Manufacturing method of welded joint
A method for welding wear-resistant steel using controlled steel and flux-cored wire compositions and designs prevents cold cracking without preheating, addressing the challenge of cold cracking in low-temperature environments.
Patent Information
- Application Number
- JP2020170056
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-07
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-10-07
AI Technical Summary
Wear-resistant steel used in construction machinery is prone to cold cracking during welding, particularly when using flux-cored wires, which require extensive preheating that is burdensome, especially in low-temperature environments.
A method involving a specific chemical composition for wear-resistant steel plates and flux-cored wires, with controlled Brinell hardness differences, reduced Mn segregation, and controlled nonmetallic inclusions, along with a seamless flux-cored wire design, allows for gas shield welding without preheating, even in low-temperature conditions.
This method significantly reduces the preheating load and prevents cold cracking, enabling reliable welding of wear-resistant steel in environments unsuitable for traditional preheating.
Smart Images

Figure 0007594173000001 
Figure 0007594173000002 
Figure 0007594173000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a welded joint that can obtain a weld metal that is less susceptible to cold cracking when welding high-hardness steel plates with excellent wear resistance that are used in the fields of construction machinery and industrial machinery. [Background technology]
[0002] For example, steel plates used in mining and construction machinery for civil engineering work need to be replaced due to wear, but to extend their useful life as long as possible, wear-resistant steels with increased hardness are used.
[0003] Wear-resistant steel has a high carbon content (C content) to ensure wear resistance, i.e. to increase hardness. This makes cold cracking a problem when welding. In particular, when welding thick steel plates as base materials, such as construction machinery, the stronger restraining force is also a factor that makes cold cracking more likely to occur.
[0004] In order to prevent this cold cracking, preheating is generally performed prior to welding. However, thick steel plates such as wear-resistant steels used in construction machinery, etc., have a very high sensitivity to cold cracking (containing a large amount of alloying elements, mainly C), and therefore require preheating at higher temperatures and for longer periods of time. Therefore, from the viewpoint of improving the working environment and work efficiency, it is desirable to reduce the preheating work as much as possible.
[0005] On the other hand, in the case of a flux-cored wire in which a steel sheath is filled with flux, various functions can be imparted during welding, such as making the bead appearance beautiful and reducing the generation of spatter, by including arc stabilizers, alloy materials, deoxidizers, etc. in the flux. However, since the flux can also be a source of hydrogen absorption, there is a risk of low-temperature cracking occurring when welding wear-resistant steel. For example, when welding high-strength steel with a proof stress of 690 MPa or more, it is said that when the amount of diffusible hydrogen in the weld metal exceeds 4 ml / 100 g, the susceptibility of the weld metal of the high-strength steel to low-temperature cracking increases (see Patent Document 1).
[0006] A method of suppressing cold cracking in such flux-cored wires by adding an appropriate amount of fluoride is known (see, for example, Patent Document 2). That is, it is considered that diffusible hydrogen in the weld metal is reduced by the decomposition of fluoride by the welding arc, and the fluorine generated by the decomposition combines with hydrogen to form HF gas, and this HF gas dissipates into the atmosphere or hydrogen is fixed in the weld metal as HF.
[0007] Furthermore, when abrasion-resistant steel with a Brinell hardness of 450 to 600 is welded, the welded portion, especially the heat-affected zone (HAZ), becomes extremely hard, which affects the occurrence of cold cracking, and in response to this, a method for manufacturing a welded joint has been proposed in which the amount of diffusible hydrogen in the weld metal immediately after welding is less than 1.0 ml / 100 g (see Patent Document 3). That is, in this method, in order to sufficiently reduce the amount of diffusible hydrogen in the weld metal, the flux contains predetermined amounts of fluoride and oxide, and a flux-cored wire is used in which the compounding ratio of these is within a predetermined range.
[0008] Furthermore, a method has been proposed for welding wear-resistant steel while preventing low-temperature cracking by using a flux-cored wire that can sufficiently reduce the amount of diffusible hydrogen in the weld metal as described above and by setting the CEN, which is determined by the alloy components in the weld metal, within a specified range when welding wear-resistant steel (see Patent Document 4). [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 5136466 [Patent Document 2] Patent No. 5644984 [Patent Document 3] International Publication No. 2017 / 154122 [Patent Document 4] Patent No. 5696824 Summary of the Invention [Problem to be solved by the invention]
[0010] As mentioned above, wear-resistant steel has an aspect that it is easy to cause cold cracking during welding. On the other hand, flux-cored wire is more likely to bring in hydrogen than cored wire that does not use flux. Therefore, in order to weld wear-resistant steel using flux-cored wire, preheating work before welding is required, but for thick steel plates such as wear-resistant steel used in construction machines, the preheating work places a great burden on the operator. In order to reduce such preheating work, the above-mentioned Patent Documents 3 and 4 propose a method in which a specific flux-cored wire is used to lower the preheating temperature or to weld wear-resistant steel without preheating work.
[0011] However, even if these flux-cored wires are used, it may not be possible to completely prevent cold cracking unless preheating is performed. For example, when replacing wear-resistant steel used in construction machinery at the work site, or in cold regions or low-temperature environments where the outside air temperature is below 5°C, cold cracking may occur if preheating is insufficient. Therefore, it can be said that there is still room for improvement.
[0012] Under such circumstances, the inventors of the present invention have studied a method for reducing the load of preheating work and enabling welding of wear-resistant steel even in an environment unsuitable for welding, such as a low-temperature environment. In this study, the inventors also focused on the wear-resistant steel to be welded, and thought that measures were necessary not only for the flux-cored wire, which is the welding material, but also for the steel material in order to improve cold cracking. As a result of repeated experiments, it was found that the local alloy-enriched area and the presence of non-metallic inclusions due to solidification segregation in the center of the steel plate thickness become the starting point of cold cracking in wear-resistant steel. Therefore, it was found that the above-mentioned problems can be solved by welding a wear-resistant steel in which this is controlled using a specified flux-cored wire, and the present invention was completed.
[0013] Therefore, an object of the present invention is to provide a method for producing a welded joint by substantially reducing the load of preheating work when welding wear-resistant steel. [Means for solving the problem]
[0014] That is, the gist of the present invention is as follows. (1) Chemical composition, in mass%, C: 0.100~0.350%; Si: 0.10-1.00%; Mn: 0.50-1.50%; P: 0.020% or less; S: 0.005% or less; Al: 0.010~0.100%; B: 0.0005~0.0030%; N: 0.008% or less; O: 0.0050% or less; Cu: 0-1.0%; Ni: 0~3.0%; Cr: 0~2.0%; Mo: 0-2.0%; Nb: 0~0.100%; V: 0~0.100%; Ti: 0~0.100%; Ca: 0~0.005%; Mg: 0~0.005%; REM: 0~0.005%; Balance: Fe and impurities; A method for manufacturing a welded joint by gas-shielded welding using a flux-cored wire having a steel outer sheath filled with flux on an abrasion-resistant steel plate having a plate thickness of 12 to 100 mm, (a) the wear-resistant steel plate has a surface Brinell hardness Y1, which is the Brinell hardness at a depth of 1 mm from the surface, of 400 to 550, and a difference (Y1-Y2) between a central Brinell hardness Y2, which is the Brinell hardness at the center of the plate thickness, and the surface Brinell hardness Y1 is within 40% of the surface Brinell hardness Y1, and is produced by continuous casting, and the amount of Mn segregation in the center of the plate thickness is 2.0% or less, (b) the flux-cored wire contains 0.10 to 2.50% of fluoride in terms of F with respect to the total mass of the wire, has a moisture content of 300 ppm or less, and has a seamless shape with no slit-like gaps in the steel sheath; (c) the chemical composition of the weld metal of the weld joint, in mass%, C: 0.01-0.15%; Si: 0.10-2.00%; Mn: 0.50-2.00%; P: 0.050% or less; S: 0.020% or less; Al: 0.003~0.100%; N: 0.015% or less; B: 0.0100% or less; O: 0.100% or less; Ti: 0.010~0.100%; Cu: 0-1.0%; Ni: 0~3.0%; Cr: 0~2.0%; Mo: 0-2.0%; Nb: 0~0.100%; V: 0~0.100%; Ca: 0~0.005%; Mg: 0~0.005%; REM: 0~0.005%; Balance: Fe and impurities; A method for manufacturing a welded joint, comprising: (2) The wear-resistant steel plate has a density of non-metallic inclusions with a major axis of 10 μm or more observed in the center of the plate thickness of 5.0 pieces / mm 2 A method for manufacturing a welded joint according to (1), which is as follows: (3) The method for manufacturing a welded joint according to (1) or (2), in which a welded joint is manufactured without performing a preheat treatment when gas-shielded welding is performed on the wear-resistant steel plate. (4) The method for manufacturing a welded joint according to any one of (1) to (3), wherein when gas-shielded welding is performed on the wear-resistant steel plate in a low-temperature environment of 5°C or lower, a welded joint is manufactured without performing a preheat treatment. Effect of the Invention
[0015] According to the present invention, even in an environment unsuitable for welding, such as a low-temperature environment, it is possible to prevent low-temperature cracking and weld wear-resistant steel while substantially reducing the load of preheating work, by lowering the preheating temperature, shortening the preheating time, or even eliminating the preheating work. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] In general, in order to improve the wear resistance of wear-resistant steel, it is necessary to add various metals and alloys, and the C content also increases, but this also makes it more susceptible to cold cracking during welding. There is a limit to what the steel material itself can do to improve both wear resistance and cold cracking resistance, so up until now, most research has focused on flux-cored wire, which is a welding material. In contrast, in the present invention, a welded joint is manufactured based mainly on three aspects: the wear-resistant steel plate as the steel material, the flux-cored wire as the welding material, and the weld metal which is affected by the components of both of these materials. This makes it possible to substantially reduce the load of the preheating work and prevent low-temperature cracking even in environments unsuitable for welding, such as low-temperature environments. Each of these will be explained in detail below.
[0017] [Wear-resistant steel plate] In the present invention, the wear-resistant steel plate used as the base material has a surface Brinell hardness Y1, which is the Brinell hardness at a depth of 1 mm from the surface, of 400 to 550, preferably 420 to 530, and the difference (Y1-Y2) between the central Brinell hardness Y2, which is the Brinell hardness at the center of the plate thickness, and the surface Brinell hardness Y1, is set to be within 40%, preferably within 37%, and more preferably within 35%, as a ratio [(Y1-Y2) / Y1] to the surface Brinell hardness Y1.
[0018] If the surface layer Brinell hardness Y1 is 400 to 550, the wear resistance required for a wear-resistant steel plate can be satisfied. If it is less than 400, the wear resistance is insufficient, and if it exceeds 550, it is difficult to ensure the toughness of the steel plate itself, which causes problems in practical use in construction machinery and the like. In addition, if the difference (Y1-Y2) between the central Brinell hardness Y2 and the surface Brinell hardness Y1 is within 40% of the surface Brinell hardness Y1, good wear resistance can be ensured even after the plate thickness is reduced due to long-term use. Here, the central Brinell hardness Y2 only needs to satisfy the above ratio [(Y1-Y2) / Y1], and the value is preferably Y2=300 to 550. The Brinell hardness here represents the Brinell hardness (HBW10 / 3000) measured by the Brinell hardness test specified in JIS Z2243-1:2018 and JIS Z2243-2:2018.
[0019] In addition, in the manufacturing method of the welded joint in the present invention, the wear-resistant steel plate manufactured by continuous casting is used, and the amount of Mn segregation in the center of the plate thickness is 2.0% or less. Generally, there are blooming method and continuous casting method as manufacturing methods of steel material. Of these, the continuous casting method is often used from the viewpoint of manufacturing cost, but in the continuous casting method, an alloy element enriched region due to solidification segregation is formed in the center of the plate thickness, which becomes the final solidified part in the manufacturing process. And, the inventors thought that these become the starting point of cold cracking. That is, in the y-shaped weld crack test method specified in JIS Z3158:1993 used for cold cracking test, cold cracking occurs in the center of the plate thickness, so it is considered that the local alloy element enriched region in the center of the plate thickness becomes a hardened structure during welding and becomes the starting point of cold cracking. The tendency of solidification segregation differs depending on the type of element, but it is considered that the segregation of Mn affects cold cracking, especially in combination with the welding material in the present invention. Therefore, in order to reduce the load of the preheating work, a steel plate with an amount of Mn segregation of 2.0% or less in the center of the plate thickness is used. As described later in the Examples, the amount of Mn segregation was determined by linearly analyzing the Mn concentration in a range of 2 mm or more in the plate thickness direction, with the center position in the thickness direction of the cross section of the wear-resistant steel plate as the median, using an electron probe microanalyzer (EPMA). The maximum value (C) was divided by the overall average value (Co) to determine the component value ratio (C / Co), which was defined as the amount of Mn segregation.
[0020] In addition to the concentration of alloying elements, inclusions are also present in the center of the plate thickness. If the number of coarse inclusions among these inclusions increases, they can become the starting points of cold cracking. In particular, inclusions such as MnS that extend in the rolling direction are likely to act as starting points. Therefore, in addition to the amount of Mn segregation, it is good to control coarse Mn-based inclusions (non-metallic inclusions) such as MnS. Specifically, when the number density of coarse Mn-based inclusions (non-metallic inclusions) with a major axis of 10 μm or more observed in the center of the plate thickness is less than 5.0 pieces / mm 2 It is preferable that the number of particles is 4.0 or less per mm. 2The amount of Mn segregation in the plate thickness center and the number of nonmetallic inclusions with a major axis of 10 μm or more per unit area can be measured by the method described in the Examples below. At present, it is considered that the effective methods for controlling Mn segregation and nonmetallic inclusions in the plate thickness center are solidification structure control during continuous casting and high-temperature heat treatment of the slab, which is the steel plate material. Incidentally, it has been considered macroscopically that low-temperature cracking occurs in proportion to the hardness of the steel material, and that it is important to control the hardness of the weld metal. However, the present invention is characterized in that it controls from a microscopic perspective, such as Mn segregation and metallic inclusions. The method for controlling Mn-based coarse inclusions (nonmetallic inclusions) with a major axis of 10 μm or more is as described above, but it is difficult to reliably reduce the number density to zero, and the lower limit is 0.01 pieces / mm 2 , or 0.1 pieces / mm 2 is the actual value.
[0021] The thickness of the wear-resistant steel plate is generally called thick steel plate and is 12 to 100 mm, which is widely used in places where wear resistance is required in civil engineering and construction machinery, industrial machinery, etc. The reason for specifying the chemical composition of the wear-resistant steel plate is as follows. In these explanations, "%" means "mass %" unless otherwise specified.
[0022] (C:0.100~0.350%) C is the most effective element for improving the surface hardness of wear-resistant steel plates, and is also an inexpensive element. If the C content is less than 0.100%, it becomes necessary to add other alloy elements to compensate for the reduced hardness, which increases costs. On the other hand, if the C content exceeds 0.350%, the workability is significantly deteriorated and the delayed fracture resistance is significantly impaired.
[0023] (Si: 0.10 to 1.00%) Silicon contributes to improving the surface hardness and delayed fracture resistance of wear-resistant steel plates. If the silicon content is less than 0.10%, these effects are insufficient. On the other hand, if the silicon content exceeds 1.00%, the workability is significantly deteriorated and the toughness, which affects the thermal cracking resistance, is deteriorated.
[0024] (Mn: 0.50-1.50%) Mn improves the surface hardness of wear-resistant steel plates by improving hardenability. If the Mn content is less than 0.50%, other alloy elements must be added to compensate for the hardness, which increases costs. On the other hand, if the Mn content exceeds 1.50%, the workability is significantly deteriorated and the delayed fracture resistance is significantly impaired.
[0025] (P:0.020% or less) P is present as an inevitable impurity in steel and segregates at grain boundaries, degrading the delayed fracture resistance and toughness of the steel, so it is desirable to keep its content as low as possible. In particular, if the P content exceeds 0.020%, the degradation becomes significant.
[0026] (S:0.005% or less) S is an inevitable impurity element that deteriorates the ductility and toughness of steel. If the S content exceeds 0.005%, such adverse effects become evident.
[0027] (Al: 0.010~0.100%) Al effectively suppresses the overgrowth of primary austenite grains by generating AlN during slab heating. If the Al content is less than 0.010%, this effect is small. On the other hand, if the Al content exceeds 0.100%, the workability and toughness are significantly deteriorated.
[0028] (B: 0.0005~0.0030%) B is an element effective in improving hardenability. In order to promote the formation of martensite and increase the Brinell hardness of the wear-resistant steel plate, the B content is set to 0.0005% or more. On the other hand, if the B content is excessive, the toughness of the base material and the welded part deteriorates, so the upper limit is set to 0.0030%.
[0029] (N:0.008% or less) N is an unavoidable impurity contained in steel. If present in large quantities, it causes deterioration of HAZ toughness. Furthermore, if the N content exceeds 0.008%, it significantly deteriorates workability and the toughness of both the base material and the HAZ cannot be avoided.
[0030] (O:0.0050% or less) O is also an impurity that is inevitably contained in steel. If the O content exceeds 0.0050%, the amount of nonmetallic inclusions in the steel increases, significantly deteriorating the workability and impairing the low-temperature toughness.
[0031] (Cu:0~1.0%, Ni:0~3.0%, Cr:0~2.0%, Mo:0~2.0%) Cu, Ni, Cr, and Mo have the effect of improving the strength and toughness of the base material, so they may be added as necessary. However, if their contents are excessive, the hardness of the HAZ in particular may increase and the toughness may be impaired, so the upper limits are specified as above. The preferred contents (lower limits) for obtaining the effect of addition are 0.05% for Cu, 0.05% for Ni, 0.05% for Cr, and 0.02% for Mo.
[0032] (Nb:0~0.100%, V:0~0.100%, Ti:0~0.100%) Nb, V, and Ti may be added as necessary because they have the effect of suppressing the coarsening of crystal grains by forming carbides and nitrides. However, if the content is excessive, the coarsening of precipitates becomes significant and there is a risk of reducing toughness, so the upper limit is specified for each as above. The preferred content (lower limit) for obtaining the effect of addition is 0.010% for Nb, 0.010% for V, and 0.005% for Ti.
[0033] (Ca:0~0.005%, Mg:0~0.005%, REM:0~0.005%) Ca, Mg, and REM may be contained as necessary because nonmetallic inclusions become spheroidized and low-temperature toughness can be improved when contained. However, if the content is excessive, the inclusions become coarse and may become the starting point of fracture, which may impair toughness, so the upper limit is specified for each as above. The preferred content (lower limit) for obtaining the effect of addition is 0.001% for Ca, 0.001% for Mg, and 0.001% for REM. Here, REM refers to a total of 17 elements, including 15 elements with atomic numbers 57 to 71, and two elements Sc and Y, and any one of them or a mixture of two or more of them can be used. The content of REM is the total content of the 17 elements.
[0034] The balance of the above components is iron (Fe) and impurities. Here, the term "impurities" refers to components that are mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, during industrial production of steel, and are permissible within a range that does not adversely affect the present invention.
[0035] In addition, the carbon equivalent (Ceq) expressed by the following formula (1) and calculated from the steel components (mass%) is preferably 0.35 to 0.70%. By making Ceq 0.35% or more, it is easy to ensure wear resistance. On the other hand, by making Ceq 0.70% or less, low temperature cracking can be more reliably suppressed. Ceq=C+Mn / 6+(Cu+Ni) / 15+(Cr+Mo+V) / 5 ···(1) [C, Mn, Cu, Ni, Cr, Mo and V represent the content (mass%) of each element, and if not contained, it is set to 0.]
[0036] [Flux-cored wire] In the present invention, the welding material is a flux-cored wire in which a steel sheath is filled with flux, and this flux-cored wire contains 0.10 to 2.50% of fluoride, preferably 0.15 to 2.00%, in terms of F, relative to the total mass of the wire. As described above, in general, in a flux-cored wire, the flux is a hydrogen adsorption source, so that cold cracking is likely to occur, but the amount of hydrogen in the arc atmosphere during welding can be reduced by adding an appropriate amount of fluoride. This is considered to be because fluorine and hydrogen form a compound during welding. In order to realize such a function, the content of fluoride in terms of F must be 0.10% or more relative to the total mass of the flux-cored wire. On the other hand, excessive addition may impair weldability, such as the generation of spatters, so the upper limit is set to 2.50% or less. In the explanation of the flux-cored wire, "%" means "mass %" unless otherwise specified.
[0037] There is no particular restriction on the fluoride, but it is preferable to use one or more of CaF2, BaF2, SrF2, MgF2, LiF, NaF, K2ZrF6, K2SiF6, Na3AlF6, etc. Ca, Ba, Sr, Mg, Li, Na, K, Zr, Si, and Al generated by ionization of these fluorides combine with oxygen to act as deoxidizing elements that reduce the amount of oxygen in the weld metal, so these fluorides are advantageous in terms of improving the toughness of the weld metal. Note that the F equivalent value indicates the amount of fluorine (F) contained in the fluoride in mass% relative to the total mass of the flux-cored wire, so for example, in the case of the above-mentioned fluoride, this F equivalent value can be calculated from the following formula (2). Here, the chemical formula of the fluoride in formula (2) indicates the mass% of the fluoride corresponding to each chemical formula relative to the total mass of the flux-cored wire. The coefficients of the chemical formula of each fluoride were calculated from the chemical formula weight of each fluoride. 0.487×CaF2+0.610×MgF2+0.732×LiF+0.452×NaF+0.402×K2ZrF6+0.217×BaF2+0.517×K2SiF6+0.543×Na3AlF6… …Formula (2)
[0038] The moisture content of the flux-cored wire used in the present invention is set to 300 ppm or less, preferably 250 ppm or less. As mentioned above, the flux-cored wire may contain a large amount of hydrogen, which is a cause of low-temperature cracking. Therefore, in order to reduce the load of preheating work as in the present invention, and to reduce the load of preheating work and enable welding of wear-resistant steel even under conditions unsuitable for welding, such as low-temperature environments, it is necessary to reduce the moisture content in the wire as described above in addition to adding a specified fluoride.
[0039] Here, even if the hydrogen content of the flux-cored wire is reduced during its manufacturing process, moisture absorption may occur due to changes over time until the actual welding process. In particular, when the flux-cored wire is stored for a long period of time after manufacturing, the problem of moisture absorption becomes more pronounced with the crimping method that is sometimes used when filling the wire with flux. Therefore, in the present invention, a seamless flux-cored wire is used, in which there are no slit-shaped gaps in the steel sheath.
[0040] To produce such seamless type flux-cored wire, for example, a steel strip to be the steel outer sheath is formed into an open tube (U-shaped) by a forming roll while being fed in the longitudinal direction, and this is used as the steel outer sheath. In this case, flux is supplied from the opening of the open tube during the forming of the steel strip, and after the forming of the steel strip, the opposing edge faces of the opening are butt-welded to obtain a seamless tube. Next, this seamless tube is drawn, and the seamless tube is annealed during or after the drawing process, thereby producing a seamless type flux-cored wire. In this way, by completely sealing the flux inside by forming it into a seamless shape, it becomes possible to remove moisture brought inside by the flux, for example by the above-mentioned annealing process. The method for reducing the moisture content is not limited to the annealing treatment. For example, the flux components to be filled as the flux may be melted by arc or high-frequency induction heating, and then extracted into a crucible, and then crushed into amorphous powder, or may be made into amorphous powder by gas atomization, and then filled as a molten flux that is less likely to absorb moisture.
[0041] The flux may contain one or more metal oxides such as TiO2, SiO2, ZrO2, MgO, Al2O3, CaO, etc., as slag forming materials having the effect of maintaining the weld bead shape in good condition. Furthermore, the flux may contain metal oxides contained in binders, etc., used for granulating the flux. In addition to these, the flux may contain, for example, iron powder or other alloy powder, and may contain metal carbonates (CaCO3) or the like as arc stabilizers.
[0042] [Welding metal] In the present invention, as described above, a welded joint is manufactured by gas-shielded welding a given wear-resistant steel plate using the above-mentioned flux-cored wire, but in order to suppress cold cracking, the component values of the weld metal must also be considered. In particular, since the chemical components of the weld metal are determined by the supply from the welding material and dilution from the base metal, the target chemical composition of the weld metal when setting the components of the flux-cored wire and wear-resistant steel plate is as described below. In these descriptions, "%" stands for "mass %" unless otherwise specified.
[0043] (C: 0.01~0.15%) C is the element that has the greatest effect on the hardness of weld metal. If the steel is to be made wear-resistant, the C content must be 0.15% or less in order to omit preheating. On the other hand, an excessive decrease in C content leads to a decrease in the strength of the weld metal, so it must be 0.01% or more.
[0044] (Si: 0.10~2.00%) Silicon is a deoxidizing element, and in order to reduce the O content in the weld metal and increase its cleanliness, a certain amount of silicon must be added to the flux of the flux-cored wire, which must be at least 0.10%. However, excessive addition of silicon deteriorates the toughness of the weld metal, so the content must be kept at 2.00% or less.
[0045] (Mn: 0.50~2.00%) Mn forms MnS and has the effect of suppressing grain boundary embrittlement caused by S. In addition, Mn is an element that has the effect of ensuring the hardenability of the weld metal and increasing its strength, so it is necessary to obtain a stable hardness, and so its content is set to 0.50% or more. On the other hand, if it is contained excessively, the grain boundary embrittlement susceptibility increases and the toughness of the weld metal deteriorates, so it is set to 2.00% or less.
[0046] (P:0.050% or less) P is an impurity element that deteriorates toughness. Therefore, it is necessary to reduce its content as much as possible, but the P content in the weld metal is set to 0.050% or less as the allowable range for the adverse effect on toughness.
[0047] (S:0.020% or less) S is also an impurity element, and since excessive presence in the weld metal deteriorates both toughness and ductility, it is preferable to reduce it as much as possible. The S content in the weld metal is set to 0.020% or less, which is the allowable range for adverse effects on toughness and ductility.
[0048] (Al: 0.003 to 0.100%) Al is a deoxidizing element, and like Si, it has the effect of improving the cleanliness of the weld metal by reducing the O content in the weld metal, so it is necessary to include it at 0.003% or more. On the other hand, if it is included in excess, it forms nitrides and oxides that deteriorate the toughness of the weld metal, so the content is set to 0.100% or less.
[0049] (N: 0.015% or less) N is unavoidably contained in weld metal. However, excessive N content forms coarse AlN and BN, which reduces toughness, so the content is set to 0.015% or less.
[0050] (B:0.0100% or less) When an appropriate amount of B is contained in the weld metal, it combines with solute N to form BN, which has the effect of reducing the adverse effect of solute N on toughness. B also has the effect of improving hardenability and contributing to improved strength. To obtain these effects, it can be included as a selective element. On the other hand, if the B content exceeds 0.0100%, the B in the weld metal becomes excessive, resulting in the formation of coarse BN and Fe. 23 This is not preferable because it forms B compounds such as (C, B)6, which in turn deteriorates toughness. Therefore, the upper limit of the B content when B is included is set to 0.0100%. The preferable lower limit for obtaining such an effect is 0.0003%. Note that if the flux-cored wire does not contain B and the B content in the wear-resistant steel plate is close to the lower limit, there is a possibility that the amount of B in the weld metal will be so small that it falls below the analytical limit, so no lower limit is specified here.
[0051] (O: 0.100% or less) O is unavoidably contained in weld metal. However, if contained in excess, it is unavoidable that it adversely affects toughness and ductility. Therefore, the upper limit of the O content is set at 0.100%.
[0052] (Ti: 0.010~0.100%) Like Al, Ti is also effective as a deoxidizing element and has the effect of reducing the O content in the weld metal, so it is necessary to contain 0.010% or more. On the other hand, if it is excessive, it causes deterioration in toughness due to the formation of coarse oxides and deterioration in toughness due to excessive precipitation strengthening, so the upper limit is set at 0.100%.
[0053] (Cu:0~1.0%, Ni:0~3.0%, Cr:0~2.0%, Mo:0~2.0%) Cu, Ni, Cr, and Mo can be added as optional elements because they can improve the strength and toughness of the weld metal as solid solution elements. However, excessive addition of these elements not only impairs economic efficiency but can also lead to a decrease in toughness, so the upper limits of each element are specified as above. The preferred contents (lower limits) for obtaining the effect of addition are 0.05% for Cu, 0.05% for Ni, 0.05% for Cr, and 0.03% for Mo.
[0054] (Nb: 0-0.100%, V: 0-0.100%) Nb and V are elements effective in improving the hardness of the weld metal as solid solution elements or by forming carbonitrides, and can be included as optional elements. On the other hand, excessive inclusion of these elements can reduce toughness, so the upper limits of each element are specified as above. The preferred contents (lower limits) for obtaining the effect of addition are 0.010% for Nb and 0.010% for V.
[0055] (Ca:0~0.005%, Mg:0~0.005%, REM:0~0.005%) Mg, Ca, and REM change the structure of sulfides in the weld metal and are effective in improving ductility and toughness by reducing the size of sulfides and oxides, and can be included as optional elements. On the other hand, excessive inclusion of these elements causes the sulfides and oxides to coarsen, leading to deterioration of ductility and toughness, so the upper limits for each element are specified as above. The preferred contents (lower limits) for obtaining the effect of addition are 0.001% for Ca, 0.001% for Mg, and 0.001% for REM. The same applies to REM as described above.
[0056] The weld metal having the above chemical composition may contain impurities mixed in during the manufacturing process, etc., to the extent that the remainder, which is mainly composed of iron (Fe), does not impair the characteristics of the welded joint according to this embodiment.
[0057] In the present invention, not only a specified flux-cored wire is used as the welding material, but also a specified wear-resistant steel plate is used as the steel material, so that the load of the preheating work can be substantially reduced and cold cracking can be prevented. For example, the preheating temperature can be lowered, the time of the preheating work can be shortened, and cold cracking can be prevented even when a welded joint is manufactured without preheating work. In particular, according to the present invention, the load of the preheating work can be reduced even in a situation unsuitable for welding, such as a low-temperature environment. Until now, the y-type weld cracking test method specified in JIS Z3158:1993 has usually been used to evaluate cold cracking, and the heat input is 17 kJ / cm and the evaluation is performed at room temperature. On the other hand, there may be a situation where the environment is even lower in temperature and the heat input is even smaller during actual construction, so in the present invention, as shown in the examples described later, the load of the preheating work can be reduced and cold cracking can be prevented even in a low-temperature environment of 5°C or less.
[0058] In the present invention, the method of gas-shielded arc welding is not particularly limited, and a commonly used method can be adopted. For example, as the shielding gas, a mixed gas of Ar gas and 3-20 vol% CO2 gas, etc. can be used in addition to 100% CO2 gas. The flow rate of the shielding gas can be set to normal conditions, that is, about 15-30 L / min. There is also no particular limit to the welding conditions such as current and voltage, and for example, the current is 200-350 A, and the voltage is 25-35 V. In this case, the welding speed may be controlled so that the welding heat input is 10-50 kJ / cm.
[0059] Furthermore, the shape of the welded joint to be manufactured is determined according to the application, etc., and is not particularly limited. It can be applied to welded joints that form a groove, such as normal butt joints, corner joints, and T-joints. Therefore, the shape of the steel plate to be welded may be such that at least the portion that forms the welded joint is plate-shaped, and the entire shape does not have to be a plate, and includes, for example, shaped steel. In addition, it is not limited to being composed of separate steel plates, and may be a butt welded joint of a single steel plate formed into a predetermined shape, such as a tubular shape. EXAMPLES
[0060] Next, the present invention will be described based on examples, but the present invention is not limited to these examples.
[0061] (Test Example 1) Steel plates 1 to 35 having the components shown in Table 1-1 (the balance being Fe and impurities) and the plate thicknesses shown in Table 1-2 were used as the base materials (materials to be welded). The same steel plates as the base materials were used as backing metals for welding. Ceq in Table 1-1 is the carbon equivalent expressed by the above formula (1).
[0062] To obtain these steel plates, slabs of 250 mm thickness were produced by continuous casting. In order to control inclusions at the center of the plate thickness, the temperature of the molten steel was not excessively high during the continuous casting process, and the difference was controlled to within 50°C from the solidification temperature determined by the molten steel composition. Furthermore, electromagnetic stirring was performed immediately before solidification and reduction was performed during solidification. The slab was subjected to a heat treatment of holding it at 1200 to 1300°C for 5 hours or more as necessary to control center segregation. Subsequently, steel plates of 12 to 100 mm thickness were produced by hot rolling. The rolled steel plates were heated at 900 to 1000°C and then water-cooled to adjust the surface hardness. The steel plates may be directly water-cooled after rolling.
[0063] For the obtained steel plates 1 to 35, the amount of Mn segregation in the center of the plate thickness in the cross section perpendicular to the rolling direction (C direction) of the steel plate was determined, and non-metallic inclusions with a major axis of 10 μm or more were measured. Of these, the amount of Mn segregation was determined using an electron probe microanalyzer (EPMA). Specifically, the Mn concentration was linearly analyzed using an electron probe microanalyzer (EPMA) in a range of 2 mm or more in the plate thickness direction, with the center position in the thickness direction of the cross section of the wear-resistant steel plate as the median, and the component value ratio (C / Co) was determined by dividing the maximum value (C) by the overall average value (Co), and this was taken as the amount of Mn segregation. On the other hand, the measurement of non-metallic inclusions with a major axis of 10 μm or more was performed using the center position in the thickness direction as the median. and Observe the area of 2 mm in the plate thickness direction and 10 mm wide with an optical microscope, and count the number of nonmetallic inclusions with a major axis of 10 μm or more. 2 ) was calculated.
[0064] In addition, the surface Brinell hardness Y1, which is the Brinell hardness at a depth of 1 mm from the surface of these steel plates 1 to 35, and the central Brinell hardness Y2, which is the Brinell hardness at the center of the plate thickness, were measured. Among these, in the measurement of the surface Brinell hardness Y1, grinding was performed in the plate thickness direction, and the test surface was polished as a test surface at a depth of 1 mm from the surface, and the Brinell hardness was measured in accordance with JIS Z2243-1:2018 and JIS Z2243-2:2018. In addition, in the measurement of the central Brinell hardness Y2, grinding and cutting were performed to the center of the plate thickness, and the test surface was polished as a test surface at the center of the plate thickness, and the Brinell hardness was measured in accordance with JIS Z2243-1:2018 and JIS Z2243-2:2018. These results are shown in Table 1-2, and the ratio of the difference between the surface Brinell hardness Y1 and the central Brinell hardness Y2 to the surface Brinell hardness Y1 is also shown. For the measurement of the Brinell hardness, a tungsten hard ball with a diameter of 10 mm was used, the load was set to 3000 kgf, the test was performed at five points on each test surface, and the average value of the five points was taken as the Brinell hardness HBW (10 / 3000).
[0065] [Table 1-1]
[0066] [Table 1-2]
[0067] In addition, the flux-cored wires used as the welding materials were Wires 1 to 35 shown in Table 2. These were manufactured by the following method. First, the flux was made into a bond type by mixing oxide, fluoride and metal powders, granulating them with a binder, and drying them to make the flux. The fluorides in the flux were one or more selected from CaF2, BaF2, SrF2, MgF2, LiF, NaF, K2ZrF6, K2SiF6 and Na3AlF6, and the F equivalent values were as shown in Table 2. In addition, metal oxides were included as slag forming materials and arc stabilizers.
[0068] In addition, a steel strip was formed as a steel outer skin into a U-shaped open tube, and during this forming process, flux was supplied from the opening of the open tube, and both opposing edges of the opening were butt-welded (seam-welded) to form a seamless tube without a seam. At this time, a portion was used as a comparative material, and instead of seam welding, it was crimped to form a tube with a gap. Each of these was drawn to obtain a flux-cored wire with a final wire diameter of φ1.2 mm. At this time, the seamless tube without a seam was annealed at a temperature range of 650 to 950°C for more than 4 hours during the drawing process.
[0069] The moisture content (moisture content) of the wires 1 to 35 obtained above was measured. The moisture content was measured by the Karl Fischer method (KF method) in accordance with JIS K 0068:2001. The measurement samples were prepared by cutting the wires to lengths of 1 to 2 mm, and 1 to 5 g of the sample was collected. The measurement samples were inserted into a furnace heated to 900°C, and the vaporized moisture was measured by coulometric titration.
[0070] [Table 2]
[0071] Using this flux-cored wire, the above steel plates were butted together with a root gap of 16 mm and a groove angle of 20°, and welded using a backing metal. The welding conditions were a current of 270 A, a voltage of 30 V, and a welding speed of 30 cm / min. 100% CO2 was used as the shielding gas, with a flow rate of 25 L / min. Preheating was not performed, and the temperature between welding passes was set to 200°C or less. The chemical composition analysis results of the obtained weld metal are shown in Table 3. Note that each test number of this welding test indicates a combination of the number of the steel plate, which is the base material, and the number of the flux-cored wire. In other words, test number 1-1 means that welding was performed using steel plate 1 as the base material and wire 1 as the welding material, and similarly, the test number below indicates a combination of "steel plate number-wire number".
[0072] In addition, a low-temperature cracking test was conducted on the welds with the same combination of steel plate and flux-cored wire as above, using the test number. The low-temperature cracking test was conducted in accordance with JIS Z3158:2016 (Y-type weld cracking test method). However, the test temperature was 5°C. At that time, the flux-cored wire side was made positive, the welding position was downward, the current value was 270A, the voltage was 30V, and the welding speed was 30cm / min. In addition, 100% CO2 was used as the shielding gas, and the flow rate was 25L / min. If there were no cracks on either the surface or the cross section, the test was considered to have passed (no cracks), and if cracks were found on either one, the test was considered to have failed (cracks). Furthermore, the amount of diffusible hydrogen per mass of the weld metal was measured when the same combination of steel plate and flux-cored wire was used as above and welded. The measurements were performed using a gas chromatograph method in accordance with JIS Z 3118:2007 (Method for measuring hydrogen content in steel welds), with 100% CO2 used as the shielding gas at a flow rate of 25 L / min, the welding position facing downward, the current value of 270 A, the voltage of 30 V, and the welding speed of 35 cm / min. The results are shown in Table 4.
[0073] [Table 3]
[0074] [Table 4]
[0075] As shown in Table 4, the method according to the present invention can provide a welded joint free of cracks in the y-type weld crack test method with a test temperature of 5° C. Therefore, by performing gas shielded welding using a specified flux-cored wire on an abrasion-resistant steel plate with a small amount of Mn segregation in the center of the plate thickness, it becomes possible to prevent low-temperature cracking and weld the abrasion-resistant steel while substantially reducing the load of the preheating work by lowering the preheating temperature, shortening the preheating time, or not performing the preheating work, even in a low-temperature environment unsuitable for welding.
Claims
1. The chemical composition, in mass%, is C: 0.100-0.350%; Si: 0.10-1.00%; Mn: 0.50-1.50%; P: 0.020% or less; S: 0.005% or less; Al: 0.010-0.100%; B: 0.0005-0.0030%; N: 0.008% or less; O: 0.0050% or less; Cu: 0-1.0%; Ni: 0-3.0%; Cr: 0-2.0%; Mo: 0-2.0%; Nb: 0-0.100%; V: 0-0.100%; Ti: 0-0.100%; Ca: 0-0.005%; Mg: 0-0.005%; REM: 0-0.005%; Balance: Fe and impurities; The method comprises the steps of: performing gas shield welding on an abrasion-resistant steel plate having a plate thickness of 12 to 100 mm using a flux-cored wire having a steel outer sheath filled with flux, and manufacturing a welded joint, (a) The wear-resistant steel plate has a surface Brinell hardness Y, which is the Brinell hardness at a depth of 1 mm from the surface. 1 is 400 to 550, and the central Brinell hardness Y is the Brinell hardness at the center of the thickness of the wear-resistant steel plate, which is the center position in the thickness direction of the wear-resistant steel plate. 2 and the surface layer Brinell hardness Y 1 The difference between 1 -Y 2 ) is the surface layer Brinell hardness Y 1 and the steel sheet is produced by continuous casting, and the amount of Mn segregation determined by linear analysis of a range of 2 mm in the thickness direction including the center portion of the thickness direction using an electron probe microanalyzer is 2.0% or less. (b) the flux-cored wire contains 0.10 to 2.50% of fluoride in terms of F with respect to the total mass of the wire, has a moisture content of 300 ppm or less, and has a seamless shape with no slit-like gaps in the steel sheath; (c) the chemical composition of the weld metal of the weld joint, in mass%, C: 0.01-0.15%; Si: 0.10-2.00%; Mn: 0.50-2.00%; P: 0.050% or less; S: 0.020% or less; Al: 0.003-0.100%; N: 0.015% or less; B: 0.0100% or less; O: 0.100% or less; Ti: 0.010-0.100%; Cu: 0-1.0%; Ni: 0-3.0%; Cr: 0-2.0%; Mo: 0-2.0%; Nb: 0-0.100%; V: 0-0.100%; Ca: 0-0.005%; Mg: 0-0.005%; REM: 0-0.005%; Balance: Fe and impurities; and A method for producing a welded joint, characterized in that Ceq calculated by the following formula (1) is 0.35 to 0.70%. Ceq=C+Mn / 6+(Cu+Ni) / 15+(Cr+Mo+V) / 5...(1)
2. The wear-resistant steel plate has a number density of nonmetallic inclusions having a major axis of 10 μm or more of 5.0 pieces / mm when observed with an optical microscope within a range of 2 mm in the plate thickness direction and 10 mm in width from the plate thickness center. 2 The method for manufacturing a welded joint according to claim 1, wherein:
3. The method for manufacturing a welded joint according to claim 1 or 2, wherein a welded joint is manufactured without performing a preheat treatment when gas-shielded welding is performed on the wear-resistant steel plate.
4. The method for manufacturing a welded joint according to any one of claims 1 to 3, wherein when gas-shielded welding is performed on the wear-resistant steel plate in a low-temperature environment of 5°C or less, a welded joint is manufactured without performing a preheat treatment.
Citation Information
Patent Citations
Isoshichijinrui no seizoho
JP1976036466A
Print head driving system of dot printer
JP1981044984A
Manufacture of stabilizer for discharge lamp
JP1981096824A
Method for removing deposit of electrode tip in resistance welding machine and device therefor
JP1996025061A
Thick-walled high temperature wear resistant steel with high toughness
JP2001049387A
Cited By
Flux-cored wire for gas shielded arc welding and method for manufacturing welded joints
JP2026164547A