Semiconductor device, manufacturing method thereof, and electronic device
A graded Al composition cap layer in the semiconductor device structure addresses high contact resistance issues by enhancing ohmic contact, leading to a high-performance device with low on-resistance.
Patent Information
- Application Number
- JP2020186659
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-09
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-11-09
AI Technical Summary
Semiconductor devices using nitride semiconductors face high contact resistance due to the large bandgap of the barrier layer, leading to increased resistance in the electron transport path and potential failure to achieve high performance characteristics.
A semiconductor device configuration with a channel layer, a barrier layer, and a cap layer having a graded Al composition that increases from the barrier layer side toward the source and drain electrodes, reducing contact resistance by introducing positive charges and expressing n-type properties, thereby lowering the barrier at the electrode contacts.
The configuration achieves good ohmic contact and reduces contact resistance, resulting in a high-performance semiconductor device with low on-resistance.
Smart Images

Figure 0007594176000001 
Figure 0007594176000002 
Figure 0007594176000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor device, a method for manufacturing a semiconductor device, and an electronic device. [Background technology]
[0002] As a semiconductor device using a nitride semiconductor, for example, a high electron mobility transistor (HEMT) using GaN (gallium nitride) for the channel layer (also called "electron transport layer") and AlGaN (aluminum gallium nitride) for the barrier layer (also called "electron supply layer") is known. Regarding such HEMT, a technology is known in which a cap layer of GaN or InAlGaN (indium aluminum gallium nitride) is further provided on the barrier layer of AlGaN.
[0003] Also, a HEMT is known that uses GaN for the channel layer and InAlN (indium aluminum nitride) for the barrier layer. Regarding such HEMTs, other known technologies include a technology of providing an InAlN barrier layer on a Ga-polarity GaN channel layer, a technology of providing a GaN channel layer on an N-polarity InAlN barrier layer, and a technology of further providing an InGaN (indium gallium nitride) or AlN (aluminum nitride) cap layer on the channel layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-041542 A [Patent Document 2] JP 2016-187025 A Summary of the Invention [Problem to be solved by the invention]
[0005] In a semiconductor device using a nitride semiconductor, a structure in which a barrier layer of a nitride semiconductor having a larger band gap is provided on a channel layer of the nitride semiconductor can be adopted. Two-dimensional electron gas (2DEG) is generated in the channel layer due to spontaneous polarization of the barrier layer and piezoelectric polarization caused by strain due to the difference in lattice constant between the barrier layer and the channel layer.
[0006] However, in a semiconductor device employing such a structure, the barrier between the electrode and the barrier layer is large due to the relatively large band gap, and the contact resistance may become high. If the contact resistance becomes high in this way, the resistance of the electron transport path in the semiconductor device increases, and there is a risk that a high-performance semiconductor device with sufficient characteristics cannot be obtained.
[0007] In one aspect, the present invention aims to realize a high-performance semiconductor device having low contact resistance. [Means for solving the problem]
[0008] In one embodiment, a channel layer including a first nitride semiconductor and a gate insulating film provided on a first surface side of the channel layer, Contains Al and In The present invention provides a semiconductor device having: a barrier layer including a second nitride semiconductor; a first cap layer provided on a second surface side of the barrier layer opposite to the channel layer side, the first cap layer including a third nitride semiconductor containing Al and at least one of Ga and In, the Al composition increasing from the barrier layer side toward the third surface side opposite to the barrier layer side; a source electrode and a drain electrode provided on the third surface side of the first cap layer and in contact with the third surface; and a gate electrode provided on the third surface side of the first cap layer, located between the source electrode and the drain electrode, the gate electrode having a lower end on the barrier layer side located on the third surface side of the first cap layer.
[0009] In another aspect, there is provided a method for manufacturing the semiconductor device as described above, and an electronic device including the semiconductor device as described above. Effect of the Invention
[0010] In one aspect, it is possible to realize a high-performance semiconductor device having low contact resistance. [Brief description of the drawings]
[0011] [Figure 1] 1A and 1B are diagrams illustrating an example of a semiconductor device. [Diagram 2] 1A to 1C are diagrams illustrating problems that may occur in a semiconductor device. [Diagram 3] 1A to 1C are diagrams illustrating a low-resistance layer regrowth technique for a semiconductor device. [Figure 4] FIG. 1 is a diagram illustrating an example of a semiconductor device according to a first embodiment. [Diagram 5] FIG. 2 is a diagram for explaining the relationship between the Al composition and spontaneous polarization of a nitride semiconductor. [Figure 6] FIG. 2 is a diagram illustrating an energy band structure of an example of the semiconductor device according to the first embodiment. [Figure 7] 1A to 1C are diagrams illustrating a modified example of the semiconductor device according to the first embodiment. [Figure 8] 1A to 1C are diagrams for explaining an example of a method for forming a semiconductor device according to a first embodiment; [Figure 9] 5A to 5C are diagrams (part 2) illustrating an example of a method for forming a semiconductor device according to the first embodiment; [Figure 10] 5A to 5C are views (part 3) illustrating an example of a method for forming a semiconductor device according to the first embodiment; [Figure 11] FIG. 11 is a diagram illustrating an example of a semiconductor device according to a second embodiment. [Figure 12] 11A to 11C are diagrams for explaining an example of a method for forming a semiconductor device according to a second embodiment; [Figure 13] 13A to 13C are diagrams (part 2) illustrating an example of a method for forming a semiconductor device according to a second embodiment; [Figure 14]13A to 13C are views (part 3) illustrating an example of a method for forming a semiconductor device according to a second embodiment; [Figure 15] 13A to 13C are diagrams illustrating an example of a semiconductor device according to a third embodiment. [Figure 16] FIG. 13 is a diagram illustrating an energy band structure of an example of a semiconductor device according to a third embodiment. [Figure 17] 13A to 13C are diagrams (part 1) illustrating an example of a method for forming a semiconductor device according to a third embodiment. [Figure 18] 13A to 13C are diagrams (part 2) illustrating an example of a method for forming a semiconductor device according to a third embodiment; [Figure 19] 13A to 13C are views (part 3) illustrating an example of a method for forming a semiconductor device according to a third embodiment; [Figure 20] FIG. 13 is a diagram illustrating an example of a semiconductor device according to a fourth embodiment. [Figure 21] 13A to 13C are diagrams illustrating an example of a semiconductor package according to a fifth embodiment. [Figure 22] FIG. 13 is a diagram illustrating an example of a power factor correction circuit according to a sixth embodiment. [Figure 23] FIG. 13 is a diagram illustrating an example of a power supply device according to a seventh embodiment. [Figure 24] FIG. 13 is a diagram illustrating an example of an amplifier according to an eighth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Semiconductor devices using nitride semiconductors are being developed as high-voltage, high-output devices by utilizing the characteristics of nitride semiconductors such as high saturation electron velocity, wide band gap, etc. As semiconductor devices using nitride semiconductors, many reports have been made on field effect transistors (FETs), for example, HEMTs.
[0013] Fig. 1 is a diagram for explaining examples of semiconductor devices. Fig. 1(A) shows a schematic cross-sectional view of a main part of a first example of a semiconductor device. Fig. 1(B) shows a schematic cross-sectional view of a main part of a second example of a semiconductor device.
[0014] The semiconductor device 1000 shown in FIG. 1A is an example of a HEMT, and includes a channel layer 1010, a barrier layer 1030, a gate electrode 1050, a source electrode 1060, and a drain electrode 1070. The channel layer 1010 is made of, for example, GaN. The barrier layer 1030 is made of, for example, AlGaN, which has a larger band gap than GaN. The barrier layer 1030 is provided on the channel layer 1010. The gate electrode 1050, the source electrode 1060, and the drain electrode 1070 are each made of a predetermined metal. The gate electrode 1050 is provided on the barrier layer 1030 to function as a Schottky electrode, and the source electrode 1060 and the drain electrode 1070 are provided on the barrier layer 1030 to function as ohmic electrodes.
[0015] In the semiconductor device 1000, a 2DEG 2000 is generated in the channel layer 1010 by spontaneous polarization of the AlGaN of the barrier layer 1030 and piezoelectric polarization generated in the AlGaN of the barrier layer 1030 due to strain caused by the difference in lattice constant between the barrier layer 1030 and the GaN of the channel layer 1010. When the semiconductor device 1000 is in operation, a predetermined voltage is supplied between the source electrode 1060 and the drain electrode 1070, and a predetermined gate voltage is supplied to the gate electrode 1050. A channel through which carrier electrons are transported is formed in the GaN of the channel layer 1010 between the source electrode 1060 and the drain electrode 1070, and the transistor function of the semiconductor device 1000 is realized.
[0016] In addition to the HEMT illustrated in FIG. 1(A), i.e., a HEMT using GaN for the channel layer 1010 and AlGaN for the barrier layer 1030, in recent years, HEMTs using nitride semiconductors such as InAlN and InAlGaN (also referred to as "In-based nitride semiconductors") for the barrier layer have been proposed.
[0017] The semiconductor device 1100 shown in FIG. 1B is an example of a HEMT using such an In-based nitride semiconductor, and includes a channel layer 1110, a spacer layer 1120, a barrier layer 1130, a gate electrode 1150, a source electrode 1160, and a drain electrode 1170. The channel layer 1110 is made of, for example, GaN. The spacer layer 1120 is made of, for example, AlN or AlGaN having a larger band gap than GaN, and in the example of FIG. 1B, AlN is used. The spacer layer 1120 is provided on the channel layer 1110. The barrier layer 1130 is made of, for example, InAlN or InAlGaN having a larger band gap than GaN, and in the example of FIG. 1B, InAlGaN is used. The barrier layer 1130 is provided on the spacer layer 1120. The gate electrode 1150, the source electrode 1160, and the drain electrode 1170 are each made of a predetermined metal. A gate electrode 1150 is provided on the barrier layer 1130 to function as a Schottky electrode, and a source electrode 1160 and a drain electrode 1170 are provided on the barrier layer 1130 to function as ohmic electrodes.
[0018] In the semiconductor device 1100, a 2DEG 2000 is generated in the channel layer 1110 by spontaneous polarization of the AlN of the spacer layer 1120 and the InAlGaN of the barrier layer 1130, and piezoelectric polarization caused by strain due to the difference in lattice constant between the GaN of the channel layer 1110 and the AlN of the barrier layer 1120. When the semiconductor device 1100 is in operation, a predetermined voltage is supplied between the source electrode 1160 and the drain electrode 1170, and a predetermined gate voltage is supplied to the gate electrode 1150. A channel through which carrier electrons are transported is formed in the GaN of the channel layer 1110 between the source electrode 1160 and the drain electrode 1170, and the transistor function of the semiconductor device 1100 is realized.
[0019] InAlN or InAlGaN (InAlGaN in the example of FIG. 1B) used in the barrier layer 1130 of the semiconductor device 1100 shown in FIG. 1B is a type of nitride semiconductor that can realize a high Al composition. For example, In 0.18 Al 0.82N is lattice-matched with GaN used in the channel layer 1110, and is strain-free. InAlN and InAlGaN, which have an increased Al composition, have very strong spontaneous polarization. Therefore, InAlN and InAlGaN used in the barrier layer 1130 of the semiconductor device 1100 (FIG. 1(B)) can generate a higher concentration of 2DEG 2000 than AlGaN used in the barrier layer 1030 of the semiconductor device 1000 (FIG. 1(A)). InAlN and InAlGaN are expected to be materials that can realize high-power devices.
[0020] Here, problems that may occur in the semiconductor devices 1000 and 1100 described above will be described. Figure 2 is a diagram for explaining problems that may occur in a semiconductor device. Figure 2(A) shows a schematic cross-sectional view of a main part of an example of a semiconductor device. Figure 2(B) shows a schematic energy band structure of an example of a semiconductor device. In Figure 2(B), Ec represents the conduction band, Ev represents the valence band, and Ef represents the Fermi level.
[0021] Here, an example is taken of an In-based nitride semiconductor such as InAlN or InAlGaN. A semiconductor device 1100a shown in Fig. 2(A) corresponds to the semiconductor device 1100 shown in Fig. 1(B) above, and shows an example in which GaN is used for the channel layer 1110, AlN (or AlGaN) is used for the spacer layer 1120, and InAlGaN (or InAlN) is used for the barrier layer 1130.
[0022] In the semiconductor device 1100a, as described above, the barrier layer 1130 is made of InAlGaN or the like that can realize a high Al composition, and the strong spontaneous polarization of the barrier layer 1130 makes it possible to generate a high-concentration 2DEG 2000. On the other hand, when the Al composition of the barrier layer 1130 is increased, the barrier between the source electrode 1160 and the drain electrode 1170 connected to the barrier layer 1130 becomes large due to the large band gap caused by the high Al composition, as shown in FIG. 2(B). When the barrier becomes large, the contact resistance 3000 between the barrier layer 1130 and the source electrode 1160 and the drain electrode 1170 becomes high, and good ohmic connection of the source electrode 1160 and the drain electrode 1170 may not be realized. When the contact resistance 3000 becomes high and good ohmic connection is not realized, the resistance of the electron transport path formed between the source electrode 1160 and the drain electrode 1170 becomes high as a whole, the on-resistance increases, and there is a risk that the semiconductor device 1100a that shows sufficient output characteristics may not be obtained.
[0023] A technique for regrowing a low resistance layer has been proposed as one of the techniques for reducing the contact resistance 3000. Such a technique for regrowing a low resistance layer will be described with reference to the following FIG.
[0024] 3A and 3B are diagrams for explaining a low-resistance layer regrowth technique for a semiconductor device, each of which shows a schematic cross-sectional view of a main part of one step in the low-resistance layer regrowth technique.
[0025] In the low-resistance layer regrowth technique, first, a stacked body 1200 (FIG. 3(A)) is formed by crystal growth of GaN of the channel layer 1110, AlN (or AlGaN) of the spacer layer 1120, and InAlGaN (or InAlN) of the barrier layer 1130. Next, as shown in FIG. 3(A), for example, a recess 1210 reaching the channel layer 1110 is formed in a region of the stacked body 1200 where a source electrode 1160 and a drain electrode 1170 are to be formed. After that, as shown in FIG. 3(B), for example, a GaN (n-GaN) layer 1220 doped with Si (silicon) or the like as an n-type impurity is regrown by crystal growth in the formed recess 1210. A source electrode 1160 and a drain electrode 1170 are formed on the regrown n-GaN layer 1220, and a gate electrode 1150 is formed on the barrier layer 1130, to obtain a semiconductor device 1100b as shown in FIG. 3(B).
[0026] In the semiconductor device 1100b, the regrown n-GaN layer 1220 reduces the contact resistance of the source electrode 1160 and the drain electrode 1170, and the on-resistance is expected to be reduced. However, if such a technique for forming the n-GaN layer 1220 by regrowth is adopted, the number of steps increases with the formation of the n-GaN layer 1220. In addition, when the n-GaN layer 1220 is regrown, damage 1230 such as growth defects may occur in the barrier layer 1130, for example, in the surface layer. When an In-based nitride semiconductor such as InAlGaN is used for the barrier layer 1130, if the n-GaN layer 1220 is regrown at a temperature higher than the growth temperature, In in the barrier layer 1130 may be desorbed, causing damage 1230 such as growth defects. The damage 1230 occurring in the barrier layer 1130 due to the regrowth of the n-GaN layer 1220 may cause a decrease in the 2DEG 2000 in the semiconductor device 1100b, an increase in the on-resistance, etc.
[0027] Here, the semiconductor device 1100a (semiconductor device 1100 in FIG. 2(A) or FIG. 1(B)) using an In-based nitride semiconductor such as InAlGaN or InAlN for the barrier layer 1130 is taken as an example. The comparatively large band gap of the barrier layer 1130 increases the contact resistance of the source electrode 1160 and the drain electrode 1170, and the application of a low-resistance layer regrowth technique for regrowing the n-GaN layer 1220 to deal with this has been described. However, the low-resistance layer regrowth technique is not limited to the semiconductor device 1100a using an In-based nitride semiconductor, and may be applied. For example, the low-resistance layer regrowth technique may be similarly applied to the semiconductor device 1000 (FIG. 1(A)) using other nitride semiconductors with comparatively large band gaps such as AlGaN or AlN for the barrier layer 1030 in order to reduce the contact resistance of the source electrode 1060 and the drain electrode 1070. That is, the problem of reducing the contact resistance of the source electrode and the drain electrode is not limited to the case where an In-based nitride semiconductor is used for the barrier layer, but may occur similarly when other nitride semiconductors are used. Moreover, if the low-resistance layer regrowth technique is applied to such a problem that may occur when a nitride semiconductor other than an In-based nitride semiconductor is used for the barrier layer, there is a risk of increasing the number of steps and damaging the barrier layer, as described above.
[0028] In view of the above, a configuration as shown in the following embodiment is adopted to realize a high-performance semiconductor device with low contact resistance. [First embodiment] Fig. 4 is a diagram for explaining an example of the semiconductor device according to the first embodiment. Fig. 4 is a schematic cross-sectional view of a main part of the example of the semiconductor device according to the first embodiment.
[0029] 4 is an example of a HEMT using an In-based nitride semiconductor. The semiconductor device 1A includes a channel layer 10, a spacer layer 20, a barrier layer 30, a cap layer 40, a gate electrode 50, a source electrode 60, and a drain electrode 70.
[0030] The channel layer 10 may be made of, for example, GaN. The channel layer 10 may be made of, in addition to GaN, AlGaN or InGaN. FIG. 4 shows an example in which the channel layer 10 is made of GaN. The channel layer 10 is formed on a predetermined base substrate (not shown) by, for example, a metal organic chemical vapor deposition (MOCVD) or metal organic vapor phase epitaxy (MOVPE) method or a molecular beam epitaxy (MBE) method. The base substrate on which the channel layer 10 is formed may be a substrate such as Si, SiC (silicon carbide), or GaN, or a substrate having a nucleation layer or buffer layer such as AlN formed thereon. The channel layer 10 is formed on a predetermined base substrate by, for example, a MOVPE method, such that one surface 10a of the channel layer 10 is a (0001) surface, i.e., a group III polar surface.
[0031] The spacer layer 20 may be made of, for example, AlN. The spacer layer 20 may be made of AlGaN instead of AlN. FIG. 4 shows an example in which the spacer layer 20 is made of AlN. The spacer layer 20 is provided on the surface 10a of the channel layer 10. The spacer layer 20 is formed on the surface 10a of the channel layer 10, which is the group III polar surface of the GaN channel layer 10 in this example, by using an MOVPE method or the like. In this case, the surface 20a of the spacer layer 20 opposite to the channel layer 10 is the (0001) surface, i.e., the group III polar surface.
[0032] The barrier layer 30 may be made of, for example, InAlGaN. The barrier layer 30 may be made of InAlN in addition to InAlGaN. FIG. 4 shows an example in which the barrier layer 30 is made of InAlGaN. The barrier layer 30 may be made of a nitride semiconductor containing Al and In, or a nitride semiconductor containing at least Al and In among Al, Ga, and In, that is, a so-called In-based nitride semiconductor. The barrier layer 30 is provided on the surface 20a of the spacer layer 20. The barrier layer 30 is formed on the surface 20a of the spacer layer 20, which is the group III polar surface of the AlN spacer layer 20 in this example, by using an MOVPE method or the like. In this case, the surface 30a of the barrier layer 30 opposite to the spacer layer 20 side is a (0001) surface, that is, a group III polar surface.
[0033] The cap layer 40 is a nitride semiconductor containing Al and at least one of Ga and In, in which the Al composition increases from the barrier layer 30 side toward the face 40a side opposite to the barrier layer 30 side. The cap layer 40 will be described in detail later. The cap layer 40 is provided on the face 30a of the barrier layer 30. The cap layer 40 is formed on the face 30a of the barrier layer 30, which is the group III polar face of the barrier layer 30 of InAlGaN in this example, by using a MOVPE method or the like. In this case, the face 40a of the cap layer 40 opposite to the barrier layer 30 side is a (0001) face, i.e., a group III polar face.
[0034] The gate electrode 50 is provided on the opposite side of the cap layer 40 to the barrier layer 30 side. The gate electrode 50 is provided on the surface 40a of the cap layer 40. The gate electrode 50 is provided on the surface 40a of the cap layer 40, for example, so as to be in contact with the surface 40a. In addition, the gate electrode 50 may be provided on the surface 40a of the cap layer 40 via a gate insulating film (not shown) using an oxide, nitride, oxynitride, or the like. The gate electrode 50 may be made of a metal. For example, the gate electrode 50 is a metal electrode having Ni (nickel) and Au (gold) provided thereon. The gate electrode 50 is formed by using a deposition method or the like. The gate electrode 50 functions as, for example, a Schottky electrode.
[0035] The source electrode 60 and the drain electrode 70 are provided on both sides of the gate electrode 50. The source electrode 60 and the drain electrode 70 are provided on the surface 40a of the cap layer 40. The source electrode 60 and the drain electrode 70 are provided on the surface 40a of the cap layer 40, for example, so as to be in contact with the surface 40a. The source electrode 60 and the drain electrode 70 may be made of a metal. For example, the source electrode 60 and the drain electrode 70 are provided as metal electrodes having Ta (tantalum) and Al provided thereon. The source electrode 60 and the drain electrode 70 are formed by using a deposition method or the like. The source electrode 60 and the drain electrode 70 function as ohmic electrodes.
[0036] 4 as an example, in the semiconductor device 1A having the configuration shown in FIG. 4, spontaneous polarization of the AlN of the spacer layer 20 and the InAlGaN of the barrier layer 30, and piezoelectric polarization caused by the difference in lattice constant with the GaN of the channel layer 10, generate a 2DEG 100 in the channel layer 10 near the junction interface with the spacer layer 20. By making the Fermi level higher (higher energy side) than the conduction band of the junction interface between the channel layer 10 and the spacer layer 20, the 2DEG 100 is generated in the channel layer 10 near the junction interface with the spacer layer 20.
[0037] In the semiconductor device 1A, an In-based nitride semiconductor, for example, InAlGaN, is used for the barrier layer 30, and by increasing the Al composition, it is possible to strengthen spontaneous polarization and generate a high-concentration 2DEG 100. However, as described above, when the source electrode 60 and the drain electrode 70 are directly connected to the barrier layer 30 having a high Al composition, the contact resistance becomes high. In contrast, in the semiconductor device 1A, a cap layer 40 having a so-called graded Al composition, in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, is provided on the barrier layer 30. The source electrode 60 and the drain electrode 70 are provided on the cap layer 40 having such a graded Al composition. As a result, the contact resistance of the source electrode 60 and the drain electrode 70 is reduced in the semiconductor device 1A.
[0038] The graded Al composition cap layer 40 will now be described. Fig. 5 is a diagram for explaining the relationship between the Al composition and spontaneous polarization of a nitride semiconductor. Fig. 5(A) is a diagram showing a schematic diagram of spontaneous polarization in an AlN layer. Fig. 5(B) is a diagram showing a schematic diagram of spontaneous polarization in a GaN layer or the like. Fig. 5(C) is a diagram showing a schematic diagram of spontaneous polarization in an AlGaN layer or the like.
[0039] Nitride semiconductors have a spontaneous polarization along the
[0001] direction (c-axis). As an example, the spontaneous polarization of AlN is -0.081 C / m 2 The spontaneous polarization of GaN is -0.029C / m 2 The spontaneous polarization of InN (indium nitride) is -0.032C / m 2 GaN and InN have similar spontaneous polarizations, while AlN has a stronger spontaneous polarization.
[0040] When the (0001) plane is used, for example, as shown in FIG. 5(A) and FIG. 5(B), negative charges (indicated by "-") are generated on the upper end side of each of the nitride semiconductor layers 150a and 150b, and positive charges (indicated by "+") are generated on the lower end side. Since AlN has a stronger spontaneous polarization than GaN, the amount of charge generated in the AlN layer 150a is larger than the amount of charge generated in the GaN layer 150b. Since InN has the same degree of spontaneous polarization as GaN, the same can be said about InN and InGaN, in which part of GaN is replaced with InN, as well as GaN (FIG. 5(B)).
[0041] AlGaN in which a part of GaN is replaced by AlN (or AlGaN in which a part of AlN is replaced by GaN) has an intermediate charge between AlN and GaN depending on the Al composition. At this time, when the Al composition of AlGaN is increased toward the upper end of the layer, the relatively small amount of negative charge generated at the upper end side of the lower layer in the layer is offset by the relatively large amount of positive charge generated at the lower end side of the upper layer stacked directly above it. Therefore, in the entire layer including them, spontaneous polarization occurs as shown in layer 150c shown in FIG. 5(C), and positive charges are generated not only near the lower end of layer 150c but also over a wide area in layer 150c. AlGaN in which the Al composition is increased toward the upper end of layer 150c exhibits the properties of an n-type semiconductor (also called "n-type semiconductor property" or "n-type property") due to the generation of positive charges over a wide area in layer 150c, that is, the generation of positive fixed charges spreading throughout layer 150c. In addition, since InN and GaN have the same degree of spontaneous polarization, the same can be said about InAlN, in which part of InN is replaced with AlN, and about InAlGaN, in which part of InGaN is replaced with InN, and part of InAlGaN is replaced with AlN.
[0042] In the semiconductor device 1A shown in FIG. 4, a nitride semiconductor with a graded Al composition, in which the Al composition increases toward one surface side of the layer to thereby exhibit n-type properties, is used for the cap layer 40.
[0043] For example, in the semiconductor device 1A, for the cap layer 40 with a graded Al composition, AlGaN with an increasing Al composition toward the surface 40a side where the source electrode 60 and the drain electrode 70 are connected from the barrier layer 30 side can be used. For the cap layer 40 with a graded Al composition, InAlN with an increasing Al composition toward the surface 40a side from the barrier layer 30 side can also be used. For the cap layer 40 with a graded Al composition, InAlGaN with an increasing Al composition toward the surface 40a side from the barrier layer 30 side can also be used. Further, for the cap layer 40 with a graded Al composition, as long as the Al composition increases toward the surface 40a side from the barrier layer 30 side, a combination of two or more of AlGaN, InAlN, and InAlGaN may be used. The uppermost layer (the side where the source electrode 60 and the drain electrode 70 are connected) of the cap layer 40 with a graded Al composition may contain a layer of AlN.
[0044] For the cap layer 40 with a graded Al composition, a nitride semiconductor containing Al and at least one of Ga and In can be used, and a nitride semiconductor represented by In x Al y Ga 1-(x+y) N (0 ≦ x < 1, 0 < y ≦ 1, 0 < x + y ≦ 1) can be used. The cap layer 40 with a graded Al composition is formed on the surface 30a of the barrier layer 30 by using the MOVPE method or the like so that the Al composition increases toward the surface 40a side from the barrier layer 30 side.
[0045] FIG. 6 is a diagram for explaining the energy band structure of an example of a semiconductor device according to the first embodiment. In FIG. 6, Ec represents the conduction band, Ev represents the valence band, and Ef represents the Fermi level. In FIG. 6, the energy band structure of the semiconductor device 1A (FIG. 4) provided with the cap layer 40 with a graded Al composition according to the first embodiment is represented by a solid line. For comparison, in FIG. 6, the energy band structure (FIG. 2(B)) of the semiconductor device 1100a (FIG. 2(A)) without the cap layer 40 with a graded Al composition is represented by a dotted line.
[0046] In the semiconductor device 1A shown in Fig. 4, an AlN spacer layer 20 is provided on a surface 10a of a GaN channel layer 10, an InAlGaN barrier layer 30 is provided on the surface 20a, and a cap layer 40 with a graded Al composition is provided on the surface 30a. The energy band structure of the semiconductor device 1A having such a configuration is as shown by the solid line in Fig. 6. A 2DEG 100 is generated in the channel layer 10 near the junction interface with the spacer layer 20 due to spontaneous polarization of the spacer layer 20 and the barrier layer 30, and piezoelectric polarization caused by the difference in lattice constant with the channel layer 10.
[0047] In the semiconductor device 1A, the cap layer 40 is provided so as to have a gradient Al composition, that is, so that the Al composition increases from the barrier layer 30 side toward the surface 40a toward the source electrode 60 side and the drain electrode 70 side. The source electrode 60 and the drain electrode 70 are connected to the surface 40a of the cap layer 40 having such a gradient Al composition. As described above, the cap layer 40 having a gradient Al composition, which is provided so that the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, generates positive charges in the layer (FIG. 5(C)), and exhibits n-type properties.
[0048] In the semiconductor device 1A, the cap layer 40 with a graded Al composition that exhibits such n-type properties is interposed between the barrier layer 30 and the source electrode 60 and the drain electrode 70. As a result, the barrier at the contact of the source electrode 60 and the drain electrode 70 is reduced compared to when the cap layer 40 with a graded Al composition is not interposed. That is, in the semiconductor device 1100a (FIG. 2(A)) in which the cap layer 40 with a graded Al composition is not interposed, the barrier at the contact of the source electrode 60 and the drain electrode 70 is relatively large, as seen in the energy band structure shown by the dotted line in FIG. 6 (solid line in FIG. 2(B)). In contrast, in the semiconductor device 1A (FIG. 4) in which the cap layer 40 with a graded Al composition is interposed, the barrier at the contact of the source electrode 60 and the drain electrode 70 is reduced due to the n-type properties of the cap layer 40, as seen in the energy band structure shown by the solid line in FIG. In the semiconductor device 1A, the barrier is reduced in this way, and good ohmic contact of the source electrode 60 and the drain electrode 70 is realized.
[0049] According to the semiconductor device 1A having the cap layer 40 with a graded Al composition, good ohmic contact is achieved and contact resistance is reduced even when a barrier layer 30 such as InAlGaN with a high Al composition is used, which can generate a high concentration 2DEG 100 in the channel layer 10. By reducing the contact resistance of the source electrode 60 and the drain electrode 70, a high performance semiconductor device 1A with low on-resistance is realized.
[0050] In the semiconductor device 1A, the cap layer 40 with a graded Al composition has an increase in its Al composition, i.e., an increase in the Al composition per unit length (1 nm) in the direction from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, of 0.1 nm. -1 For example, the Al composition of the cap layer 40 is uniformly increased by 0.1 nm from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side. -1 It may be increased by 0.5 nm in increments or evenly. -1 You can increase the size by 1.0 nm or evenly. -1They may increase step by step. Also, the Al composition of the cap layer 40 does not necessarily have to increase evenly as long as it increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side.
[0051] The cap layer 40 with a gradient Al composition is set, for example, to have a film thickness in the range of 1 nm to 3 nm. This is because if the film thickness of the cap layer 40 is less than 1 nm, the effects of inclining the Al composition and expressing n-type properties may become small. Also, if the film thickness of the cap layer 40 exceeds 3 nm, the width of the Schottky barrier of the conduction band Ec between the barrier layer 30 such as InAlGaN and the source electrode 60 and the drain electrode 70 will widen, and the tunneling effect of electrons and the effect of reducing the barrier at the contact of the source electrode 60 and the drain electrode 70 may become small.
[0052] Also, FIG. 7 is a diagram for explaining a modified example of the semiconductor device according to the first embodiment. FIGS. 7(A) to 7(C) schematically show cross-sectional views of main parts of an example of the semiconductor device.
[0053] In FIGS. 4 and 6 above, an example in which AlN is used for the spacer layer 20 and InAlGaN is used for the barrier layer 30 is shown. However, as described above, and as in the semiconductor device 1Aa shown in FIG. 7(A), InAlN can also be used for the barrier layer 30. Further, as described above, and as in the semiconductor device 1Ab shown in FIG. 7(B), AlGaN can also be used for the spacer layer 20. For the barrier layer 30, an In-based nitride semiconductor represented by In x Al y Ga 1-(x+y) N (0 <x <1, 0 <y <1, 0 <x + y ≦ 1) can be used, and for the spacer layer 20, Al z Ga 1-zA nitride semiconductor represented by N(0 < z ≤ 1) can be used. Incidentally, the In composition x of the barrier layer 30 is preferably set in the range of 0 < x ≤ 0.2 from the viewpoints of the lattice constant difference from the channel layer 10 and the spacer layer 20, the magnitude of the generated piezoelectric polarization, etc. When the In composition x exceeds 0.20, electron leakage may occur, resulting in a decrease in breakdown voltage, or the lattice mismatch may increase, making it impossible to obtain an appropriate piezoelectric polarization. Also, the Al composition z of the spacer layer 20 is preferably set in the range of 0.4 ≤ z ≤ 1 from the viewpoints of the lattice constant difference from the channel layer 10 and the barrier layer 30, the magnitude of the generated piezoelectric polarization, etc. When the Al composition z is less than 0.40, the confinement effect of the 2DEG 100 becomes small, and there is a possibility of being affected by alloy scattering of the barrier layer 30.
[0054] When a spacer layer 20 of AlN or AlGaN is provided as in the semiconductor devices 1A, 1Aa, and 1Ab above, it is possible to suppress the influence of alloy scattering from the barrier layer 30 and reduce the on-resistance. However, as in the semiconductor device 1Ac shown in FIG. 7(C), it is also possible to directly bond the barrier layer 30, for example, an InAlGaN barrier layer 30, onto the GaN channel layer 10 without providing the spacer layer 20. In this case, the 2DEG 100 is generated near the bonding interface of the channel layer 10 with the barrier layer 30.
[0055] Subsequently, a method for forming a semiconductor device including the above-described configuration will be described with reference to FIGS. 8 to 10. FIGS. 8 to 10 are diagrams for explaining an example of a method for forming a semiconductor device according to the first embodiment. FIGS. 8(A), 8(B), 9(A), 9(B), 10(A), and 10(B) schematically show cross-sectional views of the main parts of examples of each step of forming a semiconductor device according to the first embodiment.
[0056] First, as shown in Fig. 8(A), a channel layer 10, a spacer layer 20, and a barrier layer 30 are sequentially grown by MOVPE on a given base substrate, for example, a base substrate having an AlN nucleation layer 3 formed on a semi-insulating SiC substrate 2. Here, a case is taken as an example in which a GaN channel layer 10, an AlGaN spacer layer 20, and an InAlGaN barrier layer 30 are grown on the AlN nucleation layer 3 of the base substrate. For example, a GaN channel layer 10 having a thickness of 3 µm is grown on the AlN nucleation layer 3 having a thickness of 100 nm, an AlGaN spacer layer 20 having a thickness of 2 nm is grown on the surface 10a, and an InAlGaN barrier layer 30 having a thickness of 6 nm is grown on the surface 20a.
[0057] 8(B), a cap layer 40 with a graded Al composition containing Al and at least one of In and Ga is grown on the InAlGaN barrier layer 30 by MOVPE. The cap layer 40 with a graded Al composition may be made of AlGaN, InAlN or InAlGaN, or may be a combination of two or more of AlGaN, InAlN and InAlGaN, and may contain AlN in its uppermost layer. For example, the cap layer 40 with a graded Al composition having a thickness of 2 nm is grown on the face 30a of the barrier layer 30, with the Al composition increasing from 0.1 nm from the face 30a side toward the face 40a side of the cap layer 40 to be grown. -1 It grows so that it increases more.
[0058] In this manner, a multilayer structure 5 is formed on the base substrate, in which a GaN channel layer 10, an AlGaN spacer layer 20, an InAlGaN barrier layer 30, and a cap layer 40 with a graded Al composition are stacked. In the multilayer structure 5, a 2DEG 100 is generated near the junction interface between the GaN of the channel layer 10 and the spacer layer 20. In the multilayer structure 5, the spacer layer 20 may be made of AlN in addition to AlGaN. In the barrier layer 30, the barrier layer 30 may be made of InAlN in addition to InAlGaN. The barrier layer 30 may be directly formed on the channel layer 10 without providing the spacer layer 20.
[0059] In the growth of each layer by MOVPE, a mixed gas of trimethylgallium (TMGa) and ammonia (NH3) as a Ga source is used for the growth of GaN. A mixed gas of trimethylaluminum (TMAl), TMGa, and NH3 as an Al source is used for the growth of AlGaN. A mixed gas of TMAl and NH3 is used for the growth of AlN. A mixed gas of trimethylindium (TMIn), TMAl, TMGa, and NH3 as an In source is used for the growth of InAlGaN. A mixed gas of TMIn, TMAl, and NH3 is used for the growth of InAlN. The supply and stop (switching) of TMGa, TMAl, and TMIn, and the flow rate during supply (mixing ratio with other raw materials) are appropriately set according to the nitride semiconductor to be grown. The growth pressure is about 1 kPa to 100 kPa, and the growth temperature is about 700°C to 1200°C.
[0060] 8(B), a layered structure 5 is formed in which a channel layer 10, a spacer layer 20, a barrier layer 30, and a cap layer 40 having a graded Al composition are layered, and then a mask (not shown) having an opening in a region where an isolation region is to be formed is formed using a photolithography technique. Then, an isolation region (not shown) is formed in a predetermined region of the layered structure 5 by dry etching using a chlorine-based gas or ion implantation of Ar (argon) or the like. After the isolation region is formed, the mask is removed.
[0061] Next, as shown in FIG. 9(A), a source electrode 60 and a drain electrode 70 are formed on the surface 40a of the cap layer 40 having a graded Al composition in the laminate structure 5. At this time, first, an electrode metal is formed in the region where the source electrode 60 and the drain electrode 70 are to be formed using photolithography, deposition, and lift-off techniques. For example, a laminate of Ta having a thickness of 20 nm and Al having a thickness of 200 nm is formed as the electrode metal. Then, a heat treatment is performed in a nitrogen atmosphere at 400° C. to 1000° C., for example, 550° C., to establish an ohmic contact of the electrode metal. As a result, a state in which the source electrode 60 and the drain electrode 70 are formed on the cap layer 40 having a graded Al composition is obtained, as shown in FIG. 9(A).
[0062] Next, as shown in FIG. 9(B), a passivation film 80 is formed on the stacked structure 5 on which the source electrode 60 and the drain electrode 70 are formed. For example, the passivation film 80 is formed to a thickness of 2 nm to 500 nm, for example, 100 nm, by using a plasma CVD (Chemical Vapor Deposition) method. The passivation film 80 may be formed by an atomic layer deposition (ALD) method, a sputtering method, or the like. For example, an oxide, a nitride, or an oxynitride containing at least one of Si, Al, Hf (hafnium), Zr (zirconium), Ti (titanium), Ta, and W (tungsten) is used for the passivation film 80. For example, SiN (silicon nitride) is formed as the passivation film 80. As a result, a state in which the passivation film 80 is formed on the stacked structure 5 on which the source electrode 60 and the drain electrode 70 are formed, as shown in FIG. 9(B), is obtained.
[0063] Next, as shown in FIG. 10(A), the passivation film 80 in the region where the gate electrode 50 is to be formed is removed, and a part of the cap layer 40 with a graded Al composition is exposed. At that time, a mask (not shown) having an opening in the region where the gate electrode 50 is to be formed is first formed using a photolithography technique, and dry etching is performed. By this etching, the passivation film 80 exposed from the opening of the mask is removed. The etching of the passivation film 80 is performed by dry etching using, for example, a fluorine-based or chlorine-based gas. Alternatively, the etching of the passivation film 80 may be performed by wet etching using hydrofluoric acid, buffered hydrofluoric acid, or the like. After etching of the passivation film 80, the mask is removed. As a result, a state is obtained in which the passivation film 80 in the region where the gate electrode 50 is to be formed is removed and a part of the cap layer 40 with a graded Al composition is exposed, as shown in FIG. 10(A).
[0064] Thereafter, using photolithography, deposition and lift-off techniques, an electrode metal, for example, a laminate of Ni having a thickness of 30 nm and Au having a thickness of 400 nm is formed on the cap layer 40 having the graded Al composition exposed from the passivation film 80, to form the gate electrode 50. The gate electrode 50 functions as a Schottky electrode.
[0065] 10(B), a semiconductor device 1Ad is formed having a structure in which the cap layer 40 with a graded Al composition is interposed between the barrier layer 30 and the source electrode 60 and drain electrode 70. By providing the cap layer 40 with a graded Al composition in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, a high-performance semiconductor device 1Ad with low contact resistance and low on-resistance is realized.
[0066] The types of metals and layer structures used for the gate electrode 50, source electrode 60, and drain electrode 70 of the semiconductor device 1Ad are not limited to the above examples, and the methods for forming them are not limited to the above examples either. The gate electrode 50, source electrode 60, and drain electrode 70 may each have a single-layer structure or a multilayer structure. When forming the source electrode 60 and drain electrode 70, it is not necessary to perform the heat treatment as described above as long as ohmic contact is achieved by forming the metal for the electrodes. When forming the gate electrode 50, a further heat treatment may be performed after the metal for the electrodes is formed.
[0067] Here, an example is shown in which a semi-insulating SiC substrate 2 is used as the base substrate, but other substrate materials may be used as long as a nitride semiconductor is used in the structure having the function of a field effect transistor. A semi-insulating substrate or a conductive substrate may be used as the base substrate. In addition to a semi-insulating SiC substrate, a conductive SiC substrate, a sapphire substrate, a GaN substrate, a Si substrate, a diamond substrate, or the like may be used as the base substrate.
[0068] Here, an example has been shown in which the semiconductor device 1Ad is provided with the gate electrode 50 functioning as a Schottky electrode, but a gate insulating film made of an oxide, nitride, oxynitride, or the like may be provided between the gate electrode 50 and the cap layer 40 to form a MIS (Metal Insulator Semiconductor) type gate structure.
[0069] [Second embodiment] Fig. 11 is a diagram for explaining an example of a semiconductor device according to the second embodiment, which diagrammatically shows a cross-sectional view of a main part of an example of the semiconductor device according to the second embodiment.
[0070] The semiconductor device 1B shown in FIG. 11 is an example of a HEMT using an In-based nitride semiconductor. The semiconductor device 1B has a channel layer 10, a spacer layer 20, a barrier layer 30, a cap layer 40, a gate electrode 50, a source electrode 60, and a drain electrode 70. In the semiconductor device 1B, a cap layer 40 having a graded Al composition in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side is provided between the barrier layer 30 and the source electrode 60 and the drain electrode 70. The cap layer 40 having a graded Al composition is not provided between the barrier layer 30 and the gate electrode 50. The semiconductor device 1B differs from the semiconductor device 1A described in the first embodiment in that it has such a configuration.
[0071] In the semiconductor device 1B, the channel layer 10, the spacer layer 20, the barrier layer 30, and the cap layer 40 with graded Al composition may be the same as those described for the semiconductor device 1A in the first embodiment. That is, the channel layer 10 may be made of GaN or AlGaN. The spacer layer 20 may be made of AlN or AlGaN. The barrier layer 30 may be made of InAlGaN or InAlN. FIG. 11 shows an example in which the channel layer 10 is made of GaN, the spacer layer 20 is made of AlN, and the barrier layer 30 is made of InAlGaN. The cap layer 40 with graded Al composition may be made of a combination of two or more of AlGaN, InAlN, and InAlGaN, in addition to AlGaN, InAlN, or InAlGaN, and the top layer may contain AlN. A 2DEG 100 is generated in the vicinity of the junction interface between the channel layer 10 and the spacer layer 20.
[0072] In the semiconductor device 1B, the spacer layer 20 may not be provided, and the barrier layer 30 may be provided directly on the channel layer 10. In this case, the 2DEG 100 is generated in the vicinity of the junction interface between the channel layer 10 and the barrier layer 30.
[0073] In the semiconductor device 1B, the gate electrode 50, the source electrode 60, and the drain electrode 70 may be the same as those described for the semiconductor device 1A in the first embodiment. That is, the gate electrode 50, the source electrode 60, and the drain electrode 70 are made of a predetermined metal, the gate electrode 50 functions as a Schottky electrode, and the source electrode 60 and the drain electrode 70 function as ohmic electrodes. The gate electrode 50 is provided, for example, on the surface 30a of the barrier layer 30 so as to be in contact with the surface 30a. In addition, the gate electrode 50 may be provided on the surface 30a of the barrier layer 30 via a gate insulating film (not shown) made of an oxide, nitride, oxynitride, or the like. The source electrode 60 and the drain electrode 70 are provided on the surface 40a of the cap layer 40 having a graded Al composition so as to be in contact with the surface 40a.
[0074] In the semiconductor device 1B, a cap layer 40 having a graded Al composition, in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, is provided between the barrier layer 30 and the source electrode 60 and the drain electrode 70. This reduces the barrier at the contact of the source electrode 60 and the drain electrode 70, and realizes good ohmic contact of the source electrode 60 and the drain electrode 70. Even if a barrier layer 30 having a high Al composition such as InAlGaN that can generate a high concentration 2DEG 100 is used in the channel layer 10, good ohmic contact is realized and the contact resistance is reduced. A high-performance semiconductor device 1B with low contact resistance and low on-resistance is realized.
[0075] Furthermore, in the semiconductor device 1B, the cap layer 40 with a graded Al composition is not provided between the barrier layer 30 and the gate electrode 50, and the gate electrode 50 is provided directly on the barrier layer 30 or via a gate insulating film (not shown). This prevents the barrier from being reduced at the contact of the gate electrode 50, realizes a good Schottky contact of the gate electrode 50, and effectively prevents leakage current from the gate electrode 50.
[0076] According to the semiconductor device 1B, it is possible to reduce the contact resistance of the source electrode 60 and the drain electrode 70 while suppressing the leakage current from the gate electrode 50, thereby reducing the on-resistance.
[0077] Next, a method for forming a semiconductor device having the above-mentioned configuration will be described with reference to FIGS. Figures 12 to 14 are diagrams for explaining an example of a method for forming a semiconductor device according to the second embodiment. Figures 12(A), 12(B), 13(A), 13(B), 14(A), and 14(B) each show a schematic cross-sectional view of a main part of an example of each step of forming a semiconductor device according to the second embodiment.
[0078] First, as shown in Fig. 12(A), a channel layer 10, a spacer layer 20, and a barrier layer 30 are sequentially grown by MOVPE on a given base substrate, for example, a base substrate having an AlN nucleation layer 3 formed on a semi-insulating SiC substrate 2. Here, a case is taken as an example in which a GaN channel layer 10, an AlGaN spacer layer 20, and an InAlGaN barrier layer 30 are grown on the AlN nucleation layer 3 of the base substrate. For example, a GaN channel layer 10 having a thickness of 3 µm is grown on the AlN nucleation layer 3 having a thickness of 100 nm, an AlGaN spacer layer 20 having a thickness of 2 nm is grown on the surface 10a, and an InAlGaN barrier layer 30 having a thickness of 6 nm is grown on the surface 20a.
[0079] 12(A), a cap layer 40 with a graded Al composition, containing Al and at least one of In and Ga, is grown on the InAlGaN barrier layer 30 by MOVPE. The cap layer 40 with a graded Al composition may be made of AlGaN, InAlN, or InAlGaN, or may be a combination of two or more of AlGaN, InAlN, and InAlGaN, and may contain AlN in its uppermost layer. For example, the cap layer 40 with a graded Al composition of 2 nm is grown on the face 30a of the barrier layer 30, with the Al composition increasing from 0.1 nm from the face 30a toward the face 40a of the cap layer 40 to be grown. -1It grows so that it increases more.
[0080] In this manner, a multilayer structure 6 is formed on the base substrate, in which a GaN channel layer 10, an AlGaN spacer layer 20, an InAlGaN barrier layer 30, and a cap layer 40 with a graded Al composition are stacked. In the multilayer structure 6, a 2DEG 100 is generated near the junction interface between the GaN of the channel layer 10 and the spacer layer 20. In the multilayer structure 6, the spacer layer 20 may be made of AlN in addition to AlGaN. In the barrier layer 30, the barrier layer 30 may be made of InAlN in addition to InAlGaN. The barrier layer 30 may be directly formed on the channel layer 10 without providing the spacer layer 20.
[0081] In the growth of each layer using the MOVPE method, a mixed gas of TMGa and NH3 is used for the growth of GaN. A mixed gas of TMAl, TMGa, and NH3 is used for the growth of AlGaN. A mixed gas of TMAl and NH3 is used for the growth of AlN. A mixed gas of TMIn, TMAl, TMGa, and NH3 is used for the growth of InAlGaN. A mixed gas of TMIn, TMAl, TMGa, and NH3 is used for the growth of InAlN. The supply and stop (switching) of TMGa, TMAl, and TMIn, and the flow rate during supply (mixing ratio with other raw materials) are appropriately set according to the nitride semiconductor to be grown. The growth pressure is about 1 kPa to 100 kPa, and the growth temperature is about 700°C to 1200°C.
[0082] 12(A), a layered structure 6 is formed in which a channel layer 10, a spacer layer 20, a barrier layer 30, and a cap layer 40 having a graded Al composition are stacked, and then a mask (not shown) having an opening in a region where an isolation region is to be formed is formed using a photolithography technique. Then, an isolation region (not shown) is formed in a predetermined region of the layered structure 6 by dry etching using a chlorine-based gas or ion implantation of Ar or the like. After the isolation region is formed, the mask is removed.
[0083] Next, a protective film (not shown) is formed on the stacked structure 6 by, for example, a plasma CVD method. The protective film may be formed by, for example, an ALD method, a sputtering method, or the like. For the protective film, an oxide, a nitride, or an oxynitride containing at least one of Si, Al, Hf, Zr, Ti, Ta, and W is used. For example, SiO2 (silicon oxide) is formed as the protective film. A mask (not shown) is formed on the formed protective film by using a photolithography technique to cover the region where the source electrode 60 and the drain electrode 70 are to be formed, and dry etching is performed using a chlorine-based gas. By this etching, the exposed protective film that is not covered by the mask is removed, and further the cap layer 40 below it is removed. Thereafter, the remaining mask and protective film are removed from the stacked structure 6. As a result, a state is obtained in which the cap layer 40 with a graded Al composition is formed (remained) in the region where the source electrode 60 and the drain electrode 70 are to be formed of the stacked structure 6, as shown in FIG. 12(B).
[0084] Next, as shown in FIG. 13(A), a source electrode 60 and a drain electrode 70 are formed on the surface 40a of the cap layer 40 with graded Al composition in the laminated structure 6. At that time, first, an electrode metal is formed in the region where the source electrode 60 and the drain electrode 70 are to be formed using photolithography, deposition, and lift-off techniques. For example, a laminate of Ta with a thickness of 20 nm and Al with a thickness of 200 nm is formed as the electrode metal. Then, a heat treatment is performed in a nitrogen atmosphere at 400° C. to 1000° C., for example, 550° C., to establish an ohmic contact of the electrode metal. As a result, a state in which the source electrode 60 and the drain electrode 70 are formed on the cap layer 40 with graded Al composition is obtained as shown in FIG. 13(A).
[0085] Next, as shown in FIG. 13(B), a passivation film 80 is formed on the stacked structure 6 in which the source electrode 60 and the drain electrode 70 are formed and the cap layer 40 between them is partially removed. For example, the passivation film 80 is formed to a thickness of 2 nm to 500 nm, for example, 100 nm, by using a plasma CVD method. The passivation film 80 may be formed by an ALD method, a sputtering method, or the like. For example, an oxide, a nitride, or an oxynitride containing at least one of Si, Al, Hf, Zr, Ti, Ta, and W is used for the passivation film 80. For example, SiN is formed as the passivation film 80. As a result, a state is obtained in which the source electrode 60 and the drain electrode 70 are formed and the cap layer 40 between them is partially removed, as shown in FIG. 13(B), and the passivation film 80 is formed on the stacked structure 6.
[0086] Next, as shown in FIG. 14(A), the passivation film 80 in the region where the gate electrode 50 is to be formed is removed, and a part of the barrier layer 30 is exposed. At this time, a mask (not shown) having an opening in the region where the gate electrode 50 is to be formed is first formed using a photolithography technique, and dry etching is performed. By this etching, the passivation film 80 exposed from the opening of the mask is removed. The etching of the passivation film 80 is performed by dry etching using, for example, a fluorine-based or chlorine-based gas. Alternatively, the etching of the passivation film 80 may be performed by wet etching using hydrofluoric acid, buffered hydrofluoric acid, or the like. After etching of the passivation film 80, the mask is removed. As a result, a state is obtained in which the passivation film 80 in the region where the gate electrode 50 is to be formed is removed and a part of the barrier layer 30 is exposed, as shown in FIG. 14(A).
[0087] Thereafter, using photolithography, deposition and lift-off techniques, an electrode metal, for example, a laminate of Ni having a thickness of 30 nm and Au having a thickness of 400 nm is formed on the barrier layer 30 exposed from the passivation film 80, to form the gate electrode 50. The gate electrode 50 functions as a Schottky electrode.
[0088] 14(B), a semiconductor device 1Ba is formed having a structure in which the cap layer 40 with a graded Al composition is interposed between the barrier layer 30 and the source electrode 60 and the drain electrode 70, and the cap layer 40 with a graded Al composition is not interposed between the barrier layer 30 and the gate electrode 50. By providing the cap layer 40 with a graded Al composition in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, a high-performance semiconductor device 1Ba with low contact resistance and low on-resistance is realized. Furthermore, by not interposing the cap layer 40 with a graded Al composition between the barrier layer 30 and the gate electrode 50, a semiconductor device 1Ba in which leakage current from the gate electrode 50 is effectively suppressed is realized.
[0089] The types of metals and layer structures used for the gate electrode 50, source electrode 60, and drain electrode 70 of the semiconductor device 1Ba are not limited to the above examples, and the methods for forming them are not limited to the above examples. The gate electrode 50, source electrode 60, and drain electrode 70 may each have a single layer structure or a laminated structure. When forming the source electrode 60 and drain electrode 70, it is not necessary to perform the heat treatment as described above as long as ohmic contact is achieved by forming the electrode metal. When forming the gate electrode 50, a further heat treatment may be performed after forming the electrode metal.
[0090] Here, an example is shown in which a semi-insulating SiC substrate 2 is used as the base substrate, but other substrate materials may be used as long as a nitride semiconductor is used in the structure having the function of a field effect transistor. A semi-insulating substrate or a conductive substrate may be used as the base substrate. In addition to a semi-insulating SiC substrate, a conductive SiC substrate, a sapphire substrate, a GaN substrate, a Si substrate, a diamond substrate, or the like may be used as the base substrate.
[0091] Here, an example has been shown in which the semiconductor device 1Ba is provided with the gate electrode 50 functioning as a Schottky electrode, but a gate insulating film made of an oxide, nitride, oxynitride, or the like may be provided between the gate electrode 50 and the barrier layer 30 to form an MIS-type gate structure.
[0092] [Third embodiment] Fig. 15 is a diagram for explaining an example of a semiconductor device according to the third embodiment. Fig. 15 is a schematic cross-sectional view of a main part of an example of a semiconductor device according to the third embodiment.
[0093] The semiconductor device 1C shown in FIG. 15 is an example of a HEMT using an In-based nitride semiconductor. The semiconductor device 1C has a channel layer 10, a spacer layer 20, a barrier layer 30, a cap layer 40, a cap layer 90, a gate electrode 50, a source electrode 60, and a drain electrode 70. In the semiconductor device 1C, a cap layer 40 having a graded Al composition in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side is provided between the barrier layer 30 and the source electrode 60 and the drain electrode 70. A cap layer 40 having a graded Al composition and a cap layer 90 provided thereon are provided between the barrier layer 30 and the gate electrode 50. The semiconductor device 1C differs from the semiconductor device 1A described in the first embodiment in that it has such a configuration.
[0094] In the semiconductor device 1C, the channel layer 10, the spacer layer 20, the barrier layer 30, and the cap layer 40 with graded Al composition may be the same as those described for the semiconductor device 1A in the first embodiment. That is, the channel layer 10 may be made of GaN or AlGaN. The spacer layer 20 may be made of AlN or AlGaN. The barrier layer 30 may be made of InAlGaN or InAlN. FIG. 15 shows an example in which the channel layer 10 is made of GaN, the spacer layer 20 is made of AlN, and the barrier layer 30 is made of InAlGaN. The cap layer 40 with graded Al composition may be made of a combination of two or more of AlGaN, InAlN, and InAlGaN, in addition to AlGaN, InAlN, or InAlGaN, and the top layer may contain AlN. A 2DEG 100 is generated in the vicinity of the junction interface between the channel layer 10 and the spacer layer 20.
[0095] The semiconductor device 1C may also have a configuration in which the spacer layer 20 is not provided and the barrier layer 30 is provided directly on the channel layer 10. In this case, a 2DEG 100 is generated in the vicinity of the junction interface between the channel layer 10 and the barrier layer 30.
[0096] In the semiconductor device 1C, a nitride semiconductor containing Ga, for example, GaN, is used for the cap layer 90 provided on the cap layer 40 with the graded Al composition. The cap layer 90 is formed on the surface 40a of the cap layer 40 with the graded Al composition by using a MOVPE method or the like.
[0097] In the semiconductor device 1C, the gate electrode 50, the source electrode 60, and the drain electrode 70 may be the same as those described for the semiconductor device 1A in the first embodiment. That is, the gate electrode 50, the source electrode 60, and the drain electrode 70 are made of a predetermined metal, the gate electrode 50 functions as a Schottky electrode, and the source electrode 60 and the drain electrode 70 function as ohmic electrodes. The gate electrode 50 is provided, for example, on a surface 90a of the cap layer 90 so as to be in contact with the surface 90a. In addition, the gate electrode 50 may be provided on the surface 90a of the cap layer 90 via a gate insulating film (not shown) made of an oxide, a nitride, an oxynitride, or the like. The source electrode 60 and the drain electrode 70 are provided on a surface 40a of the cap layer 40 having a graded Al composition so as to be in contact with the surface 40a.
[0098] In the semiconductor device 1C, a cap layer 40 having a graded Al composition, in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, is provided between the barrier layer 30 and the source electrode 60 and the drain electrode 70. This reduces the barrier at the contact of the source electrode 60 and the drain electrode 70, and achieves good ohmic contact of the source electrode 60 and the drain electrode 70. Even if a barrier layer 30 having a high Al composition such as InAlGaN that can generate a high concentration 2DEG 100 is used in the channel layer 10, good ohmic contact is achieved and the contact resistance is reduced. A high-performance semiconductor device 1C with low contact resistance and low on-resistance is achieved.
[0099] The semiconductor device 1C further includes a cap layer 40 having a graded Al composition and a cap layer 90 using, for example, GaN between the barrier layer 30 and the gate electrode 50. The cap layer 90 using GaN has a function of suppressing the generation of leakage current from the gate electrode 50 in addition to a function of protecting the cap layer 40 having a graded Al composition.
[0100] Fig. 16 is a diagram for explaining an example of an energy band structure of a semiconductor device according to the third embodiment. In Fig. 16, Ec represents a conduction band, Ev represents a valence band, and Ef represents a Fermi level. Fig. 16 shows the energy band structure of the semiconductor device 1C (Fig. 15) in a region where a GaN cap layer 90 is provided on a cap layer 40 having a graded Al composition according to the third embodiment.
[0101] In the semiconductor device 1C, the GaN cap layer 90 is provided to raise the conduction band Ec of the AlN spacer layer 20 bonded to the GaN channel layer 10 and the InAlGaN barrier layer 30 bonded thereto. When the conduction band Ec at the junction interface between the spacer layer 20 and the channel layer 10 becomes higher than the Fermi level Ef, the 2DEG 100 disappears. In the semiconductor device 1C, the insertion of the GaN cap layer 90 provides such an energy band structure, thereby raising the barrier at the contact of the gate electrode 50, realizing a good Schottky contact of the gate electrode 50, and effectively suppressing the generation of leakage current from the gate electrode 50.
[0102] The insertion of the cap layer 90 is one method for making the semiconductor device 1C normally-off. When a positive bias is applied to the gate electrode 50, the conduction band Ec is pulled downward from the energy band structure shown in FIG. 16, whereby the 2DEG 100 is generated, and electrical continuity is established between the source electrode 60 and the drain electrode 70, turning the device into an on state.
[0103] According to the semiconductor device 1C, it is possible to reduce the contact resistance of the source electrode 60 and the drain electrode 70 while suppressing the leakage current from the gate electrode 50, thereby reducing the on-resistance.
[0104] Here, an example in which GaN is used for the cap layer 90 has been shown, but the cap layer 90 is not limited to GaN, and may be made of InGaN, a laminate of InGaN and GaN, or the like. Next, a method for forming a semiconductor device having the above-mentioned configuration will be described with reference to FIGS.
[0105] Figures 17 to 19 are diagrams for explaining an example of a method for forming a semiconductor device according to the third embodiment. Figures 17(A), 17(B), 18(A), 18(B), 19(A) and 19(B) each show a schematic cross-sectional view of a main part of an example of each step of forming a semiconductor device according to the third embodiment.
[0106] First, as shown in Fig. 17(A), a channel layer 10, a spacer layer 20, and a barrier layer 30 are sequentially grown by MOVPE on a given base substrate, for example, a base substrate having an AlN nucleation layer 3 formed on a semi-insulating SiC substrate 2. Here, a case is taken as an example in which a GaN channel layer 10, an AlGaN spacer layer 20, and an InAlGaN barrier layer 30 are grown on the AlN nucleation layer 3 of the base substrate. For example, a GaN channel layer 10 having a thickness of 3 µm is grown on the AlN nucleation layer 3 having a thickness of 100 nm, an AlGaN spacer layer 20 having a thickness of 2 nm is grown on the surface 10a, and an InAlGaN barrier layer 30 having a thickness of 6 nm is grown on the surface 20a.
[0107] 17(A), a cap layer 40 with a graded Al composition, containing Al and at least one of In and Ga, is grown on the InAlGaN barrier layer 30 by MOVPE. The cap layer 40 with a graded Al composition may be made of AlGaN, InAlN, or InAlGaN, or may be a combination of two or more of AlGaN, InAlN, and InAlGaN, and may contain AlN in its uppermost layer. For example, the cap layer 40 with a graded Al composition of 2 nm is grown on the face 30a of the barrier layer 30, with the Al composition increasing from 0.1 nm from the face 30a side toward the face 40a side of the cap layer 40 to be grown. -1 17(A), a GaN cap layer 90 is grown on the cap layer 40 with graded Al composition by MOVPE. For example, a GaN cap layer 90 having a thickness of about 1 nm to 10 nm is grown on the surface 40a of the cap layer 40 with graded Al composition.
[0108] In this manner, a multilayer structure 7 is formed on the base substrate, in which a GaN channel layer 10, an AlGaN spacer layer 20, an InAlGaN barrier layer 30, a cap layer 40 with a graded Al composition, and a GaN cap layer 90 are stacked. In the multilayer structure 7, a 2DEG 100 is generated near the junction interface between the GaN of the channel layer 10 and the spacer layer 20. In the multilayer structure 7, the spacer layer 20 may be made of AlN in addition to AlGaN. In the barrier layer 30, the barrier layer 30 may be made of InAlN in addition to InAlGaN. The barrier layer 30 may be directly formed on the channel layer 10 without providing the spacer layer 20.
[0109] In the growth of each layer using the MOVPE method, a mixed gas of TMGa and NH3 is used for the growth of GaN. A mixed gas of TMAl, TMGa, and NH3 is used for the growth of AlGaN. A mixed gas of TMAl and NH3 is used for the growth of AlN. A mixed gas of TMIn, TMAl, TMGa, and NH3 is used for the growth of InAlGaN. A mixed gas of TMIn, TMAl, TMGa, and NH3 is used for the growth of InAlN. The supply and stop (switching) of TMGa, TMAl, and TMIn, and the flow rate during supply (mixing ratio with other raw materials) are appropriately set according to the nitride semiconductor to be grown. The growth pressure is about 1 kPa to 100 kPa, and the growth temperature is about 700°C to 1200°C.
[0110] 17(A), a layered structure 7 is formed in which a channel layer 10, a spacer layer 20, a barrier layer 30, a cap layer 40 having a graded Al composition, and a cap layer 90 made of GaN are layered, and then a mask (not shown) having an opening in a region where an isolation region is to be formed is formed using photolithography. Then, an isolation region (not shown) is formed in a predetermined region of the layered structure 7 by dry etching using a chlorine-based gas or ion implantation of Ar or the like. After the isolation region is formed, the mask is removed.
[0111] Next, a protective film (not shown) is formed on the stacked structure 7 by, for example, plasma CVD. The protective film may be formed by ALD, sputtering, or the like. For example, an oxide, nitride, or oxynitride containing at least one of Si, Al, Hf, Zr, Ti, Ta, and W is used for the protective film. For example, SiO2 is formed as the protective film. A mask (not shown) having openings in the regions where the source electrode 60 and the drain electrode 70 are to be formed is formed on the formed protective film by photolithography, and dry etching is performed using a chlorine-based gas. This etching removes the protective film exposed from the openings of the mask, and further removes the cap layer 90 below it. Thereafter, the remaining mask and protective film are removed from the stacked structure 7. As a result, a state is obtained in which the GaN cap layer 90 is formed (remains) between the regions where the source electrode 60 and the drain electrode 70 are to be formed in the stacked structure 7, as shown in FIG. 17(B).
[0112] Next, as shown in FIG. 18(A), a source electrode 60 and a drain electrode 70 are formed on the surface 40a of the cap layer 40 having a graded Al composition in the laminate structure 7. At this time, first, an electrode metal is formed in the region where the source electrode 60 and the drain electrode 70 are to be formed using photolithography, deposition, and lift-off techniques. For example, a laminate of Ta having a thickness of 20 nm and Al having a thickness of 200 nm is formed as the electrode metal. Then, a heat treatment is performed in a nitrogen atmosphere at 400° C. to 1000° C., for example, 550° C., to establish an ohmic contact of the electrode metal. As a result, a state in which the source electrode 60 and the drain electrode 70 are formed on the cap layer 40 having a graded Al composition is obtained, as shown in FIG. 18(A).
[0113] Next, as shown in FIG. 18(B), a passivation film 80 is formed on the stacked structure 7 in which the source electrode 60 and the drain electrode 70 are formed and the GaN cap layer 90 is formed therebetween. For example, the passivation film 80 is formed to a thickness of 2 nm to 500 nm, for example, 100 nm, by using a plasma CVD method. The passivation film 80 may be formed by an ALD method, a sputtering method, or the like. For example, an oxide, a nitride, or an oxynitride containing at least one of Si, Al, Hf, Zr, Ti, Ta, and W is used for the passivation film 80. For example, SiN is formed as the passivation film 80. As a result, a state is obtained in which the passivation film 80 is formed on the stacked structure 7 in which the source electrode 60 and the drain electrode 70 are formed and the GaN cap layer 90 is formed therebetween, as shown in FIG. 18(B).
[0114] Next, as shown in FIG. 19(A), the passivation film 80 in the region where the gate electrode 50 is to be formed is removed, and a part of the GaN cap layer 90 is exposed. At this time, a mask (not shown) having an opening in the region where the gate electrode 50 is to be formed is first formed using a photolithography technique, and dry etching is performed. By this etching, the passivation film 80 exposed from the opening of the mask is removed. The etching of the passivation film 80 is performed by dry etching using, for example, a fluorine-based or chlorine-based gas. Alternatively, the etching of the passivation film 80 may be performed by wet etching using hydrofluoric acid, buffered hydrofluoric acid, or the like. After etching of the passivation film 80, the mask is removed. As a result, a state is obtained in which the passivation film 80 in the region where the gate electrode 50 is to be formed is removed and a part of the GaN cap layer 90 is exposed, as shown in FIG. 19(A).
[0115] Thereafter, photolithography, deposition and lift-off techniques are used to form an electrode metal, for example, a laminate of Ni having a thickness of 30 nm and Au having a thickness of 400 nm, on the GaN cap layer 90 exposed from the passivation film 80, to form the gate electrode 50. The gate electrode 50 functions as a Schottky electrode.
[0116] Through the above-mentioned steps, a semiconductor device 1Ca is formed, as shown in Fig. 19(B), in which the cap layer 40 with graded Al composition is interposed between the barrier layer 30 and the source electrode 60 and drain electrode 70, and the cap layer 40 with graded Al composition and the GaN cap layer 90 are interposed between the barrier layer 30 and the gate electrode 50. By providing the cap layer 40 with graded Al composition, in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, a high-performance semiconductor device 1Ca with low contact resistance and low on-resistance is realized. In addition, by interposing the GaN cap layer 90 between the barrier layer 30 and the gate electrode 50, a semiconductor device 1Ca in which leakage current from the gate electrode 50 is effectively suppressed is realized.
[0117] The types of metals and layer structures used for the gate electrode 50, source electrode 60, and drain electrode 70 of the semiconductor device 1Ca are not limited to the above examples, and the methods for forming them are not limited to the above examples. The gate electrode 50, source electrode 60, and drain electrode 70 may each have a single layer structure or a multilayer structure. When forming the source electrode 60 and drain electrode 70, it is not necessary to perform the heat treatment as described above as long as ohmic contact is achieved by forming the electrode metal. When forming the gate electrode 50, a further heat treatment may be performed after forming the electrode metal.
[0118] Here, an example is shown in which a semi-insulating SiC substrate 2 is used as the base substrate, but other substrate materials may be used as long as a nitride semiconductor is used in the structure having the function of a field effect transistor. A semi-insulating substrate or a conductive substrate may be used as the base substrate. In addition to a semi-insulating SiC substrate, a conductive SiC substrate, a sapphire substrate, a GaN substrate, a Si substrate, a diamond substrate, or the like may be used as the base substrate.
[0119] Here, an example has been shown in which the semiconductor device 1Ca is provided with the gate electrode 50 functioning as a Schottky electrode, but a gate insulating film made of an oxide, nitride, oxynitride, or the like may be provided between the gate electrode 50 and the barrier layer 30 to form an MIS-type gate structure.
[0120] The first to third embodiments have been described above. The semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, and 1Ca described in the first to third embodiments may employ a so-called asymmetric structure in which the distance between the gate electrode 50 and the drain electrode 70 is wider than the distance between the gate electrode 50 and the source electrode 60. By employing the asymmetric structure, the electric field between the gate electrode 50 and the drain electrode 70 is alleviated and the breakdown voltage is improved.
[0121] In addition, two or more of the semiconductor device 1A described in the first embodiment, the semiconductor device 1B described in the second embodiment, and the semiconductor device 1C described in the third embodiment can be mixed on a common base substrate.
[0122] [Fourth embodiment] Fig. 20 is a diagram for explaining an example of a semiconductor device according to the fourth embodiment. Fig. 20(A) and Fig. 20(B) each show a schematic cross-sectional view of a main part of an example of a semiconductor device according to the fourth embodiment.
[0123] 20A is an example of a Schottky barrier diode (SBD). The semiconductor device 1D includes a channel layer 10, a spacer layer 20, a barrier layer 30, a cap layer 40, a cathode electrode 110 (ohmic electrode), and an anode electrode 120 (Schottky electrode).
[0124] In the semiconductor device 1D, the channel layer 10, the spacer layer 20, the barrier layer 30, and the cap layer 40 with graded Al composition may be the same as those described for the semiconductor device 1A in the first embodiment. That is, the channel layer 10 may be made of GaN or AlGaN. The spacer layer 20 may be made of AlN or AlGaN. The barrier layer 30 may be made of InAlGaN or InAlN. FIG. 20 shows an example in which the channel layer 10 is made of GaN, the spacer layer 20 is made of AlN, and the barrier layer 30 is made of InAlGaN. The cap layer 40 with graded Al composition may be made of a combination of two or more of AlGaN, InAlN, and InAlGaN, in addition to AlGaN, InAlN, or InAlGaN, and the top layer may contain AlN. A 2DEG 100 is generated in the vicinity of the junction interface between the channel layer 10 and the spacer layer 20.
[0125] The semiconductor device 1D may also have a configuration in which the spacer layer 20 is not provided and the barrier layer 30 is provided directly on the channel layer 10. In this case, a 2DEG 100 is generated in the vicinity of the junction interface between the channel layer 10 and the barrier layer 30.
[0126] The cathode electrode 110 and the anode electrode 120 of the semiconductor device 1D are each made of a predetermined metal, with the cathode electrode 110 functioning as an ohmic electrode and the anode electrode 120 functioning as a Schottky electrode. In the semiconductor device 1D, the cap layer 40 with a graded Al composition is provided between the barrier layer 30 and the cathode electrode 110 such that the Al composition increases from the barrier layer 30 side toward the cathode electrode 110 side. The cathode electrode 110 is provided on a surface 40a of the cap layer 40 with a graded Al composition, and the anode electrode 120 is provided on a surface 30a of the barrier layer 30.
[0127] In the semiconductor device 1D, the cap layer 40 with graded Al composition is provided between the barrier layer 30 and the cathode electrode 110, thereby reducing the barrier at the contact of the cathode electrode 110 and realizing good ohmic contact of the cathode electrode 110. Even if the barrier layer 30 is made of InAlGaN or the like with a high Al composition that can generate a high concentration 2DEG 100 in the channel layer 10, good ohmic contact is realized and the contact resistance is reduced. This realizes a high-performance semiconductor device 1D that has high electron transport efficiency in the channel layer 10 when a forward bias is applied and functions as an SBD with excellent conduction characteristics.
[0128] In the semiconductor device 1D, the cap layer 40 having a graded Al composition is provided under the cathode electrode 110, and if it is not provided under the anode electrode 120, it may be provided so as to extend from under the cathode electrode 110 toward the outside thereof.
[0129] 20(B) shows a semiconductor device 1E, which is another example of an SBD. The semiconductor device 1E has a configuration in which a cap layer 40 having a graded Al composition extending from under the cathode electrode 110 and a cap layer 90 provided on the cap layer 40 except for under the cathode electrode 110 are interposed between the barrier layer 30 and the anode electrode 120. The semiconductor device 1E differs from the semiconductor device 1D (FIG. 20(A)) in having such a configuration.
[0130] The cap layer 90 of the semiconductor device 1E may be the same as the cap layer 90 described for the semiconductor device 1C in the third embodiment. That is, GaN is used for the cap layer 90. The GaN cap layer 90 is provided on the surface 40a of the cap layer 40 having a graded Al composition.
[0131] In the semiconductor device 1E, a cap layer 40 with a graded Al composition is provided between the barrier layer 30 and the cathode electrode 110, thereby reducing the barrier at the contact with the cathode electrode 110 and realizing a good ohmic contact with low contact resistance. In addition, a cap layer 90 of GaN is provided between the barrier layer 30 and the anode electrode 120 in the semiconductor device 1E, thereby increasing the barrier at the contact with the anode electrode 120 and realizing a good Schottky contact. This realizes a high-performance semiconductor device 1E that functions as an SBD with excellent conductive characteristics when a forward bias is applied and excellent non-conductive characteristics when a reverse bias is applied.
[0132] In the semiconductor device 1E, the cap layer 40 having a graded Al composition may be selectively provided under the cathode electrode 110 and the anode electrode 120, and the GaN cap layer 90 may be selectively provided under the anode electrode 120.
[0133] The semiconductor devices 1D and 1E described in the fourth embodiment can also be mounted on a common base substrate together with the semiconductor device 1A described in the first embodiment, the semiconductor device 1B described in the second embodiment, and the semiconductor device 1C described in the third embodiment.
[0134] Although the first to fourth embodiments have been described above, the cap layer 40 with the graded Al composition as described above is not limited to In-based nitride semiconductors such as InAlGaN and InAlN, but can also be applied to cases where other nitride semiconductors are used for the barrier layer 30. For example, the cap layer 40 with the graded Al composition can be provided between the barrier layer 30 using AlGaN or AlN and the electrodes (the source electrode 60 and the drain electrode 70, or the cathode electrode 110) that are in ohmic contact, according to the examples described in the first to fourth embodiments. Even in a semiconductor device with such a configuration, it is possible to reduce the barrier at the contact of the electrodes and reduce the contact resistance, compared to a case where the barrier layer 30 using AlGaN or AlN is directly connected to the electrodes that are in ohmic contact. As a result, a high-performance semiconductor device with low contact resistance and low on-resistance can be realized.
[0135] The semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, 1D, 1E, etc. having the configurations described above in the first to fourth embodiments can be applied to various electronic devices. As an example, the application of the semiconductor device having the above configuration to a semiconductor package, a power factor correction circuit, a power supply device, and an amplifier will be described below.
[0136] [Fifth embodiment] Here, an example of application of a semiconductor device having the above-mentioned configuration to a semiconductor package will be described as the fifth embodiment.
[0137] Fig. 21 is a diagram for explaining an example of a semiconductor package according to the fifth embodiment, which diagrammatically shows a plan view of a main part of the example of the semiconductor package according to the fifth embodiment.
[0138] 21 is an example of a discrete package. The semiconductor package 200 includes, for example, the semiconductor device 1A described in the first embodiment, a lead frame 210 on which the semiconductor device 1A is mounted, and a resin 220 that seals them.
[0139] The semiconductor device 1A is mounted on a die pad 210a of a lead frame 210 using a die attach material or the like (not shown). The semiconductor device 1A is provided with a pad 50a connected to the gate electrode 50, a pad 60a connected to the source electrode 60, and a pad 70a connected to the drain electrode 70. The pads 50a, 60a, and 70a are connected to the gate lead 211, the source lead 212, and the drain lead 213 of the lead frame 210, respectively, using wires 230 made of Al or the like. The lead frame 210, the semiconductor device 1A mounted thereon, and the wires 230 connecting them are sealed with resin 220 so that parts of the gate lead 211, the source lead 212, and the drain lead 213 are exposed.
[0140] For example, the semiconductor device 1A described in the first embodiment is used to obtain a semiconductor package 200 having such a configuration. Here, the semiconductor device 1A is taken as an example, but it is possible to obtain a similarly high-performance semiconductor package by using other semiconductor devices 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. functioning as HEMTs, or semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. in which semiconductor devices 1D, 1E, etc. functioning as SBDs are mixed.
[0141] As described above, in the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc., the cap layer 40 having a graded Al composition, in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, is provided between the barrier layer 30 and the source electrode 60 and the drain electrode 70. This realizes a high-performance HEMT with low contact resistance and low on-resistance. The semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. having such excellent characteristics are used to realize a high-performance semiconductor package 200.
[0142] Also, a discrete package can be obtained using the semiconductor device 1D, 1E, etc. that functions as an SBD. As described above, the semiconductor device 1D, 1E, etc. improves the characteristics of the SBD when a forward bias or even a reverse bias is applied. By using the semiconductor device 1D, 1E, etc. that has such excellent characteristics, a high-performance semiconductor package can be realized.
[0143] [Sixth embodiment] Here, an example of application of the semiconductor device having the above-mentioned configuration to a power factor correction circuit will be described as the sixth embodiment.
[0144] Fig. 22 is a diagram for explaining an example of a power factor correction circuit according to the sixth embodiment. Fig. 22 shows an equivalent circuit diagram of an example of the power factor correction circuit according to the sixth embodiment. The power factor correction (PFC) circuit 300 shown in FIG. 22 includes a switch element 310, a diode 320, a choke coil 330, a capacitor 340, a capacitor 350, a diode bridge 360, and an AC power supply 370 (AC).
[0145] In the PFC circuit 300, a drain electrode of a switch element 310 is connected to an anode terminal of a diode 320 and one terminal of a choke coil 330. A source electrode of the switch element 310 is connected to one terminal of a capacitor 340 and one terminal of a capacitor 350. The other terminal of the capacitor 340 is connected to the other terminal of the choke coil 330. The other terminal of the capacitor 350 is connected to a cathode terminal of the diode 320. A gate driver is connected to the gate electrode of the switch element 310. An AC power supply 370 is connected between both terminals of the capacitor 340 via a diode bridge 360, and a DC power supply (DC) is taken out from between both terminals of the capacitor 350.
[0146] For example, the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. functioning as HEMTs are used in the switch element 310 of the PFC circuit 300 having such a configuration.
[0147] As described above, in the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc., the cap layer 40 having a graded Al composition, in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, is provided between the barrier layer 30 and the source electrode 60 and the drain electrode 70. This realizes a high-performance HEMT with low contact resistance and low on-resistance. The semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. having such excellent characteristics are used to realize a high-performance PFC circuit 300.
[0148] The diode 320 and the diode bridge 360 of the PFC circuit 300 may use the above-mentioned semiconductor devices 1D, 1E, etc., which function as SBDs. As described above, the semiconductor devices 1C, 1D, etc. improve the characteristics of the SBD when a forward bias or further when a reverse bias is applied. The semiconductor devices 1D, 1E, etc., having such excellent characteristics are used to realize a high-performance PFC circuit 300.
[0149] [Seventh embodiment] Here, an example of application of a semiconductor device having the above-mentioned configuration to a power supply device will be described as the seventh embodiment.
[0150] Fig. 23 is a diagram for explaining an example of a power supply device according to the seventh embodiment. Fig. 23 shows an equivalent circuit diagram of the example of the power supply device according to the seventh embodiment. The power supply device 400 shown in FIG. 23 includes a primary side circuit 410, a secondary side circuit 420, and a transformer 430 provided between the primary side circuit 410 and the secondary side circuit 420.
[0151] The primary side circuit 410 includes the PFC circuit 300 as described in the sixth embodiment, and an inverter circuit, for example, a full-bridge inverter circuit 440, connected between both terminals of the capacitor 350 of the PFC circuit 300. The full-bridge inverter circuit 440 includes a plurality of (four in this example) switch elements 441, 442, 443, and 444.
[0152] The secondary side circuit 420 includes a plurality of (three in this example) switch elements 421, 422, and 423. For example, the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. functioning as HEMTs are used for the switch element 310 of the PFC circuit 300 included in the primary side circuit 410 of the power supply device 400 having such a configuration, and for the switch elements 441-444 of the full bridge inverter circuit 440. For example, normal MIS type FETs using Si are used for the switch elements 421-423 of the secondary side circuit 420 of the power supply device 400.
[0153] As described above, in the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc., a cap layer 40 having a graded Al composition, in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, is provided between the barrier layer 30 and the source electrode 60 and the drain electrode 70. This realizes a high-performance HEMT with low contact resistance and low on-resistance. A high-performance power supply device 400 is realized by using the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. having such excellent characteristics.
[0154] Furthermore, the diode 320 and the diode bridge 360 of the PFC circuit 300 included in the primary side circuit 410 may use the above-mentioned semiconductor devices 1D, 1E, etc., functioning as SBDs, as described in the sixth embodiment. As described above, the semiconductor devices 1D, 1E, etc. improve the characteristics of the SBD when a forward bias or further a reverse bias is applied. By using the semiconductor devices 1D, 1E, etc., having such excellent characteristics, a high-performance PFC circuit 300 is realized. By using such a PFC circuit 300, a high-performance power supply device 400 is realized.
[0155] [Eighth embodiment] Here, an example of application of the semiconductor device having the above-mentioned configuration to an amplifier will be described as the eighth embodiment.
[0156] Fig. 24 is a diagram for explaining an example of an amplifier according to the eighth embodiment. Fig. 24 shows an equivalent circuit diagram of an example of the amplifier according to the eighth embodiment. The amplifier 500 shown in FIG. 24 includes a digital predistortion circuit 510, a mixer 520, a mixer 530, and a power amplifier 540.
[0157] The digital predistortion circuit 510 compensates for nonlinear distortion of the input signal. The mixer 520 mixes the input signal SI, for which the nonlinear distortion has been compensated, with an AC signal. The power amplifier 540 amplifies the signal obtained by mixing the input signal SI with the AC signal. In the amplifier 500, for example, by switching a switch, the output signal SO can be mixed with the AC signal in the mixer 530 and sent to the digital predistortion circuit 510. The amplifier 500 can be used as a high-frequency amplifier or a high-power amplifier.
[0158] The power amplifier 540 of the amplifier 500 having such a configuration uses the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. functioning as HEMTs.
[0159] As described above, in the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc., the cap layer 40 having a graded Al composition, in which the Al composition increases from the barrier layer 30 side toward the source electrode 60 side and the drain electrode 70 side, is provided between the barrier layer 30 and the source electrode 60 and the drain electrode 70. This realizes a high-performance HEMT with low contact resistance and low on-resistance. The semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, etc. having such excellent characteristics are used to realize a high-performance amplifier 500.
[0160] Furthermore, when a diode is used in the amplifier 500, the diode may be an SBD such as the semiconductor device 1D, 1E. As described above, in the semiconductor device 1D, 1E, etc., the characteristics of the SBD when a forward bias or further when a reverse bias is applied are improved. By using the semiconductor device 1D, 1E, etc. having such excellent characteristics, a high-performance amplifier 500 is realized.
[0161] Various electronic devices to which the semiconductor devices 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, 1D, 1E and the like are applied (such as the semiconductor package 200, the PFC circuit 300, the power supply device 400, and the amplifier 500 described in the fourth to seventh embodiments) can be mounted in various electronic devices or electronic devices. For example, the devices can be mounted in various electronic devices or electronic devices such as computers (personal computers, supercomputers, servers, and the like), smartphones, mobile phones, tablet terminals, sensors, cameras, audio equipment, measuring equipment, inspection equipment, and manufacturing equipment.
[0162] The following supplementary notes are further provided with respect to the above-described embodiment. (Supplementary Note 1) A channel layer including a first nitride semiconductor; a barrier layer provided on the first surface side of the channel layer and including a second nitride semiconductor; a first cap layer provided on a second surface side of the barrier layer opposite to the channel layer side, the first cap layer including a third nitride semiconductor containing Al and at least one of Ga and In, the Al composition increasing from the barrier layer side toward a third surface side opposite to the barrier layer side; A semiconductor device comprising:
[0163] (Appendix 2) The semiconductor device according to appendix 1, wherein the second nitride semiconductor of the barrier layer contains Al and In. (Note 3) The increase in the Al composition per unit length of the first cap layer in the direction from the barrier layer side to the third surface side is 0.1 nm -1 The semiconductor device according to claim 1 or 2, characterized in that:
[0164] (Note 4) A source electrode and a drain electrode are provided on the third surface side of the first cap layer and in contact with the third surface; a gate electrode provided between the source electrode and the drain electrode on the second surface side of the barrier layer; 4. The semiconductor device according to claim 1, further comprising:
[0165] (Supplementary Note 5) The semiconductor device according to Supplementary Note 4, wherein the gate electrode is provided on the third surface side of the first cap layer provided between the source electrode and the drain electrode.
[0166] (Appendix 6) The semiconductor device according to appendix 4, wherein the gate electrode penetrates the first cap layer and contacts the barrier layer. (Note 7) A second cap layer is provided between the source electrode and the drain electrode on the third surface side of the first cap layer, the second cap layer including a fourth nitride semiconductor containing Ga; 5. The semiconductor device according to claim 4, wherein the gate electrode is provided on a fourth surface side of the second cap layer opposite to the first cap layer side.
[0167] (Note 8) A cathode electrode is provided on the third surface side of the first cap layer and in contact with the third surface; an anode electrode provided on the second surface side of the barrier layer; 4. The semiconductor device according to claim 1, further comprising:
[0168] (Supplementary Note 9) The semiconductor device according to any one of Supplementary Notes 1 to 8, further comprising a spacer layer provided between the channel layer and the barrier layer, the spacer layer including a fifth nitride semiconductor. (Appendix 10) The semiconductor device according to any one of appendices 1 to 9, wherein the first surface of the channel layer is a (0001) surface.
[0169] (Appendix 11) A step of forming a channel layer including a first nitride semiconductor; forming a barrier layer including a second nitride semiconductor on the first surface side of the channel layer; forming a cap layer on a second surface side of the barrier layer opposite to the channel layer side, the cap layer including a third nitride semiconductor containing Al and at least one of Ga and In, the Al composition increasing from the barrier layer side toward a third surface side opposite to the barrier layer side; 1. A method for manufacturing a semiconductor device comprising the steps of:
[0170] (Supplementary Note 12) A channel layer including a first nitride semiconductor; a barrier layer provided on the first surface side of the channel layer and including a second nitride semiconductor; a cap layer provided on a second surface side of the barrier layer opposite to the channel layer side, the cap layer including a third nitride semiconductor containing Al and at least one of Ga and In, the Al composition increasing from the barrier layer side toward a third surface side opposite to the barrier layer side; An electronic device comprising a semiconductor device having the [Explanation of symbols]
[0171] 1A, 1Aa, 1Ab, 1Ac, 1Ad, 1B, 1Ba, 1C, 1Ca, 1D, 1E, 1000, 1100, 1100a, 1100b Semiconductor device 2. Semi-insulating SiC substrate 3 AlN nucleation layer 5,6,7 Laminated structure 10,1010,1110 Channel Layer 10a,20a,30a,40a,90a side 20,1120 Spacer layer 30,1030,1130 Barrier layer 40,90 Cap layer 50,1050,1150 Gate electrode 50a, 60a, 70a pads 60,1060,1160 Source electrode 70,1070,1170 Drain electrode 80 Passivation Film 100,2000 2DEG 110 Cathode electrode 120 Anode electrode 150a,150b,150c layer 200 Semiconductor Packages 210 Lead Frame 210a Die pad 211 Gate Lead 212 Source Read 213 Drain Lead 220 Resin 230 Wire 300 PFC circuit 310,421,422,423,441,442,443,444 Switching elements 320 Diode 330 Choke Coil 340,350 Capacitor 360 Diode Bridge 370 AC power supply 400 power supply 410 Primary circuit 420 Secondary circuit 430 Trans 440 Full-bridge inverter circuit 500 Amplifier 510 Digital Pre-Distortion Circuit 520,530 Mixer 540 Power Amplifier 1200 Laminate 1210 Recess 1220 n-GaN layer 1230 Damage 3000 Contact Resistance
Claims
1. a channel layer including a first nitride semiconductor; a barrier layer provided on the first surface side of the channel layer and including a second nitride semiconductor containing Al and In; a first cap layer provided on a second surface side of the barrier layer opposite to the channel layer side, the first cap layer including a third nitride semiconductor containing Al and at least one of Ga and In, the Al composition increasing from the barrier layer side toward a third surface side opposite to the barrier layer side; a source electrode and a drain electrode provided on the third surface side of the first cap layer and in contact with the third surface; a gate electrode provided on the third surface side of the first cap layer, located between the source electrode and the drain electrode, and having a lower end on the barrier layer side located on the third surface side of the first cap layer; A semiconductor device comprising:
2. a second cap layer provided between the source electrode and the drain electrode on the third surface side of the first cap layer, the second cap layer including a fourth nitride semiconductor containing Ga; 2 . The device according to claim 1 , wherein the gate electrode is provided on a fourth surface side of the second cap layer opposite to the first cap layer side.
3. forming a channel layer including a first nitride semiconductor; forming a barrier layer including a second nitride semiconductor containing Al and In on the first surface side of the channel layer; forming a cap layer on a second surface side of the barrier layer opposite to the channel layer side, the cap layer including a third nitride semiconductor containing Al and at least one of Ga and In, the Al composition increasing from the barrier layer side toward a third surface side opposite to the barrier layer side; forming a source electrode and a drain electrode on the third surface side of the cap layer so as to be in contact with the third surface; forming a gate electrode on the third surface side of the cap layer, the gate electrode being located between the source electrode and the drain electrode, the gate electrode having a lower end on the barrier layer side being located on the third surface side of the cap layer; 1. A method for manufacturing a semiconductor device comprising the steps of:
4. a channel layer including a first nitride semiconductor; a barrier layer provided on the first surface side of the channel layer and including a second nitride semiconductor containing Al and In; a cap layer provided on a second surface side of the barrier layer opposite to the channel layer side, the cap layer including a third nitride semiconductor containing Al and at least one of Ga and In, the Al composition increasing from the barrier layer side toward a third surface side opposite to the barrier layer side; a source electrode and a drain electrode provided on the third surface side of the cap layer and in contact with the third surface; a gate electrode provided on the third surface side of the cap layer, located between the source electrode and the drain electrode, and having a lower end on the barrier layer side located on the third surface side of the cap layer; An electronic device comprising a semiconductor device having the
Citation Information
Patent Citations
Field effect transistor
JP2008124373A
Cap layer including aluminum nitride for nitride-based transistor, and method of fabricating the same
JP2008227501A
Semiconductor device and method of manufacturing same
JP2010109117A
HEMT device and method for manufacturing the same
JP2011523218A
Semiconductor device
JP2016187025A