Thin-film transistor

A multi-layered metal oxide thin film structure in thin film transistors enhances mobility and stability, addressing the limitations of silicon-based transistors for flexible displays.

JP7593955B2Active Publication Date: 2024-12-03JUSUNG ENG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021577145
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-05
Filing Date
2020-07-03
Publication Date
2024-12-03
Estimated Expiration
2040-07-03

AI Technical Summary

Technical Problem

Thin film transistors using silicon substrates are heavy and inflexible, limiting their application in flexible display devices, and require high-speed operation which is challenging with amorphous silicon, necessitating the development of metal oxide thin films as active layers.

Method used

A thin film transistor with a multi-layered active layer comprising a first metal oxide thin film with high conductivity, a second metal oxide thin film with lower conductivity, and a third metal oxide thin film with even lower conductivity, formed from indium-zinc oxide or indium-gallium-zinc oxide, to enhance mobility and stability.

Benefits of technology

The multi-layered metal oxide thin film structure improves the mobility and stability of the thin film transistor, enabling high-speed operation and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593955000001
    Figure 0007593955000001
  • Figure 0007593955000002
    Figure 0007593955000002
  • Figure 0007593955000003
    Figure 0007593955000003
Patent Text Reader

Abstract

A thin film transistor according to an embodiment of the present invention is a thin film transistor comprising an active layer formed between a gate insulating film and source and drain electrodes, the active layer comprising a first metal oxide thin film, a second metal oxide thin film disposed between the first metal oxide thin film and the gate insulating film and having a lower electrical conductivity than the first metal oxide thin film, and a third metal oxide thin film disposed between the first metal oxide thin film and the source and drain electrodes and having a lower electrical conductivity than the first metal oxide thin film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thin film transistor, and more particularly to a thin film transistor using a metal oxide thin film as an active layer. [Background technology]

[0002] 2. Description of the Related Art Thin film transistors (TFTs) are used as circuits for independently driving each pixel in semiconductor devices, liquid crystal displays (LCDs), organic electroluminescence (EL) displays, and the like.

[0003] Such a thin film transistor is formed on a lower substrate of a display device together with a gate line and a data line, that is, the thin film transistor includes a gate electrode which is a part of the gate line, an active layer used as a channel, a source electrode and a drain electrode which are a part of the data line, and a gate insulating film.

[0004] The active layer of a thin film transistor forms a channel region between the gate electrode and the source and drain electrodes, and has been formed using amorphous silicon or crystalline silicon. However, a substrate for a thin film transistor using silicon has the disadvantages of being heavy because a glass substrate must be used, and not being flexible, making it impossible to use it as a flexible display device. In addition, in order to realize high-speed elements, i.e., to improve mobility, the need to apply a crystalline thin film with high carrier concentration and excellent electrical conductivity to the active layer is gradually increasing, and for this reason, efforts are being actively made on technology that uses a metal oxide thin film as the active layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Republic of Korea Publication Patent No. 10-2004-0013273 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention provides a thin film transistor that uses a metal oxide thin film as an active layer and has high mobility and improved stability. [Means for solving the problem]

[0007] A thin film transistor according to an embodiment of the present invention is a thin film transistor comprising an active layer formed between a gate insulating film and source and drain electrodes, the active layer comprising a first metal oxide thin film, a second metal oxide thin film disposed between the first metal oxide thin film and the gate insulating film and having a lower electrical conductivity than the first metal oxide thin film, and a third metal oxide thin film disposed between the first metal oxide thin film and the source and drain electrodes and having a lower electrical conductivity than the first metal oxide thin film.

[0008] The first metal oxide thin film may be formed of an oxide of a first metal material including indium (In) and zinc (Zn), the second metal oxide thin film may be formed of an oxide of a second metal material including indium (In), gallium (Ga) and zinc (Zn), and the third metal oxide thin film may be formed of an oxide of a third metal material including indium (In), gallium (Ga) and zinc (Zn).

[0009] The indium (In) in the first metal oxide thin film may be contained in an amount of 30 at % or more and less than 80 at % with respect to the entire first metal substance.

[0010] The gallium (Ga) in the second metal oxide thin film may be contained at 30 at% or more and less than 60 at% relative to the entire second metal material, and the gallium (Ga) in the third metal oxide thin film may be contained at 30 at% or more and less than 60 at% relative to the entire third metal material.

[0011] The third metal oxide thin film may have a lower electrical conductivity than the second metal oxide thin film.

[0012] The amount of gallium (Ga) contained in the third metal material may be greater than the amount of gallium (Ga) contained in the second metal material.

[0013] The first metal material may further contain gallium (Ga), and the gallium (Ga) in the first metal oxide thin film may be contained in an amount of less than 30 at % based on the total amount of the first metal material.

[0014] The gallium (Ga) in the first metal oxide thin film may be contained in an amount of 20 at % or more and less than 60 at % with respect to the gallium (Ga) contained in the entire active layer.

[0015] The second metal oxide thin film may have a thickness smaller than that of the first metal oxide thin film, and the third metal oxide thin film may have a thickness larger than that of the first metal oxide thin film.

[0016] The first metal oxide thin film is formed to a thickness of 100 Å or more and less than 150 Å; The second metal oxide thin film may be formed to a thickness of less than 50 Å, and the third metal oxide thin film may be formed to a thickness of 150 Å or more and less than 200 Å.

[0017] The first metal oxide thin film may comprise a zinc oxide (ZnO) thin film doped with a first impurity, the second metal oxide thin film may comprise a zinc oxide (ZnO) thin film doped with a first impurity and a second impurity, and the third metal oxide thin film may comprise a zinc oxide (ZnO) thin film doped with a first impurity and a second impurity, wherein the first impurity includes indium (In) and the second impurity includes at least one of gallium (Ga) and tin (Sn).

[0018] The first metal oxide thin film may be further doped with a second impurity.

[0019] The gallium (Ga) content may vary gradually.

[0020] The gallium (Ga) content may have two or more non-consecutive values. Effect of the Invention

[0021] According to the thin film transistor of the embodiment of the present invention, by varying the ratio of gallium in the metal oxide thin film constituting the active layer, it is possible to operate at high speed and improve stability.

[0022] Furthermore, when the active layer is formed from a plurality of metal oxide thin film layers, by varying the proportion of gallium in each of the plurality of metal oxide thin films contained in the active layer, it is possible to operate at high speed and improve stability.

[0023] That is, the mobility can be improved by adjusting the composition and thickness of the first metal oxide thin film that forms the main charge transfer path between the gate electrode and the source and drain electrodes, and the stability of the device can be improved by adjusting the composition and thickness of the second metal oxide thin film that forms the interface between the gate insulating film and the first metal oxide thin film and the third metal oxide thin film that forms the interface between the first metal oxide thin film and the source and drain electrodes. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a schematic diagram of a thin film transistor according to an embodiment of the present invention. [Diagram 2] FIG. 2 illustrates an active layer comprising a metal oxide thin film according to an embodiment of the present invention. [Diagram 3] FIG. 4 is a schematic diagram of a thin film transistor according to another embodiment of the present invention; [Figure 4] FIG. 2 is a schematic diagram illustrating a deposition apparatus used in manufacturing a thin film transistor according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, the present invention will be described in more detail with reference to the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, and may be embodied in various different forms. These embodiments are provided merely to complete the disclosure of the present invention and to fully convey the scope of the invention to those skilled in the art.

[0026] Throughout the specification, when a component, such as a film, region, or substrate, is referred to as being "on" another component, it may be interpreted that the component may be directly in contact with the other component, or that there may be additional components interposed therebetween.

[0027] Additionally, relative terms such as "upper" or "lower" may be used herein to describe the relative relationship of one element to another element as illustrated. The relative terms may be understood to be intended to include other orientations of the elements in addition to the orientation depicted in the figures. Herein, in order to explain the invention in detail, the figures may be exaggerated, and in the figures, the same reference numerals refer to the same elements.

[0028] FIG. 1 is a schematic diagram of a thin film transistor according to an embodiment of the present invention, and FIG. 2 is a diagram showing an active layer comprising a metal oxide thin film according to an embodiment of the present invention.

[0029] 1 and 2, a thin film transistor according to an embodiment of the present invention is a thin film transistor comprising a gate insulating film 120, source and drain electrodes 140, and an active layer 130 formed between the gate insulating film 120 and the source and drain electrodes 140, the active layer 130 comprising a first metal oxide thin film 130a, a second metal oxide thin film 130b disposed between the first metal oxide thin film 130a and the gate insulating film 120 and having a lower electrical conductivity than the first metal oxide thin film 130a, and a third metal oxide thin film 130c disposed between the first metal oxide thin film 130a and the source and drain electrodes 140 and having a lower electrical conductivity than the first metal oxide thin film 130a.

[0030] Here, the thin film transistor according to an embodiment of the present invention may be a bottom gate type thin film transistor including a gate electrode 110 formed on a substrate 100, a gate insulating film 120 formed on the gate electrode 110, an active layer 130 formed on the gate insulating film 120, and source and drain electrodes 140 formed spaced apart from each other on the active layer 130, as shown in FIG. 1.

[0031] The substrate 100 may be a transparent substrate, such as a silicon substrate, a glass substrate, or a plastic substrate in the case of implementing a flexible display. The substrate 100 may be a reflective substrate, in which case a metal substrate may be used. The metal substrate may be made of stainless steel (SUS), titanium (Ti), molybdenum (Mo), or an alloy thereof. Meanwhile, when a metal substrate is used as the substrate 100, it is preferable to form an insulating film on the metal substrate.

[0032] The gate electrode 110 may be formed using a conductive material, for example, at least one of aluminum (Al), neodymium (Nd), silver (Ag), chromium (Cr), titanium (Ti), tantalum (Ta), molybdenum (Mo), and copper (Cu), or an alloy containing these metals. The gate electrode 110 may be formed not only as a single layer, but also as a multilayer consisting of multiple metal layers. That is, the gate electrode 110 may be formed as a double layer including a metal layer such as chromium (Cr), titanium (Ti), tantalum (Ta), or molybdenum (Mo) having excellent physicochemical properties and an aluminum (Al), silver (Ag), or copper (Cu) metal layer having low resistivity.

[0033] The gate insulating film 120 is formed at least on the upper part of the gate electrode 110. That is, the gate insulating film 120 may be formed on the substrate 100 including the upper and side parts of the gate electrode 110. The gate insulating film 120 may be formed using one or more insulating materials selected from inorganic insulating materials such as silicon oxide (SiO2), silicon nitride (SiN), alumina (Al2O3), and zirconia (ZrO2), which have excellent adhesion to metal materials and excellent dielectric strength.

[0034] The active layer 130 is formed between the gate insulating film 120 and the source and drain electrodes 140, and is formed so that at least a portion of the active layer 130 overlaps with the gate electrode 110. Here, the active layer 130 may be formed from a single metal oxide thin film 130, or may be formed from a plurality of metal oxide thin films. In the case of a plurality of metal oxide thin films, the active layer 130 is formed from a plurality of metal oxide thin films including a first metal oxide thin film 130a, a second metal oxide thin film 130b, and a third metal oxide thin film 130c. According to an embodiment of the present invention, the second metal oxide thin film 130b may be formed between the gate insulating film 120 and the source and drain electrodes 140, the first metal oxide thin film 130a may be formed between the gate insulating film 120 and the second metal oxide thin film 130b, and the third metal oxide thin film 130c may be formed between the first metal oxide thin film 130a and the source and drain electrodes 140.

[0035] Here, the second metal oxide thin film 130b and the third metal oxide thin film 130c may have a lower electrical conductivity than the first metal oxide thin film 130a. More specifically, the second metal oxide thin film 130b and the third metal oxide thin film 130c may have a higher resistance value than the first metal oxide thin film 130a, and thus the second metal oxide thin film 130b and the third metal oxide thin film 130c may have a lower electrical conductivity than the first metal oxide thin film 130a. The electrical conductivity of the first metal oxide thin film 130a, the second metal oxide thin film 130b, and the third metal oxide thin film 130c may be adjusted by controlling the type and content of the metal element contained in the first metal oxide thin film 130a, the second metal oxide thin film 130b, and the third metal oxide thin film 130c, respectively, and the thickness of each metal oxide thin film.

[0036] Here, the first metal oxide thin film 130a forms a main channel between the gate electrode 110 and the source and drain electrodes 140. The first metal oxide thin film 130a forms a main path for charge transfer in the active layer 130 when a voltage is applied to the gate electrode 110, and therefore needs to have a relatively high electrical conductivity in order to improve mobility.

[0037] Meanwhile, the second metal oxide thin film 130b forms an interface between the gate insulating film 120 and the first metal oxide thin film 130a. The second metal oxide thin film 130b also plays a role in preventing hydrogen (H) ions contained in the gate insulating film 120 from diffusing into the first metal oxide thin film 130a. That is, when manufacturing a thin film transistor, hydrogen (H) ions are inevitably present in the thin film depending on the materials used and the process. Although such hydrogen (H) ions have the advantage of filling the vacant space in the active layer 130 and ensuring the stability of driving, when excessive hydrogen (H) ions diffuse from the gate insulating film 120, they cause the inconvenience of deteriorating the interface charge characteristics. For this reason, the second metal oxide thin film 130b is required to have improved stability and is required to have a lower electrical conductivity than the first metal oxide thin film 130a.

[0038] The third metal oxide thin film 130c forms an interface between the first metal oxide thin film 130a and the source and drain electrodes 140. The third metal oxide thin film 130c also plays a role in blocking hydrogen (H) ions and hydroxide (OH) ions penetrating from the external environment. The third metal oxide thin film 130c serves to prevent the thin film from becoming a conductor due to the formation of a channel, and therefore the third metal oxide thin film 130c is required to have high stability and a lower electrical conductivity than the first metal oxide thin film 130a.

[0039] In this case, the second metal oxide thin film 130b may have a higher electrical conductivity than the third metal oxide thin film 130c. As described above, the second metal oxide thin film 130b is disposed adjacent to the gate insulating film 120. Therefore, when a voltage is applied to the gate electrode 110, charges are accumulated in the second metal oxide thin film 130b, and a main transfer path of the charges via the first metal oxide thin film 130a is formed, so that the second metal oxide thin film 130b is formed to have a higher electrical conductivity than the third metal oxide thin film 130c. In addition, the third metal oxide thin film 130c is closely related to making a thin film transistor a conductor. In other words, if the electrical conductivity of the third metal oxide thin film 130c is high, the active layer 130 will have the disadvantage of forming a path for charge transfer between the source and drain electrodes 140 regardless of the application of a voltage to the gate electrode 110, so the resistance of the third metal oxide thin film 130c needs to be higher than that of the second metal oxide thin film 130b.

[0040] Here, in the thin film transistor according to the embodiment of the present invention, the electrical conductivity of the first metal oxide thin film 103a, the second metal oxide thin film 130b, and the third metal oxide thin film 130c may be adjusted by controlling the type and content of the metal element contained in each metal oxide thin film.

[0041] Indium (In) is a metal with a relatively low band gap and a relatively high standard electrode potential, and is characterized by lowering resistance and increasing electrical conductivity to improve mobility, whereas gallium (Ga) is a metal with a relatively high band gap and a relatively high standard electrode potential, and is characterized by increasing resistance and decreasing electrical conductivity to improve stability.

[0042] Therefore, the first metal oxide thin film 130a may be formed of an oxide of a first metal material containing indium (In) and zinc (Zn) or containing indium (In), gallium (Ga) and zinc (Zn) to improve mobility, the second metal oxide thin film 130b may be formed of an oxide of a second metal material containing indium (In), gallium (Ga) and zinc (Zn) to improve stability, and the third metal oxide thin film 130b may be formed of an oxide of a third metal material containing indium (In), gallium (Ga) and zinc (Zn) to improve stability.

[0043] That is, the first metal oxide thin film 130a may comprise a zinc oxide (ZnO) thin film doped with indium (In) or doped with indium (In) and gallium (Ga), the second metal oxide thin film 130b may comprise a zinc oxide (ZnO) thin film doped with indium (In) and gallium (Ga), and the third metal oxide thin film 130b may comprise a zinc oxide (ZnO) thin film doped with indium (In) and gallium (Ga). Here, indium (In) or gallium (Ga) may be an impurity and may be doped into the zinc oxide (ZnO) thin film, and at least a part or all of the gallium (Ga) doped into the zinc oxide (ZnO) thin film may be replaced with tin (Sn). The following description will focus on an embodiment in which the second metal oxide thin film 130b and the third metal oxide thin film 130b contain gallium (Ga); however, it goes without saying that the following content can be applied as it is even when tin (Sn) is contained.

[0044] More specifically, the first metal oxide thin film 130a may include indium-zinc oxide (IZO; In-Zn-O) or indium-gallium-zinc oxide (IGZO; In-Ga-Zn-O), and the second metal oxide thin film 130b and the third metal oxide thin film 130c may include indium-gallium-zinc oxide (IGZO; In-Ga-Zn-O).

[0045] The first metal oxide thin film 130a may contain indium (In) and zinc (Zn). The indium (In) in the first metal oxide thin film 130a may be contained in an amount of 30 at% or more and less than 80 at% based on the entire first metal material. If the indium (In) is contained in an amount of less than 30 at%, the electrical conductivity decreases and the mobility decreases, and if the indium (In) is contained in an amount of 80 at% or more, the electrical conductivity increases excessively, and leakage current and off current increase. For this reason, the indium (In) in the first metal oxide thin film 130a may be contained in a range of 30 at% or more and less than 80 at% based on the entire first metal material, or may be contained in at least two or more contents having discontinuous values ​​within the range, or may be continuously different within the range. In this case, it is possible to have improved mobility while minimizing leakage current and off-current.

[0046] Here, when the first metal material forming the first metal oxide thin film contains indium (In) and zinc (Zn), zinc (Zn) may be contained at 20 to 70 at% (atomic %) with respect to the entire first metal material.

[0047] Also, the first metal material forming the first metal oxide thin film 130a may further contain gallium (Ga). That is, the first metal oxide thin film 130a may be formed from an oxide of a first metal material containing indium (In), gallium (Ga) and zinc (Zn), and in this case, the gallium (Ga) in the first metal oxide thin film 130a may be contained in an amount of less than 30 at% with respect to the entire first metal material in the first metal oxide thin film 130a. The gallium (Ga) in the first metal material is contained to improve stability, and if the content of gallium (Ga) is 30 at% or more with respect to the entire first metal material, resistance increases excessively, so the gallium (Ga) in the first metal oxide thin film 130a may be contained in an amount of more than 0 at% and less than 30 at% with respect to the entire first metal material. Meanwhile, in order to improve stability and maintain electrical conductivity of the first metal oxide thin film 130a forming the main channel, the gallium (Ga) contained in the first metal material may be 20 at% or more and less than 60 at% of the gallium (Ga) contained in the entire active layer 130, or may be contained in at least two or more contents having discontinuous values ​​within the range, or the contents may vary continuously within the range. The above content is similarly applicable even when the first metal oxide thin film 130a further contains tin (Sn) instead of gallium (Ga).

[0048] Meanwhile, the content of gallium (Ga) in the second metal oxide thin film 130b may be 30 at% or more and less than 60 at% with respect to the entire second metal material in the second metal oxide thin film 130b. If the content of gallium (Ga) is less than 30 at%, there is a disadvantage that stability-related properties such as negative bias temperature instability (NBTS) and positive bias temperature instability (PBTI) are degraded, and if the content of gallium (Ga) is 60 at% or more, there is a disadvantage that a porous film is formed, resulting in an increase in surface roughness and a significant decrease in mobility. Therefore, the gallium (Ga) content in the second metal oxide thin film 130b may be within a range of 30 at % or more and less than 60 at % of the entire second metal material, or may be at least two or more contents having discontinuous values ​​within the range, or may be continuously different contents within the range, in which case the stability of the device can be improved.

[0049] Furthermore, the third metal oxide thin film 130c may contain gallium (Ga) in an amount of 30 at% or more and less than 60 at% based on the total amount of the third metal material in the third metal oxide thin film 130c. If the amount of gallium (Ga) is less than 30 at%, the thin film transistor is likely to become conductive, whereas if the amount of gallium (Ga) is more than 60 at%, a porous film is formed, resulting in increased surface roughness and a significant decrease in mobility. As described above, if gallium (Ga) is contained in at least two or more contents having discontinuous values ​​within the range of 30 at% or more and less than 60 at%, or if the contents are continuously different within the range, the stability of the device can be improved while preventing the active layer 130 of the thin film transistor from becoming conductive.

[0050] The amount of gallium (Ga) contained in the third metal material in the third metal oxide thin film 130c may be greater than the amount of gallium (Ga) contained in the second metal material in the second metal oxide thin film 130b. As described above, the second metal oxide thin film 130b is formed to have a higher electrical conductivity than the third metal oxide thin film 130c. Here, since gallium (Ga) has the characteristic of increasing resistance and decreasing electrical conductivity to improve stability, the amount of gallium (Ga) contained in the third metal material in the third metal oxide thin film 130c is greater than the amount of gallium (Ga) contained in the second metal material in the second metal oxide thin film 130b, thereby relatively improving the stability of the third metal oxide thin film 130c compared to the second metal oxide thin film 130b, and preventing the thin film transistor from becoming conductive.

[0051] Meanwhile, in the thin film transistor according to the embodiment of the present invention, the electrical conductivity of the first metal oxide thin film 130a, the second metal oxide thin film 130b, and the third metal oxide thin film 130c may be adjusted by controlling the thickness of each metal oxide thin film.

[0052] More specifically, the electrical conductivity of the first metal oxide thin film 130a may be controlled by adjusting the content of indium (In) contained in the first metal material forming the first metal oxide thin film 130a. Also, the electrical conductivity of the second metal oxide thin film 130b and the third metal oxide thin film 130c may be controlled by controlling the thicknesses of the second metal oxide thin film 130b and the third metal oxide thin film 130c. To this end, the thickness d2 of the second metal oxide thin film 130b may be thinner than the thickness d1 of the first metal oxide thin film 130a, and the thickness d3 of the third metal oxide thin film 130c may be thicker than the thickness d1 of the first metal oxide thin film 130a.

[0053] The first metal oxide thin film 130a forms a main channel between the gate electrode 110 and the source and drain electrodes 140, and the second metal oxide thin film 130b and the third metal oxide thin film 130c are for device stability. The first metal oxide thin film 130a has a higher indium (In) content than the second metal oxide thin film 130b and the third metal oxide thin film 130c, and if gallium (Ga) is included, the content of gallium (Ga) is reduced, so that the first metal oxide thin film 130a has a low resistance and high electrical conductivity.

[0054] On the other hand, the second metal oxide thin film 130b is for device stability, but since the second metal oxide thin film 130b is disposed adjacent to the gate insulating film 120, it is necessary for the second metal oxide thin film 130b to have electrical conductivity at a predetermined level or higher. For this reason, the second metal oxide thin film 130 has a lower content of indium (In) and an increased content of gallium (Ga) compared to the first metal oxide thin film 130a, and the thickness d2 of the second metal oxide thin film 130b is formed thinner than the thickness d1 of the first metal oxide thin film 130a, so that the second metal oxide thin film 130b has electrical conductivity at a predetermined level or higher.

[0055] The third metal oxide thin film 130c, like the second metal oxide thin film 130b, is for device stability, but if the third metal oxide thin film 130c has high electrical conductivity, the thin film transistor may become conductive. Therefore, the third metal oxide thin film 130c has a lower indium (In) content and a higher gallium (Ga) content than the first metal oxide thin film 130a, and the thickness d3 of the third metal oxide thin film 130c is formed thicker than the thickness d1 of the first metal oxide thin film 130a to increase resistance and ensure device stability. The first metal oxide thin film 130a may be formed to a thickness of 100 Å or more and less than 150 Å, the second metal oxide thin film 130b may be formed to a thickness less than 50 Å, and the third metal oxide thin film 130c may be formed to a thickness of 150 Å or more and less than 200 Å.

[0056] The source and drain electrodes 140 are formed on the active layer 130 and partially overlap the gate electrode 110, so that the source electrode and the drain electrode are formed separately from each other with the gate electrode 110 sandwiched therebetween. The source and drain electrodes 140b may be formed by the same process using the same material, or may be formed using a conductive material, for example, at least one metal selected from aluminum (Al), neodymium (Nd), silver (Ag), chromium (Cr), titanium (Ti), tantalum (Ta), and molybdenum (Mo), or an alloy containing these metals. That is, the source and drain electrodes 140 may be formed using the same material as the gate electrode 110, or may be formed using a material different from that of the gate electrode 110. The source and drain electrodes 140 may be formed not only as a single layer, but also as a multilayer of multiple metal layers.

[0057] FIG. 3 is a schematic diagram of a thin film transistor according to another embodiment of the present invention.

[0058] Referring to FIG. 3, a thin film transistor according to another embodiment of the present invention may be a top gate type thin film transistor including source and drain electrodes 140 formed separately from each other on a substrate 100, an active layer 130 formed on the source and drain electrodes, a gate insulating film 120 formed on the active layer, and a gate electrode 110 formed on the gate insulating film.

[0059] Even in the case of such a top gate type thin film transistor, the contents described above in connection with Figs. 1 and 2 can be applied as they are. That is, even in the case of the thin film transistor according to the other embodiment of the present invention, the active layer 130 may be formed of a plurality of metal oxide thin films, in which case the third metal oxide thin film 130c is located between the source and drain electrodes 140 and the first metal oxide thin film 130a, and the second metal oxide thin film 130b is located between the gate insulating film 120 and the first metal oxide thin film 130a. As such, even in the case of the thin film transistor according to the other embodiment of the present invention, the only difference is the stacking order of the metal oxide thin films, and the contents described in the thin film transistor according to the embodiment of the present invention can be applied as they are, so that the overlapping description will be omitted.

[0060] FIG. 4 is a schematic diagram illustrating a deposition apparatus used in manufacturing a thin film transistor according to an embodiment of the present invention.

[0061] Referring to FIG. 4, the thin film transistor according to the embodiment of the present invention is manufactured using a deposition apparatus capable of forming a plurality of metal oxide thin films in the same reaction chamber by performing a chemical vapor deposition (CVD) process or an atomic layer deposition (ALD) process, or by performing a chemical vapor deposition (CVD) process and an atomic layer deposition (ALD) process in this order.

[0062] The deposition apparatus used in the embodiment of the present invention includes a reaction chamber 300 having a predetermined reaction space, a susceptor 310 provided at the lower side inside the reaction chamber 300, an injector 320 provided at the upper side inside the reaction chamber 300 corresponding to the susceptor 310, a first raw gas supply unit 330 for supplying indium (In) gas, a second raw gas supply unit 340 for supplying gallium (Ga) gas, a third raw gas supply unit 350 for supplying zinc (Zn) gas, and a reaction gas supply unit 360 for supplying oxygen (O) gas. Here, as the reaction gas, a substance containing oxygen (O) may be used, and O2, N2O, CO2 may be excited into a plasma state and used, and O3 may be used. Although not shown, the deposition apparatus may further include a purge gas supply unit for supplying a purge gas such as an inert gas.

[0063] Here, the first, second and third raw material gas supply units 330, 340 and 350 may include raw material storage units 332, 342 and 352 for storing the respective raw materials, bubblers 334, 344 and 354 for vaporizing the raw materials to generate raw material gases, and raw material supply pipes 336, 346 and 356 for forming a supply path for the raw materials. The reactant gas supply unit 360 may include a reactant storage unit 362 for storing the reactant and a reactant supply pipe 366 for forming a supply path for the reactant, and may further include a bubbler when H2O or the like is used as the reactant. Meanwhile, the susceptor 310 may be incorporated with a heater (not shown) and a cooling means (not shown) to keep the substrate 100 at a desired process temperature. Here, a gate electrode, a gate insulating film and the like may be formed on the substrate 100, and at least one substrate 100 may be placed on the susceptor 310.

[0064] Here, the first metal oxide thin film 330a of the thin film transistor according to the embodiment of the present invention may be formed by a chemical vapor deposition process (CVD) or an atomic layer deposition process (ALD) using the deposition apparatus, and the second metal oxide thin film 130b and the third metal oxide thin film 130c may also be formed by a chemical vapor deposition process (CVD) or an atomic layer deposition process (ALD) using the deposition apparatus. Meanwhile, it goes without saying that the first metal oxide thin film 330a may be formed by a chemical vapor deposition process (CVD) using the deposition apparatus, and the second metal oxide thin film 130b and the third metal oxide thin film 130c may also be formed by an atomic layer deposition process (ALD) using the deposition apparatus. In the thin film transistor according to the embodiment of the present invention, the active layer 130 is formed by a chemical vapor deposition process or an atomic layer deposition process, so that a thin film can be deposited while maintaining a uniform film quality, and a multi-layered active layer can be easily formed by adjusting the supply amount of the raw material gas and the reaction gas.

[0065] In this case, for the second metal oxide thin film 130b, the first metal oxide thin film 130a, and the third metal oxide thin film 130c stacked in this order, the content of indium (In) or gallium (Ga) may be gradually increased or decreased in the interface region between the second metal oxide thin film 130b and the first metal oxide thin film 130a and the interface region between the first metal oxide thin film 130a and the third metal oxide thin film 130c. Also, the content of indium (In) or gallium (Ga) may be discontinuously or gradually increased or decreased in each of the second metal oxide thin film 130b, the first metal oxide thin film 130a, and the third metal oxide thin film 130c. In the embodiment of the present invention, the active layer 130 is formed using a deposition process such as a chemical vapor deposition process or an atomic layer deposition process, and such a change in content does not occur when the active layer 130 is formed using a sputtering process in which a target must be changed depending on the type of thin film to be formed.

[0066] For example, when the first metal oxide thin film 130a includes indium-zinc oxide (IZO), indium (In) gas and zinc (Zn) gas may be supplied through the first raw material gas supply unit 330 and the third raw material gas supply unit 350, and oxygen (O) gas may be supplied to the reaction chamber 300 through the reactive gas supply unit 360. In this case, in the chemical vapor deposition process, the raw material gas and the reactive gas are simultaneously supplied to the reaction chamber 300. In addition, in the atomic layer deposition process, the raw material gas is supplied to the reaction chamber 300 to adsorb the raw material on the substrate 100. Then, the supply of the raw material gas is stopped, and a purge gas such as an inert gas is supplied to purge the unadsorbed raw material gas. Then, oxygen (O) gas is supplied into the reaction chamber 300 through the reactive gas supply unit 360 to oxidize the raw material adsorbed on the substrate 100, thereby forming an atomic layer metal oxide thin film. The supply of the reaction gas is stopped, and unreacted reaction gas is purged by supplying a purge gas such as an inert gas into the reaction chamber 300. This cycle of supplying and purging the source gas and supplying and purging the reaction gas is repeated multiple times to form a metal oxide thin film of a desired thickness.

[0067] On the other hand, in the case where the first metal oxide thin film 130a contains indium gallium zinc oxide (IGZO), or the second metal oxide thin film 130b and the third metal oxide thin film 130c contain indium gallium zinc oxide (IGZO), the only difference is that indium (In) gas, gallium (Ga) gas, and zinc (Zn) gas are used as source gases and in the amounts supplied, so a duplicated description will be omitted.

[0068] Here, the processes of forming the first metal oxide thin film 130a, the second metal oxide thin film 130b, and the third metal oxide thin film 130c may be performed in the same reaction chamber 200. Also, in order to form the above-mentioned bottom gate type thin film transistor, the only difference is that the third metal oxide thin film 130c is formed on the source and drain electrodes 140, the second metal oxide thin film 130b is formed, and then the first metal oxide thin film 130a is formed, and therefore a duplicated description will be omitted.

[0069] As described above, according to the thin film transistor of the embodiment of the present invention, the electrical conductivities of the metal oxide thin films 130a, 130b, and 130c included in the active layer 130 are adjusted to be different from each other, thereby enabling the thin film transistor to operate at high speed and have improved stability.

[0070] That is, the mobility can be improved by adjusting the components and thickness of the first metal oxide thin film 130a, which forms the main charge transport path between the gate electrode 110 and the source and drain electrodes 140, and the stability of the device can be improved by adjusting the components and thicknesses of the second metal oxide thin film 130b, which forms the interface between the gate insulating film 120 and the first metal oxide thin film 130a, and the third metal oxide thin film 130c, which forms the interface between the first metal oxide thin film 130a and the source and drain electrodes 140.

[0071] Although the preferred embodiment of the present invention has been described and illustrated using specific terms, these terms are merely for the purpose of clearly describing the present invention, and it is clear that the embodiments of the present invention and the described terms can be modified and changed in various ways without departing from the technical spirit and scope of the claims. These modified embodiments should not be understood separately from the spirit and scope of the present invention, but should be considered to belong to the scope of the claims of the present invention.

Claims

1. A thin film transistor comprising an active layer formed between a gate insulating film and source and drain electrodes, The active layer is a first metal oxide thin film; a second metal oxide thin film disposed between the first metal oxide thin film and a gate insulating film and having a lower electrical conductivity than the first metal oxide thin film; a third metal oxide thin film disposed between the first metal oxide thin film and the source and drain electrodes, the third metal oxide thin film having a lower electrical conductivity than the first metal oxide thin film; Equipped with The first metal oxide thin film is formed of an oxide of a first metal material including indium (In) and zinc (Zn); The second metal oxide thin film is formed of an oxide of a second metal material including indium (In), gallium (Ga), and zinc (Zn); The third metal oxide thin film is formed of an oxide of a third metal material including indium (In), gallium (Ga), and zinc (Zn); The third metal oxide thin film has a lower electrical conductivity than the second metal oxide thin film.

2. 2. The thin film transistor of claim 1, wherein the indium (In) content in the first metal oxide thin film is 30 at % or more and less than 80 at % with respect to the entire first metal material.

3. The gallium (Ga) in the second metal oxide thin film is contained in an amount of 30 at % or more and less than 60 at % with respect to the entire second metal substance, 2. The thin film transistor according to claim 1, wherein the third metal oxide thin film contains gallium (Ga) in an amount of 30 at % or more and less than 60 at % with respect to the entire third metal material.

4. The thin film transistor of claim 1 , wherein the amount of gallium (Ga) contained in the third metal material is greater than the amount of gallium (Ga) contained in the second metal material.

5. The first metal material further includes gallium (Ga); 3. The thin film transistor of claim 2, wherein the gallium (Ga) in the first metal oxide thin film is contained in an amount of less than 30 at % based on the total amount of the first metal material.

6. A thin film transistor comprising an active layer formed between a gate insulating film and source and drain electrodes, The active layer is a first metal oxide thin film; a second metal oxide thin film disposed between the first metal oxide thin film and a gate insulating film and having a lower electrical conductivity than the first metal oxide thin film; a third metal oxide thin film disposed between the first metal oxide thin film and a source and drain electrode, the third metal oxide thin film having a lower electrical conductivity than the first metal oxide thin film; Equipped with The first metal oxide thin film is formed of an oxide of a first metal material including indium (In) and zinc (Zn); The second metal oxide thin film is formed of an oxide of a second metal material including indium (In), gallium (Ga), and zinc (Zn); The third metal oxide thin film is formed of an oxide of a third metal material including indium (In), gallium (Ga), and zinc (Zn); The first metal material further includes gallium (Ga); A thin film transistor, wherein the gallium (Ga) in the first metal oxide thin film is contained in an amount of 20 at % or more and less than 60 at % with respect to the gallium (Ga) contained in the entire active layer.

7. the thickness of the second metal oxide thin film is smaller than the thickness of the first metal oxide thin film; The thin film transistor of claim 1 , wherein the third metal oxide thin film has a thickness greater than a thickness of the first metal oxide thin film.

8. The first metal oxide thin film is formed to a thickness of 100 Å or more and less than 150 Å; The second metal oxide thin film is formed to a thickness of less than 50 Å; 8. The thin film transistor according to claim 7, wherein the third metal oxide thin film is formed to a thickness of 150 Å or more and less than 200 Å.

9. the first metal oxide thin film comprises a zinc oxide (ZnO) thin film doped with a first impurity; the second metal oxide thin film comprises a zinc oxide (ZnO) thin film doped with a first impurity and a second impurity; the third metal oxide thin film comprises a zinc oxide (ZnO) thin film doped with a first impurity and a second impurity; The first impurity includes indium (In), The thin film transistor of claim 1 , wherein the second impurity includes at least one of gallium (Ga) and tin (Sn).

10. 10. The thin film transistor of claim 9, wherein the first metal oxide thin film is further doped with a second impurity.

11. A thin film transistor as described in claim 1 or claim 5, wherein the gallium (Ga) content gradually changes in the interface region between the second metal oxide thin film and the first metal oxide thin film and in the interface region between the first metal oxide thin film and the third metal oxide thin film.

12. A thin film transistor as described in claim 1 or claim 5, wherein the gallium (Ga) content has two or more non-consecutive values ​​in the interface region between the second metal oxide thin film and the first metal oxide thin film and in the interface region between the first metal oxide thin film and the third metal oxide thin film.

Citation Information

Patent Citations

  • Thin film field effect transistor

    JP2010067954A

  • Semiconductor device and method of manufacturing the same

    JP2014045173A

  • Oxide semiconductor laminated film and semiconductor device

    JP2014045178A

  • Semiconductor device and manufacturing method of the same

    JP2014057049A

  • Thin Film Transistor and the same method

    KR1020040013273A