Insulation products with loose mineral wool
Aeration and compaction of mineral wool using turbulent gas flow in a chamber addresses the homogeneity issue in bulk mineral wool insulation, enhancing thermal performance and airflow resistance.
Patent Information
- Application Number
- JP2023115263
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-12-29
- Filing Date
- 2023-07-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2036-12-23
AI Technical Summary
Existing methods for producing bulk mineral wool insulation products are not sufficiently homogeneous, leading to suboptimal thermal performance due to non-uniform distribution of mineral wool nodules or flakes, which results in thermal bridging and inefficient thermal conductivity.
A method involving a venting process using a chamber with turbulent gas flow to aerate mineral wool nodules or flakes, creating a recirculation of mineral wool entrained in opposite directions to achieve a homogeneous structure, resembling 'down' with individualized fibers, and subsequent compaction to maintain homogeneity.
The method significantly improves thermal performance by reducing thermal conductivity and enhancing airflow resistance, achieving a more uniform distribution of mineral wool that is virtually indistinguishable in size, resulting in improved insulation properties.
Smart Images

Figure 0007594052000006 
Figure 0007594052000007 
Figure 0007594052000008
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulation product comprising mineral wool. [Background technology]
[0002] Mineral wool is a very good thermal and sound insulator, since it has intertwined mineral fibers that give it a porous and elastic structure. Such a structure can trap air and absorb or attenuate noise. Moreover, mineral wool is essentially made from mineral materials, in particular from natural materials or recycled products (recycled glass), and is therefore attractive from the point of view of environmental balance. And, since mineral wool is based on materials that are inherently non-combustible, it will not ignite or spread fire. Preferably, the mineral wool is selected from glass wool and rock wool.
[0003] A distinction is made, on the one hand, between panel or roll type insulating products (insulating products) obtained in the form of sheets or mats of fibers whose cohesion is ensured by binders (also called sizes) that bind the fibers together by specific point adhesion, and, on the other hand, loose-packed type products, which take the form of small bundles of entangled fibers forming centimeter-scale particles, in which there is no binder present that ensures the cohesion of the fibers in the bundles.
[0004] The production of so-called loose mineral wool comprises at least the following steps: - melting raw materials such as glass in a furnace; - fiberization; - forming a mineral wool mat; - Nodulation using a grinding process.
[0005] The production of loose mineral wool may further comprise the steps of: - coating with agents such as antistatic agents and / or binders prior to, simultaneously with or after nodule formation; and / or - Packing process.
[0006] After the nodule formation process, the mineral wool in nodule or flake form may be used as such, by spreading it, by blowing it, or by filling it into cavities, as a bulk insulation product or as bulk insulation, which represents a variety of materials in the building industry that are provided in the form of small particles, the texture of which varies from granular to flaky.
[0007] Mineral wool is advantageously used in nodule or flake form as the primary component of bulk insulation products for difficult to access spaces, such as attic space floors that are undeveloped or difficult to access and not suitable for renovation.
[0008] These bulk insulation products are generally applied by mechanical spraying using a spray machine capable of spraying the insulation product from an outlet pipe onto a surface or into a cavity. These bulk insulation products are therefore primarily installed by spraying them directly into the space to be insulated, such as an attic space, or by injecting them into wall cavities. These bulk insulation products are also referred to as sprayed insulation products.
[0009] A sprayed insulation product needs to be as homogeneous as possible to avoid thermal bridges and thereby improve thermal performance. However, when the insulation product is sprayed, the mineral wool in the form of nodules or flakes is not completely homogeneous, regardless of the diameter of the exit tube. The thermal conductivity of the resulting insulation product is not optimized.
[0010] A number of solutions have been considered to improve the uniformity of bulk insulation products during their pneumatic transport.
[0011] The '691 and '683 patent applications disclose flexible pipes having mechanical means that allow the loose insulation to spread as it is installed. These mechanical means are ridges extending across the inner surface of the pipe. The patent application US 2005 / 0133663 A1 discloses a complex method for spreading rock wool before storing it in a storage tank, which comprises a step in which the fibre agglomerates are conveyed by a turbulent airflow defined by a Reynolds number higher than 200,000 inside a duct equipped with a series of needles and uneven areas, so that the agglomerates colliding with it undergo mechanical fibre defibration. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] European Patent No. 1165998 [Patent Document 2] US Patent Application Publication No. 2006 / 0266429 [Patent Document 3] JP 2006-328609 A Summary of the Invention [Problem to be solved by the invention]
[0013] These solutions are often overly complicated and entirely unsatisfactory.
[0014] We have developed a new preparation method which makes it possible to obtain insulation products with mineral wool having improved thermal performance. [Means for solving the problem]
[0015] The method of the invention comprises a step of performing an aeration process inside an apparatus comprising a chamber and at least one means capable of generating a turbulent gas flow.
[0016] During this aeration process, a flow of carrier gas is introduced into the chamber and the mineral wool in the form of nodules or flakes is subjected to a turbulent flow of this carrier gas with entrainment in one sense, direction A, and in a counter-sense direction B opposite to direction A, so that within the chamber there is at least one plane perpendicular to direction A, where the mineral wool entrained in direction A intersects with the mineral wool entrained in direction B.
[0017] The profile of the average velocity of the mineral wool in a flow in direction A comprises at least one recirculation point where the velocity component parallel to direction A is negative and capable of generating a flow in direction B. Preferably, there are multiple recirculation points, whereby one or more recirculation loops or bubbles are formed in the flow.
[0018] It should be noted that the method of the present invention uses unsteady-state turbulent flows. The descriptions given in this application regarding the velocity profile of the flow relate to time-averaged velocities averaged over a period of time sufficient to characterize the observed phenomena.
[0019] This aeration step significantly reduces the density of the mineral wool in the form of nodules or flakes, but above all homogenizes its structure. Surprisingly, the spreading and / or homogenization of the mineral wool subjected to the aeration step of the invention is much better than can be obtained by known homogenization methods. The insulating product obtained may be compressed after the aeration step while maintaining a more homogenous structure.
[0020] The improvement in thermal performance is especially shown by a reduction in thermal conductivity at the same density, or by a reduction in density at the same thermal conductivity, relative to mineral wool that has not been subjected to the ventilation treatment according to the method of the present invention. The resulting insulating product also has a much higher ventilation resistance at the same density.
[0021] When this method is applied to existing mineral wool nodules, the present invention allows the nodules or flakes to spread out so that their individual dimensions are virtually impossible to determine, which can be demonstrated by simple visual inspection of the insulation product.
[0022] The loose-filled mineral wool according to the invention therefore takes on a novel form that can be called down, since it is very similar to the down covering material of animals. Therefore, by "down" in this application we mean a loose-filled mineral wool product in which the fibers that make up the mineral wool are largely individualized and the bundled structure of the flakes is practically destroyed.
[0023] The mineral wool is selected from glass wool or rock wool.
[0024] Glass wool is generally defined as a product obtained from molten mineral material derived from a mixture of vitrifiable raw materials and converted into fibers by a process that is usually centrifugal spinning. By melting the glass into a relatively viscous liquid form, relatively long and thin fibers are obtained.
[0025] Rock wool is generally defined as a product obtained from molten mineral material derived from natural rock and converted into fibers by a process involving a series of rotating wheels. By melting the natural rock into a highly mobile liquid form, relatively short, thick fibers are obtained.
[0026] When using rock wool, it can be difficult to obtain a down morphology, and the present invention also includes a novel structure of rock wool flakes. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 includes photographs showing, respectively: FIG. 1A: glass wool in the form of nodules or flakes that have not undergone an aeration process according to the invention, and FIG. 1B: glass wool in the form of down that has undergone an aeration process according to the invention. [Diagram 2] FIG. 2 contains photographs showing, respectively: FIG. 2A: rock wool in the form of nodules or flakes that have not undergone an aeration process according to the invention, and FIG. 2B: "spread out" rock wool in the form of nodules or flakes that have undergone an aeration process according to the invention. [Diagram 3] The tomographic images in Figure 3 respectively show: - Figure 3A: glass wool in the form of nodules or flakes that have not undergone an aeration process according to the invention, with a density of 10 kg / m3; - Figure 3B: insulating product comprising loose-filled glass wool in the form of down that has undergone an aeration process according to the invention, with a density of 4 kg / m3; - Figure 3C: insulating product comprising loose-filled glass wool in the form of down that has undergone an aeration process and a compression process according to the invention, with a density of 10 kg / m3. [Figure 4] Figure 4 shows a graph representing the variation of greyscale level with volume, which is a processed version of the image of Figure 3. The abscissa axis is a plot of intensity and the ordinate axis is a plot of the number of pixels exhibiting that intensity. The points on the curve correspond to the number of pixels found in the image at a given greyscale level. Curves (a), (b), and (c) correspond to the insulating products of Figures 3A, 3B, and 3C, respectively. [Diagram 5] FIG. 5 shows an apparatus making it possible to carry out the aeration process according to the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The better homogeneity obtained by the method of the present invention is clearly evident from a simple visual inspection of the insulation products. In contrast, characterization of these new products by their macroscopic and microscopic structure is difficult to establish.
[0029] To this end, applicants have developed a method for measuring agglomerate size distribution using a vibrating screen, as shown below.
[0030] The method of the present invention makes it possible to spread glass wool and rock wool.
[0031] The present invention relates to an insulating product in the form of down with loose glass wool, characterized in that the mass distribution of agglomerates obtained by screening 2 to 5 g of insulating product with a vibrating sieve shaker equipped with multiple layers of screens and a maximum vibration amplitude of 3 mm, with a vibration amplitude set between 1.5 and 2.5 mm, preferably between 1.8 and 2.2 mm and even better still at 2 mm, for 5 minutes, is: - the percentage by weight of agglomerates passing through a 6 mm screen is less than 5% by weight, preferably less than 3% by weight; and / or the weight percentage of agglomerates passing through a 13 mm screen is less than 50% by weight, preferably less than 40% by weight, or even less than 35% by weight.
[0032] The present invention relates to an insulating product comprising loose rock wool in the form of down, nodules or flakes, characterized in that the mass distribution of agglomerates obtained by screening 2-5 g of insulating product for 5 minutes using a vibrating sieve shaker with multiple layers of screens and a maximum vibration amplitude of 3 mm, with the vibration amplitude set to 1.5-2.5 mm, preferably 1.8-2.2 mm and even better still 2 mm, satisfies the following relationship: (% agglomerates 6-13)-(% agglomerates<6)≧5%, wherein: - (% Agglomerates 6-13) corresponds to the mass percent of agglomerates passing through both the 6 mm and 13 mm screens, and - (% agglomerates <6) corresponds to the mass percent of agglomerates passing through a 6 mm screen.
[0033] The insulating products according to the invention have a much lower thermal conductivity and a much higher airflow resistance. Another possible way to characterize the products according to the invention can be based on the "thermal conductivity / density" combination or the "airflow resistance / density" combination.
[0034] The present invention also provides a method for determining the amount of 3 Units of density "d" and mW m -1 ·K-1 The thermal conductivity of the material is 7 to 14 kg / m 3 It also relates to an insulating product comprising loose-filled glass wool in the form of down, characterized in that, at a density d where d is the density of the insulating product, the following relationship is satisfied: λ <A+0.3d+205 / d (wherein A ranges from 17 to 23, inclusive).
[0035] In the above formula, A has a value of 22, 21, 20, 19, 18, or 17, in order of increasing preference, whereby λ<23+0.3d+205 / d, λ<20+0.3d+205 / d, or λ<18+0.3d+205 / d It becomes.
[0036] The present invention also provides a composition having a viscosity of 9.5 to 10.5 kg / m 3 At a density d of 42 mW m -1 ·K -1 Less than 41 mW m -1 ·K -1 The present invention also relates to an insulating product comprising loose-filled glass wool in the form of down, characterized in that it exhibits a thermal conductivity "λ" of less than 1000 nm.
[0037] The present invention also provides a method for producing a 10 to 20 kg / m 3 , preferably 10 to 15 kg / m 3 At a density of 1 kPa s / m 2 More than 2kPa·s / m 2 More than 5kPa·s / m 2 It also relates to an insulating product comprising loose-filled glass wool in the form of down, characterized in that it exhibits the above airflow resistance (in accordance with standard EN 29053).
[0038] The present invention also provides a method for determining the amount of 3 Units of density "d" and mW m -1 ·K -1 The thermal conductivity of the material is expressed as "λ" in units of 50 to 80 kg / m 3The present invention also relates to an insulating product comprising rock wool in the form of down, nodules or flakes, characterized in that at a density d where d=0.05, the following relationship is satisfied: λ<-0.1d+45, Preferably, λ<-0.1d+44.5, λ<-0.1d+44, λ<-0.1d+43.
[0039] The present invention also relates to an insulating product comprising rock wool, characterized in that the airflow resistance (according to standard EN 29053) is: - 40~50kg / m 3 At a density of 1 kPa s / m 2 More than 2kPa·s / m 2 More than 3kPa·s / m 2 or more, and / or - 60~80kg / m 3 At a density of 10 kPa s / m 2 More than 15kPa·s / m 2 The end.
[0040] The invention then relates to a method of thermal insulation by spraying the insulating product according to the invention directly onto a surface or by injecting it into a cavity.
[0041] The preferred features which form the main part of the remainder of this specification are applicable to the various insulation products containing glass wool or rock wool, just as they are applicable to the methods of insulation, where applicable.
[0042] The insulating product according to the invention is essentially based on spread mineral wool. - non-aerated mineral wool in the form of nodules or flakes is the name given to mineral wool that does not have the novel structural features that can be obtained after the aeration step according to the invention; - mineral wool in the form of spread or aerated nodules or flakes, or in the form of down, is the name given to mineral wool having novel structural characteristics which can be obtained after the aeration step according to the invention.
[0043] The mineral wool is selected from glass wool and rock wool.
[0044] Mineral wool nodules or flakes are not individualized fibers like textile glass fibers, but are bundles of fibers. These mineral wool nodules or flakes have a length of 0.05 to 5 cm, in particular 0.1 to 1 cm. These flakes or nodules are formed from entangled fibers in the form of small bundles, small rovings, or "pillings". By length of the flakes or nodules in this specification is meant the length of the longest dimension of these bundles.
[0045] Ideally, the mineral wool is spread out sufficiently that the nodules and flakes can no longer be easily distinguished.
[0046] When the insulating product comprises glass wool, the flakes or nodules can no longer be distinguished. The insulating product takes the form of a down, i.e. a product in the form of a layer of discontinuous fibres that remain together, or in the form of a down-like web, where the fibres are simply entangled (not bonded) in a loose, fluffy structure. Portions of the down or web can be removed without affecting the volumetric structure.
[0047] Glass wool comprises glass fibres. Nodules or flakes of glass wool obtained by fibreisation of glass using an apparatus in particular comprising a centrifuge or a centrifugal spinner and a basket are described, for example, in patent EP 2511586. A stream of molten glass is fed into the centrifuge and flows out into the basket. The glass wool fibres are formed into nodules as described in patent application FR 2661687 A1. These glass fibres are intertwined with each other.
[0048] Glass wool fibres differ from the so-called "textile grade" glass fibres which are obtained in the form of sized filaments by high speed mechanical drawing of molten glass.
[0049] Glass wool exhibits the following Micronaire values in order of increasing preference: - Less than 20L / min, Less than 15L / min, Less than 12L / min, Less than 10L / min, - More than 2L / min, more than 3L / min, more than 4L / min, more than 5L / min.
[0050] The Mycnaire value is measured according to the method described in WO 03 / 098209(A).
[0051] The glass fibers of the glass wool are discontinuous. They preferably have an average diameter of less than 5 μm, or even less than 4 μm.
[0052] The glass wool globules or flakes are, for example, flakes made of glass wool of the type used for blown wool insulation, for example those sold under the trade names Comblissimo™ or Kretsull™ by the company Saint-Gobain Isover, or under the trade name Insulsafe™ by the company Certainteed. These flakes are generally binder-free and may contain anti-dust and / or anti-static agents, such as oils. According to certain embodiments, insulation products comprising glass wool satisfy one or more of the following characteristics: - the percentage by weight of agglomerates passing both the 25 mm screen and the 32 mm screen relative to the agglomerates passing the 32 mm screen is less than 10% by weight, preferably less than 5% by weight, or even less than 3% by weight; - the percentage by mass of the agglomerates passing both the 19 mm screen and the 25 mm screen relative to the mass of the agglomerates passing the 32 mm screen is greater than 10%, preferably greater than 20%, greater than 30%, or even greater than 40% by mass; - the percentage by mass of the agglomerates passing both the 13 mm screen and the 25 mm screen relative to the mass of the agglomerates passing the 32 mm screen is greater than 50%, preferably greater than 55%, greater than 60%, greater than 70%; - the percentage by mass of the agglomerates passing both the 13 mm screen and the 32 mm screen relative to the mass of the agglomerates passing the 32 mm screen is greater than 60%, preferably greater than 65%, greater than 70%, greater than 80%; - It comprises at least 75% and preferably at least 95% glass wool, based on the total mass of the insulation product.
[0053] Rock wool comprises rock fibres. It has a Fasonaire value of at least 250. This parameter, also called fineness index, is measured by a method conventional in the field of rock wool. The Fasonaire value is determined as follows: a test specimen (5 g) consisting of one tuft of mineral wool, free of oil and binder, but which may contain non-fibrous constituents (non-fibrous or "slag" or "shot"), is weighed. This test specimen is compressed to a defined volume and a gas stream (dry air or nitrogen) is passed through it, maintained at a constant flow rate. The measurement of the Fasonaire value is then the drop in pressure head through the test specimen, evaluated by a water column graduated in conventional units. Conventionally, the result of the Fasonaire value is the average of the drop in pressure head observed over 10 test specimens.
[0054] According to certain embodiments, the insulation product comprising rock wool satisfies one or more of the following characteristics: - satisfy the following relationship: (% aggregates 6-13)-(% aggregates < 6) ≥ 10%; - The mass percentage of agglomerates passing the 6 mm screen is: - Less than 40%, less than 45%, less than 30%, and / or - More than 10% or more than 20%; - The mass percentage of agglomerates passing the 13 mm screen is: - Less than 95%, less than 90%, less than 80%, and / or - More than 50%, 60% or 70%; - the mass percentage of agglomerates passing both the 6 mm and 13 mm screens is greater than 40%, preferably greater than 45%, greater than 50%, greater than 60%; - the mass percentage of agglomerates passing both the 6 mm and 19 mm screens is greater than 50%, preferably greater than 55%, greater than 60%, greater than 70%; - the mass percent of agglomerates passing through a 25 mm screen or a 34 mm screen is 100%; - the rock wool comprises intertwined mineral fibres having a Fasonaire value of at least 250;
[0055] The insulation product comprises, in order of increasing preference, at least 75%, at least 80%, at least 85%, at least 90%, at least 94%, at least 95%, at least 96%, at least 97%, at least 98%, at least 99% mineral wool by total mass of the insulation product, preferably the mineral wool is selected from glass wool and rock wool.
[0056] The insulation product comprises, in order of increasing preference, at least 75%, at least 80%, at least 85%, at least 90%, at least 94%, at least 95%, at least 96%, at least 97%, at least 98%, at least 99% mineral fibers, preferably glass fibers or rock fibers, based on the total mass of the insulation product.
[0057] The insulation product comprises, in order of increasing preference, at least 75%, at least 80%, at least 85%, at least 90%, at least 94%, at least 95%, at least 96%, at least 97%, at least 98%, at least 99% mineral material based on the total mass of the insulation product.
[0058] The invention also relates to a method of insulation by spraying or spraying an insulating product according to the invention directly into the space to be insulated, or by injecting an insulating product according to the invention into a cavity, in particular into a wall cavity, or into any other hollow wall shape to be insulated.
[0059] I. Protocol for Measuring Agglomerate Size Mass Distribution This measurement makes it possible to characterize the structure of insulation products with mineral wool, in particular with glass or rock mineral wool. The principle behind the measurement is to vibrate layers of screens with different diameters and to classify the agglomerates (or solid particles) according to their size as a result of the vibration process.
[0060] The screen is used for classifying the agglomerates and is fixed to a frame, which corresponds to a grid of relatively large or relatively small mesh size. The screen is vibrated by means of a sieve shaker, which corresponds to the vibrating device on which the screen is placed.
[0061] After the aeration process, it may not be possible to determine the size of the nodules or flakes, especially if the insulation product comprises glass wool, in which case the insulation product takes the form of a product in the form of a down, i.e. a layer of discontinuous fibres gathered together in the form of a web (see FIG. 1B) with an aerated fluffy texture.
[0062] Mass distribution measurements are destructive because vibration tends to separate the down into clumps.
[0063] Similarly, even if nodules or flakes are still present after the aeration process, as can be the case with rock wool, vibration can change their dimensions.
[0064] According to the present invention, the term "agglomerates" is used to refer to the material collected on each screen or in the container below during the screening process. Thus: - nodules or flakes resulting from the mineral wool manufacturing process or remaining after the aeration process; and - the agglomerates obtained after vibration, A distinction is made between EXAMPLES
[0065] 1. Equipment and devices The equipment required for this measurement is: - mineral wool test specimens, preferably sprayed; - Precision balance with an accuracy of up to ±0.05g, - a plastic beaker with a capacity of approximately 500 mL, - Screen and lower container (without holes), - Automatic sieve shaker "Retsch Sieve Shaker" model RX-24, Equipped with.
[0066] A 20 cm (8 inch) diameter screen with the following hole sizes: - 6mm(0.25inch), - 13mm(0.5 inch), - 19mm(0.75inch), - 25mm(1 inch), - 32mm(1.25inch), - 38mm(1.5inch), - 44mm(1.75inch), was used.
[0067] 2. Procedure The following steps are carried out: - Representative specimens of the aerated mineral wool or insulating product (hereinafter referred to as samples) are collected in boxes with dimensions of approximately 40 x 40 x 40 cm or more. The mineral wool must not be compressed during handling or transportation. - Weigh 3.0-3.5+ / -0.1g of product into a plastic beaker. - Stack the screens on a sieve shaker, from the smallest mesh size (6mm) to the largest mesh size. - Gently place the specimen on the top screen, i.e. the screen with the largest mesh size. It is important to maximise the surface area covered so that larger agglomerates do not prevent smaller agglomerates from falling through. - Cover the multi-layer screen and tighten it tightly. If the screen is not properly centered and / or secured, the vibrations will be too strong and the measurement will not be correct. - Start the sieve shaker and set its power, then set the measurement time to 5 minutes. - After vibration is complete, weigh the material on each screen. Calculate the mass percent by dividing the mass of the material on that screen by the sum of the masses of all screens.
[0068] The vibrating sieve shaker is equipped with multiple layers of screens and a maximum vibration amplitude of 3 mm. The vibration amplitude is set to 1.5-2.5 mm, preferably 1.8-2.2 mm, and even better 2 mm. The vibration is continued for 5 minutes. The power of the sieve shaker is set in order to obtain the desired vibration amplitude. For example, the power of the sieve shaker is set to 65% when 4 screens are used and 45%-65% when 7 screens are used in order to obtain the same level of vibration.
[0069] 3. Expression of results The results are expressed as mass percent per screen. At least five measurements are made on new samples. The mean and standard deviation are then calculated.
[0070] II. Examples In these examples, glass wool and rock wool were used, none of which was aerated and which was in the form of nodules or flakes.
[0071] Before the aeration process, the glass wool in the form of nodules or flakes has glass fibers with a Micronaire value of 5.6 L / min. It has a density of 11.6 kg / m 3 The density of is shown.
[0072] Before the aeration process, rock wool in the form of nodules or flakes has rock fibres with a Fasonaire value of 250. It has a viscosity of 74 kg / m 3The density of is shown.
[0073] An apparatus making it possible to carry out the aeration process according to the invention is shown in Figure 5. This apparatus comprises: - an air injection system 1 generating a first air jet; - Chamber 2, - outlet opening 3, Equipped with.
[0074] The dimensions of the apparatus are as follows: 30 cm x 30 cm x 40 cm, with the longest side oriented towards the jet.
[0075] In the case of glass wool, the first air jet is a "high pressure" jet with an inlet pressure of about 4 bar.
[0076] In the case of rock wool, the first air jet is the jet obtained from a gun providing sufficient inlet pressure.
[0077] Mineral wool in the form of nodules or flakes is introduced into the chamber 2 by means not shown. For example, approximately 100 g of glass wool are typically introduced. In the case of rock wool, approximately the same volumetric amount is introduced.
[0078] The mineral wool in the form of nodules or flakes is then subjected to a turbulent flow by being entrained with a carrier gas in direction A with the aid of a first high pressure air jet generated by an air injection system 1 .
[0079] The chamber is configured such that a turbulent setting is established in which the mineral wool can be entrained with the carrier gas in a counter-going direction B, opposite to direction A, so that within the chamber there is at least one plane perpendicular to direction A, where the mineral wool entrained in direction A and the mineral wool entrained in the counter-going direction B intersect each other. In Figure 5, A and B represent two velocity vectors of the same and opposite direction. By convention, the velocity along vector A is referred to as positive and the velocity along vector B is referred to as negative.
[0080] Entrainment with the carrier gas in a direction B, opposite to direction A, is the result of an appropriate selection of the ratio between the cross section of the first jet and the size of the chamber.
[0081] Representing the average velocity profile, there is at least one, and preferably multiple, recirculation points within the chamber, where the velocity component in direction A is negative, which corresponds to a flow in direction B, and therefore the recirculation motion is countercurrent to A.
[0082] This recirculation zone corresponds to a quantity "q" of mineral wool which at any instant returns in the opposite direction to direction A, passing the same point at least twice. The streamlines plotted in Figure 5 suggest that a quantity of mineral wool makes multiple loops passing the same point multiple times.
[0083] In addition, the chamber dimensions are: - the dimension perpendicular to the direction of the initial jet is large enough to generate recirculation points in the plane of the chamber; and - The dimension parallel to the jet direction is small enough to allow for repeated recirculation motion It is adjusted as follows.
[0084] Once the mineral wool has been sufficiently aerated, the insulation product is discharged from the chamber through the outlet opening 3, either by actuation of an opening mechanism or by sizing the chamber so that the residence time between the introduction of the mineral wool and the opening of the outlet corresponds to the time required to achieve the desired degree of homogeneity.
[0085] Like this: - Mineral wool in the form of down, or - down or rock wool in the form of spread nodules or flakes; An insulating product according to the invention is obtained comprising:
[0086] The device is capable of aerating 3 kg of insulating products, including glass wool, per hour.
[0087] The insulating products according to the invention have a low density after the ventilation process, in particular about 4 kg / m for products based on glass wool. 3 , and approx. 50 kg / m for rockwool-based products. 3 These products may optionally be subjected to a compression step, which may be performed by pressing the product between two plates.
[0088] The ratio of pre-aeration density to post-aeration density is preferably greater than 2, preferably greater than 2.5. Density is very important in spray insulation products because it determines the coverage of the product, which is the area that can be covered with a given mass of product to a specified depth.
[0089] 1. Visual Observation and Tomographic Observation Figures 1 and 2 respectively: FIG. 1A: glass wool in the form of nodules or flakes that have not undergone an aeration treatment step according to the invention; FIG. 1B: insulation product comprising loose-filled glass wool in the form of down that has undergone a ventilation treatment process according to the invention; FIG. 2A: Rock wool in the form of nodules or flakes that have not undergone an aeration treatment step according to the invention; FIG. 2B: Insulation product comprising "spread" rock wool in the form of nodules or flakes that have undergone an aeration process according to the invention; The present invention is provided with a photograph showing the above.
[0090] These photographs show the better homogeneity of the insulation product obtained according to the invention.
[0091] The tomographic images in Figure 3 are: FIG. 3A: Glass wool in the form of nodules or flakes that have not undergone an aeration process according to the invention, density 10 kg / m 3 , FIG. 3B: Insulation product containing loose-filled glass wool in the form of down that has undergone a ventilation treatment process according to the present invention, with a density of 4 kg / m 3 , FIG. 3C: Insulation product containing loose-filled glass wool in the form of down, which has been subjected to aeration and compression processes according to the present invention, with a density of 10 kg / m 3 , Shows.
[0092] Processing of these images is shown in the graph of Figure 4, which represents the variation of greyscale level with volume. The abscissa axis is a plot of intensity and the ordinate axis is a plot of the number of pixels exhibiting that intensity. The points on the curve correspond to the number of pixels found in the image at a given greyscale level. Curves (a), (b), and (c) correspond to the insulating products of Figures 3A, 3B, and 3C, respectively.
[0093] These images and the processing of these images also show a better homogeneity of the insulation product according to the invention, which is manifested by a better distribution in terms of greyscale levels: the insulation product according to the invention has a broader and more Gaussian peak, whereas the non-ventilated glass wool has a narrower and more asymmetrical distribution.
[0094] And the insulation product that has been subjected to the compression process after the ventilation process shown in image 3C maintains the advantageous property of homogeneity. Thus, the present invention makes it possible to obtain a homogeneous insulation product with variable density.
[0095] 2. Measurement of the mass distribution of aggregate sizes The vibrating screen method was used to determine the agglomerate size distribution for the following products: - PI LV A: insulating products containing aerated mineral wool in the form of down; - PI LV NA: insulation products containing non-ventilated glass wool in the form of nodules or flakes; - PI LR A: insulation products containing aerated rock wool in the form of nodules or flakes; - PI LR NA: Insulation products containing non-aerated rock wool in the form of nodules or flakes.
[0096] Insulation products containing glass wool are in the form of loose wool down. Here, the down is separated into agglomerates by distribution measurement using vibrating screens. However, a large, sometimes very large amount of material is found on the upper screens with a hole size of 32 mm or more, i.e. on the 32 mm, 38 mm and 44 mm screens. The presence and distribution of the agglomerates on these screens is random. For this reason, the mass distribution for agglomerates with a size of 0-32 mm in aerated glass wool-based insulation products was also calculated. For this purpose, the mass percentage is calculated by dividing the mass of the material on the relevant screen by the sum of the masses of all material present below the screens with a hole size equal to 32 mm.
[0097] In other insulation products, 100% of the agglomerates pass through a screen smaller than 32 mm. The distribution in terms of mass percentage ranges from 0 to 32 mm.
[0098] Table 1 shows that for glass wool based insulation products: - agglomerates with various sizes ranging from 0 to over 44 mm; - agglomerates with various sizes from 0 to 32 mm; The distribution results as mass percent for
[0099] Table 2 contains the cumulative mass percent and inverse cumulative mass percent for glass wool based insulation products having agglomerates passing through a screen from 0 to over 44 mm.
[0100] Table 3 contains the cumulative mass percent and inverse cumulative mass percent for glass wool based insulation products having agglomerates passing through a 0-32 mm screen.
[0101] Table 4 shows the insulation properties of rock wool-based insulation products containing agglomerates with different sizes from 0 to 32 mm: - the distribution results as mass percent, - cumulative mass percent, Includes.
[0102] When the mass distribution is represented as a graph, where the abscissa axis is a plot of agglomerate size as a function of the screens passed in increasing order, and the ordinate axis is a plot of mass fraction, a curve is obtained which shows one or two peaks, the highest peak being considered the main peak.
[0103] The aeration process has the effect of shifting this peak to the right and flattening it, meaning that the aeration process increases the size of the agglomerates and makes the distribution more uniform, especially in the 0-32 mm range.
[0104] This difference in distribution is believed to contribute to the better properties obtained in terms of thermal performance.
[0105] [Table 1]
[0106] [Table 2]
[0107] [Table 3]
[0108] [Table 4]
[0109] 3. Measurement of thermal conductivity and ventilation resistance Thermal conductivity measurements were carried out on insulating products. The thermal conductivity λ of a product is its ability to pass a heat flux through it and is expressed in W / (m·K). The lower this conductivity, the more insulating the product is and therefore the better it is at insulating. The thermal conductivity values as a function of density were measured according to standard EN14064.
[0110] The insulation product specimens were conditioned at 23°C and approximately 50% relative humidity (RH) to allow the mass to stabilize. The measurements were carried out on an R-matic type device at an average temperature of 10°C on product cases with dimensions of 590 x 590 mm and a crushed measured thickness of 108 mm. The actual measurement zone measured was 254 x 254 mm. The average thermal conductivity of the insulation products is given in the table below.
[0111] Air flow resistance measurements according to standard EN 29053 (method A) were carried out on the same specimens as those used for the thermal conductivity measurements.
[0112] These tests used several pieces of glass wool and one piece of rock wool.
[0113] The thermal conductivity and air flow resistance of the following insulation product specimens were measured: - PI LV1 NA: Insulation products containing type 1 glass wool, not ventilated; - PI LV1 A type 1 glass wool containing insulation products, ventilated, - PI LV2 NA: Insulation products containing glass wool type 2, not ventilated; - PI LV2 A: Insulation products containing glass wool of type 2, with ventilation treatment; - PI LV3 A: Insulation products containing glass wool of type 3, with ventilation treatment; - PI LV4 A: Insulation products containing glass wool of type 4, with ventilation treatment; - PI LR NA: Insulation product containing rock wool, not ventilated, - PI LR A: Insulation product containing rock wool, ventilated.
[0114] [Table 5]
[0115] In terms of performance, the insulating product according to the invention obtained after the venting process has a very significantly lower thermal conductivity.
[0116] All glass wool based insulation products according to the invention have a ductility of 9.5-10.5 kg / m 3 At a density of 43 mW m -1 K -1 or even 41 mW m -1 K -1 It has a lower thermal conductivity than
[0117] Insulation products containing the vented glass wool exhibit an improvement in thermal conductivity of more than 15%, preferably more than 20%, compared to insulation products with non-vented glass wool at the same density. For any given performance, half the glass wool is needed to obtain the same heat resistance.
[0118] Substantially non-permeable glass wool in the form of nodules or flakes has a density of 10 kg / m 3 At a density of about 53 mW m -1 K-1 The thermal conductivity of
[0119] At the same density, the insulating product according to the invention has a resistance of about 37 mW m -1 K -1 This means that for the same spray thickness, the thermal conductivity is 16mW m -1 K -1 This corresponds to a decrease in heat resistance of 30% and an increase in heat resistance of 30%.
[0120] The insulation product according to the invention has a thermal conductivity of 4.8 kg / m 3 This indicates a density of 5.2 kg / m 3 This corresponds to a drop in the material usage rate, representing a material savings of 52%. The invention according to the present disclosure includes the following aspects: <Aspect 1> 1. An insulating product comprising loose-filled glass wool in the form of down, characterized in that the mass distribution of the agglomerates obtained by screening 2 to 5 g of insulating product for 5 minutes using a vibrating sieve shaker equipped with multiple layers of screens and a maximum vibration amplitude of 3 mm, said vibration amplitude being set to 1.5 to 2.5 mm, preferably 1.8 to 2.2 mm and even better to 2 mm, is: - the percentage by weight of agglomerates passing through a 6 mm screen is less than 5% by weight, preferably less than 3% by weight; and / or the weight percentage of agglomerates passing through a 13 mm screen is less than 50% by weight, preferably less than 40% by weight, or even less than 35% by weight. <Aspect 2> 2. An insulating product comprising loose-filled glass wool in the form of down according to aspect 1, characterized in that the percentage by weight of agglomerates passing both the 25mm screen and the 32mm screen relative to the agglomerates passing the 32mm screen is less than 10% by weight, preferably less than 5% by weight, or even less than 3% by weight. <Aspect 3> 3. An insulating product comprising loose-filled glass wool in the form of down according to aspect 1 or 2, characterized in that the percentage by mass of agglomerates passing both the 19mm and 25mm screens relative to the mass of agglomerates passing the 32mm screen is greater than 10%, preferably greater than 20%, 30% or even greater than 40% by mass. <Aspect 4> An insulating product comprising loose-filled glass wool in the form of down according to any one of aspects 1 to 3, characterized in that the percentage by mass of agglomerates passing both the 13 mm screen and the 25 mm screen relative to the mass of agglomerates passing the 32 mm screen is greater than 50%, preferably greater than 55%, greater than 60%, greater than 70%. <Aspect 5> An insulating product comprising loose-filled glass wool in the form of down according to any one of the preceding claims, characterized in that the percentage by mass of agglomerates passing through both the 13mm screen and the 32mm screen relative to the mass of agglomerates passing through the 32mm screen is greater than 60%, preferably greater than 65%, greater than 70%, greater than 80%. <Aspect 6> kg / m 3 Units of density d and mW m -1 ·K -1 The thermal conductivity λ is 7 to 14 kg / m 3 An insulating product comprising loosely packed glass wool in the form of down, characterized in that at a density d where d is the density of the down, the following relationship is satisfied: λ <A+0.3d+205 / d (A is between 17 and 23 inclusive). <Aspect 7> 9.5~10.5kg / m 3 At a density d of 42 mW m -1 ·K -1 Less than 41 mW m -1 ·K -1 1. An insulating product comprising loose-filled glass wool in the form of down, characterized in that it has a thermal conductivity λ of less than 100 nm. <Aspect 8> 10~20kg / m 3 The density is preferably 10 to 15 kg / m 3 At a density of 1 kPa s / m 2 More than 2kPa·s / m 2 More than 5kPa·s / m 2 1. An insulating product comprising loose-filled glass wool in the form of down, characterized in that it has an airflow resistance of at least 100%. <Aspect 9> Insulation product comprising loose-filled glass wool in the form of down according to any one of aspects 1 to 8, characterized in that said glass wool has a micronaire value of: - less than 20 L / min, preferably less than 10 L / min, - More than 2L / min, preferably more than 4L / min, more than 5L / min. <Aspect 10> 10. An insulating product comprising loose-filled glass wool in the form of down according to any one of aspects 1 to 9, characterized in that it comprises at least 75%, preferably at least 95% of glass wool relative to the total mass of the insulating product. <Aspect 11> 1. A bulk insulation product comprising rock wool in the form of down, nodules or flakes, characterized in that the mass distribution of agglomerates obtained by screening 2-5 g of insulation product for 5 minutes using a vibrating sieve shaker with multiple layers of screens and a maximum vibration amplitude of 3 mm, said vibration amplitude being set to 1.5-2.5 mm, preferably 1.8-2.2 mm and even better 2 mm, satisfies the following relationship: (% agglomerates 6-13)-(% agglomerates<6)≧5%: Where: - (% Agglomerates 6-13) corresponds to the mass percent of agglomerates passing through both the 6 mm and 13 mm screens, and - (% agglomerates <6) corresponds to the mass percent of agglomerates passing through a 6 mm screen. <Aspect 12> An insulating product comprising rock wool according to embodiment 11, characterized in that the following relationships are satisfied: (%agglomerates6~13)-(%agglomerates<6)≧10% <Aspect 13> 13. An insulation product comprising rock wool according to any one of aspects 11 and 12, characterized in that the mass percentage of agglomerates passing a 6 mm screen is: - Less than 40%, less than 45%, less than 30%, and / or - More than 10%, more than 20%. <Aspect 14> 14. An insulation product comprising rock wool according to any one of aspects 11 to 13, characterized in that the mass percentage of agglomerates passing through a 13 mm screen is: - Less than 95%, less than 90%, less than 80%, and / or - More than 50%, more than 60%, more than 70%. <Aspect 15> 15. An insulation product comprising rock wool according to any one of aspects 11 to 14, characterized in that the mass percentage of agglomerates passing through both the 6 mm and 13 mm screens is greater than 40%, preferably greater than 45%, greater than 50%, greater than 60%. <Aspect 16> 16. An insulation product comprising rock wool according to any one of aspects 11 to 15, characterized in that the mass percentage of agglomerates passing through both the 6 mm and 19 mm screens is greater than 50%, preferably greater than 55%, greater than 60%, greater than 70%. <Aspect 17> 17. An insulation product comprising rock wool according to any one of aspects 11 to 16, characterized in that the mass percentage of agglomerates passing through a 25 mm screen or a 34 mm screen is 100%. <Aspect 18> 18. An insulating product comprising rock wool according to any one of aspects 11 to 17, characterized in that the rock wool comprises entangled mineral fibers having a Fasonaire value of at least 250. <Aspect 19> kg / m 3 Units of density d and mW m -1 ·K -1 The thermal conductivity λ in units of 50 to 80 kg / m 3 1. An insulating product comprising rock wool in the form of down, nodules or flakes, characterized in that, at a density d where d=0.05, the following relationship is satisfied: λ<-0.1d+45; Preferably, λ<-0.1d+44.5; λ<-0.1d+44; λ<-0.1d+43. <Aspect 20> 1. An insulation product comprising rock wool in the form of down, nodules, or flakes, characterized in that it exhibits an airflow resistance of: - 40~50kg / m 3 At a density of 3 kPa s / m 2 and / or - 60~80kg / m 3 At a density of 10 kPa s / m 2 The end.
Claims
1. kg / m 3 Units of density d and mW m -1 K -1 The thermal conductivity λ is expressed in units of 50 to 80 kg / m 3 An insulating product comprising rock wool in the form of down, nodules or flakes, characterized in that at a density d where d is the density of the insulation product, the following relationship is satisfied: λ<-0.1d+45; Preferably, λ<-0.1d+44.5; λ<-0.1d+44; λ<-0.1d+43.
2. An insulating product comprising rock wool in the form of down, nodules, or flakes, characterized in that it exhibits an airflow resistance of: -40~50kg / m 3 At a density of 3 kPa·s / m 2 and / or -60~80kg / m 3 At a density of 10 kPa·s / m 2 The end.
Citation Information
Patent Citations
Improvement to HOSE used to install loose fill insulation
EP1165998A2
Isolating product
EP2511586A1
Composite material using mineral fiber as raw material, apparatus thereof and application of composite material
JP1990182956A
Method for opening rockwool
JP2006097203A
Method for opening rock wool
JP2006328609A