Manufacturing method and use of tea-based composite board

A tea-based composite board made from agricultural and food waste addresses environmental issues by creating a high-strength, biodegradable material suitable for furniture and building materials, providing a sustainable alternative to traditional wood.

JP7594311B2Active Publication Date: 2024-12-04ZENCE OBJECT HOLDING (HONG KONG) LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023071170
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-07-14
Filing Date
2023-04-24
Publication Date
2024-12-04
Estimated Expiration
2043-04-24

AI Technical Summary

Technical Problem

The accumulation and disposal of tea dregs and coffee grounds as waste leads to environmental pollution and greenhouse gas emissions, with limited effective reuse, while the demand for high-grade building materials continues to grow.

Method used

A manufacturing method for a tea-based composite board material using a blend of tea fibers, coffee grounds, and other agricultural and food waste, combined with additives, to create a biodegradable and high-strength material suitable for building applications.

Benefits of technology

The method produces a composite board with high mechanical strength, bacteriostatic properties, and fragrance release, offering a sustainable alternative to traditional wood materials with diverse applications in furniture and building products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a manufacturing method and a usage of a composite board with tea as a base material.SOLUTION: A manufacturing method of a composite board with tea as a base material comprises: Step 1 of arranging a composition of raw material consisting of 60-70 parts of discarded tea grounds, 20-50 parts of tea stalks, 12-30 parts of grain culm flour, 10-30 parts of tea pectin fiber element, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of coloring agent, 0.1-3 parts of antioxidant, 0.1-3 parts of stabilizer; Step 2 of soaking the tea stalks in hot water at 60-80°C, then washing, drying, and crushing to obtain tea powder; Step 3 of mixing the discarded tea grounds, tea powder, grain culm flour, tea pectin fiber element, coffee grounds, compatibilizer, and lubricant at 120-150°C for 20-30 min; and Step 4 of cooling the mixture to 50-60°C, and then adding colorant, antioxidant, and stabilizers, mixing uniformly, and forming under hydraulic pressure at 50-118°C to obtain composite board material with tea as a base material. The composite board material can be used as an alternative to the high-grade wood which is currently available on the market and can be also used for furniture products.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of building board technology, in particular to the manufacturing method and use of tea-based composite boards. [Background technology]

[0002] China is a major tea producing country, and ranks first in the world in total tea production, cultivation area and total production value. With the rapid growth of the new tea beverage industry, the amount of tea waste generated annually reaches tens of millions of tons. According to statistics, in the tea production and processing process, tea stick waste accounts for more than 20% of the total weight of tea leaves every year. As a production waste, tea leaves are piled up and rotted or incinerated, which not only causes waste, but also causes environmental pollution and greenhouse gas emissions. At present, tea leaves are mostly reused as fertilizer and feed, and the sales volume of tea beverages is increasing day by day, and the amount of tea leaves is also increasing accordingly. In addition, as the demand for coffee by the people gradually increases, the amount of coffee residue generated cannot be ignored, so the development and reuse of discarded tea sticks, defective tea leaves, coffee residue and other agricultural waste and food waste has become a problem that needs to be solved quickly. Summary of the Invention [Problem to be solved by the invention]

[0003] In response to the problems of the prior art, the present invention provides a manufacturing method and use of a tea-based composite board material, the tea-based composite material being a composite of tea leaf fiber, tea residue, coffee grounds and other agricultural waste and food waste, and having the advantages of being biodegradable, having high mechanical strength and excellent adsorption. [Means for solving the problem]

[0004] The technical solutions of the present invention are as follows: In a first aspect, the present invention provides a method for producing a tea based composite board, comprising:

[0005] Step 1: Blending raw materials based on a weight composition, the raw material composition is 60-70 parts of discarded tea leaves, 20-50 parts of tea sticks, 12-30 parts of cereal straw powder, 10-30 parts of tea pectin cellulose, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of colorant, 0.1-3 parts of antioxidant, and 0.1-3 parts of stabilizer; Step 2: soaking the tea leaves in hot water at 60-80°C, washing, drying and crushing to 10-20 mesh to obtain tea powder; Step 3: mixing the discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, compatibilizer, and lubricant at 120-150°C for 20-30 minutes;

[0006] and step 4 of cooling to 50-60°C, adding and uniformly mixing colorants, antioxidants, and stabilizers, and hydroforming at 50-118°C to obtain a tea-based composite board.

[0007] Furthermore, the raw material composition is replaced as follows: 40-50 parts of discarded tea leaves, 20-50 parts of tea sticks, 12-30 parts of stalk powder, 10-30 parts of tea pectin cellulose, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of colorant, 0.1-3 parts of antioxidant, 0.1-3 parts of stabilizer, and 15-30 parts of reinforced resin glass fiber powder.

[0008] Furthermore, when the raw material contains reinforced resin glass fiber powder, in the step 3, discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, reinforced resin glass fiber powder, compatibilizer, and lubricant are mixed at 120 to 150°C for 20 to 30 minutes.

[0009] Furthermore, the raw material composition is replaced as follows: 30-40 parts of discarded tea leaves, 20-50 parts of tea sticks, 12-30 parts of stalk powder, 10-30 parts of tea pectin cellulose, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of colorant, 0.1-3 parts of antioxidant, 0.1-3 parts of stabilizer, and 30-40 parts of industrial wood flour.

[0010] Furthermore, when the raw material contains reinforced resin glass fiber powder, in the step 3, discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, industrial wood flour, compatibilizer, and lubricant are mixed at 120 to 150°C for 20 to 30 minutes.

[0011] Furthermore, the raw material composition is replaced as follows: 30-40 parts of discarded tea leaves, 20-50 parts of tea sticks, 12-30 parts of stalk powder, 10-30 parts of tea pectin cellulose, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of colorant, 0.1-3 parts of antioxidant, 0.1-3 parts of stabilizer, 20-30 parts of industrial wood flour, and 15-20 parts of reinforced resin glass fiber powder.

[0012] Furthermore, when the raw material contains reinforced resin glass fiber powder, in the step 3, discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, reinforced resin glass fiber powder, industrial wood powder, compatibilizer, and lubricant are mixed at 120 to 150°C for 20 to 30 minutes.

[0013] Furthermore, the method for producing said tea pectin cellulose comprises drying and sterilizing at least one of tea sticks, tea leaves and tea residue, pulverizing and grinding them into powder, cooking them at 60-80°C and squeezing them, then soaking them in water to obtain tea pectin cellulose, which is then filtered and dried to complete the process. Furthermore, the moisture content of the coffee grounds is less than 10%. Optionally, the hydroforming is replaced by hot press molding. In a second aspect, the present invention provides a tea based composite board, manufactured using the above method. Furthermore, the composite board based on said tea has a compressive strength of 400Mpa or more, a bacteriostatic time of 8h or more, and a folding endurance of 1900 times or more. In a third aspect, the present invention provides the use of said tea based composite board in eco-furniture products. The eco-friendly furniture products include indoor furniture, kitchen and bathroom paneling products, doors, flooring, etc. Effect of the Invention

[0014] Compared with the prior art, the advantages of the present invention are as follows: The manufacturing method of the tea-based composite board of the present invention solves the problem of high waste and large amount of waste in China's current tea industry, and at the same time makes full use of coffee powder in food waste. The manufacturing process is simple, the reaction conditions are mild, and the obtained material has the advantages of being decomposable, bacteriostatic, hygroscopic, high strength and low cost. It can achieve complete biodegradation, has tea leaf fiber adsorption and aroma sustained release properties, and can replace the high-grade wood currently on the market. The board has multiple sides and any shape, and can be used according to various stretched building materials, and the use forms are diverse and wide-ranging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In describing the present invention, it should be noted that unless specific conditions are specified in the examples, they are carried out according to normal conditions or conditions suggested by the manufacturer. The reagents or equipment used are normal products that can be purchased and obtained commercially unless the manufacturer is specified.

[0016] The present invention will be described in more detail below in light of the embodiments for carrying out the invention, thereby helping those skilled in the art to have a more complete, accurate and in-depth understanding of the ideas and technical solutions of the invention. The scope of protection of the present invention includes but is not limited to the following examples. Any modifications made to the details and forms of the technical solutions of the present invention without departing from the spirit and scope of the present application will also fall within the scope of protection of the present invention.

[0017] In this embodiment, the preparation method of tea pectin cellulose is as follows: at least one of tea sticks, tea leaves and tea residue is dried and sterilized, then crushed and ground into powder, digested at 70°C and pressed, then soaked in water to obtain tea pectin cellulose, which is filtered and dried to complete the process. Example 1 This embodiment provides a method for producing a composite board based on tea, specifically,

[0018] Step 1, mixing raw materials based on a weight composition, the raw material composition being 60 parts of discarded tea leaves, 35 parts of tea sticks, 20 parts of cereal straw powder, 20 parts of tea pectin cellulose, 40 parts of coffee grounds, 3 parts of compatibilizer, 1.5 parts of lubricant, 2 parts of colorant, 1 part of antioxidant, and 1 part of stabilizer, and the moisture content of the coffee grounds is 10% or less; Step 2: soaking the tea leaves in 70°C hot water, washing, drying and crushing to 10-20 mesh to obtain tea powder; Step 3: Mixing the discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, compatibilizer, and lubricant at 140°C for 20 min; and step 4, cooling to 55°C, further adding and uniformly mixing colorant, antioxidant and stabilizer, and hydroforming at 80°C to obtain a tea-based composite board.

[0019] The composite board based on tea in this Example 1 has a compressive strength of 418Mpa, a bacteriostatic time of more than 10 hours, a folding time of 1985 times, and a strong moisture absorption ability. Example 2 This embodiment provides a method for producing a composite board based on tea, specifically,

[0020] Step 1, mixing raw materials based on a weight composition, the raw material composition being 40 parts of discarded tea leaves, 35 parts of tea sticks, 20 parts of stalk powder, 20 parts of tea pectin cellulose, 30 parts of coffee grounds, 3 parts of compatibilizer, 1 part of lubricant, 3 parts of colorant, 3 parts of antioxidant, 1 part of stabilizer, 20 parts of reinforced resin glass fiber powder, and the moisture content of the coffee grounds is 10% or less; Step 2: soaking the tea leaves in 80°C hot water, washing, drying and crushing to 10-20 mesh to obtain tea powder; Step 3: mixing the discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, reinforced resin glass fiber powder, compatibilizer, and lubricant at 140°C for 25 minutes; and step 4, cooling to 50°C, further adding and uniformly mixing colorant, antioxidant and stabilizer, and hydroforming at 80°C to obtain a tea-based composite board.

[0021] The composite board based on tea in this Example 1 was detected to have a compressive strength of 429 MPa, a bacteriostatic time of 8.5 hours, a folding time of 1922 times, and a strong moisture absorption ability. Example 3 This embodiment provides a method for producing a composite board based on tea, specifically,

[0022] Step 1, mixing raw materials based on a weight composition, the raw materials are composed of 30 parts of discarded tea leaves, 50 parts of tea sticks, 15 parts of stalk powder, 30 parts of tea pectin cellulose, 30 parts of coffee grounds, 4 parts of compatibilizer, 1 part of lubricant, 1 part of colorant, 2 parts of antioxidant, 2 parts of stabilizer, and 35 parts of industrial wood flour, and the moisture content of the coffee grounds is 10% or less; Step 2: soaking the tea leaves in 70°C hot water, washing, drying and crushing to 10-20 mesh to obtain tea powder; Step 3 is to mix the discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, industrial wood flour, compatibilizer, and lubricant at 120°C for 30 minutes; and step 4, cooling to 55°C, further adding and uniformly mixing colorant, antioxidant and stabilizer, and hydroforming at 80°C to obtain a tea-based composite board.

[0023] The composite board based on tea in this Example 1 has a compressive strength of 408Mpa, a bacteriostatic time of more than 10 hours, a folding time of 1943 times, and a strong moisture absorption ability. Example 4 This embodiment provides a method for producing a composite board based on tea, specifically,

[0024] Step 1, mixing raw materials based on a weight composition, the raw material composition being 30 parts of discarded tea leaves, 40 parts of tea sticks, 30 parts of stalk powder, 10 parts of tea pectin cellulose, 40 parts of coffee grounds, 5 parts of compatibilizer, 0.5 parts of lubricant, 3 parts of colorant, 3 parts of antioxidant, 0.5 parts of stabilizer, 20 parts of industrial wood flour, and 20 parts of reinforced resin glass fiber powder, and the moisture content of the coffee grounds is 10% or less; Step 2: soaking the tea leaves in 70°C hot water, washing, drying and crushing to 10-20 mesh to obtain tea powder;

[0025] Step 3 is to mix the discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, reinforced resin glass fiber powder, industrial wood powder, compatibilizer, and lubricant at 140°C for 20 minutes; and step 4, cooling to 55°C, further adding and uniformly mixing colorant, antioxidant and stabilizer, and hydroforming at 80°C to obtain a tea-based composite board.

[0026] The composite board based on tea in this Example 1 has a compressive strength of 421 MPa, a bacteriostatic time of more than 10 hours, a folding time of 1962 times, and a strong moisture absorption ability. The tea based composite board produced by the present invention can be used to replace high quality wood currently available on the market and can be used in any furniture product.

[0027] The above-mentioned examples only represent some embodiments of the present invention, and the description is specific and detailed, but should not be understood as a limitation on the patent scope of the present invention. It should be noted that those skilled in the art can make some modifications and improvements without departing from the idea of ​​the present invention, all of which are within the scope of protection of the present invention. Therefore, the scope of protection of the patent of the present invention shall be subject to the appended claims.

Claims

1. Step 1 is to mix raw materials based on a weight ratio, the raw materials being composed of 60-70 parts of discarded tea leaves, 20-50 parts of tea sticks, 12-30 parts of stalk powder, 10-30 parts of tea pectin cellulose, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of colorant, 0.1-3 parts of antioxidant, and 0.1-3 parts of stabilizer; Step 2: soaking the tea leaves in hot water at 60-80°C, washing, drying and crushing to 10-20 mesh to obtain tea powder; Step 3: mixing the discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, compatibilizer, and lubricant at 120-150° C. for 20-30 min; Step 4: cooling to 50-60°C, adding coloring agent, antioxidant, and stabilizer, mixing uniformly, and hydroforming at 50-118°C to obtain a composite board based on tea. A method for producing a composite board material using tea as a base material.

2. The raw material composition is replaced as follows: 40-50 parts of discarded tea leaves, 20-50 parts of tea sticks, 12-30 parts of stalk powder, 10-30 parts of tea pectin cellulose, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of colorant, 0.1-3 parts of antioxidant, 0.1-3 parts of stabilizer, 15-30 parts of reinforced resin glass fiber powder; A method for producing the tea-based composite board according to claim 1.

3. When the raw material contains reinforced resin glass fiber powder, the step 3 includes mixing the discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, reinforced resin glass fiber powder, compatibilizer, and lubricant at 120 to 150 ° C for 20 to 30 minutes; A method for producing the tea-based composite board according to claim 2.

4. The raw material composition is replaced as follows: 30-40 parts of discarded tea leaves, 20-50 parts of tea sticks, 12-30 parts of stalk powder, 10-30 parts of tea pectin cellulose, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of colorant, 0.1-3 parts of antioxidant, 0.1-3 parts of stabilizer, 30-40 parts of industrial wood flour; A method for producing the tea-based composite board according to claim 1.

5. The raw material composition is replaced as follows: 30-40 parts of discarded tea leaves, 20-50 parts of tea sticks, 12-30 parts of stalk powder, 10-30 parts of tea pectin cellulose, 30-40 parts of coffee grounds, 2-5 parts of compatibilizer, 0.2-1.5 parts of lubricant, 2-3 parts of colorant, 0.1-3 parts of antioxidant, 0.1-3 parts of stabilizer, 20-30 parts of industrial wood flour, 15-20 parts of reinforced resin glass fiber powder; A method for producing the tea-based composite board according to claim 1.

6. When the raw material contains reinforced resin glass fiber powder, the step 3 includes mixing the discarded tea leaves, tea powder, stalk powder, tea pectin cellulose, coffee grounds, reinforced resin glass fiber powder, industrial wood powder, compatibilizer, and lubricant at 120 to 150 ° C for 20 to 30 minutes; A method for producing the tea-based composite board according to claim 5.

7. The method for producing said tea pectin cellulose is to dry and sterilize at least one of tea sticks, tea leaves and tea residue, then crush and grind into powder, cook and squeeze at 60-80°C, and then soak in water to obtain tea pectin cellulose, which is then filtered and dried to complete the process. A method for producing a composite board material based on tea according to any one of claims 1 to 6.

8. Use of a tea-based composite board obtained by the process according to any one of claims 1 to 6 in eco-furniture.

Citation Information

Patent Citations

  • Processing method for tea leaf home decoration plate

    CN109648680A

  • Production method and application of myopia-preventing eye-protecting paper

    CN113481742A

  • Production method of used tea leaf board, and used tea leaf board

    JP2016175325A