Lithium-ion secondary battery

The lithium ion secondary battery design with optimized graphite particles and layered structure enhances lithium ion mobility, addressing the challenge of high-rate charging and discharging in all-solid batteries.

JP7593966B2Active Publication Date: 2024-12-03TOYOTA JIDOSHA KK +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022088996
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-31
Publication Date
2024-12-03
Estimated Expiration
2042-05-31

AI Technical Summary

Technical Problem

Lithium ion secondary batteries, particularly all-solid lithium ion secondary batteries, face challenges in improving charging and discharging characteristics, especially at high rates.

Method used

The battery design incorporates graphite particles with a specific crystallite size ratio of the (004) plane to the (110) plane, optimized for lithium ion diffusion, and a layered structure with solid electrolyte and active materials, enhancing lithium ion mobility.

Benefits of technology

The design results in improved charge and discharge characteristics, particularly at high rates, by increasing lithium ion diffusivity through the graphite particles and reducing electrode resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593966000003
    Figure 0007593966000003
  • Figure 0007593966000004
    Figure 0007593966000004
  • Figure 0007593966000005
    Figure 0007593966000005
Patent Text Reader

Abstract

To provide a lithium ion secondary battery that has enhanced charge and discharge characteristics.SOLUTION: The lithium ion secondary battery of the present disclosure includes: a positive electrode body layer; a separator layer; and a negative electrode body layer in this order. The negative electrode body layer contains a solid electrolyte and a negative electrode active material; and the negative electrode active material is a graphite particle in which a ratio of a crystallite size of a (004) plane to a crystallite size of a (110) plane (crystallite size of (004) plane / crystallite size of (110) plane) is 0.683 or larger, which is measured by X-ray crystal diffraction measurement with the use of a Cu-Kα ray.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to lithium-ion secondary batteries. [Background technology]

[0002] Patent Document 1 discloses a method for producing graphite powder, comprising a step of carbonizing bulk mesophase carbon, a step of graphitizing the obtained carbonized material, and a step of pulverization, wherein the bulk mesophase carbon has an anisotropic domain diameter of 1300 Å or more as determined by small-angle X-ray scattering, and the pulverization step includes carrying out at least one of high-speed pulverization and shear pulverization prior to the graphitization step.

[0003] Patent Document 2 discloses a method for measuring the X-ray diffraction patterns of a group of carbon samples, measuring the crystallite size distribution of the (102) or (104) plane, which is a plane for evaluating the a-axis and c-axis directions of the group of carbon samples, from the X-ray diffraction patterns of the group of carbon samples using a fundamental parameter method (FP method) and measuring the peak top or distribution width of the crystallite size distribution, and performing a low-temperature characteristic evaluation and / or a high-rate charge / discharge characteristic evaluation for a group of batteries produced by using, as electrode materials for each battery, carbon samples from the group of carbon samples that have different peak tops or distribution widths of the crystallite size distribution, and then calculating the low-temperature characteristic evaluation results and / or the high-rate charge / discharge characteristic evaluation results. The present invention discloses a method for evaluating carbon, comprising the steps of: deriving data showing a correlation between the peak top or distribution width of the crystallite size distribution of a group of carbon samples; measuring the peak top or distribution width of the crystallite size distribution of an evaluation carbon that corresponds to the peak top or distribution width of the crystallite size distribution of the group of carbon samples based on the data showing the correlation; and evaluating the low-temperature battery characteristics and / or high-rate charge / discharge battery characteristics of the evaluation carbon from the peak top or distribution width of the crystallite size distribution of the evaluation carbon. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-316105 A [Patent Document 2] JP 2019-83163 A Summary of the Invention [Problem to be solved by the invention]

[0005] 2. Description of the Related Art Lithium ion secondary batteries, particularly all-solid-state lithium ion secondary batteries, are required to have improved charge / discharge characteristics, particularly when charging / discharging at a high rate, that is, when rapid charging is performed.

[0006] An object of the present disclosure is to provide a lithium ion secondary battery with improved charge / discharge characteristics. [Means for solving the problem]

[0007] The present inventors have found that the above object can be achieved by the following means: Aspect 1 The positive electrode layer, the separator layer, and the negative electrode layer are arranged in this order. The negative electrode layer contains a solid electrolyte and a negative electrode active material, The negative electrode active material is graphite particles having a ratio of the crystallite size of the (004) plane to the crystallite size of the (110) plane (crystallite size of the (004) plane / crystallite size of the (110) plane) of 0.683 or more, as measured by X-ray crystal diffraction measurement using CuKα radiation. Lithium-ion secondary battery. Aspect 2 2. The lithium ion secondary battery of claim 1, wherein the graphite particles are spherical particles or scaly particles. Aspect 3 3. The lithium ion secondary battery according to aspect 1 or 2, wherein the graphite particles have a crystallite size of a (104) plane of 40 Å or less as measured by X-ray crystal diffraction measurement using CuKα radiation. Aspect 4 The lithium ion secondary battery according to any one of aspects 1 to 3, wherein the graphite particles have a ratio of integrated intensity of a (004) plane to an integrated intensity of a (110) plane of 4.0 or more, as measured by X-ray crystal diffraction measurement using CuKα radiation. Aspect 5 the negative electrode layer has a structure in which a negative electrode active material layer and a negative electrode current collector layer are laminated on each other in this order from the separator layer side, The negative electrode active material and the solid electrolyte are contained in the negative electrode active material layer. The lithium ion secondary battery according to any one of aspects 1 to 4. Aspect 6 The lithium ion secondary battery according to any one of Aspects 1 to 5, wherein the positive electrode layer has a structure in which a positive electrode active material layer and a positive electrode current collector layer are laminated on each other in this order from the separator layer side. Aspect 7 7. The lithium ion secondary battery according to any one of aspects 1 to 6, wherein the separator layer is a solid electrolyte layer. Aspect 8 8. The lithium ion secondary battery according to any one of aspects 1 to 7, wherein the solid electrolyte is a sulfide solid electrolyte. Effect of the Invention

[0008] According to the present disclosure, it is possible to provide a lithium ion secondary battery having improved charge / discharge characteristics during high-rate charging / discharging. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram showing an all-solid-state lithium-ion secondary battery 1 according to a first embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram of a graphite particle 100 contained in the all-solid-state lithium-ion secondary battery 1 according to the first embodiment of the present disclosure. [Diagram 3] FIG. 3 is a schematic diagram of a portion of a graphite particle 100 contained in an all-solid-state lithium-ion secondary battery 1 according to the first embodiment of the present disclosure. [Figure 4] FIG. 4 is a graph showing the crystallite sizes of the (104) plane of the graphite particles of Example 1 and Comparative Example 1, measured by X-ray crystal diffraction measurement using CuKα radiation. [Diagram 5] FIG. 5 is a graph showing the ratio of the crystallite size of the (004) plane to the crystallite size of the (110) plane (crystallite size of the (004) plane / crystallite size of the (110) plane) of the graphite particles of Example 1 and Comparative Example 1, as measured by X-ray crystal diffraction measurement using CuKα radiation. [Figure 6] FIG. 6 is a graph showing the integrated intensity of the (004) plane relative to the integrated intensity of the (110) plane of the graphite particles of Example 1 and Comparative Example 1, measured by X-ray crystal diffraction measurement using CuKα radiation. [Figure 7] FIG. 7 is a graph showing the charge / discharge rate characteristics of the all-solid-state lithium ion secondary batteries of Example 1 and Comparative Example 1. [Figure 8] FIG. 8 shows the equivalent circuit of the symmetric cell in AC impedance measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0011] The lithium ion secondary battery of the present disclosure has a positive electrode layer, a separator layer, and a negative electrode layer in this order. The negative electrode layer contains a solid electrolyte and a negative electrode active material. The negative electrode active material is graphite particles in which the ratio of the crystallite size of the (004) plane to the crystallite size of the (110) plane (crystallite size of the (004) plane / crystallite size of the (110) plane) measured by X-ray crystal diffraction measurement using CuKα radiation is 0.683 or more.

[0012] FIG. 1 is a schematic diagram showing an all-solid-state lithium-ion secondary battery 1 according to a first embodiment of the present disclosure.

[0013] As shown in Fig. 1, an all-solid-state lithium-ion secondary battery 1 according to the first embodiment of the present disclosure has a positive electrode layer 10, a solid electrolyte layer 20 as a separator layer, and a negative electrode layer 30, in this order. Here, the positive electrode layer 10 has a structure in which a positive electrode active material layer 12 and a positive electrode current collector layer 11 are laminated on each other, in this order from the solid electrolyte layer 20 side. In addition, the negative electrode layer 30 has a structure in which a negative electrode active material layer 32 and a negative electrode current collector layer 31 are laminated on each other, in this order from the solid electrolyte layer 20 side. The negative electrode active material and the solid electrolyte are contained in the negative electrode active material layer 32.

[0014] In general, in lithium ion secondary batteries, particularly all-solid-state lithium ion secondary batteries, there is an issue regarding improvement of high-rate charge / discharge characteristics, particularly rapid charging performance.

[0015] It is believed that the high-rate charge / discharge characteristics of all-solid-state lithium-ion secondary batteries are significantly affected by the composition of the negative electrode layer. One of the reasons for this is that, unlike liquid-based lithium-ion secondary batteries, all-solid-state lithium-ion secondary batteries do not have a solid electrolyte interphase (SEI) between the electrolyte and the negative electrode active material that allows smooth diffusion of lithium ions, but rather a high-resistance SEI formed by the reductive decomposition of the electrolyte, and there are grain boundaries where the electrolyte cannot penetrate, resulting in a decrease in the diffusibility of lithium ions.

[0016] In this regard, it is believed that the high-rate charge / discharge characteristics can be improved by improving the lithium diffusibility on the surface and inside of the negative electrode active material.

[0017] The lithium ion secondary battery of the present disclosure contains, as a negative electrode active material, graphite particles having a ratio of the crystallite size of the (004) plane to the crystallite size of the (110) plane (crystallite size of the (004) plane / crystallite size of the (110) plane) of 0.683 or more, as measured by X-ray crystal diffraction measurement using CuKα radiation.

[0018] Such graphite particles are isotropic particles, and as shown in Figures 2 and 3, the edge faces 120 of the graphite particles 100 are large, so that lithium ions can be easily inserted and removed from the edge faces 120, and the lithium diffusibility on the surface of the graphite particles 100 is improved. In addition, since there are many interfaces 130 between the crystallites 110, lithium ions can be easily inserted and removed from the interfaces 130 between the crystallites 110, and the lithium diffusibility inside the graphite particles 100 is improved. In addition, since lithium ions can move across the crystallites 110, the lithium diffusibility in the stacking direction can be improved with respect to the stacking structure of the crystal structure of the graphite particles 100.

[0019] As a result, the lithium ion secondary battery of the present disclosure has improved charge and discharge characteristics, particularly improved charge and discharge characteristics during high-rate charge and discharge.

[0020] 《Negative electrode body layer》 The negative electrode layer contains a solid electrolyte and a negative electrode active material, and may further contain a binder and / or a conductive assistant.

[0021] The negative electrode layer may have a structure in which, for example, a negative electrode active material layer and a negative electrode current collector layer are laminated on each other in this order from the separator layer side, and the negative electrode active material and the solid electrolyte may be contained in the negative electrode active material layer. The negative electrode active material layer may optionally contain a binder and a conductive assistant in addition to the negative electrode active material and the solid electrolyte.

[0022] The material used for the negative electrode current collector layer may be, but is not limited to, stainless steel (SUS), aluminum, copper, nickel, iron, titanium, carbon, etc. Among these, the material for the negative electrode current collector layer is preferably copper.

[0023] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0024] <Negative electrode active material> The negative electrode active material is graphite particles having a ratio of the crystallite size of the (004) plane to the crystallite size of the (110) plane (crystallite size of the (004) plane / crystallite size of the (110) plane) of 0.683 or more, as measured by X-ray crystal diffraction measurement using CuKα radiation.

[0025] The graphite particles can be spherical or flake-like particles.

[0026] X-ray crystal diffraction measurement using CuKα radiation may be performed, for example, using a fully automatic multipurpose horizontal X-ray diffractometer SmartLab (9 kW), using a focusing optical system, D / teX Ultra, a Cu-Kα tube, an output of 45 kV-200 mA, a continuous scan mode, a sampling interval of 0.01°, a scan speed of 1° / min, and a scan angle of 10 to 90°.

[0027] The crystallite sizes of the (004) and (110) planes can be calculated from the half-width of the peak representing the (004) or (110) plane in an X-ray diffraction spectrum obtained by X-ray crystal diffraction measurement.

[0028] More specifically, it can be calculated by the following formula, where D is the crystallite size, K is the Scherrer constant, λ is the wavelength of X-rays, B is the half-width, and θ is the Bragg angle: D = Kλ / BCosθ

[0029] The graphite particles may have a ratio of the crystallite size of the (004) plane to the crystallite size of the (110) plane (crystallite size of the (004) plane / crystallite size of the (110) plane) of 0.683 to 1.000, as measured by X-ray crystal diffraction measurement using CuKα radiation.

[0030] The crystallite size of the (004) plane / the crystallite size of the (110) plane may be 0.683 or more, 0.685 or more, 0.690 or more, or 0.700 or more, and may be 1.000 or less, 0.900 or less, 0.800 or less, 0.750 or less, or 0.700 or less.

[0031] The graphite particles may have a crystallite size of 40 Å or less in the (104) plane as measured by X-ray crystal diffraction measurement using CuKα radiation.

[0032] The crystallite size of the (104) plane may be 40 Å or less, 35 Å or less, 30 Å or less, or 25 Å or less, and may be 5 Å or more, 10 Å or more, 15 Å or more, or 20 Å or more.

[0033] The graphite particles may have a ratio of the integrated intensity of the (004) plane to the integrated intensity of the (110) plane of 4.0 or more, as measured by X-ray crystal diffraction measurement using CuKα radiation.

[0034] The ratio of the integrated intensity of the (004) plane to the integrated intensity of the (110) plane may be 4.0 or more, 4.5 or more, 5.0 or more, or 5.5 or more, and may be 8.0 or less, 7.5 or less, 7.0 or less, or 6.5 or less.

[0035] The graphite particles as the negative electrode active material of the present disclosure can be produced, for example, by the following method:

[0036] The raw ore is crushed, and graphite is recovered and classified by flotation. After that, halogen gas is sprayed onto the graphite to perform a high-purity treatment, obtaining natural flake graphite. Next, the natural flake graphite is dispersed in a high-velocity air stream, and while it is volumetrically and surface-pulverized, it is spheroidized by applying shear force to obtain natural spherical graphite. Note that when using natural flake graphite, spheroidization is not performed.

[0037] For the obtained natural flake graphite or natural spheroidized graphite, the crystallite sizes and optionally the integrated intensities of the (004) and (110) planes are obtained by X-ray crystal diffraction measurement using CuKα radiation.

[0038] A preset value of (004) plane crystallite size / (110) plane crystallite size is used as the negative electrode active material of the present disclosure.

[0039] The desired crystallite size and integrated intensity of the (004) and (110) planes can be obtained by appropriately changing the conditions of volume milling and surface milling in the milling and spheroidization of the raw ore.

[0040] <Solid electrolyte> The solid electrolyte is preferably an inorganic solid electrolyte, such as a sulfide solid electrolyte, an oxide solid electrolyte, or a nitride solid electrolyte.

[0041] Examples of sulfide solid electrolytes include, but are not limited to, sulfide-based amorphous solid electrolytes, sulfide-based crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li 2 SP 2 S 5 System (Li 7 P 3 S 11 , Li 3 P.S. 4 , Li 8 P 2 S 9 etc.), Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2 S 5 , LiI-LiBr-Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -GeS 2 (Li 13 GeP 3 S 16 , Li 10 GeP 2 S 12 etc.), LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 , Li 7-x P.S. 6-x Clx etc.; or combinations thereof, but are not limited to these.

[0042] An example of an oxide solid electrolyte is Li 7 La 3 Zr 2 O 12、 Li 7-x La 3 Zr 1-x Nb x O 12、 Li 7-3x La 3 Zr 2 Al x O 12 , Li 3x La 2 / 3-x TiO 3 , Li 1+x Al x Ti 2-x (PO 4 ) 3 , Li 1+x Al x Ge 2-x (PO 4 ) 3 , Li 3 PO 4 , or Li 3+x PO 4-x N x (LiPON), but is not limited to these.

[0043] The solid electrolyte may be a glass, a glass ceramic, or a crystalline material. The glass may be a raw material composition (e.g., Li 2 S and P 2 S 5 The glass ceramics can be obtained by subjecting a mixture of the raw material composition to an amorphous treatment. Examples of the amorphous treatment include mechanical milling. The mechanical milling may be dry mechanical milling or wet mechanical milling, with the latter being preferred. This is because the raw material composition can be prevented from adhering to the wall of a container or the like. Glass ceramics can be obtained by heat treating glass. Crystalline materials can be obtained, for example, by subjecting the raw material composition to a solid-phase reaction treatment.

[0044] The solid electrolyte is preferably in the form of particles. The solid electrolyte has an average particle size (D50) of, for example, 0.01 μm or more. On the other hand, the solid electrolyte has an average particle size (D50) of, for example, 10 μm or less, and may be 5 μm or less. The lithium ion conductivity of the solid electrolyte at 25° C. is, for example, 1×10 -4 S / cm or more, 1×10 -3 It is preferable that the viscosity is S / cm or more.

[0045] <Binder> The binder may be, for example, but is not limited to, materials such as polyvinylidene fluoride (PVdF), carboxymethyl cellulose (CMC), butadiene rubber (BR) or styrene butadiene rubber (SBR), or combinations thereof.

[0046] <Conductive assistant> The conductive assistant may be a known one, for example, a carbon material, metal particles, etc. The carbon material may be at least one selected from the group consisting of carbon black such as acetylene black or furnace black, vapor grown carbon fiber (VGCF), carbon nanotubes, and carbon nanofibers, and from the viewpoint of electronic conductivity, may be at least one selected from the group consisting of VGCF, carbon nanotubes, and carbon nanofibers. The metal particles may be nickel, copper, iron, stainless steel, etc.

[0047] <Separator layer> The separator layer may be, for example, a solid electrolyte layer.

[0048] The solid electrolyte layer may contain the above-mentioned solid electrolyte and optionally a binder and the like.

[0049] Positive electrode layer The positive electrode layer may have a structure in which a positive electrode active material layer and a positive electrode current collector layer are laminated on each other in this order from the separator layer side.

[0050] The positive electrode active material layer can contain a positive electrode active material and, optionally, a solid electrolyte, a binder, and a conductive additive.

[0051] The positive electrode active material is, for example, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganate (LiMn 2 O 4 ), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O 2 , Li 1+x Mn 2-x-y M y O 4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), or the like, but is not limited thereto.

[0052] In addition, such a positive electrode active material may be, for example, a sulfur-based active material. Here, the sulfur-based active material is an active material containing at least S element. The sulfur-based active material may or may not contain Li element. Examples of the sulfur-based active material include elemental sulfur and lithium sulfide (Li 2 S), lithium polysulfide (Li 2 S x , 2≦x≦8).

[0053] The material used for the positive electrode current collector layer may be, but is not limited to, stainless steel (SUS), aluminum, copper, nickel, iron, titanium, carbon, etc. Among these, the material for the positive electrode current collector layer is preferably aluminum.

[0054] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0055] The binder and the conductive assistant may be the same as those exemplified for the negative electrode layer. EXAMPLES

[0056] Examples 1 to 4 and Comparative Examples 1 to 3 <Manufacture of all-solid-state secondary batteries and all-solid-state symmetric cells> The shape and the crystallite size of the (004) plane / the crystallite size of the (110) plane (L) in the X-ray crystal diffraction measurement using CuKα radiation are shown in Table 1 below. 004 / L 110 ) were used to fabricate all-solid-state secondary batteries for the graphite particles of Example 1 and Comparative Example 1, and all-solid-state symmetric cells were fabricated for the graphite particles of Examples 2 to 4 and Comparative Examples 2 and 3.

[0057] [Table 1]

[0058] The all-solid-state secondary batteries and all-solid-state symmetric cells of each example were produced using nickel manganese cobalt oxide as the positive electrode active material, graphite particles shown in Table 1 as the negative electrode active material, and a sulfide solid electrolyte as the solid electrolyte.

[0059] [Procedure for fabricating all-solid-state secondary batteries] Specifically, the positive electrode active material contained in the positive electrode active material layer is Li(NiCoMn)O with an element molar ratio of Ni:Co:Mn=5:2:3. 2 (hereinafter referred to as NCM523) was used. An argyrodite-type sulfide solid electrolyte was used as the solid electrolyte contained in the positive electrode active material layer. VGCF (registered trademark) was used as the conductive assistant. A rubber-based binder was used as the binder contained in the positive electrode active material layer. NCM523, the sulfide solid electrolyte, the binder, and the conductive assistant were mixed in an organic solvent at a predetermined blending ratio, and a dispersion process was performed to prepare a positive electrode slurry. The obtained positive electrode slurry was applied onto a stainless steel foil, which is a positive electrode current collector, and a vacuum drying process was performed to evaporate the organic solvent, thereby producing a positive electrode. The weight of the positive electrode active material layer was 1 cm 2 The dose was 15.4 mg per dose.

[0060] The solid electrolyte contained in the solid electrolyte layer was the same argyrodite-type sulfide solid electrolyte as that used in the positive electrode active material layer. The weight of the solid electrolyte layer was 1 cm 2 The dose was 100 mg per dose.

[0061] The graphite particles contained in the negative electrode active material layer were those shown in Table 1, and the solid electrolyte was the same argyrodite-type sulfide solid electrolyte as that used in the positive electrode active material layer and the solid electrolyte layer, but with a different average particle size. The volumetric blending ratio of the graphite particles and the sulfide solid electrolyte to the total volume of the solid powder contained in the negative electrode active material layer was 50%:50%. The weight of the negative electrode active material layer was 1 cm 2 The dose was 12.3 mg per dose.

[0062] 1cm 2 100 mg of the above-mentioned argyrodite-type sulfide solid electrolyte powder was placed in a hollow Macor with a hole of 1 tf / cm 2 The solid electrolyte layer was primarily molded by pressing at a pressure of 1 tf / cm for 1 minute. Next, 12.3 mg of the negative electrode powder mixture having the volumetric blend ratio of 50%:50% was placed under the primarily molded solid electrolyte layer. 2 The lower negative electrode active material layer was formed by pressing at a pressure of 1000 MPa for 1 minute. Next, a layer with a cross-sectional area of ​​1 cm2 was placed on the upper side of the solid electrolyte layer. 2 The above-mentioned positive electrode, which had been punched into a circular shape, was inserted so that the density was 6 tf / cm 2 After the final molding, the mixture was pressed at a pressure of 6tf / cm for 1 minute. 2 Release the pressure and use the restraining tool to reduce it to 1.53tf / cm 2 Here, assuming that the theoretical capacity of graphite is 372 mAh / g and the specific capacity of the positive electrode using NCM523 is 162 mAh / g, the ratio of the capacity of the negative electrode active material layer to the capacity of the positive electrode active material layer (capacity of the negative electrode active material layer / capacity of the positive electrode active material layer) was 1.51.

[0063] [Procedure for fabricating all-solid-state symmetrical cell] An all-solid-state symmetrical cell is a cell in which a negative electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer are stacked from bottom to top in this order. By setting the material composition, weight, and thickness (filling rate) of the bottommost negative electrode active material layer and the topmost negative electrode active material layer to be as identical as possible, it is possible to accurately measure the ion transport resistance (Ω) by the AC impedance method.

[0064] Specifically, the solid electrolyte contained in the intermediate solid electrolyte layer was the same argyrodite-type sulfide solid electrolyte as that used in the positive electrode active material layer and solid electrolyte layer of the all-solid-state secondary battery. The weight of the solid electrolyte layer was 1 cm 2 The dose was 100 mg per dose.

[0065] The graphite particles contained in the bottom and top negative electrode active material layers were those shown in Table 1, and the solid electrolyte was the same argyrodite-type sulfide solid electrolyte as that used in the negative electrode active material layers of the all-solid-state secondary battery. The volumetric blending ratio of the graphite particles and the sulfide solid electrolyte to the total volume of the solid powder contained in the negative electrode active material layer was 50%:50%. The weight of the negative electrode active material layer was 1 cm 2 The dose was 11.4 mg per dose.

[0066] 1cm 2 100 mg of the above-mentioned argyrodite-type sulfide solid electrolyte powder was placed in a hollow Macor with a hole of 1 tf / cm 2 The solid electrolyte layer was primarily molded by pressing at a pressure of 1 tf / cm for 1 minute. Next, 11.4 mg of the negative electrode powder mixture having the volumetric blend ratio of 50%:50% was placed under the primarily molded solid electrolyte layer. 2 The bottom negative electrode active material layer was primarily molded by pressing at a pressure of 1 tf / cm for 1 minute. Next, 11.4 mg of the negative electrode powder mixture having the volumetric blend ratio of 50%:50% was placed on the top side of the solid electrolyte layer, and 2 The uppermost negative electrode active material layer was formed by pressing for 1 minute at a pressure of 6 tf / cm 2 After the final molding, the mixture was pressed at a pressure of 6tf / cm for 1 minute. 2 Release the pressure and use the restraining tool to reduce it to 1.53tf / cm 2 was detained under pressure.

[0067] X-ray crystal diffraction measurements using CuKα radiation were performed using a fully automatic, multipurpose horizontal X-ray diffractometer SmartLab (9kW) with a focusing optical system, D / teX Ultra, a Cu-Kα tube, an output of 45kV-200mA, a continuous scanning mode, a sampling interval of 0.01°, a scanning speed of 1° / min, and a scanning angle of 10° to 90°.

[0068] For reference, the crystallite size of the (004) plane, the crystallite size of the (004) plane / the crystallite size of the (110) plane, and the ratio of the integrated intensity of the (004) plane to the integrated intensity of the (110) plane in X-ray crystal diffraction measurements using CuKα radiation for the graphite particles used in Example 1 and Comparative Example 1 are shown in Figures 4 to 6.

[0069] <Evaluation of rate characteristics> The solid-state batteries of Example 1 and Comparative Example 1 were left in a thermostatic chamber at 25° C. for 8 hours, and then CC-charged at 0.17 mA with a cutoff voltage of 4.2 V at 25° C., CV-charged at 4.2 V with a cutoff current of 0.017 mA, CC-discharged at 0.17 mA with a cutoff voltage of 3.0 V at 25° C., and CC-discharged at a cutoff current of 0.017 mA to evaluate the initial characteristics. This charge and discharge was repeated a total of three times, and the third CC-CV discharge capacity was used as the cell capacity to determine the current value for the rate characteristic evaluation.

[0070] Next, the battery was CC-charged at 0.1C to 2C in 0.1C increments with a cutoff voltage of 4.2V at 25°C, and then CC-discharged at the same current value as CC-charged at a cutoff voltage of 3.0V at 25°C without CV-charging, and then CC-discharged at a cutoff current of 0.01C to evaluate the rate characteristics. The ratio (%) of the charge capacity when CC-charged from 0.1C to 2C was calculated relative to the charge capacity when CC-charged at 0.1C.

[0071] The measurement results are shown in Figure 7.

[0072] As shown in FIG. 7, in the all-solid-state secondary battery of Example 1, in which the crystallite size of the (004) plane / the crystallite size of the (110) plane was 0.693, the ratio (%) of the discharge capacity to the discharge capacity was larger than the ratio (%) of the discharge capacity to the discharge capacity in the all-solid-state secondary battery of Comparative Example 1, in which the crystallite size of the (004) plane / the crystallite size of the (110) plane was 0.641.

[0073] <AC impedance measurement> The graphite particles used in Examples 2 to 4 and Comparative Examples 2 and 3 were used as the negative electrode active material to form a negative electrode active material layer, and lithium foil was used on the positive electrode side to prepare all-solid-state symmetrical cells. An AC voltage with a voltage amplitude of 10 mV and a frequency range of 7 MHz to 100 mHz was applied between the bottom and top negative electrode active material layers of the all-solid-state symmetrical cell, and AC impedance measurement was performed using a BioLogic VMP300. The circuit constants were fitted in the equivalent circuit shown in FIG. 8, and the resistance value Wo-R of the Warburg open circuit was calculated. Since the calculated resistance value Wo-R indicates the ion transport resistance value of the two layers of the negative electrode active material layers, the bottom layer and the top layer, 1 / 2 of the resistance value Wo-R of the Warburg open circuit corresponds to the ion transport resistance (Ω) of a single layer of the negative electrode active material layer.

[0074] For each of the all-solid-state symmetrical cells, the ion transport resistance (Ω) was evaluated by AC impedance measurement (at 25° C. and 60° C.).

[0075] The results are shown in Table 2.

[0076] [Table 2]

[0077] As shown in Table 2, in Examples 2 to 4, in which the (004) plane crystallite size / (110) plane crystallite size was 0.695, 0.691, and 0.683, respectively, the ion transport resistance measured by AC impedance was lower than that in Comparative Examples 2 and 3, in which the (004) plane crystallite size / (110) plane crystallite size was 0.596 and 0.593, respectively.

[0078] Thus, in the all-solid-state symmetric cells of Examples 2 to 4 in which isotropic graphite particles were used as the negative electrode active material, a reduction in electrode resistance was confirmed, and it can be said that the diffusibility of lithium ions in the negative electrode is extremely good. [Explanation of symbols]

[0079] 1. All-solid-state lithium-ion secondary battery 10 Positive electrode layer 11 Positive electrode current collector layer 12 Cathode active material layer 20 Solid electrolyte layer 30 Negative electrode body layer 31 Negative electrode current collector layer 32 Negative electrode active material layer 100 graphite particles 110 Crystal 120 Edge Face 130 Interface

Claims

1. The positive electrode layer, the separator layer, and the negative electrode layer are arranged in this order. The negative electrode layer contains a solid electrolyte and a negative electrode active material, the negative electrode active material is graphite particles having a ratio of a crystallite size of a (004) plane to a crystallite size of a (110) plane (crystallite size of the (004) plane / crystallite size of the (110) plane) of 0.683 or more, as measured by X-ray crystal diffraction measurement using CuKα radiation; the separator layer is a solid electrolyte layer; and The solid electrolyte is a sulfide solid electrolyte. Lithium-ion secondary battery.

2. The lithium ion secondary battery according to claim 1 , wherein the graphite particles are spherical particles or scaly particles.

3. 2. The lithium ion secondary battery according to claim 1, wherein the graphite particles have a crystallite size of a (104) plane of 40 Å or less as measured by X-ray crystal diffraction measurement using CuKα radiation.

4. 2. The lithium ion secondary battery according to claim 1, wherein the graphite particles have a ratio of integrated intensity of a (004) plane to an integrated intensity of a (110) plane of 4.0 or more as measured by X-ray crystal diffraction measurement using CuKα radiation.

5. 4. The lithium ion secondary battery according to claim 3, wherein the graphite particles have a ratio of integrated intensity of a (004) plane to an integrated intensity of a (110) plane of 4.0 or more as measured by X-ray crystal diffraction measurement using CuKα radiation.

6. The lithium ion secondary battery of claim 1, wherein the crystallite size of the (004) plane / the crystallite size of the (110) plane is 0.700 or less.

7. the negative electrode layer has a structure in which a negative electrode active material layer and a negative electrode current collector layer are laminated on each other in this order from the separator layer side, The negative electrode active material and the solid electrolyte are contained in the negative electrode active material layer. The lithium ion secondary battery according to any one of claims 1 to 6.

8. The lithium ion secondary battery according to any one of claims 1 to 6, wherein the positive electrode layer has a structure in which a positive electrode active material layer and a positive electrode current collector layer are laminated on each other in this order from the separator layer side.

Citation Information

Patent Citations

  • Negative active material for lithium secondary battery and lithium secondary battery using this

    JP2000133267A

  • Manufacturing method of graphite powder

    JP2001316105A

  • Negative electrode and battery using same

    JP2007179955A

  • Negative electrode mix for lithium battery, negative electrode for lithium battery, lithium battery, device, and manufacturing method of negative electrode mix for lithium battery

    JP2009283344A

  • Method for evaluating carbon

    JP2019083163A