the other hand, if the volume content of the oxide-based lithium ion conductive solid electrolytes 204, 206 in the electrodes is too high, the internal resistance of the electrodes cannot be effectively reduced. The volume content of the oxide-based lithium ion conductive solid electrolytes 204, 206 in the electrodes is more preferably 10 vol% or more and 40 vol% or less, and even more preferably 20 vol% or more and 40 vol% or less.

[0042] In addition, the volume content of the ionic liquids 224, 226 in the electrodes (positive electrode 114 and negative electrode 116) is preferably 3 vol% or more and 35 vol% or less. If the volume content of the ionic liquids 224, 226 in the electrodes is too low, the internal resistance of the electrodes cannot be effectively reduced, while if the volume content of the ionic liquids 224, 226 in the electrodes is too high, there is a risk of the ionic liquid seeping out. It is more preferable that the volume content of the ionic liquids 224, 226 in the electrodes is 10 vol% or more and 25 vol% or less.

[0043] In the electrodes (positive electrode 114 and negative electrode 116), if the volume content of the active material (positive electrode active material 214, negative electrode active material 216) is 40 vol% or more and 85 vol% or less, the volume content of the oxide-based lithium ion conductive solid electrolytes 204, 206 is 5 vol% or more and 40 vol% or less, and the volume content of the ionic liquids 224, 226 is 3 vol% or more and 35 vol% or less, it is possible to effectively improve the lithium ion conductivity within the electrodes and at the interface between the electrodes and other members (e.g., solid electrolyte layer 112) while suppressing the occurrence of corrosion of the current collector and the occurrence of seepage of the ionic liquid, and it is possible to effectively improve the performance of the battery body 110 using the electrodes.

[0044] A-3. Manufacturing method of the all-solid-state battery 102: Next, an example of a method for manufacturing the all-solid-state battery 102 of this embodiment will be described. First, the solid electrolyte layer 112 is produced. For example, the powder of an oxide-based lithium ion conductive solid electrolyte is mixed with an ionic liquid, and the mixture is pressurized and molded at a predetermined pressure, or a binder is added to form the mixture into a sheet, thereby producing the solid electrolyte layer 112.

[0045] In addition, the positive electrode 114 and the negative electrode 116 are separately prepared. Specifically, a powder of the oxide-based lithium ion conductive solid electrolyte 204 is mixed with an ionic liquid 224, and a powder of the positive electrode active material 214 (when a conductive assistant is used, a mixture of the powder of the positive electrode active material 214 and the conductive assistant) is added to this mixture and further mixed. The positive electrode 114 is prepared by pressing and molding this mixture at a predetermined pressure or adding a binder and forming it into a sheet. Similarly, a powder of the oxide-based lithium ion conductive solid electrolyte 206 is mixed with an ionic liquid 226, and a powder of the negative electrode active material 216 (when a conductive assistant is used, a mixture of the powder of the negative electrode active material 216 and the conductive assistant) is added to this mixture and further mixed. The negative electrode 116 is prepared by pressing and molding this mixture at a predetermined pressure or adding a binder and forming it into a sheet.

[0046] Next, the positive electrode side current collector 154, the positive electrode 114, the solid electrolyte layer 112, the negative electrode 116, and the negative electrode side current collector 156 are laminated in this order and integrated by applying pressure. Through the above steps, the all-solid-state battery 102 having the above-mentioned configuration is manufactured.

[0047] A-4. Advantages of this embodiment: As described above, the electrodes (positive electrode 114 and negative electrode 116) for the battery body 110 of this embodiment contain the oxide-based lithium ion conductive solid electrolytes 204, 206, the active materials (positive electrode active material 214, negative electrode active material 216), and the ionic liquids 224, 226. In this manner, the electrodes (positive electrode 114 and negative electrode 116) of this embodiment contain the oxide-based lithium ion conductive solid electrolytes 204, 206 that are not likely to generate toxic gas, rather than a sulfide-based lithium ion conductive solid electrolyte that is likely to generate toxic gas, and therefore can avoid the generation of toxic gas. In addition, since the oxide-based lithium ion conductive solid electrolytes 204, 206 are materials that are difficult to plastically deform, unless sintering is performed, the contact between the particles becomes insufficient and high lithium ion conductivity cannot be exhibited, but since the electrodes (positive electrode 114 and negative electrode 116) of this embodiment contain ionic liquids 224, 226 that are nonvolatile and flame-retardant and function as a fluid lithium ion conductive component, the presence of the ionic liquids 224, 226 can improve the lithium ion conductivity in the electrodes and at the interface between the electrodes and other members (for example, the solid electrolyte layer 112). Therefore, if the battery body 110 is constructed using the electrodes of this embodiment, the performance of the battery body 110 can be improved.

[0048] In addition, since the electrodes (positive electrode 114 and negative electrode 116) of this embodiment contain the oxide-based lithium ion conductive solid electrolytes 204, 206, the area where the ionic liquids 224, 226 come into contact with the current collectors (positive electrode side current collector 154 and negative electrode side current collector 156) provided adjacent to the electrodes can be reduced compared to a configuration that does not contain the oxide-based lithium ion conductive solid electrolytes 204, 206, and corrosion of the current collectors can be suppressed. As described above, when the concentration of lithium salt contained in the ionic liquids 224, 226 is high (specifically, when it is 0.4 mol / L or more), corrosion of the current collectors is likely to occur, so the effect of suppressing corrosion of the current collectors by containing the oxide-based lithium ion conductive solid electrolytes 204, 206 becomes more useful.

[0049] In addition, in the electrodes (positive electrode 114 and negative electrode 116) of this embodiment, the volume content of the active material (positive electrode active material 214, negative electrode active material 216) is preferably 40 vol% or more and 85 vol% or less, the volume content of the oxide-based lithium ion conductive solid electrolytes 204, 206 is preferably 5 vol% or more and 40 vol% or less, and the volume content of the ionic liquids 224, 226 is preferably 3 vol% or more and 35 vol% or less. With such a configuration, it is possible to effectively improve the lithium ion conductivity in the electrodes and at the interface between the electrodes and other members (for example, the solid electrolyte layer 112). Therefore, if the battery body 110 is constructed using the electrodes having such a configuration, it is possible to effectively improve the performance of the battery body 110.

[0050] In addition, the oxide-based lithium ion conductive solid electrolytes 204, 206 included in the electrodes (positive electrode 114 and negative electrode 116) of this embodiment are preferably solid electrolytes (LLZ-based lithium ion conductive solid electrolytes) having a garnet-type crystal structure containing at least Li, La, Zr, and O. The LLZ-based lithium ion conductive solid electrolyte has a wider potential window than other oxide-based lithium ion conductive solid electrolytes, so that the material selection range of the active material of the electrode (positive electrode active material 214, negative electrode active material 216) can be widened, and an electrode containing an optimal active material can be configured. For example, the positive electrode material can be LCO, LiMn2O4, LiFePO4, NCM, NCA, etc., and the negative electrode material can be Li metal, Li-Al alloy, LTO, carbon (graphite, natural graphite, artificial graphite, core-shell graphite with a surface coated with low crystalline carbon), Si (silicon), SiO, etc.

[0051] A-5. How to determine the composition of the electrode (volume content of each component): The composition of the electrodes (positive electrode 114, negative electrode 116) constituting the battery body 110, i.e., the volume content (vol%) of each of the active materials (positive electrode active material 214, negative electrode active material 216), the oxide-based lithium ion conductive solid electrolytes 204, 206, and the ionic liquids 224, 226, is determined as follows.

[0052] The target electrode mixture is dissolved in a solvent (e.g., chloroform) and separated into soluble matter (binder, ionic liquid) and precipitate (active material, oxide-based lithium ion conductive solid electrolyte, conductive additive). For the soluble matter, a qualitative analysis of the material components (ionic liquid, binder) is performed using LC-MS measurement (liquid chromatography mass spectrometry) to identify the binder components and ionic liquid components. In addition, a calibration curve is created for each material component, and the content of each component in the total soluble matter is calculated from the results of each material component.

[0053] For the precipitate, the weight of the entire precipitate is measured. In addition, the precipitate is subjected to XRD measurement (X-ray analysis) to analyze the chemical composition and identify the material components of the active material and the oxide-based lithium ion conductive solid electrolyte. In addition, the precipitate is subjected to XRF measurement (X-ray fluorescence analysis) to measure the ratio of the material components. This identifies the ratio of the active material, oxide-based lithium ion conductive solid electrolyte, and conductive assistant. The content of the active material and oxide-based lithium ion conductive solid electrolyte is calculated from the weight of the entire precipitate and the ratio of the active material, oxide-based lithium ion conductive solid electrolyte, and conductive assistant.

[0054] The volume content of each component (binder, ionic liquid, active material, oxide-based lithium ion conductive solid electrolyte) is determined from the content of each component calculated above.

[0055] The ratio of the active material and the oxide-based lithium ion conductive solid electrolyte can also be determined by the following method: the target electrode is frozen with liquid nitrogen or the like to fix each material, a cross section is obtained by the CP method (cross section polisher method), and element mapping is performed on this cross section by EDS (energy dispersive X-ray analysis), making it possible to determine the volume ratio of the active material and the oxide-based lithium ion conductive solid electrolyte.

[0056] A-6.Performance evaluation: Performance evaluation was carried out on the electrodes (positive electrode 114, negative electrode 116) for the battery body 110. Figures 5 and 6 are explanatory diagrams showing the results of the performance evaluation on the positive electrode 114, and Figures 7 and 8 are explanatory diagrams showing the results of the performance evaluation on the negative electrode 116. Also, Figure 9 is an explanatory diagram that typically shows the configurations of a pressing jig 300 and sample S used in the performance evaluation on the positive electrode 114, and Figure 10 is an explanatory diagram that typically shows the configurations of a pressing jig 300 and sample S used in the performance evaluation on the negative electrode 116.

[0057] 5 and 6, 12 samples (S1 to S12) were used for the performance evaluation of the positive electrode 114. Also, as shown in Figures 7 and 8, 13 samples (S21 to S33) were used for the performance evaluation of the negative electrode 116. The samples for the positive electrode 114 and the negative electrode 116 differ from each other in composition (material and volume content of each component).

[0058] As shown in Fig. 5 and Fig. 6, regarding the positive electrode 114, samples S1 to S10 are sheet-shaped molded bodies containing a positive electrode active material 214, an oxide-based lithium ion conductive solid electrolyte 204, an ionic liquid 224, a conductive assistant, and a binder. Sample S11 is a compact containing the positive electrode active material 214, an oxide-based lithium ion conductive solid electrolyte 204, an ionic liquid 224, and a conductive assistant, but does not contain a binder. On the other hand, sample S12 is a sheet-shaped molded body containing the positive electrode active material 214, an oxide-based lithium ion conductive solid electrolyte 204, a conductive assistant, and a binder, but does not contain the ionic liquid 224, unlike the other samples.

[0059] In addition, in the samples S1 to S9 and S12, the positive electrode active material 214 was the above-mentioned NCA (LiNi 0.8 Co 0.15 Al 0.05 O2) was used in sample S10, the above-mentioned LCO(LiCoO2) was used in sample S11, and the above-mentioned NCM(Li(Co 1 / 3 Ni 1 / 3 Mn 1 / 3)O2) was used. As the oxide-based lithium ion conductive solid electrolyte 204, the above-mentioned LLZ-Mg,Sr was used in all samples. As the ionic liquid 224, the samples S1 to S9 used ionic liquid EMI-FSI (hereinafter referred to as "Li-FSI (EMI-FSI)") in which the above-mentioned lithium salt Li-FSI was dissolved (lithium salt concentration: 1.0M (=mol / L)), and the samples S10 and S11 used ionic liquid EMI-FSI (hereinafter referred to as "Li-TFSI (EMI-FSI)") in which the above-mentioned lithium salt Li-TFSI was dissolved (lithium salt concentration: 0.8M). As the conductive assistant, the samples S1 to S6, S11, and S12 used acetylene black (AB), and the samples S7 to S10 used vapor grown carbon fiber (VGCF). As the binder, the above-mentioned PVDF-HFP was used in all of the samples (S1 to S10, S12) that contained a binder.

[0060] As shown in FIG. 7 and FIG. 8, regarding the negative electrode 116, the samples S21 to S30, and S32 are sheet-shaped molded bodies containing the negative electrode active material 216, the oxide-based lithium ion conductive solid electrolyte 206, the ionic liquid 226, and a binder. The samples S29, S30, and S32 further contain a conductive additive (VGCF). The sample S31 is a compact containing the negative electrode active material 216, the oxide-based lithium ion conductive solid electrolyte 206, and the ionic liquid 226, but does not contain a binder. On the other hand, the sample S33 is a sheet-shaped molded body containing the negative electrode active material 216, the oxide-based lithium ion conductive solid electrolyte 206, and a binder, but does not contain the ionic liquid 226, unlike the other samples.

[0061] As the negative electrode active material 216, artificial graphite (MCMB) was used in samples S21 to S27 and S31 to S33, and natural graphite was used in samples S28 to S30. As the oxide-based lithium ion conductive solid electrolyte 206, the above-mentioned LLZ-Mg,Sr was used in all samples. As the ionic liquid 226, 1.0M Li-FSI (EMI-FSI) was used in all samples (S21 to S32) containing the ionic liquid 226. As the binder, the above-mentioned PVDF-HFP was used in all samples (S21 to S30, S32, S33) containing the binder.

[0062] Each sample was prepared according to the following procedure, and the discharge capacity of each sample was measured. First, LLZ-MgSr powder as an oxide-based lithium ion conductive solid electrolyte was prepared as follows. 6.95 Mg 0.15 La 2.75 Sr 0.25 Zr 2.0 O 12 Li2CO3, MgO, La(OH)3, SrCO3, and ZrO2 were weighed out to obtain a mixture of LLZ-MgSr. At this time, taking into consideration the volatilization of Li during firing, Li2CO3 was further added so that the amount was about 15 mol% in excess in terms of elemental conversion. This raw material was placed in a nylon pot together with zirconia balls, and ground and mixed in an organic solvent for 15 hours using a ball mill. After grinding and mixing, the slurry was dried and pre-fired on an MgO plate at 1100°C for 10 hours. A binder was added to the pre-fired powder, and ground and mixed in an organic solvent for 15 hours using a ball mill. After grinding and mixing, the slurry was dried, placed in a mold with a diameter of 12 mm, and pressed to a thickness of about 1.5 mm, and then pressed into a mold with a thickness of 1.5 t / cm using a cold isostatic press (CIP). 2A hydrostatic pressure of 1000 MPa was applied to the compact to obtain a molded body. This molded body was covered with calcined powder of the same composition as the molded body and sintered at 1100°C for 4 hours in a reducing atmosphere to obtain a sintered body. This sintered body was pulverized in a glove box in an argon atmosphere to obtain LLZ-MgSr powder. The particle size of the obtained LLZ-MgSr was about 0.3 to 0.8 μm.

[0063] The thus obtained oxide-based lithium ion conductive solid electrolyte (LLZ-MgSr) powder was mixed with an ionic liquid determined for each sample in a mortar to obtain a composite material of the solid electrolyte and the ionic liquid. For the positive electrode 114, the positive electrode active material 214 and the conductive assistant determined for each sample were added and mixed in a mortar, and this mixture was added to the above-mentioned composite material of the solid electrolyte and the ionic liquid (solid electrolyte for sample S12) and mixed to obtain an electrode composite powder. For the negative electrode 116, the negative electrode active material 216 determined for each sample was added to the above-mentioned composite material of the solid electrolyte and the ionic liquid (solid electrolyte for sample S33) and mixed to obtain an electrode composite powder.

[0064] For the sample containing a binder, the electrode composite powder was mixed in an agate mortar with a 10 wt% PVDF-DMC (dimethyl carbonate) solution added dropwise, and the DMC solvent was added dropwise to adjust the viscosity to obtain an electrode composite slurry. The electrode composite slurry was applied with an applicator onto a metal foil that was evenly attached to glass using DMC and a roller, and the electrode composite sheet was obtained by drying under reduced pressure at 80°C for 10 hours.

[0065] Next, as shown in FIG. 9 and FIG. 10, a Macol tube was set on the short axis of the pressure jig 300, and 150 mg of a composite material (material of the solid electrolyte layer) of a separately prepared oxide-based lithium ion conductive solid electrolyte (LLZ-MgSr) and an ionic liquid (1.0M Li-FSI (EMI-FSI)) was weighed and put in. Then, the long axis was set in the Macol tube and pressurized at 100 MPa. After pressurization, the short axis was removed, and the material of the electrode (positive electrode 114 or negative electrode 116), that is, an electrode composite sheet (or an electrode composite powder) punched to a diameter of 10 mm, was put in, and the short axis was set in the Macol tube and pressurized at 500 MPa. Then, the pressure jig was inverted to remove the long axis, and the material of the counter electrode, that is, an In-Li foil punched to a diameter of 10 mm, was put in, and further a Cu foil punched to a diameter of 10 mm was put in, and then the long axis was set in the Macol tube and pressurized at 80 MPa. After that, a fixing jig (collar) was attached and the bolts were tightened with 8N.

[0066] In this state, the current density is 50 μA / cm 2 The battery was discharged and the initial discharge capacity was measured under the following conditions: measurement temperature: 25° C., cutoff voltage: 2.0 to 3.9 V (when NCM was used as the positive electrode active material 214 in the sample of the positive electrode 114), 2.0 to 3.7 V (when NCA or LCO was used as the positive electrode active material 214 in the sample of the positive electrode 114), and −0.6 to 1.0 V (sample of the negative electrode 116). For the positive electrode 114, if the discharge capacity was less than 50 μAh, it was judged as “×” (fail), if the discharge capacity was 50 μAh or more but less than 400 μAh, it was judged as “◯” (pass), and if the discharge capacity was 400 μAh or more, it was judged as “◎” (excellent). For the negative electrode 116, if the discharge capacity was less than 100 μAh, it was judged as "X" (fail), if the discharge capacity was 100 μAh or more and less than 400 μAh, it was judged as "O" (pass), and if the discharge capacity was 400 μAh or more, it was judged as "◎" (excellent).

[0067] 5 and 6, for the positive electrode 114, sample S12 not containing ionic liquid 224 had a discharge capacity of less than 50 μAh and was therefore determined to be unsatisfactory (×). Because sample S12 does not contain ionic liquid 224, the contact between the particles of the oxide-based lithium ion conductive solid electrolyte 204 becomes point contact, increasing the resistance between the particles, which is thought to result in reduced lithium ion conductivity within the electrode and at the interfaces between the electrode and other members, resulting in reduced battery capacity.

[0068] In contrast, in the samples S1 to S11 (except for sample S6) containing the ionic liquid 224, the discharge capacity was 50 μAh or more, and therefore they were judged to be pass (◯) or excellent (◎). Since these samples contain the ionic liquid 224, the ionic liquid 224 that functions as a lithium ion conductive path is interposed between the particles of the oxide-based lithium ion conductive solid electrolyte 204, improving the lithium ion conductivity at the grain boundaries, and as a result, it is considered that the lithium ion conductivity in the electrode and at the interface between the electrode and other members is improved, and the capacity of the battery is increased. From this result, it can be said that when the positive electrode 114 contains the ionic liquid 224 in addition to the oxide-based lithium ion conductive solid electrolyte 204 and the positive electrode active material 214, the lithium ion conductivity in the electrode and at the interface between the electrode and other members can be improved.

[0069] In addition, samples S7 to S11 were judged to be excellent (◎) because the discharge capacity was 400 μAh or more. In these samples, the volume content of the positive electrode active material 214 was 40 vol% or more and 85 vol% or less, the volume content of the oxide-based lithium ion conductive solid electrolyte 204 was 5 vol% or more and 40 vol% or less, and the volume content of the ionic liquid 224 was 3 vol% or more and 35 vol% or less. On the other hand, sample S6 was judged to be unmeasurable (-) because the ionic liquid exuded during molding. From these results, it can be said that if the electrode satisfies the above conditions for the volume content, the lithium ion conductivity in the electrode and at the interface between the electrode and other members can be effectively improved while suppressing the occurrence of the exudation of the ionic liquid.

[0070] 7 and 8, the negative electrode 116 was determined to be unsatisfactory (×) because the discharge capacity of sample S33, which does not contain ionic liquid 226, was less than 100 μAh. Since sample S33 does not contain ionic liquid 226, the contact between the particles of the oxide-based lithium ion conductive solid electrolyte 206 becomes point contact, and the resistance between the particles increases, which is thought to result in a decrease in lithium ion conductivity within the electrode and at the interface between the electrode and other members, resulting in a decrease in the capacity of the battery.

[0071] In contrast, samples S21 to S32 (except sample S26) containing ionic liquid 226 had a discharge capacity of 100 μAh or more, and were therefore judged to be pass (◯) or excellent (◎). Since these samples contain ionic liquid 226, ionic liquid 226 functioning as a lithium ion conductive path is present between particles of oxide-based lithium ion conductive solid electrolyte 206, improving lithium ion conductivity at the grain boundaries, and as a result, lithium ion conductivity within the electrode and at the interface between the electrode and other members is improved, and the capacity of the battery is increased. From this result, it can be said that when negative electrode 116 contains ionic liquid 226 in addition to oxide-based lithium ion conductive solid electrolyte 206 and negative electrode active material 216, lithium ion conductivity within the electrode and at the interface between the electrode and other members can be improved.

[0072] In addition, samples S27 to S32 were judged to be excellent (◎) because the discharge capacity was 400 μAh or more. In these samples, the volume content of the negative electrode active material 216 was 40 vol% or more and 85 vol% or less, the volume content of the oxide-based lithium ion conductive solid electrolyte 206 was 5 vol% or more and 40 vol% or less, and the volume content of the ionic liquid 226 was 3 vol% or more and 35 vol% or less. On the other hand, sample S26 was judged to be unmeasurable (-) because the ionic liquid exuded during molding. From these results, it can be said that if the electrode satisfies the above conditions for the volume content, the lithium ion conductivity in the electrode and at the interface between the electrode and other members can be effectively improved while suppressing the occurrence of the exudation of the ionic liquid.

[0073] A-7. Preferred embodiments of LLZ-based ion conductive powder: As described above, the lithium ion conductor in this embodiment contains LLZ-based ion conductive powder (ion conductive solid electrolyte powder having a garnet-type crystal structure containing at least Li, La, Zr, and O). As the LLZ-based ion conductive powder, it is preferable to adopt one containing at least one element selected from the group consisting of Mg, Al, Si, Ca (calcium), Ti, V (vanadium), Ga (gallium), Sr, Y (yttrium), Nb (niobium), Sn (tin), Sb (antimony), Ba (barium), Hf (hafnium), Ta (tantalum), W (tungsten), Bi (bismuth), and lanthanoid elements. With this configuration, the LLZ-based ion conductive powder exhibits good lithium ion conductivity.

[0074] It is also preferable to adopt an LLZ-based ion-conductive powder that contains at least one of Mg and element A (A is at least one element selected from the group consisting of Ca, Sr and Ba), and in which the molar ratios of the contained elements satisfy the following formulas (1) to (3). Since Mg and element A are relatively abundant and inexpensive, the use of Mg and / or element A as a substitution element for the LLZ-based ion-conductive powder is expected to ensure a stable supply of the LLZ-based ion-conductive powder and reduce costs. (1) 1.33≦Li / (La+A)≦3 (2) 0≦Mg / (La+A)≦0.5 (3) 0≦A / (La+A)≦0.67

[0075] It is more preferable to adopt an LLZ-based ion-conductive powder that contains both Mg and element A, and in which the molar ratios of the contained elements satisfy the following formulas (1') to (3'). (1´)2.0≦Li / (La+A)≦2.5 (2´)0.01≦Mg / (La+A)≦0.14 (3´)0.04≦A / (La+A)≦0.17

[0076] In other words, it is preferable that the LLZ-based ion-conductive powder satisfies any one of the following (a) to (c), and among these, it is more preferable that it satisfies (c), and even more preferable that it satisfies (d). (a) Mg is contained, and the content of each element satisfies, in terms of molar ratio, 1.33≦Li / La≦3 and 0≦Mg / La≦0.5. (b) The element A is contained, and the content of each element satisfies, in terms of molar ratio, 1.33≦Li / (La+A)≦3 and 0≦A / (La+A)≦0.67. (c) Contains Mg and element A, and the content of each element satisfies, in molar ratio, 1.33≦Li / (La+A)≦3, 0≦Mg / (La+A)≦0.5, and 0≦A / (La+A)≦0.67. (d) Contains Mg and element A, and the content of each element satisfies, in molar ratio, 2.0≦Li / (La+A)≦2.5, 0.01≦Mg / (La+A)≦0.14, and 0.04≦A / (La+A)≦0.17.

[0077] When the LLZ-based ion-conductive powder satisfies the above (a), that is, when it contains Li, La, Zr and Mg in a molar ratio that satisfies the above formulas (1) and (2), it exhibits good lithium ion conductivity. Although the mechanism is not clear, for example, when the LLZ-based ion-conductive powder contains Mg, since the ionic radius of Li and the ionic radius of Mg are close, Mg is likely to be arranged at the Li site where Li is arranged in the LLZ crystal phase, and when Li is replaced by Mg, vacancies are generated at the Li site in the crystal structure due to the difference in charge between Li and Mg, making it easier for Li ions to move, and as a result, it is considered that the lithium ion conductivity is improved. In the LLZ-based ion-conductive powder, when the molar ratio of Li to the sum of La and element A is less than 1.33 or exceeds 3, not only the ion-conductive powder having a garnet-type crystal structure but also another metal oxide is likely to be formed. As the content of another metal oxide increases, the content of the ion-conductive powder having a garnet-type crystal structure becomes smaller relatively, and the lithium ion conductivity of the other metal oxide is low, so that the lithium ion conductivity decreases. As the Mg content in the LLZ-based ion-conductive powder increases, Mg is placed at the Li site, creating vacancies at the Li site and improving the lithium ion conductivity, but if the molar ratio of Mg to the sum of La and element A exceeds 0.5, another metal oxide containing Mg is likely to be formed. As the content of this other metal oxide containing Mg increases, the content of the ion-conductive powder having a garnet-type crystal structure decreases relatively. Since the lithium ion conductivity of the other metal oxide containing Mg is low, if the molar ratio of Mg to the sum of La and element A exceeds 0.5, the lithium ion conductivity decreases.

[0078] When the LLZ-based ion-conductive powder satisfies the above (b), that is, when it contains Li, La, Zr and element A in such a molar ratio that it satisfies the above formulas (1) and (3), it exhibits good lithium ion conductivity. Although the mechanism is not clear, for example, when the LLZ-based ion-conductive powder contains element A, since the ionic radius of La and the ionic radius of element A are close, element A is likely to be arranged at the La site where La is arranged in the LLZ crystal phase, and La is replaced by element A, which generates lattice distortion, and the number of free Li ions increases due to the difference in charge between La and element A, thereby improving the lithium ion conductivity. In the LLZ-based ion-conductive powder, when the molar ratio of Li to the sum of La and element A is less than 1.33 or exceeds 3, not only the ion-conductive powder having a garnet-type crystal structure but also other metal oxides are likely to be formed. As the content of other metal oxides increases, the content of the ion-conductive powder having a garnet-type crystal structure decreases relatively, and the lithium ion conductivity of the other metal oxides is low, so that the lithium ion conductivity decreases. As the content of element A in the LLZ-based ion-conductive powder increases, more of element A is placed at the La site, the lattice distortion increases, and the difference in charge between La and element A increases the number of free Li ions, improving the lithium ion conductivity, but if the molar ratio of element A to the sum of La and element A exceeds 0.67, another metal oxide containing element A is likely to be formed. As the content of this other metal oxide containing element A increases, the content of the ion-conductive powder having a garnet-type crystal structure decreases relatively, and the lithium ion conductivity of the other metal oxide containing element A is low, so the lithium ion conductivity decreases.

[0079] The element A is at least one element selected from the group consisting of Ca, Sr, and Ba. Ca, Sr, and Ba are group 2 elements in the periodic table, and have the common property of easily becoming divalent cations and having similar ionic radii. Ca, Sr, and Ba all have similar ionic radii to La, and therefore are likely to replace La located at the La site in the LLZ-based ion-conductive powder. It is preferable that the LLZ-based ion-conductive powder contains Sr among these elements A, because it can be easily formed by sintering and high lithium ion conductivity can be obtained.

[0080] When the LLZ-based ion-conductive powder satisfies the above (c), that is, when it contains Li, La, Zr, Mg, and element A in a molar ratio that satisfies the above formulas (1) to (3), it can be easily formed by sintering, and the lithium ion conductivity is further improved. When the LLZ-based ion-conductive powder satisfies the above (d), that is, when it contains Li, La, Zr, Mg, and element A in a molar ratio that satisfies the above formulas (1') to (3'), the lithium ion conductivity is further improved. Although the mechanism is not clear, it is considered that, for example, Li at the Li site in the LLZ-based ion-conductive powder is replaced by Mg, and La at the La site is replaced by element A, which creates vacancies at the Li site and increases the number of free Li ions, thereby further improving the lithium ion conductivity. Furthermore, it is preferable that the LLZ-based ion conductive powder contains Li, La, Zr, Mg and Sr so as to satisfy the above formulas (1) to (3), particularly so as to satisfy the above formulas (1') to (3'), in order to obtain a lithium ion conductor having high lithium ion conductivity and high relative density.

[0081] In any of the above cases (a) to (d), the LLZ-based ion-conductive powder preferably contains Zr in a molar ratio that satisfies the following formula (4). By containing Zr in this range, it becomes easier to obtain an ion-conductive powder having a garnet-type crystal structure. (4) 0.33≦Zr / (La+A)≦1

[0082] B. Variations: The technology disclosed in this specification is not limited to the above-described embodiments, and can be modified in various forms without departing from the spirit of the invention. For example, the following modifications are also possible.

[0083] The configuration of the all-solid-state battery 102 in the above embodiment is merely an example and can be modified in various ways. For example, in the above embodiment, the positive electrode 114 and the negative electrode 116 contain an oxide-based lithium ion conductive solid electrolyte, an active material, and an ionic liquid, but the positive electrode 114 and the negative electrode 116 may contain components other than these.

[0084] In the above embodiment, a configuration containing an oxide-based lithium ion conductive solid electrolyte, an active material, and an ionic liquid is adopted for both the positive electrode 114 and the negative electrode 116, but such a configuration may be adopted for only one of the positive electrode 114 and the negative electrode 116. For example, a configuration may be adopted in which the positive electrode 114 contains an ionic liquid, but the negative electrode 116 does not contain an ionic liquid.

[0085] In the above embodiment, the materials forming each element constituting the all-solid-state battery 102 are merely examples, and each element may be formed of other materials. In the above embodiment, the manufacturing method of the all-solid-state battery 102 is merely an example, and other manufacturing methods may be adopted.

[0086] Furthermore, the technology disclosed in this specification is not limited to electrodes for the all-solid-state battery 102, but can also be applied to electrodes for other electricity storage devices (for example, lithium-air batteries, lithium flow batteries, solid-state capacitors, etc.). [Explanation of symbols]

[0087] 102: All-solid-state lithium-ion secondary battery 110: Battery body 112: Solid electrolyte layer 114: Positive electrode 116: Negative electrode 154: Positive electrode side current collector 156: Negative electrode side current collector 204, 206: Oxide-based lithium ion conductive solid electrolyte 214: Positive electrode active material 216: Negative electrode active material 224, 226: Ionic liquid 300: Pressurizing jig

Claims

1. In an electrode for an electricity storage device, an oxide-based lithium ion conductive solid electrolyte; An active material; An ionic liquid; Contains The active material is LiFePO 4 or NCA, The volume content of the active material is 40 vol% or more and 85 vol% or less, The volume content of the oxide-based lithium ion conductive solid electrolyte is 5 vol% or more and 40 vol% or less, An electrode for an electricity storage device, wherein a volume content of the ionic liquid is 3 vol % or more and 35 vol % or less.

2. The electrode for an electricity storage device according to claim 1 , The oxide-based lithium ion conductive solid electrolyte has a garnet-type crystal structure containing at least Li, La, Zr, and O. An electrode for an electricity storage device.

3. An electricity storage device including a solid electrolyte layer, a positive electrode, a negative electrode, and a current collector, The positive electrode is the electrode for an electricity storage device according to claim 1 or 2. The present invention relates to an electricity storage device.

Citation Information

Patent Citations

  • Positive electrode mixture composition

    JP2013191547A

  • High conducting oxide - sulfide composite lithium superionic conductor

    US20150171463A1

  • Solid electrolyte composition, binder particle, all-solid secondary battery sheet, all-solid secondary battery electrode sheet and all-solid secondary battery, and production method therefor

    WO2017099248A1