Optical laminated film with pressure-sensitive adhesive layer and image display device

By incorporating a thick protective film with high tensile modulus and a thin optical film, the optical laminated film minimizes dents, ensuring high reliability and reduced optical defects in image display devices.

JP7594362B2Active Publication Date: 2024-12-04NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020007847
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-30
Filing Date
2020-01-21
Publication Date
2024-12-04
Estimated Expiration
2040-01-21

AI Technical Summary

Technical Problem

Optical laminated films with adhesive layers tend to develop dents during storage, especially when thinner optical films are used, which can lead to optical defects in image display devices.

Method used

The optical laminated film is designed with a protective film having a thickness of 30 μm or more and a tensile modulus of 1 GPa or more, along with an optical film thickness of 80 μm or less, to disperse pressure and suppress denting.

Benefits of technology

This configuration effectively reduces the occurrence of dents in the adhesive layer during storage, enhancing the reliability and optical quality of image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594362000005
    Figure 0007594362000005
  • Figure 0007594362000006
    Figure 0007594362000006
  • Figure 0007594362000007
    Figure 0007594362000007
Patent Text Reader

Abstract

To provide an optical layered film having an adhesive layer wherein the degree of dents that may occur at the time of storing can be controlled.SOLUTION: An optical layered film 1 having an adhesive layer includes a protective film 2, an optical film 3, an adhesive layer 4, and a separator 5 layered in the given order, wherein: the optical film 3 has a thickness of 80 μm or less; the protective film 2 has a thickness of 30 μm or more; and the protective film 2 has a tensile modulus of elasticity of 1 GPa or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive layer-attached optical laminate film and an image display device. [Background technology]

[0002] Various thin image display devices such as liquid crystal displays and organic EL displays usually have a laminated structure including an image forming layer such as a liquid crystal layer and an organic EL light emitting layer, and one or more optical films. A pressure sensitive adhesive layer is generally used to bond each layer constituting the image display device, and a method of manufacturing an image display device by attaching an optical film with a pressure sensitive adhesive layer, which has a pressure sensitive adhesive layer on at least one side, to an image forming layer is widely adopted (see Patent Document 1). In addition, when supplying an optical film with a pressure sensitive adhesive layer, it may be supplied as an optical laminated film with a pressure sensitive adhesive layer further provided with a separator for protecting the pressure sensitive adhesive layer and / or a protective film for protecting the optical film. The separator is peeled off when the optical laminated film is used, for example, when it is attached to the image forming layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-28573 A Summary of the Invention [Problem to be solved by the invention]

[0004] The optical laminated film with a pressure-sensitive adhesive layer is usually stored in a rolled state or in a laminated state as sheets before being combined with an image forming layer or the like to manufacture an image display device. However, according to the study by the present inventors, it was found that the above-mentioned storage tends to cause minute dents in the pressure-sensitive adhesive layer, and that this tendency is intensified when a thin optical film is provided. The dents can be optical defects. In addition, similar dents can occur during storage of the image display device after its manufacture. Patent Document 1 does not take these points into consideration.

[0005] An object of the present invention is to provide a pressure-sensitive adhesive layer-attached optical laminate film capable of suppressing the degree of depression that may occur during storage. [Means for solving the problem]

[0006] The present invention relates to A pressure-sensitive adhesive layer-attached optical laminate film in which a protective film, an optical film, a pressure-sensitive adhesive layer, and a separator are laminated in this order, The optical film has a thickness of 80 μm or less, a pressure-sensitive adhesive layer-attached optical laminate film, wherein the protective film has a thickness of 30 μm or more and a tensile modulus of elasticity of the protective film of 1 GPa or more; to provide.

[0007] In another aspect, the present invention provides a method for producing a composition comprising: An image display device comprising a portion of the pressure-sensitive adhesive layer-attached optical laminate film of the present invention excluding the separator; to provide. Effect of the Invention

[0008] In the pressure-sensitive adhesive layer-attached optical laminate film according to the present invention, while having a thin optical film with a thickness of 80 μm or less, by setting both the thickness and tensile modulus of the protective film to a predetermined value or more, the pressure generated by the trapped foreign matter can be dispersed, and the progression of the dent that may occur in the pressure-sensitive adhesive layer due to the trapped foreign matter can be suppressed. Therefore, in the pressure-sensitive adhesive layer-attached optical laminate film according to the present invention, the degree of dent that may occur during storage can be suppressed. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a pressure-sensitive adhesive layer-attached optical laminate film of the present invention. [Figure 2A] FIG. 2A is a schematic diagram for explaining a method for measuring the creep amount ΔCr for a pressure-sensitive adhesive layer. [Figure 2B] FIG. 2B is a schematic diagram for explaining a method for measuring the creep amount ΔCr for the pressure-sensitive adhesive layer. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates an example of an image display device of the present invention. [Figure 4] FIG. 4 is a schematic diagram for explaining a method for producing the λ / 4 plate and the λ / 2 plate used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The present invention is not limited to the embodiment described below.

[0011] An example of the pressure-sensitive adhesive layer-attached optical laminate film of the present invention is shown in Figure 1. The pressure-sensitive adhesive layer-attached optical laminate film 1 of Figure 1 comprises a protective film 2, an optical film 3, a pressure-sensitive adhesive layer 4, and a separator 5. The protective film 2, the optical film 3, the pressure-sensitive adhesive layer 4, and the separator 5 are laminated in this order. The thickness of the optical film 3 is 80 µm or less. The thickness of the protective film 2 is 30 µm or more. The tensile modulus of elasticity of the protective film 2 is 1 GPa or more. The tensile modulus of elasticity of the protective film 2 is a value at room temperature (23°C).

[0012] [Optical film] The optical film 3 is, for example, a polarizing film or a retardation film. The optical film 3 may be a laminated film or an optical laminate including a polarizing film and / or a retardation film. However, the optical film 3 is not limited to the above examples. The optical film 3 may include a glass film.

[0013] The optical film 3 has a thickness of 80 μm or less. According to the study by the present inventors, when the optical laminate film 1 has a thinned optical film 3 having a thickness of 80 μm or less, the degree of depression of the adhesive layer 4 that may occur during storage tends to become large. However, the optical laminate film 1 can suppress the degree of depression of the adhesive layer 4 that may occur during storage while having the thinned optical film 3. The thickness of the optical film 3 may be 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, or even 35 μm or less. The lower limit of the thickness of the optical film 3 is, for example, 1 μm or more.

[0014] The polarizing film includes a polarizer. A polarizer protective film may be bonded to at least one surface of the polarizer. Any adhesive or bonding agent may be used to bond the polarizer and the polarizer protective film. The polarizer is typically a polyvinyl alcohol (PVA) film in which iodine is oriented by stretching such as air stretching (dry stretching) or stretching in boric acid water.

[0015] The retardation film is a film having birefringence in the in-plane direction and / or the thickness direction, and is, for example, a stretched resin film or a film in which a liquid crystal material is oriented and fixed.

[0016] The retardation film is, for example, a λ / 4 plate, a λ / 2 plate, an anti-reflection retardation film (see, for example, paragraphs 0221, 0222, and 0228 of JP 2012-133303 A), a retardation film for compensating a viewing angle (see, for example, paragraphs 0225 and 0226 of JP 2012-133303 A), and an inclined orientation retardation film for compensating a viewing angle (see, for example, paragraph 0227 of JP 2012-13303 A). However, the retardation film is not limited to the above examples as long as it has birefringence in the in-plane direction and / or the thickness direction. There are also no limitations on the retardation value, arrangement angle, three-dimensional birefringence, whether it is a single layer or a multilayer, and the like, of the retardation film. A known film can be used for the retardation film.

[0017] The thickness of the retardation film is, for example, 50 μm or less.

[0018] The optical film 3 may be a single-layer film or a multi-layer film composed of two or more layers.

[0019] [Protective film] The protective film 2 has a function of protecting the optical film 2 during distribution and storage of the optical laminate film 1 and in a state where the optical laminate film 1 is incorporated in an image display device. The protective film 2 may be a film that functions as a window to the external space in a state where it is incorporated in an image display device. The protective film 2 is typically a resin film. The resin constituting the protective film 2 is, for example, polyester such as polyethylene terephthalate (PET), polyolefin such as polyethylene and polypropylene, acrylic, cycloolefin, polyimide, polyamide, and polyester is preferable. In other words, the protective film 2 may be a polyester film. However, the protective film 2 is not limited to the above examples. The protective film may be a glass film or a laminate film including a glass film. The protective film 2 may be subjected to surface treatment such as anti-glare, anti-reflection, and anti-static.

[0020] The thickness of the protective film 2 is 30 μm or more. The thickness of the protective film 2 may be 35 μm or more, 40 μm or more, 45 μm or more, or even 50 μm or more. The upper limit of the thickness of the protective film 2 is, for example, 100 μm or less.

[0021] The protective film 2 has a tensile modulus of 1 GPa or more. The protective film 2 may have a tensile modulus of 2 GPa or more, 3 GPa or more, or even 4 GPa or more. The upper limit of the tensile modulus of the protective film 2 is, for example, 100 GPa or less.

[0022] The protective film 2 may be bonded to the optical film 3 by an arbitrary pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer bonding the protective film 2 and the optical film 3 may have a configuration described in the description of the pressure-sensitive adhesive layer 4 below.

[0023] [Adhesive layer] The adhesive layer 4 is composed of various adhesive compositions such as acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, fluorine adhesives, epoxy adhesives, and polyether adhesives. The adhesive layer 4 is preferably composed of an acrylic adhesive composition containing a (meth)acrylic polymer, since it has excellent properties such as optical transparency, processability, durability, and adhesion. In this specification, "(meth)acrylic" means acrylic and methacrylic. Also, "(meth)acrylate" means acrylate and methacrylate.

[0024] The type of the adhesive composition constituting the adhesive layer 4 is, for example, an emulsion type, a solvent type (solution type), an active energy ray curing type, or a hot melt type (hot melt type). Among these, a solvent type or active energy ray curing type adhesive composition is preferred, and an active energy ray curing type adhesive composition is preferred from the viewpoints of productivity and ease of forming a thick adhesive layer 4. However, the type of the adhesive composition is not limited to the above examples.

[0025] The acrylic pressure-sensitive adhesive composition capable of forming the pressure-sensitive adhesive layer 4 will now be described.

[0026] [(Meth)acrylic polymer] The (meth)acrylic polymer preferably has as its main unit a structural unit derived from a (meth)acrylic monomer (A) having an alkyl group having 1 to 30 carbon atoms on its side chain. The alkyl group may be linear or branched. The (meth)acrylic polymer may have one or more structural units derived from the (meth)acrylic monomer (A). Examples of the (meth)acrylic monomer (A) include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, and the like. acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate (lauryl (meth)acrylate), n-tridecyl (meth)acrylate, and n-tetradecyl (meth)acrylate. In this specification, the term "main unit" refers to a unit that accounts for, for example, 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 94% by mass or more of all the structural units contained in the polymer.

[0027] The (meth)acrylic polymer may have a structural unit derived from a (meth)acrylic monomer (A) having a long-chain alkyl group on the side chain. The structural unit is, for example, n-dodecyl (meth)acrylate (lauryl (meth)acrylate). In this specification, the term "long-chain alkyl group" refers to an alkyl group having 6 to 30 carbon atoms.

[0028] The (meth)acrylic polymer may have a structural unit derived from a (meth)acrylic monomer (A) that, when made into a homopolymer, has a glass transition temperature (Tg) in the range of −70 to −20° C. An example of such a structural unit is 2-ethylhexyl acrylate.

[0029] The (meth)acrylic polymer may have a structural unit other than the structural unit derived from the (meth)acrylic monomer (A). The structural unit is derived from a monomer (B) copolymerizable with the (meth)acrylic monomer (A). The (meth)acrylic polymer may have one or more types of the structural unit.

[0030] The monomer (B) is, for example, a (meth)acrylic monomer (C) having a hydroxy group. The (meth)acrylic monomer (C) is, for example, a hydroxyalkyl (meth)acrylate such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, or 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. Since the durability and adhesion of the pressure-sensitive adhesive layer 4 can be improved, the (meth)acrylic monomer (C) is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate.

[0031] The monomer (B) may be a carboxyl group-containing monomer, an amino group-containing monomer, or an amide group-containing monomer. By using these monomers (B), the adhesion of the pressure-sensitive adhesive layer 4 can be improved. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Examples of the amino group-containing monomer include N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate. Examples of the amide group-containing monomer include acrylamide-based monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropylacrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylol-N-propane(meth)acrylamide, aminomethyl(meth)acrylamide, aminoethyl(meth)acrylamide, mercaptomethyl(meth)acrylamide, and mercaptoethyl(meth)acrylamide; N-acryloyl heterocyclic monomers such as N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, and N-(meth)acryloylpyrrolidine; and N-vinyl group-containing lactam monomers such as N-vinylpyrrolidone and N-vinyl-ε-caprolactam.

[0032] The monomer (B) may be a polyfunctional monomer. By using a polyfunctional monomer, the gel fraction of the pressure-sensitive adhesive layer 4 and the cohesive strength can be adjusted. Examples of the polyfunctional monomer include polyfunctional acrylates such as hexanediol di(meth)acrylate (1,6-hexanediol di(meth)acrylate), butanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; and divinylbenzene. The polyfunctional acrylate is preferably 1,6-hexanediol diacrylate or dipentaerythritol hexa(meth)acrylate.

[0033] Examples of the other monomers (B) other than those mentioned above include (meth)acrylic acid alkoxyalkyl esters such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 4-ethoxybutyl (meth)acrylate; epoxy group-containing monomers such as glycidyl (meth)acrylate and methyl glycidyl (meth)acrylate; sulfonic acid group-containing monomers such as sodium vinyl sulfonate; phosphoric acid group-containing monomers; (meth)acrylate, ... p) (meth)acrylic acid esters having an alicyclic hydrocarbon group, such as cyclopentyl acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, etc.; (meth)acrylic acid esters having an aromatic hydrocarbon group, such as phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, etc.; vinyl esters such as vinyl acetate, vinyl propionate, etc.; aromatic vinyl compounds such as styrene, vinyl toluene, etc.; olefins or dienes such as ethylene, propylene, butadiene, isoprene, isobutylene, etc.; vinyl ethers such as vinyl alkyl ether; and vinyl chloride.

[0034] The total content of the structural units derived from the (meth)acrylic monomer (C) having a hydroxyl group, the carboxyl group-containing monomer, the amino group-containing monomer, the amide group-containing monomer, and the polyfunctional monomer in the (meth)acrylic polymer is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 8% by mass or less, and particularly preferably 5% by mass or less. When the (meth)acrylic polymer has the structural units, the total content of the structural units is, for example, 0.01% by mass or more, and may be 0.05% by mass or more.

[0035] The total content of the structural units derived from the other monomer (B) in the (meth)acrylic polymer is, for example, 30% by mass or less, may be 10% by mass or less, and is preferably 0% by mass (not including such structural units).

[0036] The (meth)acrylic polymer can be formed by polymerizing one or more of the above-mentioned monomers by a known method. A monomer and a partial polymer of the monomer may be polymerized. The polymerization can be carried out, for example, by solution polymerization, emulsion polymerization, bulk polymerization, thermal polymerization, or active energy ray polymerization. Since a pressure-sensitive adhesive layer 4 having excellent optical transparency can be formed, solution polymerization and active energy ray polymerization are preferred. The polymerization is preferably carried out while avoiding contact between the monomer and / or the partial polymer and oxygen, and for this purpose, for example, polymerization in an inert gas atmosphere such as nitrogen or polymerization in a state where oxygen is blocked by a resin film or the like can be adopted. The (meth)acrylic polymer to be formed may be in any form such as a random copolymer, a block copolymer, or a graft copolymer.

[0037] The polymerization system for forming the (meth)acrylic polymer may contain one or more polymerization initiators. The type of polymerization initiator can be selected depending on the polymerization reaction, and may be, for example, a photopolymerization initiator or a thermal polymerization initiator.

[0038] Examples of the solvent used in the solution polymerization include esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; and ketones such as methyl ethyl ketone and methyl isobutyl ketone. However, the solvent is not limited to the above examples. The solvent may be a mixed solvent of two or more solvents.

[0039] The polymerization initiator used in the solution polymerization is, for example, an azo-based polymerization initiator, a peroxide-based polymerization initiator, or a redox-based polymerization initiator. The peroxide-based polymerization initiator is, for example, dibenzoyl peroxide or t-butyl permaleate. Among them, the azo-based polymerization initiator disclosed in JP-A-2002-69411 is preferable. The azo-based polymerization initiator is, for example, 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate) dimethyl, or 4,4'-azobis-4-cyanovaleric acid. However, the polymerization initiator is not limited to the above examples. The amount of the azo-based polymerization initiator used is, for example, 0.05 to 0.5 parts by weight, or may be 0.1 to 0.3 parts by weight, based on 100 parts by weight of the total amount of the monomers.

[0040] The active energy rays used in the active energy ray polymerization are, for example, ionizing radiation such as α rays, β rays, γ rays, neutron rays, and electron beams, and ultraviolet rays. The active energy rays are preferably ultraviolet rays. Polymerization by irradiation with ultraviolet rays is also called photopolymerization. The polymerization system of the active energy ray polymerization typically contains a photopolymerization initiator. The polymerization conditions of the active energy polymerization are not limited as long as a (meth)acrylic polymer is formed.

[0041] Examples of the photopolymerization initiator include a benzoin ether-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an α-ketol-based photopolymerization initiator, an aromatic sulfonyl chloride-based photopolymerization initiator, a photoactive oxime-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzyl-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, a ketal-based photopolymerization initiator, and a thioxanthone-based photopolymerization initiator, although the photopolymerization initiator is not limited to the above examples.

[0042] Examples of the benzoin ether-based photopolymerization initiator include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one, and anisole methyl ether. Examples of the acetophenone-based photopolymerization initiator include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of the α-ketol-based photopolymerization initiator include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of the aromatic sulfonyl chloride-based photopolymerization initiator include 2-naphthalenesulfonyl chloride. An example of the photoactive oxime-based photopolymerization initiator is 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime. An example of the benzoin-based photopolymerization initiator is benzoin. An example of the benzyl-based photopolymerization initiator is benzil. An example of the benzophenone-based photopolymerization initiator is benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, α-hydroxycyclohexylphenyl ketone. An example of the ketal-based photopolymerization initiator is benzyl dimethyl ketal. An example of the thioxanthone-based photopolymerization initiator is thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.

[0043] The amount of the photopolymerization initiator used is, for example, 0.01 to 1 part by weight, and may be 0.05 to 0.5 parts by weight, relative to 100 parts by weight of the total amount of the monomers.

[0044] The polyfunctional monomer (polyfunctional acrylate, etc.) as monomer (B) can be used in both solvent-based and active energy ray-curable pressure-sensitive adhesive compositions. When both the polyfunctional monomer and the photopolymerization initiator are used for a solvent-based pressure-sensitive adhesive composition, for example, the solvent may be removed by thermal drying, and then the pressure-sensitive adhesive composition may be cured by irradiation with active energy rays.

[0045] The weight average molecular weight (Mw) of the (meth)acrylic polymer is, for example, 1,000,000 to 2,500,000, and is preferably 1,200,000 to 2,000,000, and more preferably 1,400,000 to 1,800,000 from the viewpoint of the durability and heat resistance of the pressure-sensitive adhesive layer 4. Note that the weight average molecular weight (Mw) of the polymer and oligomer in this specification is a value (polystyrene equivalent) based on measurement by GPC (gel permeation chromatography).

[0046] The content of the (meth)acrylic polymer in the acrylic pressure-sensitive adhesive composition is, for example, 50 mass % or more, and may be 60 mass % or more, or even 70 mass % or more, in terms of solid content.

[0047] [(Meth)acrylic oligomer] The acrylic pressure-sensitive adhesive composition may further contain a (meth)acrylic oligomer. The inclusion of the (meth)acrylic oligomer reduces entanglement between molecular chains of the (meth)acrylic polymer, thereby improving the stress relaxation properties of the pressure-sensitive adhesive layer 4.

[0048] The (meth)acrylic oligomer may have the same composition as the above-mentioned (meth)acrylic polymer, except for the weight average molecular weight (Mw). The weight average molecular weight (Mw) of the (meth)acrylic oligomer may be, for example, 1000 or more, 2000 or more, 3000 or more, or even 4000 or more. The upper limit of the weight average molecular weight (Mw) of the (meth)acrylic oligomer may be, for example, 30000 or less, 15000 or less, 10000 or less, or even 7000 or less. The (meth)acrylic oligomer having a weight average molecular weight (Mw) within these ranges can further improve the stress relaxation property of the pressure-sensitive adhesive layer 4.

[0049] The (meth)acrylic oligomer has, for example, one or more structural units derived from each of the following monomers: methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, and isooctyl. (meth)acrylate, alkyl (meth)acrylates such as nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate; esters of (meth)acrylic acid and alicyclic alcohols such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; aryl (meth)acrylates such as phenyl (meth)acrylate and benzyl (meth)acrylate; and (meth)acrylates obtained from alcohols derived from terpene compounds.

[0050] The (meth)acrylic oligomer preferably has a structural unit derived from an acrylic monomer having a relatively bulky structure. In this case, the adhesive property of the pressure-sensitive adhesive layer 4 can be further improved. The acrylic monomer is, for example, an alkyl (meth)acrylate having an alkyl group having a branched structure, such as isobutyl (meth)acrylate and t-butyl (meth)acrylate; an ester of (meth)acrylic acid and an alicyclic alcohol, such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; and an aryl (meth)acrylate, such as phenyl (meth)acrylate and benzyl (meth)acrylate. The acrylic monomer preferably has a cyclic structure, and more preferably has two or more cyclic structures. Furthermore, when ultraviolet irradiation is performed during polymerization of the (meth)acrylic oligomer and / or formation of the adhesive layer 4, it is preferable that the acrylic monomer does not have an unsaturated bond, since this makes it difficult to inhibit the progress of the polymerization and / or formation. For example, an alkyl (meth)acrylate having an alkyl group with a branched structure, or an ester of (meth)acrylic acid and an alicyclic alcohol can be used.

[0051] Specific examples of the (meth)acrylic oligomer include a copolymer of butyl acrylate, methyl acrylate, and acrylic acid, a copolymer of cyclohexyl methacrylate and isobutyl methacrylate, a copolymer of cyclohexyl methacrylate and isobornyl methacrylate, a copolymer of cyclohexyl methacrylate and acryloylmorpholine, a copolymer of cyclohexyl methacrylate and diethylacrylamide, a copolymer of 1-adamantyl acrylate and methyl methacrylate, a copolymer of dicyclopentanyl methacrylate and isobornyl methacrylate, a copolymer of at least one selected from dicyclopentanyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, isobornyl acrylate, and cyclopentanyl methacrylate and methyl methacrylate, a homopolymer of dicyclopentanyl acrylate, a homopolymer of 1-adamantyl methacrylate, and a homopolymer of 1-adamantyl acrylate.

[0052] As the polymerization method for the (meth)acrylic oligomer, the above-mentioned polymerization method for the (meth)acrylic polymer can be used.

[0053] When the pressure-sensitive adhesive composition contains a (meth)acrylic oligomer, the blending amount thereof may be, for example, 70 parts by weight or less, 50 parts by weight or less, or even 40 parts by weight or less, relative to 100 parts by weight of the (meth)acrylic polymer. The lower limit of the blending amount may be, for example, 1 part by weight or more, 2 parts by weight or more, or even 3 parts by weight or more, relative to 100 parts by weight of the (meth)acrylic polymer.

[0054] The (meth)acrylic oligomer can be used in both solvent-based and active energy ray-curable pressure-sensitive adhesive compositions. However, when the (meth)acrylic oligomer is dissolved in a solvent when used in an active energy ray-curable pressure-sensitive adhesive composition, the mixture containing the (meth)acrylic oligomer may be cured by irradiation with active energy rays after removing the solvent by, for example, heat drying.

[0055] [Crosslinking agent] The acrylic pressure-sensitive adhesive composition may further contain a crosslinking agent. By using a crosslinking agent, the cohesive strength of the pressure-sensitive adhesive layer 4 is improved.

[0056] The crosslinking agent is, for example, an organic crosslinking agent or a polyfunctional metal chelate. The organic crosslinking agent is, for example, an isocyanate crosslinking agent, a peroxide crosslinking agent, an epoxy crosslinking agent, or an imine crosslinking agent. The polyfunctional metal chelate has a structure in which a polyvalent metal and an organic compound are covalently bonded or coordinately bonded. The polyvalent metal is, for example, Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, or Ti. The atom in the organic compound to which the polyvalent metal is covalently bonded or coordinately bonded is typically an oxygen atom. The organic compound is, for example, an alkyl ester, an alcohol compound, a carboxylic acid compound, an ether compound, or a ketone compound. The organic crosslinking agent and the polyfunctional metal chelate can be used for both solvent-based and active energy ray-curable pressure-sensitive adhesive compositions.

[0057] When the adhesive composition is a solvent-based one, the crosslinking agent is preferably a peroxide-based crosslinking agent or an isocyanate-based crosslinking agent, and more preferably a peroxide-based crosslinking agent. Since the peroxide-based crosslinking agent promotes crosslinking between side chains of the (meth)acrylic polymer, the crosslinking by the peroxide-based crosslinking agent increases the degree of freedom of the molecular chain after crosslinking compared to crosslinking by the isocyanate-based crosslinking agent. Therefore, the stress relaxation property can be more reliably ensured while increasing the cohesive force of the adhesive layer 4. On the other hand, the crosslinking by the isocyanate-based crosslinking agent can improve the durability of the adhesive layer 4 compared to crosslinking by the peroxide-based crosslinking agent. However, since the crosslinking by the bifunctional isocyanate crosslinking agent forms a two-dimensional crosslinked structure, it is possible to more reliably ensure the stress relaxation property of the adhesive layer 4, although not as much as the crosslinking by the peroxide-based crosslinking agent. When the isocyanate-based crosslinking agent is used, a trifunctional crosslinking agent that forms a strong three-dimensional crosslinked structure may be used in combination with the bifunctional crosslinking agent to improve the balance between durability and stress relaxation property. In order to further improve the balance, a peroxide-based crosslinking agent and an isocyanate-based crosslinking agent may be used in combination. The polyfunctional monomer (B) may be used in combination with a crosslinking agent.

[0058] When the pressure-sensitive adhesive composition contains a crosslinking agent, the amount of the crosslinking agent is, for example, 0.1 to 10 parts by weight, and may be 0.2 to 5 parts by weight, or even 0.3 to 3 parts by weight, relative to 100 parts by weight of the (meth)acrylic polymer.

[0059] When the peroxide-based crosslinking agent is used alone, the amount added is, for example, 0.2 to 5 parts by weight, and may be 1 to 3 parts by weight, based on 100 parts by weight of the (meth)acrylic polymer.

[0060] When a peroxide-based crosslinking agent and an isocyanate-based crosslinking agent are used in combination, the weight ratio of the peroxide-based crosslinking agent to the isocyanate-based crosslinking agent is preferably 1.2 or more, more preferably 1.5 or more, and even more preferably 3 or more. The upper limit of the weight ratio is, for example, 500 or less, 300 or less, or even 200 or less.

[0061] [Additives] The acrylic pressure-sensitive adhesive composition may contain other additives, such as silane coupling agents, polyether compounds (polyalkylene glycols including polypropylene glycols), colorants such as pigments and dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, softeners, antioxidants, antiaging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, antistatic agents (alkali metal salts, which are ionic compounds, ionic liquids, ionic solids, etc.), inorganic fillers, organic fillers, powders such as metal powders, particles, and foils.

[0062] [Formation of adhesive layer 4] The adhesive layer 4 composed of the acrylic adhesive composition can be formed as follows. When the adhesive composition is a solvent type, for example, a mixture of a (meth)acrylic polymer and a solvent, and if necessary, a (meth)acrylic oligomer, a crosslinking agent, an additive, etc. is applied onto a substrate film, and the mixture is dried to form the adhesive layer 4. When the adhesive composition is an active energy ray curable type, for example, a mixture of a monomer (group) that becomes a (meth)acrylic polymer by polymerization, and if necessary, a partial polymer of the monomer (group), a polymerization initiator, a (meth)acrylic oligomer, a crosslinking agent, an additive, a solvent, etc. is applied onto a substrate film, and the solvent is removed by drying if necessary, and then the adhesive layer 4 can be formed by irradiating with active energy rays. The substrate film may be a film whose surface has been subjected to a release treatment. The adhesive layer 4 formed on the substrate film can be transferred to any layer. The substrate film may also be an optical film, and in this case, a protective film 2 and a separator 5 are further arranged to obtain an optical laminated film with an adhesive layer having the adhesive layer 4. The base film may also be a separator 5. In this case, by further arranging an optical film 3 and a protective film 2, a pressure-sensitive adhesive layer-attached optical laminate film having a pressure-sensitive adhesive layer 4 is obtained.

[0063] The mixture can be applied to the substrate film by a known method, such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, or extrusion coating using a die coater.

[0064] The mixture to be applied to the substrate film preferably has a viscosity suitable for handling and coating. For this reason, when the pressure-sensitive adhesive composition is an active energy ray curable type, the mixture preferably contains a partial polymer of the monomer(s).

[0065] The release film that can be used for the base film is, for example, a resin film whose surface has been subjected to a release treatment with a silicone compound.

[0066] The temperature for drying the mixture is, for example, 40 to 200° C., and may be 50 to 180° C., or further 70 to 170° C. The time for drying the mixture is, for example, 5 seconds to 20 minutes, and may be 5 seconds to 10 minutes, or further 10 seconds to 5 minutes.

[0067] When the pressure-sensitive adhesive layer 4 has a thickness of 25 μm or more, the degree of the above-mentioned depression that may occur during storage as the optical laminate film 1 tends to increase. Therefore, when the pressure-sensitive adhesive layer 4 has a thickness of 25 μm or more, the effect of the present invention becomes more remarkable. The thickness of the pressure-sensitive adhesive layer 4 may be 30 μm or more, 40 μm or more, or even 50 μm or more. The upper limit of the thickness of the pressure-sensitive adhesive layer 4 is, for example, 150 μm or less. However, the thickness of the pressure-sensitive adhesive layer 4 is not limited to the above example, and may be 1 to 200 μm, 5 to 150 μm, or even 10 to 100 μm.

[0068] The gel fraction of the pressure-sensitive adhesive layer 4 is preferably 60% or more, and may be 65% or more, or even 70% or more. The upper limit of the gel fraction of the pressure-sensitive adhesive layer 4 is, for example, 95% or less, and may be 90% or less. When the gel fraction of the pressure-sensitive adhesive layer 4 is within this range, the effect of suppressing the degree of the above-mentioned depression can be more reliably obtained.

[0069] The weight average molecular weight (Mw) of the sol content in the pressure-sensitive adhesive layer 4 is, for example, 50,000 or more, and may be 80,000 or more, 100,000 or more, 150,000 or more, or even 200,000 or more. The upper limit of the weight average molecular weight (Mw) of the sol content is, for example, 1,200,000 or less. When the weight average molecular weight (Mw) of the sol content in the pressure-sensitive adhesive layer 4 is within this range, and preferably 150,000 or more, the effect of suppressing the degree of dents can be more reliably obtained.

[0070] The indentation hardness of the adhesive layer 4 is 3.0×10 4 When the indentation hardness of the pressure-sensitive adhesive layer 4 is 3.0×10 Pa or less, the degree of the above-mentioned depression that may occur during storage of the optical laminate film 1 tends to increase. 4 The effect of the present invention becomes more remarkable when the indentation hardness of the pressure-sensitive adhesive layer 4 is 1.4×10 Pa or less.4 Pa or less, 1.2×10 4 Pa or less, 1.0×10 4 Pa or less, 8×10 3 Pa or less, even 5×10 3 The lower limit of the indentation hardness may be, for example, 1×10 2 Pa or more.

[0071] The indentation hardness of the adhesive layer 4 can be measured by an indentation test based on the nanoindentation method. Specifically, the method is as follows. The adhesive layer 4 to be evaluated is cut into a size of about 1 cm x 1 cm, and the cut adhesive layer 4 is fixed to the surface of a support to prepare a measurement sample. The support has a smooth surface to fix the adhesive layer 4, and is made of a material, typically glass or metal, that has sufficient hardness not to affect the measurement results. The support is, for example, a plate. Next, the measurement sample is set in a nanoindentation device, and an indentation test is performed by pressing the indenter at a constant speed using a spherical indenter with a curvature radius of 10 μm at room temperature to a depth of 5000 nm from the surface of the adhesive layer 4. The indentation speed of the indenter is 1000 nm / sec. The maximum load obtained at this time is divided by the projected area of ​​the part of the indenter that is in contact with the measurement sample when the maximum load is obtained, relative to the sample, and the value can be the indentation hardness of the adhesive layer 4.

[0072] The creep amount ΔCr of the pressure-sensitive adhesive layer 4 at 70° C. determined by the following test is, for example, 65 μm or less, and may be 50 μm or less, 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, or even 15 μm or less. The lower limit of the creep amount ΔCr is, for example, 0.5 μm. Test: A pressure-sensitive adhesive layer is attached to a stainless steel test plate at a joint surface of 20 mm long x 20 mm wide. With the test plate fixed, a load of 500 gf is applied vertically downward. The creep amount (displacement amount) of the pressure-sensitive adhesive layer relative to the test plate is measured at 100 seconds and 3600 seconds after the load is applied, and the creep amount (displacement amount) of the pressure-sensitive adhesive layer relative to the test plate is measured at each time point. 100 and Cr 3600 The measured Cr100 and Cr 3600 From the formula ΔCr = Cr 3600 -Cr 100 The creep amount ΔCr is calculated by the following.

[0073] When the creep amount ΔCr of the pressure-sensitive adhesive layer 4 at 70° C. is within these ranges, the effect of suppressing the degree of the above-mentioned depression can be more reliably obtained.

[0074] The creep amount ΔCr of the adhesive layer 4 can be evaluated as follows (see FIG. 2A and FIG. 2B). A laminate of the adhesive layer 4 to be evaluated and the support film 51 is cut into a rectangular shape of 20 mm×30 mm to prepare a test piece 52. The support film 51 is arranged for the purpose of suppressing deformation of the portion of the adhesive layer 4 to which the load is applied during the test, thereby enabling more accurate measurement of the creep amount ΔCr. For example, a resin film such as a polyethylene terephthalate (PET) film can be used as the support film 51. The support film 51 may be an optical film that is bonded (bonded) to the adhesive layer 4 in the image display device. The thickness of the support film 51 may be any thickness that does not deform itself due to the load, and is, for example, 20 to 200 μm. The support film 51 may be an optical film 3 or a laminated film including the optical film 3. The laminated film is, for example, a laminate of the optical film 3 and the protective film 2. Next, as shown in FIG. 2A and FIG. 2B, the test piece 52 is attached to the surface of the stainless steel test plate 53 by the adhesive layer 4 at a joint surface of 20 mm long x 20 mm wide. FIG. 2B is a cross section BB of FIG. 2A. The test piece 52 is attached to the test plate 53 so that no air bubbles are mixed between the test plate 53 and the adhesive layer 4. After the test piece 52 is attached by hand, the test piece 52 is placed in an autoclave at 50°C and 5 atmospheres (absolute pressure) for 15 minutes to homogenize the bond between the test plate 53 and the adhesive layer 4, and then left in an atmospheric pressure atmosphere at 60°C for 2 hours to complete aging. Next, the test plate 53 and the test piece 52 are held vertically with the test plate 53 facing upward and left in an atmosphere at 70°C for at least 5 minutes, and then a weight of 500 g is fixed to the center of the lower end of the test piece 52 with the test plate 53 fixed, and a load 54 of 500 gf is applied vertically downward. The creep amount (displacement amount) of the adhesive layer 4 with respect to the test plate 53 at each time point, 100 seconds and 3600 seconds after the load 54 was started to be applied, was measured as the falling amount of the weight at each time point. 100 and Cr 3600 The measured Cr 100 and Cr 3600 From the formula ΔCr = Cr 3600 -Cr 100The creep amount ΔCr can be calculated by the following. A laser displacement meter can be used to measure the fall of the weight. 100 The reason for using this as the standard is that there is a large variation in the amount of fall of the weight immediately after the application of the load 54, even for the same test piece, and the influence of this unavoidable variation in the initial stage is to be eliminated as much as possible, thereby improving the accuracy of the measurement.

[0075] In order to control the creep amount ΔCr of the pressure-sensitive adhesive layer 4 at 70° C., for example, the following methods can be used alone or in combination. In order to more reliably control the creep amount ΔCr of the pressure-sensitive adhesive layer 4 at 70° C., it is preferable to combine the following methods. However, the control methods are not limited to the examples shown below. ·Method 1 The composition of the (meth)acrylic monomer contained in the pressure-sensitive adhesive composition is controlled. For example, when the (meth)acrylic monomer has a structural unit derived from the (meth)acrylic monomer (C) having a hydroxy group and / or has a structural unit derived from the monomer (B) which is a crosslinkable monomer, the creep amount ΔCr of the pressure-sensitive adhesive layer 4 at 70° C. usually shows a tendency to decrease. ·Method 2 The type and amount of crosslinking agent added to the adhesive composition are controlled. By increasing the amount of crosslinking agent, the creep amount ΔCr of the adhesive layer 4 at 70°C usually tends to decrease. In addition, since this tendency differs depending on the type of crosslinking agent, the creep amount ΔCr of the adhesive layer 4 at 70°C can be more precisely controlled by combining crosslinking agents of different types. For example, when the adhesive composition is a solvent-based adhesive, a peroxide-based crosslinking agent is more likely to reduce the creep amount ΔCr at 70°C while suppressing the increase in the elastic modulus of the adhesive layer 4 and maintaining the stress relaxation property, compared to a trifunctional crosslinking agent. In addition, an active energy ray-curable adhesive composition that is cured by a photopolymerization initiator and a polyfunctional monomer is more likely to reduce the creep amount ΔCr at 70°C, compared to a solvent-based adhesive composition, and the degree of the above-mentioned depression can be more reliably suppressed. ·Method 3 By adding a (meth)acrylic oligomer to the pressure-sensitive adhesive composition, the creep amount ΔCr of the pressure-sensitive adhesive layer 4 at 70° C. usually tends to increase due to the incorporation of the (meth)acrylic oligomer.

[0076] [Separator] The separator 5 is typically a resin film. The resin constituting the separator 5 is, for example, polyester such as PET, polyolefin such as polyethylene and polypropylene, polycarbonate, acrylic, polystyrene, polyamide, or polyimide. The surface of the separator 5 that contacts the pressure-sensitive adhesive layer 4 may be subjected to a release treatment. The release treatment can be performed, for example, by using a silicone compound. However, the separator 5 is not limited to the above example. The separator 5 is peeled off when the optical laminate film 1 is used, for example, when it is attached to the image forming layer.

[0077] The thickness of the separator 5 is, for example, 20 μm or more, and may be 30 μm or more, 35 μm or more, 40 μm or more, 45 μm or more, 50 μm or more, or even 75 μm or more. When the thickness of the separator 5 is 45 μm or more, particularly 75 μm or more, the degree of the above-mentioned dent that may occur in the pressure-sensitive adhesive layer 4 during storage of the optical laminate film 1 can be more reliably suppressed. This is because the thickness of the separator 5 can disperse the pressure generated by the trapped foreign matter.

[0078] The pressure-sensitive adhesive-attached optical laminate film of the present invention may have layers other than those described above.

[0079] The pressure-sensitive adhesive layer-attached optical laminate film 1 can be distributed and stored, for example, as a roll in which the strip-shaped film 1 is rolled up, or as a laminate of the sheet-shaped film 1.

[0080] The pressure-sensitive adhesive layer-attached optical laminate film 1 is typically used in an image display device. The image display device is, for example, a liquid crystal display or an organic EL display. The type and configuration of the image display device are not limited.

[0081] [Image display device] An example of the image display device of the present invention is shown in Fig. 3. The image display device 6 shown in Fig. 3 has an optical laminate in which a substrate 8, an image forming layer (e.g., an organic EL layer) 7, an adhesive layer 4, an optical film 3, and a protective film 2 are laminated in this order. The image display device 6 has a portion of the optical laminate film 1 excluding the separator 5. The substrate 8 and the image forming layer 7 may have the same configurations as the substrate and the image forming layer, respectively, of a known image display device. The image display device 6 has advantages such as high reliability and few optical defects because the degree of the above-mentioned recess that may occur in the adhesive layer 4 is suppressed.

[0082] 3 is an organic EL display. However, the type and configuration of the image display device 6 are not limited.

[0083] The image display device of the present invention may have any configuration as long as it includes the parts of the pressure-sensitive adhesive layer-attached optical laminate film 1 excluding the separator 5 . EXAMPLES

[0084] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.

[0085] First, the evaluation methods for the optical laminate films and pressure-sensitive adhesive layers produced in the examples and comparative examples will be described.

[0086] [Weight average molecular weight (Mw)] The weight average molecular weight (Mw) of the (meth)acrylic polymer and (meth)acrylic oligomer was measured by GPC under the following measurement conditions. Analytical equipment: Waters, Acquity APC Column: Tosoh, G7000HXL+GMHXL+GMHXL Column temperature: 40℃ Eluent: Tetrahydrofuran (with added acid) ·Flow rate: 0.8mL / min ·Injection volume: 100μL Detector: Differential refractometer (RI) Standard sample: Agilent, polystyrene (PS)

[0087] [Creep amount ΔCr at 70℃] The creep amount ΔCr at 70°C for the pressure-sensitive adhesive layer thus prepared was evaluated by the method described above. The separator used in preparing the optical laminate film was used as the support film 51. A SUS304 plate (30mm x 75mm, thickness 2.5mm) was used as the test plate 53. Keyence LK-H057 / LK-HD500 was used as the laser displacement meter. In addition, the test plate 53 was left in an atmosphere at 70°C for 5 minutes between the time the test plate 53 was held vertically with the upper side facing up and the start of the test.

[0088] [Gel fraction] The gel fraction of the prepared adhesive layer was evaluated as follows. First, about 0.2 g was scraped off from the prepared adhesive layer to obtain a small piece. Next, the obtained small piece was wrapped in a stretched porous film of polytetrafluoroethylene (NTF1122 manufactured by Nitto Denko, average pore size 0.2 μm) and tied with a kite string to obtain a test piece. Next, the weight A of the obtained test piece was measured. Weight A is the total weight of the small piece of the adhesive layer, the stretched porous film, and the kite string. The total weight B of the stretched porous film and the kite string used was measured in advance. Next, the test piece was immersed in a container with an internal volume of 50 mL filled with ethyl acetate and left to stand at 23 ° C. for one week. After standing, the test piece was taken out of the container and dried in a dryer set at 130 ° C. for two hours, and then the weight C of the test piece was measured. The gel fraction of the pressure-sensitive adhesive layer was calculated from the measured weights A, B, and C according to the formula: gel fraction (wt %)=(CB) / (AB)×100(%).

[0089] [Weight average molecular weight (Mw) of the sol content in the adhesive layer] The adhesive layer was dissolved in tetrahydrofuran to obtain a solution with a concentration of 0.2% by weight, which was left at room temperature for 20 hours.Then, the solution was filtered through a membrane filter with a filtration accuracy of 0.45 μm, and the weight average molecular weight (Mw) of the obtained filtrate was measured by GPC, and the obtained value was taken as the weight average molecular weight (Mw) of the sol content in the adhesive layer.The measurement conditions for GPC were the same as those for measuring the weight average molecular weight (Mw) of the (meth)acrylic polymer and the (meth)acrylic oligomer.

[0090] [Tensile modulus] The tensile modulus of the protective film was evaluated by a tensile test using a tensile tester (Shimadzu Corporation AG-IS). The shape of the sample was a strip of 15 mm width × 50 mm length, the initial chuck distance was 30 mm, and the tensile speed was 20 mm / min. The measurement was performed at 23°C.

[0091] [Dent amount] The degree of dents that may occur in the adhesive layer of the prepared optical laminate film was evaluated as "dent amount" as follows. A digital thickness gauge with a measuring stage (Digital Upright Gauge DG-205 manufactured by Ozaki Manufacturing Co., Ltd.) was prepared, and an iron ball with a diameter of 5.5 mm was fixed to the tip of the gauge head via double-sided adhesive tape (No. 500 manufactured by Nitto Denko Corporation). Next, the thickness gauge was operated to move the gauge head up and down, and the iron ball fixed to the tip of the gauge head was pressed against the measuring stage and released 10 times, and then the gauge head was lowered and the iron ball was pressed against the measuring stage with a constant load of 100 gf for 3 minutes, thereby sufficiently compressing the double-sided adhesive tape in the thickness direction and stabilizing the fixed state between the gauge head and the iron ball, so that a highly accurate measurement could be performed. Next, the position where the iron ball and the measuring stage contacted after the above treatment was set as the zero point. Next, the prepared optical laminate film was placed on the measuring stage so that the protective film was the exposed surface. Next, the thickness gauge was operated, the gauge was lowered, and the iron ball was pressed against the protective film with a constant load of 100 gf. The pressure applied to the protective film by the iron ball was about 2 MPa. The displacement of the iron ball from the zero point at the time when the iron ball contacted the protective film (0 seconds after pressing) and the displacement of the iron ball from the zero point at the time when 60 seconds had passed from that time (60 seconds after pressing) were measured by the thickness gauge, and the absolute value of the difference was taken as the dent amount, which is the amount of pressing in the thickness direction of the adhesive layer. The setting of the zero point and the evaluation of the dent amount were performed at 23°C.

[0092] Next, the method for producing each pressure-sensitive adhesive layer of the examples and comparative examples will be described.

[0093] The correspondence between the abbreviations or names and the compounds shown in the following explanation is as follows. BA: n-Butyl acrylate LA: Lauryl acrylate MA: Methyl acrylate NVP: N-vinylpyrrolidone AA: Acrylic acid HBA: 4-hydroxybutyl acrylate DCPMA: dicyclopentanyl methacrylate (Hitachi Chemical, FA-513M) HEA: 2-hydroxyethyl acrylate 2EHA: 2-Ethylhexyl acrylate MMA: Methyl methacrylate AIBN: 2,2'-azobisisobutyronitrile Omnirad651: 2,2-dimethoxy-2-phenylacetophenone (IGM Resins BV) Omnirad184: 1-Hydroxycyclohexyl phenyl ketone (IGM Resins BV) D110N: Trimethylolpropane / xylylene diisocyanate adduct (Takenate D110N manufactured by Mitsui Chemicals) C / L: Trimethylolpropane / tolylene diisocyanate (Coronate L made by Nippon Polyurethane Industry Co., Ltd.) A-HD-N: Hexanediol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.) Peroxide: Benzoyl peroxide (Niper BMT, manufactured by Nippon Oil & Fats) Irganox 1010: Pentaerythritol tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate) (manufactured by BASF)

[0094] [Preparation of (meth)acrylic polymer] (Synthesis Example 1) 99 parts by weight of BA and 1 part by weight of HBA were charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Next, 0.1 parts by weight of AIBN was added as a polymerization initiator to 100 parts by weight of a mixture of BA and HBA, and nitrogen gas was introduced while gently stirring to replace the atmosphere in the flask with nitrogen. The liquid temperature in the flask was kept at about 55°C, and the polymerization reaction was allowed to proceed for 7 hours. Next, ethyl acetate was added to the obtained reaction liquid to adjust the solid content concentration to 30% by weight, and a solution of (meth)acrylic polymer A1 was obtained. The weight average molecular weight (Mw) of the (meth)acrylic polymer A1 was 1.6 million.

[0095] (Synthesis Examples 2 and 3) (Meth)acrylic polymers A2 and A3 were obtained in the same manner as in Synthesis Example 1, except that the types and amounts of monomers and polymerization initiators shown in Table 1 below were charged into the flask.

[0096] [Preparation of (meth)acrylic monomer syrup] (Synthesis Example 4) In a four-neck flask equipped with a nitrogen gas inlet tube and a spindle connected to a B-type viscometer (rotational viscometer), 40 parts by weight of 2EHA, 50 parts by weight of LA, 9 parts by weight of NVP, 1 part by weight of HBA, and 0.05 parts by weight each of Ominirad651 and Omnirad184, which are photopolymerization initiators, were charged. Next, nitrogen gas was introduced into the flask while rotating the spindle to replace the atmosphere with nitrogen, and then photopolymerization was carried out by irradiating ultraviolet light until the viscosity of the polymerization system measured by the viscometer reached about 15 Pa·s, to obtain (meth)acrylic monomer syrup A4 containing a partial polymer of the monomer group. The viscometer used was a BH model manufactured by Toki Sangyo, and the rotation speed of the spindle (rotor No. 5) was set to 10 rpm. The liquid temperature in the flask was maintained at 30°C.

[0097] (Synthesis Example 5) A (meth)acrylic monomer syrup A5 was obtained in the same manner as in Synthesis Example 4, except that the types and amounts of monomers and photopolymerization initiators shown in Table 1 below were charged into the flask.

[0098] [Preparation of (meth)acrylic oligomer] (Synthesis Example 6) In a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser, 95 parts by weight of BA, 3 parts by weight of MA, 2 parts by weight of AA, 0.1 parts by weight of AIBN as a polymerization initiator, and 140 parts by weight of toluene were charged. Next, nitrogen gas was introduced while gently stirring to replace the atmosphere in the flask with nitrogen, and the liquid temperature in the flask was kept at about 70°C to allow the polymerization reaction to proceed for 8 hours, thereby obtaining a solution of (meth)acrylic oligomer B1. The weight average molecular weight of (meth)acrylic oligomer B1 was 4500.

[0099] (Synthesis Example 7) 60 parts by weight of DCPMA and 40 parts by weight of MMA as monomer components, 3.5 parts by weight of α-thioglycerol as a chain transfer agent, and 100 parts by weight of toluene as a polymerization solvent were mixed and stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by weight of AIBN was added as a thermal polymerization initiator, and the mixture was reacted at 70°C for 2 hours, and then heated to 80°C and reacted for 2 hours. Thereafter, the reaction liquid was heated to 130°C, and the toluene, chain transfer agent, and unreacted monomers were dried and removed to obtain a (meth)acrylic oligomer B2.

[0100] The compositions (monomer charging ratios) and weight average molecular weights (Mw) of the (meth)acrylic polymers, (meth)acrylic monomer syrups, and (meth)acrylic oligomers prepared in each synthesis example are shown in Table 1 below.

[0101] [Table 1]

[0102] [Preparation of adhesive layer] (Manufacturing Examples 1 to 8, 11) A solvent-based adhesive composition was obtained by mixing a (meth)acrylic polymer, a (meth)acrylic oligomer, a crosslinking agent, and additives to obtain the composition shown in Table 2 below. Next, the obtained adhesive composition was applied to the surface of a PET film (thickness 38 μm, 50 μm, or 75 μm) serving as a separator, and then dried for 2 minutes in an air-circulating thermostatic oven set at 155° C. to form the adhesive layers (thickness 50 μm) of Production Examples 1 to 8 and 11. A fountain coater was used to apply the adhesive composition.

[0103] (Examples 9 and 10) A mixture was obtained by mixing a (meth)acrylic monomer syrup, a crosslinking agent, and an additive to obtain the composition shown in Table 2 below. Next, the mixture was applied to the surface of a PET film (thickness 38 μm) that was a separator, and then another PET film was placed on the mixture coating, and the coating film was sandwiched between the pair of PET films. Next, the illuminance was 4 mW / cm. 2 and light intensity 1200mJ / cm2 The coating film was cured by irradiating with ultraviolet light under the irradiation conditions of: After the adhesive layer was formed, the additional PET film was peeled off to expose the adhesive layer.

[0104] [Table 2]

[0105] The evaluation results for each of the pressure-sensitive adhesive layers prepared in Production Examples 1 to 11 are shown in Table 3 below.

[0106] [Table 3]

[0107] [Preparation of optical laminated film] Based on the combinations shown in Table 4 below, the separator and adhesive layer prepared in Production Examples 1 to 11, the optical film, and the protective film were laminated in order to obtain optical laminated films of Examples 1 to 12 and Comparative Examples 1 to 3. However, in Comparative Example 1, the protective film was not arranged. For the optical film, a polarizing plate having a thickness of 31 μm was used, in which a polarizer protective film (thickness 20 μm), a polarizer (thickness 5 μm), a λ / 2 plate (½ wavelength plate, thickness 3 μm), and a λ / 4 plate (¼ wavelength plate, thickness 3 μm) were laminated in order from the side to be bonded to the protective film. For the protective film, a PET film (thickness 25 μm, 38 μm, or 50 μm) was used for Examples 1 to 12 and Comparative Example 3, and a polyethylene film (thickness 30 μm) was used for Comparative Example 2. The protective film was bonded to the optical film via an acrylic adhesive layer (thickness 10 μm). The layers constituting the optical film and the optical film were prepared as follows.

[0108] (λ / 4 plate and λ / 2 plate) The retardation film, which is a laminate of a λ / 4 plate (1 / 4 wavelength plate) and a λ / 2 plate (1 / 2 wavelength plate), was prepared using a polymerizable liquid crystal material (BASF, Paliocolor LC242) that exhibits a nematic liquid crystal phase after the formation of an alignment film. Specifically, the polymerizable liquid crystal material and a photopolymerization initiator (BASF, Irgacure 907) were dissolved in toluene, and then a fluorine-based surfactant (DIC, Megafac) was further added at 0.1 to 0.5% by weight depending on the liquid crystal thickness to improve coating properties, to prepare coating liquid L. The solid content concentration of coating liquid L was set to 25% by weight.

[0109] Next, a retardation film manufacturing apparatus 200 shown in FIG. 4 was prepared. The manufacturing apparatus 200 includes a supply reel 221 for supplying a strip-shaped PET substrate 214, pressure rollers 224, 234, shaping rollers 230, 240, peeling rollers 226, 236, a conveying roller 231, dies 222, 229, 232, 239, and ultraviolet irradiation devices 225, 227, 235, 237 for irradiating ultraviolet rays from a high-pressure mercury lamp. Next, a solution 210 of ultraviolet curable resin was applied to one side of the PET substrate 214 unwound from the supply reel 221 by the die 222. Next, the pressure roller 224 brought the coating film into contact with the shaping roller 230, and the PET substrate 214 was conveyed along the shaping roller 230 while both were in contact with each other, and the ultraviolet irradiation device 225 irradiated ultraviolet rays from the side of the PET substrate 214 to harden the coating film. On the conveying surface of the PET substrate 214 on the shaping roller 230, linear irregularities (extending in a direction at 75° to the MD direction of the PET substrate) that will form a λ / 4 plate when an alignment film of the polymerizable liquid crystal material is further formed are formed, and a cured film of ultraviolet curable resin having a shape corresponding to the irregularities on the exposed surface is formed by the curing. Next, the PET substrate 214 on which the cured film has been formed is peeled off from the shaping roller 230 by the peeling roller 226, and then the coating liquid L is applied to the exposed surface of the cured film by the die 229, and the coating film is aligned and cured by irradiating ultraviolet rays by the ultraviolet irradiation device 227. In this way, a λ / 4 plate (thickness 3 μm) consisting of a cured film of ultraviolet curable resin and an aligned and cured film of the polymerizable liquid crystal material is formed on the PET substrate 214.

[0110] Next, the PET substrate 214 on which the λ / 4 plate was formed was transported by the transport roller 231, and the solution 212 of the ultraviolet curable resin was applied to the exposed surface of the λ / 4 plate by the die 232 to form a coating film. Next, the pressure roller 234 brought the coating film into contact with the shaping roller 240, and the PET substrate 214 was transported along the shaping roller 240 while both were in contact, and the ultraviolet irradiation device 235 irradiated ultraviolet light from the side of the PET substrate 214 to harden the coating film. On the transport surface of the PET substrate 214 on the shaping roller 240, linear irregularities (extending in a direction at 15° to the MD direction of the PET substrate) were formed, which would form a λ / 2 plate when an alignment film of the polymerizable liquid crystal material was further formed, and a cured film of the ultraviolet curable resin having a shape corresponding to the irregularities on the exposed surface was formed by the curing. Next, the PET substrate 214 on which the cured film was formed was peeled off from the shaping roller 240 by the peeling roller 236, and then the coating liquid L was applied to the exposed surface of the cured film by the die 239, and the coating film was aligned and cured by irradiating it with ultraviolet light by the ultraviolet irradiation device 237. In this way, a λ / 2 plate (thickness 3 μm) consisting of a cured film of an ultraviolet curable resin and an aligned and cured film of a polymerizable liquid crystal material was further formed on the λ / 4 plate of the PET substrate 214, to obtain a laminate (b).

[0111] (Polarizing film) A polarizing film, which is a laminate of a polarizer and a polarizer protective film, was prepared as follows.

[0112] As a thermoplastic resin substrate, an amorphous IPA-copolymerized PET film (thickness 100 μm) containing 7 mol% of isophthalic acid (IPA) units was prepared, and its surface was corona-treated (58 W / m 2 / min) was applied. Separately, PVA (polymerization degree 4200, saponification degree 99.2%) to which 1% by weight of acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., Gohsefimer Z200, average polymerization degree 1200, saponification degree 98.5 mol%, acetoacetylation degree 5 mol%) was added was dissolved in water to obtain a PVA coating solution with a concentration of 5.5% by weight. Next, the above PVA coating solution was applied to the corona-treated surface of the IPA copolymerized PET film so that the film thickness after drying was 12 μm, and the coating film was dried for 10 minutes by hot air drying at 60 ° C. to obtain a laminate consisting of a substrate and a PVA layer on the substrate.

[0113] Next, the obtained laminate was free-end stretched (air-assisted stretching) at a stretch ratio of 1.8 times at 130°C in air to obtain a stretched laminate. Next, the stretched laminate was immersed in a boric acid insolubilizing aqueous solution at a liquid temperature of 30°C for 30 seconds to insolubilize the PVA layer. The content of boric acid in the boric acid insolubilizing aqueous solution was 3 parts by weight per 100 parts by weight of water. Next, the stretched laminate with the PVA layer insolubilized was dyed to obtain a colored laminate. The dyeing was performed by immersing the stretched laminate in a dyeing solution containing iodine and potassium iodide at a liquid temperature of 30°C. In the dyeing, the PVA layer included in the stretched laminate was dyed with iodine. The dyeing time was adjusted so that the single transmittance of the PVA layer constituting the finally obtained polarizer was in the range of 40 to 44%. For the dyeing solution, an aqueous solution with an iodine concentration of 0.1 to 0.4% by weight and a potassium iodide concentration of 0.7 to 2.8% by weight was used. The ratio of the potassium iodide concentration to the iodine concentration in the dye solution was set to 7. Next, the colored laminate was immersed in a boric acid crosslinking aqueous solution at a liquid temperature of 30°C for 60 seconds to perform a crosslinking treatment to form a crosslinked structure between PVA molecules in the PVA layer that adsorbed iodine. The boric acid content and potassium iodide content in the boric acid crosslinking aqueous solution were both 3 parts by weight per 100 parts by weight of water.

[0114] Next, the colored laminate after the crosslinking treatment was stretched in a boric acid aqueous solution at a stretching temperature of 70°C and a stretching ratio of 3.05 times (stretching in boric acid water) to obtain a stretched laminate with a final stretching ratio of 5.50 times. The stretching direction of the stretching in boric acid water was the same as the stretching direction of the first air-assisted stretching. Next, the stretched laminate after stretching was taken out of the boric acid aqueous solution, and the boric acid attached to the surface of the PVA layer was washed with a potassium iodide solution (potassium iodide content was 4 parts by weight per 100 parts by weight of water). Next, the stretched laminate after washing was dried by hot air drying at 60°C to obtain a laminate of the substrate and the polarizer (thickness 5 μm) formed on the substrate.

[0115] Next, a stretched film of a methacrylic resin having a glutarimide ring unit (thickness: 20 μm, moisture permeability: 160 g / m2) was used as a polarizer protective film. 2 ) was prepared. Next, the prepared polarizer protective film was bonded to the exposed surface of the polarizer in the laminate prepared above, to obtain a laminate (c) of the substrate and the polarizing film having the polarizer and the polarizer protective film. A known acrylic adhesive was used to bond the polarizer and the polarizer protective film.

[0116] Next, an optical film was produced using the laminate (b) and laminate (c) produced above as follows. First, the substrate was peeled off from the laminate (c) to expose the polarizer. Next, the exposed polarizer and the λ / 2 plate of the laminate (b) were bonded with a known acrylic adhesive to obtain an optical film. The bonding between the optical film and the pressure-sensitive adhesive layer was performed by peeling off the PET substrate 214 from the laminate (b) to expose the λ / 4 plate.

[0117] Table 4 below shows the configurations of the optical layered films of the Examples and Comparative Examples and the evaluation results thereof.

[0118] [Table 4]

[0119] As shown in Table 4, the amount of depression was reduced in the optical layered films of the examples. [Industrial Applicability]

[0120] The pressure-sensitive adhesive layer-attached optical laminate film of the present invention can be used in the production of an image display device. [Explanation of symbols]

[0121] 1. Optical laminated film with adhesive layer 2 Protective film 3. Optical Film 4 Adhesive layer 5. Separator 6 Image display devices 7 Image forming layer (organic EL layer) 8 Substrate

Claims

1. A pressure-sensitive adhesive layer-attached optical laminate film in which a protective film, an optical film, a pressure-sensitive adhesive layer, and a separator are laminated in this order, The optical film has a thickness of 80 μm or less, The thickness of the protective film is 30 μm or more and 50 μm or less, and the tensile modulus of the protective film is 1 GPa or more, The pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer formed from an acrylic pressure-sensitive adhesive composition.

2. The pressure-sensitive adhesive layer-attached optical laminate film according to claim 1 , wherein the protective film is a polyester film.

3. The pressure-sensitive adhesive layer-attached optical laminate film according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has a thickness of 25 μm or more.

4. 4. The pressure-sensitive adhesive layer-attached optical laminate film according to claim 1, wherein the separator has a thickness of 45 μm or more.

5. The pressure-sensitive adhesive layer-attached optical laminate film according to any one of claims 1 to 4, wherein the pressure-sensitive adhesive layer has a gel fraction of 60% or more.

6. 6. The pressure-sensitive adhesive layer-attached optical laminate film according to claim 1, wherein the weight average molecular weight (Mw) of the sol content in the pressure-sensitive adhesive layer is 50,000 or more.

7. 7. The pressure-sensitive adhesive layer-attached optical laminate film according to claim 1, wherein the pressure-sensitive adhesive layer has a creep amount ΔCr of 50 μm or less at 70° C. as determined by the following test. Test: A pressure-sensitive adhesive layer is attached to a stainless steel test plate at a joint surface of 20 mm long x 20 mm wide. With the test plate fixed, a load of 500 gf is applied vertically downward. The creep amount (displacement amount) of the pressure-sensitive adhesive layer with respect to the test plate is measured at 100 seconds and 3600 seconds after the start of the load application, and the Cr 100 and Cr 3600 The measured Cr 100 and Cr 3600 From the formula ΔCr = Cr 3600 -Cr 100 The creep amount ΔCr is calculated by the following equation.

8. 8. An image display device comprising a portion of the pressure-sensitive adhesive layer-attached optical laminate film according to claim 1 excluding the separator.

Citation Information

Patent Citations

  • Polarizing plate, manufacturing method therefor, and composite polarizing plate using the same

    JP2010039458A

  • Composite polarizing plate and liquid crystal display

    JP2013011853A

  • Removal method of release film and manufacturing method of optical display panel

    JP2017181789A

  • Laminate for flexible image display device and flexible image display device

    JP2018028573A

  • Optical laminate and image display device

    JP2018120119A