Copper-coated iron powder, manufacturing method for copper-coated iron powder, and method for recovering ruthenium

Copper-coated iron powder addresses inefficiencies in ruthenium recovery by suppressing arsine gas generation and enhancing recovery efficiency, providing a cost-effective solution for selective ruthenium extraction.

JP7594420B2Active Publication Date: 2024-12-04JX NIPPON MINING & METALS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020200391
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-02
Publication Date
2024-12-04
Estimated Expiration
2040-12-02

AI Technical Summary

Technical Problem

Existing methods for recovering ruthenium from acidic solutions containing arsenic are inefficient and pose risks of generating toxic arsine gas due to the use of metals like zinc, magnesium, and aluminum, and uncoated copper poses cost issues and inefficiencies in acid dissolution.

Method used

Copper-coated iron powder is used to selectively recover ruthenium by coating the surface of iron powder with copper, which suppresses arsine gas generation and enhances recovery efficiency.

Benefits of technology

The copper-coated iron powder effectively recovers ruthenium from acidic solutions while minimizing arsine gas production and reducing copper costs, achieving high purity and selective recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594420000006
    Figure 0007594420000006
  • Figure 0007594420000007
    Figure 0007594420000007
  • Figure 0007594420000008
    Figure 0007594420000008
Patent Text Reader

Abstract

To provide a copper-coated iron powder, a copper-coated iron powder producing method and a ruthenium recovering method, capable of selectively recovering ruthenium from an acidic solution containing ruthenium and arsenic.SOLUTION: A copper-coated iron powder for ruthenium cementation comprises an iron powder coated with copper at a surface and allows for selectively depositing ruthenium from an acidic solution containing ruthenium and arsenic.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to copper-coated iron powder, a method for producing the copper-coated iron powder, and a method for recovering ruthenium. [Background technology]

[0002] In copper pyrometallurgy, copper concentrate is melted and processed into crude copper with a purity of 99% or more in a converter and a refining furnace, after which electrolytic refining produces electrolytic copper with a purity of, for example, 99.99% or more. In recent years, metal scraps containing precious metals from electronic parts have been input as recycled raw materials into the converter, and valuable materials other than copper are precipitated as slime during electrolytic refining.

[0003] This slime also contains precious metals, rare metals, and the selenium and tellurium contained in copper concentrate. These elements are separated and recovered individually as by-products of copper smelting.

[0004] In many cases, hydrometallurgy is used to treat this slime. For example, Patent Document 1 discloses a method in which silver is recovered from slime using hydrochloric acid-hydrogen peroxide, dissolved gold is recovered by solvent extraction, and other valuables are subsequently reduced and recovered using sulfur dioxide. Patent Document 2 discloses a method in which gold and silver are recovered using a similar method, and then valuables are reduced and precipitated using sulfur dioxide, and only selenium is removed by distillation to concentrate precious metals.

[0005] The solution after the precious metals are recovered contains rare metal ions, tellurium, and selenium, and it is necessary to further recover these valuable materials. Known recovery methods include recovering the precipitate generated by the reduction agent, mixing the solution with copper concentrate, drying it with a dryer, and then returning it to the smelting furnace. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-316735 A [Patent Document 2] JP 2016-160479 A [Patent Document 3] JP 2019-147990 A Summary of the Invention [Problem to be solved by the invention]

[0007] The method of recovering precipitates produced by sulfur dioxide, as shown in Patent Document 1, has many advantages in terms of cost and production scale. In addition, since each element precipitates sequentially, it is also effective for separation and purification.

[0008] In the method of recovering valuables using sulfur dioxide, valuables can be recovered by successive reduction of the metals after dissolution. Platinum and palladium precipitate first. Selenium is then reduced. Iridium, ruthenium, and rhodium have relatively low redox potentials and are less susceptible to reduction, so they remain in the solution until the end. Ruthenium in the solution is generally recovered as ruthenium dioxide by distillation after oxidizing it with a strong oxidizing agent such as bromic acid.

[0009] Patent Document 3 discloses a method in which the ruthenium remaining in the solution until the end is cemented with metallic copper. By using copper as the metal used for cementation, it is possible to prevent the coexisting arsenic from being generated as arsine gas.

[0010] Cementation is a relatively simple method that does not require large-scale equipment and is effective even when the concentration of ruthenium is low. Therefore, it is an effective method for separating and concentrating ruthenium from other elements before refining.

[0011] In order to increase the purity of crude ruthenium before refining, it is necessary to first roughly separate and concentrate the ruthenium species in a harmless form. During concentration, the solution is reduced to recover ruthenium and other elements as a precipitate. The other elements that are commonly used are selenium, tellurium, and rhodium.

[0012] As disclosed in Patent Document 3, ruthenium can be recovered as crude ruthenium by cementation with copper. However, it is necessary to remove copper from the recovered ruthenium-containing precipitate, which must be dissolved in sulfuric acid. Copper needs to be heated when dissolved in sulfuric acid, and the surface of unreacted copper is covered with substances such as selenium and tellurium precipitated by cementation, so acid dissolution reaction is not said to be efficient. It is preferable to bring in as little copper as possible to the precipitate treatment process.

[0013] Furthermore, copper is a relatively expensive metal. When used in cementation, the cost cannot be ignored. However, typical base metals such as zinc and aluminum may react with arsenic under acidic conditions to generate arsine gas. Also, metals that react with acid to generate hydrogen may generate hydrogen suddenly when added, which may cause an overflow.

[0014] In view of the above-mentioned conventional circumstances, the present invention provides a copper-coated iron powder capable of selectively recovering ruthenium from an acidic solution containing ruthenium and arsenic, a method for producing the copper-coated iron powder, and a method for recovering ruthenium, which are particularly suitable for a solution containing dissolved electrolytic sediment generated in the electrolytic refining process in copper smelting. [Means for solving the problem]

[0015] As a result of intensive research conducted by the present inventors in order to solve the above problems, it has been found that it is possible to recover ruthenium by cementing an acidic solution containing ruthenium and arsenic with copper-coated iron powder. (1) A copper-coated iron powder for ruthenium cementation, characterized in that the surface of the iron powder is coated with copper, and that ruthenium can be selectively precipitated from an acidic solution containing ruthenium and arsenic. (2) The copper-coated iron powder according to (1), characterized in that the copper content is 10 to 80 mass %. (3) The copper-coated iron powder according to (1) or (2), characterized in that the bulk density is 60% or less of the bulk density of iron powder having the same particle size as the copper-coated iron powder. (4) The copper-coated iron powder according to any one of (1) to (3), characterized in that the bulk density is 1.3 g / ml or less. (5) The copper-coated iron powder according to any one of (1) to (4), characterized in that P80 is 100 μm to 5 mm. (6) The copper-coated iron powder according to any one of (1) to (5), characterized in that when immersed in 1 mol / L hydrochloric acid at 30°C and stirred, the iron dissolution rate per added mass is calculated as the slope of the regression line up to the time at which the iron concentration reaches the midpoint of the saturation concentration, and is 4.0 mass% / min or less of the copper-coated iron powder. (7) A method for producing copper-coated iron powder for cementing valuable materials from an acidic solution containing at least one of ruthenium, selenium, and tellurium, and arsenic, the method comprising the steps of: A method for producing copper-coated iron powder, comprising the step of contacting iron powder with an aqueous solution of pH 5 or less containing a water-soluble copper salt to coat the surface of the iron powder with copper. (8) The method for producing a copper-coated iron powder according to (7), wherein the aqueous solution containing the water-soluble copper salt has a copper concentration of 2 to 40 g / L. (9) The method for producing a copper-coated iron powder according to (7) or (8), wherein the aqueous solution containing the water-soluble copper salt has a copper concentration of 0.15 to 3.0 times by mass the iron concentration. (10) The method for producing a copper-coated iron powder according to any one of (7) to (9), characterized in that the aqueous solution containing the water-soluble copper salt is brought into contact with the iron powder while adjusting the liquid temperature to 20 to 60°C. (11) The method for producing a copper-coated iron powder according to any one of (7) to (10), wherein the iron powder has a P80 of 150 μm or less. (12) A method for producing a copper-coated iron powder according to any one of (7) to (11), characterized in that a reaction time of the contact is adjusted so that the bulk density of the iron powder having the same particle size as the iron powder having the copper-coated surface is 60% or less of the bulk density of the iron powder. (13) The method for producing a copper-coated iron powder according to any one of (7) to (12), characterized in that the aqueous solution containing the water-soluble copper salt is continuously supplied to a container containing the iron powder, thereby bringing the iron powder into contact with the aqueous solution containing the water-soluble copper salt. (14) A method for recovering ruthenium, comprising the steps of: adjusting the liquid temperature of an acidic solution containing ruthenium and arsenic to 20°C or higher and 80°C or lower using the copper-coated iron powder according to any one of (1) to (6); and contacting the copper-coated iron powder and arsenic in the liquid to precipitate ruthenium. Effect of the Invention

[0016] According to the embodiments of the present invention, it is possible to provide a copper-coated iron powder capable of selectively recovering ruthenium from an acidic solution containing ruthenium and arsenic, a method for producing the copper-coated iron powder, and a method for recovering ruthenium. [Brief description of the drawings]

[0017] [Figure 1] 1 is a graph plotting the amount of ruthenium precipitation / the amount of arsenic precipitation for each copper grade of copper-coated iron powder according to an experimental example. [Diagram 2] 1 is a graph plotting the amount of ruthenium precipitation / the amount of arsenic precipitation for each bulk density of copper-coated iron powder according to an experimental example. [Diagram 3] 1 is a graph plotting the change in iron concentration over time when copper-coated iron powders prepared with various copper concentrations are dissolved in hydrochloric acid according to an experimental example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] <Copper-coated iron powder> The copper-coated iron powder according to the embodiment of the present invention is used for ruthenium cementation. The copper-coated iron powder according to the embodiment of the present invention is an iron powder whose surface is coated with copper, and is capable of selectively precipitating ruthenium from an acidic solution containing ruthenium and arsenic. Cementation with Fe is the best way to recover ruthenium more quickly and efficiently. Fe + Ru 2+ → Fe 2+ + Ru However, in acidic solutions containing arsenic, the iron reacts with the acid to generate hydrogen, which then reacts with the arsenic to generate arsine gas. 3Fe + H3AsO3 + 6H+ → 3Fe 2+ + H3As + 3H2O On the other hand, even when copper is in an acidic solution containing arsenic, copper arsenide is produced and arsine gas is not generated. 6Cu + 2H3AsO3 + 6H + → 2Cu3As + 6H2O Therefore, if copper is present near the iron, the concentration of arsenic in the solution in contact with the iron will decrease due to the copper, making it possible to suppress the generation of arsine and recover ruthenium. Copper-coated iron powder, in which the surface of the iron is coated with copper, is effective.

[0019] The copper-coated iron powder according to the embodiment of the present invention preferably has a copper content of 10 to 80% by mass. If the copper content in the copper-coated iron powder is less than 10% by mass, there is a risk of arsine being generated by hydrogen generated during use of the copper-coated iron powder. If the copper content in the copper-coated iron powder is more than 80% by mass, the effect becomes almost the same as that of copper powder, and the advantages of a low reaction temperature, easy disposal of unreacted matter, and low price are lost. The copper-coated iron powder according to the embodiment of the present invention more preferably has a copper content of 30 to 65% by mass.

[0020] The bulk density of the copper-coated iron powder according to the embodiment of the present invention is preferably 60% or less of the bulk density of iron powder having the same average particle size as the iron powder having a copper-coated surface. The bulk density indicates the density when the powder is filled to the brim in a container of a certain volume, and the internal volume is taken as the volume. If the iron is in the form of a powder, the surface irregularities can be quantified as the bulk density. If the bulk density of the copper-coated iron powder is 60% or less of the bulk density of iron powder having the same average particle size as the iron powder having a copper-coated surface, the copper-coated iron powder has high reaction efficiency. It is more preferable that the bulk density of the copper-coated iron powder according to the embodiment of the present invention is 50% or less of the bulk density of iron powder having the same average particle size as the iron powder having a copper-coated surface.

[0021] The copper-coated iron powder according to the embodiment of the present invention preferably has a bulk density of 1.3 g / ml or less. When the copper-coated iron powder according to the embodiment of the present invention has a bulk density of 1.3 g / ml or less, the cementation efficiency is improved, and further, the separation efficiency of ruthenium and arsenic is improved. The bulk density of the copper-coated iron powder is more preferably 1.0 g / ml or less.

[0022] The copper-coated iron powder according to the embodiment of the present invention preferably has a P80 of 100 μm to 5 mm. When the copper-coated iron powder has a P80 of 100 μm or more, it can be uniformly dispersed in a solution during a reaction. When the copper-coated iron powder has a P80 of 5 mm or less, a high reaction rate is exhibited. The copper-coated iron powder according to the embodiment of the present invention more preferably has a P80 of 180 μm to 1 mm.

[0023] In the copper-coated iron powder according to the embodiment of the present invention, "iron powder" generally refers to iron powder having a particle size of several hundred micrometers or less. The iron powder before copper coating according to the embodiment of the present invention is not special, and commercially available iron powder can be used. In addition, the copper-coated iron powder according to the embodiment of the present invention is not particularly restricted in particle size because it is used for cementation of ruthenium, but it is preferable that it has a particle size that can be widely dispersed when stirred. Metallic iron classified as particles having a particle size of 10 mm or less can also be used if the surface is coated with copper, and in the embodiment of the present invention, these are referred to as "iron powder".

[0024] The electrolytic sediment produced during the electrolytic refining process of non-ferrous metal smelting, especially copper smelting, is concentrated with platinum group elements, heavy metals, and toxic elements. Platinum group elements and toxic elements are never smelted separately, but are recovered as by-products of other metals or separated from recycled materials such as waste catalysts. Therefore, this method can also be applied to recycling from waste materials.

[0025] The electrolytic precipitate can be dissolved by adding hydrochloric acid and hydrogen peroxide, but the silver immediately dissolves and forms an insoluble silver chloride precipitate with chloride ions. If a solution containing an oxidizing agent and chlorine, such as aqua regia or chlorine water, is used, the precious metals will dissolve and the silver can be separated as silver chloride. The pregnant leach solution (PLS) contains platinum group elements, rare metal elements, chalcogen elements, arsenic, antimony, etc.

[0026] The pregnant leach solution (PLS) is cooled, and the chlorides of base metals such as lead and antimony are precipitated and separated. The gold is then separated into an organic phase by solvent extraction. Dibutyl carbitol (DBC) is the most commonly used gold extractant.

[0027] Valuable materials can be precipitated and recovered by reducing the PLS after gold extraction, but because the redox potential differs depending on the element, the order of precipitation is naturally determined. Gold, platinum, and palladium precipitate first, followed by chalcogens such as selenium and tellurium, and then inactive precious metals such as ruthenium and iridium. Elements with low redox potentials, such as arsenic, do not precipitate and are treated directly in the waste liquid treatment process.

[0028] Reducing sulfur is used as a reducing agent in terms of cost and efficiency, and sulfur dioxide is the most suitable, since it can be supplied in large quantities and at low cost by roasting converter gas and sulfide ores. The reduction rate of inert precious metals is extremely slow with sulfur dioxide and sulfite. The content is not high to begin with, for example, ruthenium in copper electrolytic precipitate solution is about 150-300 mg / L, and it cannot be purified by distillation as it is, so it needs to be concentrated once. In the current process, ruthenium is precipitated with sulfur dioxide and re-dissolved. The ruthenium recovery rate at this time is about 30-50% after a reaction time of 6-8 hours, but it is expected that more than 10 hours will be required to completely precipitate it. This is too long and is not a realistic reaction time.

[0029] Therefore, the most efficient way to precipitate ruthenium is by cementation with a metal. It is known that ruthenium can be reduced to metallic ruthenium by metals such as zinc, magnesium, and aluminum that generate hydrogen in the presence of acid.

[0030] However, in an acidic solution containing arsenic, the above metals react with arsenic to generate arsine gas. Alternatively, there is a risk that nascent hydrogen may generate arsine gas. For this reason, cementation using copper is effective, but in the embodiment of the present invention, copper-coated iron powder is used, in which the surface of the iron powder is coated with copper, in order to address the issues of unreacted copper and cost. By coating the surface of iron with copper, almost no nascent hydrogen is generated, making it possible to selectively recover ruthenium from an acidic solution containing ruthenium and arsenic.

[0031] When copper electrolytic sediment is dissolved in acid, the ruthenium concentration in the solution is generally 150-300mg / L and the arsenic concentration is about 0.5-2.0g / L, although this depends on the conditions. The copper electrolytic sediment dissolution solution is 15ml per treatment. 3 When sulfur dioxide is used as a reducing agent, the ruthenium recovery rate is about 30 to 50% after a reaction time of 6 to 8 hours. The copper-coated iron powder according to the embodiment of the present invention may be used after a portion of the ruthenium is recovered with sulfur dioxide, or may be charged without recovering ruthenium with sulfur dioxide.

[0032] Ruthenium undergoes cementation with both iron and copper. In terms of the redox potential, cementation with iron is efficient, but in an acidic solution containing arsenic, hydrogen generated by reaction with iron may generate highly toxic arsine gas, which is a concern. In contrast, the copper-coated iron powder according to the embodiment of the present invention makes it possible to suppress the generation of arsine gas.

[0033] The copper on the surface of the copper-coated iron powder gradually dissolves in the sulfuric acid solution. The dissolved areas regenerate the iron surface. Ruthenium is cemented on this regenerated iron surface. Alternatively, copper is precipitated again to cover the iron, and the arsenic generation reaction has a low priority and can be hardly considered.

[0034] The copper-coated iron powder according to the embodiment of the present invention can be easily dissolved with a mineral acid such as sulfuric acid even if unreacted parts are mixed into the recovered ruthenium when an excessive amount is added. After cementation, the excess iron can be removed by acid washing to further increase the purity of the ruthenium.

[0035] If there is a risk that some arsine may be generated even with copper-coated iron powder, it is preferable to adjust the copper concentration of the solution to 0.05 g / L or more in advance. With this configuration, even if arsine is generated, it can react with copper ions and be trapped as copper arsenide. The copper concentration can be adjusted with water-soluble copper salts such as copper sulfate (II) and copper chloride (II), and a copper electrolyte may be added. As the reaction progresses, the copper that coated the surface of the iron powder dissolves, so there is no need to add more copper during the reaction.

[0036] The degree to which the copper-coated iron powder according to the embodiment of the present invention is coated with copper can be evaluated by the dissolution rate of iron in an acidic solution. If the coating is small, the dissolution rate of iron is high, and if the coating is large, the dissolution rate is low. In the present invention, a specific index is the iron dissolution rate per added mass when immersed and stirred in 1 mol / L hydrochloric acid at 30° C. The rates were then compared by calculating the slope of the regression line up to the time when the iron concentration reached the intermediate value of the saturation concentration (the average value between the maximum iron concentration and the minimum iron concentration excluding zero). As for the iron dissolution rate, if the slope of the regression line of the copper-coated iron powder is 4.0 mass% / min or less, it is considered sufficient for the copper-coated iron powder to exhibit the effects of the present invention. Therefore, the slope of the regression line is 4.0 mass% / min or less, more preferably 2.5 mass% / min or less.

[0037] <Method of manufacturing copper-coated iron powder> The method for producing copper-coated iron powder according to an embodiment of the present invention is a method for producing copper-coated iron powder for cementing valuables from an acidic solution containing at least one of ruthenium, selenium, and tellurium as valuables, and arsenic. The method for producing copper-coated iron powder according to an embodiment of the present invention includes a step of contacting iron powder with an aqueous solution containing a water-soluble copper salt and having a pH of 5 or less, to coat the surface of the iron powder with copper.

[0038] The simplest way to coat the surface with copper is to immerse the iron in a solution of water-soluble copper salts such as copper sulfate (II) or copper chloride (II). Iron particles or iron blocks can also be used, but iron powder is the most reactive when recovering ruthenium in a batch reactor. The reaction principle is the same as long as the surface of the iron is coated with copper, so it is also possible to prepare copper-coated iron of various shapes and pass the target liquid continuously through them.

[0039] The aqueous solution containing a water-soluble copper salt may be prepared by using an aqueous sulfuric acid solution and a water-soluble copper salt, but it may also be used by adjusting the acid concentration of industrial waste liquid containing copper, such as an electrolytic copper foil treatment solution or an etching waste liquid.

[0040] The aqueous solution containing the water-soluble copper salt is brought into contact with the iron powder at a pH of 5 or less. When the aqueous solution containing the water-soluble copper salt is alkaline, the iron substituted with copper is oxidized and precipitates on the surface of the iron powder. This iron oxide is inactive in the cementation of ruthenium, and the reaction efficiency decreases. In the method for producing copper-coated iron powder according to the embodiment of the present invention, as described above, the aqueous solution containing the water-soluble copper salt is brought into contact with the iron powder at a pH of 5 or less, so that the generation of such iron oxide is effectively suppressed and the reaction efficiency of the cementation of ruthenium is improved.

[0041] The aqueous solution containing the water-soluble copper salt preferably has a pH of 2 or less. If the aqueous solution containing the water-soluble copper salt has a pH of 2 or less, hydrogen bubbles are generated from the surface of the iron powder when copper is precipitated on the surface, and when the copper and iron are replaced, the surface becomes uneven, increasing the surface area. The increased surface area improves the reaction efficiency in the cementation of ruthenium.

[0042] The time for which the iron powder is brought into contact with the aqueous solution of pH 5 or less containing a water-soluble copper salt and allowed to react is preferably adjusted so that the bulk density of the copper-coated iron powder is 60% or less of the bulk density of iron powder of the same particle size as the iron powder whose surface is coated with copper. This allows the production of copper-coated iron powder with better reaction efficiency.

[0043] The iron powder may be commercially available iron powder, but the size is preferably one having a P80 of 150 μm or less. In this specification, "P80" refers to the particle size at which 80% passes through a sieve. When the iron powder has a P80 of 150 μm or less, the recovered copper-coated iron powder has high reactivity. It is more preferable that the iron powder has a P80 of 120 μm or less.

[0044] The aqueous solution containing the water-soluble copper salt preferably has a copper concentration of 2 to 40 g / L. If the copper concentration of the aqueous solution containing the water-soluble copper salt exceeds 40 g / L, the copper grade of the copper-coated iron powder may be high, and the recovery efficiency of ruthenium may be reduced. If the copper concentration of the aqueous solution containing the water-soluble copper salt is less than 2 g / L, the copper grade of the copper-coated iron powder may be low, and the amount of arsenic mixed into the valuable material to be recovered may be increased. The aqueous solution containing the water-soluble copper salt more preferably has a copper concentration of 2 to 10 g / L.

[0045] When covering the surface of iron powder with copper, if a batch reaction is used in a tank, it is preferable to set the copper concentration to 0.15 to 3.0 times the mass of iron. In the case of a continuous reaction in which an aqueous solution of copper salt is passed through iron packed in a tubular reactor, the copper concentration should be as described above, and the end point of the covering reaction should be when the discharged copper concentration becomes 1 g / L or less.

[0046] The aqueous solution containing the water-soluble copper salt is preferably adjusted to a temperature of 20 to 60°C before contacting with the iron powder. That is, the temperature (reaction temperature) of the aqueous solution containing the water-soluble copper salt during the production of the copper-coated iron powder is preferably 20 to 60°C. If the reaction temperature exceeds 60°C, a large amount of hydrogen may be suddenly generated, which may cause a safety problem. If the reaction temperature is lower than 20°C, the reaction efficiency may decrease. Since the reaction of iron with acid generates reaction heat, it is more preferable to set the reaction temperature to 20 to 40°C from the viewpoint of reaction stability.

[0047] In the step of contacting iron powder with an aqueous solution containing a water-soluble copper salt to coat the surface of the iron powder with copper, the aqueous solution containing the water-soluble copper salt may be continuously supplied to a container containing the iron powder, thereby contacting the iron powder with the aqueous solution containing the water-soluble copper salt. By continuously supplying the aqueous solution containing the water-soluble copper salt in this manner, an appropriate amount of copper can be precipitated on the iron surface even when a solution with a low copper concentration is used.

[0048] After the reaction, the copper-coated iron powder recovered can be separated by an appropriate method. Generally, filtration with a filter press is used, but it is also possible to separate it by magnetic force. The produced copper-coated iron powder can be used without drying.

[0049] Furthermore, ruthenium can be recovered by adjusting the liquid temperature of an acidic solution containing ruthenium and arsenic to 20°C or higher and 80°C or lower, and contacting the copper-coated iron powder prepared as described above in the acidic solution to precipitate ruthenium. EXAMPLES

[0050] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these.

[0051] (Experimental Example 1) Copper was removed from the electrolytic sediment recovered from the copper electrorefining process of copper smelting using sulfuric acid. Concentrated hydrochloric acid and 60% hydrogen peroxide were added to dissolve the precipitate, and solid-liquid separation was performed to obtain PLS (pregnant leach solution). The PLS was cooled to 6°C to precipitate and remove the base metals. The acid concentration was adjusted to 2N or more, and DBC (dibutyl carbitol) and PLS were mixed to extract gold. After gold extraction, the PLS was heated to 70°C, and a mixture of sulfur dioxide and air (sulfur dioxide concentration 5-20%) was blown in to reduce the precious metals and selenium, resulting in solid-liquid separation. The selenium concentration of the solution after selenium separation was 6mg / L, tellurium concentration 18mg / L, ruthenium concentration 130mg / L, copper concentration 0.55g / L, and arsenic concentration 1.5g / L. 3-30g of copper sulfate pentahydrate was weighed out and dissolved in 200ml of sulfuric acid at pH 0.5. 3g of iron powder (P80=150μm) was added and stirred. After 20-60 seconds, the mixture was filtered to separate the solid and liquid, and copper-coated iron powder with the specified bulk density and copper content was obtained. It was then washed with water, then with ethanol, and air-dried.

[0052] An appropriate amount of copper-coated iron powder was placed in a measuring cylinder and the volume and weight were measured. The measurement was repeated five times, and the bulk density was calculated from the slope of the weight versus volume. The measuring cylinder was not tapped when measuring the bulk density.

[0053] Next, 200 ml of the post-selenium separation liquid (an acidic solution containing ruthenium and arsenic from which ruthenium is to be recovered) was measured and 0.8 g of copper sulfate pentahydrate was added. 1 g of copper-coated iron powder prepared by heating to 50°C to 55°C was added. After 30 minutes and 60 minutes, analytical samples were taken and the reaction was terminated. The precipitate was filtered and dried, and then its weight was measured.

[0054] As Comparative Example 1, cementation was carried out by heating 1 g of copper powder to 75° C. to 80° C. As Comparative Example 2, cementation was also attempted by adding 1 g of iron powder together with 3.5 g of copper sulfate pentahydrate at 50° C.

[0055] 2 ml of the test sample was taken and adjusted to 50 ml. The concentrations of ruthenium, arsenic, and copper in the solution were quantified using ICP-OES (Seiko SPS3100). For the analysis of the residue, about 0.1 g was measured and dissolved in aqua regia, and the concentrations were measured using ICP-OES to calculate the amounts of copper and arsenic precipitation. An example of the results is shown in Table 1. Figures 1 and 2 show graphs plotting the amount of ruthenium precipitation / arsenic precipitation according to the copper content and bulk density of all copper-coated iron powder obtained under each condition. The reason for using the amount of ruthenium precipitation / arsenic precipitation in the plot is that a large ratio means that the reaction of ruthenium precipitation occurs preferentially, and a small ratio means that the reaction of arsenic precipitation occurs preferentially, making it easy to understand the balance between the two reactions.

[0056] [Table 1]

[0057] In Examples 1 to 6, the concentration of ruthenium in the solution was significantly reduced, and all of them were comparable to the copper powder of Reference Example 1. It was also found that the coated iron powder was more effective than the uncoated iron powder of Reference Example 2.

[0058] On the other hand, the amount of arsenic precipitation was smaller in all of Examples 1 to 6 than in Reference Example 1, and there is a tendency that the amount of arsenic precipitation decreases as the copper content in the copper-coated iron powder increases. Also, as can be seen from Figure 1, the amount of arsenic derived from the raw material solution was 300 mg, but the copper content in the copper-coated iron was 10 to 70%, and the arsenic precipitation rate was 25% or less, indicating that arsenic precipitation was sufficiently suppressed.

[0059] Figure 1 shows that there is a positive correlation between the copper content and the ruthenium / arsenic ratio in the precipitate. In the range of copper content from 10% to 80%, the separation efficiency increases linearly as the copper content of the copper-coated iron powder used for cementation increases.

[0060] In Examples 1 to 6, various bulk densities were produced, which are related to the acid and copper ion concentration when copper is precipitated. When the bulk density is large, the mass of the recovered residue tends to increase. A large mass of the recovered residue means that it contains more impurities other than valuable metals such as ruthenium.

[0061] According to Examples 1 to 6, the copper-coated iron powder was highly effective when the bulk density was 1.3 g / ml or less. Figure 2 shows that the effect of separating and recovering arsenic and ruthenium does not change when the bulk density exceeds 1.0 g / ml. Since the bulk density of the original iron powder was 2.32 g / ml, it is sufficient to coat the iron powder with copper so that the bulk density becomes 60% or less of the original iron powder.

[0062] (Experimental Example 2) 3 g of commercially available iron powder (Wako Pure Chemical Industries, P80 = 150 μm) was weighed out. 15 g of copper sulfate pentahydrate was added to various sulfuric acid aqueous solutions with acid concentrations ranging from pH 5 to 3N as shown in Table 2, and dissolved (copper concentration 19 g / L) and mixed with the iron powder. After stirring for 20 seconds, the solution was filtered and washed with water. The solution was rinsed with ethanol to obtain copper-coated iron powder. The solution was air-dried and weighed. An appropriate amount was taken and the volume and weight were measured using a 10 ml measuring cylinder. The volume and weight were measured five times, and the bulk density was determined from the slope of the approximate straight line. The bulk density of the commercially available iron powder was 2.32 g / ml.

[0063] Copper electrolytic sediment from copper smelting was dissolved in concentrated hydrochloric acid and 60% hydrogen peroxide, and solid-liquid separation was performed to obtain PLS (pregnant leach solution). Gold was extracted by mixing the PLS with DBC (dibutyl carbitol). After gold extraction, the PLS was heated to 70°C and a mixture of sulfur dioxide and air (sulfur dioxide concentration 5-20%) was blown in to reduce the precious metals and selenium, resulting in solid-liquid separation. The selenium concentration of the solution after selenium separation was 6 mg / L, tellurium concentration 18 mg / L, ruthenium concentration 130 mg / L, copper concentration 0.55 g / L, and arsenic concentration 1.5 g / L.

[0064] 200 ml of the post-selenium separation liquid (an acidic solution containing ruthenium and arsenic from which ruthenium is to be recovered) was weighed out. 0.8 g of copper sulfate pentahydrate was added and dissolved, and the solution was heated to 50°C. 1 g of each copper-coated iron powder was added and stirred. The reaction was completed in 60 minutes. The precipitate was filtered off, dried, and then weighed.

[0065] 2 ml of the sample was taken for analysis and adjusted to 50 ml. The concentrations of ruthenium, arsenic, and copper in the solution were quantified using an ICP-OES (Seiko SPS3100). For the analysis of the residue, about 0.1 g was measured and dissolved in aqua regia, and the concentration was measured using ICP-OES to calculate the arsenic content. The results are shown in Table 2.

[0066] [Table 2]

[0067] From the results in Table 2, we can see that when producing copper-coated iron powder, the higher the acid concentration of the copper solution, the lower the bulk density and the larger the surface area. The higher the acid concentration during surface coating, the higher the copper grade. This suggests that reduction by hydrogen generated by the acid occurs.

[0068] In the case of cementation using copper-coated iron powder, selenium and tellurium were not detected in the solution after 60 minutes. This is the effect of cementation.

[0069] The recovery of ruthenium was less effective as the acid concentration increased, but considering that the concentration of the raw solution was 130 mg / L, this was not a problem. In terms of selectivity to arsenic, the higher the acid concentration, the more effective it was. Therefore, the acid concentration when preparing copper-coated iron powder should be pH 5 or less, and more preferably pH 2 or less in terms of selectivity to arsenic.

[0070] (Experimental Example 3) 3 g of commercially available iron powder (Wako Pure Chemical Industries, Ltd., P80 = 150 μm) was weighed out. Copper sulfate pentahydrate was added to 200 ml of an aqueous solution whose pH had been adjusted to 0.5 with sulfuric acid to adjust the copper concentration to the values ​​shown in Table 3. The rest of the procedure was the same as in Experimental Example 2 to obtain copper-coated iron powder. The copper concentration in the solution after the coating reaction was also quantified. The obtained copper-coated iron powder was subjected to a cementation test using the same post-selenium separation liquid as in Experimental Example 2. The results are shown in Table 3.

[0071] [Table 3]

[0072] From the results in Table 3, it can be seen that the higher the copper concentration of the copper solution used to prepare the copper-coated iron powder, the lower the bulk density and the higher the surface area. The higher the copper concentration, the higher the copper grade.

[0073] The effect of ruthenium cementation was lower the higher the copper concentration when preparing the copper-coated iron powder. In terms of selectivity with arsenic, the higher the copper concentration when preparing the copper-coated iron powder, the more effective it was. The copper concentration after the coating reaction dropped to 2g / L, so a copper concentration of at least 2g / L is necessary. In addition, at a copper concentration of 25g / L or more, the copper grade and bulk density did not change significantly with the amount added. It is presumed that at 40g / L or more, there is no significant effect on the properties. Therefore, it is preferable to set the copper concentration when preparing copper-coated iron powder to 2 to 40g / L. Since it was prepared by adding 3g of iron powder, it is preferable to adjust the copper concentration to 15g / L, and 0.15 to 3.0 times the amount of iron.

[0074] (Experimental Example 4) 3 g of commercially available iron powder (Wako Pure Chemical Industries, P80 = 150 μm) was weighed out. 15 g of copper sulfate pentahydrate was added to 200 ml of an aqueous solution adjusted to pH 2 with sulfuric acid to prepare a copper salt aqueous solution. Separately, 15 g of copper sulfate pentahydrate was added to 200 ml of tap water to prepare a copper salt aqueous solution. These two solutions were contacted with the iron powder at a reaction temperature adjusted to 20 to 60 ° C. The copper-coated iron powder was obtained by operating in accordance with Experimental Example 1. The obtained copper-coated iron powder was subjected to a cementation test using the same post-selenium separation liquid as in Experimental Example 2. The results are shown in Table 4.

[0075] [Table 4]

[0076] It can be seen that the higher the temperature during preparation of the copper-coated iron powder, the higher the copper content. When copper-coated iron powder prepared at temperatures between 20°C and 60°C was used for cementation, the recovery of ruthenium was high and the precipitation of arsenic was not a problem.

[0077] (Experimental Example 5) A copper salt aqueous solution was prepared by adding a specified amount of copper sulfate pentahydrate shown in Table 5 to 150 ml of an aqueous solution whose pH had been adjusted to 1 with sulfuric acid. 3 g of commercially available iron powder (Wako Pure Chemical Industries, P80=150 μm) was weighed out and added to the copper salt aqueous solution and stirred for 20 seconds to prepare copper-coated iron powder. The copper-coated iron powder was filtered, washed with water, then washed with ethanol and air-dried. Next, 0.8 g of copper-coated iron powder was weighed out and added to 200 ml of 1 mol / L hydrochloric acid and stirred at 30°C. To measure the change in iron concentration in hydrochloric acid over time, samples were taken at predetermined times, filtered, and titrated with potassium dichromate to determine the concentration. For comparison, the same procedure was performed with iron powder to examine the iron dissolution rate. Figure 3 shows the change in iron concentration over time. To compare the cementation rate, the slope of the regression line was calculated. The slope of the regression line was calculated by calculating the average value of the maximum and minimum iron concentrations excluding zero as the intermediate value of the saturated iron concentration, and performing a linear regression process up to the time when this value was reached, and was calculated as the slope of the regression line. For example, in the case of a copper content of 21% in Figure 3, the saturation concentration of iron has a maximum value of 60.15% at 50 minutes, a minimum value excluding zero of 10.43% at 1 minute, an intermediate value (average value) of 35.29%, and the time to reach this value is 9 minutes. Therefore, regression processing was performed for 0% at 0 minutes, 10.43% at 1 minute, 17.34% at 3 minutes, 30.62% at 6 minutes, and 36.99% at 9 minutes, and 4.0 mass% / min was calculated as the slope of the linear regression line. In order to make the slope of the regression line more general, the concentration is calculated as a percentage by dividing the dissolved iron concentration (g / L) by the amount of iron powder added in this experiment, which was 4g / L. In addition, 0.4 g of the copper-coated iron powder was weighed out and subjected to a cementation test using the same selenium separation solution as in Experimental Example 2. After one hour, the concentrations of ruthenium and arsenic were quantified. The results are shown in Table 5.

[0078] [Table 5]

[0079] 36g of copper sulfate pentahydrate is equivalent to 9.1g of copper. Copper-coated iron powder was obtained that selectively recovered ruthenium even when coated with copper at a concentration three times the weight of the iron powder. When 26.7g of copper sulfate pentahydrate was added, the equivalent was 6.8g of copper, but the bulk density was smaller and the copper content was higher than when 36g was added. Although differences in properties were observed, the cementation behavior was almost the same for both.

[0080] Looking at the slope of the regression line in Table 5, it shows that the weight of the metal powder added to 1 mol / L hydrochloric acid is reduced at a rate of 0.9 to 4.4 mass% / min. Figure 3 shows the change over time when iron powder is dissolved with a copper content of 0%, and the slope of the regression line calculated in the same manner was 7.4 mass% / min. Even with a copper content of 9%, the slope of the regression line was about 40% lower than in the case of iron.

[0081] From the results in Table 5, it can be seen that if the slope of the regression line is 4.0 mass% / min or less, the cementation rate is such that ruthenium is efficiently cemented relative to arsenic. This is because the exposed surface of iron is appropriately small, and the surface area is also kept large. The slope of the regression line is more preferably 2.5 mass% / min or less.

Claims

1. A copper-coated iron powder for ruthenium cementation, which is an iron powder whose surface is coated with copper, and which is characterized in that ruthenium is selectively precipitated from an acidic solution containing ruthenium and arsenic.

2. The copper-coated iron powder according to claim 1, characterized in that the copper content is 10 to 80 mass %.

3. 3. The copper-coated iron powder according to claim 1, wherein the bulk density is 60% or less of the bulk density of iron powder having the same particle size as the copper-coated iron powder.

4. The copper-coated iron powder according to any one of claims 1 to 3, characterized in that the bulk density is 1.3 g / ml or less.

5. The copper-coated iron powder according to any one of claims 1 to 4, characterized in that P80 is 100 μm to 5 mm.

6. The copper-coated iron powder according to any one of claims 1 to 5, characterized in that when immersed in 1 mol / L hydrochloric acid at 30°C and stirred, the iron dissolution rate per added mass is calculated as the slope of the regression line up to the time at which the iron concentration reaches the intermediate value of the saturation concentration, and is 4.0 mass% / min or less of the copper-coated iron powder.

7. A method for producing copper-coated iron powder for cementing valuable materials from an acidic solution containing ruthenium, at least one of selenium and tellurium, and arsenic as valuable materials, comprising: A method for producing copper-coated iron powder, comprising the step of contacting iron powder with an aqueous solution of pH 5 or less containing a water-soluble copper salt to coat the surface of the iron powder with copper.

8. 8. The method for producing copper-coated iron powder according to claim 7, wherein the aqueous solution containing the water-soluble copper salt has a copper concentration of 2 to 40 g / L.

9. 9. The method for producing a copper-coated iron powder according to claim 7 or 8, wherein the aqueous solution containing the water-soluble copper salt has a copper concentration of 0.15 to 3.0 times by mass the iron concentration.

10. The method for producing copper-coated iron powder according to any one of claims 7 to 9, characterized in that the aqueous solution containing the water-soluble copper salt is contacted with the iron powder while adjusting the liquid temperature to 20 to 60°C.

11. The method for producing copper-coated iron powder according to any one of claims 7 to 10, characterized in that the iron powder has a P80 of 150 μm or less.

12. The method for producing copper-coated iron powder according to any one of claims 7 to 11, characterized in that the reaction time of the contact is adjusted so that the bulk density is 60% or less of the bulk density of iron powder of the same particle size as the iron powder whose surface is coated with copper.

13. The method for producing the copper-coated iron powder according to any one of claims 7 to 12, characterized in that the aqueous solution containing the water-soluble copper salt is continuously supplied to a container containing the iron powder, thereby contacting the iron powder with the aqueous solution containing the water-soluble copper salt.

14. A method for recovering ruthenium, comprising the steps of: adjusting the liquid temperature of an acidic solution containing ruthenium and arsenic to 20° C. or higher and 80° C. or lower using the copper-coated iron powder according to any one of claims 1 to 6; and contacting the copper-coated iron powder and arsenic in the liquid to precipitate ruthenium.

Citation Information

Patent Citations

  • JP1972003019A

  • Production of metal-coated powder

    JP1988183101A

  • Method for treating anode slime

    JP2001316735A

  • Method for separating selenium, tellurium and platinum group metal

    JP2016160479A

  • Method of recovering ruthenium

    JP2019147990A