Masterbatch containing positive electrode active material and irreversible additive, and positive electrode slurry for lithium secondary battery containing the same

The masterbatch with lithium cobalt oxide enhances dispersibility and process efficiency, addressing the challenges of low irreversible additive use in lithium secondary batteries, resulting in improved electrical properties and reliability.

JP7594098B2Active Publication Date: 2024-12-03LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023517380
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-31
Filing Date
2022-05-06
Publication Date
2024-12-03
Estimated Expiration
2042-05-06

AI Technical Summary

Technical Problem

Conventional lithium secondary batteries face challenges in ensuring dispersibility and process efficiency when using low amounts of irreversible additives due to structural instability and loss during manufacturing, limiting their reliability and design freedom.

Method used

A masterbatch containing lithium cobalt oxide with specific chemical formulations and controlled particle sizes is used to disperse a high content of irreversible additives uniformly within the positive electrode slurry, enhancing dispersibility and reducing losses during production.

Benefits of technology

The solution ensures high electrical properties and reliability of lithium secondary batteries with improved dispersibility and process efficiency, allowing for increased design freedom and reduced oxygen gas generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594098000001
    Figure 0007594098000001
  • Figure 0007594098000002
    Figure 0007594098000002
  • Figure 0007594098000003
    Figure 0007594098000003
Patent Text Reader

Abstract

The present invention relates to a masterbatch for a positive electrode additive and a positive electrode slurry for a lithium secondary battery containing the same. The masterbatch contains a high content of an irreversible additive together with the positive electrode active material, thereby enabling a small amount of the irreversible additive to be dispersed in the positive electrode slurry with high dispersibility and without loss during the preparation of the positive electrode. Therefore, the positive electrode for a lithium secondary battery prepared using the masterbatch not only has high electrical properties and reliability, but also has the advantage of improving design flexibility during the preparation of the positive electrode.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a masterbatch for a positive electrode additive containing a high content of a non-reversible additive together with a positive electrode active material, and a positive electrode slurry for a lithium secondary battery containing the same.

[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0069635 dated May 31, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. [Background technology]

[0003] With the development of technology and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and working potential, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0004] Recently, as lithium secondary batteries have come to be used as power sources for medium to large devices such as electric vehicles, there has been an increasing demand for lithium secondary batteries with higher capacity, higher energy density, and lower costs, and the irreversible additives used in electrodes are also required to have higher irreversible capacity.

[0005] In response to these demands, conventional irreversible additives such as Li6CoO4 have been developed. However, conventional irreversible additives are structurally unstable and can generate large amounts of oxygen gas (O2) as the secondary battery is charged, as described below. Therefore, the use of a high content of irreversible additive in the positive electrode is limited in terms of the charge / discharge efficiency and safety of the lithium secondary battery. As a result, efforts are ongoing to improve the irreversibility of lithium secondary batteries by using low content of irreversible additives:

[0006] [ka]

[0007] However, when the irreversible additive is used in a low content, particularly in a trace amount of 2 wt % or less based on the total weight of the positive electrode slurry, it is difficult to ensure its dispersion in the positive electrode slurry, which reduces the reliability of the lithium secondary battery, and the low-particle irreversible additive disperses during the manufacturing process of the positive electrode, increasing the amount of loss and reducing the freedom of process design.

[0008] Therefore, when a trace amount of a non-reversible additive is used, there is a need to develop a technology that can prevent loss of the non-reversible additive during the manufacture of a positive electrode, improve processability and freedom of process design, and ensure the dispersibility of the non-reversible additive in the positive electrode slurry to ensure the reliability of the lithium secondary battery. Summary of the Invention [Problem to be solved by the invention]

[0009] Therefore, an object of the present invention is to provide a positive electrode slurry containing a significantly small amount of a non-reversible additive with high dispersion without loss during preparation of a positive electrode, and a positive electrode for a lithium secondary battery prepared using the same. [Means for solving the problem]

[0010] To solve the above problems, In one embodiment, the present invention comprises: A master batch for a positive electrode additive is provided, which contains 0.5 to 50 parts by weight of lithium cobalt oxide represented by the following Chemical Formula 1 relative to 100 parts by weight of a first positive electrode active material:

[0011] [Chemical formula 1] Li p Co 1-q M 1 q O4

[0012] In the above chemical formula 1, M 1is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4.

[0013] In this case, the positive electrode additive master batch may contain 1 to 10 parts by weight of the first binder with respect to 100 parts by weight of the first positive electrode active material.

[0014] In addition, the average particle size (D 50 ) may be 0.05 mm to 10 mm, and the average particle size (D 50 The first positive electrode active material has an average particle size (D 50 ) may be 1 to 200 μm, and the average particle size of the lithium cobalt oxide may be larger than the average particle size of the first positive electrode active material.

[0015] In one embodiment, the present invention provides a method for producing a composition comprising: A master batch for a positive electrode additive of a lithium secondary battery according to the present invention, comprising 0.5 to 50 parts by weight of a lithium cobalt oxide represented by the following Chemical Formula 1, based on 100 parts by weight of the first positive electrode active material; A second positive electrode active material; A conductive material; and a second binder.

[0016] [Chemical formula 1] Li p Co 1-q M 1 q O4

[0017] In the above chemical formula 1, M 1is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4.

[0018] At this time, the lithium cobalt oxide contained in the master batch and represented by Chemical Formula 1 may be contained in an amount of 0.05 to 2.0 parts by weight based on 100 parts by weight of the total positive electrode slurry.

[0019] The positive electrode additive masterbatch may be included in an amount of 1 to 150 parts by weight based on 100 parts by weight of the second positive electrode active material.

[0020] The first and second positive electrode active materials may each contain a lithium metal composite oxide represented by the following Chemical Formula 2:

[0021] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u

[0022] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and x, y, z, w, v, and u are 1.0≦x≦1.30, 0.1≦y<1, 0.01 <z≦0.6、0.01<w≦0.6、0≦v≦0.2、1.5≦u≦5である。

[0023] The conductive material may be contained in an amount of 1 to 5 parts by weight relative to 100 parts by weight of the total positive electrode slurry.

[0024] In addition, the content of the second binder may be 1 to 5 parts by weight with respect to 100 parts by weight of the total positive electrode slurry.

[0025] In one embodiment, the present invention provides a method for producing a composition comprising: The positive electrode current collector, the first positive electrode mixture layer, and the second positive electrode mixture layer are sequentially stacked, The first positive electrode mixture layer and the second positive electrode mixture layer are each formed using the positive electrode slurry for a lithium secondary battery according to the present invention, thereby providing a positive electrode for a lithium secondary battery.

[0026] At this time, the content of the lithium cobalt oxide represented by the following Chemical Formula 1 contained in the first positive electrode mixture layer is 0.5 to 2.0 parts by weight with respect to 100 parts by weight of the first positive electrode mixture layer, The content of the lithium cobalt oxide represented by the following Chemical Formula 1 contained in the second positive electrode mixture layer may be 0.01 to 0.5 parts by weight per 100 parts by weight of the second positive electrode mixture layer:

[0027] [Chemical formula 1] Li p Co 1-q M 1 q O4

[0028] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4.

[0029] In addition, the total content of lithium cobalt oxide contained in the first positive electrode mixture layer and the second positive electrode mixture layer may be 0.5 parts by weight or less relative to 100 parts by weight of the total positive electrode active material contained in the first positive electrode mixture layer and the second positive electrode mixture layer.

[0030] The ratio of the average thickness of the first positive electrode mixture layer to the second positive electrode mixture layer may be 0.1 to 0.9.

[0031] Moreover, in one embodiment, the present invention provides There is provided a lithium secondary battery comprising the positive electrode according to the present invention, a negative electrode, and a separator located between the positive electrode and the negative electrode. Effect of the Invention

[0032] The masterbatch for positive electrode additives according to the present invention contains a high content of irreversible additive together with a positive electrode active material, and thus a small amount of irreversible additive can be dispersed in a positive electrode slurry with a high degree of dispersion without loss during the manufacture of the positive electrode. Therefore, a positive electrode for a lithium secondary battery manufactured using the masterbatch not only has high electrical properties and reliability, but also has the advantage of improving design freedom during the manufacture of the positive electrode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] While the present invention may be modified in many ways and have various embodiments, specific embodiments will be described in detail in the detailed description.

[0034] However, it should be understood that this is not intended to limit the invention to the particular embodiment, but includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the invention.

[0035] In the present invention, the terms "comprise" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0036] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "located on" may include not only the case where it is located at the top, but also the case where it is located at the bottom.

[0037] In the present invention, the term "masterbatch for positive electrode additive" refers to a solid composition in which components used in manufacturing a positive electrode of a lithium secondary battery are formed into a pellet shape of mm size, and the component contains a non-reversible additive in the form of fine particles at a higher content than the content actually contained in the positive electrode mixture layer, where "high content" means at least twice the content contained in the positive electrode mixture layer.

[0038] In addition, in the present invention, a "major component" means 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, or 97.5% by weight or more of the total weight of the composition or specific component, and in some cases, it can also mean 100% by weight when it constitutes the entire composition or specific component.

[0039] In the present invention, "Ah" is a unit of capacity of a lithium secondary battery, and is called "ampere-hour" and means the amount of current per hour. For example, if a battery capacity is "3000mAh", it means that it can be discharged at a current of 3000mA for one hour.

[0040] The present invention will now be described in more detail.

[0041] <Masterbatch for cathode additives> In one embodiment, the present invention comprises: A master batch for a positive electrode additive is provided, which contains 0.5 to 50 parts by weight of lithium cobalt oxide represented by the following Chemical Formula 1 relative to 100 parts by weight of a first positive electrode active material:

[0042] [Chemical formula 1] Li p Co 1-q M 1 q O4

[0043] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4.

[0044] The masterbatch for positive electrode additives according to the present invention is used for manufacturing a positive electrode mixture layer of a positive electrode for a lithium secondary battery. In general, when a non-reversible additive is contained in an amount of 2 wt% or less based on the total weight of the positive electrode mixture layer during manufacturing of a positive electrode mixture layer to be provided on a positive electrode, the content is significantly small, so that a large amount is lost during the process and it is difficult to disperse uniformly, resulting in a limitation in that the reliability of the manufactured positive electrode and the lithium secondary battery including the same is low. However, the masterbatch for positive electrode additives according to the present invention contains a high content of lithium cobalt oxide represented by Chemical Formula 1 used as the non-reversible additive together with the first positive electrode active material, so that the non-reversible additive can be uniformly dispersed in the positive electrode slurry without loss during manufacturing of the positive electrode mixture layer.

[0045] At this time, the lithium cobalt oxide is included in the master batch as a non-reversible additive that imparts non-reversible capacity together with a positive electrode active material that exhibits electrical activity, and includes lithium cobalt oxide represented by the following Chemical Formula 1:

[0046] [Chemical formula 1] Li p Co 1-q M 1 q O4 In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4.

[0047] Specifically, the lithium cobalt oxide is not particularly limited as long as it is a lithium cobalt oxide represented by Chemical Formula 1, but is preferably Li6CoO4, Li6Co 0.5 Zinc 0.5 O4, Li6Co 0.7 Zinc 0.3 It may also include O4.

[0048] The lithium cobalt oxide shown in the above formula 1 is a lithium cobalt oxide (Li p CoO4, 5≦p≦7) or has a structure in which a transition metal is doped at the cobalt site of the lithium cobalt oxide. In this case, the amount of the doped transition metal may be 40 molar fraction or less (q≦0.4), specifically, 20 to 40 molar fraction (0.2≦q≦0.4), 10 to 30 molar fraction (0.1≦q≦0.3), 15 to 30 molar fraction (0.15≦q≦0.3), 30 to 40 molar fraction (0.3≦q≦0.4), or 5 to 20 molar fraction (0.05≦q≦0.2). In the present invention, by adjusting the doping amount of the metal to the above molar fraction range, it is possible to reduce the amount of oxygen gas generated by releasing a large amount of lithium ions.

[0049] The lithium cobalt oxide represented by the above chemical formula 1 may have a tetragonal crystal structure, and may have a space group of P42 / nmc.

[0050] In addition, the lithium cobalt oxide represented by Chemical Formula 1 may be included in the master batch at 0.5 to 50 parts by weight relative to 100 parts by weight of the first positive electrode active material, specifically, 0.5 to 40 parts by weight, 0.5 to 30 parts by weight, 0.5 to 25 parts by weight, 0.5 to 20 parts by weight, 0.5 to 10 parts by weight, 2 to 30 parts by weight, 2 to 15 parts by weight, 8 to 15 parts by weight, 8 to 28 parts by weight, 15 to 30 parts by weight, 9 to 22 parts by weight, or 4 to 11 parts by weight relative to 100 parts by weight of the first positive electrode active material. By controlling the content of the lithium cobalt oxide included in the master batch as described above, the present invention can prevent the amount of the master batch used in the positive electrode slurry from being significantly reduced and not being uniformly dispersed due to an excessive amount of irreversible additive included in the master batch, and can prevent a decrease in the efficiency of master batch production due to a trace amount of irreversible additive.

[0051] In addition, the average particle size (D 50 The average particle size (D) of the positive electrode additive masterbatch may be 0.05 mm to 10 mm, specifically, 0.1 mm to 10 mm, 0.5 mm to 10 mm, 1 mm to 10 mm, 0.1 mm to 2 mm, 5 mm to 10 mm, 1 mm to 5 mm, or 3 mm to 7 mm. 50 By controlling the amount of the master batch to be added within the above range, it is possible to prevent loss of the master batch due to scattering during the production of the positive electrode slurry and to prevent changes in the composition of the positive electrode slurry, thereby improving the efficiency of the work process.

[0052] In addition, the average particle size (D 50 The first positive electrode active material has an average particle size (D 50 The first positive electrode active material may have an average particle size (D ) of 1 to 200 μm, and the average particle size of the lithium cobalt oxide may be larger than the average particle size of the first positive electrode active material. 50), and the lithium cobalt oxide may have an average particle size (D 50 The present invention relates to a method for producing a lithium cobalt oxide having an average particle size (D 50 ) in the above range, the charge / discharge capacity and efficiency of the manufactured lithium secondary battery can be increased, and the amount of oxygen gas generated from the lithium cobalt oxide that releases a large amount of lithium ions can be reduced. In addition, by including a larger irreversible additive than the first positive electrode active material, the side reaction of the irreversible additive can be reduced.

[0053] In addition, the masterbatch for a positive electrode additive according to the present invention may further include 1 to 10 parts by weight of a first binder relative to 100 parts by weight of the first positive electrode active material contained in the masterbatch in order to form a pellet of mm size containing the first positive electrode active material and the lithium cobalt oxide represented by Chemical Formula 1. Specifically, the masterbatch may further include 1 to 5 parts by weight, 5 to 10 parts by weight, 3 to 8 parts by weight, or 4 to 6 parts by weight of the first binder relative to 100 parts by weight of the first positive electrode active material.

[0054] Here, the first binder can be used without any particular limitation as long as it is one that can be normally used in a positive electrode composite layer. For example, the first binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.

[0055] As described above, the present invention controls the composition of the master batch for the positive electrode additive, thereby dispersing a small amount of the irreversible additive in the positive electrode slurry with a high degree of dispersion without loss during the production of the positive electrode, thereby improving the performance and reliability of the manufactured lithium secondary battery.

[0056] <Positive electrode slurry for lithium secondary batteries> In one embodiment, the present invention provides a method for producing a composition comprising: A master batch for a positive electrode additive of a lithium secondary battery according to the present invention, comprising 0.5 to 50 parts by weight of a lithium cobalt oxide represented by the following Chemical Formula 1 relative to 100 parts by weight of a first positive electrode active material; A second positive electrode active material; A conductive material; and a second binder.

[0057] [Chemical formula 1] Li p Co 1-q M 1 q O4

[0058] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4.

[0059] The positive electrode slurry for a lithium secondary battery according to the present invention is for producing a positive electrode mixture layer to be provided in a positive electrode for a lithium secondary battery, and contains a second positive electrode active material, a conductive material, and a second binder in addition to the above-mentioned masterbatch for positive electrode additives.

[0060] Here, the positive electrode slurry may contain the positive electrode additive masterbatch according to the present invention in an amount of 1 to 150 parts by weight relative to 100 parts by weight of the second positive electrode active material. More specifically, the positive electrode slurry may contain the positive electrode additive masterbatch in an amount of 120 to 150 parts by weight, 1 to 100 parts by weight, 1 to 50 parts by weight, 1 to 30 parts by weight, 1 to 20 parts by weight, 1 to 9 parts by weight, 2 to 19 parts by weight, 4 to 17 parts by weight, 20 to 30 parts by weight, 10 to 20 parts by weight, or 1 to 7 parts by weight relative to 100 parts by weight of the second positive electrode active material.

[0061] In addition, the positive electrode slurry may contain 0.05 to 2.0 parts by weight of the lithium cobalt oxide represented by Chemical Formula 1 as the irreversible additive contained in the master batch, relative to 100 parts by weight of the total positive electrode slurry. More specifically, the positive electrode slurry may contain 0.05 to 1.5 parts by weight, 0.05 to 1.0 parts by weight, 0.05 to 0.5 parts by weight, 0.1 to 1.5 parts by weight, 0.1 to 1.0 parts by weight, or 0.1 to 0.9 parts by weight of the lithium cobalt oxide represented by Chemical Formula 1, relative to 100 parts by weight of the total positive electrode slurry.

[0062] In the present invention, by controlling the content of the positive electrode additive masterbatch and the lithium cobalt oxide represented by Chemical Formula 1 contained in the positive electrode slurry within the above range, the dispersibility of the lithium cobalt oxide in the positive electrode slurry can be increased, and the charge / discharge capacity of the manufactured lithium secondary battery can be maximized.

[0063] Meanwhile, the positive electrode slurry according to the present invention includes a first positive electrode active material and a second positive electrode active material contained in a positive electrode additive masterbatch, which are materials capable of reversible intercalation and deintercalation, and in this case, the first positive electrode active material and the second positive electrode active material each include a lithium metal composite oxide represented by Chemical Formula 2, and the components thereof may be the same or different:

[0064] [Chemical formula 2] Li x [Ni y Co z Mn w M2 v ]O u

[0065] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and x, y, z, w, v, and u are 1.0≦x≦1.30, 0.1≦y<1, 0.01 <z≦0.6、0.01<w≦0.6、0≦v≦0.2、1.5≦u≦5である。

[0066] The lithium metal composite oxide represented by the above chemical formula 2 is a composite metal oxide containing lithium, nickel, cobalt and manganese, and in some cases, other transition metals (M 2 For example, the first positive electrode active material and the second positive electrode active material may each be independently doped with LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.05 Al 0.05 O2 and LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2. As an example, the first positive electrode active material and the second positive electrode active material are each a lithium metal composite metal oxide represented by Chemical Formula 2, LiNi 0.6 Co 0.2 Mn 0.2 O2 and LiNi 0.8 Co 0.1 Mn 0.1 O2 can be used alone or in combination.

[0067] The total content of the first positive electrode active material and the second positive electrode active material may be 85 to 95 parts by weight, specifically, 88 to 95 parts by weight, 90 to 95 parts by weight, 86 to 90 parts by weight, or 92 to 95 parts by weight, relative to 100 parts by weight of the positive electrode slurry.

[0068] Moreover, the positive electrode slurry may further include a conductive material and a second binder in addition to the first positive electrode active material and the second positive electrode active material, and in some cases, may further include other additives that can improve the physical properties of the positive electrode.

[0069] In this case, the conductive material can be used to improve the performance of the positive electrode, such as the electrical conductivity, and can be one or more carbon-based materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber. For example, the conductive material may include acetylene black.

[0070] The conductive material may be contained in an amount of 1 to 5 parts by weight, specifically 1 to 4 parts by weight, or 2 to 4 parts by weight, per 100 parts by weight of the total positive electrode slurry.

[0071] The second binder may contain the same or different components as the first binder contained in the positive electrode additive master batch. Specifically, the second binder may contain one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the second binder may contain polyvinylidene fluoride.

[0072] The second binder may be included in an amount of 1 to 5 parts by weight, specifically 1 to 4 parts by weight, or 2 to 4 parts by weight, based on 100 parts by weight of the total positive electrode slurry. The total amount of the first binder and the second binder included in the positive electrode additive masterbatch does not exceed 6 parts by weight based on 100 parts by weight of the total positive electrode slurry.

[0073] In the present invention, by controlling the composition of the positive electrode slurry for lithium secondary batteries as described above, it is possible to prepare a positive electrode slurry in which a small amount of irreversible additive is quantitatively and uniformly dispersed without loss. Therefore, the positive electrode for lithium secondary batteries manufactured using the same has the advantages of not only having high electrical properties and reliability, but also improving design freedom during the manufacture of the positive electrode.

[0074] <Positive electrodes for lithium secondary batteries> In addition, in one embodiment, the present invention provides The positive electrode current collector, the first positive electrode mixture layer, and the second positive electrode mixture layer are sequentially stacked, The first positive electrode mixture layer and the second positive electrode mixture layer are each formed using the above-mentioned positive electrode slurry for a lithium secondary battery of the present invention, thereby providing a positive electrode for a lithium secondary battery.

[0075] The positive electrode for a lithium secondary battery according to the present invention includes a first positive electrode mixture layer and a second positive electrode mixture layer which are produced by applying the above-mentioned positive electrode slurry according to the present invention onto a positive electrode current collector, drying and pressing the same.

[0076] Here, the first positive electrode mixture layer and the second positive electrode mixture layer may have different contents of the lithium cobalt oxide represented by Chemical Formula 1 contained in each layer in order to increase the irreversible efficiency of the lithium cobalt oxide represented by Chemical Formula 1 as the irreversible additive during initial charge and discharge:

[0077] [Chemical formula 1] Li p Co 1-q M 1 q O4

[0078] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.4.

[0079] Specifically, the content of the lithium cobalt oxide represented by Chemical Formula 1 contained in the first positive electrode mixture layer may be 0.5 to 2.0 parts by weight per 100 parts by weight of the first positive electrode mixture layer, and the content of the lithium cobalt oxide represented by Chemical Formula 1 contained in the second positive electrode mixture layer may be 0.01 to 0.5 parts by weight per 100 parts by weight of the second positive electrode mixture layer.

[0080] More specifically, the first positive electrode mixture layer may contain 0.5 to 1.5 parts by weight, 0.5 to 1.0 parts by weight, 0.5 to 0.9 parts by weight, 0.8 to 1.3 parts by weight, or 0.5 to 0.7 parts by weight of the lithium cobalt oxide represented by Chemical Formula 1, relative to 100 parts by weight of the total. The second positive electrode mixture layer may contain 0.05 to 0.5 parts by weight, 0.05 to 0.35 parts by weight, 0.01 to 0.4 parts by weight, 0.01 to 0.3 parts by weight, 0.1 to 0.4 parts by weight, or 0.01 to 0.09 parts by weight of the lithium cobalt oxide represented by Chemical Formula 1, relative to 100 parts by weight of the total.

[0081] As an example, the lithium cobalt oxide represented by Chemical Formula 1 may be included in the first positive electrode mixture layer at 0.6±0.05 parts by weight based on 100 parts by weight of the total first positive electrode mixture layer, and may be included in the second positive electrode mixture layer at 0.2±0.05 parts by weight based on 100 parts by weight of the total second positive electrode mixture layer.

[0082] Furthermore, in the positive electrode for a lithium secondary battery according to the present invention, the total content of the lithium cobalt oxide represented by Chemical Formula 1 contained in the entire positive electrode mixture layer including the first positive electrode mixture layer and the second positive electrode mixture layer may be 0.5 parts by weight or less based on 100 parts by weight of the entire positive electrode active material contained in the two positive electrode mixture layers, i.e., the first positive electrode active material and the second positive electrode active material. More specifically, the total content of the lithium cobalt oxide contained in the entire positive electrode mixture layer of the positive electrode may be 0.01 to 0.5 parts by weight, 0.1 to 0.5 parts by weight, 0.05 to 0.4 parts by weight, 0.05 to 0.25 parts by weight, 0.1 to 0.4 parts by weight, 0.2 to 0.5 parts by weight, 0.1 to 0.3 parts by weight, or 0.4 to 0.5 parts by weight based on 100 parts by weight of the entire positive electrode active material and the second positive electrode active material.

[0083] By controlling the total content of the lithium cobalt oxide represented by Chemical Formula 1 contained in the entire positive electrode composite layer within the above range, the present invention can effectively replenish lithium ions consumed in an irreversible reaction during the initial charge and discharge of a lithium secondary battery, and can prevent a large amount of oxygen gas from being generated due to side reactions or subsequent reactions caused by residues.

[0084] Here, the content of lithium cobalt oxide contained in the positive electrode mixture layer can be adjusted by controlling the content of lithium cobalt oxide contained in the positive electrode slurry of the present invention and the average thickness of each layer. For this purpose, the average thickness of the second positive electrode mixture layer may be formed to be thicker than the average thickness of the first positive electrode mixture layer. Specifically, the ratio of the average thickness of the first positive electrode mixture layer to the second positive electrode mixture layer can be adjusted to 0.1 to 0.9, and more specifically, the ratio of the average thickness of the second positive electrode mixture layer to the first positive electrode mixture layer can be adjusted to 0.1 to 0.8, 0.1 to 0.6, 0.1 to 0.5, 0.1 to 0.3, 0.3 to 0.6, 0.4 to 0.8, 0.2 to 0.5, or 0.6 to 0.9.

[0085] On the other hand, the total thickness of the first positive electrode composite layer and the second positive electrode composite layer is not particularly limited, but may be specifically 50 μm to 300 μm, and more specifically 100 μm to 200 μm, 80 μm to 150 μm, 120 μm to 170 μm, 150 μm to 300 μm, 200 μm to 300 μm, or 150 μm to 190 μm.

[0086] In addition, the positive electrode can be a positive electrode current collector having high conductivity without inducing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. can be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can be formed with fine irregularities on the surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the positive electrode to be manufactured.

[0087] <Lithium secondary battery> Further, in one embodiment, the present invention provides There is provided a lithium secondary battery comprising the positive electrode according to the present invention, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.

[0088] The lithium secondary battery according to the present invention includes the above-described positive electrode of the present invention, and can induce delithiation of the positive electrode additive at a high rate under a low voltage condition equal to or lower than the available voltage during initial charging. Therefore, the amount of oxygen gas generated during subsequent charging and discharging is significantly reduced, and thus the lithium secondary battery has excellent electrical performance and safety.

[0089] The lithium secondary battery of the present invention has a structure including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.

[0090] Here, the negative electrode is manufactured by applying, drying, and pressing a negative electrode active material onto a negative electrode current collector, and may optionally further contain the same conductive material, organic binder polymer, additive, etc. as the positive electrode.

[0091] In addition, the negative electrode active material can be, for example, graphite having a complete layered crystal structure like natural graphite, soft carbon having a low crystalline layered crystal structure (graphene structure; a structure in which hexagonal honeycomb-shaped planes of carbon are arranged in layers), and hard carbon in which such a structure is mixed with an amorphous part, artificial graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, carbon nanotube, fullerene, activated carbon, and other carbon and graphite materials; LixFe2O3 (0 ≦ x ≦ 1), LixWO2 (0 ≦ x ≦ 1), SnxMe1-xMe’yOz (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0 < x ≦ 1, 1 ≦ y ≦ 3, 1 ≦ z ≦ 8), and other metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; titanium oxides; lithium titanium oxides, etc.

[0092] As an example, the negative electrode active material may contain both graphite and silicon (Si)-containing particles. The graphite may include any one or more of natural graphite having a layered crystal structure and artificial graphite having an isotropic structure. The silicon (Si)-containing particles are particles mainly containing silicon (Si) as a metal component, and may include silicon (Si) particles, silicon oxide (SiO2) particles, or a mixture of the silicon (Si) particles and silicon oxide (SiO2) particles.

[0093] In this case, the negative electrode active material may contain 80 to 95 parts by weight of graphite and 1 to 20 parts by weight of silicon (Si)-containing particles, based on a total of 100 parts by weight. By adjusting the contents of graphite and silicon (Si)-containing particles contained in the negative electrode active material within the above ranges, the present invention can reduce lithium consumption and irreversible capacity loss during initial charging and discharging of the battery, and improve the charging capacity per unit mass.

[0094] The negative electrode mixture layer may have an average thickness of 100 μm to 200 μm, specifically, 100 μm to 180 μm, 100 μm to 150 μm, 120 μm to 200 μm, 140 μm to 200 μm, or 140 μm to 160 μm.

[0095] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, copper, stainless steel, nickel, titanium, calcined carbon, etc. can be used. In the case of copper or stainless steel, it is also possible to use a material that has been surface-treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode current collector can be formed with fine irregularities on the surface like the positive electrode current collector to strengthen the binding force with the negative electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the negative electrode current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the negative electrode to be manufactured.

[0096] The separator is a thin insulating membrane having high ion permeability and mechanical strength, which is interposed between the positive and negative electrodes. The separator is not particularly limited as long as it is one commonly used in the industry. Specifically, a sheet or nonwoven fabric made of chemically resistant and hydrophobic polypropylene, glass fiber, or polyethylene may be used. In some cases, a composite separator in which inorganic particles / organic particles are coated with an organic binder polymer on a porous polymer substrate such as the sheet or nonwoven fabric may be used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte may also serve as the separator. The pore diameter of the separator may be an average of 0.01 to 10 μm, and the thickness may be an average of 5 to 300 μm.

[0097] Meanwhile, the positive and negative electrodes may be wound in a jelly roll form and housed in a cylindrical battery, a prismatic battery, or a pouch battery, or may be housed in a pouch battery in a folded or stack-and-folded form, but is not limited thereto.

[0098] The lithium salt-containing electrolyte according to the present invention may be composed of an electrolyte and a lithium salt. The electrolyte may be a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte.

[0099] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0100] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymeric materials containing ionic dissociation groups.

[0101] Examples of the inorganic solid electrolyte that can be used include nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.

[0102] The lithium salt is a substance that is easily dissolved in a non-aqueous electrolyte, and examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium tetraphenylboronate, imides, etc. can be used.

[0103] In addition, for the purpose of improving charge / discharge characteristics, flame retardancy, etc., the electrolyte may contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In some cases, in order to impart non-flammability, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further contained, and in order to improve high-temperature storage characteristics, carbon dioxide gas may be further contained, and fluoroethylene carbonate (FEC), propene sultone (PRS), etc. may be further contained.

[0104] The present invention will now be described in more detail with reference to examples and experimental examples.

[0105] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.

[0106] <Examples 1 to 4 and Comparative Examples 1 to 2. Production of Masterbatches for Positive Electrode Additives> LiNi as the first positive electrode active material 0.6 Co 0.2 Mn 0.2 O2(average particle size(D 50 ):1±0.05μm), Li6Co as a non-reversible additive 0.7 Zinc 0.3 O4(average particle size(D 50 The mixture was then uniformly dry-mixed for about 90 minutes to obtain a pellet-shaped mixture with an average particle size (D 50 ) 0.3±0.005 mm positive electrode additive master batch was produced.

[0107] [Table 1]

[0108] <Examples 5 to 11 and Comparative Examples 3 to 6. Production of Positive Electrode Slurry and Positive Electrode for Lithium Secondary Battery> The positive electrode additive master batches prepared in the above Examples 1 to 4 and Comparative Examples 1 to 2; 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, acetylene black as a conductive material, and PVDF as a second binder were prepared and weighed as shown in Tables 2 and 3 below, and charged into a reactor together with N-methylpyrrolidone (NMP). Next, the mixture was mixed at 3,000 rpm for about 60 minutes to prepare first and second positive electrode slurries for forming a first positive electrode composite layer and a second positive electrode composite layer, respectively.

[0109] Next, the first positive electrode slurry and the second positive electrode slurry were sequentially applied to one side of an aluminum current collector having a size of 10 cm x 20 cm, dried at 100 ° C., and rolled to manufacture a positive electrode. At this time, the total thickness of the positive electrode mixture layer was 130 μm, and the total thickness of the manufactured positive electrode was about 200 μm. In addition, the average thickness T of the first positive electrode mixture layer was 1st and the average thickness T of the second positive electrode composite layer 2nd That is, the ratio T of the average thickness of the second positive electrode composite layer to the average thickness of the first positive electrode composite layer. 1st / T 2nd The ratios of the contents of the components shown in Tables 2 and 3 below may be the same for the positive electrode slurry and the positive electrode mixture layer.

[0110] [Table 2]

[0111] [Table 3]

[0112] <Experimental Example> In order to evaluate the performance of the masterbatch according to the present invention and the positive electrode slurry and positive electrode for lithium secondary batteries containing the masterbatch, the following experiments were carried out.

[0113] B) Evaluation of the amount of oxygen gas generated during initial charging and discharging A negative electrode active material was prepared by mixing natural graphite and silicon particles (Si purity: ≧99.8%) in a weight ratio of 85:15, and 100 parts by weight of the prepared negative electrode active material was mixed with 3 parts by weight of styrene-butadiene rubber (SBR) as a binder to prepare a negative electrode slurry. The prepared negative electrode slurry was coated on one side of a copper current collector with a size of 10 cm × 20 cm and dried to form a negative electrode composite layer (average thickness: 120 μm). At this time, the temperature of the circulating air was 80 ° C. Then, it was rolled and dried in a vacuum oven at 130 ° C for 12 hours to prepare a negative electrode.

[0114] A separator (thickness: about 16 μm) made of a porous polyethylene (PE) film was interposed between the positive electrode and the negative electrode prepared in the above examples and comparative examples, and E2DVC was injected as an electrolyte to prepare a full cell.

[0115] Here, "E2DVC" refers to a type of carbonate-based electrolyte, a solution in which lithium hexafluorophosphate (LiPF6, 1.0M) and vinyl carbonate (VC, 2% by weight) are mixed with a mixture of ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 1:1:1 (volume ratio).

[0116] The produced full cell was activated by charging it at a temperature of 25° C. with a charging current of 0.05 C to a charge cut-off voltage of 4.2 to 4.25 V, and then charging it at 0.02 V until the current density reached 0.01 C. The amount of oxygen gas generated during this process was measured, and the results are shown in Table 4 below.

[0117] B) Evaluation of initial charge / discharge capacity and capacity retention rate Using the positive electrodes prepared in the examples and comparative examples, full cells were prepared in the same manner as the full cell prepared when the amount of oxygen gas generated was measured. The prepared full cells were charged at a temperature of 25° C. with a charging current of 0.05 C to a charge end voltage of 4.2 to 4.25 V, and then activated by charging at 0.02 V until the current density reached 0.01 C. Thereafter, the cells were discharged at a discharge current of 0.05 C to a charge end voltage of 2 V, and the resistance of the electrodes and the initial charge / discharge capacity per unit mass were measured.

[0118] Next, each activated full cell was charged and discharged 100 times (n=100) at 25° C. under the conditions of a charge cut-off voltage of 4.25 V, a discharge cut-off voltage of 2.5 V, and 0.5 C / 0.5 C, to measure the capacity retention (Capacity Retention [%]). The capacity retention was calculated using the following formula 1, and the results are shown in Table 4:

[0119] [Formula 1] Capacity retention rate (%) = (discharge capacity after n charge / discharge cycles / discharge capacity after 1 charge / discharge cycle) x 100

[0120] C) Battery resistance evaluation Using the positive electrodes prepared in the Examples and Comparative Examples, full cells were prepared in the same manner as the full cells prepared when measuring the amount of oxygen gas generated. The prepared full cells were subjected to high-speed charging for 10 seconds to an SOC of 50%, and the surface resistance of the charged secondary battery was measured using the EIS method. The results are shown in Table 4 below.

[0121] [Table 4]

[0122] As shown in Table 4 above, the positive electrode slurry according to the present invention includes a masterbatch containing a high content of a non-reversible additive, and has excellent dispersibility for the non-reversible additive. Therefore, most of the non-reversible additive reacts during the activation step, thereby realizing high charge capacity and charge / discharge capacity retention, and showing low surface resistance.

[0123] More specifically, the lithium secondary battery of the embodiment using the master batch of the embodiment 1-4 containing a high content of lithium cobalt oxide represented by the chemical formula 1 as an irreversible additive in the positive electrode mixture layer has a configuration in which the irreversible additive having a remarkably low content of about 0.55-1.8 parts by weight per 100 parts by weight of the total positive electrode mixture layer is uniformly dispersed in the mixture layer without loss, and it was shown that the amount of oxygen gas generated increases as the irreversible additive reacts at a high rate during the activation stage, thereby confirming that the initial charge capacity is high. It was also shown that the increase in surface resistance due to the use of the irreversible additive is improved.

[0124] From these results, the masterbatch for positive electrode additives according to the present invention contains a high content of irreversible additive together with a positive electrode active material, and thus a small amount of irreversible additive can be dispersed in the positive electrode slurry with a high degree of dispersion without loss during the manufacture of the positive electrode. Therefore, the positive electrode for a lithium secondary battery manufactured using the masterbatch not only has high electrical properties and reliability, but also has the advantage of improving design freedom during the manufacture of the positive electrode.

[0125] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.

[0126] Therefore, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.

Claims

1. A master batch for a positive electrode additive, comprising 0.5 to 50 parts by weight of a lithium cobalt oxide represented by the following Chemical Formula 1 relative to 100 parts by weight of a first positive electrode active material; A second positive electrode active material; A conductive material; a second binder, The lithium cobalt oxide represented by Chemical Formula 1 contained in the master batch is contained in an amount of 0.05 to 2.0 parts by weight based on 100 parts by weight of the total solid content in the positive electrode slurry. Positive electrode slurry for lithium secondary batteries: [Chemical formula 1] Li p Co 1-q M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are within the range of 5≦p≦7 and 0≦q≦0.

4.

2. 2. The positive electrode slurry for lithium secondary batteries according to claim 1, wherein the positive electrode additive master batch contains 1 to 10 parts by weight of the first binder per 100 parts by weight of the first positive electrode active material.

3. Average particle size of the masterbatch for positive electrode additive (D 50 2. The positive electrode slurry for lithium secondary batteries according to claim 1, wherein the particle size is 0.05 mm to 10 mm.

4. The average particle size (D 50 ) is 0.5 to 100 μm, Average particle size of lithium cobalt oxide (D 50 ) is 1 to 200 μm, and 2. The positive electrode slurry for a lithium secondary battery according to claim 1, wherein the average particle size of the lithium cobalt oxide is larger than the average particle size of the first positive electrode active material.

5. The positive electrode slurry for a lithium secondary battery according to claim 1, wherein the lithium cobalt oxide represented by Chemical Formula 1 contained in the master batch is contained in an amount of 0.05 to 1.5 parts by weight based on 100 parts by weight of the total solid content of the positive electrode slurry.

6. 2. The positive electrode slurry for lithium secondary batteries according to claim 1, wherein the positive electrode additive master batch is contained in an amount of 1 to 150 parts by weight per 100 parts by weight of the second positive electrode active material.

7. The positive electrode slurry for a lithium secondary battery according to claim 1, wherein the first positive electrode active material and the second positive electrode active material each contain a lithium metal composite oxide represented by the following Chemical Formula 2: [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u In the above Chemical Formula 2, M 2 represents one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and x, y, z, w, v, and u are each within the ranges of 1.0≦x≦1.30, 0.1≦y<1, 0.01<z≦0.6, 0.01<w≦0.6, 0≦v≦0.2, and 1.5≦u≦5, respectively.

8. 2. The positive electrode slurry for a lithium secondary battery according to claim 1, wherein the conductive material is contained in an amount of 1 to 5 parts by weight based on 100 parts by weight of the total solid content of the positive electrode slurry.

9. 2. The positive electrode slurry for a lithium secondary battery according to claim 1, wherein the second binder is present in an amount of 1 to 5 parts by weight based on 100 parts by weight of the total solid content of the positive electrode slurry.

10. a positive electrode current collector, a first positive electrode mixture layer, and a second positive electrode mixture layer are laminated in this order; The positive electrode for a lithium secondary battery, wherein the first positive electrode mixture layer and the second positive electrode mixture layer are each formed using the positive electrode slurry for a lithium secondary battery according to claim 1 .

11. The content of the lithium cobalt oxide represented by the following Chemical Formula 1 contained in the first positive electrode mixture layer is 0.5 to 2.0 parts by weight per 100 parts by weight of the first positive electrode mixture layer, The content of the lithium cobalt oxide represented by the following Chemical Formula 1 contained in the second positive electrode mixture layer is 0.05 to 0.5 parts by weight per 100 parts by weight of the second positive electrode mixture layer. [Chemical formula 1] Li p Co 1-q M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are within the range of 5≦p≦7 and 0≦q≦0.

4.

12. 11. The positive electrode for a lithium secondary battery according to claim 10, wherein a total content of lithium cobalt oxide contained in the first positive electrode mixture layer and the second positive electrode mixture layer is 0.5 parts by weight or less, based on 100 parts by weight of a total positive electrode active material contained in the first positive electrode mixture layer and the second positive electrode mixture layer.

13. The positive electrode for lithium secondary batteries according to claim 10, wherein a ratio of an average thickness of the first positive electrode mixture layer to that of the second positive electrode mixture layer is 0.1 to 0.

9.

14. A lithium secondary battery comprising the positive electrode according to claim 10, a negative electrode, and a separator located between the positive electrode and the negative electrode.

Citation Information

Patent Citations

  • Nonaqueous electrolyte battery

    JP1997147863A

  • Pre-doping material, positive electrode including pre-doping material, and method for producing non-aqueous electrolyte secondary battery including positive electrode thereof, and method for producing metal oxide

    JP2020123460A

  • Positive electrode additive, method for producing the same, positive electrode and lithium secondary battery containing the same

    JP2020521285A

  • Additive for cathode, method for preparing the same, cathode including the same, and lithium secondary battery including the same

    US20190165412A1

  • Positive electrode for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery

    WO2014118834A1