Piezoelectric substrates, sensors, actuators, and bioinformation acquisition devices
The piezoelectric base material with an optically active polypeptide fiber layer and adhesive winding addresses sensitivity and attachment efficiency issues, providing improved piezoelectric sensitivity and durability.
Patent Information
- Application Number
- JP2023511502
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-31
- Filing Date
- 2022-03-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-03-30
AI Technical Summary
Existing piezoelectric base materials, such as those described in Patent Document 1, suffer from poor piezoelectric sensitivity and inefficient terminal attachment preparation due to the mechanical integration of components, which can lead to damage and increased work time during terminal attachment.
A piezoelectric base material design featuring a piezoelectric layer made of optically active polypeptide fibers wound around an internal conductor, with an adhesive maintaining the winding and allowing for easy detachment, and an optional outer conductor for improved piezoelectric sensitivity and electrostatic shielding.
The design achieves enhanced piezoelectric sensitivity and efficient terminal attachment preparation by minimizing damage to the piezoelectric layer and conductor during preparation, enabling better durability and stability.
Smart Images

Figure 0007594093000007 
Figure 0007594093000008 
Figure 0007594093000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a piezoelectric substrate, a sensor, an actuator, and a bioinformation acquisition device. [Background technology]
[0002] In recent years, applications of piezoelectric materials containing a polypeptide having optical activity (hereinafter referred to as "optically active polypeptide") to piezoelectric devices such as sensors and actuators have been considered. Patent Document 1 discloses a piezoelectric substrate using a filamentary piezoelectric body. The piezoelectric substrate specifically disclosed in Patent Document 1 includes a tinsel wire, a specific raw silk, and a copper foil ribbon. The tinsel wire functions as a core material. The raw silk is an example of a fiber made of an optically active polypeptide. The raw silk is wound around the tinsel wire in a spiral shape without gaps so that the tinsel wire is not exposed. Hereinafter, the raw silk wound around the tinsel wire is referred to as a "raw silk layer." The copper foil ribbon is wound around the raw silk wound around the tinsel wire in a spiral shape without gaps so that the raw silk is not exposed. Hereinafter, the copper foil ribbon wound around the raw silk wound around the tinsel wire is referred to as a "copper foil ribbon layer." The tinsel wire, the raw silk layer, and the copper foil ribbon layer are bonded with a cyanoacrylate adhesive. In other words, the tinsel wire, the raw silk layer, and the copper foil ribbon layer are mechanically integrated. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2018 / 092886 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0004] However, there is a demand for a piezoelectric substrate having a piezoelectric sensitivity superior to that of the piezoelectric substrate described in Patent Document 1.
[0005] On the other hand, when manufacturing a line sensor with a coaxial line structure using the piezoelectric substrate disclosed in Patent Document 1 (for example, when used as a part or the whole of a wearable product), it is necessary to cut the piezoelectric substrate to a desired length according to the form of use and attach terminals to the piezoelectric substrate. As a process prior to this terminal attachment, it is necessary to perform preparation for terminal attachment. In the preparation for terminal attachment, the raw silk layer and the copper foil ribbon layer are peeled off from both ends of the piezoelectric substrate to expose the tinsel wire. More specifically, in the preparation for terminal attachment, the copper foil ribbon layer is peeled off from the raw silk layer, and an appropriate length (usually about several mm) of the raw silk layer is removed for removing the tinsel wire, and the tinsel wire is removed. However, in the piezoelectric substrate disclosed in Patent Document 1, the tinsel wire, the raw silk layer, and the copper foil ribbon layer are mechanically integrated. Therefore, when the raw silk layer is removed in preparation for terminal attachment, there is a risk that the copper foil ribbon layer or the tinsel wire may be damaged. Furthermore, there is a risk that the work time for terminal attachment preparation may be long. Therefore, there is a demand for a piezoelectric substrate that allows for efficient preparation for terminal attachment. Furthermore, there is a demand for a piezoelectric substrate that has a piezoelectric sensitivity superior to that of conventional piezoelectric substrates.
[0006] One embodiment of the present disclosure has been made in consideration of the above circumstances. That is, an object of one embodiment of the present disclosure is to provide a piezoelectric substrate, a sensor, an actuator, and a bioinformation acquisition device that have excellent piezoelectric sensitivity. An object of another embodiment of the present invention is to provide a piezoelectric substrate, a sensor, an actuator, and a bioinformation acquisition device that enable efficient preparation for terminal attachment and have excellent piezoelectric sensitivity. [Means for solving the problem]
[0007] Means for solving the above problems include the following embodiments. <1> A long inner conductor; a piezoelectric layer covering an outer circumferential surface of the internal conductor; Equipped with The piezoelectric layer is A piezoelectric yarn wound around the internal conductor; an adhesive portion that holds the piezoelectric yarn wound around the internal conductor; having The piezoelectric yarn comprises an optically active polypeptide fiber, which represents a fiber made of an optically active polypeptide; The piezoelectric layer has an elastic modulus Y of 1.0 GPa or more and 8.0 GPa or less, as measured by a microhardness tester (in accordance with JIS Z 2255). <2> The length direction of the piezoelectric yarn and the main orientation direction of the optically active polypeptide are approximately parallel to each other. <1> The piezoelectric substrate according to claim 1. <3> The degree of orientation F of the optically active polypeptide fiber, which is calculated by the following formula (a) from X-ray diffraction measurement, is 0.50 or more and less than 1.00. <1> or <2> The piezoelectric substrate according to claim 1. Orientation degree F=(180°-α) / 180° … Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.] <4> The piezoelectric yarn is spirally wound in one direction. <1> ~ <3> 13. The piezoelectric substrate according to claim 12, <5> The helix angle between the axial direction of the internal conductor and the longitudinal direction of the piezoelectric yarn is 20° to 70°. <4> The piezoelectric substrate according to claim 1. <6> the adhesive portion is made of at least one selected from an epoxy adhesive, a urethane adhesive, a vinyl acetate resin emulsion type adhesive, an ethylene vinyl acetate emulsion type adhesive, an acrylic resin emulsion type adhesive, a styrene butadiene rubber latex type adhesive, a silicone resin adhesive, an α-olefin adhesive, a vinyl chloride resin solvent type adhesive, a rubber adhesive, an elastic adhesive, a chloroprene rubber solvent type adhesive, a nitrile rubber solvent type adhesive, and a cyanoacrylate adhesive; <1> ~ <5> 13. The piezoelectric substrate according to claim 12, <7> Further, an outer conductor is provided on an outer periphery of the piezoelectric layer, The inner conductor and the outer conductor are not electrically connected to each other. <1> ~ <6> 13. The piezoelectric substrate according to claim 12, <8> The optically active polypeptide has a β-sheet structure. <1> ~ <7> 13. The piezoelectric substrate according to claim 12, <9> The optically active polypeptide comprises at least one of fibroin and spider silk protein. <1> ~ <8> 13. The piezoelectric substrate according to claim 12, <10> The optically active polypeptide fiber includes at least one of silk and spider silk. <1> ~ <9> 13. The piezoelectric substrate according to claim 12, <11> The silk is degummed silk. <10> The piezoelectric substrate according to claim 1 . <12> each of the piezoelectric yarns comprises a plurality of optically active polypeptide fibers; The twist number of the piezoelectric yarn is 500 T / m or less. <1> ~ <11> 13. The piezoelectric substrate according to claim 12, <13> The outermost periphery further includes an electrical insulator. <1> ~ <12> 13. The piezoelectric substrate according to claim 12, <14> The above <1> ~ <13> A sensor comprising a piezoelectric substrate according to any one of claims 1 to 5. <15> The above <1> ~ <13> An actuator comprising the piezoelectric substrate according to any one of the above items. <16> The above <1> ~ <13> A bioinformation acquisition device comprising a piezoelectric substrate according to any one of the above items. <17> A long inner conductor; a piezoelectric layer covering an outer circumferential surface of the internal conductor; Equipped with the piezoelectric layer is formed by winding a long piezoelectric body around the internal conductor and is not fixed to the internal conductor; The long piezoelectric element includes a plurality of piezoelectric yarns and a bundle that bundles the plurality of piezoelectric yarns, A piezoelectric substrate comprising an optically active polypeptide fiber, at least one of the plurality of piezoelectric yarns being a fiber made of an optically active polypeptide. <18> the length direction of the long piezoelectric body is approximately parallel to the main orientation direction of the optically active polypeptide; <17> The piezoelectric substrate according to claim 1. <19> The degree of orientation F of the optically active polypeptide fiber, which is calculated by the following formula (a) from X-ray diffraction measurement, is 0.50 or more and less than 1.00. <17> or <18> The piezoelectric substrate according to claim 1. Orientation degree F=(180°-α) / 180° … Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.] <20> The long piezoelectric element is wound in a spiral shape in one direction. <17> A piezoelectric substrate according to any one of claims 19 to 20. <21> a helical angle between the axial direction of the internal conductor and the longitudinal direction of the long piezoelectric body is 20° to 70°; <20> The piezoelectric substrate according to claim 1. <22> The bundle bundles the piezoelectric yarns in a state in which the piezoelectric yarns are arranged in parallel in a direction perpendicular to the longitudinal direction of the piezoelectric yarns and adjacent piezoelectric yarns among the piezoelectric yarns are in contact with each other. <17> ~ <21> 13. The piezoelectric substrate according to claim 12, <23> The convergent is made of at least one adhesive selected from the group consisting of an epoxy adhesive, a urethane adhesive, a vinyl acetate resin emulsion type adhesive, an ethylene vinyl acetate emulsion type adhesive, an acrylic resin emulsion type adhesive, a styrene butadiene rubber latex type adhesive, a silicone resin adhesive, an α-olefin adhesive, a vinyl chloride resin solvent type adhesive, a rubber adhesive, an elastic adhesive, a chloroprene rubber solvent type adhesive, a nitrile rubber solvent type adhesive, and a cyanoacrylate adhesive. <17> ~ <22> 13. The piezoelectric substrate according to claim 12, <24> The thickness of the long piezoelectric body is 0.001 mm to 0.4 mm, The width of the long piezoelectric body is 0.1 mm to 30 mm, The ratio of the width of the long piezoelectric element to the thickness of the long piezoelectric element is 2 or more. <17> ~ <23> 13. The piezoelectric substrate according to claim 12, <25> The elastic modulus Y of the long piezoelectric body measured by a microhardness tester (in accordance with JIS Z 2255) is 1 GPa or more and 10 GPa or less. <17> ~ <24> 13. The piezoelectric substrate according to claim 12, <26> Further, an outer conductor is provided on an outer periphery of the piezoelectric layer, The inner conductor and the outer conductor are not electrically connected to each other. <17> ~ <25> 13. The piezoelectric substrate according to claim 12, <27> The optically active polypeptide has a β-sheet structure. <17> ~ <26> 13. The piezoelectric substrate according to claim 12, <28> The optically active polypeptide comprises at least one of fibroin and spider silk protein. <17> ~ <27> 13. The piezoelectric substrate according to claim 12, <29> The fiber made of the optically active polypeptide contains at least one of silk and spider silk. <17> ~ <28> 13. The piezoelectric substrate according to claim 12, <30> The silk is degummed silk. <29> The piezoelectric substrate according to claim 1. <31> each of said plurality of piezoelectric yarns comprises a plurality of said optically active polypeptide fibers; The number of twists of each of the plurality of piezoelectric yarns is 500 T / m or less. <17> ~ <30> 13. The piezoelectric substrate according to claim 12, <32> The outermost periphery further includes an electrical insulator. <17> ~ <31> 13. The piezoelectric substrate according to claim 12, <33> The above <17> ~ <32> A sensor comprising a piezoelectric substrate according to any one of claims 1 to 5. <34> The above <17> ~ <32> An actuator comprising the piezoelectric substrate according to any one of the above items. <35> The above <17> ~ <32> A bioinformation acquisition device comprising a piezoelectric substrate according to any one of the above items. Effect of the Invention
[0008] According to the present disclosure, there are provided a piezoelectric substrate, a sensor, an actuator, and a bioinformation acquisition device having excellent piezoelectric sensitivity. According to the present disclosure, a piezoelectric substrate, a sensor, an actuator, and a bioinformation acquisition device that enable efficient preparation for terminal attachment and have excellent piezoelectric sensitivity are provided. [Brief description of the drawings]
[0009] [Figure 1A] 1 is a schematic side view illustrating an external appearance of a piezoelectric substrate according to a first embodiment of the first aspect of the present disclosure. [Figure 1B] FIG. 1B is a cross-sectional view taken along line IB-IB of FIG. [Diagram 2] FIG. 4 is a schematic side view illustrating an external appearance of a piezoelectric substrate according to a second embodiment of the first aspect of the present disclosure. [Figure 3A] FIG. 4 is a schematic side view illustrating an external appearance of a piezoelectric substrate according to a first embodiment of a second aspect of the present disclosure. [Figure 3B] 1 is a schematic front view showing the appearance of a long piezoelectric element according to a first embodiment of a second aspect of the present disclosure. FIG. [Figure 3C] 3C is a cross-sectional view taken along line IC-IC in FIG. 3B. [Figure 3D] 3B is a cross-sectional view taken along line ID-ID in FIG. 3A. [Figure 4] FIG. 4 is a schematic side view illustrating an external appearance of a piezoelectric substrate according to a second embodiment of the second aspect of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits.
[0011] (1) First aspect (1.1) Piezoelectric substrate The piezoelectric substrate according to the first aspect of the present disclosure includes a long internal conductor and a piezoelectric layer covering the outer circumferential surface of the internal conductor. The piezoelectric layer includes a piezoelectric yarn wound around the internal conductor and an adhesive portion that maintains the state in which the piezoelectric yarn is wound around the internal conductor. The piezoelectric yarn includes an optically active polypeptide fiber that is a fiber made of an optically active polypeptide. The elastic modulus Y of the piezoelectric layer measured by a microhardness meter (in accordance with JIS Z 2255) is 1.0 GPa or more and 8.0 GPa or less. It is preferable that the length direction of the piezoelectric yarn and the main orientation direction of the optically active polypeptide are approximately parallel to each other. The degree of orientation F of the optically active polypeptide fiber, which is determined by X-ray diffraction measurement using the following formula (a), is preferably 0.50 or more and less than 1.00. Orientation degree F=(180°-α) / 180° … Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.]
[0012] In this disclosure, "piezoelectric yarn" refers to a piezoelectric material in the form of a yarn. In the present disclosure, an "optically active polypeptide" refers to a polypeptide that has an asymmetric carbon atom and has a bias in the abundance of optical isomers. In the present disclosure, "substantially parallel" means that, when the angle between two line segments is expressed in the range of 0° to 90°, the angle between the two line segments is 0° or more and less than 30° (preferably 0° or more and 22.5° or less, more preferably 0° or more and 10° or less, even more preferably 0° or more and 5° or less, and particularly preferably 0° or more and 3° or less). In the present disclosure, the degree of orientation F of a piezoelectric yarn is an index showing the degree of orientation of an optically active polypeptide contained in the piezoelectric yarn.
[0013] The piezoelectric substrate according to the first aspect of the present disclosure has the above-mentioned configuration and therefore has superior piezoelectric sensitivity to conventional piezoelectric substrates such as those described in Patent Document 1.
[0014] (1.1.1) Piezoelectric layer The piezoelectric substrate of the first aspect of the present disclosure includes a piezoelectric layer.
[0015] The piezoelectric layer covers the outer circumferential surface of the internal conductor, and preferably covers the entire outer circumferential surface of the internal conductor.
[0016] The elastic modulus Y of the piezoelectric layer is 1.0 GPa or more and 8.0 GPa or less. If the elastic modulus Y of the piezoelectric layer is within the above range, the piezoelectric substrate has better piezoelectric sensitivity. In particular, from the viewpoint of improving the piezoelectric sensitivity of the piezoelectric substrate, the elastic modulus Y of the piezoelectric layer is preferably within the first range or the second range, and more preferably within the second range. The first range is from 1.0 GPa to 3.6 GPa, preferably from 1.5 GPa to 3.5 GPa, more preferably from 2.0 GPa to 3.4 GPa, even more preferably from 2.5 GPa to 3.3 GPa, and particularly preferably from 2.5 GPa to 3.2 GPa. The second range is from 4.0 GPa to 8.0 GPa, preferably from 4.2 GPa to 7.0 GPa, more preferably from 4.4 GPa to 6.5 GPa, even more preferably from 4.6 GPa to 6.0 GPa, and particularly preferably from 4.9 GPa to 5.5 GPa. The method for measuring the elastic modulus Y of the piezoelectric layer is the same as the measuring method described in the Examples.
[0017] As a method for setting the elastic modulus Y of the piezoelectric layer within the above range, for example, a method of adjusting the material of the adhesive portion constituting the piezoelectric layer can be mentioned.
[0018] The thickness of the piezoelectric layer is not particularly limited, but is preferably 0.02 mm or more and 2.00 mm or less, and more preferably 0.05 mm or more and 1.00 mm or less.
[0019] The piezoelectric layer may or may not be secured to the inner conductor. In this disclosure, "fixed to the internal conductor" means that the piezoelectric layer is mechanically integrated with the internal conductor by means of an adhesive or the like. In this disclosure, "not fixed to the internal conductor" means that the piezoelectric layer is not mechanically integrated with the internal conductor by an adhesive or the like. In particular, it is preferable that the piezoelectric layer is not fixed to the internal conductor. This allows the piezoelectric layer to be more easily removed from the internal conductor when preparing the piezoelectric substrate for terminal attachment, as described below, than when the piezoelectric layer and the internal conductor are mechanically integrated. In this case, the internal conductor is less likely to be damaged because it is not mechanically integrated with the piezoelectric layer. As a result, the piezoelectric substrate allows efficient preparation for terminal attachment of the piezoelectric substrate. When manufacturing a line sensor with a coaxial line structure using a piezoelectric substrate (for example, when used as a part or the entirety of a wearable product), it is necessary to cut the piezoelectric substrate to the desired length according to the form of use and attach terminals to the piezoelectric substrate. Before attaching the terminals, it is necessary to prepare for terminal attachment. In the preparation for terminal attachment, the raw silk layer and the copper foil ribbon layer are peeled off from both ends of the piezoelectric substrate to expose the tinsel wire. More specifically, in the preparation for terminal attachment, the copper foil ribbon layer is peeled off from the raw silk layer, and an appropriate length of the raw silk layer (usually about a few mm) is removed to remove the tinsel wire. Furthermore, the piezoelectric layer is displaceable relative to the internal conductor in the axial direction of the internal conductor. This allows the piezoelectric substrate to be deformed more easily than conventional piezoelectric substrates when an external stress acts on the piezoelectric substrate. Therefore, the internal stress of the piezoelectric substrate caused by the action of the external stress is less likely to concentrate locally. As a result, the durability of the piezoelectric substrate is excellent.
[0020] The piezoelectric layer includes a piezoelectric yarn and an adhesive portion. The piezoelectric yarn is wound around the internal conductor. The adhesive portion holds the piezoelectric yarn wound around the internal conductor. The piezoelectric yarn may be wound directly around the outer circumferential surface of the inner conductor. When an inner electrical insulator (described later) is disposed on the outer circumferential surface of the inner conductor, the piezoelectric yarn may be wound indirectly around the inner conductor by being wound around the outer circumferential surface of the inner electrical insulator.
[0021] The method of winding the piezoelectric yarn is not particularly limited, and the piezoelectric yarn may be wound helically around the internal conductor in the axial direction of the internal conductor, or may not be wound helically around the internal conductor in the axial direction of the internal conductor. In particular, from the viewpoint of improving the piezoelectric sensitivity of the piezoelectric substrate, it is preferable that the piezoelectric yarn is wound helically around the internal conductor in the axial direction of the internal conductor. The piezoelectric yarn may be wound so as to overlap, or may be wound so as not to overlap. In the piezoelectric substrate according to the first embodiment of the present disclosure, electric charges are easily generated when a shear stress is applied to the helically wound piezoelectric yarn, which makes it easy for piezoelectricity to be exhibited. The shear stress on the piezoelectric yarn can be applied, for example, by a first non-plastic deformation, a second non-plastic deformation, or a third non-plastic deformation, etc. The first non-plastic deformation refers to pulling the entire helically wound piezoelectric yarn in the direction of the helical axis. The second non-plastic deformation refers to twisting a portion of the helically wound piezoelectric yarn (i.e., twisting a portion of the piezoelectric yarn around the helical axis). The third non-plastic deformation refers to bending part or all of the helically wound piezoelectric yarn.
[0022] The piezoelectric yarn is preferably spirally wound in one direction around the internal conductor. "Spiral wound in one direction" refers to a first winding manner or a second winding manner. The first winding mode indicates that the piezoelectric yarn is wound spirally around the internal conductor so as to be left-handed (i.e., counterclockwise) from the front side to the back side when viewed from one end of the piezoelectric substrate. The second winding manner indicates that the piezoelectric yarn is wound helically around the internal conductor so as to be right-handed (ie, clockwise) from the front side to the back side when viewed from one end of the piezoelectric substrate. When the piezoelectric yarn is wound in a spiral shape in one direction, the phenomenon in which the polarities of the generated charges cancel each other out (i.e., the phenomenon in which the piezoelectricity decreases) is suppressed, and therefore the piezoelectricity of the piezoelectric substrate is further improved.
[0023] The embodiment in which the piezoelectric substrate has piezoelectric yarn wound spirally in one direction includes not only an embodiment in which only one layer of piezoelectric yarn is provided, but also an embodiment in which multiple layers of piezoelectric yarn are stacked on top of each other. An example of an embodiment in which multiple layers made of piezoelectric yarn are stacked on top of each other is an embodiment in which a first layer made of piezoelectric yarn is wound spirally in one direction, and a second layer made of piezoelectric yarn is wound spirally in the same direction as the first layer. In one embodiment of the piezoelectric substrate, the piezoelectric yarn includes a first piezoelectric yarn that is helically wound in one direction and a second piezoelectric yarn that is helically wound in a direction different from the one direction. In this embodiment, the chirality of the optically active polypeptide contained in the first piezoelectric yarn is different from the chirality of the optically active polypeptide contained in the second piezoelectric yarn.
[0024] The helix angle is preferably from 20° to 70°, more preferably from 25° to 65°, and further preferably from 30° to 60°. The "helical angle" refers to the angle between the axial direction of the internal conductor and the longitudinal direction of the piezoelectric yarn. When the piezoelectric substrate has an external conductor, which will be described later, the method for measuring the helical angle is to remove the external conductor from the piezoelectric substrate, then place the piezoelectric layer straight in the axial direction of the internal conductor, photograph it with an optical microscope, and measure the angle of the piezoelectric yarn relative to the axial direction of the internal conductor at five points using image processing, excluding any extremely misaligned points, and calculate the average value.
[0025] (1.1.1.1) Piezoelectric yarn The piezoelectric yarn includes an optically active polypeptide fiber. "Optical active polypeptide fiber" refers to a fiber made of an optically active polypeptide. The inclusion of an optically active polypeptide in the piezoelectric yarn contributes to the expression of piezoelectricity in the piezoelectric substrate.
[0026] The piezoelectric yarn may be a twisted yarn or a non-twisted yarn. In particular, the piezoelectric yarn is preferably a twisted yarn from the viewpoint of piezoelectricity. Examples of the non-twisted yarn include a single original yarn (fiber) and an aggregate of multiple original yarns (fibers). The number of original yarns (fibers) constituting the twisted yarn is not particularly limited, and is preferably 3 to 120, and more preferably 4 to 30, from the viewpoint of ensuring the strength of the piezoelectric yarn. The raw yarn (fiber) constituting the twisted yarn may contain fibers other than optically active polypeptide fibers, so long as it contains at least one optically active polypeptide fiber. In particular, from the viewpoint of improving the piezoelectric sensitivity of the piezoelectric substrate, it is preferable that the raw yarn (fiber) constituting the twisted yarn is composed only of a plurality of optically active polypeptide fibers.
[0027] Each of the piezoelectric yarns includes a plurality of optically active polypeptide fibers, and the twist number of each of the piezoelectric yarns is preferably 500 T / m or less, more preferably 300 T / m or less. When the twist number of each of the piezoelectric yarns is within this range, the piezoelectric yarn is less likely to break, and the piezoelectric sensitivity of the piezoelectric substrate is superior.
[0028] The thickness of the piezoelectric yarn (when the piezoelectric yarn is an assembly of multiple fibers, the thickness of the entire assembly) is not particularly limited, and is preferably 0.0001 mm to 2 mm, more preferably 0.001 mm to 1 mm, and even more preferably 0.005 mm to 0.8 mm. When the piezoelectric yarn is a single original yarn or an assembly of multiple original yarns, the fineness of each original yarn is preferably 0.01 denier to 10,000 denier, more preferably 0.1 denier to 1,000 denier, and even more preferably 1 denier to 100 denier.
[0029] (1.1.1.1.1) Optically active polypeptide fibers The optically active polypeptide fiber is preferably a long fiber, which allows the shear stress applied to the piezoelectric substrate to be more easily transmitted to the piezoelectric substrate than when the optically active polypeptide fiber is a short fiber, thereby improving the piezoelectric sensitivity of the piezoelectric substrate. In the present disclosure, the term "long fiber" refers to a fiber having a length that allows it to be wound continuously from one end to the other end in the length direction of a piezoelectric substrate. Silk (silk thread), wool, mohair, cashmere, camel, llama, alpaca, vicuna, angora, and spider silk are all long fibers. Among the long fibers, silk and spider silk are preferred from the viewpoint of piezoelectricity.
[0030] The degree of orientation F of the optically active polypeptide fiber is preferably within the range of 0.50 or more and less than 1.00. When the degree of orientation F of the optically active polypeptide fiber is 0.50 or more, it contributes to the expression of piezoelectricity in the piezoelectric substrate.When the degree of orientation F of the optically active polypeptide fiber is less than 1.00, it contributes to the productivity of the piezoelectric substrate. The degree of orientation F of the optically active polypeptide fiber is preferably 0.50 or more and 0.99 or less, more preferably 0.70 or more and 0.98 or less, and even more preferably 0.80 or more and 0.97 or less. An orientation degree F of an optically active polypeptide fiber of 1.00 indicates that the main orientation direction of the optically active polypeptide contained in the optically active polypeptide fiber is parallel to the length direction of the optically active polypeptide fiber. Furthermore, an orientation degree F of an optically active polypeptide fiber of 0.80 or more and less than 1.00 indicates that the main orientation direction of the optically active polypeptide contained in the optically active polypeptide fiber is approximately parallel to the length direction of the optically active polypeptide fiber. The degree of orientation F of an optically active polypeptide fiber is determined by stacking the piezoelectric yarn as a reference axis and fixing the sample to a sample holder, measuring the azimuth angle distribution intensity near the peak due to orientation, for example, in the case of silk, near 2θ=20°, from X-ray diffraction measurement, and calculating the value according to the following formula (a), which means the degree of c-axis orientation. Orientation degree F=(180°-α) / 180° … Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.]
[0031] It is preferable that the length direction of the piezoelectric yarn and the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn are approximately parallel. The longitudinal direction of the piezoelectric yarn and the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn being approximately parallel contribute to the expression of piezoelectricity in the piezoelectric substrate. The fact that the length direction of the piezoelectric yarn is approximately parallel to the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn indicates that the piezoelectric yarn has excellent tensile strength in the length direction, and therefore is less likely to break when wound in a spiral shape. When the piezoelectric yarn is silk or spider silk, during the production process of the silk or spider silk, the length direction of the piezoelectric yarn (silk or spider silk) and the main orientation direction of the optically active polypeptide (e.g., fibroin or spider silk protein) contained in the piezoelectric yarn are approximately parallel. The fact that the longitudinal direction of the piezoelectric yarn and the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn are approximately parallel can be confirmed by comparing the installation direction of the sample (piezoelectric yarn) and the azimuth angle of the crystal peak in X-ray diffraction measurements. Examples of methods for making the length direction of the piezoelectric yarn approximately parallel to the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn include a method of using a twisted yarn containing a plurality of specific optically active polypeptide fibers as the piezoelectric yarn. The specific optically active polypeptide fiber refers to an optically active polypeptide fiber having an orientation degree F of the optically active polypeptide fiber of 0.80 or more and less than 1.00.
[0032] From the viewpoint of the piezoelectricity and strength of the piezoelectric yarn, it is preferable that the optically active polypeptide has a β-sheet structure.
[0033] Examples of optically active polypeptides having a β-sheet structure include optically active animal proteins and optically active synthetic proteins. Examples of optically active animal proteins include fibroin, spider silk protein, sericin, collagen, keratin, elastin, etc. As the spider silk protein, the spider silk protein described in Patent Document 1 can be used. As the spider silk protein, artificial spider silk obtained by an artificial synthesis method can be used. In particular, the optically active polypeptide preferably contains at least one of fibroin and spider silk protein, and more preferably contains fibroin. Examples of synthetic proteins having optical activity include synthetic spider silk (e.g., "QMONOS (registered trademark)", synthetic bagworm silk, synthetic proteins (e.g., "Brewed Protein (registered trademark)", etc.). The form of the synthetic protein having optical activity is preferably thread-like. Thread-like fibers containing the above synthetic proteins can also be obtained from threads or clothing containing "Brewed Protein (registered trademark)".
[0034] Examples of optically active polypeptide fibers having a β-sheet structure include fibers made of animal proteins having optical activity, such as silk, wool, mohair, cashmere, camel, llama, alpaca, vicuna, angora, and spider silk. Among these, from the viewpoint of piezoelectricity, the optically active polypeptide fiber preferably contains at least one of silk and spider silk, more preferably consists of at least one of silk and spider silk, and particularly preferably consists of silk.
[0035] Examples of silk include raw silk, refined silk, regenerated silk, and fluorescent silk. As the silk, raw silk or refined silk is preferred, and refined silk is particularly preferred. "Refined silk" refers to silk that has had sericin removed from raw silk, which has a double structure of sericin and fibroin. "Refining" refers to the process of removing sericin from raw silk. Raw silk is a dull white color, but by removing sericin from raw silk (i.e., refining), the color changes from dull white to a lustrous silvery white. Refining also enhances the silk's soft texture.
[0036] (1.1.1.2) Adhesive part The adhesive portion holds the piezoelectric yarn wrapped around the inner conductor. This makes it easier for shear stress caused by external stress to act on the piezoelectric yarn when external stress is applied to the piezoelectric substrate.
[0037] The adhesive portion may cover the entire exposed surface of the piezoelectric yarn, or may cover only a portion of the exposed surface of the piezoelectric yarn. In particular, from the viewpoint of improving the piezoelectric sensitivity of the piezoelectric substrate, it is preferable that the adhesive portion covers only a portion of the exposed surface of the piezoelectric yarn.
[0038] The adhesive portion is preferably made of at least one selected from an epoxy-based adhesive, a urethane-based adhesive, a vinyl acetate resin-based emulsion type adhesive, an ethylene vinyl acetate-based emulsion type adhesive, an acrylic resin-based emulsion type adhesive, a styrene butadiene rubber-based latex type adhesive, a silicone resin-based adhesive, an α-olefin-based adhesive, a vinyl chloride resin-based solvent type adhesive, a rubber-based adhesive, an elastic adhesive, a chloroprene rubber-based solvent type adhesive, a nitrile rubber-based solvent type adhesive, and a cyanoacrylate-based adhesive. Hereinafter, the material of the adhesive joint may be referred to as a "binding agent."
[0039] It is preferable that the surface of the adhesive portion is free of irregularities. If the surface of the adhesive portion is free of irregularities, for example, when the external conductor is formed by winding a long conductor (described later) on the outer peripheral surface of the piezoelectric layer, the occurrence of irregular winding of the long conductor can be suppressed. In other words, if the surface of the adhesive portion is free of irregularities, the yield of the winding process of the long conductor is improved. Furthermore, the occurrence of a decrease in piezoelectric sensitivity caused by irregular winding of the long conductor can be suppressed. Methods for preventing unevenness from forming on the surface of the adhesive joint include, for example, wiping off excess binder from the piezoelectric yarn wound around the internal conductor before the binder hardens, and using an adhesive containing a large amount of solvent as a binder. An adhesive containing a large amount of solvent refers to an adhesive whose resin component (solid content) content is 60 mass% or less of the total amount of adhesive.
[0040] (1.1.2) Inner conductor The piezoelectric substrate according to the first aspect of the present disclosure includes an elongated internal conductor. The inner conductor functions as the core of the piezoelectric substrate. The internal conductor is preferably an electrically good conductor, such as copper wire, aluminum wire, SUS (Steel Use Stainless) wire, metal wire coated with an insulating film, carbon fiber, resin fiber integrated with carbon fiber, tinsel wire, organic conductive material, etc. The tinsel wire is formed by spirally winding copper foil around a fiber. The outer diameter of the fiber is appropriately adjusted according to the desired characteristics of the piezoelectric substrate, and is preferably 0.1 mm or more and 10 mm or less. Among these, the internal conductor is preferably made of tinsel wire or carbon fiber from the viewpoints of improving the piezoelectric sensitivity and stability of the piezoelectric output and imparting high flexibility, and in particular, tinsel wire is preferable from the viewpoint of low electrical resistance.
[0041] (1.1.3) Outer conductor From the viewpoint of improving piezoelectric sensitivity and electrostatic shielding properties, the piezoelectric substrate according to the first embodiment of the present disclosure preferably further includes an external conductor. The outer conductor is disposed on the outer periphery of the piezoelectric layer, and the inner conductor and the outer conductor are not electrically connected to each other.
[0042] The outer conductor serves as a companion conductor to the inner conductor, for example, to detect electrical signals from the piezoelectric substrate. The external conductor may cover at least a portion of the piezoelectric layer. More specifically, the external conductor may cover a portion of the outer circumferential surface of the piezoelectric layer, or may cover the entire outer circumferential surface of the piezoelectric layer.
[0043] The external conductor may or may not be fixed to the piezoelectric layer. "The external conductor is fixed to the piezoelectric layer" means that the external conductor and the piezoelectric layer are mechanically integrated using a known adhesive. In particular, it is preferable that the external conductor is not fixed to the piezoelectric layer. This allows the external conductor to be easily removed from the piezoelectric layer when preparing the piezoelectric substrate for terminal attachment. At this time, the piezoelectric layer is not mechanically integrated with the external conductor, and is therefore less likely to be damaged. As a result, the piezoelectric substrate allows for more efficient preparation of the piezoelectric substrate for terminal attachment. Furthermore, the external conductor is displaceable in the axial direction of the internal conductor relative to the piezoelectric layer. As a result, when an external stress acts on the piezoelectric substrate, the piezoelectric substrate is more easily deformed than a conventional piezoelectric substrate. Therefore, the internal stress of the piezoelectric substrate caused by the action of the external stress is less likely to be concentrated locally. As a result, the durability of the piezoelectric substrate is superior.
[0044] The outer conductor is formed, for example, by winding a long conductor. The cross-sectional shape of the long-sized conductor may be, for example, a circular shape, an elliptical shape, a rectangular shape, an irregular shape, etc. Among these, from the viewpoint of closely adhering to the piezoelectric substrate in a plane and improving the piezoelectric sensitivity of the piezoelectric substrate, the cross-sectional shape of the long-sized conductor is preferably a rectangular shape. The material of the long conductor is not particularly limited, and the following are main examples depending on the cross-sectional shape: Examples of long conductors having a rectangular cross section include copper foil ribbons and aluminum foil ribbons which are formed by rolling copper wires having a circular cross section into a flat plate. Examples of long conductors having a circular cross section include copper wire, aluminum wire, SUS wire, metal wire coated with an insulating film, carbon fiber, resin fiber integrated with carbon fiber, and tinsel wire in which copper foil is spirally wound around fiber. The long conductor may be an organic conductive material coated with an insulating material. Methods for winding a long conductor include, for example, a method of spirally winding copper foil or the like around a piezoelectric substrate, a method of braiding copper wire or the like into a tubular shape and wrapping the piezoelectric substrate, and a method of enclosing the piezoelectric substrate in a cylindrical shape.
[0045] (1.1.4) Electrical insulator The piezoelectric substrate according to the first aspect of the present disclosure may further include an electrical insulator (hereinafter referred to as a "first insulator"). The first insulator is disposed on the outermost periphery of the piezoelectric substrate. In other words, at least a portion of the outer periphery of the piezoelectric substrate is constituted by the first insulator. It is preferable that the first insulator covers the entire outermost periphery of the piezoelectric substrate. In other words, it is preferable that the entire outer periphery of the piezoelectric substrate is composed of the first insulator. This makes it possible to electrostatically shield the internal conductor. As a result, the change in piezoelectric sensitivity caused by external static electricity can be suppressed. The first insulator is formed, for example, by winding a long piece in a spiral shape around the outer circumferential surface of the outer conductor. The material for the first insulator may be any material having electrical insulation properties, such as polyvinyl chloride resin, polyethylene resin, polypropylene resin, ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene resin (PTFE), tetrafluoroethylene-perfluoropropyl vinyl ether copolymer (PFA), fluororubber, polyester resin, polyimide resin, polyamide resin, polyethylene terephthalate resin (PET), rubber (including elastomer), etc.
[0046] When the piezoelectric substrate according to the first embodiment of the present disclosure includes an outer conductor, the first insulator may or may not be fixed to the outer conductor. The phrase "the first insulator is fixed to the outer conductor" means that the first insulator and the outer conductor are mechanically integrated with each other using a known adhesive. In particular, it is preferable that the first insulator is not fixed to the external conductor. This allows the first insulator to be easily removed from the external conductor when preparing the piezoelectric substrate for terminal attachment. At this time, the external conductor is not easily damaged because it is not mechanically integrated with the first insulator. As a result, the piezoelectric substrate allows more efficient preparation for terminal attachment of the piezoelectric substrate. Furthermore, the first insulator is displaceable in the axial direction of the inner conductor relative to the outer conductor. This allows the piezoelectric substrate to be deformed more easily than conventional piezoelectric substrates when an external stress acts on the piezoelectric substrate. Therefore, the internal stress of the piezoelectric substrate caused by the action of the external stress is less likely to be concentrated locally. As a result, the durability of the piezoelectric substrate is superior.
[0047] (1.1.5) Inner electrical insulation When the piezoelectric substrate according to the first embodiment of the present disclosure includes an outer conductor, the piezoelectric substrate may further include an inner electrical insulator (hereinafter, referred to as a "second insulator") disposed, for example, between the piezoelectric layer and the inner conductor and / or between the piezoelectric layer and the outer conductor. This can further prevent the occurrence of a short circuit between the inner conductor and the outer conductor. The second insulator is, for example, a long piece wound in a spiral shape around the outer circumferential surface of the inner conductor. Examples of materials for the second insulator include the same materials as those exemplified as the materials for the first insulator.
[0048] The second insulator may or may not be fixed to at least one of the internal conductor, the piezoelectric layer, and the external conductor (hereinafter referred to as the "internal conductor, etc."). "The second insulator is fixed to the internal conductor, etc." means that the second insulator and the internal conductor, etc. are mechanically integrated using a known adhesive. In particular, it is preferable that the second insulator is not fixed to the external conductor from the viewpoint of enabling more efficient preparation for terminal attachment of the piezoelectric substrate.
[0049] (1.1.6) Functional Layer The piezoelectric substrate of the first embodiment of the present disclosure may further include a functional layer. When the piezoelectric substrate does not include an external conductor, the functional layer is disposed between the piezoelectric layer and the internal conductor. When the piezoelectric substrate of the first embodiment of the present disclosure includes an external conductor, the functional layer is disposed at least one of between the piezoelectric layer and the internal conductor and between the piezoelectric layer and the external conductor. Examples of layers constituting the functional layer (hereinafter referred to as "constituent layers") include an easy-adhesion layer, a hard coat layer, a refractive index adjusting layer, an anti-reflection layer, an anti-glare layer, an easy-slip layer, an anti-blocking layer, a protective layer, an antistatic layer, a heat dissipation layer, an ultraviolet absorbing layer, an anti-Newton ring layer, a light scattering layer, a polarizing layer, a gas barrier layer, a hue adjusting layer, and an electrode layer. The functional layer may be a single-layer structure consisting of a single constituent layer, or may be a multiple-layer structure consisting of two or more constituent layers. When the functional layer has a multiple-layer structure, each of the multiple constituent layers may be the same or different. When the piezoelectric substrate has a functional layer between the piezoelectric layer and the internal conductor and between the piezoelectric layer and the external conductor, the functional layer between the piezoelectric layer and the internal conductor and the functional layer between the piezoelectric layer and the external conductor may be the same or different. The thickness of the functional layer is not particularly limited, but is preferably within the range of 0.01 μm or more and 10 μm or less. The material of the functional layer is appropriately selected depending on the function required for the functional layer, and examples thereof include inorganic substances such as metals and metal oxides, organic substances such as resins, composite compositions containing resins and fine particles, etc. Examples of the resin include cured products obtained by curing with temperature or active energy rays.
[0050] The functional layer may or may not be fixed to the internal conductor, etc. "The functional layer is fixed to the internal conductor, etc." means that the second insulator and the internal conductor, etc. are mechanically integrated using a known adhesive. In particular, it is preferable that the functional layer is not fixed to the external conductor from the viewpoint of enabling more efficient preparation for terminal attachment of the piezoelectric substrate.
[0051] Specific examples of the piezoelectric substrate according to the first embodiment will be described below with reference to the drawings, but the piezoelectric substrate according to the first embodiment of the present disclosure is not limited to the following specific examples. In addition, substantially the same elements are given the same symbols throughout the drawings and descriptions thereof will not be repeated.
[0052] (1.1.7) Piezoelectric substrate according to the first embodiment of the first aspect A piezoelectric substrate 10A according to a first embodiment of the first aspect will be described with reference to Figures 1A to 1D. Figure 1A is a schematic side view showing the appearance of the piezoelectric substrate 10A according to the first embodiment of the first aspect of the present disclosure. Figure 1B is a cross-sectional view taken along line IB-IB of Figure 1A.
[0053] As shown in Fig. 1A, the piezoelectric substrate 10A according to the first embodiment of the first aspect includes an elongated internal conductor 12A and a piezoelectric layer 14A. The piezoelectric layer 14A is spirally wound in one direction along the outer circumferential surface of the internal conductor 12A from one end to the other end at a helix angle β1 without any gaps. The piezoelectric layer 14A is not fixed to the internal conductor 12A. The piezoelectric layer 14A is formed by winding the piezoelectric yarn 140A counterclockwise around the outer peripheral surface of the internal conductor 12A, and holding the state in which the piezoelectric yarn 140A is wound around the internal conductor 12A with an adhesive portion (not shown). Specifically, when the piezoelectric substrate 10A is viewed from one end side (the right end side in FIG. 1A) in the axial direction of the internal conductor 12A, the piezoelectric yarn 140A is wound counterclockwise from the front side to the back side of the internal conductor 12A. The piezoelectric yarn 140A includes an optically active polypeptide fiber. The helix angle β1 is the angle between the direction of the helix axis G1 (the axial direction of the internal conductor 12A) and the length direction of the piezoelectric yarn 140A in a side view. The elastic modulus Y (GPa) of the piezoelectric layer 14A is not less than 1.0 GPa and not more than 8.0 GPa. This provides the piezoelectric substrate 10A with excellent piezoelectric sensitivity. 1A, the double-headed arrow E1 indicates the main orientation direction of the optically active polypeptide contained in the piezoelectric layer 14A. That is, in the first embodiment of the first aspect, the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn 140A and the length direction of the piezoelectric yarn 140A are approximately parallel to each other.
[0054] The effects of the piezoelectric substrate 10A will be described below. For example, when tension is applied in the longitudinal direction of the piezoelectric substrate 10A, a shear stress is applied to the optically active polypeptide contained in the piezoelectric layer 14A, and the optically active polypeptide is polarized. The polarization of the optically active polypeptide is considered to occur in phase with each other in the radial direction of the piezoelectric substrate 10A, as shown by the arrows in FIG. 1B. This causes the piezoelectricity of the piezoelectric substrate 10A to be expressed. The piezoelectric substrate 10A has excellent piezoelectric sensitivity.
[0055] (1.1.8) Piezoelectric substrate according to the second embodiment of the first aspect A piezoelectric substrate 20A according to a second embodiment of the first aspect will be described with reference to Fig. 2. Fig. 2 is a schematic side view showing the external appearance of the piezoelectric substrate 20A according to the second embodiment of the first aspect.
[0056] The piezoelectric substrate 20A according to the second embodiment of the first aspect differs from the piezoelectric substrate 10A according to the first embodiment of the first aspect in that it includes an external conductor 22A. As shown in FIG. 2, the piezoelectric substrate 20A according to the second embodiment of the first aspect includes an internal conductor 12A, a piezoelectric layer 14A, and an external conductor 22A. The external conductor 22A is disposed on the outer periphery side of the piezoelectric layer 14A. The external conductor 22A is formed by winding a copper foil ribbon in a spiral shape around (on the outer periphery of the piezoelectric layer 14A) a piezoelectric thread 140A that is wound in a spiral shape around (on the outer periphery of) the internal conductor 12A. The internal conductor 12A and the external conductor 22A are not electrically connected. As shown in Fig. 2, in the second embodiment of the first aspect, the end of the piezoelectric layer 14A (i.e., the helically wound piezoelectric yarn 140A) and the end of the external conductor 22A are misaligned in side view. This ensures that the internal conductor 12A and the external conductor 22A are insulated from each other. However, the positions of these ends do not necessarily need to be misaligned, and as long as the internal conductor 12A and the external conductor 22A are electrically insulated from each other, the positions of these ends may overlap in side view.
[0057] The piezoelectric substrate 20A provides the same effects as the piezoelectric substrate 10A. Furthermore, since the piezoelectric substrate 20A includes the internal conductor 12A, an electrical signal (voltage signal or charge signal) generated in the piezoelectric layer 14A can be more easily extracted via the internal conductor 12A. Furthermore, since the piezoelectric substrate 20A includes the external conductor 22A, the inside of the piezoelectric substrate 20A (the piezoelectric layer 14A and the internal conductor 12A) can be electrostatically shielded by the external conductor 22A. This makes it possible to suppress voltage changes in the internal conductor 12A caused by static electricity outside the piezoelectric substrate 20A, resulting in more stable piezoelectricity.
[0058] (1.1.9) Applications of piezoelectric substrates Applications of the piezoelectric substrate according to the first embodiment of the present disclosure are not particularly limited, and examples thereof include force sensors, pressure sensors, displacement sensors, deformation sensors, motion sensors, vibration sensors, impact sensors, ultrasonic sensors, actuators, and energy harvesters. The use of the piezoelectric substrate according to the first aspect of the present disclosure is the same as the use of the piezoelectric substrate described in Patent Document 1.
[0059] (1.2) Sensors The sensor of the first aspect of the disclosure comprises a piezoelectric substrate of the first aspect of the disclosure. The sensor according to the first embodiment of the present disclosure includes the piezoelectric substrate according to the first embodiment of the present disclosure, and therefore has excellent piezoelectric sensitivity. The sensors according to the first aspect of the present disclosure include force sensors, pressure sensors, displacement sensors, deformation sensors, motion sensors, vibration sensors, impact sensors, ultrasonic sensors, and the like.
[0060] (1.3) Actuator The actuator of the first aspect of the present disclosure comprises the piezoelectric substrate of the first aspect of the present disclosure. The actuator according to the first embodiment of the present disclosure includes the piezoelectric substrate according to the first embodiment of the present disclosure, and therefore has excellent piezoelectric sensitivity.
[0061] (1.4) Biometric information acquisition device The bioinformation acquisition device according to the first aspect of the present disclosure includes the piezoelectric substrate according to the first aspect of the present disclosure. The bioinformation acquisition device of the first embodiment of the present disclosure acquires bioinformation of a subject by detecting a biosignal of a subject or test animal (hereinafter collectively referred to as "subject") using the piezoelectric substrate of the first embodiment of the present disclosure. Examples of biosignals include presence / absence, body movement, pulse wave signal (heart rate signal), respiratory signal, body movement signal, ballistocardiogram, biotremor, etc. Biotremor is a rhythmic involuntary movement of a body part (fingers, hand, forearm, upper limb, etc.). Ballistocardiogram detection also includes detection of the force effect due to the cardiac function of the body. That is, when the heart pumps blood into the aorta and pulmonary artery, the body experiences a recoil force in the opposite direction to the blood flow. The magnitude and direction of this recoil force change with the functional stage of the heart. This recoil force is detected by sensing the ballistocardiogram outside the body. The article in which the biometric information acquisition device according to the first embodiment of the present disclosure is disposed is similar to the article in which the biometric information acquisition device described in Patent Document 1 is disposed. The biometric information acquisition device of the first aspect of the present disclosure may be embedded in a seat, a steering wheel, a seat, a seat belt, a shift knob, an armrest, a headrest, a handle, or the like, or in clothing, a hat, or the like worn by the driver. The biometric information acquisition device of the first aspect of the present disclosure is suitably used as a detection unit of an information processing device. The information processing device acquires a biometric signal of the subject from the biometric information acquisition device of the first aspect of the present disclosure, and detects abnormalities, abnormal physical conditions, etc. of the subject based on the acquired biometric signal using artificial intelligence (AI). The AI includes a trained model.
[0062] (2) Second mode (2.1) Piezoelectric substrate The piezoelectric substrate according to the second aspect of the present disclosure includes a long internal conductor and a piezoelectric layer covering the outer peripheral surface of the internal conductor. The piezoelectric layer is formed by winding a long piezoelectric body around the internal conductor and is not fixed to the internal conductor. The long piezoelectric body has a plurality of piezoelectric yarns and a bundle that bundles the plurality of piezoelectric yarns. At least one of the plurality of piezoelectric yarns includes an optically active polypeptide fiber that is a fiber made of an optically active polypeptide. It is preferable that the length direction of the long piezoelectric body and the main orientation direction of the optically active polypeptide are approximately parallel to each other. The degree of orientation F of the optically active polypeptide fiber, which is determined by the following formula (a) from X-ray diffraction measurement, is preferably 0.50 or more and less than 1.00. Orientation degree F=(180°-α) / 180° … Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.]
[0063] In this disclosure, "not fixed to the internal conductor" means that the piezoelectric layer is not mechanically integrated with the internal conductor by an adhesive or the like. The terms "piezoelectric yarn," "optically active polypeptide," and "substantially parallel" in the second embodiment are the same as in the first embodiment. In the present disclosure, the orientation degree F of the optically active polypeptide fiber is an index showing the degree of orientation of the optically active polypeptide contained in the piezoelectric yarn.
[0064] The piezoelectric substrate according to the second embodiment of the present disclosure has the above-mentioned configuration, and therefore allows for more efficient preparation for terminal attachment and has superior piezoelectric sensitivity compared to conventional piezoelectric substrates such as those described in Patent Document 1.
[0065] (2.1.1) Piezoelectric layer A piezoelectric substrate according to a second aspect of the present disclosure includes a piezoelectric layer.
[0066] The piezoelectric layer covers the outer circumferential surface of the internal conductor, and preferably covers the entire outer circumferential surface of the internal conductor.
[0067] The thickness of the piezoelectric layer is not particularly limited, but is preferably 0.02 mm to 2.00 mm, more preferably 0.05 mm to 0.50 mm. From the viewpoint of improving the piezoelectric sensitivity of the piezoelectric substrate, the thickness of the piezoelectric layer is preferably the same as the thickness of the long piezoelectric element.
[0068] The piezoelectric layer is not fixed to the internal conductor. This allows the piezoelectric layer to be more easily removed from the internal conductor when preparing the piezoelectric substrate for terminal attachment than in a configuration in which the piezoelectric layer and the internal conductor are mechanically integrated. In this case, the internal conductor is less likely to be damaged because it is not mechanically integrated with the piezoelectric layer. As a result, the piezoelectric substrate allows efficient preparation for terminal attachment of the piezoelectric substrate. Furthermore, the piezoelectric layer is displaceable relative to the internal conductor in the axial direction of the internal conductor. This allows the piezoelectric substrate to be more easily deformed than conventional piezoelectric substrates when an external stress acts on the piezoelectric substrate. Therefore, the internal stress of the piezoelectric substrate caused by the action of the external stress is less likely to concentrate locally. As a result, the durability of the piezoelectric substrate is superior to that of conventional piezoelectric substrates.
[0069] The piezoelectric layer is formed by winding a long piezoelectric element around an internal conductor. The long piezoelectric element may be wound directly around the outer circumferential surface of the internal conductor. When an inner electrical insulator, which will be described later, is disposed on the outer circumferential surface of the internal conductor, the long piezoelectric element may be wound indirectly around the internal conductor by being wound around the outer circumferential surface of the inner electrical insulator. The long piezoelectric element wound around the outer peripheral surface of the internal conductor may be mechanically integrated as long as the piezoelectric layer is not fixed to the internal conductor. This improves the mechanical strength of the piezoelectric layer. For example, a method for mechanically integrating the long piezoelectric element wound around the outer peripheral surface of the internal conductor includes a method of applying a known adhesive to the surface of the long piezoelectric element wound around the outer peripheral surface of the internal conductor opposite the internal conductor, and then fixing and bonding the long piezoelectric element wound around the outer peripheral surface of the internal conductor.
[0070] The way in which the long piezoelectric body is wound is not particularly limited, and the long piezoelectric body may be wound helically around the internal conductor in the axial direction of the internal conductor, or may not be wound helically around the internal conductor in the axial direction of the internal conductor. In particular, from the viewpoint of improving the piezoelectric sensitivity of the piezoelectric substrate, the way in which the long piezoelectric body is wound is preferably such that the long piezoelectric body is wound helically around the internal conductor in the axial direction of the internal conductor. The long piezoelectric body may be wound so as to overlap, or may be wound so as not to overlap. In the piezoelectric substrate according to the second embodiment of the present disclosure, when a shear stress is applied to the helically wound long piezoelectric element, electric charges are easily generated, which makes it easier for the piezoelectricity to be exhibited. The shear stress can be applied to the long piezoelectric element by, for example, a first non-plastic deformation, a second non-plastic deformation, or a third non-plastic deformation. The first non-plastic deformation refers to the entirety of the helically wound long piezoelectric element being stretched in the direction of the helical axis. The second non-plastic deformation refers to twisting a part of the long piezoelectric element that is wound in a spiral shape (that is, twisting a part of the long piezoelectric element around the spiral axis). The third non-plastic deformation refers to bending a part or the whole of the helically wound long piezoelectric element.
[0071] The long piezoelectric element is preferably wound spirally in one direction around the internal conductor. The term "spirally wound in one direction" in the second embodiment is the same as in the first embodiment. When the long piezoelectric element is wound in a spiral shape in one direction, the phenomenon in which the polarities of the generated electric charges cancel each other out (i.e., the phenomenon in which the piezoelectricity decreases) is suppressed, and therefore the piezoelectricity of the piezoelectric substrate is further improved.
[0072] The embodiment having a long piezoelectric body in which a piezoelectric substrate is spirally wound in one direction includes not only an embodiment having only one layer of long piezoelectric body, but also an embodiment in which multiple layers of long piezoelectric body are stacked on top of each other. An example of an embodiment in which multiple layers made of long-sized piezoelectric material are stacked on top of each other is an embodiment in which a first layer made of long-sized piezoelectric material is spirally wound in one direction, and then a second layer made of long-sized piezoelectric material is stacked on top of the first layer made of long-sized piezoelectric material and spirally wound in the same direction as the first direction. An example of the piezoelectric substrate is one in which the long piezoelectric body includes a first long piezoelectric body that is spirally wound in one direction and a second long piezoelectric body that is spirally wound in a direction different from the first direction. In this example, the chirality of the optically active polypeptide contained in the first long piezoelectric body is different from the chirality of the optically active polypeptide contained in the second long piezoelectric body.
[0073] The helix angle is preferably from 20° to 70°, more preferably from 25° to 65°, and further preferably from 30° to 60°. The term "helical angle" and the method for measuring the helix angle in the second embodiment are the same as in the first embodiment.
[0074] (2.1.1.1) Long piezoelectric body The long piezoelectric body has a plurality of piezoelectric yarns and a bundle. The bundle bundles the plurality of piezoelectric yarns. Each of the plurality of piezoelectric yarns bundled in the bundle may be aligned or random. For example, the plurality of piezoelectric yarns may be bundled in the bundle by intentionally manipulating the bundle so that the length direction of each of the plurality of piezoelectric yarns is in one direction, or the plurality of piezoelectric yarns may be bundled in the bundle randomly.
[0075] The elastic modulus Y of the long piezoelectric body is preferably 1 GPa or more and 10 GPa or less. In order for shear stress to act effectively on the piezoelectric yarn when the piezoelectric layer is deformed in the tensile direction, the bundle must have a rigidity that makes it less susceptible to deformation than the piezoelectric yarn. If the elastic modulus Y of the long piezoelectric body is within the above range, stress is more likely to be effectively transmitted to the piezoelectric yarn when external stress is applied to the piezoelectric layer. In other words, if the elastic modulus of the long piezoelectric body is within the above range, the piezoelectric sensitivity of the piezoelectric substrate is improved. Furthermore, the durability of the piezoelectric substrate is superior, and the piezoelectric substrate allows for more efficient preparation for terminal attachment. The elastic modulus Y of the long piezoelectric body is more preferably 1 GPa or more and 10 GPa or less, and further preferably 2 GPa or more and 10 GPa or less, from the viewpoints of the piezoelectric sensitivity of the piezoelectric substrate and the winding processability of the long piezoelectric body. The elastic modulus Y of the long piezoelectric body is measured by a microhardness meter (based on JIS Z 2255). The measurement environment for the microhardness meter measurement (based on JIS Z 2255) is a temperature of 23±2°C and a humidity of 50±5°C.
[0076] The shape of the long piezoelectric element may be, for example, a ribbon shape. The "ribbon shape" refers to a flat, elongated shape. The size of the long piezoelectric element is not particularly limited. It is preferable that the thickness of the long piezoelectric element is 0.001 mm to 0.4 mm, the width of the long piezoelectric element is 0.1 mm to 30 mm, and the ratio of the width to the thickness of the long piezoelectric element is 2 or more. From the viewpoints of the piezoelectric sensitivity and mechanical strength of the piezoelectric substrate, the thickness of the long piezoelectric element is more preferably 0.02 mm to 0.4 mm, and further preferably 0.05 mm to 0.2 mm. From the viewpoints of the piezoelectric sensitivity of the piezoelectric substrate and thinning of the piezoelectric substrate, the width of the long piezoelectric element is more preferably 0.1 mm to 5.0 mm, and further preferably 0.4 mm to 1.0 mm. The ratio of the width of the long piezoelectric element to the thickness is more preferably 2 to 20, and further preferably 3 to 10, from the viewpoints of the piezoelectric sensitivity of the piezoelectric substrate and thinning of the piezoelectric substrate.
[0077] In the long piezoelectric element, the positional relationship between the piezoelectric yarns and the bundling body is not particularly limited, but it is preferable that the bundling body bundles the piezoelectric yarns in a state in which the piezoelectric yarns are arranged in parallel along a direction perpendicular to the length direction of the piezoelectric yarns and adjacent piezoelectric yarns among the piezoelectric yarns are in contact with each other. In other words, it is preferable that the arrangement state of the piezoelectric yarns is maintained in a predetermined state by the bundling body. The predetermined state refers to a state in which the piezoelectric yarns are arranged in parallel along a direction perpendicular to the length direction of the piezoelectric yarns and adjacent piezoelectric yarns among the piezoelectric yarns are in contact with each other. This improves the piezoelectric sensitivity of the piezoelectric substrate.
[0078] The number of piezoelectric yarns is appropriately selected depending on the application of the piezoelectric substrate, and is preferably 2 to 20, and more preferably 2 to 8, from the viewpoint of processability. Alternatively, the long piezoelectric element may be produced by slitting a long piezoelectric element precursor obtained by producing a wide width.
[0079] (2.1.1.1.1) Piezoelectric Yarn At least one of the plurality of piezoelectric yarns includes an optically active polypeptide fiber. The inclusion of the optically active polypeptide in the piezoelectric yarn contributes to the expression of piezoelectricity of the piezoelectric substrate. The piezoelectric yarn of the second embodiment is similar to the piezoelectric yarn of the first embodiment.
[0080] Each of the piezoelectric yarns includes a plurality of optically active polypeptide fibers, and the twist number of each of the piezoelectric yarns is preferably 500 T / m or less, more preferably 300 T / m or less. When the twist number of each of the piezoelectric yarns is within this range, the piezoelectric yarn is less likely to break, and the piezoelectric sensitivity of the piezoelectric substrate is superior.
[0081] (2.1.1.1.1.1) Optically active polypeptide fibers The optically active polypeptide fiber of the second embodiment is the same as the example of the optically active polypeptide fiber of the first embodiment.
[0082] The degree of orientation F of the optically active polypeptide fiber is preferably within the range of 0.50 or more and less than 1.00. The technical reasons for setting the degree of orientation F within the above range in the second embodiment, the preferred range of the degree of orientation F, and the method for measuring the degree of orientation F are the same as those in the first embodiment.
[0083] It is preferable that the length direction of the long piezoelectric body and the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn are approximately parallel to each other. The longitudinal direction of the long piezoelectric body and the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn being approximately parallel contribute to the expression of piezoelectric properties of the piezoelectric substrate. The fact that the length direction of the long piezoelectric body and the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn are approximately parallel indicates that the long piezoelectric body has excellent tensile strength in the length direction, and therefore the piezoelectric yarn is less likely to break when the long piezoelectric body is wound in a spiral shape. For example, when the piezoelectric yarn is silk or spider silk, during the process of producing the silk or spider silk, the length direction of the piezoelectric yarn (silk or spider silk) and the main orientation direction of the optically active polypeptide (e.g., fibroin or spider silk protein) contained in the piezoelectric yarn are approximately parallel. The fact that the longitudinal direction of the long piezoelectric body and the main orientation direction of the optically active polypeptide contained in the piezoelectric yarn are approximately parallel can be confirmed by comparing the installation direction of the sample (long piezoelectric body) and the azimuth angle of the crystal peak in X-ray diffraction measurement. An example of a method for making the length direction of a long piezoelectric body and the main orientation direction of an optically active polypeptide contained in a piezoelectric yarn approximately parallel is to arrange multiple specific piezoelectric yarns in parallel along a direction perpendicular to the length direction of the specific piezoelectric yarn when producing a long piezoelectric body. The specific piezoelectric yarn refers to a twisted yarn containing multiple specific optically active polypeptide fibers. The specific optically active polypeptide fiber refers to an optically active polypeptide fiber having an orientation degree F of the optically active polypeptide fiber of 0.80 or more and less than 1.00.
[0084] From the viewpoint of the piezoelectricity and strength of the piezoelectric yarn, it is preferable that the optically active polypeptide has a β-sheet structure.
[0085] The optically active polypeptide preferably contains at least one of fibroin and spider silk protein, and more preferably contains fibroin.
[0086] From the viewpoint of piezoelectricity, the optically active polypeptide fiber preferably contains at least one of silk and spider silk, more preferably consists of at least one of silk and spider silk, and particularly preferably consists of silk.
[0087] As the silk, raw silk or refined silk is preferred, and refined silk is particularly preferred.
[0088] (2.1.1.1.2) Convergence body The bundling body bundles the plurality of piezoelectric yarns, i.e., the bundling body integrates the plurality of piezoelectric yarns. This makes it easier for shear stress caused by external stress to act on the piezoelectric yarn when external stress is applied to the piezoelectric substrate.
[0089] The bundling body is not particularly limited as long as it can bundle a plurality of piezoelectric yarns, and examples of the bundling body include an adhesive body, a shrink film, and the like.
[0090] When a shrink film is used as the bundle, for example, a plurality of piezoelectric yarns are placed in a bag made of the shrink film, and the bag is heated to shrink the bag, thereby obtaining a long piezoelectric element. When an adhesive is used as the bundle, for example, a long piezoelectric body using the adhesive can be obtained by impregnating the piezoelectric yarns with an adhesive and bonding the piezoelectric yarns together. In this case, the adhesive may cover the entire outer circumferential surface of each of the piezoelectric yarns, or may cover a portion of the outer circumferential surface of each of the piezoelectric yarns. In particular, the adhesive may be formed only in the gaps between the outer circumferential surfaces of adjacent piezoelectric yarns that face each other.
[0091] The convergent (i.e., adhesive) is preferably made of at least one selected from the group consisting of epoxy adhesives, urethane adhesives, vinyl acetate resin emulsion adhesives, ethylene vinyl acetate emulsion adhesives, acrylic resin emulsion adhesives, styrene butadiene rubber latex adhesives, silicone resin adhesives, α-olefin adhesives, vinyl chloride resin solvent adhesives, rubber adhesives, elastic adhesives, chloroprene rubber solvent adhesives, nitrile rubber solvent adhesives, and cyanoacrylate adhesives, which allow the piezoelectric yarns to be integrated and function as a piezoelectric layer.
[0092] (2.1.2) Inner conductor The piezoelectric substrate according to the second embodiment of the present disclosure includes an elongated internal conductor. The piezoelectric substrate of the second embodiment is similar to the piezoelectric substrate exemplified in the first embodiment.
[0093] (2.1.3) Outer conductor The piezoelectric substrate according to the second aspect of the present disclosure may further include an external conductor from the viewpoint of improving piezoelectric sensitivity and electrostatic shielding. The external conductor is disposed on the outer periphery of the piezoelectric layer. The internal conductor and the external conductor are not electrically connected. The outer conductor of the second embodiment is similar to the one exemplified as the outer conductor of the first embodiment.
[0094] (2.1.4) Electrical insulators The piezoelectric substrate according to the second aspect of the present disclosure may further include an electrical insulator (hereinafter referred to as a "first insulator"). The first insulator is disposed on the outermost periphery of the piezoelectric substrate. In other words, at least a portion of the outer periphery of the piezoelectric substrate is constituted by the first insulator. The first insulator of the second embodiment is similar to the first insulator exemplified in the first embodiment.
[0095] (2.1.5) Inner Electrical Insulation When the piezoelectric substrate according to the second aspect of the present disclosure includes an external conductor, the piezoelectric substrate may further include an inner electrical insulator (hereinafter, referred to as a "second insulator"), which is disposed, for example, between the piezoelectric layer and the internal conductor and / or between the piezoelectric layer and the external conductor. This can further prevent the occurrence of a short circuit between the inner conductor and the outer conductor. The second insulator of the second embodiment is similar to the second insulator exemplified in the first embodiment.
[0096] (2.1.6) Functional Layer The piezoelectric substrate of the second aspect of the present disclosure may further include a functional layer. When the piezoelectric substrate of the second aspect of the present disclosure does not include an external conductor, the functional layer is disposed between the piezoelectric layer and the internal conductor. When the piezoelectric substrate of the second aspect of the present disclosure includes an external conductor, the functional layer is disposed at least one of between the piezoelectric layer and the internal conductor and between the piezoelectric layer and the external conductor. The functional layer of the second embodiment is similar to the functional layer exemplified in the first embodiment.
[0097] Specific examples of the piezoelectric substrate according to the second embodiment will be described below with reference to the drawings, but the piezoelectric substrate according to the second embodiment of the present disclosure is not limited to the following specific examples. Throughout the drawings, substantially identical elements are given the same reference numerals and descriptions thereof will not be repeated.
[0098] (2.1.7) Piezoelectric substrate according to the first embodiment of the second aspect The piezoelectric substrate 10B according to the first embodiment of the second aspect will be described with reference to Fig. 3A to Fig. 3D. Fig. 3A is a schematic side view showing the appearance of the piezoelectric substrate 10B according to the first embodiment of the second aspect of the present disclosure. Fig. 3B is a schematic front view showing the appearance of the long piezoelectric body 140B according to the first embodiment of the second aspect of the present disclosure. Fig. 3C is a cross-sectional view taken along line IC-IC in Fig. 3B. Fig. 3D is a cross-sectional view taken along line IC-IC in Fig. 3A.
[0099] As shown in Fig. 3A, the piezoelectric substrate 10B according to the first embodiment of the second aspect includes a long internal conductor 12B and a piezoelectric layer 14B. The piezoelectric layer 14B is spirally wound in one direction along the outer circumferential surface of the internal conductor 12B from one end to the other end at a helix angle β1 without any gaps. The piezoelectric layer 14B is not fixed to the internal conductor 12B. The piezoelectric layer 14B is formed by winding the long piezoelectric body 140B counterclockwise around the outer circumferential surface of the internal conductor 12B. Specifically, when the piezoelectric substrate 10B is viewed from one axial end side of the internal conductor 12B (the right end side in FIG. 3A), the long piezoelectric body 140B is wound counterclockwise from the front side to the back side of the internal conductor 12B. The helix angle β1 is the angle between the direction of the helix axis G1 (the axial direction of the internal conductor 12B) and the longitudinal direction of the long piezoelectric element 140B in a side view. As shown in FIG. 3B, the long piezoelectric body 140B is composed of four piezoelectric yarns 141 and a bundle 142. In the first embodiment of the second aspect, the piezoelectric yarns 141 are twisted yarns composed of a plurality of optically active polypeptides. The bundle 142 is composed of a cyanoacrylate adhesive. The four piezoelectric yarns 141 are arranged in parallel in a direction perpendicular to the length direction of the piezoelectric yarns 141. Adjacent piezoelectric yarns 141 among the four piezoelectric yarns 141 are in contact with each other. The bundle 142 maintains the above-mentioned arrangement of the four piezoelectric yarns 141. More specifically, as shown in FIG. 3C, the bundle 142 is formed only in the gap portion constituted by a part of the outer circumferential surface where adjacent piezoelectric yarns 141 among the four piezoelectric yarns 141 face each other. This allows the piezoelectric substrate 10B to be efficiently prepared for terminal attachment. 3A, the double-headed arrow E1 indicates the main orientation direction of the optically active polypeptide contained in the piezoelectric layer 14B. That is, in the first embodiment of the second aspect, the main orientation direction of the optically active polypeptide and the length direction of the long piezoelectric body 140B are substantially parallel to each other.
[0100] The effects of the piezoelectric substrate 10B will be described below. For example, when tension is applied in the longitudinal direction of the piezoelectric substrate 10B, a shear stress is applied to the optically active polypeptide contained in the piezoelectric layer 14B, and the optically active polypeptide is polarized. The polarization of the optically active polypeptide is considered to occur in phase with each other in the radial direction of the piezoelectric substrate 10B, as shown by the arrows in FIG. 3D. This causes the piezoelectricity of the piezoelectric substrate 10B to be expressed. The piezoelectric substrate 10B has excellent piezoelectric sensitivity.
[0101] (2.1.8) Piezoelectric substrate according to the second embodiment of the second aspect A piezoelectric substrate 20B according to a second embodiment of the second aspect will be described with reference to Fig. 4. Fig. 4 is a schematic side view showing the external appearance of the piezoelectric substrate 20B according to the second embodiment of the second aspect.
[0102] A piezoelectric substrate 20B according to a second embodiment of the second aspect differs from the piezoelectric substrate 10B according to the first embodiment of the second aspect in that it includes an external conductor 22B. As shown in FIG. 4, the piezoelectric substrate 20B according to the second embodiment of the second aspect includes an internal conductor 12B, a piezoelectric layer 14B, and an external conductor 22B. The external conductor 22B is disposed on the outer periphery side of the piezoelectric layer 14B. The external conductor 22B is formed by spirally winding a copper foil ribbon around (on the outer periphery of the piezoelectric layer 14B) the long piezoelectric body 140B which is spirally wound around (on the outer periphery of) the internal conductor 12B. The internal conductor 12B and the external conductor 22B are not electrically connected. The piezoelectric layer 14B is not fixed to the internal conductor 12B. The external conductor 22B is not fixed to the piezoelectric layer 14B. 4, in the second embodiment of the second aspect, the end of the piezoelectric layer 14B (i.e., the long piezoelectric body 140B wound in a spiral shape) is misaligned with the end of the external conductor 22B in side view. This ensures that the internal conductor 12B and the external conductor 22B are insulated from each other. However, the ends do not necessarily need to be misaligned, and as long as the internal conductor 12B and the external conductor 22B are electrically insulated from each other, the ends may overlap in side view.
[0103] The piezoelectric substrate 20B provides the same effects as those of the piezoelectric substrate 10B. Furthermore, since the piezoelectric substrate 20B includes the internal conductor 12B, an electrical signal (voltage signal or charge signal) generated in the piezoelectric layer 14B can be more easily extracted via the internal conductor 12B. Furthermore, since the piezoelectric substrate 20B includes the external conductor 22B, the inside of the piezoelectric substrate 20B (the piezoelectric layer 14B and the internal conductor 12B) can be electrostatically shielded by the external conductor 22B. This makes it possible to suppress voltage changes in the internal conductor 12B caused by static electricity outside the piezoelectric substrate 20B, resulting in more stable piezoelectricity.
[0104] (2.1.9) Applications of piezoelectric substrates Applications of the piezoelectric substrate according to the second embodiment of the present disclosure are similar to the applications exemplified for the piezoelectric substrate according to the first embodiment.
[0105] (2.2) Sensors The sensor of the second aspect of the present disclosure comprises a piezoelectric substrate of the second aspect of the present disclosure. The sensor according to the second embodiment of the present disclosure includes the piezoelectric substrate according to the second embodiment of the present disclosure, and therefore has excellent piezoelectric sensitivity. The sensors according to the second aspect of the present disclosure include force sensors, pressure sensors, displacement sensors, deformation sensors, motion sensors, vibration sensors, impact sensors, ultrasonic sensors, and the like.
[0106] (2.3) Actuator The actuator of the second aspect of the present disclosure comprises a piezoelectric substrate of the second aspect of the present disclosure. The actuator according to the second aspect of the present disclosure includes the piezoelectric substrate according to the second aspect of the present disclosure, and therefore has excellent piezoelectric sensitivity.
[0107] (2.4) Biometric information acquisition device A bioinformation acquisition device according to a second aspect of the present disclosure includes the piezoelectric substrate according to the second aspect of the present disclosure. The bioinformation acquisition device of the second aspect of the present disclosure acquires bioinformation of a subject by detecting a biosignal of a subject or test animal (hereinafter collectively referred to as "subject") using a piezoelectric substrate of the second aspect of the present disclosure. The biosignal, the article on which the bioinformation acquisition device is disposed, and the uses of the bioinformation acquisition device of the second embodiment are similar to those exemplified in the first embodiment. EXAMPLES
[0108] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples. However, the present invention is not limited to the description of these examples. Examples 1 to 4 and Comparative Examples 1 to 4 correspond to the first aspect of the present disclosure, and Example 5 and Comparative Example 5 correspond to the second aspect of the present disclosure.
[0109] [Example 1] <Preparation of optically active polypeptide fibers> Raw silk was prepared as an optically active polypeptide fiber. Raw silk is a long fiber made of an optically active polypeptide. The raw silk was 21 denier. The thickness of the raw silk was 0.06 mm to 0.04 mm.
[0110] (Measurement of the degree of orientation F of optically active polypeptide fibers) Using a wide-angle X-ray diffraction apparatus (Rigaku Corporation's "RINT2550", accessories: rotating sample stage, X-ray source: CuKα, output: 40 kV 370 mA, detector: scintillation counter), raw silk (optically active polypeptide fiber) was fixed to a holder and the azimuthal distribution intensity of the crystal plane peak [2θ = 20°] was measured. In the obtained azimuth angle distribution curve (X-ray interference diagram), the orientation degree F (c-axis orientation degree) of raw silk (optically active polypeptide fiber) was calculated from the half-width (α) of the peak according to the following formula (a). The degree of orientation F of the optically active polypeptide fibers was 0.91. Orientation degree (F)=(180°-α) / 180° … (a) (α is the half-width of the peak due to the orientation)
[0111] <Preparation of piezoelectric yarn> Raw silk was used as piezoelectric yarn by a known method, and six single-twisted yarns (twist number 150 T / m) were refined to produce refined silk. The degree of orientation F of the twisted yarn of this refined silk was 0.86. Since the orientation degree F of the optically active polypeptide fiber was 0.86 and six single-strand twisted yarns (piezoelectric yarns) were produced using refined silk, it can be evaluated that the length direction of the piezoelectric yarn and the main orientation direction of the optically active polypeptide contained in the refined silk (optically active polypeptide fiber) are approximately parallel.
[0112] <Preparation of two-layer piezoelectric substrate> As the internal conductor, a tinsel wire "U24-01-00" (wire diameter 0.26 mm, length 200 mm) manufactured by Meisei Sangyo Co., Ltd. was prepared. The piezoelectric yarn was wound around the outer circumferential surface of the internal conductor with a left-handed helix with a helix angle of about 45°, with as few gaps as possible. This formed a layer (hereinafter referred to as the "piezoelectric yarn layer") on the outer circumferential surface of the internal conductor, and a piezoelectric substrate precursor was obtained. The piezoelectric yarn layer covered the entire outer circumferential surface of the internal conductor. In other words, the outer circumferential surface of the internal conductor was not exposed. Note that "left-handed" means that the piezoelectric thread is wound left-handed from the front side to the back side of the internal conductor when viewed from one end of the axial direction of the internal conductor (tinsel wire). "Spiral angle" means the angle between the axial direction of the internal conductor and the length direction of the piezoelectric thread. As a converging agent, "901H3" (cyanoacrylate adhesive) manufactured by Toagosei Co., Ltd. was prepared. A binder (cyanoacrylate adhesive) was dropped onto the outer surface of the piezoelectric thread layer of the piezoelectric substrate precursor, and allowed to soak into the inside of the piezoelectric thread. The excess binder was then immediately wiped off from the outer surface of the piezoelectric thread with a Kimwipe, and the material was left at room temperature to harden the binder. This resulted in a piezoelectric layer being formed from the piezoelectric thread layer, and a two-layer piezoelectric substrate was obtained. At this time, the piezoelectric layer was partially attached to the internal conductor, but was not fixed to the internal conductor, meaning that the piezoelectric layer and the internal conductor were not mechanically integrated, making it easy to remove the piezoelectric layer from the internal conductor.
[0113] In order to determine the elastic modulus of the piezoelectric layer, a part of the two-layer piezoelectric substrate was cut to obtain a measurement sample (two-layer piezoelectric substrate). The elastic modulus of the piezoelectric layer of the measurement sample (two-layer piezoelectric substrate) was measured by the following method. The measurement results are shown in Table 1.
[0114] (Measurement of elastic modulus Y of piezoelectric layer) The elastic modulus Y of the piezoelectric layer was measured as the indentation elastic modulus of the piezoelectric layer by a method in accordance with JIS Z2255 using a dynamic ultra-microhardness tester. Specifically, the elastic modulus Y of the piezoelectric layer was evaluated by pressing an indenter into the outer peripheral surface of the piezoelectric layer of the measurement sample (two-layer piezoelectric substrate). The outer peripheral surface of the piezoelectric layer of the measurement sample (two-layer piezoelectric substrate) was a surface formed by impregnating and curing the piezoelectric thread layer obtained by winding the piezoelectric thread on the outer peripheral surface of the internal conductor with a binder. The device used here was a dynamic ultra-microhardness tester "DUH-211R" (Shimadzu Corporation), with a diamond triangular pyramidal indenter (edge angle 115°) as the indenter. Measurements were performed under softness test measurement conditions in an environment with a temperature of 23±2°C and a humidity of 50±5°C. The elastic modulus Y of the piezoelectric layer is a value evaluated from the degree of initial elastic recovery in the unloading process, and is calculated using the following equations [Equation 1] to [Equation 4]. The elastic modulus Y used here is a value calculated as the elastic modulus assuming the Poisson's ratio of the measurement sample (two-layer piezoelectric substrate) to be 0 without considering it.
[0115]
number
[0116]
number
[0117]
number
[0118]
number
[0119] The symbols in [Number 1] to [Number 4] represent the following items. "Y" indicates the elastic modulus (Pa) of the measured sample, including the Poisson's ratio. The calculated elastic modulus includes an error due to the deviation of the indenter from the ideal shape. "E" indicates the elastic modulus (Pa) of the measured sample. "E i" is the elastic modulus of the diamond indenter (1.14 × 10 12 (Pa). "E r " indicates the composite elastic modulus (Pa) of the measured sample and indenter. "v" indicates the Poisson's ratio of the measured sample. "v i " indicates the Poisson's ratio of the diamond indenter (0.07). "A" is the indentation projected area (m 2 ) is shown. "dP / dh" indicates the gradient (N / m) at the start of unloading in the load-indentation depth diagram. "h c " indicates the effective contact depth (m). "h max " indicates the maximum indentation depth (m) (hereinafter referred to as "depth 1"). "h r " indicates the intersection (m) of the tangent line and the depth axis at the start of unloading (hereinafter referred to as "depth 3"). "h max- h r " indicates (depth 1)-(depth 3).
[0120] <Preparation of three-layer piezoelectric substrate> After measuring the elastic modulus Y of the piezoelectric layer, a portion of the piezoelectric layer at both ends of the measurement sample (two-layer piezoelectric substrate) was removed to expose the internal conductor. With the internal conductor exposed, crimp terminals were attached to both ends of the measurement sample (piezoelectric substrate). In this way, a two-layer piezoelectric substrate with terminals was obtained. The crimp terminals were fixed parts for evaluating the piezoelectric sensitivity of the piezoelectric substrate and were lead terminals for the internal electrodes. Here, the distance between the crimp terminals was adjusted to 150 mm.
[0121] A rolled copper foil ribbon with a rectangular cross section was prepared as the external conductor. The width of the rolled copper foil ribbon was 0.3 mm. The thickness of the rolled copper foil ribbon was 30 μm. This rolled copper foil ribbon was wound clockwise tightly around the outer peripheral surface of the piezoelectric layer of the terminal-attached two-layer piezoelectric substrate so that the piezoelectric layer was not exposed. This resulted in a three-layer piezoelectric substrate. The outer conductor covered the entire outer peripheral surface of the piezoelectric layer. In other words, the outer peripheral surface of the piezoelectric layer was not exposed. The outer conductor was not fixed to the piezoelectric layer with an adhesive or the like. In this manner, a three-layer piezoelectric substrate was produced.
[0122] (Measurement of generated charge per unit tensile force (piezoelectric sensitivity)) A three-layer piezoelectric substrate was used, and the amount of electric charge (generated electric charge amount) generated when a tensile force was applied to the three-layer piezoelectric substrate was measured by the following method, and the amount of electric charge generated per unit tensile force (piezoelectric sensitivity) was calculated from the generated electric charge amount. The results are shown in Table 1. Specifically, the three-layer piezoelectric substrate was chucked in a tensile tester ("Tensilon RTG1250" manufactured by A&D Co., Ltd.) with a chuck distance of 50 mm. Next, a tensile testing machine was used to repeatedly apply a stress range of 1.0 N to 2.0 N in a periodic triangular wave shape at 0.5 Hz to the three-layer piezoelectric substrate, and the amount of charge generated on the front and back of the three-layer piezoelectric substrate was measured with an electrometer (Keithley's programmable electric meter "617"). The amount of generated charge per unit tensile force was calculated as the piezoelectric sensitivity of the three-layer piezoelectric substrate from the slope of the correlation line of the scatter plot with the measured amount of generated charge Q [C] on the Y axis and the tensile force F [N] of the three-layer piezoelectric substrate on the X axis. Table 1 shows the measurement results of the elastic modulus Y of the piezoelectric layer and the piezoelectric sensitivity of the three-layer piezoelectric substrate.
[0123] [Example 2] A three-layer piezoelectric substrate was produced and evaluated in the same manner as in Example 1, except that a two-layer piezoelectric substrate was obtained as described below using a sizing agent (polyurethane adhesive A) instead of the sizing agent (cyanoacrylate adhesive). The elastic modulus Y of the piezoelectric layer and the piezoelectric sensitivity of the three-layer piezoelectric substrate were measured and the results are shown in Table 1. In Example 2, a two-layer piezoelectric substrate was produced as follows. MEK was added to a polyurethane resin solution (MT Olestar M37-50SS: manufactured by Mitsui Chemicals) to dilute it and adjust it to a solution with a solid content of 25 mass%, and a binder (polyurethane adhesive A) was obtained. A piezoelectric substrate precursor was obtained in the same manner as in Example 1. Masking tape was attached to the terminal parts for attaching the crimp terminals at both ends of the piezoelectric substrate precursor. The entire piezoelectric thread layer of the piezoelectric substrate precursor was immersed in a tank filled with a binder (polyurethane adhesive A) for 3 minutes. Then, the piezoelectric substrate precursor was pulled up from the tank filled with the binder (polyurethane adhesive A), and the dripping part of the piezoelectric substrate precursor (the binder (polyurethane adhesive A) dripping from the piezoelectric substrate precursor) was removed with a Kimwipe. Then, the piezoelectric substrate precursor was dried in a dryer at 150 ° C. for 30 minutes. As a result, a two-layer piezoelectric substrate was obtained.
[0124] [Example 3] A three-layer piezoelectric substrate was fabricated and evaluated in the same manner as in Example 2, except that a sizing agent (melamine-based adhesive) obtained by diluting a melamine resin solution (manufactured by Mitsui Chemicals) with an n-BuOH solution to a solid content of 30% by mass was used instead of the sizing agent (polyurethane-based adhesive A). The elastic modulus Y of the piezoelectric layer and the measurement results of the piezoelectric sensitivity of the three-layer piezoelectric substrate are shown in Table 1.
[0125] [Example 4] <Preparation of optically active polypeptide fibers> As an optically active polypeptide fiber, a yarn containing a synthetic protein ("Brewed Protein (registered trademark)") was prepared. The content of the synthetic protein was 30% by mass relative to the mass of the yarn. The thickness of the yarn containing the synthetic protein was about 0.5 mm to 0.7 mm.
[0126] (Measurement of the degree of orientation F of optically active polypeptide fibers) <Preparation of piezoelectric yarn> The degree of orientation F of the piezoelectric yarn containing the synthetic protein was measured using X-ray diffraction in the same manner as in Example 1 from the peak near 2θ=9° as a peak indicating orientation, and was found to be 0.58.
[0127] Except for using one woolen yarn containing synthetic protein as the piezoelectric yarn instead of the six-strand single-twisted yarn made of degummed silk, two-layered piezoelectric substrates and three-layered piezoelectric substrates were fabricated and evaluated in the same manner as in Example 1. The elastic modulus Y of the piezoelectric layer and the measurement results of the piezoelectric sensitivity of the three-layered piezoelectric substrate are shown in Table 2.
[0128] [Comparative Example 1] A three-layer piezoelectric substrate was produced and evaluated in the same manner as in Example 1, except that a cyanoacrylate adhesive "201" (manufactured by Toagosei Co., Ltd.) was used as the binder (cyanoacrylate adhesive) instead of the binder ("901H3"). The measurement results of the elastic modulus Y of the piezoelectric layer and the piezoelectric sensitivity of the three-layer piezoelectric substrate are shown in Table 1.
[0129] [Comparative Example 2] A three-layer piezoelectric substrate was produced and evaluated in the same manner as in Example 2, except that a sizing agent (polyurethane adhesive B) prepared as described below was used instead of the sizing agent (polyurethane adhesive A). The elastic modulus Y of the piezoelectric layer and the measurement results of the piezoelectric sensitivity of the three-layer piezoelectric substrate are shown in Table 1. The sizing agent of Comparative Example 2 (polyurethane adhesive B) was prepared as follows. "Takelac A-3210" (manufactured by Mitsui Chemicals, Inc.) and "Takenate A-3070" (manufactured by Mitsui Chemicals, Inc.) were mixed in a mass ratio of 1:1 to obtain a mixed solution. The mixed solution was then diluted with ethyl acetate to adjust the solid content to 20 mass % to obtain a sizing agent (polyurethane adhesive B).
[0130] [Comparative Example 3] A three-layer piezoelectric substrate was prepared and evaluated in the same manner as in Example 2, except that a polyurethane adhesive C "Takenate 6335" was used instead of the sizing agent (polyurethane adhesive A). The elastic modulus Y of the piezoelectric layer and the measurement results of the piezoelectric sensitivity of the three-layer piezoelectric substrate are shown in Table 1.
[0131] [Comparative Example 4] A three-layer piezoelectric substrate was fabricated and evaluated in the same manner as in Example 4, except that a cyanoacrylate adhesive "201" (manufactured by Toagosei Co., Ltd.) was used instead of the sizing agent ("901H3"). The elastic modulus Y of the piezoelectric layer and the measurement results of the piezoelectric sensitivity of the three-layer piezoelectric substrate are shown in Table 2.
[0132] <Deterioration evaluation when load is applied> The three-layer piezoelectric substrate of Example 1 with a total length of 150 mm was set in the tensile tester used to measure the piezoelectric sensitivity, and the degradation when a load was applied to the three-layer piezoelectric substrate was evaluated. In detail, in the tensile tester in which the three-layer piezoelectric substrate was set, the crosshead was moved slowly and manually in the tensile direction and fixed at a position where the tensile load was 0.2 N. This position was set as the displacement reference point zero, and the operation of pulling 2 mm from this position and returning to the zero position was repeated 100 times. At this time, the crosshead speed was set to 30 mm / sec. Before and after this test, a sensitivity evaluation was performed by applying a load of 1N to 2N in the same manner as in Example 1, and the change in sensitivity was calculated by dividing the sensitivity after the test by the sensitivity before the test. A similar test was carried out using the three-layer piezoelectric substrate of Example 2 and the three-layer piezoelectric substrate of Comparative Example 1, and the change in sensitivity of each was calculated. The sensitivity change of the three-layered piezoelectric substrate in Example 1 was 1.00. The sensitivity change of the three-layered piezoelectric substrate in Example 2 was 0.98. The sensitivity change of the three-layered piezoelectric substrate in Comparative Example 1 was 0.80. These results show that the sensitivity change of the three-layered piezoelectric substrates of Examples 1 and 2 was small, whereas the sensitivity change of the three-layered piezoelectric substrate of Comparative Example 1 was significantly reduced.
[0133] [Table 1]
[0134] [Table 2]
[0135] The piezoelectric substrates of Comparative Examples 1 to 3 include a long internal conductor and a piezoelectric layer covering the outer peripheral surface of the internal conductor. The piezoelectric layer includes a piezoelectric yarn wound around the outer peripheral surface of the internal conductor and an adhesive portion that maintains the state in which the piezoelectric yarn is wound around the outer peripheral surface of the internal conductor. The piezoelectric yarn includes refined silk, which is an optically active polypeptide fiber. However, the elastic modulus Y of the piezoelectric layer was not within the range of 1.0 GPa or more and 8.0 GPa or less. Therefore, the piezoelectric sensitivity was 2.3 pC / N / mm or less for each of the piezoelectric substrates of Comparative Examples 1 to 3. As a result, it was found that the piezoelectric substrates of Comparative Examples 1 to 3 did not have excellent piezoelectric sensitivity. On the other hand, the piezoelectric substrates of Examples 1 to 3 include a long internal conductor and a piezoelectric layer covering the outer peripheral surface of the internal conductor. The piezoelectric layer includes a piezoelectric yarn wound around the outer peripheral surface of the internal conductor and an adhesive portion that maintains the state in which the piezoelectric yarn is wound around the outer peripheral surface of the internal conductor. The piezoelectric yarn includes refined silk, which is an optically active polypeptide fiber. The elastic modulus Y of the piezoelectric layer was within the range of 1.0 GPa to 8.0 GPa. Therefore, the piezoelectric sensitivity of each of the piezoelectric substrates of Examples 1 to 3 was 2.6 pC / N / mm or more, which was higher than that of Comparative Examples 1 to 3. As a result, it was found that the piezoelectric substrates of Examples 1 to 3 had excellent piezoelectric sensitivity.
[0136] Comparing the piezoelectric substrate of Example 1 with the piezoelectric substrate of Example 2, the elastic modulus Y of the piezoelectric layer of Example 1 was in the range of 4.0 GPa or more and 8.0 GPa or less, and therefore the piezoelectric sensitivity of Example 1 was 5.0 pC / N / mm, which was higher than that of Example 2. On the other hand, comparing the piezoelectric substrate of Example 3 with the piezoelectric substrate of Example 2, the elastic modulus Y of the piezoelectric layer of Example 3 was in the range of 1.0 GPa or more and 3.6 GPa or less, and therefore the piezoelectric sensitivity of Example 3 was 4.2 pC / N / mm, which was higher than that of Example 2.
[0137] The piezoelectric substrate of Comparative Example 4 includes a long internal conductor and a piezoelectric layer covering the outer circumferential surface of the internal conductor. The piezoelectric layer includes a piezoelectric yarn wound around the outer circumferential surface of the internal conductor and an adhesive portion that maintains the state in which the piezoelectric yarn is wound around the outer circumferential surface of the internal conductor. The piezoelectric yarn includes a woolen yarn that includes a synthetic protein that is an optically active polypeptide fiber. However, the elastic modulus Y of the piezoelectric layer is not within the range of 1.0 GPa or more and 8.0 GPa or less. Therefore, the piezoelectric sensitivity of the piezoelectric substrate of Comparative Example 4 was 0.14 pC / N / mm or less. As a result, it was found that the piezoelectric substrate of Comparative Example 4 did not have excellent piezoelectric sensitivity. On the other hand, the piezoelectric substrate of Example 4 includes a long internal conductor and a piezoelectric layer covering the outer circumferential surface of the internal conductor. The piezoelectric layer includes a piezoelectric yarn wound around the outer circumferential surface of the internal conductor and an adhesive portion that maintains the state in which the piezoelectric yarn is wound around the outer circumferential surface of the internal conductor. The piezoelectric yarn includes a woolen yarn containing a synthetic protein that is an optically active polypeptide fiber. The elastic modulus Y of the piezoelectric layer was in the range of 1.0 GPa to 8.0 GPa. Therefore, the piezoelectric sensitivity of the piezoelectric substrate of Example 4 was 0.32 pC / N / mm or more, which was higher than that of Comparative Example 4. As a result, it was found that the piezoelectric substrate of Example 4 had excellent piezoelectric sensitivity.
[0138] [Example 5] <Preparation of optically active polypeptide fibers> Raw silk was prepared as an optically active polypeptide fiber. Raw silk is a long fiber made of an optically active polypeptide. The raw silk was 21 denier. The thickness of the raw silk was 0.06 mm to 0.04 mm.
[0139] (Measurement of the degree of orientation F of optically active polypeptide fibers) Using a wide-angle X-ray diffraction apparatus (Rigaku Corporation's "RINT2550", accessories: rotating sample stage, X-ray source: CuKα, output: 40 kV 370 mA, detector: scintillation counter), raw silk (optically active polypeptide fiber) was fixed to a holder and the azimuthal distribution intensity of the crystal plane peak [2θ = 20°] was measured. In the obtained azimuth angle distribution curve (X-ray interference diagram), the orientation degree F (c-axis orientation degree) of raw silk (optically active polypeptide fiber) was calculated from the half-width (α) of the peak according to the following formula (a). The degree of orientation F of the optically active polypeptide fibers was 0.91. Orientation degree (F)=(180°-α) / 180° … (a) (α is the half-width of the peak due to the orientation)
[0140] <Preparation of piezoelectric yarn> Raw silk was used as piezoelectric yarn by a known method, and six single-twisted yarns (twist number 150 T / m) were refined to produce refined silk. The degree of orientation F of the twisted yarn of this refined silk was 0.86. Orientation degree (F)=(180°-α) / 180° … (a) (α is the half-width of the peak due to the orientation)
[0141] <Preparation of long piezoelectric body> As the adhesive, "Aron Alpha 901H3" (cyanoacrylate adhesive) manufactured by Toagosei Co., Ltd. was prepared. The four piezoelectric threads were aligned so that they would not overlap each other, and were in contact with each other laterally. Specifically, the four piezoelectric threads were arranged in parallel in a direction perpendicular to the length direction of the piezoelectric threads, and the four piezoelectric threads were arranged so that adjacent ones of the four were in contact with each other. In this state, adhesive was dripped onto the four piezoelectric threads, and the four piezoelectric threads were impregnated with the adhesive. The four piezoelectric threads were fixed and joined with the adhesive. This resulted in a long piezoelectric body. The long piezoelectric body was composed of four piezoelectric threads and an adhesive body that bundled the four piezoelectric threads. The adhesive body covered the entire outer surface of the four piezoelectric threads. This long piezoelectric body was heat-treated at 120° C. for 6 hours. The thickness of the obtained long piezoelectric body was 0.08 mm. The width of the long piezoelectric body was 0.65 mm. The ratio of the width of the long piezoelectric body to the thickness of the long piezoelectric body was 8.1. Since the orientation degree F of the optically active polypeptide fiber was 0.91, the orientation degree of the yarn (piezoelectric yarn) made by twisting six strands of refined silk in one direction was 0.86, and a long piezoelectric body was produced by arranging four piezoelectric yarns in parallel in a direction perpendicular to the longitudinal direction of the piezoelectric yarn, it can be evaluated that the longitudinal direction of the long piezoelectric body is approximately parallel to the main orientation direction of the optically active polypeptide contained in the refined silk (optically active polypeptide fiber).
[0142] <Preparation of two-layer piezoelectric substrate> As the internal conductor, a tinsel wire "U24-01-00" (wire diameter: 0.26 mm, length: 200 mm) manufactured by Meisei Sangyo Co., Ltd. was prepared.
[0143] The long piezoelectric element was wound around the outer periphery of the internal conductor with a left-handed helix with as few gaps as possible, so that the helix angle was about 45°. This formed a piezoelectric layer covering the outer periphery of the internal conductor, and a two-layer piezoelectric substrate was obtained. The piezoelectric layer covered the entire outer periphery of the internal conductor. In other words, the outer periphery of the internal conductor was not exposed. The piezoelectric layer was not fixed to the internal conductor with an adhesive or the like. "Left-handed" means that the long piezoelectric element is wound left-handed from the front side to the back side of the internal conductor when viewed from one end in the axial direction of the internal conductor (tinsel wire). "Spiral angle" means the angle between the axial direction of the internal conductor and the length direction of the long piezoelectric element.
[0144] The elastic modulus Y of the long piezoelectric body was measured by the following method. The elastic modulus Y of the long piezoelectric body was measured using a microhardness tester (based on JIS Z 2255). The measurement result of the elastic modulus Y of the long piezoelectric body was 3.9 GPa.
[0145] (Measurement of elastic modulus Y of long piezoelectric body) The elastic modulus Y of the long piezoelectric body was measured as the indentation elastic modulus of the long piezoelectric body by a method in accordance with JIS Z2255 using a dynamic ultra-microhardness tester. Specifically, the elastic modulus Y of the long piezoelectric body was obtained by unwinding the long piezoelectric body from the piezoelectric layer of the measurement sample (two-layer piezoelectric substrate). If the unwound long piezoelectric body had a curl, the curled long piezoelectric body was cut to a length of about several mm to obtain the measurement sample. The measurement sample was fixed to a substrate and evaluated by pressing an indenter into the flat part of the measurement sample. The device used here was a dynamic ultra-microhardness tester "DUH-211R" (Shimadzu Corporation), with a diamond triangular pyramidal indenter (edge angle 115°) as the indenter. Measurements were performed under softness test measurement conditions in an environment with a temperature of 23±2°C and a humidity of 50±5°C. The elastic modulus Y of the long piezoelectric body is a value evaluated from the degree of initial elastic recovery in the unloading process, and is calculated using the formulas [Formula 1] to [Formula 4] in Example 1. The elastic modulus Y used here is a value calculated as the elastic modulus when the Poisson's ratio of the measurement sample is assumed to be 0 without taking it into consideration.
[0146] <Preparation of three-layer piezoelectric substrate> A rolled copper foil ribbon with a rectangular cross section was prepared as the external conductor. The width of the rolled copper foil ribbon was 0.3 mm. The thickness of the rolled copper foil ribbon was 30 μm. This rolled copper foil ribbon was tightly wound clockwise around the outer peripheral surface of the piezoelectric layer used to measure the elastic modulus Y of the long piezoelectric body so that the piezoelectric layer was not exposed. The outer conductor covered the entire outer peripheral surface of the piezoelectric layer. In other words, the outer peripheral surface of the piezoelectric layer was not exposed. The outer conductor was not fixed to the piezoelectric layer with an adhesive or the like. In this manner, a three-layer piezoelectric substrate was produced.
[0147] Next, preparation for terminal attachment was performed as a process before terminal attachment. In preparation for terminal attachment, the piezoelectric layer and external conductor were stripped from both ends of the three-layered piezoelectric substrate to expose the tinsel wire. In detail, in preparation for terminal attachment, a portion of the length required for the terminal was unwound, and the external conductors at both ends of the three-layered piezoelectric substrate were peeled off from the piezoelectric layer. Next, a portion of the length required for the terminal was unwound, and 5 mm of the piezoelectric layer was removed to expose the tinsel wire in order to expose the internal conductor. In Example 5, the internal conductor, the piezoelectric layer, and the external conductor are not mechanically integrated by adhesives or the like. Therefore, when the piezoelectric layer is removed, the internal conductor and the external conductor are not damaged. Furthermore, the time required for preparation for terminal attachment was within 2 minutes. The time required for preparation for terminal attachment indicates the time from the start of the work to expose the tinsel wire to the time when the tinsel wire is exposed.
[0148] <Measurement of the piezoelectric sensitivity of a three-layer piezoelectric substrate (electrometer)> The piezoelectric sensitivity (pC / N·mm) of the three-layer piezoelectric substrate was measured using an electrometer by the following method. As a result, the piezoelectric sensitivity of the three-layer piezoelectric substrate was 3.3 pC / N·mm.
[0149] -Method for measuring the piezoelectric sensitivity (pC / N mm) of a three-layer piezoelectric substrate (electrometer)- The three-layered piezoelectric substrate was chucked in a tensile tester ("Tensilon RTG1250" manufactured by A&D Co., Ltd.) with a chuck distance of 150 mm. In detail, the crimp terminal (electrical and mechanical connection part) on one end of the three-layered piezoelectric substrate was chucked by one chuck member, and the crimp terminal (electrical and mechanical connection part) on the other end of the three-layered piezoelectric substrate was chucked by the other chuck member. In addition, the charge amount measuring electrode of the electrometer (Programmable Electric Meter "617" manufactured by Keithley) was connected to the crimp terminal of the three-layered piezoelectric substrate, and the ground electrode of the electrometer (Programmable Electric Meter "617" manufactured by Keithley) was connected to the external conductor (rolled copper foil ribbon) of the three-layered piezoelectric substrate. Next, a tensile testing machine was used to repeatedly apply tension to the three-layer piezoelectric substrate in a periodic triangular wave shape at a constant moving speed of 5 mm / min in a stress range of 1 N to 2 N, and the amount of charge generated on the internal conductor side of the three-layer piezoelectric substrate was measured with an electrometer (Keithley's programmable electric meter "617"). The measured amount of generated charge Q [C] was plotted on the Y-axis and the tensile force F [N] of the three-layer piezoelectric substrate was plotted on the X-axis. From the slope of the correlation line of the scatter plot, the amount of generated charge per unit tensile force was calculated, and the calculated value was divided by the distance between the crimped terminals to obtain the piezoelectric sensitivity (pC / N mm).
[0150] <Comparative Example 5> The same refined silk and inner conductor as in Example 5 were prepared. In Comparative Example 5, instead of winding the long piezoelectric body of Example 5 around the outer peripheral surface of the internal conductor, four strands of refined silk were pulled together and wound around the outer peripheral surface of the internal conductor in a spiral shape without any gaps so that the internal conductor was not exposed, and four more strands of refined silk were pulled together and wound around the inner conductor in a similar manner. The helical angle of the refined silk was about 45°, and the winding direction of the refined silk was left-handed. This resulted in the formation of a refined silk layer covering the outer circumferential surface of the internal conductor. The refined silk layer covered the entire outer circumferential surface of the internal conductor. In other words, the outer circumferential surface of the internal conductor was not exposed. The helix angle of the refined silk refers to the angle of the length of the refined silk relative to the longitudinal axis of the inner conductor.
[0151] Next, "Aron Alpha 901H3" (cyanoacrylate adhesive) manufactured by Toagosei Co., Ltd. was prepared as an adhesive. The adhesive was dropped onto the outer surface of the refined silk layer, impregnated into the refined silk layer, and then heat-treated at 120°C for 6 hours. This resulted in the refined silk layer being fixed to the internal conductor and mechanically integrated. This resulted in a piezoelectric layer covering the outer surface of the internal conductor, and a two-layer piezoelectric substrate was obtained. The piezoelectric layer was fixed to the internal conductor by the adhesive.
[0152] Next, a rolled copper foil ribbon with a rectangular cross section was prepared as an external conductor. The width of the rolled copper foil ribbon was 0.3 mm. The thickness of the rolled copper foil ribbon was 30 μm. This rolled copper foil ribbon was tightly wound clockwise around the outer peripheral surface of the piezoelectric layer used to measure the elastic modulus Y of the long piezoelectric body so that the piezoelectric layer was not exposed. The outer conductor covered the entire outer peripheral surface of the piezoelectric layer. In other words, the outer peripheral surface of the piezoelectric layer was not exposed. The outer conductor was not fixed to the piezoelectric layer with an adhesive or the like. In this manner, a three-layer piezoelectric substrate was produced.
[0153] Next, preparation for terminal attachment was performed as a process before terminal attachment. In preparation for terminal attachment, the piezoelectric layer and external conductor were stripped from both ends of the three-layered piezoelectric substrate to expose the tinsel wire. In detail, in preparation for terminal attachment, the length required for the terminal was unwound, and the external conductors at both ends of the three-layered piezoelectric substrate were peeled off from the piezoelectric layer. Next, the length required for the terminal was unwound, and 5 mm of the piezoelectric layer was removed to expose the tinsel wire in order to expose the internal conductor. In Comparative Example 5, the internal conductor and the piezoelectric layer are mechanically integrated by the adhesive. Therefore, the time required for preparation for terminal attachment was more than five times longer than that of Example 5. The time required for preparation for terminal attachment indicates the time required from the start of the work to expose the tinsel wire to the time when the tinsel wire is exposed.
[0154] The piezoelectric sensitivity (pC / N·mm) of the three-layered piezoelectric substrate was measured in the same manner as in Example 5. As a result, the piezoelectric sensitivity of the three-layered piezoelectric substrate was 2.8 pC / N·mm.
[0155] The three-layer piezoelectric substrate of Comparative Example 5 includes a long internal conductor and a piezoelectric layer covering the outer peripheral surface of the internal conductor. The piezoelectric layer is formed by winding a long piezoelectric body around the outer peripheral surface of the internal conductor. The long piezoelectric body includes four piezoelectric yarns and an adhesive that maintains the four piezoelectric yarns wound around the outer peripheral surface of the internal conductor. However, the piezoelectric layer is fixed to the internal conductor by an adhesive. Therefore, the piezoelectric sensitivity of the three-layer piezoelectric substrate was 2.8 pC / N mm. Furthermore, the time required for preparation for end attachment was more than five times that of Example 5. As a result, it was found that the three-layer piezoelectric substrate of Comparative Example 5 did not enable efficient preparation for terminal attachment, and also had poor piezoelectric sensitivity.
[0156] On the other hand, the three-layer piezoelectric substrate of Example 5 includes a long internal conductor and a piezoelectric layer covering the outer peripheral surface of the internal conductor. The piezoelectric layer is formed by winding a long piezoelectric body around the internal conductor and is not fixed to the internal conductor. The long piezoelectric body includes four piezoelectric yarns and an adhesive that binds the four piezoelectric yarns together. Therefore, the piezoelectric sensitivity of the three-layer piezoelectric substrate was 3.3 pC / N mm, which was higher than that of Comparative Example 5. Furthermore, the time required for end attachment was less than 2 minutes, which was shorter than that of Comparative Example 5. As a result, it was found that the three-layer piezoelectric substrate of Example 5 enabled efficient preparation for terminal attachment and had excellent piezoelectric sensitivity.
[0157] The disclosures of Japanese Patent Application No. 2021-061998, filed on March 31, 2021, and Japanese Patent Application No. 2021-061999, filed on March 31, 2021, are incorporated herein by reference in their entireties. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A long inner conductor; a piezoelectric layer covering an outer circumferential surface of the internal conductor; Equipped with The piezoelectric layer is A piezoelectric yarn wound around the internal conductor; an adhesive portion that holds the piezoelectric yarn wound around the internal conductor; having The piezoelectric yarn comprises an optically active polypeptide fiber, which represents a fiber made of an optically active polypeptide; A piezoelectric substrate, wherein the piezoelectric layer has an elastic modulus Y of 1.0 GPa or more and 8.0 GPa or less, as measured by a microhardness tester (in accordance with JIS Z 2255).
2. The piezoelectric substrate according to claim 1 , wherein the length direction of the piezoelectric yarn is approximately parallel to the main orientation direction of the optically active polypeptide.
3. 3. The piezoelectric substrate according to claim 1, wherein the degree of orientation F of the optically active polypeptide fibers, as determined by X-ray diffraction measurement using the following formula (a), is 0.50 or more and less than 1.
00. Orientation degree F=(180°-α) / 180°...Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.]
4. The piezoelectric substrate according to any one of claims 1 to 3, wherein the piezoelectric yarn is wound spirally in one direction.
5. The piezoelectric substrate according to claim 4, wherein a helical angle between the axial direction of the internal conductor and the longitudinal direction of the piezoelectric thread is 20° to 70°.
6. The piezoelectric substrate according to any one of claims 1 to 5, wherein the adhesive portion is made of at least one selected from an epoxy-based adhesive, a urethane-based adhesive, a vinyl acetate resin-based emulsion-type adhesive, an ethylene vinyl acetate-based emulsion-type adhesive, an acrylic resin-based emulsion-type adhesive, a styrene butadiene rubber-based latex-type adhesive, a silicone resin-based adhesive, an α-olefin-based adhesive, a vinyl chloride resin-based solvent-type adhesive, a rubber-based adhesive, an elastic adhesive, a chloroprene rubber-based solvent-type adhesive, a nitrile rubber-based solvent-type adhesive, and a cyanoacrylate-based adhesive.
7. Further, an outer conductor is provided on an outer periphery of the piezoelectric layer, The piezoelectric substrate according to any one of claims 1 to 6, wherein the internal conductor and the external conductor are not electrically connected to each other.
8. The piezoelectric substrate according to any one of claims 1 to 7, wherein the optically active polypeptide has a β-sheet structure.
9. The piezoelectric substrate according to any one of claims 1 to 8, wherein the optically active polypeptide comprises at least one of fibroin and spider silk protein.
10. The piezoelectric substrate according to any one of claims 1 to 9, wherein the optically active polypeptide fiber comprises at least one of silk and spider silk.
11. The piezoelectric substrate of claim 10 , wherein the silk is refined silk.
12. each of the piezoelectric yarns comprises a plurality of optically active polypeptide fibers; The piezoelectric substrate according to any one of claims 1 to 11, wherein the number of twists of the piezoelectric yarn is 500 T / m or less.
13. The piezoelectric substrate according to any one of claims 1 to 12, further comprising an electrical insulator on the outermost periphery.
14. A sensor comprising the piezoelectric substrate according to any one of claims 1 to 13.
15. An actuator comprising the piezoelectric substrate according to any one of claims 1 to 13.
16. A bioinformation acquisition device comprising the piezoelectric substrate according to any one of claims 1 to 13.
17. A long inner conductor; a piezoelectric layer covering an outer circumferential surface of the internal conductor; Equipped with the piezoelectric layer is formed by winding a long piezoelectric body around the internal conductor and is not fixed to the internal conductor; The long piezoelectric element includes a plurality of piezoelectric yarns and a bundle that bundles the plurality of piezoelectric yarns, At least one of the plurality of piezoelectric yarns comprises an optically active polypeptide fiber, which represents a fiber made of an optically active polypeptide; A piezoelectric substrate, wherein the elastic modulus Y of the long piezoelectric body measured by a microhardness tester (in accordance with JIS Z 2255) is 1 GPa or more and 10 GPa or less.
18. The piezoelectric substrate according to claim 17 , wherein the length direction of the long piezoelectric element is approximately parallel to the main orientation direction of the optically active polypeptide.
19. 19. The piezoelectric substrate according to claim 17 or 18, wherein the degree of orientation F of the optically active polypeptide fibers calculated from X-ray diffraction measurement using the following formula (a) is 0.50 or more and less than 1.
00. Orientation degree F=(180°-α) / 180°...Formula (a) [In formula (a), α represents the half-width (°) of the peak due to the orientation.]
20. The piezoelectric substrate according to any one of claims 17 to 19, wherein the long piezoelectric element is wound spirally in one direction.
21. The piezoelectric substrate according to claim 20, wherein a helical angle between an axial direction of the internal conductor and a longitudinal direction of the long piezoelectric element is 20° to 70°.
22. A piezoelectric substrate described in any one of claims 17 to 21, wherein the bundle aligns the multiple piezoelectric yarns in a direction perpendicular to the longitudinal direction of the multiple piezoelectric yarns and bundles the multiple piezoelectric yarns in a state in which adjacent piezoelectric yarns among the multiple piezoelectric yarns are in contact with each other.
23. The piezoelectric substrate according to any one of claims 17 to 22, wherein the convergent body is made of at least one selected from an epoxy-based adhesive, a urethane-based adhesive, a vinyl acetate resin-based emulsion-type adhesive, an ethylene vinyl acetate-based emulsion-type adhesive, an acrylic resin-based emulsion-type adhesive, a styrene butadiene rubber-based latex-type adhesive, a silicone resin-based adhesive, an α-olefin-based adhesive, a vinyl chloride resin-based solvent-type adhesive, a rubber-based adhesive, an elastic adhesive, a chloroprene rubber-based solvent-type adhesive, a nitrile rubber-based solvent-type adhesive, and a cyanoacrylate-based adhesive.
24. The thickness of the long piezoelectric element is 0.001 mm to 0.4 mm, The width of the long piezoelectric element is 0.1 mm to 30 mm, The piezoelectric substrate according to any one of claims 17 to 23, wherein a ratio of the width of the long piezoelectric element to the thickness of the long piezoelectric element is 2 or more.
25. Further, an outer conductor is provided on an outer periphery of the piezoelectric layer, The piezoelectric substrate according to any one of claims 17 to 24, wherein the internal conductor and the external conductor are not electrically connected to each other.
26. The piezoelectric substrate according to any one of claims 17 to 25, wherein the optically active polypeptide has a β-sheet structure.
27. The piezoelectric substrate according to any one of claims 17 to 26, wherein the optically active polypeptide comprises at least one of fibroin and spider silk protein.
28. The piezoelectric substrate according to any one of claims 17 to 27, wherein the fiber made of the optically active polypeptide comprises at least one of silk and spider silk.
29. 30. The piezoelectric substrate of claim 28, wherein the silk is refined silk.
30. each of said plurality of piezoelectric yarns comprises a plurality of said optically active polypeptide fibers; The piezoelectric substrate according to any one of claims 17 to 29, wherein the number of twists of each of the plurality of piezoelectric yarns is 500 T / m or less.
31. The piezoelectric substrate according to any one of claims 17 to 30, further comprising an electrical insulator on the outermost periphery.
32. A sensor comprising the piezoelectric substrate according to any one of claims 17 to 31.
33. An actuator comprising the piezoelectric substrate according to any one of claims 17 to 31.
34. A bioinformation acquisition device comprising the piezoelectric substrate according to any one of claims 17 to 31.
Citation Information
Patent Citations
Piezoelectric component, light source device, and printing device
JP2014186320A
Piezoelectric substrate, piezoelectric fabric, piezoelectric knit, piezoelectric device, force sensor, actuator, and biological information acquisition device
JP2020036027A
Charge generation yarn for bacteria countermeasure, cloth for bacteria countermeasure, cloth, clothing, medical member, bioactive charge generation yarn, and charge generation yarn for substance adsorption
WO2017212836A1
Piezoelectric base material, piezoelectric woven fabric, piezoelectric knitted fabric, piezoelectric device, force sensor, and actuator
WO2017213108A1
Piezoelectric base material, sensor, actuator, biological information acquisition device, and piezoelectric fiber structure
WO2018092886A1