Carbon fiber composite material and method for processing laminate
The carbon fiber composite material with controlled electrical discharge machining addresses tool wear and surface irregularities, enhancing strength and smoothness through dense fiber packing.
Patent Information
- Application Number
- JP2020138888
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-19
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-08-19
AI Technical Summary
Existing methods for cutting carbon fiber composite materials result in tool wear, peeling, fluffing, and uneven surfaces due to irregularities, leading to insufficient strength.
A carbon fiber composite material with densely packed carbon fibers and a processing method involving electrical discharge machining, where the laminate is heated for a short duration, using a discharge circuit with controlled voltage and current to minimize unevenness and fluffing.
The method produces a carbon fiber composite material with reduced surface irregularities, increased carbon fiber area occupancy, and improved strength, suitable for high-strength applications.
Smart Images

Figure 0007594271000004 
Figure 0007594271000005 
Figure 0007594271000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon fiber composite material and a method for processing a laminate. [Background technology]
[0002] Carbon fiber composite materials (CFRP: Carbon Fiber Reinforced Plastics) are known as high-strength, lightweight materials. Compared to steel, the specific gravity of carbon fiber composite materials is about 1 / 5 and the tensile strength is about 6 times. Therefore, carbon fiber composite materials are expected to be a material that can replace metal materials.
[0003] Carbon fiber composite materials are highly anisotropic and offer a high degree of freedom in design, and as such are used in a variety of components for aircraft, rockets, and other applications, contributing to energy conservation.
[0004] In order to utilize carbon fiber composite materials in various parts, they need to be processed into various shapes. Cutting is known as a method for processing carbon fiber composite materials. For example, Patent Document 1 describes a method for cutting carbon fiber reinforcement. FIG. 24 is an electron microscope image of a cross section of a carbon fiber composite material cut with a band saw. The area occupied by carbon fibers in the cut surface shown in FIG. 24 was about 60%. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-172317 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the method described in Patent Document 1, the tool used for cutting may be worn out. In addition, in the method described in Patent Document 1, the machined surface of the carbon fiber composite material may be torn, frayed, or have carbon fibers pulled out, resulting in unevenness and insufficient strength. In the cut surface of FIG. 24, carbon fibers are confirmed to have been pulled out, and there are unevenness.
[0007] The present invention has been made in consideration of the above problems, and has an object to provide a carbon fiber composite material having a processed surface with minimal irregularities. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention provides the following means.
[0009] (1) A carbon fiber composite material according to a first aspect of the present invention is a carbon fiber composite material formed by stacking a plurality of prepregs, each prepreg being composed of a plurality of carbon fibers and a resin that bonds the plurality of carbon fibers, in which at least some of the carbon fibers extend in the same direction and have a dense region in which the plurality of carbon fibers are densely packed together, and in which end faces of the carbon fibers are exposed on at least a portion of a surface thereof, and the maximum diameter of the end faces is greater than the center-to-center distance between end faces of adjacent carbon fibers.
[0010] (2) In the carbon fiber composite material according to the above aspect, the carbon fibers may occupy 70% or more of an area on at least a portion of a surface.
[0011] (3) A method for processing a laminate according to a second aspect of the present invention is a method for producing the carbon fiber composite material according to the first aspect by processing a laminate in which a plurality of prepregs made of carbon fibers impregnated with resin are stacked in the thickness direction, and may include a heating step of heating the laminate in a processing area of each layer stacked in the stacking direction for a time of 500 μs or less.
[0012] (4) In the method for machining a laminate according to the above aspect, the heating step is a discharge step in which electric discharge machining is performed on the laminate, and the discharge step may involve generating an electric discharge using a discharge part immersed in a machining fluid and connected to a discharge circuit, thereby thermally machining the machining area.
[0013] (5) In the method for processing a laminate according to the above aspect, the discharge circuit may include a power supply, a capacitor and a resistor connected in series to the power supply, and a discharge unit connected in parallel to the power supply and the capacitor. (6) In the method for processing a laminate according to the above aspect, the discharge circuit may further include a transistor connected in series with the power supply, the capacitor, and the resistor.
[0014] (7) In the method for processing a laminate according to the above aspect, the discharge circuit may include a power supply, a capacitor and a voltage control unit connected in series to the power supply, and a discharge unit connected in parallel to the power supply and the capacitor, and the voltage control unit may include a first unit and a second unit in which a transistor and a resistor are connected in series, and the method may include a first step of turning on the first unit and turning off the second unit, a second step of turning on the second unit after the inter-electrode voltage of the capacitor exceeds a start-up voltage, and a third step of bringing the discharge unit closer to the laminate when the potential difference between the discharge unit and the laminate is equal to or greater than a servo reference voltage, and moving the discharge unit away from the laminate when the potential difference between the discharge unit and the laminate is equal to or less than the servo reference voltage.
[0015] (8) In the method for processing a laminate according to the above aspect, the discharge circuit may include a power supply, and a voltage control unit and a discharge unit connected in series to the power supply, the voltage control unit may include a first unit and a second unit in which a transistor and a resistor are connected in series, and the discharge unit may include two opposing electrodes, and the discharge process may include a first step of turning on the first unit and turning off the second unit, a second step of turning on the second unit when the potential of the discharge unit exceeds a current superposition voltage, a third step of bringing the discharge unit closer to the laminate when the potential difference between the discharge unit and the laminate is equal to or greater than a servo reference voltage, and moving the discharge unit away from the laminate when the potential difference between the discharge unit and the laminate is equal to or less than the servo reference voltage, a fourth step of turning off the second unit when a set discharge time has elapsed after the potential of the discharge unit falls below a discharge detection voltage, and a fifth step of moving the discharge unit away from the laminate.
[0016] (9) The method for processing a laminate according to the above aspect may be a method for forming pores in the laminate, and the pores may have a diameter of 500 μm or more. Effect of the Invention
[0017] According to the present invention, it is possible to provide a carbon fiber composite material with reduced unevenness. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a perspective view of a carbon fiber composite material (laminate). [Diagram 2] FIG. 1 is an example of a cross-sectional view of a carbon fiber composite material (laminate). [Diagram 3] FIG. 1 is a perspective view of a carbon fiber composite material (laminate). [Figure 4] FIG. 1 is a perspective view of a carbon fiber composite material (laminate). [Diagram 5] FIG. 1 is a cross-sectional schematic diagram illustrating an example of a processing apparatus 200 for processing a carbon fiber composite material (laminate). [Figure 6] 1 is a circuit diagram showing a main part of a discharge circuit according to a first embodiment. [Figure 7] FIG. 4 is a circuit diagram showing a main part of a discharge circuit according to a comparative example. [Figure 8] 5 is a diagram showing a voltage and a current of a discharge part when performing electric discharge machining by the machining method according to the first embodiment. FIG. [Figure 9] 1 is an electron microscope image of the side of a carbon fiber composite material (laminate) before electrical discharge machining. [Figure 10] FIG. 2 is a perspective view showing an example of the configuration of a carbon fiber composite material after electric discharge machining. [Figure 11] 1 is an electron microscope image of the machined surface of a carbon fiber composite material after electrical discharge machining. [Figure 12] FIG. 11 is a circuit diagram showing a main part of a discharge circuit according to a first modified example. [Figure 13] 13 is a diagram showing the voltage and current of a discharge part when electric discharge machining is performed by the machining method according to the first modified example. FIG. [Figure 14] FIG. 11 is a circuit diagram showing a main part of a discharge circuit according to Modification 2. [Figure 15] 13 is a diagram showing the voltage and current of a discharge part when electric discharge machining is performed by the machining method according to the second modified example. FIG. [Figure 16] FIG. 11 is a circuit diagram showing a main part of a discharge circuit according to a modified example of the embodiment. [Figure 17] 1 is an optical microscope image of the front and back surfaces of the carbon fiber composite material of Example 1. [Figure 18] FIG. 4 is a diagram showing the voltage and current of a discharge part when electric discharge machining is performed in Example 1. [Figure 19] 1 is an electron microscope image of a processed surface of the carbon fiber composite material of Example 1. [Figure 20] 1 is an optical microscope image of a processed surface of the carbon fiber composite material of Example 1. [Figure 21] 3 is an optical microscope image of the front and back surfaces of the carbon fiber composite material of Reference Example 1. [Figure 22] FIG. 11 is a diagram showing the voltage and current of a discharge part when electric discharge machining is performed in Reference Example 1. [Figure 23]This is the carbon fiber composite material that was hollowed out in Example 2. [Figure 24] 1 is an electron microscope image of a cross section of a cut carbon fiber composite material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, numbers, arrangements, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. The present invention can be implemented by appropriately changing them within the scope of the effects of the present invention. For example, the configurations described in different embodiments can be implemented by appropriately combining them.
[0020] FIG. 1 is a perspective view showing a carbon fiber composite material (laminate) 100a, and FIG. 2 is a schematic cross-sectional view of the laminate 100a perpendicular to the lamination direction. In this specification, a carbon fiber composite material that has not been processed after laminating prepregs may be referred to as a laminate. The processing here refers to a process in which heating is performed within a predetermined time, such as a heating process described in detail below. The prepreg 10 is formed by impregnating carbon fibers 1 with resin. The prepreg 10 has a sheet shape. The laminate 100a is a structure in which a plurality of prepregs 10 are laminated in the thickness direction. The prepreg 10 includes carbon fibers 1 and resin 2 surrounding the carbon fibers 1. The carbon fibers are made of known carbon fibers. The resins are made of known thermosetting resins and thermoplastic resins. The laminate 100a is made of five layers of prepregs 10, but the number of prepregs provided in the laminate is not limited. The laminate may be made of one layer of prepreg.
[0021] The prepreg 10 has a plurality of carbon fibers. For example, it has a first carbon fiber 1a, a second carbon fiber 1b, a third carbon fiber 1c, a fourth carbon fiber 1d, and a fifth carbon fiber 1e. The first carbon fiber 1a, the second carbon fiber 1b, the third carbon fiber 1c, the fourth carbon fiber 1d, and the fifth carbon fiber 1e extend in a first direction. That is, the orientation direction of the first carbon fiber 1a, the second carbon fiber 1b, the third carbon fiber 1c, the fourth carbon fiber 1d, and the fifth carbon fiber 1e is the same. For convenience of explanation, FIG. 1 also shows the first direction. In this specification, the first carbon fiber 1a, the second carbon fiber 1b, the third carbon fiber 1c, the fourth carbon fiber 1d, and the fifth carbon fiber 1e may be collectively referred to as carbon fiber 1. The carbon fiber 1 is a fiber made of synthetic fiber or coal-based or petroleum-based pitch that is heated at high temperature to be carbonized or graphitized, or a fiber made of carbon nanotubes or graphene. That is, the carbon fiber 1 can be either a PAN (polyacrylonitrile) carbon fiber or a pitch carbon fiber. As the PAN-based carbon fiber, either a regular toe type or a large toe type having 40,000 or more fiber bundles can be used.
[0022] The regions close to the ends in the in-plane direction of the prepreg 10 are referred to as the ends 3. The ends 3 include a first end 3a and a second end 3b perpendicular to the extending direction of the carbon fibers 1, and a third end 3c and a fourth end 3d parallel to the extending direction of the carbon fibers 1. The ends 3 are, for example, regions within 1 mm from the ends in the in-plane direction of the prepreg 10.
[0023] 3 and 4 are schematic perspective views showing carbon fiber composite materials (laminates) 100b and 100c of other examples. Prepregs 11 and 20 are laminated in the laminate 100b. The prepreg 11 includes a plurality of carbon fibers in the lamination direction. The number of carbon fibers in the prepreg is arbitrary. The carbon fiber 1 provided in the center of the prepreg extends in a first direction. For example, the prepreg may include three or more layers of carbon fibers arranged in the lamination direction. The plurality of carbon fibers provided in the prepreg 20 extend in a second direction. The second direction is a direction intersecting with the first direction. As shown in FIG. 3, the laminate may have different orientation directions (extension directions) of the carbon fibers for each prepreg. For convenience of explanation, FIG. 3 illustrates an example of the first direction and the second direction.
[0024] The laminate 100c has prepregs 10, 20, and 21 laminated therein. The prepreg 21 has carbon fibers 1 extending in a first direction and carbon fibers 1A extending in a second direction. In the prepreg 21, the carbon fibers 1 and the carbon fibers 1A are woven, for example, in a twill weave. As shown in FIG. 4, one layer of prepreg may include a plurality of carbon fibers having different orientation directions. The prepreg may be plain woven, twill woven, or the like.
[0025] The orientation direction of the carbon fibers is not limited to the laminates 100a, 100b, and 100c. For example, the orientation direction of the carbon fibers is not limited to the first direction and the second direction, and is arbitrary, and the number and configuration of the prepregs included in the laminate are arbitrary.
[0026] <Processing method of laminate> The method for processing a laminate according to the first embodiment includes a step of applying heat for a predetermined time to the regions of the layers overlapping in the lamination direction of the carbon fiber composite material (laminate). The means for applying heat is, for example, laser processing or electric discharge processing. The time for applying heat to the laminate is, for example, 1 μs or more and 500 μs or less, preferably 200 μs or less, and more preferably 100 μs or less. When laser processing is used, the time for applying heat to the laminate may be 1 fs or more. The time for applying heat to the laminate may be appropriately changed depending on the output. The method for processing a laminate according to this embodiment can increase the area occupied by carbon fibers on the processed surface.
[0027] A method for machining the laminate by electrical discharge machining will be described below. The method for machining the laminate according to this embodiment can machine, for example, a part of the side surface of the laminate.
[0028] Fig. 5 is a cross-sectional schematic diagram showing an example of a processing apparatus 200 for processing a laminate. Fig. 5 is a cross-sectional schematic diagram including the center in a plan view in an in-plane direction of the laminate 100. Hereinafter, an example will be described in which a laminate 100a is subjected to electric discharge processing using the laminate processing method according to this embodiment.
[0029] The processing device 200 includes, for example, a container 30 , a precision vice 40 installed in the container 30 , a conductive auxiliary member 50 , and a discharge device 60 .
[0030] The container 30 is a container of any shape, and contains the machining liquid 70. Any known machining liquid that can maintain insulation can be used as the machining liquid 70. For example, the machining liquid 70 can be pure water, distilled water, sugar water, ethanol, or an electric discharge machining oil such as kerosene (white lamp oil). The machining liquid 70 is preferably an electric discharge machining oil. Although the details will be described later, when the electric discharge machining oil is used as the machining liquid 70, the diameter of the carbon fiber 1 can be enlarged by the decomposition carbon of the electric discharge machining oil. By performing electric discharge machining in the machining liquid 70, the electric discharge machining can be performed in an oxygen-free environment, and the safety of the machining can be improved.
[0031] The precision vice 40 has a main body 41 and a clamping part 42. The clamping part 42 extends, for example, perpendicular to the main body 41. The clamping part 42 clamps the laminate 100a. In the example shown in FIG. 5, the clamping part 42 clamps the laminate 100a via the conductive auxiliary member 50. The precision vice 40 may perform electric discharge machining by positively or negatively charging the laminate and charging the discharge part 61 to a polarity different from that of the laminate. Alternatively, electric discharge machining may be performed by connecting the discharge part 61 to an AC power source without charging the laminate. When electric discharge machining oil is used as the machining fluid 70, decomposition carbon of the electric discharge machining oil tends to gather on the positive electrode side, so it is preferable to positively charge the laminate and negatively charge the discharge part 61, which will be described in detail later. When using a machining liquid such as pure water, distilled water, sugar water, or ethanol as the machining liquid 70, it is believed that oxygen is generated on the positive electrode side due to the electrolysis of water, and the activated carbon combines with the oxygen to become gasified, so the laminate is negatively charged and the discharge section 61, which will be described in detail later, is positively charged to perform electric discharge machining.
[0032] The conductive auxiliary member 50 covers the side surface of the laminate 100a. The side surface here refers to a surface perpendicular to the lamination direction of the laminate 100a. The conductive auxiliary member 50 is a material having electrical conductivity. The conductive auxiliary member 50 is, for example, a copper film, a metal plate, or a silver paste. Conventionally, it has been thought that electrical discharge machining can be used only for conductive workpieces. However, the present inventors have found that stable electrical discharge machining is possible by covering the side surface of the laminate 100a with the conductive auxiliary member 50, even when the workpiece is a laminate 100a with low electrical conductivity.
[0033] The conductive auxiliary member 50 may have a U-shaped cross section that contacts the upper and lower surfaces of the laminate 100a as shown in Fig. 5. In such a case, the conductive auxiliary member 50 is disposed so as to cover all of the ends 3a, 3b, 3c, and 3d of the laminate 100a. Here, the ends 3a and 3b are perpendicular to the first direction. The ends 3c and 3d are perpendicular to the second direction.
[0034] Incidentally, this embodiment is not limited to the method using the conductive auxiliary member 50, and may be performed without using the conductive auxiliary member 50 by scraping the side surface, or the side surface and end portion 3, of the laminate 100a to expose the carbon fibers 1.
[0035] In the method for machining the laminate according to this embodiment, electric discharge machining is performed in a state in which the laminate 100 is clamped by the precision vice 40. The electric discharge machining is performed by an electric discharge device 60.
[0036] The discharge device 60 has a discharge unit 61, a discharge circuit 62, and a vertical drive mechanism 63. In this specification, for convenience of explanation, the discharge unit 61 may be treated as a part of the discharge circuit 62, or the discharge unit 61 and the discharge circuit 62 may be treated as existing independently. Even when the discharge unit 61 and the discharge circuit 62 are treated as existing independently, the discharge unit 61 is electrically connected to the discharge circuit 62, and therefore the discharge unit 61 and the discharge circuit 62 can be regarded as being integrated.
[0037] The discharge part 61 has a shape that matches the shape of the desired machining surface. For example, when the machining surface is to be circular, annular, or polygonal, the cross-sectional shape of the discharge part 61 perpendicular to the axial direction is circular, annular, or polygonal. That is, the discharge part 61 has a shape such as a columnar shape, a cylindrical shape, a polygonal shape, or a cone shape. It is to be noted that the present invention is not limited to this example, and the discharge part 61 may have a configuration in which multiple ends are present by branching. The diameter of the discharge part 61 is not limited to this example, but is, for example, 10 μm or more, preferably 500 μm or more, and may be 1 mm or more or 2 mm or more. By using a discharge part with a diameter of 10 μm or more, a hole with a pore diameter of 10 μm or more is formed. If the pore diameter is sufficiently large, the machining fluid 70 will sufficiently penetrate into the pore. It is to be noted that, when the cross-sectional shape perpendicular to the axial direction of the discharge part 61 is polygonal, it is preferable that the maximum distance from the center of gravity to the apex is within the above range. The discharge portion 61 is an electrode made of, for example, copper, graphite, tungsten, silver-tungsten, copper-tungsten, or the like.
[0038] The discharge unit 61 performs electric discharge machining while approaching the laminate 100a so that the distance from the machining surface of the laminate 100a is maintained at a distance that allows electric discharge machining. The discharge unit 61 may be configured not to rotate, or may be configured to be connected to a motor and rotate at high speed. The discharge unit 61 may also be configured to be connected to a swinging mechanism and swing in the in-plane direction of the laminate, or to temporarily move up and down (jump) in the stacking direction of the laminate. This configuration allows machining waste generated by electric discharge machining to escape. Below, a case where the discharge unit 61 is connected to a motor will be described. The rotation speed and vertical drive speed of the discharger 61 are preferably controlled to rotate at least once per 1 mm of approach. For example, when rotating at a high speed of 600 rpm, the vertical drive speed is preferably controlled to be 10 mm / s or less. The rotation speed of the discharger 61 is preferably 600 rpm or more, more preferably 1000 rpm or more, and even more preferably 2000 rpm or more.
[0039] By rotating the discharge part 61, a workpiece whose surface is made of an insulating material, such as the laminate 100a, can be effectively machined. Specifically, the discharge part 61 performs cutting processing to cut the surface of the laminate 100a, and the carbon fibers 1 can be exposed from the surface made of resin 2. Since the carbon fibers 1 are conductive, once the carbon fibers 1 are exposed, electric discharge processing can be performed. Here, since the resin has a lower strength than the discharge part 61, there is no wear on the tool as occurs when the laminate is machined only by cutting processing. The surface of the laminate is formed of resin 2.
[0040] Furthermore, the rotation of the discharge unit 61 also serves to remove discharge debris generated by the discharge machining from the desired machining location. The function of removing discharge debris generated by the discharge machining from the desired machining location can be more effectively achieved by using a configuration in which the discharge unit oscillates in the in-plane direction of the laminate, or a configuration in which the discharge unit temporarily moves up and down (jumps) in the lamination direction of the laminate. Note that, since the discharge unit 61 and the laminate 100a are immersed in the machining fluid 70, it is possible to prevent the discharge debris from scattering.
[0041] Fig. 6 shows an example of the main configuration of the discharge circuit 62. For ease of explanation, Fig. 6 also shows the discharge unit 61 and a workpiece 64, which is a workpiece to be processed. In this embodiment, the workpiece 64 is a laminate.
[0042] The discharge circuit 62 has, for example, a power source E0, a capacitor C0, a transistor T0, and a charging resistor R0 connected in series to the power source E0, and a discharge unit 61 connected to the power source E0 and the capacitor C0. In addition to the main components shown in Fig. 6, the discharge circuit 62 may have various additional components within the scope of its gist. For example, a voltmeter that measures the potential of the discharge unit, an ammeter that measures the current flowing through the discharge unit 61, etc. may be added.
[0043] The method for machining a laminate according to this embodiment can prevent the occurrence of irregularities on the machined surface of the laminate due to long-pulse discharge and short circuiting by performing electric discharge machining using the discharge circuit 62. Below, the action of the discharge circuit 62 and the reason why the occurrence of irregularities on the machined surface due to long-pulse discharge and short circuiting can be prevented will be described using a comparative example.
[0044] <Comparative Example> Fig. 7 is a circuit diagram showing the main parts of a discharge circuit 62h according to a comparative example. For convenience of explanation, Fig. 7 shows a discharge unit 61h and a workpiece 64h together. In the machining method for a carbon fiber composite material (laminate) according to the comparative example, electric discharge machining is performed using the discharge circuit 62h. The machining method for a laminate using the discharge circuit 62h is not included in the present invention.
[0045] In the discharge circuit 62h, an internal resistor Rh, a transistor Th, and a discharge unit 61h are connected in series. A workpiece 64h is disposed so as to face the discharge unit 61h. In the method for machining a laminate according to the comparative example, the workpiece 64h is a laminate. The workpiece 64h and the discharge unit 61h are immersed in machining fluid.
[0046] In the electric discharge machining method according to the comparative example, with the transistor Th turned on, the discharge part 61h is gradually brought closer to the workpiece 64h by a vertical drive mechanism (not shown). When the distance between the discharge part 61h and the workpiece 64h becomes equal to or smaller than a predetermined value, a discharge occurs from the discharge part 61h. When a discharge occurs, the potential of the discharge part 61h drops. The discharge circuit 62h detects the occurrence of a discharge when the potential of the discharge part 61h falls below a discharge detection voltage. The discharge detection voltage is set to a predetermined value. The discharge circuit 62h is an isopulse type discharge device that is set to maintain the potential of the discharge part 61h for a set discharge time when it detects the occurrence of a discharge, and turn off the transistor after the set discharge time has elapsed.
[0047] However, the discharge circuit 62h may set the discharge detection voltage based on the potential when a metal material is used as the workpiece 64h. When the laminate 100 is used as the workpiece 64h, the potential of the discharge section 61h does not drop as much as when a metal material is used as the workpiece 64h. This phenomenon is caused by the laminate 100 being a resistor. This comparative example describes a case where a metal material is used as the workpiece 64h. The discharge circuit 62h can detect discharge when a metal material is used as the workpiece 64h, but cannot correctly detect discharge when a laminate is used as the workpiece 64h.
[0048] Since the discharge circuit 62h cannot detect the discharge of the discharge unit 61h, the discharge unit 61h continues to approach the workpiece 64h while discharging. At this time, a high potential is applied to the discharge unit 62 by the power source Eh. While the discharge unit 61h continues to approach the workpiece 64h, the potential of the discharge unit 61h continues to decrease and falls below the discharge detection voltage later than the original time. When it falls below the discharge detection voltage, the potential of the discharge unit 61h is maintained for the discharge setting time, and after the set discharge time has elapsed, the transistor is turned off. In reality, the discharge unit 61h is generating a discharge for a time significantly longer than the set discharge time. In other words, a long pulse discharge is generated in the discharge circuit 62h.
[0049] When a long-pulse discharge occurs, the resin, which has a lower heat resistance than the carbon fiber, disappears, and the carbon fiber becomes fluffy. Then, the fluffy carbon fiber falls off, causing a short circuit between the carbon fiber and the discharge section 61h, and the resin, which is the matrix material, disappears selectively due to Joule heat caused by the short circuit. The amount of resin that disappears is dominated by the amount in the orientation direction of the carbon fiber. Therefore, in the processing method of the laminate according to the comparative example, a long-pulse discharge and a short circuit occur, and the disappearance of the resin and the fluffing of the carbon fiber cause unevenness in the processed surface.
[0050] In contrast, the method for machining a laminate according to the first embodiment uses an electric discharge device 60. The electric discharge device 60 includes a discharge circuit 62, which makes it possible to suppress long pulse discharge and to suppress the occurrence of unevenness on the machined surface.
[0051] The operation of performing electric discharge machining using the electric discharge device 60 will be described in detail below. Fig. 8 is a diagram showing the voltage and current when performing electric discharge machining. Fig. 8(a) is a diagram showing the voltage when performing electric discharge machining. Fig. 8(b) is a diagram showing the current when performing electric discharge machining.
[0052] In the method for machining a laminate according to the first embodiment, in the discharge circuit 62, first, the transistor T0 is turned on and a current is passed from the power source E0 to charge the capacitor C0. At the same time as the charging of the capacitor C0 or after the charging of the capacitor C0, the discharge unit 61 is moved closer to the workpiece 64 while comparing the potential difference between the discharge unit 61 and the workpiece 64 with the servo reference voltage. Specifically, when the potential difference between the discharge unit 61 and the workpiece 64 is equal to or greater than the servo reference voltage, the discharge unit 61 is moved closer to the workpiece 64, and when the potential difference between the discharge unit 61 and the workpiece 64 is equal to or less than the servo reference voltage, the discharge unit 61 is moved away from the workpiece 64 (servo back), thus controlling the distance between the poles (servo control). When the distance between the discharge unit 61 and the workpiece 64 becomes equal to or less than a predetermined value, a discharge occurs from the discharge unit 61 to the workpiece 64. In the discharge in the discharge circuit 62, the charge stored in the capacitor C0 flows all at once, and the potential of the discharge unit 61 reaches a discharge detection voltage V at time t1. KThen, the transistor T0 is turned off. When the discharge circuit 62 detects a discharge, it maintains the potential of the discharge unit 61 for a set discharge time and causes a current to flow from the discharge unit 61. Next, the transistor T0 is turned on to charge the capacitor C0, and the same cycle is repeated.
[0053] The capacitance that can be stored in the capacitor is fixed, and no long pulse discharge occurs.
[0054] During discharge, the current flowing to the discharge unit 61 is from the capacitor C0 and does not pass through the charging resistor R0. Therefore, the resistance value of the charging resistor R0 can be made larger than the resistance value of the internal resistance Rh. Therefore, even if a short circuit occurs when the discharge unit 61 is moved away from the workpiece 64, a large current is prevented from flowing, and the effects of such a short circuit can be reduced. In addition, burning of the resin and fluffing of the carbon fibers can be prevented, and unevenness of the machined surface can be reduced.
[0055] In addition, in the method for processing a laminate according to the present embodiment, a part of the circuit can be completely isolated by turning off the transistor T0 while a current is flowing from the capacitor C0, so that the next discharge can be performed stably.
[0056] In addition, in the laminate according to this embodiment, since short circuits can be suppressed, servo back can be suppressed and hollowing out processing is also possible. The processing method for the laminate according to this embodiment can be applied to both thermosetting carbon fiber composite materials and thermoplastic carbon fiber composite materials. In the laminate machining method according to the present embodiment, a discharge circuit in which the transistor T0 is removed from the discharge circuit 62 may be used. An example of such a discharge circuit is the discharge circuit 62' shown in FIG. 16. When the discharge circuit 62' is used, the capacitor C0 is charged, and the discharge unit 61 is moved closer to the workpiece 64 when the potential difference between the discharge unit 61 and the workpiece 64 is equal to or less than the servo reference voltage, and moved away from the workpiece 64 when the potential difference is equal to or greater than the servo reference voltage. When the distance between the discharge unit 61 and the workpiece 64 becomes equal to or less than a predetermined value, a discharge occurs from the discharge unit 61 to the workpiece 64. When a discharge occurs in the discharge circuit 62', the charge stored in the capacitor C0 is released to the workpiece 64 all at once. At this time, a current also flows from the power source E0. A short circuit may occur due to contact between the discharge unit 61 and the workpiece 64. However, even in the discharge circuit 62', the resistance value of the charging resistor R0 can be set to a value larger than the resistance value of the internal resistor Rh. In other words, the current flowing in due to a short circuit is very small, and the resin does not disappear. Therefore, even when the discharge circuit 62' is used, it is possible to suppress the occurrence of unevenness on the machined surface.
[0057] <Carbon fiber composite materials> FIG. 9 is an electron microscope image of a carbon fiber composite material (laminate) before processing by the laminate processing method according to the first embodiment. FIG. 9 is an X-ray CT image provided by the Foundation for Materials Science and Technology, which was posted on their website. In the laminate, the cross-sectional shape of the carbon fibers 1 is all circular, and the diameter of the carbon fibers is greater than the center-to-center distance between adjacent carbon fibers. On the side surface of the laminate, the occupancy rate (area occupancy rate) of the area occupied by the carbon fibers 1 is approximately uniform in every portion. The area occupancy rate (area ratio) of the carbon fibers 1 is approximately 60 to 70%, and the ratio of the area occupancy rate of the resin 2 is approximately 30 to 40%.
[0058] FIG. 10 is a perspective view that shows a schematic example of the configuration of a carbon fiber composite material 100d after processing. The carbon fiber composite material 100d includes a plurality of carbon fibers 1 and a resin 2 that bonds the plurality of carbon fibers. Electric discharge machining is performed so as to penetrate from a part of the front surface S of the carbon fiber composite material 100d toward the back surface. The parts indicated by the symbols S1 and S2 are the machined parts, and are referred to as the machined surfaces S1 and S2, respectively. The penetration direction is preferably perpendicular to the front surface S, but does not have to be perpendicular. By the electric discharge machining, holes with a small pore size shown by the broken line are formed. The machined region is, for example, a region surrounded by the machined surfaces. FIG. 11 is an electron microscope image of the machined surface S2 (the inner wall surface of the through hole) of the carbon fiber composite material 100d. Note that FIG. 11 is an electron microscope image of the machined surface of the carbon fiber composite material observed in Example 1 described later. The machined surface S2 here is a surface that is perpendicular to the first direction and perpendicular to the surface S. 11, in the carbon fiber composite material 100d, the diameter of the carbon fibers 1 is locally expanded at the end surface by electrical discharge machining. Furthermore, due to the radial expansion, adjacent carbon fibers press against each other, and the shape of the carbon fibers 1 locally changes from a circle to a polygon.
[0059] The carbon fiber composite material 100d after the electric discharge machining has a dense region where the carbon fibers are densely packed on at least a part of the side surface. The side surface here means a surface perpendicular to the front surface S, and includes the processed surface S. In the dense region, the area occupancy rate of the carbon fibers is, for example, 70% or more, preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. In the region shown in FIG. 11, the area occupancy rate of the carbon fibers is 94%. When the processing method for the laminate according to the first embodiment is performed on a laminate in which prepregs having various carbon fiber orientation methods are laminated, a dense region is generated on all processed surfaces.
[0060] Theoretically, when the carbon fibers are arranged in a square periodic close-packed charged arrangement, the area occupancy of the carbon fibers in the carbon fiber composite material is maximized, and the area occupancy of the carbon fibers in the carbon fiber composite material is 91%.
[0061] In addition, the distance L between the centers A and B of the adjacent carbon fibers 1A and 1B AB is the maximum diameter L of carbon fiber 1A A , the maximum diameter L of carbon fiber 1B B 11. Note that the carbon fibers shown in Fig. 11 are all end faces of the carbon fibers, and are exposed. Here, the end face of the carbon fiber refers to the end of the carbon fiber.
[0062] In the processing method of the laminate according to the present embodiment, it is considered that the carbon fibers take in a growth source (carbon source) and grow. The growth source is considered to be mainly decomposed carbon of the electric discharge processing oil. Another possible cause is the expansion of the carbon fibers 1 due to a change in the crystal structure. Other possible growth sources are lost carbon fibers and resin. The processing method of the laminate according to the present embodiment is not limited to a method of processing the laminate so that a through hole is formed in the laminate, and the laminate may be processed so that a groove is formed in the laminate.
[0063] The carbon fiber composite material according to this embodiment has an increased area occupancy rate of carbon fibers on the side surface, and therefore has improved hardness compared to the carbon fiber composite material (laminate) before electrical discharge machining. That is, the strength of the carbon fiber composite material is improved. Also, compared to the side surface of the laminate before electrical discharge machining, fuzzing and loss of resin are suppressed, and the machined surface after electrical discharge machining has a smooth shape. That is, it can also be used as a sliding surface.
[0064] <Variation 1> The method for machining a carbon fiber composite material (laminate) according to the first modification uses a discharge circuit 62A instead of the discharge circuit 62 of the machining device 200. FIG. 12 is a circuit diagram showing a main part of the discharge circuit 62A. The discharge circuit 62A includes a power source EA, a voltage control unit U connected to the power source EA, and a discharge unit 61. The method for machining a laminate according to the first modification can achieve the same effects as the method for machining a laminate according to the first embodiment. Configurations similar to those of the discharge circuit 62 are given the same reference numerals and descriptions thereof will be omitted.
[0065] The voltage control unit U has a first unit U1 and a second unit U2. The first unit U1 and the second unit U2 are arranged in parallel. The first unit U1 and the second unit U2 each include a transistor and a resistor. The transistor and the resistor included in the first unit U1 are referred to as a first transistor T1 and a first resistor R1, respectively. The transistor and the resistor included in the second unit U2 are referred to as a second transistor T2 and a second resistor R2, respectively. In this specification, turning on the first transistor T1 and the second transistor T2 may be expressed as turning on the first unit U1, turning on the second unit U2, etc.
[0066] The operation of the method for machining a laminate according to the first modified example will be described. Fig. 13 is a diagram showing the voltage and current when performing electric discharge machining. Fig. 13(a) is a diagram showing the voltage when performing electric discharge machining. Fig. 13(b) is a diagram showing the current when performing electric discharge machining.
[0067] The method for processing a laminate according to the first modification includes a first step, a second step, and a third step.
[0068] In the first step, the first unit U1 is turned on and the second unit U2 is turned off, i.e., a current flows from the power source EA and the capacitor CA is charged.
[0069] Charging of the capacitor CA starts at time t0, and the voltage between the electrodes of the capacitor CA rises to a voltage V T If it exceeds this, proceed to the second step. T is the voltage used to detect the charging of the capacitor CA, and is set to a value smaller than the voltage of the power supply EA. T A small value of increases the charging speed of the capacitor CA, but the rise voltage V T If the value of is too small, a large current may flow through the workpiece 64 in the event of a short circuit. Tis preferably set to between 1 / 4 and 3 / 4 times, or between 1 / 3 and 2 / 3 times, the voltage of the power supply EA, and may be 15V or higher.
[0070] In the second step, the second unit U2 is turned on. When the second step is performed, both the first unit U1 and the second unit U2 are turned on. That is, the combined resistance of the discharge circuit 62A is reduced, so that a large current flows and the charging speed of the capacitor CA is improved.
[0071] Furthermore, a third step is performed. In the third step, the discharge unit 61 is brought closer to the workpiece 64 while comparing the potential difference between the discharge unit 61 and the workpiece 64 with the servo reference voltage. Specifically, when the potential difference between the discharge unit 61 and the workpiece 64 is equal to or greater than the servo reference voltage, the discharge unit 61 is brought closer to the workpiece 64, and when the potential difference between the discharge unit 61 and the workpiece 64 is equal to or less than the servo reference voltage, the discharge unit 61 is moved away from the workpiece 64, thereby controlling the distance between the poles. When the distance between the discharge unit 61 and the workpiece 64 falls below a predetermined distance, a discharge is generated from the discharge unit 61. That is, a voltage drop occurs between the poles of the capacitor CA at time tb. When the potential of the discharge unit 61 reaches a discharge detection voltage V K When the potential of the discharge unit 61 falls below tc, the voltage control unit U is turned off and the potential of the discharge unit 61 is kept constant for the set discharge time. That is, a current flows until time tc. Next, at time tc, the first unit U1 is turned on while the discharge unit 61 is moved away from the workpiece, thereby charging the capacitor CA again. The set discharge time is, for example, 1 μs or more and 500 μs or less, and preferably 100 μs or less. The third step may be performed simultaneously with the first and second steps, or may be performed after the first and second steps have been performed.
[0072] The laminate processing method according to the first modification can achieve the same effect as the laminate processing method according to the first embodiment. In addition, the laminate processing method according to the first modification can appropriately change the combined resistance by providing a voltage control unit U. It is preferable that the combined resistance of the discharge circuit 62A is small from the viewpoint of fast charging of the capacitor CA. On the other hand, if the combined resistance is small, a large current may be generated if the discharge unit 61 comes into contact with the carbon fiber when moving the discharge unit 61 away from the workpiece. This may cause a short circuit. The laminate processing method according to the first modification can achieve both suppression of short circuits and fast charging by providing a voltage control unit U.
[0073] <Variation 2> The method for processing a carbon fiber composite material (laminate) according to Modification 2 uses a discharge circuit 62B instead of the discharge circuit 62 of the processing device 200. Fig. 14 is a circuit diagram showing a main part of the discharge circuit 62B used in the method for processing a laminate according to Modification 2. The discharge circuit 62B includes a power source E, and a voltage control unit U' and a discharge unit connected in series to the power source E.
[0074] The operation of the method for machining a laminate according to the modified example 2 will be described. Fig. 15 is a diagram showing the voltage and current when performing electric discharge machining. Fig. 15(a) is a diagram showing the voltage when performing electric discharge machining. Fig. 15(b) is a diagram showing the current when performing electric discharge machining.
[0075] The method for processing a laminate according to the modified example includes a first step, a second step, a third step, a fourth step, and a fifth step.
[0076] In the first step, the first unit U1 is turned on and the second unit U2 is turned off. That is, a current flows from the power source E and the discharge section 61 is charged. At this time, no current flows through the second unit U2.
[0077] The potential of the discharge part 61 is the current superimposed voltage V DIf it exceeds this, the second step is performed. In the second step, the second unit U2 is turned on. That is, the combined resistance of the discharge circuit 62B is reduced. That is, the speed at which the potential of the discharge unit 61 is increased can be improved.
[0078] In addition, the third step is performed. The third step may be performed simultaneously with the first step or the second step, or after the first step and the second step. In the third step, the discharge unit 61 is moved closer to the workpiece 64 while comparing the potential difference between the discharge unit 61 and the workpiece 64 with the servo reference voltage. Specifically, when the potential difference between the discharge unit 61 and the workpiece 64 is equal to or greater than the servo reference voltage, the discharge unit 61 is moved closer to the workpiece 64, and when the potential difference between the discharge unit 61 and the workpiece 64 is equal to or less than the servo reference voltage, the discharge unit 61 is moved away from the workpiece 64, thereby controlling the distance between the poles. When the distance between the discharge unit 61 and the workpiece becomes equal to or less than a predetermined distance, a discharge is generated from the discharge unit 61. The time when the discharge occurs is set to time tB. That is, a voltage drop occurs. At the same time as the voltage drop occurs, the current waveform rises, and a pulse discharge occurs. The pulse discharge ends after the set discharge time has elapsed, and the current waveform falls. The set discharge time is, for example, 1 μs or more and 500 μs or less, and is preferably 100 μs or less. K When it falls below this level, carry out the fourth step.
[0079] In the fourth step, the second unit U2 is turned off. By turning off the second unit U2, the combined resistance of the discharge circuit 62B increases.
[0080] When the potential difference between the discharge part 61 and the workpiece 64 is equal to or lower than the servo reference voltage, the discharge part 61 is moved away from the workpiece 64. At this time, if the discharge part 61 comes into contact with the carbon fiber, a short circuit may occur. However, at this time, the combined resistance of the discharge circuit 62B is set to a high value, and the short circuit current is suppressed.
[0081] The discharge circuit according to the second modification uses transistors, but the method for machining a laminate according to the second modification can provide the same effects as the method for machining a laminate according to the first embodiment. Moreover, the method for machining a laminate according to the second modification can appropriately change the combined resistance by the voltage control unit U. In other words, it is possible to further enhance the suppression of short circuits. Moreover, since charging is not required as in the case of a capacitor-type discharge circuit, it is possible to improve the throughput when performing electric discharge machining. EXAMPLES
[0082] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0083] <Example 1> The processing apparatus 200 shown in Fig. 5 was reproduced, and an opening was formed in a direction perpendicular to the in-plane direction of the carbon fiber composite material. In Example 1, a discharge circuit 62' whose main part is shown in Fig. 16 was used as the discharge circuit. The discharge circuit 62' is a discharge circuit obtained by removing the transistor T0 from the discharge circuit 62. Specific conditions and results of Example 1 will be described in detail below.
[0084] (Carbon fiber composite materials) A carbon fiber composite material (laminate) was prepared by laminating commercially available prepregs (product number: Besfight(R) W-3101-A / Q112J, manufacturer: Toho Tenax Co., Ltd.) by GH Craft Co., Ltd. This laminate is composed of eight layers of prepregs. When the laminate used in Example 1 was installed in the processing device 200, the prepregs were arranged in the order of the first layer, the second layer, the third layer, the fourth layer, the fifth layer, the sixth layer, the seventh layer, and the eighth layer from the prepreg closest to the discharge section 61. The first layer was oriented in the first direction. The orientation directions of the second layer, the third layer, the fourth layer, the fifth layer, the sixth layer, the seventh layer, and the eighth layer were rotated clockwise by 45°, 90°, -45°, -45°, 90°, 45°, and 0°, respectively, with respect to the orientation direction of the first layer. This laminate was used in Example 1.
[0085] The fiber weight of this laminate is 197 g / m 2The resin content of this laminate is 40% and the carbon fiber content is 60%.
[0086] (Processing equipment) A cylindrical copper electrode was used as the discharge part 61. The diameter of the discharge part was 3 [mm]. The discharge part 61 was negatively charged and discharge machining was performed while rotating at 2000 [rpm]. A commercially available discharge machining oil (product number: Metalwork EDFK-2, manufacturer: JXTG Energy Corporation) was used as the machining fluid 70. A precision vice 40 (product number: DS20-2, manufacturer: Japan Automatic Machine Co., Ltd.) was used as the precision vice 40. In Example 1, the laminate was positively charged using the precision vice 40. The precision vice 40 clamped the end 3a and side of both sides of the laminate via a copper film. The ends 3a, 3b, 3c, and 3d of the laminate and the entire side were covered with a copper film. The copper film had a thickness of 0.1 mm.
[0087] (discharge circuit) The no-load voltage of the discharge unit 61 was 100 [V], and the servo reference voltage was 60 [V]. The charging resistance of the capacitor C0 was 2 [kΩ]. The capacitance of the capacitor C0 was 2 [μF].
[0088] In the first embodiment, the steps of turning on transistor T0 to charge capacitor C0, bringing discharge unit 61 closer to the stack, turning off transistor T0 when discharge from discharge unit 61 is detected, and moving discharge unit 61 away from the stack are repeated.
[0089] The conditions for Example 1 described above are summarized in Table 1.
[0090] [Table 1]
[0091] (Surface observation test) In Example 1, through holes were formed in the laminate in 1 hour and 28 minutes. A surface observation test was performed on the carbon fiber composite material that had been subjected to electrical discharge machining. In the surface observation test, the front and back surfaces of the carbon fiber composite material were observed with an optical microscope. FIG. 17 is an optical microscope image of the carbon fiber composite material processed in Example 1. FIG. 17(a) is the surface (front surface) close to the discharge part 61, and FIG. 17(b) is the surface (back surface) far from the discharge part 61. FIG. 17(a) and FIG. 17(b) are optical microscope images at the same position. It is confirmed that through holes are formed in the carbon fiber composite material by electrical discharge machining according to Example 1. In addition, blackening, which is a characteristic of the case where the resin is selectively and vigorously lost in the orientation direction of the carbon fibers, is not confirmed around the through holes.
[0092] Fig. 18 is a diagram showing the voltage and current of the discharge unit 61 when electric discharge machining is performed. Fig. 18(a) is a diagram showing the voltage when electric discharge machining is performed, and Fig. 18(b) is a diagram showing the current when electric discharge machining is performed. It can be seen from Fig. 18 that a short-pulse discharge current is generated at the same time as the discharge occurs, and that no long-pulse discharge or short circuit occurs.
[0093] (Processed surface observation test) Next, a processed surface observation test was performed on the processed surface. The processed surface is the surface on which the carbon fiber composite material is processed, and is perpendicular to the lamination direction. In the processed surface observation test, the processed surface of the carbon fiber composite material was observed using an electron microscope and an optical microscope. Figure 19(a) is an electron microscope image of the processed surface. Note that Figure 19(a) is the result of observing a cross section perpendicular to the orientation direction of the third layer with an electron microscope. Figure 19(b) and Figure 11 are enlarged views of regions R1 and R2 in Figure 19(a), respectively. Region R1 is located in the first and second layers, and includes the boundary between the first and second layers. Region R2 is located in the third layer.
[0094] The electron microscope image in Figure 19 is perpendicular to the orientation direction of the first and eighth layers, and by observing these layers, it is possible to confirm that the carbon fibers are oriented. It is confirmed that the diameter of the carbon fibers in the second to seventh layers has been enlarged by the electric discharge processing. Specifically, since each carbon fiber before the electric discharge processing is circular, the center-to-center distance between adjacent carbon fibers was greater than the diameter of the carbon fiber before the electric discharge processing. However, as can be seen in Figure 11, in at least some of the carbon fibers, the center-to-center distance L AB Rather than L A and L B The maximum diameter of each carbon fiber is longer in the carbon fiber composite material R1 and R2. In other words, the carbon fibers grow so that their diameters expand due to the electric discharge machining. Furthermore, the carbon fiber composite material after the electric discharge machining has dense regions where the carbon fibers are denser than before the electric discharge machining. In the dense regions, the area occupancy rate of the carbon fibers increases. Specifically, the area occupancy rate of the carbon fibers was 60% before the electric discharge machining, but in region R2, the area occupancy rate of the carbon fibers was 94%. This area occupancy rate was found by binarizing FIG. 11 and calculating the ratio of the occupied areas.
[0095] Fig. 20 is an optical microscope image of the machined surface. From the optical microscope image shown in Fig. 20, it can be seen that the diameter of the carbon fibers in the carbon fiber composite material after electric discharge machining is enlarged over the entire machined surface.
[0096] <Reference example 1> Next, the processing method was changed from that of Example 1, and Reference Example 1 was performed. Specifically, in Reference Example 1, the discharge circuit was changed from that of Example 1. The conditions other than the change in the discharge circuit were the same as those of Example 1.
[0097] (Processing equipment) The machining device used in the reference example 1 is similar to that in the embodiment 1, except that the discharge circuit is changed to a discharge circuit 62h.
[0098] In the first reference example, the steps of bringing the discharger 61h closer to the workpiece 64h, and continuing the discharge for a set discharge time when the potential of the discharger 61h falls below the discharge detection voltage, and pausing the discharger 61h for a rest time while moving the discharger 61h away from the workpiece 64h are repeated. The set discharge time was 4 [μs], the rest time was 36 [μs], and the internal resistance Rh of the transistor Th was 10 [Ω].
[0099] The conditions for the above-mentioned Reference Example 1 are summarized in Table 2.
[0100] [Table 2]
[0101] (Surface observation test) In Reference Example 1, a through hole was formed in 1 hour and 18 minutes. A surface observation test was performed on the carbon fiber composite material that had been subjected to electrical discharge machining in the same manner as in Example 1. FIG. 21 is an optical microscope image of the carbon fiber composite material processed in Reference Example 1. FIG. 21(a) is the surface (front surface) that was close to the discharge part, and FIG. 21(b) is the surface (rear surface) that was far from the discharge part. FIG. 21(a) and FIG. 21(b) are optical microscope images at the same position. It is confirmed that a through hole was formed in the carbon fiber composite material by electrical discharge machining according to Reference Example 1. A darkened area RK is generated around the through hole. It is presumed that the color of the carbon fiber stands out in the area RK because the resin has disappeared and the carbon fiber is exposed.
[0102] FIG. 22 is a diagram showing the voltage and current of the discharge part when electric discharge machining is performed. FIG. 22(a) is a diagram showing the voltage when electric discharge machining is performed, and FIG. 22(b) is a diagram showing the current when electric discharge machining is performed. From FIG. 22, it is confirmed that long pulse discharge and short circuit occur in Reference Example 1. Specifically, it is confirmed that current occurs continuously for a long time, for example, from 1500 [μs] to 2500 [μs]. It can be seen that the pulse width is long during this time, while the set discharge time is set to 4 [μs], and long pulse discharge occurs. In addition, during the time of 2500 [μs] to 3500 [μs] and 4500 [μs] to 5000 [μs], current flows before the voltage of the discharge part has risen, and the occurrence of short circuit is confirmed. Short circuit and long pulse discharge are prominent in the latter half of electric discharge machining. Carbon fiber composite material is a resistor, and the potential when discharge occurs is unlikely to decrease. Therefore, even if a discharge occurs, the voltage does not fall below the discharge detection voltage, resulting in a long pulse discharge, which causes the carbon fibers to fluff. If the fluffed carbon fibers fall off, a short circuit occurs, and the loss of resin progresses.
[0103] The depth of the hole increases over time. In other words, the discharge part must also penetrate deep into the carbon fiber composite material, which causes the discharge part to fluff and easily short-circuit with the fallen carbon fibers. In other words, when machining the side surface of a carbon fiber composite material with high precision by electric discharge machining, it is preferable to perform the machining in such a way that long pulse discharge does not occur.
[0104] When the cross section of the carbon fiber composite material processed by the electric discharge machining method of Reference Example 1 was observed, it was confirmed that the resin had disappeared and the carbon fibers had been exposed. Therefore, the carbon fiber composite material processed by the method of Example 1 is harder and smoother than the carbon fiber composite material processed by the method of Reference Example 1.
[0105] <Example 2> In Example 2, discharge machining was performed using a cylindrical discharge part and a capacitor-controlled discharge circuit to hollow out a carbon fiber composite material (laminate).
[0106] (Carbon fiber composite materials) A carbon fiber composite material (laminate) was prepared by laminating commercially available prepregs (product number: W-3101-A / Q112J, manufacturer: Toho Tenax Co., Ltd.) by GH Craft Co., Ltd. This carbon fiber composite material is made of eight layers of prepregs. The laminate is made up of eight layers of prepregs with orientation directions of 0°, 45°, 90°, and -45°, in that order, with the orientation direction of the outermost layer being 0°.
[0107] (Processing equipment) A cylindrical copper electrode was used as the discharge part 61. The diameter of the discharge part was 3 mm, and the thickness was 0.3 mm. The discharge part 61 was negatively charged and rotated at 2000 rpm to perform electric discharge machining. A commercially available electric discharge machining oil (product number: Metal Work EDFK-2, manufacturer: JXTG Energy Corporation) was used as the machining fluid 70. A precision vice 40 (product number: DS20-2, manufacturer: Japan Automatic Machine Co., Ltd.) was used. The electric discharge machining was performed by positively charging the laminate using the precision vice 40. The precision vice 40 clamped the ends 3a, 3b, 3c, and 3d on both sides of the laminate via a copper film. The ends 3a, 3b, 3c, and 3d of the laminate and the entire side surface were covered with a copper film. The thickness of the copper film was 0.1 mm.
[0108] (discharge circuit) The no-load voltage of the discharge unit 61 was 250 [V], and the servo reference voltage was 60 [V]. The charging resistance R0 of the capacitor C0 was 2 [kΩ]. The capacitance of the capacitor C0 was 2 [μF].
[0109] In Example 1, the steps of turning on a transistor to charge a capacitor, bringing a discharge section closer to the stack, turning off the transistor when discharge from the discharge section is detected, and moving the discharge section away from the stack are repeated.
[0110] The conditions for Example 2 described above are summarized in Table 3.
[0111] [Table 3]
[0112] Fig. 23 shows the carbon fiber composite material that has been subjected to electrical discharge machining and the hollowed-out carbon fiber composite material. As shown in Fig. 23, in Example 2, it is possible to hollow out the carbon fiber composite material. In Example 2, two through holes were formed. The closest distance between the two through holes was 0.4 mm. [Industrial Applicability]
[0113] INDUSTRIAL APPLICABILITY The present invention makes it possible to realize a high-strength carbon fiber composite material, which can make mobile vehicles such as aircraft and automobiles lighter and stronger. [Explanation of symbols]
[0114] 1, 1A: carbon fiber, 2: resin, 3: end, 10, 11, 20, 21: prepreg, 30: container, 40: precision vice, 41: main body, 42: clamping part, 50: conductive auxiliary member, 60: discharge device, 61, 61h: discharge unit, 62, 62A, 62B: discharge circuit, 63: motor, 64: workpiece, 70: Processing fluid, 100a, 100b, 100c: Carbon fiber composite material (laminate), 100d: Carbon fiber composite material, 200: Processing device
Claims
1. A carbon fiber composite material comprising a plurality of prepregs each including a plurality of carbon fibers and a resin for bonding the plurality of carbon fibers, At least some of the carbon fibers extend in the same direction; A carbon fiber composite material having a dense region in which a plurality of the carbon fibers are densely packed together, At least a part of the surface has an exposed end face of the carbon fiber, the maximum diameter of the end face is greater than the center-to-center distance of the end faces of adjacent carbon fibers, A carbon fiber composite material, wherein the shape of the carbon fiber at the end surface is polygonal.
2. 2. The carbon fiber composite material according to claim 1, wherein the carbon fibers occupy 70% or more of an area of at least a portion of a surface.
3. A method for producing the carbon fiber composite material according to claim 1 or 2, comprising processing a laminate in which a plurality of prepregs each formed by impregnating carbon fibers with a resin are stacked in a thickness direction, the method comprising the steps of: A method for processing a laminate, comprising a heating step of heating the laminate in a processing region of each layer overlapping in a stacking direction for a time of 500 μs or less.
4. The heating step is a discharge step for performing electric discharge machining on the laminate, 4. The method for machining a laminate according to claim 3, wherein the discharge step comprises generating an electric discharge using a discharge unit that is immersed in the machining fluid and connected to a discharge circuit, and thermally machining the machining region.
5. The discharge circuit includes a power supply, a capacitor and a resistor connected in series to the power supply, The method for processing a laminate according to claim 4 , further comprising: a discharge section connected in parallel to the power source and the capacitor.
6. The method for processing a laminate according to claim 5 , wherein the discharge circuit further comprises a transistor connected in series with the power supply, the capacitor, and the resistor.
7. The discharge circuit includes a power supply, a capacitor and a voltage control unit connected in series to the power supply, a discharge unit connected in parallel to the power supply and the capacitor, the voltage control section includes a first unit and a second unit in which a transistor and a resistor are connected in series; a first step of turning on the first unit and turning off the second unit; a second step of turning on a second unit after the inter-electrode voltage of the capacitor exceeds a start-up voltage; The method for processing a laminate described in claim 4, further comprising three steps: moving the discharge part closer to the laminate when the potential difference between the discharge part and the laminate is equal to or greater than a servo reference voltage; and moving the discharge part away from the laminate when the potential difference between the discharge part and the laminate is equal to or less than the servo reference voltage.
8. the discharge circuit includes a power supply, and a voltage control unit and a discharge unit connected in series to the power supply; the voltage control section includes a first unit and a second unit in which a transistor and a resistor are connected in series; The discharge unit includes two opposing electrodes, the discharging step comprises: a first step of turning on the first unit and turning off the second unit; a second step of turning on the second unit when the potential of the discharge portion exceeds a current superimposition voltage; a third step of moving the discharge unit closer to the stack when a potential difference between the discharge unit and the stack is equal to or greater than a servo reference voltage, and moving the discharge unit away from the stack when a potential difference between the discharge unit and the stack is equal to or less than the servo reference voltage; a fourth step of turning off the second unit when a set discharge time has elapsed since the potential of the discharge unit falls below a discharge detection voltage; The method for processing a laminate according to claim 4, further comprising a fifth step of moving the discharge part away from the laminate.
9. A method for forming pores in the laminate, comprising the steps of: The method for processing a laminate according to any one of claims 3 to 7, wherein the pores have a diameter of 10 µm or more.
Citation Information
Patent Citations
JP1975008197A
Discharge machining device
JP1977122994A
Electric discharge machining device
JP1983211826A
Electric discharge machining power supply
JP1985255314A
Electrical discharge machining method
JP1986121825A