Ceramics, atomizing cores and atomizers

A ceramic substrate with a bismuth-based oxide modification layer addresses the issues of narrow firing range and poor thermal shock resistance, improving bonding strength and thermal stability to enhance atomization performance and durability in atomizers.

JP7594043B2Active Publication Date: 2024-12-03SHENZHEN SMOORE TECH LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023067871
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-04-18
Publication Date
2024-12-03
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Conventional ceramic surface modification layers in atomizers suffer from a narrow firing range and poor thermal shock resistance, leading to potential cracking and reduced performance.

Method used

A ceramic substrate with a modification layer containing bismuth-based oxide and other components, such as sodium, magnesium, aluminum, silicon, potassium, calcium, titanium, zinc, zirconium, and barium, is used to improve bonding strength and thermal stability, replacing lead-containing oxides to enhance thermal shock resistance and expand the firing range.

Benefits of technology

The modified ceramic substrate with a bismuth-based oxide layer reduces the melting temperature, lowers the thermal expansion coefficient, and improves thermal shock resistance, ensuring better bonding and preventing cracking, thereby enhancing the atomization performance and durability of the atomizer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594043000001
    Figure 0007594043000001
  • Figure 0007594043000002
    Figure 0007594043000002
  • Figure 0007594043000003
    Figure 0007594043000003
Patent Text Reader

Abstract

To disclose a ceramic, an atomizing core and an atomizer improving thermal shock resistance so as to improve performance of the atomization core and performance of the atomizer.SOLUTION: A ceramic 10 includes a ceramic substrate 11 and a modification layer 12 disposed on a surface of the ceramic substrate 11. The modification layer 12 contains a bismuth-based oxide and other components. The modification layer 12 is installed on a surface of the ceramic substrate 11, the compositions of the modification layer 12 are optimized, the bismuth-based oxide is added into the modification layer 12, and a lead-containing oxide in the prior art is replaced with the bismuth-based oxide, so that the modification layer 12 containing the bismuth-based oxide exhibits excellent performance. Accordingly, this configuration can lower a melting temperature of the modification layer 12 to expand a firing range, lower a thermal expansion coefficient of the modification layer 12, and improve thermal shock resistance and tensile deformation resistance so as to improve performance of the atomization core, and further improve performance of the atomizer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the ceramic material technology field and the atomizer technology field, in particular to ceramics, atomizing cores and atomizers. [Background technology]

[0002] Generally, an electronic atomizer is composed of an atomizer and a power module, the power module supplies power to the atomizer, and the atomizer heats and atomizes an aerosol-generating substrate in an electrically-conductive state to generate an aerosol, which is inhaled by a user. The atomization core is one of the core components of an electronic atomizer, and its characteristics determine the atomization effect and user experience of the electronic atomizer.

[0003] A general-purpose atomizing core is a ceramic substrate, and a heating element is provided on the ceramic substrate to heat the aerosol-generating substrate. Usually, a modification layer is provided on the surface of the ceramic substrate to enhance the bonding strength between the heating element and the ceramic substrate. However, the conventional modification layer has a narrow sintering range and poor thermal shock resistance. Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention provides a ceramic, atomizing core and atomizer that mainly solves the problem of poor thermal shock resistance due to the narrow firing range of the modified layer on the ceramic surface in the prior art. [Means for solving the problem]

[0005] In order to solve the above technical problems, the present invention provides a ceramic according to a first technical solution, which includes a ceramic substrate and a modification layer formed on the surface of the ceramic substrate, the modification layer including a bismuth-based oxide and other components.

[0006] The ceramic substrate is made of porous ceramics.

[0007] The bismuth-based oxide includes bismuth oxide.

[0008] The mass percentage of the bismuth element in the modification layer is 50% to 80%.

[0009] The other components include at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, calcium, titanium, zinc, zirconium, and barium.

[0010] The other components include zinc element, and the mass percentage of the zinc element in the modification layer is 5% to 7%.

[0011] Moreover, the modification layer does not contain lead element.

[0012] In addition, the modified layer has a continuous porous structure.

[0013] In order to solve the above technical problems, the present invention provides a second technical solution for an atomizing core, which includes a ceramic and a heat-generating layer. The ceramic is any of the ceramics described above. The heat-generating layer is laminated on the surface of the modified layer that is away from the ceramic substrate.

[0014] In order to solve the above technical problems, the present invention provides a third technical solution of an atomizer, which includes a reservoir chamber for storing an aerosol-generating substrate and the above-mentioned atomizing core, which absorbs, heats and atomizes the aerosol-generating substrate in the reservoir chamber.

[0015] The present invention has the following remarkable effects. Different from the prior art, the present invention discloses a ceramic, an atomizing core and an atomizer. The ceramic includes a ceramic substrate and a modification layer provided on the surface of the ceramic substrate. The modification layer includes bismuth-based oxide and other components. The modification layer is provided on the surface of the ceramic substrate, and the composition of the modification layer is optimized, and bismuth-based oxide is added into the modification layer, replacing the lead-containing oxide of the prior art with bismuth-based oxide, so that the modification layer containing bismuth-based oxide has excellent performance, thereby lowering the melting temperature of the modification layer and widening the firing range, reducing the thermal expansion coefficient of the modification layer and improving the thermal shock resistance, thereby improving the performance of the atomizing core and further improving the performance of the atomizer. [Brief description of the drawings]

[0016] In order to more clearly explain the embodiments of the present invention or the technical solutions of the prior art, the drawings necessary in the description of the embodiments will be briefly described below. However, the drawings described below are only some of the embodiments of the present invention, and it is obvious that a person skilled in the art can conceive of other drawings based on these drawings without any creative effort. [Figure 1] FIG. 1 is a diagram showing a configuration of an embodiment of a ceramic according to the present invention. [Diagram 2] FIG. 1 is a diagram showing the configuration of an embodiment of an electronic atomizer according to the present invention. [Diagram 3] FIG. 3 is a diagram showing the configuration of an atomizer in the electronic atomizer shown in FIG. 2. [Figure 4] FIG. 4 is a diagram showing the configuration of an atomizing core in the atomizer shown in FIG. [Diagram 5] FIG. 5 is a top view showing the configuration of the atomizing core of FIG. 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in more detail below with reference to the drawings and examples. The following examples are only for explaining the present invention, and do not limit the scope of the present invention. Similarly, the following examples are only some of the examples of the present invention, not all of the examples. All other examples obtained by those skilled in the art based on the examples of the present invention without creative work should be included in the scope of protection of the present invention.

[0018] The terms "first", "second" and "third" in the present invention are used for descriptive purposes only and should not be construed as indicating or suggesting relative importance or implying the number of technical features shown. Thus, features defined by "first", "second" and "third" can include at least one feature, either explicitly or implicitly. In the present description, "plurality" means at least two, e.g., two, three, etc., unless otherwise specifically defined. Also, the terms "comprise" and "have" and any variations thereof are intended to be non-exclusively inclusive. For example, a process, method, system, product or apparatus that includes a series of steps or units is not limited to the listed steps or units, and may optionally further include unlisted steps or units, or may further include other steps or units inherent to these processes, methods, products or apparatus.

[0019] In this specification, the term "embodiment" means that a particular feature, structure, or characteristic described in conjunction with the embodiment is included in at least one embodiment of the present invention. The appearance of the word in each location in this specification does not necessarily mean that all of the words refer to the same embodiment, nor are they mutually exclusive independent or alternative embodiments of other embodiments. Those skilled in the art will understand, both explicitly and implicitly, that the embodiments described in this specification may be combined with other embodiments.

[0020] Generally, the modification layer on the surface of conventional ceramics uses a glaze containing lead element, which has problems such as a narrow firing range and poor thermal shock resistance, etc. Therefore, the present invention provides a ceramic 10, which is specifically described as follows.

[0021] Please refer to Fig. 1. Fig. 1 is a diagram showing the structure of one embodiment of the ceramic according to the present invention.

[0022] The present invention provides a ceramic 10. As shown in FIG. 1, the ceramic 10 includes a ceramic substrate 11 and a modification layer 12 disposed on the surface of the ceramic substrate 11. The modification layer 12 includes bismuth-based oxide and other components. The modification layer 12 is disposed on the surface of the ceramic substrate 11, and the composition of the modification layer 12 is optimized, and bismuth-based oxide is added into the modification layer 12, replacing the lead-containing oxide of the prior art with bismuth-based oxide. The modification layer 12 containing bismuth-based oxide has excellent performance, so that the melting temperature and thermal expansion coefficient of the modification layer 12 are reduced, the sintering range of the modification layer 12 is expanded, and the thermal shock resistance and tensile deformation resistance are improved. In addition, the modification layer 12 disposed on the surface of the ceramic substrate 11 can effectively improve the strength and thermal stability of the ceramic 10, prevent the ceramic substrate 11 from being eroded by liquids, gases, etc., and modify the surface of the ceramic substrate 11, thereby increasing the surface flatness of the ceramic substrate 11.

[0023] Specifically, the bismuth-based oxide in the modified layer 12 is mainly bismuth oxide. Bismuth oxide has more stable performance and both melting point and boiling point are lower than lead oxide, and compared to the conventional modified layer containing lead-containing oxide, it can lower the melting temperature of the entire modified layer 12, widen the firing range, and lower the sintering temperature of the modified layer 12. In addition, the thermal expansion coefficient of bismuth oxide is lower than that of lead oxide, and compared to the conventional modified layer containing lead-containing oxide, it can effectively lower the thermal expansion coefficient of the entire modified layer 12, improve the thermal shock resistance and tensile deformation resistance of the modified layer 12, and better bond the modified layer 12 to the ceramic surface, thereby suppressing the occurrence of the problem of cracks occurring in the modified layer 12 on the ceramic surface.

[0024] The mass percentage of the bismuth element in the modified layer 12 is 50% to 80%. If the content of the bismuth element in the modified layer 12 is too low, the performance of the modified layer 12, such as the thermal expansion coefficient and melting temperature, is not effectively reduced, and the performance of the modified layer 12, such as the firing range, thermal shock resistance, and tensile deformation resistance, is not favorably affected, and the performance of the modified layer 12 is adversely affected.

[0025] Other components in the modification layer 12 include one or more of the elements sodium, magnesium, aluminum, silicon, potassium, calcium, titanium, zinc, zirconium, and barium.

[0026] Preferably, the other components in the modified layer 2 include zinc element, and the mass percentage of zinc element in the modified layer 12 is 5% to 7%. The zinc element in the modified layer 12 exists in the form of an oxide. Zinc oxide, as a flux for the modified layer 12, lowers the sintering temperature of the modified layer 12 and increases the tensile deformation resistance of the modified layer 12, further reduces the thermal expansion coefficient of the entire modified layer 12, improves thermal shock resistance, and increases the thermal compatibility between the modified layer 12 and the ceramic surface, making it less likely to crack during subsequent use.

[0027] In this embodiment, the composition of the modification layer 12 includes the elements oxygen, sodium, magnesium, aluminum, silicon, potassium, calcium, zinc, bismuth, titanium, zirconium, and barium. Specifically, the mass percentage of the oxygen element in the modified layer 12 is 21.94 wt%, the mass percentage of the sodium element in the modified layer 12 is 1.04 wt%, the mass percentage of the magnesium element in the modified layer 12 is 0.14 wt%, the mass percentage of the aluminum element in the modified layer 12 is 0.59 wt%, the mass percentage of the silicon element in the modified layer 12 is 12.79 wt%, the mass percentage of the potassium element in the modified layer 12 is 1.17 wt%, the mass percentage of the calcium element in the modified layer 12 is 0.43 wt%, the mass percentage of the zinc element in the modified layer 12 is 6.185 wt%, the mass percentage of the bismuth element in the modified layer 12 is 55.715 wt%, and the elements titanium, zirconium and barium are trace elements in the modified layer 12 and their content in the modified layer 12 is small, and their mass percentage relative to the modified layer 12 is less than 0.009%.

[0028] The ceramic substrate 11 has a porous structure. Preferably, the ceramic substrate 11 is directly manufactured by selecting a porous ceramic material. For example, the porous ceramic may be a diatomaceous earth-based porous ceramic, an alumina-based porous ceramic, a mullite-based porous ceramic, a composite porous ceramic made of at least two of these materials, or a composite porous ceramic made of alumina and mullite, or may be a porous ceramic substrate 11 formed by selecting a dense ceramic material and drilling holes, or may be specially designed as necessary.

[0029] The porosity of the porous ceramic material may be 30% to 70%, specifically, 30%, 35%, 50%, or 70%. The pore size of the porous ceramic material is 200 nm to 200 μm.

[0030] The ceramic base 11 may have any shape, such as a cylindrical shape, a circular shape, a rectangular parallelepiped shape, a cube, or a prismatic shape, and may be set to any size, but is not limited thereto. In this embodiment, the ceramic base 11 has a rectangular parallelepiped shape, as shown in FIG.

[0031] Specifically, the modification layer 12 can be manufactured on the surface of the ceramic substrate 11 by a deposition process such as physical vapor deposition or chemical vapor deposition. For example, the modification layer 12 may be manufactured by a process technique such as sputtering, vapor deposition, or atomic layer deposition, and the surface of the ceramic substrate 11 may be formed into a continuous porous structure or a continuous network structure to modify the ceramic substrate 11. Alternatively, a raw material slurry containing the modification layer 12 components may be directly applied to the surface of the ceramic substrate 11. Examples of application methods include, but are not limited to, various application methods such as spraying, printing application, transfer, and silk printing. After the modification layer 12 is manufactured on the surface of the ceramic substrate 11, the ceramic substrate 11 and the modification layer 12 are subjected to a sintering process. The sintering temperature is 500°C to 900°C, and by sintering at this sintering temperature, a ceramic 10 with excellent performance can finally be obtained.

[0032] The thickness of the modified layer 12 is 50 μm to 300 μm. In order to form a continuous porous structure of the modified layer 12, the thickness of the modified layer 12 needs to be close to or smaller than the pore size of the porous ceramics. The thickness of the modified layer 12 is preferably 50 μm to 200 μm. The modified layer 12 of this thickness can form a relatively flat surface on the porous ceramic substrate 11, and can ensure the continuous porous structure and ensure the liquid conductivity of the porous ceramics.

[0033] In this embodiment, a modification layer 12 containing bismuth oxide is installed on the surface of the ceramic substrate 11, and the toxic lead element is replaced with bismuth element to ensure the safety of the modification layer 12. At the same time, the components such as bismuth oxide and zinc oxide in the modification layer 12 can reduce the sintering temperature of the modification layer 12 and prevent damage to the ceramic substrate 11 during sintering if the sintering temperature is too high. The thermal expansion coefficient of the modification layer 12 can be effectively reduced and the thermal shock resistance can be improved, thereby improving the tensile deformation resistance and thermal stability of the ceramic 10, and the thermal compatibility between the modification layer 12 and the ceramic substrate 11 can be further improved to make the bonding closer, and the performance of the ceramic 10 can be further enhanced.

[0034] The present invention further provides a method for producing the above ceramic 10. The method specifically includes the following steps.

[0035] S1: Obtain a ceramic substrate.

[0036] Specifically, depending on the needs of a particular design, a porous ceramic material may be selected to directly manufacture the ceramic base 11, or a dense ceramic material may be selected and holes may be drilled to manufacture the ceramic base 11 having a porous structure. In this embodiment, a porous ceramic material is selected to manufacture the ceramic base 11, and the shape of the manufactured ceramic base 11 is a rectangular parallelepiped.

[0037] S2: A modified layer is formed on the surface of the ceramic substrate.

[0038] Specifically, the modification layer 12 is manufactured and formed on the surface of the rectangular parallelepiped ceramic substrate 11 manufactured by the above steps by a deposition process or coating method. Preferably, a deposition process such as physical vapor deposition or chemical vapor deposition may be selected, and the modification layer 12 may be manufactured on the surface of the ceramic substrate 11 by a process technique such as sputtering, vapor deposition, or atomic layer deposition. The modification layer 12 may also be applied to the surface of the ceramic substrate 11 by various coating methods such as spraying, printing coating, transfer, and silk printing. According to the above process method, the modification layer 12 having a continuous structure is formed on the surface of the ceramic substrate 11. The modification layer 12 manufactured on the surface of the ceramic substrate 11 includes bismuth-based oxide and other components. The bismuth-based oxide is mainly bismuth oxide, and the other components include one or more elements of sodium, magnesium, aluminum, silicon, potassium, calcium, titanium, zinc, zirconium, and barium, but may be specially designed as needed. As the raw material of the modified layer 12, oxides, salts, simple substances, etc. containing the above-mentioned components are usually used, and specifically, the raw material of the modified layer 12 may be selected depending on the process selected. When the coating process is selected, for example, salts or oxides containing one or more elements of bismuth oxide, sodium, magnesium, aluminum, silicon, potassium, calcium, titanium, zinc, zirconium, and barium may be selected as bismuth-based oxides. For example, bismuth oxide, zirconia, zinc oxide, magnesium oxide, calcium oxide, silicon fine powder, barium oxide, sodium carbonate, potassium carbonate, calcium carbonate, sodium silicate, potassium sodium tartrate, etc. may be used. In addition, the above-mentioned raw materials are mixed to prepare a raw material slurry, which is then applied to the ceramic substrate 11.

[0039] S3: The ceramic substrate and the modification layer are subjected to a sintering process.

[0040] Specifically, the ceramic base 11 and the modified layer 12 manufactured in the above steps are subjected to a sintering process at a sintering temperature of 500°C to 900°C, and after the sintering process, a ceramic 10 having excellent performance and excellent bonding between the modified layer 12 and the ceramic base 11 is finally obtained.

[0041] Please refer to Figures 2 and 3. Figure 2 is a diagram showing the configuration of one embodiment of an electronic atomizer according to the present invention, and Figure 3 is a diagram showing the configuration of the atomizer in the electronic atomizer shown in Figure 2.

[0042] 2, the present invention provides an electronic atomizer 300. The electronic atomizer 300 includes an atomizer 100 and a power module 200. The power module 200 provides energy to the atomizer 100. When the atomizer 100 is in an energized state, it heats and atomizes an aerosol-generating substrate to generate an aerosol, which is inhaled by a user.

[0043] Preferably, the atomizer 100 and the power module 200 in the electronic atomizer 300 may be of integral construction or may be detachably coupled, but may also be specially designed as required.

[0044] As shown in Fig. 3, the atomizer 100 includes a liquid storage chamber 90, an exhaust pipe 30, an atomizing core 20, and an atomizing chamber 40 formed in the atomizer 100. The liquid storage chamber 90 stores an aerosol-generating base material, and the atomizing core 20 absorbs the aerosol-generating base material in the liquid storage chamber 90 and heats and atomizes the absorbed aerosol-generating base material to finally generate an aerosol. The atomized aerosol flows through the exhaust pipe 30 in the atomizing chamber 40 together with the external airflow, and finally flows out of the atomizer 100 to be inhaled by the user.

[0045] Please refer to Fig. 4 and Fig. 5. Fig. 4 is a diagram showing the configuration of the atomizing core in the atomizer shown in Fig. 3, and Fig. 5 is a top view showing the configuration of the atomizing core in Fig. 4.

[0046] Refer to FIG. 4. The atomizing core 20 includes a ceramic 10 and a heat generating layer 21. The ceramic 10 is the ceramic 10 according to the present invention, and includes a ceramic base 11 and a modified layer 12. The modified layer 12 is disposed on the surface of the ceramic base 11. The heat generating layer 21 is disposed on the surface of the modified layer 12 that is away from the ceramic base 11. The performance of the ceramic-based atomizing core 20 is often affected by the quality of the ceramic base 11, and it is necessary to modify the surface of the ceramic base 11. The modified layer 12 exerts a modifying function on the surface of the ceramic base 11, forms the surface of the ceramic base 11 into a continuous porous structure, and contributes to the uniform heat generation and liquid induction of the atomizing core 20. In addition, the heat generating layer 21 can be better bonded to the ceramic base 11 by the modified layer 12, which can increase the heat generation efficiency of the atomizing core 20 and further increase the atomization efficiency of the atomizing core 20.

[0047] In this embodiment, the compositional components of the modified layer 12 formed on the surface of the ceramic base 11 and the mass percentages of each component in the modified layer 12 may be determined by referring to the above description, and therefore detailed description thereof will be omitted here.

[0048] The inventors of the present invention conducted multiple tests to test the thermal shock resistance of the modified layer 12 on the surface of the ceramic substrate 11 in the atomizing core 20. Specifically, multiple tests were conducted by changing the mass percentage of the bismuth element in the modified layer 12, and the thermal shock resistance of the modified layer 12 was evaluated by detecting whether the modified layer 12 on the surface of the ceramic substrate 11 had cracks.

[0049] During normal use of the electronic atomizer 300, the temperature range of the atomizing core 20 is 50°C to 350°C. To test the thermal shock resistance of the modified layer 12 in the atomizing core 20, the present inventors conducted limit tests on the modified layer 12 at temperatures of 400°C to 800°C.

[0050] The inventors of the present invention conducted seven tests, namely Test 1, Test 2, Test 3, . . . Test 7. In the seven tests, the mass percentages of the bismuth element in the modification layer 12 were different from one another.

[0051] Specifically, in Test 1, the mass percentage of the bismuth element in the modification layer 12 was 50 wt%, and the sintering temperature of the ceramic base 11 on whose surface the modification layer 12 was formed was 500°C. In Test 2, the mass percentage of the bismuth element in the modification layer 12 was 55 wt%, and the sintering temperature of the ceramic base 11 on whose surface the modification layer 12 was formed was 550°C. In Test 3, the mass percentage of the bismuth element in the modification layer 12 was 60 wt%, and the sintering temperature of the ceramic base 11 on whose surface the modification layer 12 was formed was 600°C. In Test 4, the mass percentage of the bismuth element in the modification layer 12 was 65 wt%, and the sintering temperature of the ceramic base 11 on whose surface the modification layer 12 was formed was 600°C. In Test 5, the mass percentage of the bismuth element in the modification layer 12 was 68 wt%, and the sintering temperature of the ceramic base 11 on whose surface the modification layer 12 was formed was 600°C. In Test 6, the mass percentage of the bismuth element in the modification layer 12 was 70 wt%, and the sintering temperature of the ceramic base 11 on whose surface the modification layer 12 was formed was 650°C. In Test 7, the mass percentage of the bismuth element in the modification layer 12 was 80 wt%, and the sintering temperature of the ceramic base 11 on whose surface the modification layer 12 was formed was 700°C.

[0052] In the seven tests described above, the thermal shock test was performed on the modification layer 12 at a limit temperature of 400° C. to 800° C. The test results obtained through detection in the seven tests showed that no cracks were found in the modification layer 12 on the surface of the ceramic substrate 11, that is, the thermal shock resistance of the modification layer 12 was excellent in all seven different tests.

[0053] The inventors have analyzed and studied the test results of the above tests, and have found the following from the test results obtained through multiple tests. When the mass percentage of the bismuth element in the modification layer 12 is 50%-80%, and the sintering temperature of the ceramic base 11 on which the modification layer 12 is installed is 500°C-900°C, the modification layer 12 has excellent thermal shock resistance, the thermal matching between the modification layer 12 and the surface of the ceramic base 11 is higher, the bonding is better, the thermal expansion coefficient of the modification layer 12 is lower, and the tensile deformation resistance is also better. During the use of the atomizing core 20, the modification layer 12 is less likely to crack, and the problem of the modification layer 12 cracking and the heat generation layer 21 on the surface of the modification layer 12 breaking, which affects the atomizing performance and service life of the atomizing core 20, can be suppressed. This ensures the use performance and service life of the atomizing core 20 and improves the atomizing performance of the electronic atomizer 300.

[0054] The ceramic substrate 11 has a porous structure. Therefore, the modified layer 12 manufactured on the surface of the ceramic substrate 11 by a process such as physical vapor deposition, chemical vapor deposition, or a coating method has a continuous porous structure or a continuous network structure, and such a structure does not affect the liquid supply effect of the ceramic substrate 11 to the heat generating layer 21. In addition, the continuous porous structure or the continuous network structure contributes to uniform heat generation and liquid induction of the atomizing core 20, and allows the aerosol generating base material stored in the liquid storage chamber 90 to enter the atomizing core 20 more uniformly, and is heated and atomized by the heat generating layer 21 in the atomizing core 20 to generate an aerosol, thereby improving the atomization performance of the atomizing core 20 and improving the user's comfort.

[0055] The shape and size of the ceramic substrate 11 are not limited. In this embodiment, the ceramic substrate 11 is manufactured from a porous ceramic material. The porous ceramic has voids and has the functions of liquid induction and liquid storage, and the aerosol-generating substrate in the liquid storage chamber 90 is absorbed by the ceramic substrate 11, and then penetrates into the atomization surface to be heated and atomized. In addition, the porous ceramic has stable chemical performance and does not chemically react with the aerosol-generating substrate. Furthermore, the porous ceramic is resistant to high temperatures and does not deform due to excessive heating during atomization. The porous ceramic is an insulator and is electrically connected to the heating layer 21, so that a short circuit does not occur and the atomization core 20 does not break down. Furthermore, the porous ceramic is easy to manufacture and low cost. As shown in FIG. 4, the ceramic substrate 11 is a rectangular parallelepiped porous ceramic.

[0056] In some embodiments, the porosity of the porous ceramic may be 30% to 70%. The porosity refers to the ratio of the total volume of the micropores in the porous medium to the total volume of the porous medium. The magnitude of the porosity can be adjusted by the composition of the aerosol-generating substrate. For example, when the viscosity of the aerosol-generating substrate is relatively high, a high porosity is selected to ensure the liquid guiding effect.

[0057] In some other embodiments, the porosity of the porous ceramic is 50% to 60%. The porosity of the porous ceramic is 50% to 60%, which ensures high liquid induction efficiency of the porous ceramic, prevents the aerosol-generating substrate from being clogged and drying and burning, and improves the atomization effect of the atomizer 100. Meanwhile, the porosity of the porous ceramic is too large, which makes the liquid induction too fast and makes it difficult to block the liquid, which greatly increases the possibility of liquid leakage and affects the performance of the atomizer 100.

[0058] The heat generating layer 21 is disposed on the surface of the modification layer 12 away from the ceramic substrate 11, and is made of a metal or alloy material. When energized, the heat generating layer 21 generates heat to heat and atomize the aerosol-generating substrate. Preferably, the heat generating layer 21 may be at least one of a heat generating film, a heat generating coating layer, a heat generating wire, a heat generating piece, or a heat generating net. In this embodiment, the heat generating layer 21 has a porous heat generating film structure. The porous structure of the heat generating layer 21 allows the liquid aerosol-generating substrate to efficiently penetrate the heat generating layer 21, improving the liquid induction and heat conduction efficiency of the heat generating layer 21 and increasing the atomization efficiency of the atomization core 20.

[0059] The material of the heating layer 21 may be selected from materials that provide stable bonding with the modification layer 12. For example, the heating layer 21 may be made of a material such as titanium, zirconium, a titanium-aluminum alloy, a titanium-zirconium alloy, a titanium-molybdenum alloy, a titanium-niobium alloy, an iron-aluminum alloy, a tantalum-aluminum alloy, or stainless steel.

[0060] Titanium and zirconium have the following characteristics. Titanium and zirconium are metals with excellent biocompatibility, and titanium in particular is a metal element with high biocompatibility and is safer. Titanium and zirconium have a relatively high resistivity among metal materials, and after alloying at a certain ratio at room temperature, they have three times the original resistivity, making them more suitable as materials for the heating layer 21. Titanium and zirconium have a small thermal expansion coefficient, and the thermal expansion coefficient after alloying is smaller, and the thermal matching with the modification layer 12 is better. After alloying at a certain ratio, the melting point of the alloy is lower, and the film formation property of the magnetron sputtering plating film is better. After the metal plating film, electron microscope analysis shows that the fine particles are spherical, and the particles are combined to form a fine shape similar to cauliflower. However, electron microscope analysis shows that the film formed by the titanium-zirconium alloy has fine particles in a flake shape, no grain boundaries between the particles, and excellent continuity. Both titanium and zirconium have excellent plasticity and elongation, and the thermal cycle resistance and current impact property of the titanium-zirconium alloy film are superior due to the above-mentioned characteristics of titanium and zirconium. In this embodiment, the heating layer 21 is made of a titanium-zirconium alloy material.

[0061] Preferably, the heat generating layer 21 can be produced on the surface of the modified layer 12 facing away from the ceramic substrate 11 by a process such as physical vapor deposition or chemical vapor deposition, for example by a process technique such as sputtering, evaporation, or atomic layer deposition.

[0062] In this embodiment, the titanium-zirconium alloy film itself made from the titanium-zirconium alloy is a locally dense film, but since the modification layer 12 has a porous structure, the titanium-zirconium alloy film formed on the surface of the modification layer 12 also has a porous continuous structure, and the pore size distribution of the titanium-zirconium alloy film is slightly smaller than the pore size of the micropores on the surface of the modification layer 12.

[0063] Please refer to FIG. 4. In this embodiment, the atomizing core 20 further includes two electrodes 22. The two electrodes 22 are electrically connected to the power supply module 200 in the electronic atomizer 300, respectively, to supply power to the heat generating layer 21 of the atomizing core 20, so that the heat generating layer 21 generates heat in a current-carrying state, and the aerosol-generating base material absorbed in the ceramic substrate 11 is heated and atomized to generate aerosol. Specifically, as shown in FIG. 4 and FIG. 5, the two electrodes 22 are both installed on the surface of the heat generating layer 21 away from the ceramic substrate 11. In addition, the two electrodes 22 are installed at a distance from each other, so that the power supply module 200 can be easily electrically connected to the electrodes 22 to supply power to the atomizing core 20.

[0064] The present invention is different from the prior art and discloses a ceramic, an atomizing core and an atomizer. The ceramic includes a ceramic substrate and a modification layer provided on the surface of the ceramic substrate. The modification layer includes bismuth-based oxide and other components. The modification layer is provided on the surface of the ceramic substrate, and the composition of the modification layer is optimized, and bismuth-based oxide is added into the modification layer, replacing the lead-containing oxide of the prior art with bismuth-based oxide, so that the modification layer containing bismuth-based oxide has excellent performance, thereby lowering the melting temperature of the modification layer and widening the firing range, reducing the thermal expansion coefficient of the modification layer, improving the thermal shock resistance and tensile deformation resistance, improving the performance of the atomizing core and further improving the performance of the atomizer.

[0065] The above description is merely an embodiment of the present invention, and does not limit the scope of protection of the present invention. All equivalent structure or equivalent flow modifications made by the specification and accompanying drawings of the present invention, directly or indirectly applied to other related technical fields, should be included in the scope of protection of the present invention for the same reasons. [Explanation of symbols]

[0066] 11 Ceramic substrate 12 Modification layer 21 Heating layer 22 electrodes 100 Atomizer 200 Power Supply 300 Electronic Atomizer

Claims

1. A ceramic comprising a ceramic substrate and a modification layer, The ceramic substrate is a porous ceramic, the modification layer is provided on the surface of the ceramic substrate and contains a bismuth-based oxide and other components; The ceramics characterized in that the mass percentage of bismuth element in the modification layer is 50% to 80%.

2. The ceramic according to claim 1 , wherein the bismuth-based oxide includes bismuth oxide.

3. 2. The ceramic according to claim 1, wherein the other components include at least one element selected from the group consisting of sodium, magnesium, aluminum, silicon, potassium, calcium, titanium, zinc, zirconium, and barium.

4. The other components include zinc element, The ceramic according to claim 3, characterized in that the mass percentage of the zinc element in the modification layer is 5% to 7%.

5. The ceramic according to claim 1 , wherein the modified layer does not contain lead element.

6. The ceramic according to claim 1 , wherein the modified layer has a continuous porous structure.

7. An atomizing core comprising a ceramic substrate, a modification layer, and a heat generating layer, The ceramic substrate is a porous ceramic, the modification layer is provided on the surface of the ceramic substrate and contains a bismuth-based oxide and other components; The atomizing core is characterized in that the heat generating layer is disposed by being laminated on a surface of the modification layer that is remote from the ceramic substrate.

8. An atomizer, a reservoir for storing the aerosol-generating substrate; and the atomizing core according to claim 7, The atomizer is characterized in that the atomizing core absorbs, heats, and atomizes the aerosol-generating substrate in the liquid storage chamber.

Citation Information

Patent Citations

  • Photocatalytic device taking porous ceramic as carrier as well as preparation method and application thereof

    CN112675884A

  • Atomizing core and electronic atomizing device

    CN112931952A

  • Heating element, preparation method thereof, atomizer and atomizing device

    CN113475755A

  • Atomizing element, atomizer and electronic atomizing device

    CN113615887A

  • Atomization element and electronic cigarette

    EP4005419A1